Secondary battery and electric device
By adopting an asymmetric design on the negative electrode of the lithium-ion battery and setting differentiated coatings on both sides of the current collector, the contradiction between fast charging performance and high energy density is resolved, and the overall performance of the battery is improved.
Patent Information
- Application Number
- CN202611358177.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-20
AI Technical Summary
The symmetrical design of existing lithium-ion battery anode sheets makes it difficult to simultaneously meet the requirements of fast charging performance and high energy density. Traditional graphite lithium insertion/extraction kinetics are limited, and composite anode materials suffer from problems such as large expansion and poor structural stability.
The negative electrode adopts an asymmetric design, with coatings of different active materials, porosity and areal density on both sides of the current collector. The first surface is a fast charging layer and the second surface is a capacity layer, which optimizes fast charging performance and energy density respectively.
It achieves a significant reduction in fast charging time, a decrease in charging temperature rise, and an improvement in cycle life and storage stability while maintaining high energy density in lithium-ion batteries, making it suitable for power batteries, energy storage batteries, and consumer batteries.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of electrochemical energy storage technology, and in particular to a secondary battery and electrical equipment. Background Technology
[0002] Current lithium-ion battery anode sheets generally employ a double-sided, completely symmetrical coating structure. The coatings on both sides of the electrode maintain consistency in active material type, coating areal density, coating porosity, and compaction state. This results in a simple manufacturing process with high consistency, but has long presented an inherent technical contradiction: balancing fast-charging performance with energy density. To improve fast-charging capability, conventional methods typically reduce the overall areal density of the anode coating and increase its porosity to shorten lithium-ion migration distance and reduce charging polarization. However, this significantly reduces the active material loading on the electrode, leading to a substantial decrease in battery energy density. Conversely, increasing the overall areal density and reducing porosity to ensure high energy density results in narrow lithium-ion transport channels, increased interfacial polarization, and a high risk of lithium plating, overheating, and accelerated cycle degradation during high-current charging, severely limiting fast-charging performance. Meanwhile, traditional symmetrical anodes generally employ a single graphite system, and the kinetic rate of lithium insertion / extraction in graphite is limited, making it difficult to adapt to the demands of high-rate charging. If both sides use composite anode materials with high capacity and high kinetic properties, it will lead to defects such as large overall expansion, poor structural stability, and reduced cycle life. In summary, existing symmetrical anode structures are limited by a uniform material system and uniform structural parameters, making it difficult to optimize performance according to the differences in the electrochemical operating environments on both sides of the electrode, and making it difficult to simultaneously meet the increasingly demanding requirements of high-speed charging, high energy density, and long-cycle stability in power batteries. Summary of the Invention
[0003] This application aims to at least solve one of the aforementioned technical problems existing in the prior art. Therefore, one objective of this application is to provide a secondary battery. Another objective of this application is to provide an electrical device.
[0004] To achieve the above objectives, the technical solution adopted in this application is as follows: A first aspect of this application provides a secondary battery, the secondary battery comprising a negative electrode sheet; The negative electrode sheet includes: The negative electrode current collector has a first surface and a second surface opposite to the first surface; A first negative electrode coating is disposed on a first surface of the negative electrode current collector and contains a first negative electrode active material; a second negative electrode coating is disposed on a second surface of the negative electrode current collector and contains a second negative electrode active material. The first negative electrode active material includes mesophase carbon microspheres, hard carbon, graphite, and SiO2. x At least two of the following (0 < x < 2); the second negative electrode active material includes graphite; The porosity of the first negative electrode coating is greater than that of the second negative electrode coating; The areal density of the first negative electrode coating is less than that of the second negative electrode coating.
[0005] Specifically, existing lithium-ion battery anode sheets generally employ a completely symmetrical design with coatings on both sides. This means that the first and second surfaces of the anode current collector are coated with the same active material, the same areal density, and the same porosity. Under this symmetrical design, while the overall low areal density / high porosity can achieve fast charging, the energy density is significantly reduced. Conversely, while the overall high areal density / low porosity can achieve high energy density, it results in large polarization, easy lithium deposition, and poor cycle life during fast charging. In other words, the symmetrical design cannot simultaneously meet the comprehensive requirements of fast charging, high energy density, and long cycle life. Therefore, this application proposes an asymmetric design for the negative electrode sheet. By setting a first negative electrode coating and a second negative electrode coating with different active materials, different porosities, and different areal densities on the first and second surfaces of the current collector of the negative electrode sheet, one side of the negative electrode sheet has the characteristics of high porosity, low areal density, and low impedance, which is beneficial to improving the fast charging performance of the negative electrode sheet. The other side has the characteristics of high compaction, high areal density, and high energy density, which is beneficial to improving the active material load of the negative electrode sheet, thereby balancing the fast charging capability and energy density of the battery.
[0006] In some embodiments of this application, the first negative electrode active material comprises a mixture of mesophase carbon microspheres (MCMB) and hard carbon, wherein the mesophase carbon microspheres account for 90%-96% of the total mass of the first negative electrode active material. This ensures that the first negative electrode coating possesses high conductivity, high structural stability, and excellent fast-charging performance.
[0007] In some embodiments of this application, the first negative electrode active material includes graphite and SiO2. x A mixture of (0 < x < 2), the SiO x (0 < x < 2) accounts for 4%-20% of the total mass of the first negative electrode active material. This ensures that the first negative electrode coating has high conductivity, high structural stability and excellent fast charging performance.
[0008] In some embodiments of this application, the porosity of the first negative electrode coating is ≥42%, and the porosity of the second negative electrode coating is ≤36%. This allows the first negative electrode coating to maintain sufficient ion channels and reduce polarization, while the second negative electrode coating ensures high compaction density and increases energy density. Simultaneously, it can reduce lithium plating, decrease heat generation during battery charging, and improve battery cycle performance.
[0009] In some embodiments of this application, the porosity of the first negative electrode coating is 42%-48%; the porosity of the second negative electrode coating is 30%-36%.
[0010] In some embodiments of this application, the areal density of the first negative electrode coating is 215 mg / 1540.25 mm². 2 -246mg / 1540.25mm 2 The areal density of the second negative electrode coating is 275 mg / 1540.25 mm². 2 -345mg / 1540.25mm 2 This shortens the lithium-ion migration distance, improves fast charging speed, and ensures high overall electrode load and high energy output.
[0011] In some embodiments of this application, the first negative electrode coating further comprises a first conductive agent, and the second negative electrode coating further comprises a second conductive agent; the mass content of the first conductive agent in the first negative electrode coating is less than or equal to the mass content of the second conductive agent in the second negative electrode coating. Thus, by utilizing the high conductivity composite conductive agent in the first negative electrode coating, the amount of conductive agent used is reduced and the energy density is increased while ensuring low-impedance fast-charging performance; the second negative electrode coating increases the conductive agent content, ensuring the continuous and stable conductive network under high areal density loads, reducing polarization, improving cycle stability, and simultaneously reducing the rate of increase of the battery's DC resistance, which is beneficial for improving low-temperature cycle performance and battery storage performance.
[0012] In some embodiments of this application, the first conductive agent comprises a mixture of carbon nanotubes and conductive carbon black, wherein the mass ratio of the carbon nanotubes to the conductive carbon black is 1-1.5:1; the second conductive agent comprises conductive carbon black. This enables the construction of a long-range conductive network and reduces interfacial impedance; the use of conductive carbon black in the second negative electrode coating simplifies the formulation and ensures high conductivity and low cost.
[0013] In some embodiments of this application, the mass percentage of the first conductive agent in the first negative electrode coating is ≤2.5%; and the mass percentage of the second conductive agent in the second negative electrode coating is ≥2.5%. This ensures that the first negative electrode coating has low impedance while preventing the conductive agent from excessively reducing energy density, and that the second negative electrode coating maintains conductivity continuity under high loads.
[0014] In some embodiments of this application, the first conductive agent accounts for 1.5%-2.5% of the mass of the first negative electrode coating; the second conductive agent accounts for 2.5%-3.0% of the mass of the second negative electrode coating.
[0015] In some embodiments of this application, the secondary battery further includes a positive electrode, which comprises: The positive current collector has a third surface and a fourth surface opposite to the third surface; A first positive electrode coating is disposed on the third surface of the positive electrode current collector and contains a first positive electrode active material; The second positive electrode coating is disposed on the fourth surface of the positive electrode current collector and contains a second positive electrode active material; The first positive electrode active material includes a lithium transition metal oxide or a lithium transition metal oxide with at least an oxide or carbon material disposed on its surface, and the second positive electrode active material includes a lithium transition metal oxide.
[0016] Specifically, the positive electrode adopts a double-sided symmetrical or double-sided asymmetrical design. The first positive electrode coating and the second positive electrode coating are the same or different. When the first positive electrode coating and the second positive electrode coating are different, the first positive electrode coating uses lithium transition metal oxide with at least oxide or carbon material on its surface to reduce interface impedance and improve fast charging stability. The second positive electrode coating side uses lithium transition metal oxide without coating to ensure high capacity output. Together with the asymmetrical design of the negative electrode, it improves the overall performance of the battery.
[0017] In some embodiments of this application, the first positive electrode coating further comprises a third conductive agent, and the second positive electrode coating further comprises a fourth conductive agent; the mass content of the third conductive agent in the first positive electrode coating is less than the mass content of the fourth conductive agent in the second positive electrode coating. This reduces the proportion of inactive components in the first positive electrode coating, ensuring energy density, and utilizes a higher amount of the fourth conductive agent to form a continuous and stable three-dimensional conductive pathway in the second positive electrode coating, improving the utilization rate of active materials and cycle stability. The differentiated design of the conductive agent content in the two layers allows the double-sided positive electrode coatings to adapt to different operating conditions such as fast charging and high capacity.
[0018] In some embodiments of this application, the third conductive agent comprises poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT: PSS); and the fourth conductive agent comprises conductive carbon black. Thus, the first positive electrode coating can form a continuous conductive film, reduce interfacial impedance, and improve fast-charging performance; the second positive electrode coating can ensure high conductivity.
[0019] The second aspect of this application provides an electrical device, which includes the secondary battery described in the first aspect of this application, and the secondary battery serves as the power supply for the electrical device.
[0020] Specifically, the electrical equipment using the aforementioned secondary batteries possesses high energy density, excellent fast-charging performance, and long cycle life, meeting the high requirements of energy storage, power, and other scenarios.
[0021] Compared with the prior art, the beneficial effects of this application are: The secondary battery provided in this application adopts a double-sided asymmetric coating negative electrode structure. By setting functionally differentiated coatings on both sides of the current collector, it achieves synergistic optimization of high energy density and high fast-charging performance, effectively breaking through the performance bottleneck of traditional symmetrical negative electrode sheets. The first negative electrode coating on the first surface adopts mesophase carbon microspheres, hard carbon, graphite, and SiO2. x A mixture of at least two of the elements in (0 < x < 2) serves as the active material. Combined with higher porosity and lower areal density, it constructs unobstructed lithium-ion transport channels, shortens ion migration distance, effectively reduces charging polarization, and significantly improves the battery's fast-charging capability. The second negative electrode active material of the second negative electrode coating on the second surface includes graphite. Combined with lower porosity and higher areal density, it increases electrode compaction density and active material loading, ensuring the battery possesses excellent energy density and cycle stability. This design is compatible with existing coating and rolling processes without significant production line modifications. It also improves electrode interface stability and stress distribution, reducing side reactions, lithium plating risks, and coating powdering and breakage issues. Experimental data shows that batteries using this structure maintain high energy density while significantly shortening fast-charging time, reducing charging temperature rise, significantly improving cycle life and room-temperature storage stability, minimizing DC internal resistance increase, and exhibiting superior low-temperature discharge and long-term storage performance. It can be widely adapted to the multi-condition high-performance requirements of power batteries, energy storage batteries, and consumer batteries. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the secondary battery structure in Example 1; Figure 2 This is a schematic diagram of the coating process for the negative electrode sheet of the secondary battery in Example 1. Detailed Implementation
[0023] In one embodiment of this application, a secondary battery is provided, including a negative electrode sheet; the negative electrode sheet includes: The negative electrode current collector has a first surface and a second surface opposite to the first surface; A first negative electrode coating is disposed on the first surface of the negative electrode current collector and contains a first negative electrode active material; a second negative electrode coating is disposed on the second surface of the negative electrode current collector and contains a second negative electrode active material. The first negative electrode active material includes mesophase carbon microspheres, hard carbon, graphite, and SiO2. x At least two of the following (0 < x < 2); the second negative electrode active material includes graphite; The porosity of the first negative electrode coating is greater than that of the second negative electrode coating. The areal density of the first negative electrode coating is less than that of the second negative electrode coating.
[0024] This application employs a double-sided asymmetric design. The first negative electrode coating on the first surface of the negative electrode current collector is designed as a fast-charging layer, featuring high porosity and low areal density to shorten the lithium-ion migration path, reduce polarization, and suppress lithium plating. It utilizes mesophase carbon microspheres, hard carbon, graphite, and SiO2. x At least two of the materials in (0 < x < 2) are used as the first negative electrode active material, balancing fast charging dynamics and structural stability. The second negative electrode coating on the second surface of the negative electrode current collector is designed as a capacity layer, employing low porosity and high areal density to improve overall energy density. Pure graphite is used to ensure high capacity, low expansion, and mature and stable processing. By designing differentiated materials, structures, and parameters on both sides, the contradiction between fast charging performance and energy density is resolved separately. The first negative electrode coating enables high-rate charging, while the second negative electrode coating is dedicated to high energy output. Together, they achieve a comprehensive performance breakthrough of high energy density, excellent fast charging capability, and long cycle life.
[0025] The porosity of the first negative electrode coating can be tested using the following method: The negative electrode sheet is cut into rectangular pieces of 0.8cm × 2.3cm. The second negative electrode coating is removed by mechanical peeling. The pieces are then heated to 110℃ in a 3Pa vacuum oven and held for 4 hours to remove residual air and moisture from the pores, yielding the sample to be tested. The mass, total thickness, and current collector thickness of each sample are recorded. The sample is then rolled into a thin strip and loosely placed into a glass dilatometer, ensuring that the sample volume occupies 40%-70% of the effective volume of the sample tube. The dilatometer containing the sample is sealed, and the equipment is evacuated to a vacuum level. At least 3 Pa is reached, and liquid mercury is automatically injected. The pressure is gradually increased in the low-pressure zone (≤0.2 MPa), and the volume of mercury injected into the large pores (>1 μm) is recorded. After the low-pressure test is completed, the dilatometer is transferred to the high-pressure chamber (≤400 MPa), and the external pressure and the corresponding volume of mercury injected are recorded. After the test is completed, the pressure is released, the liquid mercury is recovered, and the sample is taken out. The thickness of the first negative electrode coating is obtained by subtracting the thickness of the current collector from the total thickness of the sample. The volume of the first negative electrode coating is obtained by multiplying it by the area of the negative electrode sheet. Then, the porosity of the first negative electrode coating is obtained by dividing the volume of mercury (pore volume) in the high-pressure section by the volume of the coating.
[0026] The porosity test method for the second negative electrode coating is the same as that for the first negative electrode coating. The only difference is that the first negative electrode coating is removed by mechanical peeling, and the sample is heated to 110°C in a 3Pa vacuum oven and kept for 4 hours to remove residual air and moisture in the pores, thus obtaining the sample to be tested.
[0027] The areal density of the first negative electrode coating and the second negative electrode coating can be obtained by the following method: measure the coating area of the first negative electrode coating, then mechanically peel off the first surface of the negative electrode sheet, collect the powder, weigh the mass, and calculate the ratio of the powder mass to the coating area of the first negative electrode coating, which is the areal density of the first negative electrode coating.
[0028] The method for testing the areal density of the second negative electrode coating is the same as that for the first negative electrode coating. The only difference is that the coating area of the second negative electrode coating is measured, and the second surface of the negative electrode sheet is mechanically peeled off, the powder is collected, the mass is weighed, and the ratio of the powder mass to the coating area of the second negative electrode coating is calculated, which is the areal density of the second negative electrode coating.
[0029] In some embodiments, the first negative electrode active material accounts for 95%-96% of the mass of the first negative electrode coating.
[0030] In some embodiments, the second negative electrode active material accounts for 94%-95% of the mass of the second negative electrode coating.
[0031] In some embodiments, the thickness of the negative electrode current collector is 5.2-7.8 μm; in other embodiments, the thickness of the negative electrode current collector is 5.8-7.2 μm, for example, it can be selected from any one of 5.8 μm, 6.2 μm, 6.6 μm, 7.0 μm, 7.2 μm or any range formed by any two values.
[0032] In some implementations, the negative current collector is copper foil.
[0033] In some embodiments, the diaphragm is a composite diaphragm of a polymer-based membrane and a single-sided inorganic ceramic coating; the total thickness of the diaphragm is 12-19 μm, and the thickness of the inorganic ceramic coating is 2-4 μm.
[0034] In some embodiments, the total thickness of the diaphragm is 14-18 μm, for example, it can be selected from any one of 14 μm, 15 μm, 16 μm, 17 μm, 18 μm or any range formed by any two values; the thickness of the inorganic ceramic coating is 2.5-3.5 μm, for example, it can be selected from any one of 2.5 μm, 2.8 μm, 3.1 μm, 3.3 μm, 3.5 μm or any range formed by any two values.
[0035] In some embodiments, the polymer base film is selected from polyethylene film (PE), polypropylene film (PP), or polypropylene / polyethylene bilayer composite film (PP / PE).
[0036] In some embodiments, the inorganic ceramic coating is an alumina coating or a boehmite coating.
[0037] In some embodiments, the first negative electrode active material is a mixture of mesophase carbon microspheres and hard carbon, wherein the mesophase carbon microspheres account for 90%-96% of the total mass of the first negative electrode active material; for example, it can be selected from any one of 90%, 91%, 93%, 94%, 96% or a range formed by any two values.
[0038] In some embodiments, the first negative electrode active material is graphite and SiO2.x A mixture of (0 < x < 2), SiO x (0 < x < 2) accounts for 4%-20% of the total mass of the first negative electrode active material; for example, it can be selected from any one of 4%, 5%, 7%, 9%, 10%, 20% or any range formed by any two values.
[0039] In some embodiments, the porosity of the first negative electrode coating is ≥42%, and the porosity of the second negative electrode coating is ≤36%; in other embodiments, the porosity of the first negative electrode coating is 42%-48%, for example, it can be selected from any one of 42%, 43%, 44%, 45%, 46%, 47%, 48% or any range formed by any two values; the porosity of the second negative electrode coating is 30%-36%, for example, it can be selected from any one of 30%, 32%, 34%, 35%, 36% or any range formed by any two values.
[0040] In some embodiments, the areal density of the first negative electrode coating is 215 mg / 1540.25 mm². 2 -246mg / 1540.25mm 2 The areal density of the second negative electrode coating is 275 mg / 1540.25 mm². 2 -345mg / 1540.25mm 2 In other embodiments, the areal density of the first negative electrode coating is 225 mg / 1540.25 mm². 2 -240mg / 1540.25mm 2 For example, it can be selected from 225mg / 1540.25mm 2 229mg / 1540.25mm 2 233mg / 1540.25mm 2 237mg / 1540.25mm 2 240mg / 1540.25mm 2 The range formed by any one or any two values in the range; the areal density of the second negative electrode coating is 300 mg / 1540.25 mm. 2 -320mg / 1540.25mm 2 For example, it can be selected from 300mg / 1540.25mm. 2 305mg / 1540.25mm 2 310mg / 1540.25mm 2 315mg / 1540.25mm 2 320mg / 1540.25mm 2 The range formed by any one or any two values in the range.
[0041] In some embodiments, the first negative electrode coating further comprises a first conductive agent, and the second negative electrode coating further comprises a second conductive agent; the mass content of the first conductive agent in the first negative electrode coating is less than or equal to the mass content of the second conductive agent in the second negative electrode coating.
[0042] In some embodiments, the first conductive agent comprises a mixture of carbon nanotubes and conductive carbon black, wherein the mass ratio of carbon nanotubes to conductive carbon black is 1-1.5:1; the second conductive agent comprises conductive carbon black; in other embodiments, the mass ratio of carbon nanotubes to conductive carbon black is any one of 1.5:1, 1.2:1, or 1:1.
[0043] In some embodiments, the first conductive agent has a mass percentage of ≤2.5% in the first negative electrode coating; the second conductive agent has a mass percentage of ≥2.5% in the second negative electrode coating. In other embodiments, the first conductive agent has a mass percentage of 1.5%-2.5% in the first negative electrode coating, for example, it can be selected from any one of 1.5%, 1.8%, 2.0%, 2.2%, 2.5% or a range formed by any two values; the second conductive agent has a mass percentage of 2.5%-3.5% in the second negative electrode coating, for example, it can be selected from any one of 2.5%, 2.8%, 3.0%, 3.2%, 3.5% or a range formed by any two values.
[0044] In some embodiments, the first negative electrode coating further comprises a first adhesive, which includes a composite adhesive of styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC); the mass ratio of SBR to sodium carboxymethyl cellulose is (1.5-2.0):1, for example, it can be selected from any ratio of 1.5:1, 1.6:1, 1.8:1, 1.9:1, 2.0:1.
[0045] In some embodiments, the first adhesive accounts for 2.0%-3.0% of the mass of the first negative electrode coating.
[0046] In some embodiments, the second negative electrode coating further comprises a second adhesive, and the first adhesive comprises a composite adhesive of styrene-butadiene rubber and sodium carboxymethyl cellulose.
[0047] In some embodiments, the first adhesive accounts for 2.0%-3.0% of the mass of the first negative electrode coating.
[0048] In some embodiments, the roll-forming thickness of the first negative electrode coating is 180-200 μm; in other embodiments, the roll-forming thickness of the first negative electrode coating is 185-195 μm, for example, it can be selected from any one of 185 μm, 188 μm, 191 μm, 193 μm, 195 μm or a range formed by any two values.
[0049] In some embodiments, the roll-forming thickness of the second negative electrode coating is 220-240 μm; in other embodiments, the roll-forming thickness of the second negative electrode coating is 225-235 μm, for example, it can be selected from any one of 225 μm, 228 μm, 231 μm, 233 μm, 235 μm or a range formed by any two values.
[0050] In some embodiments, the compaction density of the first negative electrode coating is 1.55-1.65 g / cm³. 3 In other embodiments, the compaction density of the first negative electrode coating is 1.55-1.60 g / cm³. 3 For example, it can be selected from 1.55 g / cm³. 3 1.56g / cm 3 1.58g / cm 3 1.59g / cm 3 1.60g / cm 3 The range formed by any one or any two values in the range.
[0051] In some embodiments, the compaction density of the second negative electrode coating is 1.70-1.80 g / cm³. 3 In other embodiments, the compaction density of the second negative electrode coating is 1.70-1.75 g / cm³. 3 For example, it can be selected from 1.70 g / cm³. 3 1.71g / cm 3 1.73g / cm 3 1.74 g / cm 3 1.75g / cm 3 The range formed by any one or any two values in the range.
[0052] In some embodiments, the secondary battery further includes a positive electrode, which comprises: The positive current collector has a third surface and a fourth surface opposite to the third surface; The first positive electrode coating is disposed on the third surface of the positive electrode current collector and contains the first positive electrode active material; The second positive electrode coating is disposed on the fourth surface of the positive electrode current collector and contains the second positive electrode active material; The first positive electrode active material is selected from lithium transition metal oxides with at least an oxide or carbon material disposed on the surface, and the second positive electrode active material includes lithium transition metal oxides; in other embodiments, the lithium transition metal oxide includes one of lithium iron phosphate and lithium nickel cobalt manganese oxide.
[0053] In some embodiments, the oxide is selected from at least one of Al2O3, TiO2, ZrO2, Li3PO4, Li2TiO3, LiAlO2, LiNbO3, and Li2MoO4, and the carbon material is selected from at least one of carbon nanotubes, conductive carbon black, or graphene.
[0054] In some embodiments, the first positive electrode coating further includes a third conductive agent, and the second positive electrode coating further includes a fourth conductive agent; the mass content of the third conductive agent in the first positive electrode coating is less than the mass content of the fourth conductive agent in the second positive electrode coating.
[0055] In some embodiments, the third conductive agent includes poly(3,4-ethylenedioxythiophene):polystyrene sulfonate (PEDOT: PSS); the fourth conductive agent includes conductive carbon black.
[0056] In some embodiments, the first positive electrode coating further comprises a third adhesive; the third adhesive includes polyvinylidene fluoride (PVDF).
[0057] In some embodiments, the second positive electrode coating further comprises a fourth adhesive; the fourth adhesive includes polyvinylidene fluoride (PVDF).
[0058] One embodiment of this application provides an electrical device including the aforementioned secondary battery, which serves as the power supply for the electrical device.
[0059] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.
[0060] Example 1 This embodiment provides a secondary battery, the preparation method of which includes the following steps: (1) Preparation of the positive electrode sheet: Carbon-coated lithium iron phosphate (particle size Dv50=1.8μm), conductive carbon black and polyvinylidene fluoride were dispersed in N-methylpyrrolidone at a mass ratio of 96:2:2 and stirred to prepare a uniform positive electrode slurry. The positive electrode slurry was uniformly coated on the third and fourth surfaces of the positive electrode current collector aluminum foil. After coating, it was dried and rolled, and then cut to obtain the positive electrode sheet. (2) Preparation of negative electrode sheet: First negative electrode slurry: Active material mesophase carbon microspheres and hard carbon (95:5, w / w), conductive agent Super P and carbon nanotubes (1:1.5, w / w), binder styrene-butadiene rubber and sodium carboxymethyl cellulose (1.8:1, w / w) are stirred and dispersed evenly at a mass ratio of 95.4:1.9:2.7 to prepare the first negative electrode slurry; Second negative electrode slurry: Artificial graphite (SG-2), conductive agent Super P, binder styrene-butadiene rubber and sodium carboxymethyl cellulose (1.8:1, w / w) are stirred and dispersed evenly at a mass ratio of 94.5:2.8:2.7 to prepare the second negative electrode slurry; Copper foil was selected as the negative electrode current collector. The current collector has a first surface and a second surface. A first negative electrode slurry was coated on the first surface, and the coating surface density was controlled to be 228 mg / 1540.25 mm². 2 A second negative electrode slurry is coated on the second surface, with the coating surface density controlled at 302 mg / 1540.25 mm². 2 After drying, the second surface is pre-rolled separately at a pressure of 8.5 MPa, and then the entire electrode sheet is lightly rolled and shaped at a pressure of 4.0 MPa, forming the first and second negative electrode coatings. After rolling, the thickness of the first negative electrode coating is 188 μm, and the compaction density is 1.56 g / cm³. 3 The porosity is 45%, the thickness of the second negative electrode coating is 226 μm, and the compaction density is 1.72 g / cm³. 3 The porosity is 34%, and it is then cut to obtain the negative electrode sheet; (3) Preparation of electrolyte: Ethylene carbonate, diethyl carbonate, and fluoroethylene carbonate were mixed in a volume ratio of 3:5:2 to obtain a mixed organic solvent. Lithium hexafluorophosphate was dissolved in the mixed solvent at a concentration of 1 mol / L. Then, 1 wt% propane sulfonic anhydride was added and stirred thoroughly to dissolve the solution, thus preparing the electrolyte.
[0061] (4) Preparation of secondary batteries: The positive electrode, separator (ceramic PE separator), and negative electrode are fed into a high-speed Z-type stacking machine and stacked in a Z-shaped alternating stacking manner to form a bare cell. After the bare cell is hot-pressed, it is placed in an aluminum alloy shell. The prepared electrolyte is injected into the dried bare cell. After standing, formation, aging and capacity testing, a secondary battery is obtained.
[0062] Figure 1 This is a schematic diagram of the secondary battery structure in Example 1. Figure 1It is known that the secondary battery includes a positive electrode, a negative electrode, and a separator. The negative electrode includes a negative current collector, which has a first surface and a second surface opposite to the first surface. The first negative electrode coating on the first surface uses mesophase carbon microspheres and hard carbon as the first negative electrode active material, and the second negative electrode coating on the second surface uses artificial graphite as the second negative electrode active material.
[0063] Figure 2 This is a schematic diagram of the coating process for the negative electrode sheet of the secondary battery in Example 1.
[0064] Example 2 This embodiment provides a secondary battery, the preparation method of which includes the following steps: (1) Preparation of the positive electrode sheet: NCM622 (particle size Dv50=1.8μm), conductive carbon black and polyvinylidene fluoride were dispersed in N-methylpyrrolidone at a mass ratio of 96:2:2 and stirred to prepare a uniform positive electrode slurry. The positive electrode slurry was uniformly coated on the third and fourth surfaces of the positive electrode current collector aluminum foil. After coating, it was dried and rolled, and then cut to obtain the positive electrode sheet. (2) Preparation of negative electrode sheet: First negative electrode slurry: Combining active materials graphite and SiO2 x (0 < x < 2) (96: 4, w / w), conductive agent Super P and carbon nanotubes (1: 1, w / w), binder styrene-butadiene rubber and sodium carboxymethyl cellulose (1.5: 1, w / w) were stirred and dispersed evenly at a mass ratio of 95.7:1.9:2.4 to prepare the first negative electrode slurry; Second negative electrode slurry: Artificial graphite (SG-1), conductive agent Super P, binder styrene-butadiene rubber and sodium carboxymethyl cellulose (1.5:1, w / w) are stirred and dispersed evenly at a mass ratio of 94.8:2.8:2.4 to prepare the second negative electrode slurry; Copper foil was selected as the negative electrode current collector. The current collector has a first surface and a second surface. A first negative electrode slurry was coated on the first surface, and the coating surface density was controlled to be 237 mg / 1540.25 mm². 2 A second negative electrode slurry is coated on the second surface, with the coating surface density controlled at 317 mg / 1540.25 mm². 2 After drying, the second surface is pre-rolled separately at a pressure of 8.5 MPa, and then the entire electrode sheet is lightly rolled and shaped at a pressure of 4.0 MPa, forming the first and second negative electrode coatings. After rolling, the thickness of the first negative electrode coating is 193 μm, and the compaction density is 1.59 g / cm³. 3 The porosity is 44%, the thickness of the second negative electrode coating is 233 μm, and the compaction density is 1.75 g / cm³. 3The porosity is 33%, and it is then cut to obtain the negative electrode sheet; (3) Preparation of electrolyte: Ethylene carbonate, diethyl carbonate, and fluoroethylene carbonate were mixed in a volume ratio of 3:6:1 to obtain a mixed organic solvent. Lithium hexafluorophosphate with a concentration of 1.15 mol / L was dissolved in the mixed solvent, and then 1 wt% vinylene carbonate was added. The mixture was stirred thoroughly to dissolve the electrolyte.
[0065] (4) Preparation of secondary batteries: The positive electrode, separator (ceramic PE separator), and negative electrode are fed into a high-speed Z-type stacking machine and stacked in a Z-shaped alternating stacking manner to form a bare cell. After the bare cell is hot-pressed, it is placed in an aluminum alloy shell. The prepared electrolyte is injected into the dried bare cell. After standing, formation, aging and capacity testing, a secondary battery is obtained.
[0066] Example 3 This embodiment provides a secondary battery, the preparation method of which includes the following steps: (1) Preparation of the positive electrode sheet: First cathode slurry: LiNbO3-coated NCM622 (particle size Dv50=1.8μm), PEDOT: PSS and polyvinylidene fluoride were dispersed in N-methylpyrrolidone at a mass ratio of 96:1.5:2.5 and stirred to prepare a uniform first cathode slurry; Second positive electrode slurry: NCM622 (particle size Dv50=1.8μm), conductive carbon black and polyvinylidene fluoride are dispersed in N-methylpyrrolidone at a mass ratio of 96:2:2 and stirred to prepare a uniform second positive electrode slurry; Aluminum foil was selected as the positive electrode current collector. The current collector has a third surface and a fourth surface. A first positive electrode slurry was coated on the third surface, and a second positive electrode slurry was coated on the fourth surface. After drying, the coating was rolled to form a first positive electrode coating and a second positive electrode coating. After rolling, the thickness of the first positive electrode coating was 130 μm, and the compaction density was 1.50 g / cm³. 3 The porosity is 38%, the thickness of the second positive electrode coating is 145 μm, and the compaction density is 1.70 g / cm³. 3 The porosity is 30%, and it is then cut to obtain the positive electrode sheet; (2) Preparation of negative electrode sheet: First negative electrode slurry: Active material mesophase carbon microspheres and hard carbon (95:5, w / w), conductive agent Super P and carbon nanotubes (1:1.5, w / w), binder styrene-butadiene rubber and sodium carboxymethyl cellulose (1.8:1, w / w) are stirred and dispersed evenly at a mass ratio of 95.4:1.9:2.7 to prepare the first negative electrode slurry; Second negative electrode slurry: Artificial graphite (SG-2), conductive agent Super P, binder styrene-butadiene rubber and sodium carboxymethyl cellulose (1.8:1, w / w) are stirred and dispersed evenly at a mass ratio of 94.5:2.8:2.7 to prepare the second negative electrode slurry; Copper foil was selected as the negative electrode current collector. The current collector has a first surface and a second surface. A first negative electrode slurry was coated on the first surface, and the coating surface density was controlled to be 228 mg / 1540.25 mm². 2 A second negative electrode slurry is coated on the second surface, with the coating surface density controlled at 302 mg / 1540.25 mm². 2 After drying, the second surface is pre-rolled separately at a pressure of 8.5 MPa, and then the entire electrode sheet is lightly rolled and shaped at a pressure of 4.0 MPa, forming the first and second negative electrode coatings. After rolling, the thickness of the first negative electrode coating is 188 μm, and the compaction density is 1.56 g / cm³. 3 The porosity is 45%, the thickness of the second negative electrode coating is 226 μm, and the compaction density is 1.72 g / cm³. 3 The porosity is 34%, and it is then cut to obtain the negative electrode sheet; (3) Preparation of electrolyte: Ethylene carbonate, diethyl carbonate, and fluoroethylene carbonate were mixed in a volume ratio of 3:5:2 to obtain a mixed organic solvent. Lithium hexafluorophosphate with a concentration of 1 mol / L was dissolved in the mixed solvent, and then 1 wt% propane sulfonic anhydride was added. The mixture was stirred thoroughly to dissolve the lithium hexafluorophosphate and obtain the electrolyte.
[0067] (4) Preparation of secondary batteries: The positive electrode, separator (ceramic PE separator), and negative electrode are fed into a high-speed Z-type stacking machine and stacked in a Z-shaped alternating stacking manner to form a bare cell. After the bare cell is hot-pressed, it is placed in an aluminum alloy shell. The prepared electrolyte is injected into the dried bare cell. After standing, formation, aging and capacity testing, a secondary battery is obtained. In the secondary battery, the third surface of the positive electrode and the second surface of the negative electrode are arranged opposite each other.
[0068] Examples 4-5 Examples 4 and 5 provide a secondary battery, which differs from Example 1 only in that the ratio of MCMB to hard carbon in the first negative electrode coating of the negative electrode sheet is adjusted.
[0069] Examples 6-7 Examples 6 and 7 provide a secondary battery, which differs from Example 2 only in that the graphite and SiO2 content in the first negative electrode coating of the negative electrode sheet is adjusted. x The proportion of (0 < x < 2).
[0070] Examples 8-9 Examples 8 and 9 provide a secondary battery that differs from Example 1 only in that the areal density of the first and second negative electrode coatings of the negative electrode sheet is adjusted, thereby changing the coating thickness, compaction density and porosity after roll pressing.
[0071] Examples 10-11 Examples 10 and 11 provide a secondary battery, which differs from Example 1 only in that the content of conductive agent in the first negative electrode coating of the negative electrode sheet is adjusted.
[0072] Comparative Example 1 This comparative example provides a secondary battery, which differs from Example 1 only in that the coating surface density and porosity of the first and second negative electrode coatings in the negative electrode sheet are the same.
[0073] Comparative Example 2 This comparative example provides a secondary battery, which differs from Example 1 only in that the active materials of the first negative electrode coating and the second negative electrode coating in the negative electrode sheet are the same.
[0074] Comparative Example 3 This comparative example provides a secondary battery, which differs from Example 1 only in that: the areal density of the first negative electrode coating in the negative electrode sheet is greater than the areal density of the second negative electrode coating, and the porosity of the first negative electrode coating is less than the porosity of the second negative electrode coating.
[0075] The detailed design parameters of the negative electrode plates of the secondary batteries in Examples 1-11 and Comparative Examples 1-3 are shown in Table 1 below: Table 1. Detailed design parameters of the negative electrode plates of the secondary batteries in Examples 1-11 and Comparative Examples 1-3
[0076] Performance testing The secondary batteries prepared in Examples 1-11 and Comparative Examples 1-3 were subjected to performance tests, and the test items are as follows: 1) Fully charge the secondary battery to 3.65V using a constant current and constant voltage (1C), then charge it at a constant voltage until the current is ≤0.05C. After letting it stand for 30 minutes, weigh it and record the mass of the secondary battery. Discharge it to 2V using a constant current (1C), and record the discharge capacity. Calculate the energy density using the formula: Energy Density = Discharge Capacity × Nominal Value. Voltage / secondary battery weight, calculate energy density; the nominal voltage of the secondary battery in the embodiments and comparative examples of this application is 3.7V.
[0077] 2) Discharge the secondary battery to 2.5V at 1C and let it stand for 30 minutes; then charge it at a constant current of 2.5C and record the charging time from 0 to 80% state of charge (SOC). 3) In a constant temperature environment of 25℃, the secondary battery is charged at a constant current of 3C. At the end of the charging period (voltage is 3.65V), a thermocouple is used to collect the center temperature of the cell surface and calculate the difference between the temperature and the initial temperature. 4) One cycle consists of charging to 3.65V at 1C constant current and constant voltage, and discharging to 2.5V at 1C constant current. Record the discharge capacity every 50 cycles. After 3000 cycles, calculate the capacity retention rate as (3000th discharge capacity / first discharge capacity) × 100%. 5) The DC internal resistance (DCIR) was tested before and after the cycle using the DC discharge method (10% depth discharge pulse). The increase in internal resistance was calculated as (DCIR after cycle - DCIR before cycle) / DCIR before cycle × 100%. 6) Use half-cell / full-cell differential capacity testing, collect dQ / dV curves with a small current charge and discharge of 0.1C, and observe whether a lithium plating characteristic peak appears at the 0.08V position to determine the risk of lithium plating. 7) Charge the secondary battery to 3.65V at 1C, let it stand for 1 hour and record the initial voltage; store it in an open circuit in a 25℃ constant temperature chamber for 90 days and record the termination voltage. Calculate the average daily self-discharge voltage drop by (initial voltage - termination voltage) / 90. 8) After fully charging the secondary battery at 25℃ (charging to a voltage of 3.65V) and letting it stand for 1 hour, the initial discharge capacity at room temperature is measured; then the secondary battery is placed in a low-temperature environment at -20℃ and left to stand for 4 hours, and discharged at a constant current of 0.5C to a cutoff voltage of 2.5V, and the low-temperature discharge capacity is measured; the low-temperature capacity retention rate is calculated as low-temperature discharge capacity / initial discharge capacity at room temperature × 100%.
[0078] Table 2 shows the performance test results of the secondary batteries in Examples 1-11 and Comparative Examples 1-3.
[0079] Table 2 shows the performance test results of the secondary batteries in Examples 1-11 and Comparative Examples 1-3. As can be seen from Table 2, the secondary batteries in Examples 1-11 using a double-sided asymmetric negative electrode structure maintain an energy density of 163-236 Wh / kg, a 2.5C charging time to 80% SOC of 16.8-24.5 min, a temperature rise of less than 15℃ at the end of 3C charging, a capacity retention rate of over 89% after 3000 1C cycles, a DCIR increase of less than 25% after 3000 cycles, no risk of lithium plating, a capacity retention rate generally higher than 80% at -20℃, and a self-discharge of less than or equal to 2 mV / day after 90 days of storage at 25℃. In Comparative Example 1, different active materials are used for the first and second negative electrode coatings, but the surface density and porosity of the coatings on both sides are the same. Compared with Example 1... It can be seen that the charging time is longer, the temperature rise is increased by 6.4℃, the polarization is large, the heat generation is large, the safety and stability are reduced, the capacity retention rate is significantly reduced after 3000 cycles at 1C, the interface stability is worse, the stress distribution is uneven, the cycle life is shortened, the internal resistance increases significantly, there is a risk of lithium plating, the safety is reduced, the capacity retention rate at -20℃ is reduced, and the overall performance is worse. In Comparative Example 2, the same active material is used for the first and second negative electrode coatings, and the difference in areal density and porosity is ensured. It can be seen that the energy density is 164 Wh / kg, the charging time to 80% SOC at 2.5C is 27 min, the temperature rise at the end of 3C charging is 15.5℃, the capacity retention rate after 3000 cycles at 1C is 88%, the DCIR increase is 28%, there is a risk of lithium plating, the capacity retention rate at -20℃ is 79%, and the self-discharge at 25℃ for 90 days is 2.0 mV / day. The overall performance is worse than that of Example 1. In Comparative Example 3, the areal density of the first negative electrode coating is greater than that of the second negative electrode coating, and the porosity of the first negative electrode coating is less than that of the second negative electrode coating. It can be seen that the energy density is 167 Wh / kg, the time to charge to 80% SOC at 2.5C is 32 min, the temperature rise at the end of 3C charging is 18.0℃, the capacity retention rate after 3000 cycles at 1C is 80%, the DCIR increase is 45%, there is a risk of lithium plating, the capacity retention rate at -20℃ is 74%, and the self-discharge rate after 90 days of storage at 25℃ is 2.3 mV / day, showing a significant deterioration in the performance of the secondary battery.
[0080] Therefore, it can be seen that by adopting the solution of this application, the secondary battery can maintain high energy density while significantly shortening the fast charging time, reducing the charging temperature rise, significantly improving cycle life and room temperature storage stability, reducing the increase in DC internal resistance, and achieving better performance in low-temperature discharge and long-term storage.
[0081] Finally, it should be noted that the above embodiments are used to illustrate the technical solutions of this application and not to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.
Claims
1. A secondary battery, characterized in that, Including the negative electrode sheet; The negative electrode sheet includes: The negative electrode current collector has a first surface and a second surface opposite to the first surface; A first negative electrode coating is disposed on the first surface of the negative electrode current collector and contains a first negative electrode active material; The second negative electrode coating is disposed on the second surface of the negative electrode current collector and contains a second negative electrode active material; The first negative electrode active material includes mesophase carbon microspheres, hard carbon, graphite, and SiO2. x At least two of the following (0 < x < 2); the second negative electrode active material includes graphite; The porosity of the first negative electrode coating is greater than that of the second negative electrode coating; The areal density of the first negative electrode coating is less than that of the second negative electrode coating.
2. The secondary battery according to claim 1, characterized in that, The first negative electrode active material comprises a mixture of mesophase carbon microspheres and hard carbon, wherein the mesophase carbon microspheres account for 90%-96% of the total mass of the first negative electrode active material.
3. The secondary battery according to claim 1, characterized in that, The first negative electrode active material includes graphite and SiO2. x A mixture of (0 < x < 2), the SiO x (0 < x < 2) accounts for 4%-20% of the total mass of the first negative electrode active material.
4. The secondary battery according to claim 1, characterized in that, The porosity of the first negative electrode coating is ≥42%, and the porosity of the second negative electrode coating is ≤36%.
5. The secondary battery according to claim 4, characterized in that, The porosity of the first negative electrode coating is 42%-48%; the porosity of the second negative electrode coating is 30%-36%.
6. The secondary battery according to claim 1, characterized in that, The areal density of the first negative electrode coating is 215 mg / 1540.25 mm². 2 -246mg / 1540.25mm 2 The areal density of the second negative electrode coating is 275 mg / 1540.25 mm². 2 -345mg / 1540.25mm 2 .
7. The secondary battery according to claim 1, characterized in that, The first negative electrode coating further comprises a first conductive agent, and the second negative electrode coating further comprises a second conductive agent; the mass content of the first conductive agent in the first negative electrode coating is less than or equal to the mass content of the second conductive agent in the second negative electrode coating.
8. The secondary battery according to claim 7, characterized in that, The first conductive agent comprises a mixture of carbon nanotubes and conductive carbon black, wherein the mass ratio of the carbon nanotubes to the conductive carbon black is 1-1.5:1; the second conductive agent comprises conductive carbon black.
9. The secondary battery according to claim 7, characterized in that, The first conductive agent has a mass percentage of ≤2.5% in the first negative electrode coating; the second conductive agent has a mass percentage of ≥2.5% in the second negative electrode coating.
10. The secondary battery according to claim 9, characterized in that, The first conductive agent accounts for 1.5%-2.5% of the mass of the first negative electrode coating; the second conductive agent accounts for 2.5%-3.0% of the mass of the second negative electrode coating.
11. The secondary battery according to claim 1, characterized in that, The secondary battery further includes a positive electrode, which comprises: The positive current collector has a third surface and a fourth surface opposite to the third surface; A first positive electrode coating is disposed on the third surface of the positive electrode current collector and contains a first positive electrode active material; A second positive electrode coating is disposed on the fourth surface of the positive electrode current collector and contains a second positive electrode active material; The first positive electrode active material includes a lithium transition metal oxide or a lithium transition metal oxide with at least an oxide or carbon material disposed on its surface, and the second positive electrode active material includes a lithium transition metal oxide.
12. The secondary battery according to claim 11, characterized in that, The first positive electrode coating further comprises a third conductive agent, and the second positive electrode coating further comprises a fourth conductive agent; the mass content of the third conductive agent in the first positive electrode coating is less than the mass content of the fourth conductive agent in the second positive electrode coating.
13. The secondary battery according to claim 12, characterized in that, The third conductive agent comprises poly(3,4-ethylenedioxythiophene):polystyrene sulfonate; the fourth conductive agent comprises conductive carbon black.
14. An electrical appliance, characterized in that, The device includes the secondary battery as described in any one of claims 1-13, wherein the secondary battery serves as the power supply for the electrical equipment.