Battery cell, battery device, and electric device
By optimizing the compaction density of the positive electrode, introducing silicon materials, and using electrolytes with chain-like carboxylic acid ester solvents, the contradiction between energy density and fast charging performance in lithium-ion batteries has been resolved, achieving a balance between high energy density and fast charging performance.
Patent Information
- Application Number
- CN202510652476.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-20
- Publication Date
- 2026-11-20
AI Technical Summary
In the process of increasing the energy density of existing lithium-ion batteries, the lithium-ion transport path becomes longer, which affects fast charging performance and makes it difficult to balance high energy density and fast charging performance.
By controlling the compaction density of the positive electrode sheet to 2.62 g/cm³-2.8 g/cm³, introducing a silicon-based negative electrode sheet, and using an electrolyte with a chain-like carboxylic acid ester solvent, the negative electrode film structure and electrolyte composition are optimized, thereby improving lithium-ion kinetics.
This technology enables lithium-ion batteries to maintain high energy density while exhibiting excellent fast-charging performance and good cycle stability.
Smart Images

Figure CN123143530A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of batteries, and more specifically, to a battery cell, a battery device, and an electrical appliance. Background Technology
[0002] In recent years, secondary batteries, mainly lithium-ion batteries, have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power plants, as well as in many fields such as power tools, electric bicycles, electric motorcycles, electric cars, military equipment, and aerospace, thus achieving great development.
[0003] Improving battery energy density has always been a key focus of battery research. Increasing energy density means more coating on the positive and negative electrodes, thicker electrode sheets, and longer lithium-ion transport paths, which affects lithium-ion kinetics and negatively impacts fast-charging performance. Therefore, there is a trade-off between battery energy density and fast-charging performance; both cannot be simultaneously achieved. How to enable batteries to possess both high energy density and excellent fast-charging performance is a pressing technical problem that needs to be solved. Summary of the Invention
[0004] This application is made in view of the above-mentioned technical problems, and its purpose is to provide a battery cell, a battery device and an electrical device, wherein the battery cell can achieve both high energy density and excellent fast charging performance.
[0005] In a first aspect, a battery cell is provided, the battery cell comprising: a positive electrode, a negative electrode, and an electrolyte; wherein the compaction density of the positive electrode is 2.62 g / cm³. 3 -2.8g / cm 3 The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one side surface of the negative current collector, the negative electrode film layer including silicon material; the electrolyte includes a chain-like carboxylic acid ester solvent.
[0006] In the secondary battery cell of this application, the compaction density of the positive electrode sheet is set at 2.62 g / cm³. 3 -2.8g / cm 3 Within a certain range, the positive electrode sheet achieves a higher compaction density, thereby increasing its energy density. Introducing silicon material into the negative electrode increases its energy density while reducing its thickness, thus shortening the lithium-ion diffusion path and improving lithium-ion kinetics. Simultaneously, selecting an electrolyte containing chain-like carboxylic acid ester solvents enhances the wettability of the electrolyte to the high-compact-density positive electrode sheet and the silicon-containing negative electrode sheet, further improving lithium-ion kinetics. Therefore, the battery cell of this application can achieve both increased energy density and good lithium-ion kinetics, balancing high energy density and excellent fast-charging performance.
[0007] In one possible implementation, the mass fraction of the chain carboxylic acid ester solvent is 8 wt% to 60 wt% based on the total mass of the electrolyte.
[0008] In one possible implementation, the chain-like carboxylic acid ester solvent includes at least one of methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl acrylate, and ethyl acrylate.
[0009] In one possible implementation, the mass fraction of silicon in the silicon material is 0.2 wt% to 2.2 wt% based on the total mass of the negative electrode film.
[0010] In one possible implementation, the negative electrode film layer includes a first negative electrode active material layer, a second negative electrode active material layer, and a third negative electrode active material layer. The first negative electrode active material layer is disposed on at least a portion of the surface of the negative electrode current collector, the second negative electrode active material layer is disposed on at least a portion of the surface of the first negative electrode active material layer, and the third negative electrode active material layer is disposed on the side of the second negative electrode active material layer away from the negative electrode current collector. The first negative electrode active material layer includes the silicon material, the second negative electrode active material layer includes a first graphite material, and the third negative electrode active material layer includes a second graphite material.
[0011] In one possible implementation, the thickness of the first negative electrode active material layer is 0.5 μm-3 μm.
[0012] In one possible implementation, the volume average particle size of the silicon material is 0.5 μm to 3 μm.
[0013] In one possible implementation, the silicon material includes at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy.
[0014] In one possible implementation, the first negative electrode active material layer includes a conductive agent, which includes at least one of conductive carbon black and carbon nanotubes; the mass fraction of the conductive agent is 15wt%-55wt% based on the total mass of the negative electrode film layer.
[0015] In one possible implementation, the first negative electrode active material layer includes a binder, the binder including at least one of polyacrylic acid and styrene-butadiene rubber; the mass fraction of the binder is 30wt%-40wt% based on the total mass of the negative electrode film layer.
[0016] In one possible implementation, the graphitization degree of the second graphite material is greater than that of the first graphite material.
[0017] In one possible implementation, the graphitization degree of the first graphite material is 93.2%-96%, and the graphitization degree of the second graphite material is 92%-93.2%.
[0018] In one possible implementation, the OI value of the first graphite material is less than the OI value of the second graphite material.
[0019] In one possible implementation, the OI value of the first graphite material is 3.80-3.85, and the OI value of the second graphite material is 3.85-4.0.
[0020] In one possible implementation, the second graphite material satisfies at least one of the following conditions (1)-(5): (1) the span value of the second graphite material is 0.9-1.25; (2) the volume average particle size Dv10 of the second graphite material is 4μm-10μm, optionally 5.5μm-7.5μm; (3) the volume average particle size Dv50 of the second graphite material is 11μm-18μm, optionally 12.5μm-15μm; (4) the volume average particle size Dv90 of the second graphite material is 17μm-25μm, optionally 21μm-25μm; (5) the specific surface area of the second graphite material is 1.00m². 2 / g-1.90m 2 / g, can be selected as 1.00m 2 / g-1.20m 2 / g.
[0021] In one possible implementation, the negative electrode sheet satisfies at least one of the following conditions (1)-(3): (1) when the negative electrode film layer is provided on both sides of the negative electrode current collector, the thickness of the negative electrode sheet is 91μm-135μm, optionally 97μm-123μm; (2) the areal density of the negative electrode sheet on one side is 6.5mg / cm³. 2 -11.0 mg / cm 2 The option is 6.8 mg / cm³. 2 -9.35mg / cm 2 (3) The compaction density of the negative electrode sheet is 1.48 g / cm³. 3 -1.7g / cm 3 The option is 1.52 g / cm³. 3 -1.65g / cm 3 .
[0022] In one possible implementation, the positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the surface of the positive current collector, the positive electrode film layer including a positive electrode active material, the positive electrode active material including lithium transition metal phosphate.
[0023] In one possible implementation, the lithium transition metal phosphate includes at least one of lithium iron phosphate and lithium manganese phosphate.
[0024] In one possible implementation, the lithium transition metal phosphate comprises a component having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes at least one of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.1.
[0025] In one possible implementation, the lithium transition metal phosphate has a carbon coating layer comprising amorphous carbon.
[0026] In one possible implementation, in a cross-section of the positive electrode film along its thickness direction, the area percentage of particles with a diameter greater than or equal to 1.5 μm is greater than or equal to 8.0% and less than or equal to 20.0%.
[0027] In one possible implementation, the area ratio of particles with a diameter greater than or equal to 5 μm in the cross-section of the positive electrode film along its thickness direction is 0.
[0028] In one possible implementation, the area percentage of particles with a diameter greater than or equal to 1.5 μm and less than 5 μm in the cross-section of the positive electrode film along its thickness direction is 9.0%-20.0%, optionally 10.0%-20.0%.
[0029] In one possible implementation, the area percentage of particles with a diameter greater than or equal to 1 μm and less than 1.5 μm in the cross-section of the positive electrode film along its thickness direction is 15.0%-25.0%, optionally 16.0%-24.0%.
[0030] In one possible implementation, the organic solvent includes a carbonate solvent, which includes at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, dimethyl carbonate, and diethyl carbonate.
[0031] In one possible implementation, the mass fraction of the carbonate solvent is 20 wt% to 80 wt% based on the total mass of the electrolyte.
[0032] In one possible implementation, the electrolyte includes additives, which include at least one of carbonate additives, sulfur-containing additives, and lithium salt additives; wherein the carbonate additives include at least one of vinylene carbonate and fluoroethylene carbonate; the sulfur-containing additives include at least one of vinyl sulfate, vinyl disulfate, butenyl sulfite, 1,3-propanesulfonyl lactone, vinyl sulfite, and methylene disulfonate; and the lithium salt additives include at least one of lithium difluorophosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, and lithium dioxalate borate.
[0033] In one possible implementation, the mass fraction of the additive is 1 wt% to 10 wt% based on the total mass of the electrolyte.
[0034] In one possible implementation, the electrolyte comprises a lithium salt, which includes at least one of a fluorosulfonate imine salt and lithium hexafluorophosphate; the fluorosulfonate imine salt includes at least one of lithium difluorosulfonate imine and lithium bistrifluoromethanesulfonate imide.
[0035] In one possible implementation, the electrolyte has an ionic conductivity of 15 mS / cm to 20 mS / cm.
[0036] In a second aspect, a battery device is provided, the battery device comprising a battery cell in any possible implementation of the first aspect.
[0037] Thirdly, an electrical device is provided, the electrical device comprising a battery cell in any possible implementation of the first aspect, or a battery device in the second aspect. Attached Figure Description
[0038] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0039] Figure 1 This is a schematic diagram of a negative electrode.
[0040] Figure 2 This is a schematic diagram of a battery device.
[0041] Figure 3 This is a schematic diagram of an electrical device. Detailed Implementation
[0042] The embodiments of this application are hereby disclosed in detail with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0043] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0044] In the description of this application, it should be noted that, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," "outer," etc., indicating orientation or positional relationships are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation on this application. Furthermore, the terms "first," "second," "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0045] Unless otherwise specified, in this application, the phrase "A and / or B" means "A, B, or both A and B". More specifically, the condition "A and / or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0046] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0047] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0048] Unless otherwise specified, any undefined terms shall have their technically accepted meanings.
[0049] The embodiments of this application will be described next.
[0050] In recent years, rechargeable batteries have seen significant development due to their high energy density and long lifespan, finding widespread application in power tools, electronic products, electric vehicles, aerospace, and other fields. Typically, a rechargeable battery cell consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the charging and discharging process, active ions repeatedly insert and extract between the positive and negative electrodes. The electrolyte acts as a conductor of these active ions between the electrodes. The separator, positioned between the positive and negative electrodes, prevents short circuits while allowing active ions to pass through, ensuring the normal electrochemical reactions within the battery cell.
[0051] Taking lithium-ion batteries as an example, a lithium-ion battery is a secondary battery that uses lithium ions as the active lithium ions. With the rapid development of new energy vehicles in China, lithium-ion batteries, as the power source for automobiles, have placed higher demands on their energy density. Under the existing material system, increasing the loading of active material on the electrode is one of the main means to improve the energy density of lithium-ion batteries. Increasing the loading of active material on the electrode generally leads to an increase in electrode thickness, which lengthens the migration path of lithium ions, affects lithium-ion kinetics, and thus affects the fast-charging performance of lithium-ion batteries. Therefore, high energy density and fast-charging performance of lithium-ion batteries are usually mutually exclusive.
[0052] In view of this, embodiments of this application provide a battery cell, a battery device, and an electrical appliance, wherein the high-energy-density battery cell can balance energy density and fast-charging performance.
[0053] Next, the battery cell provided in this application will be introduced.
[0054] [Battery cell]
[0055] Firstly, a battery cell is provided, comprising: a positive electrode, a negative electrode, and an electrolyte; wherein the compaction density of the positive electrode is 2.62 g / cm³. 3 -2.8g / cm 3 The negative electrode includes a negative current collector and a negative electrode film layer disposed on at least one side of the negative current collector, the negative electrode film layer including silicon material; the electrolyte includes a chain-like carboxylic acid ester solvent.
[0056] In this article, "the compaction density of the electrode" refers to the actual density of the electrode, which can be expressed as the mass of the material excluding the current collector in a unit volume of the electrode.
[0057] The compaction density of the positive electrode sheet can be, for example, 2.62 g / cm³. 3 2.63 g / cm 3 2.64 g / cm 3 2.65g / cm 3 2.66 g / cm 3 2.67 g / cm 3 2.68g / cm 3 2.69 g / cm 3 2.7g / cm 3 2.71 g / cm 3 2.72 g / cm 3 2.73 g / cm 3 2.74 g / cm 3 2.75g / cm 3 2.76 g / cm 3 2.77 g / cm 3 2.78g / cm 3 2.79 g / cm 3 2.8g / cm 3 , or its value is within the range obtained by combining any two of the above values.
[0058] A higher compaction density of the positive electrode sheet is more conducive to improving the energy density of the battery cell. However, it also increases the difficulty of the electrolyte wetting the positive electrode sheet, affecting lithium-ion kinetics and hindering the fast-charging performance of the battery cell. Therefore, by controlling the compaction density of the positive electrode sheet within the aforementioned range, the battery cell can maintain good wettability while achieving sufficient energy density, thus balancing energy density and fast-charging performance.
[0059] It should be understood that the compaction density of a single battery cell may differ under different conditions. The compaction density of the positive electrode sheet mentioned in this application refers to the compaction density of the single battery cell at 0% SOC. In other words, the compaction density of the positive electrode sheet is the compaction density of the single battery cell when it is discharged to 0% SOC (also known as full discharge).
[0060] Introducing silicon into the negative electrode can increase its energy density without increasing its thickness. This is because silicon has a higher specific capacity, achieving a suitable compaction density of 2.62 g / cm³. 3 -2.8g / cm 3 When using silicon as the positive electrode, compared to carbon materials, silicon materials require less coating to achieve the same energy density. Therefore, by introducing silicon material into the negative electrode, a compaction density of 2.62 g / cm³ can be achieved. 3 -2.8g / cm 3 The positive electrode plate increases the energy density of the negative electrode plate while reducing its thickness, thereby shortening the lithium-ion diffusion path and improving lithium-ion kinetics.
[0061] In this article, "carboxylic acid ester solvents" refers to organic solvents containing -COO- groups, which have low viscosity and high ionic conductivity.
[0062] Compared to carbon materials, silicon materials have poorer kinetic properties. (The text abruptly shifts to a seemingly unrelated topic: "When the compaction density is matched to 2.62 g / cm³...") 3 -2.8g / cm 3 When the positive electrode sheet is compacted, the negative electrode sheet may also have a large compaction density, which makes it more difficult for the electrolyte to wet the electrode sheet, affecting lithium ion dynamics and thus affecting the fast charging performance of the battery cell.
[0063] By selecting carboxylic acid ester solvents as at least part of the electrolyte solvent, which have high ionic conductivity and low viscosity, the wetting ability of the electrolyte to the electrode and the ionic conductivity of the electrolyte can be improved, thereby reducing the influence of silicon materials on lithium-ion dynamics in the battery cell and further improving the fast-charging performance of the battery cell.
[0064] Therefore, in this embodiment, through the design of the positive electrode, negative electrode, and electrolyte, the battery cell can have both high energy density and good lithium-ion dynamics, thus achieving a balance between energy density and fast charging performance.
[0065] In one example, the type and mass content of carboxylic acid esters or additives in the electrolyte can be determined by gas chromatography, gas chromatography-mass spectrometry (GC-MS), ion chromatography (IC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), or inductively coupled plasma optical emission spectrometry (ICP-OES). As an example, the battery cell is discharged at a constant current of 0.33C to 2.5V at 25°C, then the battery cell is disassembled, and the free electrolyte is extracted (if the amount of electrolyte in the battery cell is small, the electrolyte can be obtained by centrifuging the disassembled positive and negative electrode plates). Next, 500 μl of deuterated reagent was added to the NMR tube in an argon-filled glove box. 100 μl of the electrolyte sample was then added to the NMR tube, and the tube was shaken to dissolve the non-aqueous electrolyte in the deuterated reagent. The composition and mass of carboxylic acid esters in the electrolyte were then determined using an Oxford Instruments X-Pulse benchtop NMR spectrometer. The mass content of carboxylic acid esters in the electrolyte was calculated as the mass of carboxylic acid esters / additives divided by the total mass of the electrolyte.
[0066] In some embodiments, the mass fraction of the chain carboxylic acid ester solvent is 6 wt% to 80 wt% based on the total mass of the organic solvent.
[0067] For example, the mass fraction of the chain carboxylic acid ester solvent can be 6 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, 16 wt%, 18 wt%, 20 wt%, 22 wt%, 24 wt%, 26 wt%, 28 wt%, 30 wt%, 32 wt%, 34 wt%, 36 wt%, 38 wt%, 40 wt%, 42 wt%, 44 wt%, 46 wt%, 48 wt%, 50 wt%, 52 wt%, 54 wt%, 56 wt%, 58 wt%, 60 wt%, 62 wt%, 64 wt%, 66 wt%, 68 wt%, 70 wt%, 72 wt%, 74 wt%, 76 wt%, 78 wt%, 80 wt%, or a value within the range obtained by any combination of the above two values.
[0068] A higher mass fraction of carboxylic acid ester solvents in organic solvents results in lower electrolyte viscosity and higher ionic conductivity. However, carboxylic acid ester solvents are prone to side reactions and gas generation during the cyclic storage of battery cells, which can negatively impact the cycle performance of the battery cells. Therefore, this embodiment controls the mass content of carboxylic acid ester solvents within the aforementioned range, thereby reducing electrolyte viscosity, improving electrolyte ionic conductivity, and mitigating the risk of gas generation from carboxylic acid ester solvents. This achieves both improved fast-charging performance and optimal cycle performance of the battery cells.
[0069] In some embodiments, the chain carboxylic acid ester solvent includes at least one of methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl acrylate, and ethyl acrylate.
[0070] In some embodiments, the mass fraction of silicon in the silicon material is 0.2 wt% to 2.2 wt% based on the total mass of the negative electrode film.
[0071] For example, the mass fraction of silicon can be 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2.0wt%, 2.1wt%, or 2.2wt%, or a value within the range obtained by any combination of the above two values.
[0072] A higher silicon mass fraction is more beneficial to the energy density of a single battery cell. However, silicon materials exhibit significant volume expansion and contraction during battery cell cycling. During expansion, the material absorbs electrolyte; during contraction, it squeezes out electrolyte. If this squeezed-out electrolyte cannot be absorbed back in time during expansion, it will result in insufficient wettability of the negative electrode, affecting lithium-ion kinetics and consequently hindering the fast-charging performance of the battery cell. The degree of expansion and contraction of the negative electrode is directly related to the mass fraction of silicon in the negative electrode film. The higher the mass fraction of silicon, the more severe the expansion and contraction of the negative electrode film.
[0073] Therefore, when using an electrolyte containing carboxylic acid ester solvents, this embodiment, by controlling the mass fraction of silicon material within a suitable range, enables the electrolyte to be promptly reabsorbed during the expansion of the negative electrode, thereby improving the wettability of the electrolyte on the negative electrode during cycling. Thus, by controlling the mass fraction of silicon material in the negative electrode film within the aforementioned range, it is possible to improve the energy density of the battery cell while simultaneously achieving excellent fast-charging performance.
[0074] Figure 1 A detailed schematic diagram of a negative electrode sheet according to this application is shown.
[0075] like Figure 1As shown, in some embodiments, the negative electrode film layer 10 includes a first negative electrode active material layer 101, a second negative electrode active material layer 102, and a third negative electrode active material layer 103. The first negative electrode active material layer 101 is disposed on at least a portion of the surface of the negative electrode current collector 11, the second negative electrode active material layer 102 is disposed on at least a portion of the surface of the first negative electrode active material layer 101, and the third negative electrode active material layer 103 is disposed on the side of the second negative electrode active material layer 102 away from the negative electrode current collector 11. The first negative electrode active material layer 101 includes silicon material, the second negative electrode active material layer 102 includes a first graphite material, and the third negative electrode active material layer 103 includes a second graphite material.
[0076] During the charging process of a battery cell, lithium ions are extracted from the positive electrode active material and inserted into the negative electrode active material. Both graphite and silicon materials undergo volume expansion due to lithium ion insertion. Silicon, during expansion, easily generates localized stress on surrounding materials. If mixed with graphite, this can lead to graphite particle breakage and subsequent delamination of the negative electrode film. Graphite also restricts silicon expansion, increasing internal stress within silicon particles and causing particle splitting. In other words, graphite and silicon exhibit an expansion crosstalk effect. While mixing them as a negative electrode active material may increase the energy density of the battery cell, the continuous breakage and splitting of both materials during cycling due to the expansion crosstalk effect creates new interfaces that constantly consume active lithium ions, causing a rapid decrease in battery cell capacity and hindering long-term fast-charging cycles.
[0077] In this embodiment, the negative electrode film layer 10 has a three-layer structure design. A silicon-containing undercoat is disposed in the "lower layer" closest to the current collector, and two types of graphite materials are disposed in the "middle layer" and "upper layer" of the negative electrode film layer 10, respectively. By separately disposing of silicon and graphite materials, the expansion crosstalk effect of silicon and graphite materials during lithium intercalation can be effectively improved. Furthermore, by placing the silicon material at the bottom layer of the negative electrode film layer 10, the volume expansion of the silicon material can be limited by the graphite material, which is beneficial to the structural stability of the negative electrode sheet. As a result, the battery cell can have good fast-charging cycle performance.
[0078] In some embodiments, the thickness of the first negative electrode active material layer 101 is 0.5 μm-3 μm.
[0079] The thickness of the first negative electrode active material layer 101 can be, for example, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, 2.0μm, 2.1μm, 2.2μm, 2.3μm, 2.4μm, 2.5μm, 2.6μm, 2.7μm, 2.8μm, 2.9μm, or 3.0μm, or a value within the range obtained by any combination of the above two values.
[0080] Silicon materials with a mass fraction between 0.2 wt% and 2.2 wt% can help reduce the thickness of the first negative electrode active material layer 101 to between 0.5 μm and 3 μm, thereby reducing the thickness of the negative electrode film layer 10. The smaller the thickness of the negative electrode film layer 10, the shorter the lithium-ion diffusion path, which is more conducive to improving lithium-ion kinetics and thus enhancing the fast-charging performance of the battery cell. Therefore, controlling the thickness of the first negative electrode active material layer 101 within the above-mentioned range helps to improve the fast-charging performance of the battery cell.
[0081] In some embodiments, the volume average particle size Dv50 of the silicon material is 0.5 μm-3 μm.
[0082] In this article, "volume average particle size Dv50" refers to the particle size at which the cumulative particle size distribution percentage reaches 50% from the smallest particle size side in the particle size distribution map of the sample. Its physical meaning is: particles larger than this value account for 50% of the total number of particles in the sample, and particles smaller than or equal to this value account for 50% of the total number of particles. Dv50 is also known as the median particle size and is commonly used to represent the average particle size of a sample.
[0083] For example, the particle size of silicon material can be 1μm, 1.2μm, 1.4μm, 1.6μm, 1.8μm, 2μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, 3μm, or a value within the range obtained by any combination of the above two values.
[0084] Silicon materials with particle sizes within the aforementioned range contribute to their uniform distribution within the first negative electrode active material layer 101.
[0085] In some embodiments, the silicon material includes at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy.
[0086] In some embodiments, the silicon material is a silicon-carbon composite, which includes a porous silicon-carbon material. By selecting a silicon-carbon composite as the silicon material, it is helpful to improve the electronic conductivity of the first negative electrode active material layer 101.
[0087] In some embodiments, the first negative electrode active material layer 101 includes a conductive agent, which includes at least one of conductive carbon black and carbon nanotubes; preferably, carbon nanotubes. The mass fraction of the conductive agent is 15 wt%-55 wt% based on the total mass of the negative electrode film layer 10.
[0088] Compared to graphite, silicon has poor electrical conductivity. Adding a conductive agent to the first negative electrode active material layer 101 can effectively improve its electronic conductivity. By controlling the mass fraction of the conductive agent in the negative electrode film layer 10 within the aforementioned range, the negative electrode can achieve both good conductivity and high energy density. When carbon nanotubes are chosen as the conductive agent, their high tensile strength also helps suppress the volume expansion of silicon, thus improving the fast-charging cycle performance of the battery cell.
[0089] In some embodiments, the first negative electrode active material layer 101 includes a binder, which includes at least one of polyacrylic acid and styrene-butadiene rubber; preferably polyacrylic acid. The binder has a mass fraction of 30 wt%-40 wt% based on the total mass of the negative electrode film layer 10.
[0090] When polyacrylic acid is selected as a binder, the carboxyl groups in polyacrylic acid and the hydroxyl groups on the surface of silicon materials can form strong hydrogen bonds, which helps to suppress the volume expansion of silicon materials and help improve the fast charging cycle performance of battery cells.
[0091] In some embodiments, the degree of graphitization of the second graphite material is less than that of the first graphite material.
[0092] In this article, "degree of graphitization" refers to a numerical value that measures the extent to which carbon atoms form a close-packed hexagonal graphite crystal structure. The closer the lattice size of a carbon material is to the lattice constant of ideal graphite, the higher the degree of graphitization. In some examples, the degree of graphitization can be determined by X-ray diffraction, i.e., by first measuring the interlayer spacing d(002) of the graphite (002) crystal planes, and then substituting it into the Mering–Maire formula (also known as the Franklin formula) for calculation.
[0093] The higher graphitization degree of the first graphite material compared to the second means that the first graphite material has fewer surface oxides, defects, and impurities, which is beneficial for lithium-ion diffusion and intercalation with fewer side reactions. The second graphite material has more exposed active sites, exhibiting higher lithium-ion kinetics, enabling the surface of the third anode active material layer 103 to intercalate a large number of lithium ions in a short time. Simultaneously, the lower graphitization degree of the second graphite material compared to the first also means a larger interlayer spacing, resulting in less rebound during cycling and helping to reduce the rebound of the anode electrode.
[0094] Therefore, in this embodiment, by setting a second graphite material with higher lithium-ion kinetics on the upper layer of the negative electrode film layer 10, the surface of the negative electrode sheet can be equipped with the ability to embed a large number of lithium ions in a short time, further improving the fast-charging performance of the battery cell. Furthermore, the second graphite material also helps to reduce the rebound of the negative electrode sheet, improving the cycle stability of the battery cell. By setting a first graphite material with higher graphitization in the middle layer of the negative electrode film layer 10, side reactions during battery cell cycling can be reduced, thereby reducing lithium consumption during cycling and improving the fast-charging cycle performance of the battery cell. In addition, during the charging process of the battery cell, lithium ions continuously embed and diffuse from the surface of the negative electrode sheet into the interior of the negative electrode sheet; in other words, lithium ions diffuse from the side of the negative electrode film layer 10 away from the current collector to the side closer to the current collector. In this embodiment, the lithium-ion diffusion capability of the negative electrode film layer 10 is distributed in a stepped manner from the upper to the lower layers, gradually weakening, which is consistent with the embedding and diffusion direction of lithium ions during charging. Therefore, lithium-ion kinetics can be further improved, thereby further enhancing the fast-charging performance of the battery cell.
[0095] In some embodiments, the graphitization degree of the first graphite material is 93.2%-96%, and the graphitization degree of the second graphite material is 92%-93.2%.
[0096] For example, the degree of graphitization of the first graphite material can be 93.2%, 93.4%, 93.6%, 93.8%, 94%, 94.2%, 94.4%, 94.6%, 94.8%, 95%, or 96%, or a value within the range obtained by any combination of the above two values. The degree of graphitization of the second graphite material can be 92%, 92.2%, 92.4%, 92.6%, 92.8%, 93%, 93.1%, or 93.19%, or a value within the range obtained by any combination of the above two values.
[0097] The first graphite material with a graphitization degree within the aforementioned range exhibits high graphitization and fewer surface oxides, defects, and impurities, which is beneficial for lithium-ion diffusion and intercalation with fewer side reactions. The second graphite material with a graphitization degree within the aforementioned range exhibits high lithium-ion kinetics and a larger interlayer spacing, which can reduce the rebound of the negative electrode during cycling. Therefore, by controlling the graphitization degree of the first and second graphite materials within appropriate ranges, the lithium-ion kinetics of the negative electrode can be improved, the lithium consumption of the battery cell during cycling can be reduced, the rebound of the negative electrode during cycling can be decreased, and the fast-charging cycle performance of the battery cell can be further improved.
[0098] In some embodiments, the OI value of the first graphite material is less than the OI value of the second graphite material.
[0099] In this paper, "orientation degree" refers to the orientation degree of the internal crystal structure of graphite materials, usually expressed by the OI value. The higher the OI value, the more ordered the crystal arrangement inside the graphite is; the lower the OI value, the more disordered the crystal arrangement inside the graphite is. The OI value can be specifically expressed as the ratio of the diffraction peak intensity of the (002) or (004) crystal plane of graphite to the diffraction peak intensity of the (110) crystal plane.
[0100] A lower OI value indicates a more disordered crystal arrangement and more grain boundaries within the graphite material. This allows for the exposure of more active sites during electrochemical reactions, resulting in superior lithium-ion kinetics. Consequently, the battery cell can be charged at high current or high rate in a short time, exhibiting better fast-charging performance. Therefore, in this embodiment, by placing a second graphite material with a higher OI value in the third negative electrode active material layer 103, the negative electrode surface can be equipped with the ability to embed a large number of lithium ions in a short time, thereby further improving the fast-charging performance of the battery cell.
[0101] In some embodiments, the OI value of the first graphite material is 3.80-3.85, and the OI value of the second graphite material is 3.85-4.0.
[0102] For example, the OI value of the first graphite material can be 3.80, 3.81, 3.82, 3.83, 3.84, or 3.85, or a value within the range obtained by any combination of the above two values. The OI value of the second graphite material can be 3.851, 3.86, 3.87, 3.88, 3.89, or 4.0, or a value within the range obtained by any combination of the above two values.
[0103] In some embodiments, the second graphite material satisfies at least one of the following conditions (1)-(5):
[0104] (1) The span value of the second graphite material is 0.9-1.25.
[0105] (2) The volume average particle size Dv10 of the second graphite material is 4μm-10μm, and can be selected as 5.5μm-7.5μm.
[0106] (3) The volume average particle size Dv50 of the second graphite material is 11μm-18μm, and can be selected as 12.5μm-15μm.
[0107] (4) The volume average particle size Dv90 of the second graphite material is 17μm-25μm, and can be selected as 21μm-25μm.
[0108] (5) The specific surface area of the second graphite material is 1.00 m². 2 / g-1.90m2 / g, can be selected as 1.00m 2 / g-1.20m 2 / g.
[0109] In this paper, the "span value" refers to the particle size span of the material, which can be calculated using the formula span = (Dv90 - Dv10) / Dv50. Here, Dv10, Dv50, and Dv90 are the corresponding volume average particle size values in the material's particle size distribution diagram.
[0110] In this paper, "volume average particle size Dv10" refers to the particle size at which the cumulative particle size distribution percentage reaches 10% from the smallest particle size side in the particle size distribution map of the sample. Its physical meaning is that particles larger than this value account for 90% of the total number of particles in the sample, and particles smaller than or equal to this value account for 10% of the total number of particles.
[0111] In this paper, "volume average particle size Dv90" refers to the particle size at which the cumulative particle size distribution percentage reaches 90% from the smallest particle size side in the particle size distribution map of the sample. Its physical meaning is that particles larger than this value account for 10% of the total number of particles in the sample, and particles smaller than or equal to this value account for 90% of the total number of particles.
[0112] In this article, "specific surface area" refers to the total surface area per unit mass of material. It can be obtained by testing with a specific surface area porosity analyzer.
[0113] The span value of the second graphite material can be, for example, 0.9, 1, 1.05, 1.1, 1.15, 1.2, or 1.25, or a value within the range obtained by any combination of the above two values. The volume average particle size Dv10 of the second graphite material can be, for example, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, or 10 μm, or a value within the range obtained by any combination of the above two values. The volume average particle size Dv50 of the second graphite material can be, for example, 11 μm, 11.5 μm, 12 μm, 12.5 μm, 13 μm, 13.5 μm, 14 μm, 14.5 μm, or 15 μm, or a value within the range obtained by any combination of the above two values. The volume average particle size (Dv90) of the second graphite material can be, for example, 17 μm, 17.5 μm, 18 μm, 18.5 μm, 19 μm, 19.5 μm, 20 μm, 20.5 μm, 21 μm, 21.5 μm, 22 μm, 22.5 μm, 23 μm, 23.5 μm, 24 μm, 24.5 μm, or 25 μm, or a value within the range obtained by any combination of the above two values. The specific surface area of the second graphite material can be, for example, 1.00 m². 2 / g, 1.10m 2 / g, 1.20m 2 / g, 1.30m 2 / g, 1.40m 2 / g, 1.50m 2 / g, 1.60m 2 / g, 1.70m 2 / g, 1.80m 2 / g, 1.90m 2 / g, or its value is within the range obtained by combining any two of the above values.
[0114] The particles of the second graphite material that meet at least one of the above conditions can form a suitable pore structure, which is beneficial for the electrolyte to wet the negative electrode film 10, improve the lithium ion and electron transport performance in the negative electrode film 10, and thus improve lithium ion kinetics.
[0115] In some embodiments, the negative electrode sheet satisfies at least one of the following conditions (1)-(3):
[0116] (1) When negative electrode film layers 10 are provided on both sides of negative electrode current collector 11, the thickness of negative electrode sheet is 91μm-135μm, and can be selected as 97μm-123μm.
[0117] (2) The surface density of the negative electrode sheet is 6.5 mg / cm³. 2-11.0 mg / cm 2 The option is 6.8 mg / cm³. 2 -9.35mg / cm 2 .
[0118] (3) The compaction density of the negative electrode sheet is 1.48 g / cm³. 3 -1.7g / cm 3 The option is 1.52 g / cm³. 3 -1.65g / cm 3 .
[0119] In this paper, "area density of the electrode" refers to the actual load on the electrode after rolling, which can be expressed as the mass of the material other than the current collector in the electrode per unit area.
[0120] The thickness of the double-sided coated negative electrode sheet can be 91μm, 92μm, 93μm, 94μm, 95μm, 96μm, 97μm, 98μm, 99μm, 100μm, 101μm, 102μm, 103μm, 104μm, 105μm, 106μm, 107μm, 108μm, 109μm, 110μm, 111μm, 112μm, 113μm, 114μm. The micrometer values are 115μm, 116μm, 117μm, 118μm, 119μm, 120μm, 121μm, 122μm, 123μm, 124μm, 125μm, 126μm, 127μm, 128μm, 129μm, 130μm, 131μm, 132μm, 133μm, 134μm, and 135μm, or values within the range obtained by any combination of the above two values. The areal density of the negative electrode sheet can be 6.5 mg / cm³. 2 6.6 mg / cm 2 6.7 mg / cm 2 6.8 mg / cm 2 6.9 mg / cm 2 7.0 mg / cm 2 7.1 mg / cm 2 7.2 mg / cm 2 7.3 mg / cm 2 7.4 mg / cm 2 7.5 mg / cm 2 7.6 mg / cm 2 7.7 mg / cm 2 7.8 mg / cm 2 7.9 mg / cm 2 8.0 mg / cm 2 8.1 mg / cm 28.2 mg / cm 2 8.3 mg / cm 2 8.4 mg / cm 2 8.5 mg / cm 2 8.6 mg / cm 2 8.7 mg / cm 2 8.8 mg / cm 2 8.9 mg / cm 2 9.0 mg / cm 2 9.1 mg / cm 2 9.2 mg / cm 2 9.3 mg / cm 2 9.35 mg / cm 2 9.4 mg / cm 2 9.5 mg / cm 2 9.6 mg / cm 2 9.7 mg / cm 2 9.8 mg / cm 2 9.9 mg / cm 2 10.0 mg / cm 2 10.1 mg / cm 2 10.2 mg / cm 2 10.3 mg / cm 2 10.4 mg / cm 2 10.5 mg / cm 2 10.6 mg / cm 2 10.7 mg / cm 2 10.8 mg / cm 2 10.9 mg / cm 2 10.0 mg / cm 2 The compaction density of the negative electrode sheet can be the compaction density measured under a pressure of 20T-50T. For example, it can be 1.48 g / cm³. 3 1.49 g / cm 3 1.50g / cm 3 1.51g / cm 3 1.52g / cm 3 1.53g / cm 3 1.54g / cm 3 1.55g / cm 3 1.56g / cm 3 1.57g / cm 3 1.58g / cm 3 1.59g / cm 31.60g / cm 3 1.61 g / cm 3 1.62g / cm 3 1.63g / cm 3 1.64 g / cm 3 1.65g / cm 3 1.66 g / cm 3 1.67 g / cm 3 1.68g / cm 3 1.69 g / cm 3 1.70g / cm 3 , or its value is within the range obtained by combining any two of the above values.
[0121] With a fixed coating weight, higher areal density and compaction density of the negative electrode sheet, and a thinner sheet, are more conducive to improving its energy density. Conversely, smaller porosity and pore size hinder electrolyte wetting. Lower areal density and compaction density, and a thicker sheet, are also detrimental to lithium-ion solid-phase transport. Therefore, controlling the parameters of the negative electrode sheet within the aforementioned ranges helps to improve its energy density while maintaining good lithium-ion kinetics, thus enabling the battery cell to achieve both high energy density and fast-charging performance.
[0122] In some embodiments, the positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the surface of the positive current collector. The positive electrode film layer includes a positive electrode active material, which includes lithium transition metal phosphate.
[0123] In some embodiments, lithium transition metal phosphates include at least one of lithium iron phosphate and lithium manganese phosphate.
[0124] In some embodiments, lithium transition metal phosphates include components having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes at least one of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.1.
[0125] In some embodiments, the lithium transition metal phosphate has a carbon coating layer comprising amorphous carbon.
[0126] In this article, "carbon coating" refers to the structure of one or more layers of carbon material formed on the surface of material particles.
[0127] In this article, "amorphous carbon" refers to carbon materials with a low degree of graphitization, approaching an amorphous morphology. Coating the surface of amorphous carbon with a material helps improve its electrical conductivity.
[0128] Carbon coating on the surface of lithium transition metal phosphate can improve the conductivity of the positive electrode active material and facilitate the insertion and extraction of lithium ions, thereby improving the lithium ion kinetics of the positive electrode active material and thus enhancing the fast charging performance of the battery cell.
[0129] In some embodiments, in a cross-section of the positive electrode film along its thickness direction, the area percentage of particles with a diameter greater than or equal to 1.5 μm is greater than or equal to 8.0% and less than or equal to 20.0%.
[0130] In some embodiments, the area ratio of particles with a diameter greater than or equal to 5 μm in the cross-section of the positive electrode film along its thickness direction is 0.
[0131] In some embodiments, in the cross-section of the positive electrode film along its thickness direction, the area ratio of particles with a particle size greater than or equal to 1.5 μm and less than 5 μm is 9.0%-20.0%, optionally 10.0%-20.0%.
[0132] In some embodiments, in the cross-section of the positive electrode film along its thickness direction, the area ratio of particles with a particle size greater than or equal to 1 μm and less than 1.5 μm is 15.0%-25.0%, optionally 16.0%-24.0%.
[0133] By controlling the area ratio of particles with the above-mentioned particle size in the cross-section, the positive electrode sheet can have a higher compaction density, which helps to improve the energy density of the battery cell.
[0134] In some embodiments, the organic solvent includes carbonate solvents, which include at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, dimethyl carbonate, and diethyl carbonate.
[0135] Carbonate solvents possess low viscosity, high dielectric constant, and good electrochemical stability. Lower viscosity facilitates rapid lithium-ion migration in the electrolyte; a higher dielectric constant improves the solubility of lithium salts in the electrolyte, providing sufficient lithium-ion kinetics for the electrochemical reaction; and good electrochemical stability contributes to the cycle stability of the battery cell. Therefore, this embodiment, by combining a carboxylic acid ester solvent as a partial solvent in the electrolyte with a carbonate solvent, helps to reduce electrolyte viscosity, improve lithium-ion kinetics, and enhance the cycle performance of the battery cell, thereby giving the battery cell excellent fast-charge cycle performance.
[0136] In some embodiments, the mass fraction of the carbonate solvent is 20 wt% to 80 wt% based on the total mass of the electrolyte.
[0137] For example, the mass fraction of carbonate solvents can be 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, or a value within the range obtained by any combination of the above two values.
[0138] In some embodiments, the electrolyte includes additives, which include at least one of carbonate additives, sulfur-containing additives, and lithium salt additives; wherein the carbonate additives include at least one of vinylene carbonate and fluoroethylene carbonate; the sulfur-containing additives include at least one of vinyl sulfate, vinyl disulfate, butenyl sulfite, 1,3-propanesulfonyl lactone, vinyl sulfite, and methylene disulfonate; and the lithium salt additives include at least one of lithium difluorophosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, and lithium dioxalate borate.
[0139] Additives help improve the interfacial performance of the positive and negative electrode plates, thereby helping to improve the fast charging performance of individual battery cells.
[0140] In some embodiments, the mass fraction of the additive is 1 wt% to 10 wt% based on the total mass of the electrolyte.
[0141] For example, the mass fraction of the additive can be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, or a value within the range obtained by any combination of the above two values.
[0142] In some embodiments, the electrolyte comprises a lithium salt, which includes at least one of a fluorosulfonate imine salt and lithium hexafluorophosphate; the fluorosulfonate imine salt includes at least one of lithium difluorosulfonate imine and lithium bistrifluoromethanesulfonate imide.
[0143] The aforementioned lithium salts are easily dissociated, which facilitates the rapid migration of lithium ions in the electrolyte and helps improve the fast-charging performance of individual battery cells.
[0144] In some embodiments, the ionic conductivity of the electrolyte is 15 mS / cm-20 mS / cm.
[0145] For example, the ionic conductivity of the electrolyte can be 15 mS / cm, 16 mS / cm, 17 mS / cm, 18 mS / cm, 19 mS / cm, 20 mS / cm, or a value within the range obtained by any combination of the above two values.
[0146] Next, using a lithium-ion battery as a specific example, a detailed description of the positive electrode, negative electrode, separator, and electrolyte in a single battery cell will be provided. It should be understood that the lithium-ion battery is only an example, and the solution provided in this application can also be applied to other types of secondary batteries, such as sodium-ion batteries, magnesium-ion batteries, and lithium-sulfur batteries.
[0147] [Negative electrode plate]
[0148] The negative electrode typically includes a negative current collector 11 and a negative electrode film 10 disposed on at least one surface of the negative current collector 11. The negative electrode film 10 includes a negative electrode active material. In this document, the negative current collector 11 may be a metal foil.
[0149] As an example, the metal foil has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer 10 is disposed on either or both of the two opposite surfaces of the metal foil.
[0150] In one embodiment, the negative electrode film layer 10 further includes an adhesive. The adhesive may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0151] In one embodiment, the negative electrode film layer 10 further includes a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0152] In one embodiment, the negative electrode film layer 10 also includes other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0153] In one embodiment, the negative electrode sheet can be prepared by forming a negative electrode slurry using the components described above. For example, the negative electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., N-methylpyrrolidone) to form the negative electrode slurry. The negative electrode slurry is then coated onto a copper foil, and after drying, cold pressing, and other processes, the negative electrode sheet is obtained.
[0154] [Positive electrode plate]
[0155] The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector, the positive electrode film layer including a positive electrode active material.
[0156] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0157] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0158] In some embodiments, the positive electrode active material may be a known positive electrode active material for batteries. As an example, the positive electrode active material may include at least one of the following materials: lithium phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM523), LiNi 0.5 Co 0.25 Mn0.25 O2 (also known as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi) 0.85 Co 0.15 Al 0.05 At least one of O2 and its modified compounds. Examples of lithium-containing phosphates with an olivine structure include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium iron manganese phosphate, and lithium iron manganese phosphate and carbon composites. During the charging and discharging process, Li undergoes insertion / extraction and consumption, resulting in different molar contents of Li in the positive electrode active material when the battery is discharged to different states. In the examples of positive electrode active materials in this application, the molar content of Li refers to the initial state of the material, i.e., the state before feeding. After charge-discharge cycles, the molar content of Li changes when the positive electrode active material is applied to the battery system. In the examples of positive electrode active materials in this application, the molar content of O is only an ideal value; lattice oxygen release causes changes in the molar content of O, and the actual molar content of O will fluctuate.
[0159] In some embodiments, the positive electrode film layer further includes a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0160] In one embodiment, the positive electrode film layer further includes a conductive agent. As an example, the conductive agent may also include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, graphene, and carbon nanofibers.
[0161] In some embodiments, the positive electrode sheet can be prepared by forming a positive electrode slurry from the components described above. For example, the positive electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry. The positive electrode slurry is then coated onto a positive electrode current collector, and after drying, cold pressing, and other processes, the positive electrode sheet is obtained.
[0162] Electrolyte
[0163] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not specify any particular type of electrolyte; it can be selected according to requirements. The electrolyte includes electrolyte salts and solvents.
[0164] In one embodiment, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0165] In one embodiment, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0166] In one embodiment, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0167] [Isolation membrane]
[0168] This application does not impose any particular restrictions on the type of separator membrane. For example, any well-known porous separator membrane with good chemical and mechanical stability can be selected.
[0169] In one embodiment, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0170] [Battery Device]
[0171] This application provides a battery device including the battery cells described in the above embodiments. The battery device can be a single physical module comprising one or more battery cells to provide higher voltage and capacity. When there are multiple battery cells, the multiple battery cells are connected in series, parallel, or mixed via a busbar.
[0172] In some embodiments, the battery device may be a battery pack, and the battery includes a housing and individual battery cells, with the individual battery cells or battery modules housed in the housing.
[0173] In some embodiments, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.
[0174] In some embodiments, the battery device may be located within an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.
[0175] Figure 2 This is a schematic diagram of a battery device according to this application. Figure 2 As shown, the battery device 30 may include multiple battery cells 20 to meet different power usage needs.
[0176] The battery device 30 may further include a housing with a hollow interior, housing multiple battery cells 20. For example, multiple battery cells 20 may be connected in parallel, series, or a combination thereof and then placed inside the housing. The housing may include a first housing portion 31 and a second housing portion 32, which are closed to each other to form the housing. The shapes of the first housing portion 31 and the second housing portion 32 may be determined based on the shape of the components housed inside, for example, based on the shape of the combination of multiple battery cells 20 housed inside. At least one of the first housing portion 31 and the second housing portion 32 may have an opening. For example, as... Figure 2 As shown, only one of the first housing portion 31 and the second housing portion 32 can be a hollow cuboid with an opening, while the other is plate-shaped to cover the opening. Taking the second housing portion 32 as a hollow cuboid with one opening, and the first housing portion 31 as a plate-shaped example, then the first housing portion 31 covers the opening of the second housing portion 32 to form a housing with a closed chamber, which can be used to accommodate multiple battery cells 20.
[0177] For example, unlike Figure 2 As shown, both the first housing portion 31 and the second housing portion 32 can be hollow cuboids with one open side each. The openings of the first housing portion 31 and the second housing portion 32 are positioned opposite each other, and the first housing portion 31 and the second housing portion 32 are interlocked to form a housing with a closed chamber. This chamber can accommodate multiple battery cells 20. The multiple battery cells 20 are connected in parallel, series, or mixed and placed inside the housing formed by the interlocking of the first housing portion 31 and the second housing portion 32.
[0178] In some embodiments, the battery device 30 may further include other components. For example, the battery device 30 may further include a busbar component, which can be used to realize electrical connections between multiple battery cells 20, such as in parallel, series, or mixed connections. Specifically, the busbar component can realize electrical connections between battery cells 20 by connecting to the electrode terminals of the battery cells 20; or, the busbar component can also realize electrical connections between battery cells 20 by connecting to other components of the battery cells 20. The busbar component can be fixed to corresponding components of the battery cells 20 by welding, for example, by welding to electrode terminals, sealing structures, or housings, etc., and the embodiments of this application are not limited thereto.
[0179] The battery cells 20 can be directly assembled into the battery device 30, or they can be first assembled into battery modules, and then multiple battery modules can be assembled into the battery device 30.
[0180] [Electrical Equipment]
[0181] This application also provides an electrical device that includes the battery cell 20 in the foregoing embodiments.
[0182] Electrical equipment can include vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, and power tools, etc. Vehicles can be gasoline-powered cars, natural gas-powered cars, or new energy vehicles; new energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. Spacecraft include airplanes, rockets, space shuttles, and spacecraft, etc. Electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc. This application does not impose any special limitations on the above-mentioned electrical equipment.
[0183] like Figure 3 As shown, this application provides an electrical device, which is a vehicle.
[0184] Vehicle 40 can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A motor, a controller, and battery cells 20 can be installed inside vehicle 40. The controller is used to control the battery cells 20 to supply power to the motor. For example, battery cells 20 can be located at the bottom, front, or rear of vehicle 40. Battery cells 20 can be used to power vehicle 40; for example, they can serve as the operating power source for vehicle 40's electrical system, such as meeting the power requirements for starting, navigation, and operation. In another embodiment of this application, battery cells 20 can not only serve as the operating power source for vehicle 40 but also as the driving power source, replacing or partially replacing gasoline or natural gas to provide driving power to vehicle 40.
[0185] [Examples and Comparative Examples]
[0186] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0187] Example 1
[0188] (1) Preparation of negative electrode sheet
[0189] The active material is silicon-carbon material (particle size 1µm, specific surface area 2.1m²). 2 The following ingredients are dispersed in deionized water at a weight ratio of 20:45:32:3, with a solid content of 12% (g): conductive agent (carbon black and carbon nanotubes in a 1:1 mass ratio), binder (styrene-butadiene rubber and polyacrylic acid in a 1:1 mass ratio), and thickener sodium carboxymethyl cellulose (CMC). After being mixed evenly, a base coating slurry is prepared. The base coating slurry is then uniformly transferred onto the copper foil of the negative electrode current collector using a gravure roller in one or more passes. After drying, a silicon-containing base coating current collector with a thickness of 1.5 μm is formed, which is the negative electrode current collector including the first negative electrode active material layer.
[0190] A first graphite material (graphitization degree of 95%, higher than that of the second graphite material), a conductive agent (carbon black and carbon nanotubes in a 1:1 mass ratio), a binder (styrene-butadiene rubber and polyacrylic acid in a 1:1 mass ratio), and a thickener sodium carboxymethyl cellulose (CMC) were dispersed in deionized water at a weight ratio of 97:0.6:1.8:0.6 and mixed evenly to prepare a slurry for the second negative electrode active material layer. The second graphite material (particle size distribution 1.0, Dv50 12.7 μm, specific surface area 1.03 m²) was then prepared. 2The following components were dispersed in deionized water at a weight ratio of 97:0.6:1.8:0.6: conductive agent (carbon black and carbon nanotubes in a 1:1 mass ratio), binder (styrene-butadiene rubber and polyacrylic acid in a 1:1 mass ratio), and thickener (sodium carboxymethyl cellulose (CMC)) to prepare the third negative electrode active material layer slurry. The second and third negative electrode active material layer slurries were then uniformly coated onto the silicon-containing substrate current collector using a double-layer gasket extrusion coating method, with a mass ratio of 5:5. After drying, cold pressing, and slitting, a silicon-graphite composite negative electrode sheet was obtained. The single-sided density of the negative electrode sheet was 7.2 mg / cm³. 2 The negative electrode sheet has a double-sided thickness of 98 μm and a compaction density of 1.57 g / cm³. 2 .
[0191] (2) Preparation of positive electrode sheet
[0192] Lithium iron phosphate (Dv50 1.4μm), carbon black (conductive agent), and polyvinylidene fluoride (PVDF) (binder) were mixed uniformly at a weight ratio of 97:1:2 using N-methylpyrrolidone (NMP) as the solvent to obtain a positive electrode slurry. This slurry was then uniformly coated onto a positive electrode current collector, followed by drying, cold pressing, and slitting to obtain the positive electrode sheet. By selecting lithium iron phosphate with a suitable particle size, the area ratio of particles ≥5μm in the cross-section along the thickness direction of the positive electrode film was determined to be 0%; the area ratio of particles 1.5μm ≤ <5μm was 15%; and the area ratio of particles 1μm ≤ <1.5μm was 22%, resulting in a compaction density of 2.7 g / cm³ for the positive electrode sheet. 2 .
[0193] (3) Preparation of battery cells
[0194] In an argon-atmospheric glove box (H2O content <10ppm, O2 content <1ppm), methyl formate (a chain carboxylic acid ester) and ethylene carbonate (EC) and diethyl carbonate (DEC) were used as organic solvents. Lithium hexafluorophosphate (LiPF6) and additives vinylene carbonate (VC) and fluoroethylene carbonate (FEC) were added to the organic solvents, dissolved, and mixed thoroughly to obtain the electrolyte. Based on the total mass of the electrolyte, the mass fraction of methyl formate was 25 wt%, EC was 23.5 wt%, and DEC was 32 wt%. Based on the total mass of the electrolyte, the mass fraction of LiPF6 was 12.5 wt%, VC was 5 wt%, and FEC was 2 wt%.
[0195] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), the positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. The electrodes are then wound to form an electrode assembly. The electrode assembly is placed in a housing, dried, injected with electrolyte, and then sealed. After formation and settling processes, a single battery cell is obtained.
[0196] Examples 2-9 and Comparative Examples 1-3
[0197] The positive electrode, negative electrode, and electrolyte parameters of Examples 2-9 and Comparative Examples 1-3 are different from those of Example 1. For details, please refer to Table 1.
[0198] Table 1: Product and performance parameters of Examples 1-9 and Comparative Examples 1-3
[0199] In Table 1, "Compaction" refers to the compaction density of the positive electrode sheet. "Particle Size Concentration" refers to the particle size concentration of lithium transition metal phosphate particles in the positive electrode material. "Silicon Content" refers to the mass fraction of silicon in the silicon material of the negative electrode film. "Area Density" refers to the single-sided areal density of the negative electrode sheet. "Thickness" refers to the thickness of the negative electrode sheet. "Carboxylic Acid Ester Mass Fraction" refers to the mass fraction of chain carboxylic acid ester solvents in the organic solvent. "VED" refers to the volumetric energy density of the battery cell. "Fast Charge Performance" refers to the fast charge time of the battery cell in the fast charge test. "Storage Performance" refers to the storage time of the battery cell to 90% SOH in the storage test. "Cycling Performance" refers to the number of cycles of the battery cell to 90% SOH in the cycle test.
[0200] Comparative analysis of the data from Example 1 and Comparative Examples 1-3 shows that Example 1 exhibits superior overall performance compared to Comparative Examples 1-3. Specifically, Example 1 demonstrates better energy density, fast charging performance, and cycle performance than Comparative Example 1. This proves that the solution proposed in this application, by increasing the compaction density of the positive electrode sheet and combining it with the design of the negative electrode sheet and electrolyte, can improve the energy density, fast charging performance, and cycle performance of a single battery cell, achieving a balance between energy density and fast charging performance, while also giving the battery good cycle performance. Although Comparative Example 2 exhibits better fast charging and cycle performance than Example 1, this is because the negative electrode sheet in Comparative Example 2 does not contain silicon material, thus avoiding a severe volume expansion effect, and the lithium-ion kinetics are not affected by silicon material. However, the energy density of Comparative Example 2 is significantly lower than that of Example 1, failing to meet the design requirements for a high-energy-density battery cell. With both negative electrode sheets containing the same amount of silicon, Example 1 and Comparative Example 3 exhibited the same high energy density. Example 1 showed better fast-charging and cycle performance than Comparative Example 3. This is because the electrolyte in Comparative Example 3 did not contain carboxylic acid ester solvents, resulting in lower ionic conductivity than that of Example 1. Consequently, the lithium-ion kinetics in Comparative Example 3 were inferior to those in Example 1, affecting the fast-charging performance of the battery cells. Simultaneously, the electrolyte's wettability on the electrode sheets was less than that of Example 1, leading to increased consumption of active lithium ions due to polarization in the battery cells, thus affecting their cycle performance. Therefore, this demonstrates that the solution proposed in this application can achieve a balance between energy density and fast-charging performance, while also providing the battery with good cycle performance.
[0201] Comparative analysis of Examples 1-3 shows that the higher the compaction density of the positive electrode sheet, the higher the energy density of the battery cell. Simultaneously, the thinner the positive electrode sheet, the shorter the lithium-ion transport path within it, resulting in better lithium-ion kinetics and improved fast-charging performance of the battery cell. However, higher compaction density also makes the positive electrode active material particles more prone to breakage, increasing the likelihood of new interfaces being exposed during cycling and thus increasing lithium consumption, leading to poorer cycle performance. Furthermore, particle breakage also reduces inter-particle contact resistance, further degrading fast-charging performance. Therefore, controlling the compaction density of the positive electrode sheet within a designed range helps improve the overall performance of the battery cell, achieving a balance between high energy density, fast-charging performance, and cycle performance.
[0202] Comparative analysis of Examples 1 and 4-5 shows that a higher silicon content in the negative electrode film results in a higher energy density for the battery cell. However, this also leads to a more severe volume expansion effect of the silicon material, which significantly impacts the lithium-ion dynamics of the negative electrode and negatively affects the cycle performance and fast-charging performance of the battery cell. Therefore, by controlling the silicon content in the negative electrode film within a designed range, it is possible to improve the energy density of the battery cell while simultaneously achieving good fast-charging and cycle performance, thus balancing high energy density, fast-charging performance, and cycle performance.
[0203] Comparative analysis of Examples 1 and 6-7 shows that, with a constant compaction density, a higher areal density of the negative electrode film and a thicker negative electrode sheet result in a higher energy density of the battery cell. However, a longer lithium-ion transport path within the negative electrode sheet is less conducive to lithium-ion dynamics, leading to poorer fast-charging performance of the battery cell. Therefore, by controlling the areal density of the negative electrode film and the thickness of the negative electrode sheet within a designed range, it is possible to improve the energy density of the battery cell while maintaining good fast-charging performance.
[0204] Comparative analysis of Examples 1 and 8-9 shows that a higher mass fraction of carboxylic acid esters in the solvent is more beneficial to the fast-charging performance of the battery cell. However, carboxylic acid ester solvents are more prone to side reactions and gas generation during battery cell cycling, increasing the risk of these reactions and affecting the cell's cycle performance. Therefore, by controlling the mass fraction of carboxylic acid ester solvents within a designed range, it is possible to improve the fast-charging performance of the battery cell while maintaining good fast-charging cycle performance.
[0205] The following is a brief description of the testing methods for the physicochemical and performance parameters involved in the embodiments of this application. It should be understood that the following testing methods are only examples, and other testing methods known in the art can also be used for testing.
[0206] 1. Test method for graphitization degree
[0207] At 25℃, the battery cell was discharged at a constant current of 0.33C to 2.5V. The battery cell was then disassembled to obtain the negative electrode sheet. A scraper was used to remove the single-sided film layer of the electrode sheet, maintaining the remaining single-sided film layer thickness at 2 / 5 of the original thickness. Then, half the thickness of the active material layer near the negative electrode current collector was scraped off, thus obtaining the second negative electrode active material layer. Graphite was then separated. Specifically, the scraped powder was mixed with water, stirred, filtered, and dried to obtain a graphite sample. The degree of graphitization of the sample was tested using an X-ray diffractometer (e.g., Bruker D8 Discover) according to JB / T 4220-2011. The average interlayer spacing d002 of the C(002) crystal plane in the material's crystal structure was obtained. The degree of graphitization was calculated using the formula g = (0.344 - d002) / (0.344 - 0.3354) × 100%. In the above formula, d002 is the average interlayer spacing of the C(002) crystal plane in the material crystal structure, expressed in nanometers (nm).
[0208] As is known to those skilled in the art, the samples obtained by the above method contain conductive carbon and graphite materials, and the conductive carbon does not affect the test results of the graphite C(002) crystal plane in the above tests.
[0209] 2. Test methods for volume average particle size Dv10, Dv50, Dv90, and span value
[0210] Testing equipment: Particle size analyzer.
[0211] Testing was performed using equipment and methods known in the art. As an example, at 25°C, the battery cell was discharged at a constant current of 0.33C to 2.5V to obtain a battery cell with 0% SOC. The negative electrode was then removed from the battery cell, and the active material layer on one side of the electrode was scraped off, maintaining the remaining single-sided negative electrode film layer thickness at 3 / 5 of the original single-sided thickness. The scraped active material layer was then separated to obtain a second graphite sample. Specifically, the obtained negative electrode film powder can be mixed with water, stirred, filtered, and dried to obtain the graphite sample. According to the testing standard GB / T 19077-2016, the particle size was measured using a Mastersizer 2000E laser particle size analyzer. The particle size was calculated from smallest to largest on the volume particle size distribution curve at the 10%, 50%, and 90% positions, which are Dv10, Dv50, and Dv90, respectively.
[0212] span value = (Dv90 - Dv10) / Dv50.
[0213] 3. Test method for the proportion of particle area in electrode cross-section
[0214] The positive electrode sheet was removed from the battery cell at 0% state of charge (SOC). The positive electrode sheet was then immersed in DMC solvent for at least 72 hours to allow complete leaching of the electrolyte solvent, lithium salt, and additives. Finally, the positive electrode sheet was dried in a vacuum oven. The area of particles in the cross-section of the positive electrode film along the thickness direction of the electrode sheet was statistically analyzed as follows: The positive electrode film was cut along the thickness direction of the electrode sheet using an argon ion beam (for example, a Leica EM TIC 3X CP device could be used, operating voltage: 6kV, operating time: 6h). After exposing the cross-section, a scanning electron microscope (for example, a Hitachi SU8230 device could be used, operating voltage: 3kV, beam current: high, probe model: U (LA100), working distance <5mm) was used to observe the cross-section of the positive electrode film along the thickness direction of the electrode sheet. Images were acquired using a field emission scanning electron microscope (FESEM) at non-edge locations within the cross-section of the positive electrode film (after observing the electrode edge under the SESEM, the field of view was adjusted to the center of the sample) in secondary electron mode. Electron micrographs were taken at 10kx magnification, and the particles in the electron micrographs were analyzed using ImageJ software (1.46r, Win64 version). The specific usage of ImageJ software is as follows: load the SESEM image to be analyzed, use the Cellpose plugin to identify particles, and perform manual corrections; use ImageJ to read and analyze data. The specific method for identifying particles using the Cellpose plugin is as follows: set the segmentation diameter parameter (diameter in the Segmentation module) to 15 pixels, click "run cyto3" to identify particles, and manually mark particles in the image that were not identified by the software, were not fully identified by the software, or had identification errors. The particles in the image that were not recognized by the software, were not fully recognized by the software, or were recognized with errors mainly include the following: 1. Due to the particle being too large or having scratches on its surface, the particle cannot be recognized or cannot be fully recognized; 2. During the argon ion beam cutting process, scratches will be generated on the particle surface. The software may misjudge the scratches as particle boundaries during the recognition process, thus causing recognition errors; 3. Due to the particle being too small, it was not successfully recognized; 4. The particle is located at the edge of the electron microscope field of view, and the interior of the particle is penetrated by the edge, so the morphology cannot be fully displayed. The part is recognized instead of the whole, resulting in recognition errors.For the unidentified or misidentified particles mentioned above, manual calibration is performed. The specific process is as follows: 1. Delete large particles located around the edges of the scanning electron microscope that are not fully displayed. 2. Determine if any unidentified or misidentified particles have internal cracks or scratches. If no cracks or scratches are found, classify it as a single particle and manually mark it based on the observed particle boundary. 3. If cracks or scratches are found inside the particle, determine if they penetrate the particle. If not, classify it as a single particle and manually mark it. 4. If cracks or scratches penetrate the particle, determine if they are linear or irregular. 5. If the cracks or scratches are irregular, classify them as the boundary between particles and divide the particles along this boundary. 6. If the cracks or scratches are linear, perform contrast comparison. 7. If the contrast is not obvious and there is no crack-like appearance, classify it as a scratch and mark it as a single particle. 8. If the contrast is strong and there is a crack-like appearance, classify it as the boundary between particles and mark it as two particles. After manual marking, delete information irrelevant to the particles from the automatic image processing, thus completing the particle identification and marking in the image.
[0215] After particle identification and labeling, the images were imported into ImageJ software for analysis. Scale settings were established based on the scanning electron microscope (SEM) images. The particle diameter and area were analyzed using the "Feret diameter" and "Area" analysis functions. According to the software manual (ImageJ User Guide IJ 1.46r), the "Feret" parameter represents the maximum spacing between all parallel lines in the particle's two-dimensional projection, thus characterizing the particle diameter; the "Area" parameter represents the pixel area of the particle, thus characterizing its area. Since particles smaller than 50 nm present significant errors during the statistical process and are difficult to accurately identify, and since conductive agents generally have a particle diameter smaller than 50 nm, which can significantly influence the statistical results, particles smaller than 50 nm were not counted in this application's particle diameter statistics, and the statistical data for particles with an Area display of "NaN" were deleted. Following the above method, to ensure a statistically significant sample size, at least 10 non-overlapping SEM images were acquired for each electrode, and the area of at least 5000 particles was statistically analyzed. The sum of the "Area" parameters for particles with a diameter greater than or equal to 1.5 μm and the sum of the "Area" parameters for all particles are calculated, and these are used as the area of particles with a diameter greater than or equal to 1.5 μm and the total area of the statistically analyzed particles, respectively. The sum of the areas of particles with a diameter greater than or equal to 1.5 μm divided by the total area of the statistically analyzed particles is used as the percentage of the area of particles with a diameter greater than or equal to 1.5 μm in the cross-section of the positive electrode film along the thickness direction of the electrode sheet.
[0216] 4. Test method for the mass fraction of silicon material in the negative electrode film layer
[0217] At 25°C, the battery cells were charged to 3.8V at a constant current of 0.33C and discharged to 2.0V at a constant current of 0.33C to obtain a battery cell with 0% SOC. The negative electrode was then disassembled and soaked in DMC solvent for at least 72 hours to allow the electrolyte solvent, lithium salt, and additives to be completely leached out. The negative electrode was then dried in a vacuum oven. The negative electrode film was peeled off from the current collector and pulverized. The sample was digested with a mixed acid solution (aqua regia and HF hydrofluoric acid). The mass percentage of silicon in the digested solution was determined by inductively coupled plasma atomic emission spectrometry (ICP-OES), and the mass percentage of silicon in the negative electrode film was calculated.
[0218] 5. Test methods for film thickness
[0219] The porosity of the negative electrode sheet of a battery cell at 0% state of charge (SOC) can be detected using the following method: Disassemble the battery cell at 0% SOC to separate the negative electrode sheet. Immerse the negative electrode sheet in DMC solvent for at least 72 hours to allow the electrolyte solvent, lithium salt, and additives to completely leach out. Dry the negative electrode sheet in a vacuum oven. Take the electrode sheet to be tested and obtain a cross-sectional photograph of the film layer under a metallographic microscope. For the same sample, randomly select 30 points, and measure the film thickness at each point along a direction perpendicular to the current collector. Calculate the average value of the 30 corresponding thickness data points; this average value represents the film thickness.
[0220] 6. Test method for specific surface area (BET)
[0221] Nitrogen adsorption was used for determination. As an example, a single battery cell was discharged at a constant current of 0.33C to 2.5V at 25°C to obtain a 0% SOC battery cell. The negative electrode was then removed from the battery cell, and the corresponding active material was scraped off, followed by separation of graphite. Specifically, the powder of the negative electrode film could be mixed with water, stirred, filtered, and dried to obtain a graphite sample. Using nitrogen adsorption, the graphite sample was first placed in a storage tube, an instrument commonly known as a Quantachrome physisorption analyzer. Nitrogen gas was passed through the storage tube and brought into contact with the graphite sample at a specific temperature of 77K (-196°C). When nitrogen gas passed through the graphite sample, physisorption occurred, meaning nitrogen molecules adhered to the graphite surface. After the adsorption process was complete, the storage tube was immediately removed from the analyzer and quickly sealed to prevent the nitrogen molecules adsorbed on the graphite surface from escaping. Finally, the storage tube was placed back into the analyzer, and high-purity helium gas was introduced. Because helium has a smaller molecular weight than nitrogen, it can enter the pores of graphite, thereby displacing nitrogen molecules adsorbed on the graphite surface. By measuring the time and pressure required for helium to pass through the adsorption tube, the specific surface area of the graphite material can be calculated.
[0222] The formula for calculating specific surface area using nitrogen adsorption mainly relies on the BET formula. The BET formula is based on the Ideal Adsorption Solution Theory (IAST), which assumes that the adsorbate interacts with only a single molecule on the solid surface during adsorption. The expression for the BET formula is: Specific surface area (m²) 2 / g)=((P / P0)ln(P / P0)-1) / (RBET×(ΔP / P0));
[0223] Where P is the nitrogen pressure adsorbed on the solid surface, P0 is the nitrogen pressure before adsorption, RBET is the BET specific surface area, and ΔP is the pressure change during adsorption and desorption.
[0224] 7. OI Value Testing Methods
[0225] The test is performed using equipment and methods known in the art. As an example, the battery cell is discharged at a constant current of 0.33C to 2.5V at 25°C to obtain a battery cell with 0% SOC. The negative electrode is then removed from the battery cell. The first graphite material and the second graphite material can be obtained respectively by the following methods.
[0226] First graphite material: The active material layer on one side of the electrode is scraped off, keeping the thickness of the remaining negative electrode film layer on one side at 2 / 5 of the original thickness; the remaining 1 / 2 thickness of the active material layer is scraped off. Thus, the scraped active material layer is separated to obtain the first graphite sample.
[0227] Second graphite material: Scrape off the active material layer on one side of the electrode sheet, keeping the thickness of the remaining negative electrode film layer on one side at 3 / 5 of the original thickness on one side. Thus, the scraped active material layer is separated to obtain the second graphite sample.
[0228] Specifically, the obtained negative electrode film powder can be mixed with water, stirred, filtered, and dried to obtain a graphite sample. The OI value of the sample is tested using an X-ray diffractometer (such as a Bruker D8 Discover) according to JB / T 4220-2011, based on the formula OI value = I 004 / I 110 The OI value of the powder in the sample was calculated. 004 The integrated area of the diffraction peaks on the crystalline carbon 004 crystal plane in the powder sample, I 110 The integrated area of the diffraction peak of the 110 crystal plane of crystalline carbon in the powder sample.
[0229] 8. Test method for electrode compaction density
[0230] The compaction density of the positive electrode film layer of a single battery cell at 0% State of Charge (SOC) can be tested using the following method: Disassemble the positive electrode sheet from the battery cell at 0% SOC and measure its compaction density. For example, take a single-sided coated positive electrode sheet (if it is a double-sided coated sheet, wipe off the positive electrode film layer on one side first), cut it into a small circular piece with an area of S1, weigh it, and record its weight as M1, and measure its thickness H1. Then wipe off the positive electrode film layer of the weighed positive electrode sheet, weigh the positive current collector, record its weight as M0, and measure its thickness H0. The single-sided coating weight of the positive electrode film layer = (weight of the positive electrode sheet M1 - weight of the positive current collector M0) / S1, the thickness of the positive electrode film layer = thickness of the positive electrode sheet H1 - thickness of the positive current collector H0, and the compaction density of the positive electrode sheet = single-sided coating weight of the positive electrode film layer / thickness of the positive electrode film layer.
[0231] 9. Test methods for the energy density of a single battery cell
[0232] At 25℃, the battery cell is discharged at a constant current of 0.33C to 2.5V, left to stand for 5 minutes, charged at a constant current of 0.33C to the upper limit cutoff voltage of 3.8V, and then charged at a constant voltage to a current of 0.05C, left to stand for 5 minutes; discharged at a constant current of 0.33C to the discharge cutoff voltage of 2.5V, and the discharge capacity at this time is recorded and the discharge energy E0 is obtained, in Wh; the length, width and height of the battery cell are measured with calipers, and the volume V0 of the battery cell is calculated, in L.
[0233] Volumetric energy density (Wh / L) = Discharge energy E0 / Cell volume.
[0234] 10. Test methods for the cycle performance of individual battery cells
[0235] At 25°C, charge the battery cell to 3.8V at a charging rate of 0.5C, then charge it to 0.05C at a constant voltage of 3.8V, let it stand for 10 minutes, and then discharge it to the discharge cutoff voltage of 2.5V at a discharge rate of 0.33C, and let it stand for 10 minutes. One charge-discharge cycle is one cycle. The test is stopped when the capacity of the battery cell decays to 90% of the discharge capacity of the first cycle. This is recorded as the cycle number @ 90% SOH. The more cycle numbers, the longer the cycle life and the better the cycle performance.
[0236] 11. Test methods for the fast charging performance of individual battery cells
[0237] The fast-charging performance of a stacked three-electrode battery cell was tested. As an example, the battery cell was discharged at a constant current of 0.33C to 2.5V, then disassembled to obtain the positive electrode, negative electrode, and separator. The positive electrode, negative electrode, and separator were then immersed in DMC solvent for at least 72 hours to allow the electrolyte solvent, lithium salt, and additives to be completely leached out. The positive and negative electrodes were then dried in a vacuum oven. An electrode assembly was prepared by stacking the positive electrode, separator, third electrode (copper wire), separator, and negative electrode in that order. The electrode assembly was then placed in a housing, and the prepared electrolyte was added. After encapsulation, settling, formation, and aging processes, a three-electrode battery cell was obtained.
[0238] The battery was charged at different states of charge (SOC) with tests conducted every 5% SOC. The maximum charging current corresponding to 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, and 80% SOC was measured and recorded. The time taken to charge from 10% SOC to 80% SOC at the maximum charging current was also recorded. This time was used to measure the fast charging performance of the battery cell.
[0239] The maximum charging current corresponding to different SOCs can be obtained as follows: At 25°C, select different current densities to charge the battery cells, and record the SOC when the third electrode potential reaches 0mV under that current. Then, the current corresponds to the maximum charging current of that SOC.
[0240] Although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A battery cell, characterized in that, The battery cell includes a positive electrode, a negative electrode, and an electrolyte; The compaction density of the positive electrode sheet is 2.62 g / cm³. 3 -2.8g / cm 3 ; The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one side surface of the negative current collector, the negative electrode film layer comprising silicon material; The electrolyte includes chain-like carboxylic acid ester solvents.
2. The battery cell according to claim 1, characterized in that, The mass fraction of the chain carboxylic acid ester solvent is 8 wt%-60 wt% based on the total mass of the electrolyte.
3. The battery cell according to claim 1 or 2, characterized in that, The chain-like carboxylic acid ester solvents include at least one of methyl formate, ethyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl acrylate, and ethyl acrylate.
4. The battery cell according to any one of claims 1-3, characterized in that, Based on the total mass of the negative electrode film, the mass fraction of silicon element in the silicon material is 0.2wt%-2.2wt%.
5. The battery cell according to any one of claims 1-4, characterized in that, The negative electrode film layer includes a first negative electrode active material layer, a second negative electrode active material layer and a third negative electrode active material layer. The first negative electrode active material layer is disposed on at least a portion of the surface of the negative electrode current collector. The second negative electrode active material layer is disposed on at least a portion of the surface of the first negative electrode active material layer. The third negative electrode active material layer is disposed on the side of the second negative electrode active material layer away from the negative electrode current collector. The first negative electrode active material layer includes the silicon material, the second negative electrode active material layer includes the first graphite material, and the third negative electrode active material layer includes the second graphite material.
6. The battery cell according to any one of claims 1-5, characterized in that, The thickness of the first negative electrode active material layer is 0.5μm-3μm.
7. The battery cell according to any one of claims 1-6, characterized in that, The volume average particle size of the silicon material is 0.5μm-3μm.
8. The battery cell according to any one of claims 1-7, characterized in that, The silicon material includes at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy.
9. The battery cell according to any one of claims 1-8, characterized in that, The first negative electrode active material layer includes a conductive agent, which includes at least one of conductive carbon black and carbon nanotubes; The mass fraction of the conductive agent is 15wt%-55wt% based on the total mass of the negative electrode film.
10. The battery cell according to any one of claims 1-9, characterized in that, The first negative electrode active material layer includes an adhesive, which includes at least one of polyacrylic acid and styrene-butadiene rubber; The binder has a mass fraction of 30wt%-40wt% based on the total mass of the negative electrode film.
11. The battery cell according to any one of claims 5-10, characterized in that, The degree of graphitization of the second graphite material is less than that of the first graphite material.
12. The battery cell according to any one of claims 5-11, characterized in that, The graphitization degree of the first graphite material is 93.2%-96%, and the graphitization degree of the second graphite material is 92%-93.2%.
13. The battery cell according to any one of claims 5-12, characterized in that, The OI value of the first graphite material is less than the OI value of the second graphite material.
14. The battery cell according to any one of claims 5-13, characterized in that, The OI value of the first graphite material is 3.80-3.85, and the OI value of the second graphite material is 3.85-4.
0.
15. The battery cell according to any one of claims 5-14, characterized in that, The second graphite material satisfies at least one of the following conditions (1)-(5): (1) The span value of the second graphite material is 0.9-1.25; (2) The volume average particle size Dv10 of the second graphite material is 4μm-10μm; (3) The volume average particle size Dv50 of the second graphite material is 11μm-18μm; (4) The volume average particle size Dv90 of the second graphite material is 17μm-25μm; (5) The specific surface area of the second graphite material is 1.00 m². 2 / g-1.90m 2 / g.
16. The battery cell according to any one of claims 1-15, characterized in that, The negative electrode sheet satisfies at least one of the following conditions (1)-(3): (1) When the negative electrode film layer is provided on both sides of the negative electrode current collector, the thickness of the negative electrode sheet is 91μm-135μm; (2) The areal density of the negative electrode film layer is 6.5 mg / cm³. 2 -11.0 mg / cm 2 ; (3) The compaction density of the negative electrode sheet is 1.48 g / cm³. 3 -1.7g / cm 3 .
17. The battery cell according to any one of claims 1-16, characterized in that, The positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one side of the surface of the positive current collector. The positive electrode film layer includes a positive electrode active material, which includes lithium transition metal phosphate.
18. The battery cell according to any one of claims 1-17, characterized in that, The lithium transition metal phosphate includes at least one of lithium iron phosphate and lithium manganese phosphate.
19. The battery cell according to any one of claims 1-18, characterized in that, The lithium transition metal phosphate comprises components having the following general formula: The m Fe x P y O j Q q , Wherein, Q includes at least one of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.
1.
20. The battery cell according to any one of claims 17-19, characterized in that, The lithium transition metal phosphate has a carbon coating layer, which comprises amorphous carbon.
21. The battery cell according to any one of claims 17-20, characterized in that, In the cross-section of the positive electrode film along its thickness direction, the area ratio of particles with a diameter greater than or equal to 1.5 μm is greater than or equal to 8.0% and less than or equal to 20.0%.
22. The battery cell according to any one of claims 17-21, characterized in that, In the cross-section of the positive electrode film along its thickness direction, the area ratio of particles with a diameter greater than or equal to 5 μm is 0.
23. The battery cell according to any one of claims 17-22, characterized in that, In the cross-section of the positive electrode film along its thickness direction, the area ratio of particles with a diameter greater than or equal to 1.5 μm and less than 5 μm is 9.0%-20.0%, and can be optionally 10.0%-20.0%.
24. The battery cell according to any one of claims 17-23, characterized in that, In the cross-section of the positive electrode film along its thickness direction, the area ratio of particles with a diameter greater than or equal to 1 μm and less than 1.5 μm is 15.0%-25.0%, and can be optionally 16.0%-24.0%.
25. The battery cell according to any one of claims 1-24, characterized in that, The electrolyte includes carbonate solvents, which include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, and diethyl carbonate.
26. The battery cell according to any one of claims 1-25, characterized in that, The mass fraction of the carbonate solvent is 20wt%-80wt% based on the total mass of the electrolyte.
27. The battery cell according to any one of claims 1-26, characterized in that, The electrolyte includes additives, which include at least one of carbonate additives, sulfur-containing additives, and lithium salt additives; The carbonate additives include at least one of vinylene carbonate and fluoroethylene carbonate; The sulfur-containing additive includes at least one of vinyl sulfate, vinyl disulfate, butene sulfite, 1,3-propanesulfonate lactone, vinyl sulfite, and methylene disulfonate. The lithium salt additives include at least one of lithium difluorophosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, and lithium dioxalate borate.
28. The battery cell according to claim 27, characterized in that, The mass fraction of the additive is 1 wt% to 10 wt% based on the total mass of the electrolyte.
29. The battery cell according to any one of claims 1-28, characterized in that, The electrolyte includes a lithium salt, which includes at least one of a fluorosulfonate imine salt and lithium hexafluorophosphate. The fluorosulfonate imine salt includes at least one of lithium difluorosulfonate imine and lithium bistrifluoromethanesulfonate imine.
30. The battery cell according to any one of claims 1-29, characterized in that, The electrolyte has an ionic conductivity of 15 mS / cm-20 mS / cm.
31. A battery device, characterized in that, The battery device comprises the battery cell according to any one of claims 1-30.
32. An electrical appliance, characterized in that, The electrical equipment includes a battery cell according to any one of claims 1-30, or a battery device according to claim 31.