Electrolyte, preparation method and application thereof

By introducing a multi-coordination solvent with large-volume steric hindrance groups into the electrolyte, an entropy-driven weak coordination inner layer is formed, which solves the problems of dendrite growth and oxidative decomposition of traditional electrolytes under high voltage and high rate, and realizes the stability and efficient charge transport of electroplated anode.

CN123143532APending Publication Date: 2026-11-20WUHAN JIANA ENERGY TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611052039.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-15
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional electrolytes are prone to dendrite growth during metal plating/stripping, resulting in low coulombic efficiency and short cycle life. Strongly coordinating solvents occupy the first coordination layer of cations, leading to a high desolvation energy barrier. At high rates, the deposition overpotential increases, and the high-voltage positive electrode side is prone to oxidation and decomposition. Existing high-entropy electrolytes cannot actively intervene in the microstructure of the first solvation shell, making it difficult to guarantee stability.

Method used

By introducing a multi-coordination solvent with large volume and chemically inert steric hindrance groups, the strong coordination solvent is repelled to the outer layer by utilizing physical steric effects, forming an entropy-driven weak coordination inner layer, reducing charge transfer resistance, inhibiting dendrite formation, and improving oxidation resistance.

Benefits of technology

It achieves stability and high-rate performance of electroplated negative electrodes under high voltage, reduces charge transfer impedance, promotes uniform metal deposition, and improves the high-voltage stability of the electrolyte and the long life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application provides an electrolyte, a preparation method and application thereof. The electrolyte comprises an organic solvent, a sodium salt and an additive. The organic solvent is a fluorine-free ether solvent, which comprises a high steric hindrance multi-coordination chelating solvent and a low steric hindrance single-coordination ether solvent. The volume percentage of the high steric hindrance multi-coordination chelating solvent is 20% to 40% and the volume percentage of the low steric hindrance single-coordination ether solvent is 60% to 80% based on 100% of the total volume of the high steric hindrance multi-coordination chelating solvent and the low steric hindrance single-coordination ether solvent. The electrolyte provided by the application can meet the high-voltage and high-rate operation requirements of a metal battery with a negative electrode of electroplating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrochemical energy storage technology, and relates to an electrolyte, its preparation method and application. Specifically, it relates to an electrolyte for electroplating negative electrodes (such as sodium metal negative electrodes) and its preparation method, especially an electrolyte that actively regulates the entropy of ion solvation structure through physical steric hindrance effect, thereby simultaneously achieving high voltage stability and high rate performance. Background Technology

[0002] With the rapid development of electric vehicles and large-scale energy storage, the requirements for battery energy density and power density are becoming increasingly stringent. Matching a high-voltage positive electrode with an electroplated negative electrode, such as lithium metal or sodium metal, is a recognized approach to overcoming the energy density bottleneck. Electroplated negative electrodes, through in-situ metal deposition on the current collector during charging, possess the lowest electrochemical potential and extremely high theoretical specific capacity. However, the practical application of electroplated negative electrodes has long been limited by the limitations of the electrolyte: on the one hand, the metal deposition / stripping process easily forms dendrites and "dead metal," leading to low coulombic efficiency, short cycle life, and even internal short circuits; on the other hand, the electrolyte on the high-voltage positive electrode side is prone to oxidative decomposition, causing rapid battery failure.

[0003] The solvation structure of an electrolyte directly determines the cation transport kinetics, interfacial desolvation behavior, and the electrolyte's antioxidant capacity. Traditional electrolytes often employ strong coordination solvents (such as carbonates and chelate ethers), which are tightly coordinated with cations to form large-sized solvation sheaths. While this structure ensures salt dissociation and ion conduction, its high desolvation energy barrier significantly increases charge transfer impedance, especially at high rates, easily leading to increased metal deposition overpotential and exacerbating dendrite growth. Simultaneously, strong coordination solvents are prone to electrochemical oxidation at high voltages, generating gas and degrading the cathode structure. Although introducing fluorinated weak coordination solvents (such as hydrofluoroethers and fluorocarbonates) can lower the desolvation energy and improve antioxidant capacity, these weak coordination solvents are difficult to spontaneously enter the first solvation shell. Simple mixing leaves the strong coordination solvent still dominating the inner layer composition, failing to fundamentally solve the problem.

[0004] Existing technologies almost entirely increase the mixing entropy of the system by adding different types of lithium salts or solvent components, hoping to utilize the synergistic effect between multiple components to stabilize the interface and broaden the temperature range. However, this "stabilization" strategy has inherent drawbacks: poor thermodynamic compatibility among multiple components, complex interactions often leading to uncontrollable side reactions or phase separation, making long-term stability difficult to guarantee; more importantly, this method cannot actively intervene in the microstructure of the first coordination layer of the cation, and the ions are still firmly occupied by solvent molecules with strong coordination capabilities, resulting in a still high desolvation energy barrier and severe interfacial oxidation under high voltage. Therefore, existing high-entropy electrolytes have failed to substantially solve the problem of dendrite and side reaction coupling in high-voltage, high-rate electroplating anodes.

[0005] In summary, current traditional electrolytes cannot meet the high voltage and high rate operation requirements of electroplated negative electrode metal batteries, so it is necessary to develop a high voltage and high rate electrolyte suitable for electroplated negative electrode metal batteries. Summary of the Invention

[0006] In view of the shortcomings of the existing technology, the purpose of this invention is to provide an electrolyte, its preparation method and application.

[0007] Specifically, the following technical problems exist in the existing technology: Traditional electrolytes are prone to dendrite growth and "dead metal" during metal plating / stripping, resulting in low coulombic efficiency and short cycle life; traditional strong coordination solvents firmly occupy the first coordination layer of cations, leading to a high desolvation energy barrier, significantly increasing charge transfer impedance, and exacerbating deposition overpotential and dendrite problems at high rates; strong coordination solvents are highly polarized by cations, with high HOMO energy levels, making them prone to oxidative decomposition on the high-voltage cathode side; existing "stacked" high-entropy electrolytes cannot actively intervene in the microstructure of the first solvation shell, with strong coordination solvents still dominating the inner layer, failing to fundamentally solve the kinetic and interface stability defects; simple mixing of multiple components often leads to uncontrollable side reactions or phase separation due to complex interactions, making long-term stability difficult to guarantee.

[0008] This invention starts by regulating the microstructural entropy of the cation solvation shell, utilizing physical spatial effects rather than chemical affinity to precisely "program" the first coordination layer. By introducing a multi-coordination solvent containing large-volume, chemically inert steric hindrance groups into the electrolyte, the physical barrier and size sieving effect of these steric hindrance groups repel the larger traditional strong coordination solvents from the first solvation shell. This process significantly increases the disorder of the external solvent molecules, enhancing the structural entropy of the system. To maintain thermodynamic stability, the small-molecule, conformationally flexible weak coordination solvent, due to its rapid diffusion and low steric hindrance, is spontaneously pushed into the inner layer and coordinates. Thus, for the first time, an entropy-driven, physically confined weak coordination inner shell design is achieved. This inner shell possesses extremely low desolvation energy, significantly reducing charge transfer resistance, promoting uniform metal deposition, and suppressing dendrite formation. Simultaneously, the weakly coordinated solvent, due to its low degree of cation polarization, has an even lower highest occupied molecular orbital (HOMO) energy level, resulting in stronger intrinsic oxidation resistance. By immobilizing these inert molecules around the ions to participate in transport, the proportion of highly active components is reduced at the source, endowing the electrolyte with excellent high-voltage stability. This strategy is suitable for high-energy-density, high-rate battery systems that require both high-voltage positive electrodes and electroplated negative electrodes.

[0009] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides an electrolyte comprising an organic solvent, a sodium salt, and additives; The organic solvent is a fluorine-free ether solvent, including highly sterically hindered multi-coordination chelating solvents and low sterically hindered single-coordination ether solvents; Taking the total volume of the high-steric-hindrance multi-coordinate chelating solvent and the low-steric-hindrance monocoordinate ether solvent as 100%, the volume ratio of the high-steric-hindrance multi-coordinate chelating solvent is 20%~40%, for example 20%, 22%, 24%, 25%, 26%, 28%, 30%, 32%, 34%, 35%, 36%, 38%, 40%, etc., and specific values ​​between the above points. Due to space limitations and for the sake of brevity, this invention will not exhaustively list the specific values ​​included in the range. The volume ratio of the low-steric-hindrance monocoordinate ether solvent is 60%~80%, for example 60%, 62%, 64%, 65%, 66%, 68%, 70%, 72%, 74%, 75%, 76%, 78%, 80%, etc., and specific values ​​between the above points. Due to space limitations and for the sake of brevity, this invention will not exhaustively list the specific values ​​included in the range.

[0010] The electrolyte provided by this invention starts by regulating the entropy of the microstructure of the solvation shell. It utilizes a multi-coordinate solvent containing large-volume inert steric hindrance groups to repel strongly coordinated solvents in the outer layer through physical barriers, thereby increasing the entropy of the solvation structure. To maintain the thermodynamic stability of the solvation structure, a small-volume weakly coordinated solvent spontaneously enters the inner shell, forming for the first time an entropy-driven, physically confined weakly coordinated inner layer. This inner layer has an extremely low desolvation energy, which can reduce charge transfer impedance, promote uniform metal deposition, and suppress dendrites. At the same time, the weakly coordinated solvent has a low degree of polarization and a low HOMO energy level, reducing highly active components from the source and endowing the electrolyte with excellent high-voltage stability. It is suitable for high-energy, high-rate battery systems that balance high-voltage positive electrodes and electroplated negative electrodes.

[0011] High-steric multi-coordination chelating solvents cannot satisfy Na alone + To meet the complete coordination requirements, this invention controls the volume ratios of high-steric-impedance multi-coordination chelating solvent and low-steric-impedance mono-coordination ether solvent to be 20%~40% and 60%~80%, respectively. This forces the low-steric-impedance mono-coordination ether solvent molecules to spontaneously enter the solvation shell to complete the coordination, forming a mixed coordination structure where the high-steric-impedance multi-coordination chelating solvent provides the skeletal multidentate coordination, and the low-steric-impedance mono-coordination ether solvent fills the remaining coordination vacancies. This structure utilizes the multidentate coordination stability of the chelating solvent and avoids coordination defects caused by steric hindrance of the chelating solvent through the filling of small molecule solvents, resulting in the lowest overall solvation free energy and the best thermodynamic stability.

[0012] Preferably, the high steric hindrance multi-coordination chelating solvent includes any one or a combination of at least two of the following: triethylene glycol diethyl ether, triethylene glycol dibutyl ether, triethylene glycol dipropyl ether, triethylene glycol ethyl methyl ether, triethylene glycol butyl methyl ether, triethylene glycol butyl ethyl ether, tripropylene glycol dimethyl ether, tripropylene glycol diethyl ether, tripropylene glycol dibutyl ether, tripropylene glycol dipropyl ether, tripropylene glycol ethyl methyl ether, tripropylene glycol butyl methyl ether, tripropylene glycol butyl ethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol dibutyl ether, tetraethylene glycol dipropyl ether, tetraethylene glycol ethyl methyl ether, tetraethylene glycol butyl methyl ether, and tetraethylene glycol propyl methyl ether.

[0013] Preferably, the low-steric hindrance monocoordinate ether solvent is selected from 1,3-dioxane, 4-methyl-1,3-dioxane, 4-ethyl-1,3-dioxane, 5-methyl-1,3-dioxane, 5-ethyl-1,3-dioxane, 4,4-dimethyl-1,3-dioxane, 4,4-diethyl-1,3-dioxane, 4-methyl-4-ethyl-1,3-dioxane, 5,5-dimethyl-1,3-dioxane, 5,5-diethyl-1,3-dioxane, 5-methyl-5-ethyl-1,3-dioxane, 4,5-dimethyl-1,3-dioxane, 4-ethyl-5-methyl-1,3-dioxane, 4,5-diethyl-1,3-dioxane, 4 The following is a combination of any one or at least two of the following: 6-dimethyl-1,3-dioxane, 4,6-diethyl-1,3-dioxane, 4-ethyl-6-methyl-1,3-dioxane, 4,4,5-trimethyl-1,3-dioxane, 4,4,6-trimethyl-1,3-dioxane, 4,5,6-trimethyl-1,3-dioxane, tetrahydropyran, 2-methyltetrahydropyran, 3-methyltetrahydropyran, 4-methyltetrahydropyran, 2,2-dimethyltetrahydropyran, 2,3-dimethyltetrahydropyran, 2,4-dimethyltetrahydropyran, 2,5-dimethyltetrahydropyran, 2,6-dimethyltetrahydropyran, 3,3-dimethyltetrahydropyran, 3,4-dimethyltetrahydropyran, 3,5-dimethyltetrahydropyran, and 4,4-dimethyltetrahydropyran.

[0014] Preferably, the sodium salt comprises any one or a combination of at least two of the following: sodium perchlorate, sodium tetraphenylborate, sodium nitrate, sodium bis(oxalato)borate, sodium tetraphenoxyborate, sodium hexafluorophosphate, sodium tetrafluoroborate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoroacetate, sodium difluorooxalatoborate, sodium bis(oxalato)borate, and sodium trifluoromethanesulfonate (NaOTF).

[0015] Preferably, the concentration of sodium salt in the electrolyte is 0.3~2 mol / L, for example 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.8 mol / L, 2 mol / L, etc., and specific values ​​between the above values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list the specific values ​​included in the range. Preferably, it is 0.3~1.5 mol / L, and more preferably 0.5~1 mol / L.

[0016] If the concentration of sodium salt is too high, the viscosity of the electrolyte will increase, which will not meet the high-rate operation conditions of the battery; if the concentration of sodium salt is too low, the concentration of sodium ions in the electrolyte will be too low, resulting in low electrolyte conductivity and reduced interfacial film-forming performance of the electrolyte.

[0017] Preferably, the additive is a fluorine-free additive, including any one or a combination of at least two of tetravinylsilane, 1,3-propanesulfonyl lactone, vinyl sulfite, vinyl sulfate, tris(trimethylsilane) phosphate, trimethoxy(pentafluorophenyl)silane, and phenyltrivinylsilane.

[0018] Preferably, the content of the additive is 0.05% to 1.5% based on the total weight of the electrolyte (100%), for example, 0.05%, 0.06%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, etc., as well as specific values ​​between the above values. Due to space limitations and for the sake of brevity, this invention will not exhaustively list the specific values ​​included in the range, but preferably 0.1% to 1%.

[0019] If the proportion of additives is too high, it will result in an excessively thick film; if the proportion of additives is too low, it will not be able to play a role in constructing a stable sodium metal interface.

[0020] In a second aspect, the present invention provides a method for preparing an electrolyte as described in the first aspect, the method comprising the following steps: The electrolyte is obtained by mixing an organic solvent, a sodium salt, and an additive.

[0021] Thirdly, the present invention provides an electroplated negative electrode metal battery, the electroplated negative electrode metal battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte as described in the first aspect.

[0022] Preferably, the electroplated negative electrode metal battery includes an electroplated negative electrode sodium metal battery.

[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention breaks through the traditional chemical regulation framework that relies on solvent polarity or coordination ability, and proposes a new paradigm of entropy-driven solvation design based on physical spatial effects. By introducing large-volume, chemically inert steric groups into the electrolyte components, a crowded spatial microenvironment is constructed around the ions. These large groups act as physical barriers, utilizing the size sieving effect to exclude the large-volume traditional strong coordination solvents from the first solvation shell. This process significantly increases the disorder of the outer solvent molecules and enhances the structural entropy of the system. In order to maintain the thermodynamic stability of the solvation structure, small-volume, conformationally flexible weak coordination solvents can spontaneously enter the inner solvation shell through concentration competition. This strategy achieves precise physical manipulation of the composition and structure of the first coordination layer.

[0024] (2) The electrolyte provided by the present invention, on the one hand, the weakly coordinating solvent entering the inner layer and the ions are confined in a stable spatial configuration by the surrounding steric groups, forming a physically confined and stable ion-solvent contact pair, which effectively suppresses solvent exchange and side reactions; on the other hand, its inner layer is composed of weakly interacting solvent molecules, which makes the energy required for the ions to desolvate at the electrode interface extremely low, thereby greatly reducing the charge transfer impedance, accelerating the interfacial reaction kinetics, and facilitating the formation of a thin and dense SEI film.

[0025] (3) Traditional strong coordination solvents tightly surround sodium ions, forming highly active "free solvent-ion" complexes that are easily oxidized by losing electrons on the surface of the high-voltage cathode. The steric hindrance groups in this invention "confine" the weak coordination solvents to the solvated inner shell. These weak coordination solvents themselves have weak coordination ability and low polarization, resulting in lower highest occupied molecular orbital energy levels and stronger intrinsic antioxidant properties. Fixing these more "inert" molecules around the ions for transport is equivalent to reducing the proportion of active material from the source, thereby improving the high-voltage performance (4.5V) of the electrolyte. Detailed Implementation

[0026] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0027] Example 1 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium hexafluorophosphate) was dissolved in a mixed solvent of tetraethylene glycol diethyl ether and 2-methyltetrahydropyran at a volume ratio of 3:7, and then an additive (1,3-propane sulfonyl lactone) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 0.3 mol / L; The content of the additive is 1% based on the total weight of the electrolyte (100%).

[0028] Example 2 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium hexafluorophosphate) was dissolved in a mixed solvent of tetraethylene glycol ethyl methyl ether and 4,4-dimethyl-1,3-dioxane in a volume ratio of 3:7. Then, an additive (1,3-propane sulfonyl lactone) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 1 mol / L; The content of the additive is 0.1% based on the total weight of the electrolyte (100%).

[0029] Example 3 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium bis(fluorosulfonyl)imide) was dissolved in a mixed solvent of triethylene glycol ethyl methyl ether and tetrahydropyran at a volume ratio of 4:6, and then an additive (ethylene sulfate) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 1 mol / L; The content of the additive is 0.5% based on the total weight of the electrolyte (100%).

[0030] Example 4 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium perchlorate) was dissolved in a mixed solvent of tetraethylene glycol butyl methyl ether and 2-methyltetrahydropyran at a volume ratio of 2.5:7.5, and then an additive (1,3-propane sulfonyl lactone) was added and stirred until homogeneous to obtain the electrolyte, which was then tested at room temperature. The concentration of sodium salt in the electrolyte is 0.8 mol / L; The content of the additive is 1% based on the total weight of the electrolyte (100%).

[0031] Example 5 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium hexafluorophosphate) was dissolved in a mixed solvent of tripropylene glycol dimethyl ether and 1,3-dioxane in a volume ratio of 3:7, and then an additive (ethylene sulfite) was added. The mixture was stirred until homogeneous to obtain the electrolyte, which was then tested at room temperature. The concentration of sodium salt in the electrolyte is 0.5 mol / L; The content of the additive is 0.1% based on the total weight of the electrolyte (100%).

[0032] Example 6 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium trifluoromethanesulfonate) was dissolved in a mixed solvent of triethylene glycol dibutyl ether and 4-methyl-1,3-dioxane in a volume ratio of 4:6, and then an additive (tris(trimethylsilane) phosphate) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 0.6 mol / L; The content of the additive is 0.8% based on the total weight of the electrolyte (100%).

[0033] Example 7 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (a mixture of sodium bis(fluorosulfonyl)imide and sodium tetrafluoroborate in a molar ratio of 1:1) was dissolved in a mixed solvent of triethylene glycol ethyl methyl ether and tetrahydropyran in a volume ratio of 2:8. Then, an additive (tetravinylsilane) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The total concentration of sodium salt in the electrolyte is 1 mol / L; The content of the additive is 0.3% based on the total weight of the electrolyte (100%).

[0034] Example 8 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (bis(trifluoromethanesulfonyl)imide sodium) was dissolved in a mixed solvent of tetraethylene glycol ethyl methyl ether and 2,6-dimethyltetrahydropyran at a volume ratio of 3:7. Then, an additive (a mixture of vinyl sulfate and 1,3-propane sulpholol at a mass ratio of 1:1) was added and stirred until homogeneous to obtain the electrolyte, which was then tested at room temperature. The concentration of sodium salt in the electrolyte is 1.2 mol / L; The content of the additive is 0.5% based on the total weight of the electrolyte (100%).

[0035] Example 9 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium perchlorate) was dissolved in a mixed solvent of tripropylene glycol diethyl ether and 4,4-dimethyl-1,3-dioxane in a volume ratio of 3:7. Then, an additive (phenyltrivinylsilane) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 0.3 mol / L; The content of the additive is 0.05% based on the total weight of the electrolyte (100%).

[0036] Example 10 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium bis(fluorosulfonyl)imide) was dissolved in a mixed solvent of triethylene glycol dibutyl ether and 5-methyl-1,3-dioxane in a volume ratio of 2:8, and then an additive (ethylene sulfite) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 1.5 mol / L; The content of the additive is 1.5% based on the total weight of the electrolyte (100%).

[0037] Example 11 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (a mixture of sodium hexafluorophosphate and sodium difluorooxalate borate in a molar ratio of 2:1) was dissolved in a mixed solvent of triethylene glycol diethyl ether and tetrahydropyran in a volume ratio of 3:7. Then, an additive (tetravinylsilane) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The total concentration of sodium salt in the electrolyte is 1 mol / L; The content of the additive is 0.2% based on the total weight of the electrolyte (100%).

[0038] Example 12 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium trifluoromethanesulfonate) was dissolved in a mixed solvent of triethylene glycol dipropyl ether and 1,3-dioxane in a volume ratio of 2:8, and then an additive (phenyltrivinylsilane) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 0.7 mol / L; The content of the additive is 1% based on the total weight of the electrolyte (100%).

[0039] Example 13 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium bis(fluorosulfonyl)imide) was dissolved in a mixed solvent of triethylene glycol propyl methyl ether and 4-methyl-5-ethyl-1,3-dioxane in a volume ratio of 4:6. Then, an additive (ethylene sulfite) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 1 mol / L; The content of the additive is 0.8% based on the total weight of the electrolyte (100%).

[0040] Example 14 This embodiment provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (a mixture of sodium nitrate and sodium bis(fluorosulfonyl)imide in a molar ratio of 1:1) was dissolved in a mixed solvent of tripropylene glycol dimethyl ether and tetrahydropyran in a volume ratio of 3:7. Then, an additive (1,3-propanesulfonyl lactone) was added and stirred until homogeneous to obtain the electrolyte, which was tested at room temperature. The concentration of sodium salt in the electrolyte is 1 mol / L; The content of the additive is 0.4% based on the total weight of the electrolyte (100%).

[0041] Comparative Example 1 This comparative example provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium hexafluorophosphate) was dissolved in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, and stirred until homogeneous to obtain the electrolyte, which was then tested at room temperature. The concentration of sodium salt in the electrolyte is 1 mol / L.

[0042] Comparative Example 2 This comparative example provides an electrolyte, the preparation method of which includes the following steps: Sodium salt (sodium hexafluorophosphate) was dissolved in a mixed solvent of ethylene carbonate and methyl ethyl carbonate in a volume ratio of 3:7, and stirred until homogeneous to obtain the electrolyte, which was then tested at room temperature. The concentration of sodium salt in the electrolyte is 1 mol / L.

[0043] Comparative Example 3 The only difference between this comparative example and Example 1 is that the volume ratio of tetraethylene glycol diethyl ether to 2-methyltetrahydropyran is 1:9.

[0044] Comparative Example 4 The only difference between this comparative example and Example 1 is that the volume ratio of tetraethylene glycol diethyl ether to 2-methyltetrahydropyran is 5:5.

[0045] Performance testing In an argon-protected glove box, a sodium-copper button cell was assembled using copper foil as the working electrode, sodium metal as the counter / reference electrode, and a polypropylene membrane as the separator. The electrolyte provided in each embodiment and comparative example was injected, and the cells were incubated at 25°C with an output of 1 mA·cm⁻¹. -2 Current density deposition 1mAh·cm -2 Sodium metal was used, and then the average coulombic efficiency of sodium-copper button cells was tested after a specific number of cycles (200 cycles). The average coulombic efficiency was the average coulombic efficiency per week of sodium metal deposition cycle (coulombic efficiency = sodium metal dissolution / deposition amount × 100%). The test results are shown in Table 1.

[0046] Meanwhile, sodium / / sodium iron sulfate half-cells were assembled using sodium iron sulfate as the positive electrode material, with charge and discharge voltages of 2-4.3V. The high-voltage performance (capacity retention rate = capacity of the last cycle of the calculated number of cycles / capacity of the first cycle at the same rate, the test results are shown in Table 2) and high-rate performance (capacity retention rate = first-cycle discharge capacity at 10C / first-cycle capacity at the selected rate (1C), the test results are shown in Table 3).

[0047] Table 1 Average Coulomb Efficiency Table 2 Cycle Capacity Retention Rate of High Voltage Positive Electrode Half-Cell Table 3 Rate Test of High Voltage Positive Electrode Half-Cell As shown in Table 1, the results of Examples 1-14 and Comparative Examples 1 and 2 indicate that the electrolyte provided by the present invention has extremely high coulombic efficiency (average coulombic efficiency: 98.1%~99.9%) when used in sodium metal deposition half-cells, and its performance is significantly superior to that of commonly used carbonate electrolytes. Compared with Example 1, the volume ratio of high steric hindrance multi-coordination chelating solvent and low steric hindrance single-coordination ether solvent in Comparative Examples 3 and 4 is not within the range limited by the present invention, resulting in low sodium metal deposition efficiency and significantly lower sodium metal compatibility than in Example 1.

[0048] As shown in Table 2, the results of Examples 1-14 and Comparative Examples 1 and 2 indicate that the electrolyte provided by the present invention can be stably cycled in high-voltage cathode material half-cells, and the capacity retention rate (80.2%~96.8%) is significantly superior to that of commonly used carbonate electrolytes. Compared with Example 1, the volume ratio of high steric hindrance multi-coordination chelating solvent to low steric hindrance single-coordination ether solvent in Comparative Examples 3 and 4 exceeds the range defined by the present invention, resulting in a lower capacity retention rate of the high-voltage cathode material half-cell and significantly lower high-voltage performance than Example 1.

[0049] As shown in Table 3, the results of Examples 1-14 and Comparative Examples 1 and 2 indicate that the electrolyte provided by the present invention can cycle at high rates in high-voltage cathode material half-cells, and its capacity retention (60.5%~89.2%) is significantly superior to that of commonly used carbonate electrolytes. Compared with Example 1, when the volume ratio of high-steric hindrance multi-coordination chelating solvent to low-steric hindrance single-coordination ether solvent in Comparative Examples 3 and 4 exceeds the range defined by the present invention, the high-rate capacity retention is lower, and the high-rate performance is significantly lower than that of Example 1.

[0050] In summary, the electrolyte provided by this invention, based on an entropy-driven solvation structure regulation strategy, introduces a high-steric-hindrance multi-coordinate chelating solvent containing large-volume inert steric-hindrance groups. By utilizing the physical steric hindrance effect, the strong coordination solvent is repelled from the first solvation shell, forcing the low-steric-hindrance single-coordinate weak coordination ether solvent to spontaneously enter the inner shell, forming a physically confined weak coordination inner layer. This reduces the desolvation energy, promotes uniform sodium deposition, and inhibits dendrite formation. At the same time, it utilizes the high oxidation resistance brought by the intrinsically low HOMO energy level of the weak coordination solvent to improve the high-voltage stability of the electrolyte from the source.

[0051] The applicant declares that the present invention is illustrated by the above embodiments to demonstrate the electrolyte, its preparation method, and its application. However, the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An electrolyte, characterized in that, The electrolyte includes an organic solvent, a sodium salt, and additives; The organic solvent is a fluorine-free ether solvent, including highly sterically hindered multi-coordination chelating solvents and low sterically hindered single-coordination ether solvents; With the total volume of the high-steric-impedance multi-coordination chelating solvent and the low-steric-impedance monocoordination ether solvent being 100%, the volume ratio of the high-steric-impedance multi-coordination chelating solvent is 20%~40%, and the volume ratio of the low-steric-impedance monocoordination ether solvent is 60%~80%.

2. The electrolyte according to claim 1, characterized in that, The sterically hindered multi-coordination chelating solvent includes any one or a combination of at least two of the following: triethylene glycol diethyl ether, triethylene glycol dibutyl ether, triethylene glycol dipropyl ether, triethylene glycol ethyl methyl ether, triethylene glycol butyl methyl ether, triethylene glycol butyl ethyl ether, tripropylene glycol dimethyl ether, tripropylene glycol diethyl ether, tripropylene glycol dibutyl ether, tripropylene glycol dipropyl ether, tripropylene glycol ethyl methyl ether, tripropylene glycol butyl methyl ether, tripropylene glycol butyl ethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol dibutyl ether, tetraethylene glycol dipropyl ether, tetraethylene glycol ethyl methyl ether, tetraethylene glycol butyl methyl ether, and tetraethylene glycol propyl methyl ether.

3. The electrolyte according to claim 1 or 2, characterized in that, The low-steric hindrance monocoordinate ether solvent is selected from 1,3-dioxane, 4-methyl-1,3-dioxane, 4-ethyl-1,3-dioxane, 5-methyl-1,3-dioxane, 5-ethyl-1,3-dioxane, 4,4-dimethyl-1,3-dioxane, 4,4-diethyl-1,3-dioxane, 4-methyl-4-ethyl-1,3-dioxane, 5,5-dimethyl-1,3-dioxane, 5,5-diethyl-1,3-dioxane, 5-methyl-5-ethyl-1,3-dioxane, 4,5-dimethyl-1,3-dioxane, 4-ethyl-5-methyl-1,3-dioxane, 4,5-diethyl-1,3-dioxane, 4,6 -Dimethyl-1,3-dioxane, 4,6-diethyl-1,3-dioxane, 4-ethyl-6-methyl-1,3-dioxane, 4,4,5-trimethyl-1,3-dioxane, 4,4,6-trimethyl-1,3-dioxane, 4,5,6-trimethyl-1,3-dioxane, tetrahydropyran, 2-methyltetrahydropyran, 3-methyltetrahydropyran, 4-methyltetrahydropyran, 2,2-dimethyltetrahydropyran, 2,3-dimethyltetrahydropyran, 2,4-dimethyltetrahydropyran, 2,5-dimethyltetrahydropyran, 2,6-dimethyltetrahydropyran, 3,3-dimethyltetrahydropyran, 3,4-dimethyltetrahydropyran, 3,5-dimethyltetrahydropyran, 4,4-dimethyltetrahydropyran, any one or a combination of at least two of these.

4. The electrolyte according to any one of claims 1-3, characterized in that, The sodium salt includes any one or a combination of at least two of the following: sodium perchlorate, sodium tetraphenylborate, sodium nitrate, sodium bis(oxalato)borate, sodium tetraphenoxyborate, sodium hexafluorophosphate, sodium tetrafluoroborate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoroacetate, sodium difluorooxalatoborate, sodium bis(oxalato)borate, and sodium trifluoromethanesulfonate.

5. The electrolyte according to any one of claims 1-4, characterized in that, The concentration of sodium salt in the electrolyte is 0.3~2 mol / L, preferably 0.3~1.5 mol / L, and more preferably 0.5~1 mol / L.

6. The electrolyte according to any one of claims 1-5, characterized in that, The additive is a fluorine-free additive, including any one or a combination of at least two of tetravinylsilane, 1,3-propanesulfonyl lactone, vinyl sulfite, vinyl sulfate, tris(trimethylsilane) phosphate, trimethoxy(pentafluorophenyl)silane, and phenyltrivinylsilane.

7. The electrolyte according to any one of claims 1-6, characterized in that, Based on the total weight of the electrolyte (100%), the content of the additive is 0.05% to 1.5%, preferably 0.1% to 1%.

8. A method for preparing an electrolyte as described in any one of claims 1-7, characterized in that, The preparation method includes the following steps: The electrolyte is obtained by mixing an organic solvent, a sodium salt, and an additive.

9. A battery with an electroplated negative electrode metal, characterized in that, The electroplated negative electrode metal battery includes a positive electrode, a negative electrode, a separator, and an electrolyte as described in any one of claims 1-7.