Interface modification layer material for solid-state electrolyte and preparation method and application thereof
By reacting metallic lithium with nitrides to generate lithium-X alloy phase and lithium nitride phase composite materials, the problems of low impedance and simple preparation of oxide solid-state battery interface modification technology are solved, achieving efficient interface modification effect and industrial adaptation, and improving the cycle stability and discharge performance of the battery.
Patent Information
- Application Number
- CN202611182325.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-20
AI Technical Summary
Existing interface modification technologies cannot simultaneously achieve low interface impedance and simple and controllable preparation processes, and are difficult to adapt to industrial mass production. Interface problems in oxide solid-state batteries seriously affect the cycle stability of the batteries.
A specific ratio of metallic lithium reacts with nitrides to generate a composite material of lithium-X alloy phase and lithium nitride phase, forming a continuous interpenetrating mixed conductive permeation network, reducing interfacial charge transfer impedance, and improving interfacial contact and buffering volume changes through the synergistic effect of lithium-X alloy phase and lithium nitride phase.
It significantly reduces the interfacial impedance between the solid electrolyte and the lithium metal anode, improves the long-cycle stability of symmetrical batteries and the rate discharge performance of full batteries, and enables low-cost and easy industrial production.
Smart Images

Figure CN123143552A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of solid-state battery technology, and in particular to an interface modification layer material for solid-state electrolytes, its preparation method, and its application. Background Technology
[0002] Against the backdrop of global energy structure transformation and my country's "dual-carbon" strategy, high-safety, high-energy-density energy storage technologies have become a core research and development direction. Traditional liquid lithium-ion batteries rely on flammable organic electrolyte systems, which have inherent safety shortcomings such as thermal runaway and low-temperature performance degradation, making them unsuitable for the stringent requirements of high-safety energy storage devices in high-end equipment such as new energy vehicles and drones. Solid-state batteries, which replace traditional electrolytes and separators with solid electrolytes, can eliminate the risks of leakage, combustion, and explosion at the source, while also possessing higher theoretical energy density, making them the core technology route for next-generation energy storage batteries. Among existing solid-state electrolyte systems, oxide solid-state electrolytes have the potential for large-scale application due to their excellent ionic conductivity, wide electrochemical stability window, and good compatibility with lithium metal. However, key interface challenges exist between oxide electrolytes and lithium metal anodes, such as high solid-solid contact impedance, continuous interfacial side reactions, and lithium dendrite growth, which severely deteriorate battery cycle stability and restrict the practical application of oxide-based solid-state batteries. Therefore, efficient interface modification solutions are urgently needed to overcome these interface bottlenecks.
[0003] To address the aforementioned solid-solid interface defects, existing research has developed three main improvement methods: surface pretreatment, composite lithium anodes, and interface modification layers. However, each approach has significant technical shortcomings: First, surface treatment processes for lithium anodes, such as polishing and acid washing, can only temporarily remove the surface impurity passivation layer. Once the electrolyte / lithium anode re-exposes to air, the contamination layer quickly regenerates, leading to a rebound in interfacial impedance and a lack of long-term modification effectiveness. Second, composite lithium anode systems experience repeated volume expansion and contraction during long-term lithium deposition / stripping cycles, inducing microcracks within the electrode and continuously disrupting interfacial transport pathways, significantly shortening battery cycle life. Third, in-situ construction of interface modification layers is currently recognized as the most promising modification approach, capable of simultaneously achieving multiple functions such as interface bonding, accelerated lithium-ion conduction, and inhibition of lithium dendrites by controlling the interface layer composition. However, this route often involves stringent process conditions and is difficult to implement industrially. For example, Chinese patent application CN115548266A discloses a scheme for preparing a lithium anode modification layer by in-situ nitrogen nitridation. It relies on the reaction of metallic lithium with high-purity nitrogen to generate a dense lithium nitride interface layer, which takes into account both ion conduction and electronic insulation properties in a solid system. Although its resistance is low, the nitridation reaction in this scheme has extremely high requirements for nitrogen purity, gas flow rate, reaction temperature, and ambient water and oxygen content. The process is complex and the production threshold is high, making it difficult to adapt to low-cost, continuous industrial preparation scenarios.
[0004] In summary, there is an urgent need to develop a solid-state battery interface modification scheme with low interface impedance, mild and simple preparation conditions, and suitability for industrial mass production. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing interface modification technology, which cannot simultaneously achieve low interface impedance and simple and controllable preparation process, and to provide an interface modified material.
[0006] Another object of the present invention is to provide the application of the above-mentioned interface-modified materials in the preparation of solid electrolytes.
[0007] Another object of the present invention is to provide a modified solid electrolyte.
[0008] Another object of the present invention is to provide the application of the above-described modified solid electrolyte in the preparation of symmetrical batteries or full batteries.
[0009] Another object of the present invention is to provide a symmetrical battery.
[0010] Another object of the present invention is to provide a full battery.
[0011] Another object of the present invention is to provide a method for preparing the above-mentioned full cell.
[0012] The above-mentioned objective of this invention is achieved through the following technical solution: This invention protects an interface-modifying material, which is obtained by reacting metallic lithium with a nitride; The mass ratio of lithium metal to nitride is 10:(2~3).
[0013] To address the limitations of existing interface modification technologies in simultaneously achieving low interfacial impedance and simple, controllable processes, this invention introduces a specific ratio of metallic lithium and nitrides to in-situ generate a lithium-X alloy phase (where X is an element other than nitrogen in the nitride) and a lithium nitride phase composite material. Within this ratio range, the two phases form a continuous, interpenetrating, hybrid conductive permeation network, ensuring efficient spatial coupling of ion / electron dual-carrier transport channels, thereby significantly reducing interfacial charge transfer impedance. Furthermore, the two phases synergistically perform the following functions: firstly, they synergistically improve interfacial contact; the lithium-X alloy phase reduces the surface tension of the lithium phase, promoting uniform lithium spreading; and the lithium nitride phase provides continuous Li... + First, it optimizes both physical adhesion and ion conduction; second, it constructs a transport network and buffers volume changes, with the lithium-X alloy phase building a hybrid ion / electron conduction pathway and utilizing its tough framework to accommodate volume deformation; the lithium nitride phase enhances ion conduction and assists in supporting the interface structure; third, it synergistically suppresses lithium dendrites, with the lithium-X alloy phase inducing uniform lithium nucleation and the lithium nitride phase homogenizing the interface Li... + Flux, both regulate dendrite growth throughout the entire process from nucleation to deposition.
[0014] Furthermore, the nitride includes one or more of gallium nitride, aluminum nitride, indium nitride, titanium nitride, magnesium nitride, calcium nitride, and silicon nitride.
[0015] Furthermore, the nitride is gallium nitride.
[0016] Furthermore, the atmosphere for the reaction is argon.
[0017] Furthermore, the reaction temperature is 280~320 °C.
[0018] Furthermore, the reaction time is 10-30 min.
[0019] This invention protects the application of the above-mentioned interface-modified materials in the preparation of solid electrolytes.
[0020] This invention protects a modified solid electrolyte, comprising a solid electrolyte and the aforementioned interface modification material.
[0021] Furthermore, the solid electrolyte is an oxide electrolyte.
[0022] Furthermore, the oxide electrolyte includes Li 6.5 La3Zr 1.5 Ta 0.5 O 12 Li7La3Zr2O 12 Li 1.3 A l0.3 Ti 1.7 (PO4)3, Li 0.33 La 0.56 One or more of TiO3.
[0023] Furthermore, the thickness of the interface-modified material is 10~30 μm.
[0024] This invention protects the preparation method of the aforementioned modified solid electrolyte, comprising the following steps: The aforementioned interface modification material is uniformly coated on one side of the solid electrolyte and cooled to obtain the modified solid electrolyte.
[0025] The preparation process of this invention is simple and easy to implement, requiring no nitriding reaction and no strict control over process parameters such as nitrogen purity and gas flow rate. The difficulty of process control is greatly reduced, and it has the advantages of low cost and easy continuous industrial production.
[0026] This invention protects the application of the above-mentioned modified solid electrolyte in the preparation of symmetrical batteries or full batteries.
[0027] This invention protects a symmetrical battery, comprising a lithium electrode and a solid electrolyte, wherein the solid electrolyte comprises the aforementioned modified solid electrolyte.
[0028] Furthermore, the lithium electrode is a lithium metal sheet.
[0029] Furthermore, the method for preparing the symmetrical battery includes the following steps: The aforementioned interface modification material is coated on the other side of the aforementioned modified solid electrolyte and cooled to obtain a solid electrolyte with interface modification material coated on both sides. Then, lithium electrodes are attached to both sides of the electrolyte and assembled to obtain a symmetrical battery.
[0030] This invention protects a full battery comprising a positive electrode, a negative electrode, and a solid electrolyte, wherein the solid electrolyte comprises the aforementioned modified solid electrolyte.
[0031] Furthermore, the positive electrode includes a current collector and a positive electrode active material loaded on the current collector.
[0032] Furthermore, the current collector includes one or more of aluminum foil, carbon paper, and nickel foam.
[0033] Furthermore, the positive electrode active material includes any one of polyanionic materials, layered oxide materials, and spinel oxide materials.
[0034] Preferably, the polyanionic material includes one or more of lithium iron phosphate, lithium manganese iron phosphate, and lithium vanadium phosphate.
[0035] Furthermore, the layered oxide material is a transition metal layered oxide.
[0036] Preferably, the transition metal layered oxide includes one or more of lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide, a lithium-rich manganese-based material.
[0037] Preferably, the spinel oxide material includes one or more of lithium manganese oxide, lithium nickel manganese oxide, and lithium cobalt manganese oxide.
[0038] More preferably, the positive electrode active material is lithium iron phosphate.
[0039] Furthermore, the negative electrode includes any one of pure lithium negative electrode, lithium alloy negative electrode, carbon-based negative electrode, silicon-based negative electrode, tin-based negative electrode, phosphorus-based negative electrode, transition metal oxide negative electrode, and transition metal dichalcogenide negative electrode.
[0040] Furthermore, the lithium alloy anode includes one or more of lithium indium alloy, lithium silver alloy, lithium aluminum alloy, and lithium tin alloy.
[0041] Furthermore, the carbon-based anode includes one or more of graphite, hard carbon, soft carbon, carbon nanotubes, and graphene.
[0042] Furthermore, the silicon-based anode includes one or more of elemental silicon, silicon-carbon composite materials, and silicon oxide.
[0043] Furthermore, the tin-based anode comprises one or more of elemental tin, tin oxide, and tin alloy phases.
[0044] Furthermore, the phosphorus-based negative electrode includes one or more of black phosphorus, nickel phosphide, and iron phosphide.
[0045] Furthermore, the transition metal oxide anode includes one or more of iron-based oxides, cobalt-based oxides, manganese-based oxides, titanium-based oxides, and bimetallic composite oxides.
[0046] Furthermore, the transition metal dichalcogenides include one or more of transition metal sulfides, transition metal selenides, and transition metal tellurides.
[0047] Preferably, the negative electrode is a pure lithium negative electrode.
[0048] Furthermore, the full battery also includes an electrolyte.
[0049] Furthermore, the electrolyte comprises one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and ethylene carbonate.
[0050] Preferably, the volume of the electrolyte is 5~20 µL.
[0051] This invention protects the aforementioned method for preparing a full battery, comprising the following steps: The negative electrode is attached to the side of the modified solid electrolyte with the interface modification material, and the positive electrode is attached to the other side. After assembly, a full cell is obtained.
[0052] Furthermore, the method for preparing the positive electrode includes the following steps: The positive electrode active material, conductive agent, and binder are dispersed in a dispersant to obtain a positive electrode slurry, which is then coated onto a current collector. After drying, the positive electrode is obtained.
[0053] Furthermore, the conductive agent is carbon black.
[0054] Furthermore, the adhesive includes one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose, and sodium alginate.
[0055] Preferably, the mass ratio of the positive electrode active material, conductive agent, and binder is (7.5~8.5):1:1.
[0056] More preferably, the mass ratio of the positive electrode active material, the conductive agent, and the binder is 8:1:1.
[0057] Furthermore, the dispersant is N-methylpyrrolidone.
[0058] Furthermore, the current collector includes one or more of aluminum foil, carbon paper, and nickel foam.
[0059] Furthermore, the drying temperature is 60~100 ℃.
[0060] Furthermore, the drying time is 6 to 16 hours.
[0061] Compared with the prior art, the present invention has the following beneficial effects: This invention provides an interface-modified material obtained by reacting lithium metal with a nitride, wherein the mass ratio of lithium metal to nitride is 10:(2~3). Modified solid-state electrolytes can be prepared by using this interface-modified material to modify solid-state electrolytes. The interface-modified material exhibits excellent compatibility and wettability with the solid-state electrolyte, significantly reducing the interfacial impedance between the solid-state electrolyte and the lithium metal anode, while substantially improving the long-cycle stability of symmetrical batteries. Solid-state full batteries assembled based on this modified solid-state electrolyte possess both excellent rate discharge performance and long-cycle stability. The interface-modified material of this invention can achieve ultra-low interfacial impedance under mild preparation conditions, combining the advantages of both electrochemical performance and industrial-scale preparation. Attached Figure Description
[0062] Figure 1 The image shows the XRD pattern of the interface-modified material in Example 1.
[0063] Figure 2 This is a schematic diagram of the wettability of the modified solid electrolyte in Example 1.
[0064] Figure 3 This is a SEM image of the interface of the modified solid electrolyte in Example 1.
[0065] Figure 4 The electrochemical impedance spectroscopy results are shown for the symmetrical cells in Examples 1-2 and Comparative Examples 1-2.
[0066] Figure 5 This is a cycle test diagram of the symmetrical battery in Example 1.
[0067] Figure 6 This is a cycle test diagram of the symmetrical battery in Example 2.
[0068] Figure 7 This is a cyclic test diagram of the symmetrical battery in Comparative Example 1.
[0069] Figure 8 This is a cyclic test diagram of the symmetrical battery in Comparative Example 2.
[0070] Figure 9This is a graph showing the step cycle performance of the full cell at different rates in Example 1.
[0071] Figure 10 The graphs show the charge-discharge curves of the full battery at different rates in Example 1.
[0072] Figure 11 The graph shows the cycle performance test curves of the full battery in Example 1. Detailed Implementation
[0073] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.
[0074] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.
[0075] Example 1: Preparation of interface-modified materials, modified solid electrolytes, symmetric cells, and full cells. 1. Preparation of interface-modified materials Under an argon atmosphere, gallium nitride and lithium metal were mixed at a mass ratio of 3:10, and the mixture was heated to 300 °C to melt the lithium metal. The lithium metal was then continuously stirred and mixed with gallium nitride and allowed to react fully for 20 min to obtain the interface-modified material.
[0076] 2. Preparation of modified solid electrolytes The aforementioned molten interface modification material was coated onto the solid electrolyte sheet Li. 6.5 La3Zr 1.5 Ta 0.5 O 12 After cooling to room temperature, a modified solid electrolyte with a 25 μm interface modified material loaded on one side is obtained. 3. Preparation of symmetric cells The aforementioned molten interface modification material was coated on the other side of the aforementioned modified solid electrolyte sheet. After cooling to room temperature, a solid electrolyte sheet with 25 μm of interface modification material loaded on both sides was obtained. Subsequently, lithium metal sheets were attached to both sides of the sheet, and the symmetrical battery was assembled.
[0077] 4. Preparation of full cells S1. Lithium iron phosphate, carbon black, and PVDF are thoroughly mixed in a mass ratio of 8:1:1 to prepare a positive electrode slurry; the positive electrode slurry is coated onto aluminum foil, dried at 60 ℃ for 2 h, and then placed in a vacuum oven for continuous drying for 12 h to obtain a positive electrode sheet; S2. Attach the lithium metal negative electrode to the side of the modified solid electrolyte sheet with the interface modification material, drop 10 µL of lithium hexafluorophosphate onto the other side of the solid electrolyte sheet, and then attach the positive electrode sheet obtained in step S1 to that side. After assembly, a solid lithium metal full cell is obtained.
[0078] Example 2: Preparation of interface-modified materials, modified solid electrolytes, symmetric cells, and full cells. The difference from Example 1 is that in the preparation step of the interface modified material, the mass ratio of gallium nitride to lithium metal is adjusted from 3:10 to 2:10.
[0079] The other steps and conditions are the same as in Example 1.
[0080] Example 3: Preparation of interface-modified materials, modified solid electrolytes, symmetric cells, and full cells. The difference from Example 1 is that in the preparation step of the interface modified material, the mass ratio of gallium nitride to lithium metal is adjusted from 3:10 to 2.5:10.
[0081] The other steps and conditions are the same as in Example 1.
[0082] Comparative Example 1: Preparation of interface-modified materials, modified solid electrolytes, symmetric cells, and full cells. The difference from Example 1 is that in the preparation step of the interface modified material, the mass ratio of gallium nitride to lithium metal is adjusted from 3:10 to 4:10.
[0083] The other steps and conditions are the same as in Example 1.
[0084] Comparative Example 2: Preparation of interface-modified materials, modified solid electrolytes, symmetric cells, and full cells. The difference from Example 1 is that the solid electrolyte was not modified. The specific steps are as follows: 1. Preparation of symmetric cells: A symmetrical battery is obtained by attaching lithium metal sheets to both sides of an unmodified solid electrolyte sheet and assembling them.
[0085] 2. Preparation of full cells: S1. Lithium iron phosphate, carbon black, and PVDF are thoroughly mixed in a mass ratio of 8:1:1 to prepare a positive electrode slurry; the positive electrode slurry is coated onto aluminum foil, dried at 60 ℃ for 2 h, and then placed in a vacuum oven for continuous drying for 12 h to obtain a positive electrode sheet; S2. Attach the lithium metal negative electrode to one side of a solid electrolyte sheet on which 10 µL of lithium hexafluorophosphate has been dropped. Similarly, drop 10 µL of lithium hexafluorophosphate onto the other side of the solid electrolyte sheet. Then attach the positive electrode sheet obtained in step S1 to that side. After assembly, a solid lithium metal full cell is obtained.
[0086] Experimental Example 1: Structural Characterization of Interface-Modified Materials and Modified Solid Electrolytes The interface-modified material in Example 1 was characterized by XRD using a Bruker D8 ADVANCE instrument, and the results are as follows: Figure 1 As shown, the XRD pattern not only detected the characteristic diffraction peaks of metallic lithium, but also clearly revealed the characteristic peaks of new phases such as Li2Ga and Li3N. The results demonstrate that metallic lithium and gallium nitride undergo an interfacial chemical reaction during the preparation of the interface-modified material, generating the Li2Ga alloy phase and Li3N in situ, thus successfully constructing a multiphase composite interface-modified material.
[0087] The wettability of the modified solid electrolyte in Example 1 was characterized by visual inspection combined with a HITACHI SU5000S scanning electron microscope (SEM). The results... Figures 2-3 As shown, the lithium-gallium nitride interface modified material adheres tightly to the solid electrolyte matrix, with no obvious gaps or delamination defects at the interface, exhibiting excellent interface wettability.
[0088] Experimental Example 2: Performance Characterization of Symmetric Cells 1. Experimental Methods Electrochemical impedance spectroscopy (EIS): By measuring the impedance response of a system to an AC signal, the real, imaginary, and phase components of the impedance, as well as the phase variation with frequency, are obtained. This leads to the Nyquist and Bode plots, which are used to analyze electrode process kinetics, interfacial characteristics, and charge transport behavior. The frequency range of this experiment is 10 Hz. 7 -1 Hz, the symmetrical cells in Examples 1-2 and Comparative Examples 1-2 were tested to obtain the interface resistance; Cyclic Testing: Long-term cycle testing of the battery was conducted at room temperature using the Blue Electric CT3001A electrochemical testing system. The test employed a constant current mode with a fixed lithium deposition / stripping surface capacity, allowing continuous reversible lithium plating and deintercalation processes to occur on the lithium metal surface. The battery interface cycle stability was evaluated by monitoring the polarization voltage, voltage plateau stability, and cycle life evolution of the symmetrical battery over a long period. Test conditions: Current density 0.1 mA cm⁻² -2 Lithium deposition / stripping surface capacity: 0.05 mAh / cm³ -2 The symmetric cells of Examples 1-2 and Comparative Examples 1-2 were tested at room temperature to characterize the cycle stability of each system.
[0089] 2. Experimental Results Depend on Figure 4 The interface impedance test results show that the interface resistance of the symmetrical cell in Example 1 is 8.8 Ω cm. 2 In Example 2, the interfacial resistance of the symmetrical cell is 9.4 Ω cm.2 In contrast, in Comparative Example 1, due to the excessive addition of gallium nitride, the excess Li2Ga alloy phase agglomerated, disrupting the continuity of the ion / electron mixed conduction percolation network and causing spatial mismatch in the dual carrier transport channels, resulting in an increase in interfacial resistance to 23.9 Ω cm. 2 In Comparative Example 2, due to the lack of interface modification materials, a large porosity exists between the solid electrolyte and the lithium negative electrode, resulting in a significant increase in interfacial resistance to 332.36 Ω cm. 2 .
[0090] Symmetrical battery constant current cycling performance such as Figures 5-8 As shown, at 0.1 mA cm -2 At the current density, the symmetrical cells in Examples 1-2 can all be stably cycled for 1000 h ( Figures 5-6 Under the same test conditions, Comparative Example 1 could only be stably cycled for 700 h ( ); Figure 7 Comparative Example 2 showed a significant performance degradation, with a cycle stability time of only about 20 hours. Figure 8 The above results indicate that lithium metal and gallium nitride need to be mixed in a specific ratio to obtain low interface resistance and achieve long-term stable cycling of symmetrical cells; adding too much gallium nitride or not setting this modified interface will cause a surge in interface resistance and a significant decrease in cycle life.
[0091] The performance of the symmetrical battery in Example 3 is basically the same as that in Example 2, and will not be described again here.
[0092] Experimental Example 3: Performance Characterization of a Full Cell 1. Experimental Methods Discharge specific capacity: Obtained through isothermal charge-discharge testing, it is defined as the amount of electricity released by the actual extraction of lithium ions per unit mass (or unit area) of active material during discharge. After the test, the instrument software directly outputs this value, ranging from mAh to g. -1 By comparing the changes in discharge specific capacity at different cycle counts, the structural stability and degree of interfacial side reactions of the material can be evaluated. Stable and high discharge specific capacity indicates excellent reversible lithium-ion insertion / extraction capability of the material; rapid decay of discharge specific capacity during cycling indicates structural collapse, severe interfacial side reactions, or loss of active lithium due to lithium dendrite formation.
[0093] Coulombic efficiency: Coulombic efficiency is calculated as the ratio of discharge specific capacity to charge specific capacity in the same cycle, i.e.: Coulombic efficiency (%) = (Discharge specific capacity / Charge specific capacity) × 100%. This value is automatically calculated and output by the test system for each cycle. By monitoring the trend of coulombic efficiency with the number of cycles, the stability of the electrode / electrolyte interface and the loss of active lithium can be evaluated. High and stable coulombic efficiency means a stable electrode / electrolyte interface, low loss of active lithium, and excellent long-cycle potential of the material.
[0094] 2. Experimental Results like Figure 9 As shown, with the increase of charge / discharge rate, the battery polarization gradually increases, the discharge voltage plateau shifts slightly downward, and the discharge specific capacity shows a downward trend. When the charge / discharge rate drops back to 0.1C, the discharge specific capacity can significantly rebound, and throughout the entire test range, the battery coulombic efficiency remains at a high level with small fluctuations. Furthermore, as... Figure 10 As shown, the full cell prepared in Example 1 was tested at current densities of 0.1C, 0.2C, 0.3C, 0.4C, and 0.5C, and the discharge specific capacity reached 148.45 mAh g⁻¹, respectively. -1 138.49 mAh g -1 123.50 mAh g -1 119.21 mAh g -1 and 124.61 mAh g -1 At a relatively high rate of 0.5C, the battery still maintains a considerable discharge capacity, indicating that the interface modification material constructed in this invention effectively reduces interfacial impedance, improves charge transport dynamics, and gives the battery excellent rate adaptability. Furthermore, the capacity recovery after rate restoration also indicates that the above results demonstrate that the capacity decay under high-rate conditions mainly stems from electrochemical polarization, and that irreversible structural damage and continuous interface degradation have not occurred.
[0095] See the results of the cyclic performance test. Figure 11 The full cell can be stably cycled for 200 cycles at a current density of 0.5C, maintaining 88.8% of its initial capacity. The capacity decay is gradual under long-term cycling, which confirms the stability of the electrode / electrolyte interface, low loss of active lithium, and the excellent long-term cycling stability of the material.
[0096] The performance of the full cells in Examples 2 and 3 is basically the same as that in Example 1, and will not be described again here.
[0097] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. An interface-modified material, characterized in that, The interface-modifying material is obtained by reacting metallic lithium with nitrides; The mass ratio of lithium metal to nitride is 10:(2~3).
2. The interface-modified material according to claim 1, characterized in that, The nitrides include one or more of gallium nitride, aluminum nitride, indium nitride, titanium nitride, magnesium nitride, calcium nitride, and silicon nitride.
3. The application of the interface-modified material according to claim 1 or 2 in the preparation of solid electrolytes.
4. A modified solid electrolyte, characterized in that, It includes solid electrolytes and interface-modified materials as described in claim 1 or 2.
5. The modified solid electrolyte according to claim 4, characterized in that, The thickness of the interface-modified material is 10~30 μm.
6. The method for preparing the modified solid electrolyte according to claim 4 or 5, characterized in that, Includes the following steps: The interface modification material described in claim 1 or 2 is uniformly coated on one side of the solid electrolyte and cooled to obtain the modified solid electrolyte.
7. The application of the modified solid electrolyte according to claim 4 or 5 in the preparation of symmetrical cells or full cells.
8. A symmetrical battery, characterized in that, It includes a lithium electrode and a solid electrolyte, wherein the solid electrolyte includes the modified solid electrolyte of claim 4 or 5.
9. A full battery, characterized in that, It includes a positive electrode, a negative electrode, and a solid electrolyte, wherein the solid electrolyte includes the modified solid electrolyte as described in claim 4 or 5.
10. The method for preparing the full cell according to claim 9, characterized in that, Includes the following steps: The negative electrode is attached to the side of the modified solid electrolyte described in claim 4 or 5 that has an interface modification material, and the positive electrode is attached to the other side. After assembly, a full cell is obtained.
Citation Information
Patent Citations
Modified lithium metal, lithium metal interface modification method and all-solid-state battery
CN115548266A