A method for recycling waste plastics and retired lithium ion battery positive electrode materials in cooperation with pyrolysis

By synergistically pyrolyzing retired lithium-ion battery cathode materials and oxygen-containing plastics, we have achieved efficient recycling and high-value conversion of metals such as lithium, cobalt, nickel, and manganese. This solves the problems of high energy consumption, serious pollution, and difficulty in resource utilization in existing technologies, and provides an environmentally friendly and efficient resource utilization method.

CN123143573APending Publication Date: 2026-11-20UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611655023.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, the recycling methods for retired lithium-ion batteries are characterized by complex processes, high energy consumption, secondary pollution, toxic plastic pyrolysis byproducts, high cost of plastic resource recycling, and difficulty in achieving efficient recycling and high-value conversion of metals such as lithium, cobalt, nickel, and manganese.

Method used

A synergistic pyrolysis method is used to mix retired lithium-ion battery cathode materials with oxygen-containing plastics and pyrolyze them in a protective atmosphere to generate pyrolysis oil and residual solids. These are then mixed with water for leaching to obtain leachate and leach residue. Through drying and high-temperature calcination, the efficient recovery of metals such as lithium, cobalt, nickel, and manganese is achieved, and high-value chemicals are produced in the same way.

Benefits of technology

The process achieves efficient recovery of metals such as lithium, cobalt, nickel, and manganese under medium and low temperature conditions, reducing energy and chemical consumption, generating high-value pyrolysis oil. The process is simple and environmentally friendly, with a metal recovery rate of >97%, a pyrolysis oil yield of >48%, and good product selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143573A_ABST
    Figure CN123143573A_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of resource recycling, and particularly relates to a method for recycling waste plastics and retired positive electrode materials of lithium ion batteries by synergistic pyrolysis. Compared with the prior art, the method provided by the present application utilizes the synergistic effect of the interface chemistry of the plastic and the positive electrode material to realize the depolymerization of the plastic and the decomposition of the retired positive electrode material of the lithium ion battery under low-temperature conditions, without the need for external acid, alkali or exogenous reducing agent, so as to realize the efficient recovery of lithium, cobalt, nickel, manganese and other elements, simultaneously produce high-value pyrolysis oil (such as phenol, lactide and the like), and complete the collaborative recovery of metals and hydrocarbon resources. Compared with the traditional wet or pyrometallurgical method, the method has a short process, mild conditions and no additional reagents, so that the energy consumption and reagent consumption are greatly reduced, and the whole reaction process is environmentally friendly and safe to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of resource recycling technology, and in particular relates to a resource recovery method for synergistic pyrolysis recycling of waste plastics and retired lithium-ion battery cathode materials. Background Technology

[0002] With the rapid development of renewable energy and the consumer electronics industry, the disposal of retired lithium-ion batteries has become a significant challenge. The resource recycling of retired lithium-ion batteries (S-LIBs), specifically the recovery of their lithium, cobalt, nickel, and manganese metal resources, is crucial for protecting the ecological environment and ensuring a sustainable supply of metal raw materials. However, commonly used hydrometallurgical and pyrometallurgical methods for recycling retired lithium-ion batteries generally suffer from drawbacks such as complex processes, high energy and chemical consumption, and secondary pollution. Co-pyrolysis using waste plastics as an auxiliary reducing agent can alleviate these problems to some extent. The in-situ generation of reducing gases such as CO, CH4, and C2H4 during plastic pyrolysis can promote the reduction of metal oxides, thereby accelerating electrode disintegration and metal release, and reducing reaction temperature and energy consumption. However, this co-pyrolysis process still requires a long reaction time, and the pyrolysis of plastics also generates toxic and harmful byproducts such as aromatic hydrocarbons and produces carbon deposits, leading not only to secondary pollution but also a decrease in the purity of the recovered metal products.

[0003] On the other hand, the high-value resource utilization of waste plastics is also a major current demand. Polycarbonate (PC), polyethylene terephthalate (PET), and polylactic acid (PLA) are three typical oxygen-containing plastics. PC has high mechanical strength and thermal stability, and is often used as the casing, structural component, and new energy vehicle parts for electronic products; PET is widely used in beverage bottles and packaging materials; and PLA, as a biodegradable plastic, is increasingly widely used in packaging, textiles, and other fields. Therefore, lithium-ion batteries often coexist with PC, PET, and PLA plastics in various electronic products and consumer goods. These plastics can be pyrolyzed to obtain chemicals such as phenols, aromatic hydrocarbons, and lactide, as well as fuel gases, but the complex composition of the products and the high cost of subsequent separation limit their resource recycling. Summary of the Invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a resource utilization method for the synergistic pyrolysis recycling of waste plastics and retired lithium-ion battery cathode materials. This method utilizes the complementary characteristics of these two types of waste to achieve their efficient synergistic conversion. Under mild conditions without the addition of external chemical reagents, it achieves the efficient recovery of key metals such as lithium, cobalt, nickel, and manganese, as well as the high-value conversion of plastics such as PC, PET, and PLA. Thus, it provides a new technical approach for the synergistic low-carbon and high-value resource utilization of these two types of waste.

[0005] This invention provides a method for the resource recovery of waste plastics and retired lithium-ion battery cathode materials through synergistic pyrolysis, comprising the following steps: S1) The cathode material of a retired lithium-ion battery is mixed with plastic to obtain a mixed powder; the plastic contains oxygen. S2) In a protective atmosphere, the mixed powder is pyrolyzed to obtain pyrolysis oil and residual solids; S3) Mix the residual solid with water, stir and leach to obtain leachate and leach residue; S4) The leachate is dried to obtain lithium carbonate.

[0006] Preferred options also include: S5) The leaching residue is mixed with lithium carbonate and calcined at high temperature to obtain the cathode material.

[0007] Preferably, the retired lithium-ion battery cathode material is selected from retired lithium cobalt oxide cathode materials, retired lithium manganese oxide cathode materials, or retired ternary lithium cathode materials; And / or, the plastic is selected from one or more of polycarbonate, polyethylene terephthalate and polylactic acid.

[0008] Preferably, the particle size of the plastic and the cathode material of the retired lithium-ion battery are each independently less than 100 μm; And / or, the mass ratio of the plastic to the retired lithium-ion battery cathode material is 1:1 to 1:3; And / or, the retired ternary lithium cathode material is lithium nickel cobalt manganese oxide material, whose general formula can be represented as LiNi x Co y Mn z O2, where x+y+z=1.

[0009] Preferably, the retired lithium-ion battery cathode material is a retired lithium cobalt oxide cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material is 1:1.5 to 1:2; Alternatively, the retired lithium-ion battery cathode material may be a retired lithium manganese oxide cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material may be 1:1.5 to 1:2. Alternatively, the retired lithium-ion battery cathode material may be a retired ternary lithium cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material may be 1:1 to 1:2.

[0010] Preferably, the pyrolysis temperature is 300℃~600℃; and the pyrolysis time is 0.5~6 h.

[0011] Preferably, the solid-liquid ratio of the residual solid to water is 1 g: (15~25) mL; And / or, the temperature of the stirring leaching is 30℃~50℃; the stirring speed of the stirring leaching is 100~500 rpm; and the stirring leaching time is 1~3 h.

[0012] Preferably, the method for mixing the leaching residue with lithium carbonate is ball milling; the ball milling speed is 200~800 rpm; and the ball milling time is 4~24 h. And / or, the high-temperature calcination temperature is 800℃~1000℃; the high-temperature calcination time is 10~24 h.

[0013] Preferably, the leaching residue is first heated in a steam atmosphere to carry out a decarbonization reaction to obtain syngas and solid products; then the solid products are mixed with lithium carbonate and calcined at high temperature to obtain the cathode material.

[0014] Preferably, the decarbonization reaction temperature is 700℃~900℃; the decarbonization reaction time is 0.5~2 h.

[0015] Preferably, the retired lithium-ion battery cathode material is obtained according to the following method: After the retired lithium-ion batteries are fully discharged, the positive electrode current collector, negative electrode current collector, and shell material are removed by crushing and physical sorting methods, and then sieved to obtain the positive electrode material of the retired lithium-ion batteries.

[0016] Compared with existing technologies, the resource recovery method provided by this invention utilizes the synergistic effect of interfacial chemistry between plastics and cathode materials to achieve plastic depolymerization and decomposition of retired lithium-ion battery cathode materials under medium and low temperature conditions. Furthermore, the entire process requires no external acids, alkalis, or exogenous reducing agents, simultaneously achieving efficient recovery of elements such as lithium, cobalt, nickel, and manganese, while also co-producing high-value pyrolysis oils (such as phenol and lactide), thus completing the synergistic recovery of metals and hydrocarbon resources. Compared with traditional hydrometallurgical or pyrometallurgical methods, this method has a shorter process, milder conditions, and requires no external reagents, significantly reducing energy and reagent consumption. Moreover, the entire reaction process is environmentally friendly and safe to operate.

[0017] Experimental results show that the resource recovery method provided by this invention can recover >97% of metals such as lithium, cobalt, and nickel, with a pyrolysis oil yield of >48% and a phenol selectivity of >87% (for PC plastics). For PET and PLA plastics, it can also achieve efficient recovery of metals such as lithium, cobalt, nickel, and manganese, and co-produce high-value chemicals such as aromatic hydrocarbons and lactide. Attached Figure Description

[0018] Figure 1 A schematic diagram of the coordination structure between PC plastic and lithium cobalt oxide; Figure 2 A schematic diagram of the Li-O bond breaking energy barrier in lithium cobalt oxide after coordination with PC; Figure 3 This is a schematic diagram of the fixed-bed pyrolysis reactor used in the pyrolysis of this invention; Figure 4 A schematic flowchart illustrating a specific method for the resource recovery of waste plastics and retired lithium-ion battery cathode materials through synergistic pyrolysis, provided by this invention. Figure 5 The image shown is a GC-MS image of the pyrolysis oil collected in Example 1 of this invention. Figure 6 The above are XRD patterns of lithium carbonate recovered in Examples 1, 3 and 4 of this invention. Figure 7 The image shows the XRD pattern of the regenerated lithium cobalt oxide cathode material obtained in Example 1 of this invention. Figure 8 This is a composition diagram of the synthesis gas obtained in Example 2 of the present invention; Figure 9 The image shows the XRD pattern of the recycled ternary lithium cathode material obtained in Example 3 of this invention. Figure 10 The image shows the XRD pattern of the regenerated lithium manganese oxide cathode material obtained in Example 4 of this invention. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0020] This invention provides a method for the resource recovery of waste plastics and retired lithium-ion battery cathode materials through synergistic pyrolysis, comprising the following steps: S1) mixing retired lithium-ion battery cathode materials with plastics to obtain a mixed powder; wherein the plastics contain oxygen; S2) pyrolyzing the mixed powder in a protective atmosphere to obtain pyrolysis oil and residual solids; S3) mixing the residual solids with water and stirring to leach, thereby obtaining a leachate and leach residue; S4) drying the leachate to obtain lithium carbonate.

[0021] In this invention, there are no special restrictions on the source of any raw materials; they can be commercially available.

[0022] In one specific embodiment of the present invention, the retired lithium-ion battery cathode material is preferably a retired lithium cobalt oxide cathode material (LCO), a retired lithium manganese oxide cathode material (LMO), or a retired ternary lithium cathode material (NCM / NCA).

[0023] In one specific embodiment of the present invention, the decommissioned ternary lithium cathode material is lithium nickel cobalt manganese oxide, which can be represented by the general formula LiNi. x Co y Mn z O2, where x+y+z=1; more specifically, x is preferably 0.3~0.9, more preferably 0.6~0.9; y is preferably 0.05~0.33, more preferably 0.05~0.2.

[0024] In one specific embodiment of the present invention, the decommissioned ternary lithium cathode material is LiNi. 0.8 Co 0.1 Mn 0.1 O2.

[0025] In one specific embodiment of the present invention, the particle size of the retired lithium-ion battery cathode material is preferably less than 100 μm, more preferably less than or equal to 80 μm, and even more preferably less than or equal to 74 μm.

[0026] In a specific embodiment of the present invention, the retired lithium-ion battery positive electrode material is preferably obtained by the following method: after the retired lithium-ion battery is fully discharged, the positive electrode current collector, negative electrode current collector, and shell material are removed by crushing and physical sorting methods, and then sieved to obtain the retired lithium-ion battery positive electrode material; the retired lithium-ion battery is preferably fully discharged by immersing it in a sodium chloride solution; the mass concentration of the sodium chloride solution is preferably 5% to 10%; the immersion time is preferably 36 to 60 h, more preferably 40 to 55 h, and even more preferably 48 h; the physical sorting method includes, but is not limited to, magnetic separation, flotation, etc.; the mesh size of the sieve used for sieving is preferably 200 mesh.

[0027] In one specific embodiment of the present invention, the plastic can be any oxygen-containing plastic well known to those skilled in the art, without any special limitations. More preferably, it includes ester bonds and / or carbonate bonds, and even more preferably, it includes, but is not limited to, one or more of polycarbonate (PC), polyethylene terephthalate (PET), and polylactic acid (PLA).

[0028] In one specific embodiment of the present invention, the plastic is preferably waste plastic.

[0029] In one specific embodiment of the present invention, the particle size of the plastic is preferably less than 100 μm, more preferably less than or equal to 80 μm, and even more preferably less than or equal to 74 μm.

[0030] The cathode material of retired lithium-ion batteries is mixed with plastic to obtain a mixed powder; the mass ratio of the plastic to the cathode material of retired lithium-ion batteries is preferably 1:0.5 to 1:5, more preferably 1:1 to 1:3; optionally, the mass ratio of the plastic to the cathode material of retired lithium-ion batteries is 1:1, 1:1.25, 1:1.5, 1:1.75, 1:2, 1:2.5, 1:3 or any two of the above values; the mixing method is preferably grinding.

[0031] In one specific embodiment of the present invention, the retired lithium-ion battery cathode material is a retired lithium cobalt oxide cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material is preferably 1:1.5 to 1:2, more preferably 1:1.75.

[0032] In one specific embodiment of the present invention, the retired lithium-ion battery cathode material is a retired lithium manganese oxide cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material is preferably 1:1.5 to 1:2, more preferably 1:2.

[0033] In one specific embodiment of the present invention, the retired lithium-ion battery cathode material is a retired ternary lithium cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material is preferably 1:1 to 1:2, more preferably 1:2.

[0034] In a protective atmosphere, the mixed powder is pyrolyzed to obtain pyrolysis oil and residual solids. The protective atmosphere can be any atmosphere known to those skilled in the art and is not particularly limited; in this invention, nitrogen, helium, and argon are preferred. The pyrolysis temperature is preferably 300℃~600℃; optionally, the pyrolysis temperature is 300℃, 350℃, 400℃, 450℃, 500℃, 520℃, 550℃, 580℃, 600℃, or any range between two of the above values. The pyrolysis time, i.e., the holding time, is preferably 0.5~6 h; optionally, the pyrolysis time is 0.5 h, 1 h, 1.5 h, 3 h, 4.5 h, 6 h, or any range between two of the above values. After pyrolysis, the volatile products are condensed to obtain pyrolysis oil; the residual solids are cooled to room temperature with the furnace. This invention utilizes the interfacial coordination effect between C–O and / or C=O groups in the plastic molecular chain and Li sites on the surface of the cathode material to simultaneously promote lithium release from the cathode material and the breaking of C–O bonds in the plastic backbone, achieving deep destructive processing of the cathode material and highly selective depolymerization of the plastic at approximately 500°C. The coordination configurations of LCO and PC are as follows: Figure 1 As shown, the energy barrier for Li-O bond breaking in LCO after coordination is as follows: Figure 2 As shown. The CO2 generated in situ from the depolymerization of plastics can react with Li... +The reaction generates stable Li2CO3, achieving directional lithium fixation.

[0035] In a specific embodiment of the present invention, the pyrolysis is preferably carried out in a fixed-bed pyrolysis reactor; a schematic diagram of the fixed-bed pyrolysis reactor is shown below. Figure 3 As shown.

[0036] In one specific embodiment of the present invention, the plastic is preferably PC, PET, or PLA. During the synergistic pyrolysis process, the reducing gases (such as CO and H2) released by the pyrolysis of these oxygen-containing plastics can reduce the high-valence transition metal oxides (such as Co) in the S-LIBs cathode in situ. 3+ Ni 2+ Mn 4+ This process enables the efficient conversion and release of key metals such as lithium, cobalt, and nickel. Simultaneously, the CO2 generated during pyrolysis can react with the released Li... + The reaction forms Li₂CO₃, achieving stable lithium solidification and simultaneous carbon encapsulation. Furthermore, the metals in the battery cathode material can act as catalysts, promoting the directional pyrolysis of plastics in situ: PC mainly produces phenol and syngas, PET mainly produces aromatic hydrocarbons, and PLA mainly produces high-value chemicals such as lactide. The recovered metal products can be recycled to prepare cathode materials, and the chemicals such as phenol, aromatic hydrocarbons, and lactide can be used in organic synthesis, demonstrating excellent closed-loop utilization potential.

[0037] The residual solid is mixed with water and leached with stirring to obtain a leachate and a leaching residue. The water is preferably deionized water. The solid-liquid ratio of the residual solid to water is preferably 1 g:(15~25) mL to improve the lithium leaching efficiency and the crystallization effect of Li2CO3. Optionally, the solid-liquid ratio of the residual solid to water is 1 g:15 mL, 1 g:16 mL, 1 g:17 mL, 1 g:18 mL, 1 g:19 mL, 1 g:20 mL, 1 g:21 mL, 1 g:22 mL, 1 g:23 mL, 1 g:24 mL, 1 g:25 mL, or any two of the above ratios. The stirring leaching temperature is preferably 30℃~50℃. Optionally, the stirring leaching temperature is 30℃, 35℃, 40℃, 45℃, 50℃, or any two of the above values. The stirring leaching speed is preferably 100~500 rpm. Optionally, the stirring leaching speed is 100 rpm. The stirring and leaching time is 1 to 3 hours; optionally, the stirring and leaching time is 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, or any two of the above values.

[0038] In one specific embodiment of the present invention, the solid-liquid ratio of the residual solid to water is 1 g: 20 mL.

[0039] The leachate is dried to obtain lithium carbonate. The drying method can be any method known to those skilled in the art and is not particularly limited. In this invention, heating and evaporation are preferred. Specifically, the leachate can be treated to remove impurities before drying.

[0040] In a specific embodiment of the present invention, the method preferably further includes S5) mixing the leaching residue with lithium carbonate and calcining at high temperature to obtain a cathode material. The ratio of the leaching residue to lithium carbonate can be selected according to the type of cathode material, with the selection principle being a slight excess of lithium. Specifically, if the cathode material is LCO, the leaching residue and lithium carbonate are preferably mixed in a cobalt to lithium molar ratio of 1:(1.01~1.1), more preferably in a cobalt to lithium molar ratio of 1:1.05; if the cathode material is LMO, the leaching residue and lithium carbonate are preferably mixed in a manganese to lithium molar ratio of 2:(1.01~1.1), more preferably in a manganese to lithium molar ratio of 2:1.05; and the cathode material is a ternary cathode material. The leaching residue and lithium carbonate are preferably mixed in a molar ratio of nickel, cobalt, manganese (or aluminum) to lithium of 1:(1.01~1.1), more preferably in a molar ratio of nickel, cobalt, manganese (or aluminum) to lithium of 1:1.05; the mixing method is preferably ball milling; the ball-to-material ratio of the ball milling is preferably (3~8):1, more preferably (4~6):1, and even more preferably 5:1; the ball milling speed is preferably 200~800 rpm; optionally, the ball milling speed is 200 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm or any two of the above values; the ball milling time is preferably 4~24 h; optionally, the ball milling time is 4 h, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h. h or a range between any two of the above values; the preferred high-temperature roasting temperature is 800℃~1000℃; optionally, the high-temperature roasting temperature is 800℃, 850℃, 900℃, 950℃, 1000℃ or a range between any two of the above values; the preferred high-temperature roasting time is 10~24 h; optionally, the high-temperature roasting time is 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h or a range between any two of the above values.

[0041] In a specific embodiment of the present invention, the leaching residue is first heated in a steam atmosphere to undergo a decarbonization reaction. The residual carbon in the leaching residue undergoes a carbon-water vaporization reaction with steam under the catalysis of transition metals (Co, Ni, Mn, etc.), generating syngas rich in H2 / CO. Simultaneously, solid products enriched with transition metals and their oxides are obtained, realizing the resource utilization of residual carbon and the deep decarbonization recovery of transition metals (Co, Ni, Mn). The solid products are then mixed with lithium carbonate and calcined at high temperature to obtain the cathode material. The decarbonization reaction is preferably carried out in a fixed-bed reactor; the preferred temperature for the decarbonization reaction is 700℃~900℃; optionally, the temperature is 700℃, 750℃, 800℃, 850℃, 900℃, or any two of the above values; the preferred time for the decarbonization reaction is 0.5~2 h; optionally, the time is 0.5 h, 1 h, 1.5 h, 2 h, or any two of the above values. During the decarbonization reaction, transition metals such as Co, Ni, and Mn in the leaching residue can catalyze the carbon-water reaction to generate syngas and improve the purity of metal oxides.

[0042] In a specific embodiment provided by this invention, the flowchart of the resource recovery method for synergistic pyrolysis recycling of waste plastics and retired lithium-ion battery cathode materials is shown below. Figure 4 As shown. The method provided by this invention can upgrade waste PC plastics into phenol and syngas, and simultaneously recover valuable metals from retired lithium battery cathode materials. The process is simple, energy-efficient, and produces little pollution. It can be used for mixed waste treatment and yields a variety of high-value products.

[0043] To further illustrate the present invention, the following describes in detail, with reference to embodiments, a method for the resource recovery of waste plastics and retired lithium-ion battery cathode materials through synergistic pyrolysis.

[0044] All reagents used in the following examples are commercially available.

[0045] Example 1

[0046] Step 1): Immerse 20 g of retired lithium cobalt oxide batteries in a 5 wt% NaCl solution for 48 hours to ensure complete discharge. Use a crushing and sorting device to crush and physically separate the batteries, recovering aluminum foil, copper foil, and casing (plastic or metal) as byproducts. Pass the mixed cathode material particles obtained from the sorting through a 200-mesh sieve to obtain 7 g of mixed cathode material from retired lithium batteries.

[0047] 10 g of PC plastic taken from a computer casing was crushed and then passed through a 200-mesh sieve to obtain PC plastic powder.

[0048] Step 2): Mix PC plastic powder and retired lithium battery mixed positive electrode material at a mass ratio of 1:1.75 (total mass 10 g), and grind thoroughly for half an hour to ensure uniform powder mixing, thus obtaining a mixed material.

[0049] Step 3): Place the mixture in a fixed-bed pyrolysis reactor, such as... Figure 3 As shown, nitrogen gas (100 mL / min) was introduced to purge air for 30 minutes, then the temperature was raised to 500 °C and held for 0.5 hours. The liquid product (pyrolysis oil) was collected via a condenser, and the solid residue was cooled to room temperature with the furnace and used for subsequent processing. The GC-MS spectrum of the obtained pyrolysis oil is shown below. Figure 5 As shown.

[0050] Step 4): Mix the solid residue with deionized water at a solid-liquid ratio of 1:20 (g / mL), stir magnetically at 40°C (300 rpm) for 2 hours, filter, and collect the leachate and leachate residue.

[0051] Step 5): The leachate from Step 4) is dried by rotary evaporation to recover lithium carbonate, denoted as Li₂CO₃-LCO. The XRD pattern of the recovered lithium carbonate is shown below. Figure 6 As shown.

[0052] Step 6): Mix the leaching residue (mainly CoO) from Step 4) with Li₂CO₃ at a Co:Li molar ratio of 1:1.05, and ball mill in a planetary ball mill (zirconia grinding balls, ball-to-material ratio 5:1, speed 300 rpm) for 8 hours. Place the ball-milled product in a muffle furnace, heat to 900℃ and hold for 18 hours. After cooling, obtain the regenerated lithium cobalt oxide cathode material. The XRD pattern of the regenerated LCO is shown below. Figure 7 As shown.

[0053] Example 2

[0054] Steps 1) to 5) in this embodiment are the same as in embodiment 1.

[0055] Step 6): After drying the leaching residue obtained in Step 4), place it into a fixed-bed reactor. Heat the reactor to 800℃ at a steam flow rate of 1 mL / min and maintain this temperature for 1.5 hours. This allows the residual carbon deposits to undergo a carbon-water vaporization reaction to generate syngas (H2 / CO). The syngas obtained from the carbon-water vaporization reaction is as follows: Figure 8 As shown, metal-enriched solid residues were obtained simultaneously.

[0056] Step 7): Mix the metal-enriched solid residue (mainly CoO) from Step 6) with Li2CO3 at a Co:Li molar ratio of 1:1.05, and ball mill in a planetary ball mill (zirconia grinding balls, ball-to-material ratio 5:1, speed 300 rpm) for 8 hours. Place the ball-milled product in a muffle furnace, heat to 900℃, hold for 18 hours, and cool to obtain the regenerated lithium cobalt oxide cathode material LCO.

[0057] Example 3

[0058] The recycling method for ternary lithium batteries provided in this embodiment replaces lithium cobalt oxide in step 1) with ternary lithium (NCM, LiNi) batteries. 0.8 Co 0.1 Mn 0.1 O2), replacing PC plastic powder taken from the computer with PLA plastic powder taken from disposable straws; In step 2), the mass ratio of PLA plastic powder to positive electrode powder is changed to 1:2; Mix the leaching residue from step 4) with Li2CO3 at a molar ratio of Ni:Co:Mn:Li of 0.8:0.1:0.1:1.05; The remaining steps and process parameters are the same as in Example 1.

[0059] The XRD patterns of the recovered lithium carbonate (denoted as Li2CO3-NCM) and the recycled ternary lithium cathode material are as follows: Figure 6 and Figure 9 As shown.

[0060] Example 4

[0061] The recycling method for lithium manganese oxide batteries provided in this embodiment replaces lithium cobalt oxide in step 1) with lithium manganese oxide (LiMn2O4). Replace the PC plastic powder in step 2) with PET powder; The leaching residue (mainly manganese oxide) from step 4) is mixed with Li2CO3 at a Mn:Li molar ratio of 2:1.05; The remaining steps and process parameters are the same as in Example 1.

[0062] The XRD patterns of the recovered lithium carbonate (denoted as Li2CO3-LMO) and the regenerated lithium manganese oxide cathode material are as follows: Figure 6 and Figure 10 As shown.

[0063] Comparative Example 1

[0064] This comparative example is used to investigate the influence of oxygen-containing functional groups in plastic molecules on the deconstruction and lithium release effect of lithium cobalt oxide cathode materials.

[0065] The main difference between this comparative example and Example 1 is that the PC plastic powder used in steps 1) and 2) of Example 1 is replaced with polyethylene plastic powder that does not contain oxygen-containing functional groups. The other raw materials, operating steps and process parameters are the same as those in Example 1.

[0066] Specifically, waste polyethylene plastic is cleaned, dried and crushed, and then passed through a 200-mesh sieve to obtain polyethylene plastic powder (degree of polymerization of 1200).

[0067] The polyethylene plastic powder and the decommissioned lithium cobalt oxide cathode material powder were mixed at a mass ratio of 1:1.75, with a total mass of 10 g, and then ground thoroughly for 30 min to ensure uniform mixing of the two powders, thus obtaining a mixture.

[0068] The mixture was placed in a fixed-bed pyrolysis reactor, and nitrogen gas was introduced at a flow rate of 100 mL / min and purged for 30 min to remove air from the reactor. The temperature was then raised to 500 °C and held for 0.5 h. The volatile products generated by pyrolysis were collected by condensation to obtain liquid products, and the resulting solid residue was cooled to room temperature with the furnace.

[0069] The solid residue was mixed with deionized water at a solid-liquid ratio of 1 g: 20 mL, and leached at 40°C and 300 rpm for 2 h with stirring. After filtration, the leachate and leaching residue were collected separately. The lithium content in the leachate and the cobalt content in the leaching residue were detected, and the lithium recovery rate and cobalt recovery rate were calculated.

[0070] The recovery rate of metal elements, the yield of pyrolysis oil and the product selectivity in Examples 1-4 and Comparative Example 1 were analyzed, and the results are shown in Table 1.

[0071] Table 1. Statistical results of metal element recovery rate, pyrolysis oil yield, and product selectivity.

[0072] As shown in Table 1, the front-end pyrolysis systems of Example 1 and Example 2 are completely identical. The only difference is that Example 2 adds a carbon-water vapor gasification reaction at the back end of the product. The raw material cracking, metal enrichment, and phenol generation all occur in the front-end pyrolysis stage and are not affected by the back-end carbon-water vapor gasification reaction. Therefore, the metal recovery rate and phenol yield data are very similar.

[0073] In summary, this invention, through a co-pyrolysis synergistic strategy, achieves for the first time the highly efficient synergistic recycling of retired lithium-ion batteries (S-LIBs) and waste polycarbonate (PC), polyethylene terephthalate (PET), and polylactic acid (PLA) plastics containing oxygen groups, demonstrating significant advantages such as additive-free operation, medium-temperature pyrolysis, and co-conversion of two wastes. Specifically, the pulverized S-LIBs are mixed with PC plastic in a certain proportion and reacted directly at a medium-low temperature of approximately 500°C. Without the need for external acids, alkalis, or reducing agents, in-situ reduction of transition metal oxides, efficient release of lithium, and stable conversion to Li2CO3 are simultaneously achieved. The reducing gases (CO, H2) generated during the reaction not only promote metal reduction, but also result in high-purity metals in the reaction residue, facilitating post-processing. Simultaneously, the metal components in the S-LIBs can also catalyze the high-value pyrolysis of plastics, achieving highly selective production of high-value chemicals such as phenol (for PC), aromatic hydrocarbons (for PET), and lactide (for PLA). This process has multiple advantages, including high recovery rates of lithium, cobalt, and nickel (all exceeding 97%) and high product selectivity (over 85% for PC products, over 50% for PET products, and over 60% for PLA products). It also has good environmental friendliness and economic feasibility, providing a scalable technical path for achieving closed-loop synergistic utilization of waste batteries and waste plastics.

[0074] To investigate the effect of oxygen-containing functional groups in plastic molecules on the deconstruction of the cathode material and lithium release, Comparative Example 1 used PE plastic without oxygen-containing functional groups to replace the PC plastic in Example 1, while keeping the mass ratio of plastic to lithium cobalt oxide cathode material and other reaction conditions unchanged. Experimental results showed that, compared with Example 1, the lithium recovery rate of Comparative Example 1 was significantly reduced. This indicates that the C–O and / or C=O functional groups in the oxygen-containing plastic can promote Li–O bond activation, lithium migration and release, and lithium carbonate formation through interfacial interactions with Li sites on the cathode material surface, thus playing a positive role in the efficient recovery of lithium.

[0075] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for the resource recovery of waste plastics and retired lithium-ion battery cathode materials through synergistic pyrolysis, characterized in that, Includes the following steps: S1) The cathode material of retired lithium-ion batteries is mixed with plastic to obtain a mixed powder; the plastic contains oxygen; the mass ratio of the plastic to the cathode material of retired lithium-ion batteries is 1:1 to 1:

2. S2) In a protective atmosphere, the mixed powder is pyrolyzed to obtain pyrolysis oil and residual solids; S3) Mix the residual solid with water, stir and leach to obtain leachate and leach residue; S4) The leachate is dried to obtain lithium carbonate.

2. The resource recovery method according to claim 1, characterized in that, Also includes: S5) The leaching residue is mixed with lithium carbonate and calcined at high temperature to obtain the cathode material.

3. The resource recovery method according to claim 2, characterized in that, The retired lithium-ion battery cathode material is selected from retired lithium cobalt oxide cathode material, retired lithium manganese oxide cathode material, or retired ternary lithium cathode material; And / or, the plastic is selected from one or more of polycarbonate, polyethylene terephthalate and polylactic acid; And / or, the particle size of the plastic and the retired lithium-ion battery cathode material are each independently less than 100 μm.

4. The resource recovery method according to claim 3, characterized in that, The retired lithium-ion battery cathode material is a retired lithium cobalt oxide cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material is 1:1.5 to 1:2; Alternatively, the retired lithium-ion battery cathode material may be a retired lithium manganese oxide cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material may be 1:1.5 to 1:

2. Alternatively, the retired lithium-ion battery cathode material may be a retired ternary lithium cathode material; the mass ratio of the plastic to the retired lithium-ion battery cathode material may be 1:1 to 1:

2.

5. The resource recovery method according to claim 3, characterized in that, The retired ternary lithium cathode material is lithium nickel cobalt manganese oxide, whose general formula can be represented as LiNi x Co y Mn z O2, where x+y+z=1; And / or, the pyrolysis temperature is 300℃~600℃; the pyrolysis time is 0.5~6 h.

6. The resource recovery method according to claim 2, characterized in that, The solid-liquid ratio of the residual solid to water is 1 g: (15~25) mL; And / or, the temperature of the stirring leaching is 30℃~50℃; the stirring speed of the stirring leaching is 100~500 rpm; and the stirring leaching time is 1~3 h.

7. The resource recovery method according to claim 2, characterized in that, The method for mixing the leaching residue with lithium carbonate is ball milling; the ball milling speed is 200~800 rpm; the ball milling time is 4~24 h; And / or, the high-temperature calcination temperature is 800℃~1000℃; the high-temperature calcination time is 10~24 h.

8. The resource recovery method according to any one of claims 1 to 7, characterized in that, The leaching residue is first heated in a steam atmosphere to carry out a decarbonization reaction, yielding syngas and solid products; then the solid products are mixed with lithium carbonate and calcined at high temperature to obtain the cathode material.

9. The resource recovery method according to claim 8, characterized in that, The decarbonization reaction is carried out at a temperature of 700℃ to 900℃ and for a time of 0.5 to 2 hours.

10. The resource recovery method according to claim 1, characterized in that, The retired lithium-ion battery cathode material is obtained according to the following method: After the retired lithium-ion batteries are fully discharged, the positive electrode current collector, negative electrode current collector, and shell material are removed by crushing and physical sorting methods, and then sieved to obtain the positive electrode material of the retired lithium-ion batteries.