Asymmetric spontaneous power tin-air battery based on acid-base electrolyte gradient and application thereof

By employing an acid-base electrolyte gradient design in tin-air batteries, with an acidic cathode and an alkaline anode, and utilizing the pH gradient to construct a thermodynamic driving force, the problems of low voltage, easy corrosion, and high cost of traditional metal-air batteries are solved, enabling the application of high-efficiency and low-cost tin-air batteries.

CN123143597APending Publication Date: 2026-11-20FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611054976.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-15
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional metal-air batteries suffer from problems such as low open-circuit voltage, susceptibility to CO₂ interference, severe anode self-corrosion, and high cost, which are difficult to overcome with a single electrolyte system.

Method used

An acid-base electrolyte gradient design is adopted, with acidic electrolyte at the cathode and alkaline electrolyte at the anode. The pH gradient is used to construct an additional thermodynamic driving force. Combined with a porous gas diffusion electrode, an ion exchange membrane, and tin metal oxidation reaction, an asymmetric self-generating tin-air battery is formed.

Benefits of technology

A tin-air self-generating device with high output voltage, strong anti-CO₂ interference capability, and low cost has been realized, which improves the operational stability and life of the battery and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143597A_ABST
    Figure CN123143597A_ABST
Patent Text Reader

Abstract

The application discloses an asymmetric self-power generation tin-air battery based on an acid-base electrolyte gradient and application thereof, and belongs to the technical field of electrochemical energy storage and metal-air batteries. The battery comprises a cathode gas diffusion electrode, an ion exchange membrane and a metal tin anode. The cathode gas diffusion electrode and the metal tin anode are connected through an external circuit to form a power generation loop. The cathode gas diffusion electrode and the ion exchange membrane are filled with an acidic electrolyte, and the metal tin anode and the ion exchange membrane are filled with an alkaline electrolyte. The cathode gas diffusion electrode is loaded with an acidic oxygen reduction catalyst for catalyzing the oxygen reduction reaction of oxygen from air containing nitrogen, carbon dioxide and oxygen. The metal tin anode undergoes a tin metal oxidation reaction in the alkaline electrolyte. The theoretical open-circuit voltage of the battery is U = 1.3 + (pH base-pH acid) * 0.059 V. The application greatly improves the open-circuit voltage by using the acid-base pH gradient, completely avoids CO2 interference, does not need noble metal anode materials, and has the advantages of simple structure, low cost and excellent power generation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrochemical energy storage and metal-air battery technology, specifically relating to an asymmetric self-generating tin-air battery based on an acid-base electrolyte gradient and its application. Background Technology

[0002] Metal-air batteries, with their extremely high theoretical energy density, show great promise for applications in portable electronic devices and large-scale energy storage. However, traditional metal-air batteries mostly use a single electrolyte system, which has many insurmountable technical shortcomings.

[0003] On the one hand, if a conventional alkaline electrolyte system is used, when the battery is operating in an open air environment, the approximately 0.04% carbon dioxide (CO2) in the air readily reacts with the alkaline medium (OH-). - The reaction produces carbonate precipitates. This continuously consumes electrolyte and clogs the pores of the gas diffusion electrode, leading to a sharp decrease in the system's ionic conductivity, which severely restricts the battery's power generation efficiency, cycle life, and long-term stability.

[0004] On the other hand, while using an acidic electrolyte on the cathode side can take advantage of the extremely low solubility of CO2 under acidic conditions and the fact that it does not form carbonates, effectively avoiding CO2 interference, the metal anode in a purely acidic system often faces bottlenecks such as severe self-corrosion and slow discharge dynamics.

[0005] In addition, the open-circuit voltage of conventional single electrolyte systems is limited by a fixed thermodynamic potential, resulting in low energy output capacity; and some metal-air batteries require expensive precious metal materials for the anode, leading to high manufacturing costs and making it difficult to achieve large-scale application.

[0006] Currently, no existing technology employs an asymmetric tin-air battery with an acidic cathode and an alkaline anode gradient design. Therefore, if an asymmetric dual-electrolyte system can be combined with tin metal, placing the cathode in an acidic environment to eliminate carbonation and the anode in an alkaline environment to optimize tin oxidation kinetics, while simultaneously utilizing the pH gradient to significantly increase the system's open-circuit voltage, a novel tin-air self-generating device with a simple structure, high output voltage, strong resistance to CO2 interference, and low cost could be successfully developed, possessing extremely important practical application value. Summary of the Invention

[0007] The purpose of this invention is to provide an asymmetric self-generating tin-air battery based on an acid-base electrolyte gradient and its application, in order to solve the technical problems of traditional single-electrolyte metal-air batteries, such as low open-circuit voltage, susceptibility to CO2 interference, severe anode self-corrosion, and high cost.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an asymmetric self-generating tin-air battery based on an acid-base electrolyte gradient, comprising: Cathode gas diffusion electrode, ion exchange membrane, metallic tin anode; The cathode gas diffusion electrode and the metallic tin anode are connected by an external circuit to form a power generation circuit; The space between the cathode gas diffusion electrode and the ion exchange membrane is filled with an acidic electrolyte, and the space between the metallic tin anode and the ion exchange membrane is filled with an alkaline electrolyte. The cathode gas diffusion electrode is loaded with an acidic oxygen reduction catalyst for catalyzing the oxygen reduction reaction of oxygen in air containing nitrogen, carbon dioxide and oxygen. The tin anode undergoes a tin metal oxidation reaction in the alkaline electrolyte; The theoretical open-circuit voltage of the battery is U = 1.3 + (pH_alkali - pH_acid) × 0.059 V, where pH_alkali is the pH value of the alkaline electrolyte and pH_acid is the pH value of the acidic electrolyte.

[0009] Terminology Explanation: In this invention, the gas diffusion electrode (GDE) refers to an electrode with a porous structure.

[0010] In this invention, the oxygen reduction reaction (ORR) refers to the electrochemical reaction in which oxygen gains electrons and is reduced on the electrode surface.

[0011] In this invention, open circuit voltage (OCV) refers to the potential difference between the two terminals of a battery when no load is connected (i.e., the external circuit is disconnected).

[0012] In this invention, the ion exchange membrane is a polymer thin film with selective ion conduction function.

[0013] Derivation of the open-circuit voltage formula: In this invention, the theoretical open-circuit voltage formula U = 1.3 + (pH_base - pH_acid) × 0.059 V is derived based on the following: In an acid-base gradient dual electrolyte system, the thermodynamic driving force of the battery consists of two superimposed parts.

[0014] The first part covers the fundamental thermodynamic potentials of tin-based battery systems: the standard electrode potential for the acidic oxygen reduction reaction at the cathode is approximately +1.23 V (vs. the standard hydrogen electrode, SHE), and the anodic oxidation reaction of metallic tin (Sn→Sn²) + +2e -The standard electrode potential is approximately -0.14 V (vs. SHE), with a difference of approximately 1.37 V. Considering the overpotential loss in the actual system, the basic thermodynamic potential is taken as 1.3 V.

[0015] The second part is the additional potential contributed by the acid-base pH gradient: According to the Nernst Equation, the potential contribution for each unit pH difference is 0.059 V (RT / F×ln10≈0.059 V at 25℃, where R is the gas constant, T is the thermodynamic temperature, and F is the Faraday constant). Therefore, the additional potential contributed by the pH gradient is (pH base - pH acid)×0.059 V.

[0016] By superimposing the two parts, we obtain the theoretical open-circuit voltage formula of this invention: U = 1.3 + (pH base - pH acid) × 0.059 V. Here, SHE (Standard Hydrogen Electrode) is the standard hydrogen electrode, a reference standard for electrode potential in electrochemistry, and its potential is defined as 0 V.

[0017] In some embodiments, the metallic tin anode is at least one of tin plate, foamed tin, or an alloy containing tin. Foamed tin has a larger specific surface area, which is beneficial for increasing the anodic reaction rate; tin-containing alloys can further optimize oxidation kinetics by adjusting the alloy composition; the assembly and use of the above-mentioned alternative materials are the same as those of tin plates, and can be directly implemented by those skilled in the art.

[0018] In some embodiments, the ion exchange membrane is selected from any one of a bipolar membrane (BPM), anion exchange membrane (AEM), and cation exchange membrane (CEM).

[0019] The bipolar membrane is a special ion exchange membrane composed of a cation exchange layer and an anion exchange layer, allowing cations and anions to pass through on both sides respectively. The anion exchange membrane only allows anions to pass through; the cation exchange membrane only allows cations to pass through. The Nafion 117 proton exchange membrane is a typical example of a cation exchange membrane. All three types of ion exchange membranes mentioned above can be used in this invention to achieve effective separation of the anode and cathode chambers. Those skilled in the art can choose according to actual needs, and the usage is the same as in Example 1.

[0020] In some embodiments, the acidic oxygen reduction catalyst includes an active component and a support; the active component is selected from at least one of platinum-carbon (Pt / C), platinum-based alloys, and non-precious metal carbon-based catalysts; the support is selected from at least one of carbon paper, carbon cloth, and carbon felt.

[0021] Among them, platinum-carbon (Pt / C) refers to a commercial catalyst in which platinum nanoparticles are supported on a carbon support, exhibiting excellent acidic ORR activity; platinum-based alloys refer to alloy catalysts formed with platinum as the main active element and other metals (such as cobalt and nickel), which can reduce the amount of platinum used while maintaining high activity; non-precious metal carbon-based catalysts refer to ORR catalysts prepared by doping carbon materials with non-precious metal elements such as iron, cobalt, and nitrogen, which can effectively reduce costs. Carbon cloth, carbon felt, and carbon paper are all carbon-based porous support materials, all possessing good electrical conductivity and mechanical stability, and their usage is the same as that of carbon paper, which can be directly implemented by those skilled in the art.

[0022] In some embodiments, the acidic oxygen reduction catalyst is loaded at a rate of 0.5 mg / cm² to 3.0 mg / cm².

[0023] Optionally, the catalyst loading is selected from any value or a range of any two of 0.5 mg / cm², 1.0 mg / cm², 1.5 mg / cm², 2.0 mg / cm², 2.5 mg / cm², and 3.0 mg / cm².

[0024] Preferably, the loading of the acidic oxygen reduction catalyst is 1.0 mg / cm².

[0025] In some embodiments, the acidic electrolyte is an aqueous solution of at least one of sulfuric acid (H2SO4), phosphoric acid (H3PO4), hydrochloric acid (HCl), and perchloric acid (HClO4), and the pH value of the acidic electrolyte is in the range of 0 to 7 (excluding 7).

[0026] Optionally, the pH value of the acidic electrolyte is selected from any value of 0, 1, 2, 3, 4, 5, 6, or a range of any combination of both. The concentration of the acidic electrolyte is from 0.1 mol / L to 3.0 mol / L.

[0027] Optionally, the concentration of the acidic electrolyte is selected from any value or a range of any two of 0.1 mol / L, 0.5 mol / L, 1.0 mol / L, 2.0 mol / L, and 3.0 mol / L. Preferably, the concentration of the acidic electrolyte is 2.0 mol / L.

[0028] In some embodiments, the alkaline electrolyte is an aqueous solution of at least one of potassium hydroxide (KOH), sodium hydroxide (NaOH), and lithium hydroxide (LiOH), and the pH value of the alkaline electrolyte is in the range of 7 to 14 (excluding 7).

[0029] Optionally, the pH value of the alkaline electrolyte is selected from any value of 8, 9, 10, 11, 12, 13, 14, or a range of any combination of both. The concentration of the alkaline electrolyte is from 0.1 mol / L to 6.0 mol / L.

[0030] Optionally, the concentration of the alkaline electrolyte is selected from any value or a range of any two of 0.1 mol / L, 0.5 mol / L, 1.0 mol / L, 2.0 mol / L, 4.0 mol / L, and 6.0 mol / L. Preferably, the concentration of the alkaline electrolyte is 4.0 mol / L.

[0031] In some embodiments, the cathode gas diffusion electrode has a porous structure, allowing air to diffuse through and forming a gas-liquid-solid three-phase reaction interface with the acidic oxygen reduction catalyst and the acidic electrolyte; the coating area of ​​the cathode gas diffusion electrode is from 0.5 cm × 0.5 cm to 3.0 cm × 3.0 cm.

[0032] Optionally, the coating area is selected from any value or a range of any two of 0.5 cm × 0.5 cm, 1.0 cm × 1.0 cm, 1.5 cm × 1.5 cm, 2.0 cm × 2.0 cm, and 3.0 cm × 3.0 cm.

[0033] Preferably, the coating area of ​​the cathode gas diffusion electrode is 1.0 cm × 1.0 cm.

[0034] In some embodiments, when the pH gradient (i.e., pHbase-pHacid) between the acidic electrolyte and the alkaline electrolyte is 8 to 14, the theoretical open-circuit voltage of the battery is 1.772 V to 2.126 V.

[0035] Optionally, the pH gradient is selected from any integer value of 8, 9, 10, 11, 12, 13, 14 or a range of values ​​composed of both.

[0036] Preferably, when the pH gradient is 14, the theoretical open-circuit voltage of the battery is 2.126 V.

[0037] In a second aspect, the present invention also provides an application of the tin-air battery as described in any one of the first aspects above, wherein the battery is used in portable energy storage or self-powered sensing power supply.

[0038] The beneficial effects that this application can produce include: 1) This application adopts an acid-base asymmetric dual electrolyte system and utilizes the pH gradient to construct an additional thermodynamic driving force. The theoretical open-circuit voltage can reach 2.126 V, which effectively solves the problem of low open-circuit voltage in traditional single electrolyte metal-air batteries.

[0039] 2) The cathode of this invention adopts an acidic electrolyte environment, which completely avoids the problem of CO2 reacting with alkaline electrolyte to generate carbonate precipitates that clog the electrode pores, and significantly improves the battery's operational stability and service life.

[0040] 3) The anode of this invention uses metallic tin, which has excellent oxidation kinetics and low self-corrosion rate in alkaline environment. Furthermore, the self-corrosion rate of tin in alkaline electrolyte is much lower than that of active metals such as aluminum, eliminating the need for any precious metal materials and significantly reducing the cost of battery manufacturing.

[0041] 4) The present invention has a simple structure, readily available materials, and strong environmental adaptability, and has good prospects for industrial application. Attached Figure Description

[0042] Figure 1 This is a schematic diagram of the structure of the asymmetric self-generating tin-air battery based on the acid-base electrolyte gradient in Embodiment 1 of the present invention; Figure 2 This is a comparison diagram of the open-circuit voltage of the battery system in Embodiment 1 of the present invention; wherein the control group is a traditional single alkaline electrolyte tin-air battery, and the experimental group is the acid-base gradient system of the present invention; Figure 3 The discharge polarization curve and power density curve of the battery system in Embodiment 1 of the present invention; Figure 4 This is a voltage stability test diagram of the battery system during long-term operation in Embodiment 1 of the present invention. Detailed Implementation

[0043] To make the objectives, technical solutions, and advantages of this invention clearer, the following will describe this application in further detail with reference to specific embodiments. However, the scope of protection of this invention is not limited to these embodiments. It should be noted that, unless otherwise specifically stated, all raw materials and chemical reagents used in the embodiments of this application are commercially available conventional products, which are used directly after purchase without further purification.

[0044] The main testing instruments and core materials involved in the embodiments of this application are sourced as follows: Electrochemical performance characterization of the samples (including open-circuit voltage measurement, polarization curve testing, and constant-current discharge stability testing) was performed using a CHI760E electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd.). The commercial platinum-carbon (Pt / C) catalyst used in the experiments was purchased from Shanghai Hesen Electric Co., Ltd. The proton exchange membrane used in the experiments was Nafion 117 (DuPont Ltd.). Nafion 117 is a perfluorosulfonic acid type cation exchange membrane with a thickness of approximately 178 μm, exhibiting good proton conductivity and chemical stability.

[0045] The carbon paper electrode supported on a commercial platinum-carbon catalyst involved in the examples is prepared using the following specific process: First, prepare the mixed solvent: mix water, ethanol and Nafion solution in a volume ratio of 6:3:1; Secondly, the catalyst slurry was prepared: 10 mg of commercial platinum-carbon catalyst was weighed and added to 1000 μL of the above mixed solvent, and ultrasonically treated for 20 min to make it uniformly dispersed, so as to obtain a slurry with a catalyst mass concentration of 10 mg / mL. Finally, drop coating is performed: 150 μL of uniformly dispersed slurry is taken with a pipette and dropped onto the center of a 4 cm × 4 cm carbon paper. The coating area is controlled to be 1 cm × 1 cm. After drying, the desired gas diffusion electrode is obtained, with a catalyst loading of approximately 1.0 mg / cm².

[0046] Example 1 This embodiment provides an asymmetric self-generating tin-air battery based on an acid-base electrolyte gradient, the structure of which is referenced. Figure 1 The battery includes a cathode gas diffusion electrode, an acidic electrolyte (electrolyte I), a cation exchange membrane, an anode tin plate, and an alkaline electrolyte (electrolyte II).

[0047] Cathode gas diffusion electrode: It is made by loading a commercial platinum-carbon catalyst onto hydrophobically treated carbon paper with a catalyst loading of 1.0 mg / cm² and a coating area of ​​1.0 cm × 1.0 cm.

[0048] Ion exchange membrane: DuPont Nafion 117 proton exchange membrane (cation exchange membrane) is used.

[0049] Anode electrode: 99% pure tin plate.

[0050] Electrolyte I (cathode chamber): 2.0 mol / L H2SO4 solution, pH approximately 0.

[0051] Electrolyte II (anode chamber): 4.0 mol / L KOH solution, pH approximately 14.

[0052] Assemble the above components into a battery, with the cathode gas diffusion electrode exposed to air containing nitrogen, carbon dioxide, and oxygen. According to the theoretical open-circuit voltage formula U = 1.3 + (pH_base - pH_acid) × 0.059 V, when pH_base = 14 and pH_acid = 0, the theoretical open-circuit voltage U = 1.3 + (14 - 0) × 0.059 = 2.126 V.

[0053] Example 2 Electrochemical Performance Testing Electrochemical tests were performed on the battery assembled in Example 1, and the results are as follows: Open circuit voltage test ( Figure 2 In an air atmosphere (containing nitrogen, carbon dioxide and oxygen), the open-circuit voltage of the assembled acid-base gradient tin-air battery is close to the theoretical value of 2.126 V, which is significantly higher than that of the traditional single alkaline electrolyte tin-air battery (the open-circuit voltage of the control group is about 1.3 V). Figure 2 The comparative data show that the pH gradient has a significant contribution to improving the open-circuit voltage. In an air atmosphere containing CO2, the open-circuit voltage of the battery of the present invention does not decrease significantly, while the performance of the control alkaline system decreases due to carbonation. This proves the anti-CO2 interference effect of the acidic cathode system of the present invention.

[0054] Discharge polarization curve and power density curve ( Figure 3 In an air environment, the battery exhibits good discharge performance, maintaining a high discharge voltage at different current densities, with a peak power density of approximately 150 mW / cm². The power density curve shows that the battery has excellent output performance.

[0055] Long-term stability test Figure 4 ): Under a constant current density of 10 mA / cm², continuous discharge stability tests were conducted. By periodically replacing the electrolyte (the replacement cycle depends on the discharge current density and electrolyte consumption), this acid-base electrolyte gradient asymmetric self-generating tin-air battery can operate stably for a long time with minimal voltage decay, indicating that the battery has excellent long-term operational stability.

[0056] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. An asymmetric self-generating tin-air battery based on an acid-base electrolyte gradient, characterized in that, include: Cathode gas diffusion electrode, ion exchange membrane, metallic tin anode; The cathode gas diffusion electrode and the metallic tin anode are connected by an external circuit to form a power generation circuit; The space between the cathode gas diffusion electrode and the ion exchange membrane is filled with an acidic electrolyte, and the space between the metallic tin anode and the ion exchange membrane is filled with an alkaline electrolyte. The cathode gas diffusion electrode is loaded with an acidic oxygen reduction catalyst for catalyzing the oxygen reduction reaction of oxygen in air containing nitrogen, carbon dioxide and oxygen. The tin anode undergoes a tin metal oxidation reaction in the alkaline electrolyte; The theoretical open-circuit voltage of the battery is U = 1.3 + (pH_alkali - pH_acid) × 0.059 V, where pH_alkali is the pH value of the alkaline electrolyte and pH_acid is the pH value of the acidic electrolyte.

2. The tin-air battery according to claim 1, characterized in that, The tin anode is at least one of tin plate, tin foam, or an alloy containing tin.

3. The tin-air battery according to claim 1, characterized in that, The ion exchange membrane is selected from any one of bipolar membranes, anion exchange membranes, and cation exchange membranes.

4. The tin-air battery according to claim 1, characterized in that, The acidic oxygen reduction catalyst includes an active component and a support; The active component is selected from at least one of platinum-carbon, platinum-based alloys, and non-precious metal carbon-based catalysts; The carrier is selected from at least one of carbon paper, carbon cloth, and carbon felt.

5. The tin-air battery according to claim 4, characterized in that, The acidic oxygen reduction catalyst is loaded at a rate of 0.5 mg / cm² to 3.0 mg / cm². Preferably, the loading of the acidic oxygen reduction catalyst is 1.0 mg / cm².

6. The tin-air battery according to claim 1, characterized in that, The acidic electrolyte is an aqueous solution of at least one of sulfuric acid, phosphoric acid, hydrochloric acid, and perchloric acid, and the pH value of the acidic electrolyte is in the range of 0 to 7. The concentration of the acidic electrolyte is from 0.1 mol / L to 3.0 mol / L; Preferably, the concentration of the acidic electrolyte is 2.0 mol / L.

7. The tin-air battery according to claim 1, characterized in that, The alkaline electrolyte is an aqueous solution of at least one of potassium hydroxide, sodium hydroxide, and lithium hydroxide, and the pH value of the alkaline electrolyte is in the range of 7 to 14. The concentration of the alkaline electrolyte is from 0.1 mol / L to 6.0 mol / L; Preferably, the concentration of the alkaline electrolyte is 4.0 mol / L.

8. The tin-air battery according to claim 1, characterized in that, The cathode gas diffusion electrode has a porous structure, allowing air to diffuse through and form a gas-liquid-solid three-phase reaction interface with the acidic oxygen reduction catalyst and the acidic electrolyte. The coating area of ​​the cathode gas diffusion electrode is from 0.5 cm × 0.5 cm to 3.0 cm × 3.0 cm; Preferably, the coating area of ​​the cathode gas diffusion electrode is 1.0 cm × 1.0 cm.

9. The tin-air battery according to claim 1, characterized in that, When the pH gradient between the acidic electrolyte and the alkaline electrolyte is 8 to 14, the theoretical open-circuit voltage of the battery is 1.772 V to 2.126 V. Preferably, when the pH gradient is 14, the theoretical open-circuit voltage of the battery is 2.126 V.

10. An application of a tin-air battery as described in any one of claims 1 to 9, characterized in that, The battery is used in portable energy storage or self-powered sensing power supply.