All-solid-state cylindrical battery, method of manufacturing the same, and electric device

By filling an all-solid-state cylindrical battery with inert gas to achieve an isostatic pressure state, combined with high-strength stainless steel foil and a buffer layer, the instability of the solid-solid interface and the volume expansion problem of solid-state lithium-ion batteries are solved, thereby improving the cycle stability and energy density of the battery.

CN123143604APending Publication Date: 2026-11-20CHERY AUTOMOBILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611309100.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Solid-state lithium-ion batteries suffer from high solid-solid interface impedance, low ion transport efficiency of solid electrolytes, and large volume expansion of silicon anodes, resulting in poor cycle stability. Furthermore, the heavy pressure fixtures used in existing pouch batteries affect the energy density of the final battery pack.

Method used

It adopts an all-solid-state cylindrical battery structure, and achieves isostatic pressure by filling the casing with inert gas. High-strength stainless steel foil and buffer layer are used to ensure uniform stress on the core and avoid additional constraint tooling.

Benefits of technology

This solves the problem of solid-solid interface instability in solid cylindrical cells, reduces volume expansion, and improves solid-solid interface stability and battery energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143604A_ABST
    Figure CN123143604A_ABST
Patent Text Reader

Abstract

The application provides a full solid-state cylindrical battery and a preparation method and an electric device thereof, and relates to the technical field of lithium ion batteries.The full solid-state cylindrical battery comprises a cylindrical shell and a wound core in an isostatic pressure state in the shell;inert gas is filled in the shell to make the wound core in the isostatic pressure state;the pressure of the inert gas is 1MPa-20MPa.The application solves the problem of unstable solid-solid interface of the solid-state cylindrical battery, and achieves the technical effects of reducing volume expansion and improving the stability of the solid-solid interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of lithium-ion batteries, and in particular to an all-solid-state cylindrical battery, its preparation method, and an electrical device thereof. Background Technology

[0002] Solid-state lithium-ion batteries suffer from high solid-solid interface impedance, low ion transport efficiency of solid electrolytes, and large volume expansion of silicon anodes, resulting in poor cycle stability. Although isostatic pressing can be used during manufacturing to mitigate these issues, in practical applications, external pressure is generally required to maintain solid-solid interface stability and cycle stability.

[0003] Currently, battery cells are generally manufactured in the form of pouch cells, and a flat pressure of 0.001MPa-30MPa is typically applied during cell testing or end-use applications. Existing fixtures for applying pressure to pouch cells are bulky, significantly impacting the energy density of the final battery pack.

[0004] In view of this, the present invention is hereby proposed. Summary of the Invention

[0005] One of the objectives of this invention is to provide an all-solid-state cylindrical battery that can solve the technical problem of unstable solid-solid interface in solid cylindrical cells, thereby achieving the technical effects of reducing volume expansion and improving solid-solid interface stability.

[0006] The second objective of this invention is to provide a method for preparing an all-solid-state cylindrical battery.

[0007] The third objective of this invention is to provide an electrical device.

[0008] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: In a first aspect, there is an all-solid-state cylindrical battery, comprising a cylindrical casing and a wound core in an isostatic state located within the casing; The housing is filled with inert gas to keep the winding core in an isostatic pressure state. The pressure of the inert gas is 1 MPa-20 MPa.

[0009] Furthermore, the negative electrode foil of the all-solid-state cylindrical battery is a high-strength stainless steel foil; Preferably, the tensile strength of the high-strength stainless steel foil is between 400MPa and 2000MPa; Preferably, the inner ring of the core is filled with rigid rods to prevent the core from collapsing under isostatic pressure and / or during charging and discharging; Preferably, a buffer layer is provided between the housing and the core to ensure that the battery cell is subjected to uniform force.

[0010] Furthermore, the buffer layer comprises a fiber-reinforced silica aerogel pad; Preferably, the fiber material includes at least one of ceramic fiber, pre-oxidized fiber, and glass fiber; Preferably, the fiber material is incorporated into the silica aerogel pad at a concentration of 30%-90%. Preferably, the thickness of the buffer layer is 0.02mm-1mm.

[0011] Furthermore, the cylindrical shell includes a cylindrical steel shell, preferably a nickel-plated steel shell; Preferably, the thickness of the nickel-plated steel shell is 0.05mm-3mm, and more preferably 1mm-2mm.

[0012] Furthermore, the distance between the inner wall of the housing and the outer periphery of the winding core under isostatic pressing is 0.01mm-0.2mm, preferably 0.01mm-0.1mm.

[0013] Furthermore, the pressure of the inert gas in the casing is 3MPa-20MPa.

[0014] Furthermore, the hard rod comprises a lightweight alloy; Preferably, the diameter of the hard rod is 2mm-10mm, and more preferably 5mm-7mm.

[0015] Secondly, a method for preparing an all-solid-state cylindrical battery according to any one of the above claims includes the following steps: The core is subjected to isostatic pressing to obtain a core in an isostatic pressing state. The winding core, which is in an isostatic pressure state, is inserted into a cylindrical shell, an inert gas is introduced into the shell, and the shell is sealed to obtain the all-solid-state cylindrical battery.

[0016] Furthermore, the method for preparing the core includes the following steps: The composite negative electrode and positive electrode are wound onto a rigid rod to obtain the core. Preferably, the pressure of the isostatic pressing treatment is 100MPa-630MPa, more preferably 250MPa-500MPa; Preferably, the isostatic pressing temperature is 30℃-100℃, and more preferably 70℃-90℃; Preferably, the isostatic pressing treatment time is 3 min-10 min, more preferably 5 min-8 min; Preferably, the preparation method further includes the following steps: A fiber-reinforced silica aerogel pad is attached between the casing and the battery cell as a buffer layer.

[0017] Thirdly, an electrical device comprising the all-solid-state cylindrical battery described in any of the preceding claims.

[0018] Compared with the prior art, the present invention has at least the following beneficial effects: The all-solid-state cylindrical battery provided by this invention includes a cylindrical casing and a wound core in an isostatic state located within the casing. Because the casing is filled with an inert gas at a pressure of 1MPa-20MPa, the casing is under high pressure. The casing provides constraint force to the wound core, thus keeping it in an isostatic state at all times. This overcomes electrode defects caused by the cell manufacturing process and compensates for pressure unevenness caused by these defects. No additional constraint fixtures are needed after the cylindrical cell is formed. In summary, this invention solves the technical problem of unstable solid-solid interface in solid-state cylindrical cells, achieving the technical effects of reducing volume expansion and improving solid-solid interface stability. Attached Figure Description

[0019] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0020] Figure 1 This is a schematic diagram of the structure of an all-solid-state cylindrical battery according to one embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of an electrical device provided in one embodiment of the present invention. Detailed Implementation

[0021] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] According to a first aspect of the present invention, an all-solid-state cylindrical battery is provided, see Figure 1 It includes a cylindrical shell and a core in an isostatically compressed state located within the shell; The shell is filled with inert gas to keep the core in an isostatic pressure state. The pressure of the inert gas is 1MPa-20MPa, for example, it can be 1MPa, 3MPa, 5MPa, 10MPa, 15MPa, 20MPa, but is not limited to this, which effectively ensures that the core is in an isostatic pressure state. Inert gases are unreactive gases, and common unreactive gases can be selected, such as nitrogen, argon, and helium, but are not limited to these.

[0023] The all-solid-state cylindrical battery of the present invention includes a cylindrical shell and a core in an isostatic pressure state located in the shell. Since the shell is filled with an inert gas at a pressure of 1MPa-20MPa, the shell is in a high-pressure state. The shell provides a constraint force for the core, so the core is always in an isostatic pressure state, thereby overcoming the electrode defects caused by the cell manufacturing process and compensating for the pressure unevenness caused by the defects. No additional constraint tooling is required after the cylindrical cell is formed.

[0024] In a preferred embodiment, the negative electrode foil of the all-solid-state cylindrical battery can be a high-strength stainless steel foil with a tensile strength between 400MPa and 2000MPa. It can be selected from at least one of Fe-Cr-Ni alloy foil, iron-nickel foil, nickel-cobalt foil, and Ni-P amorphous foil. It can provide high structural strength, suppress cell deformation, provide uniform pressure, suppress sulfide corrosion, and reduce the occurrence of side reactions.

[0025] In a preferred embodiment, the inner ring of the core may be filled with rigid rods to prevent the core from collapsing under isostatic pressure and / or during charging and discharging.

[0026] In a preferred embodiment, a buffer layer can be provided between the shell and the core, which helps to achieve uniform stress on the solid core.

[0027] In summary, the all-solid-state cylindrical battery of this invention achieves uniform stress on the solid core by filling it with inert gas, filling the inner ring of the core with hard rods, and setting a buffer layer between the shell and the core (i.e., the cell), thus solving the problem of unstable solid-solid interface in solid cylindrical cells.

[0028] In a preferred embodiment, the buffer layer can be selected from fiber-reinforced silica aerogel pads, which have balanced insulation, thermal conductivity and mechanical strength, and are lightweight, allowing for more uniform stress on the battery cell.

[0029] In a preferred embodiment, the fiber material includes, but is not limited to, at least one of ceramic fiber, pre-oxidized fiber, and glass fiber.

[0030] In a preferred embodiment, the amount of fiber material in the silica aerogel pad can be 30%-90%, for example, 30%, 40%, 50%, 60%, 70%, 80%, 90%, but not limited to this, which is more conducive to making the battery cell bear force evenly; if the amount of fiber material is too small, the buffer layer is prone to deformation and the buffering effect is poor; if the amount of fiber material is too large, the surface defects of the buffer layer are large, there are stress points, and the force is uneven during buffering.

[0031] In a preferred embodiment, the thickness of the buffer layer can be 0.02mm-1mm, for example, 0.02mm, 0.03mm, 0.04mm, 0.05mm, 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, or 1mm, but is not limited to these values. This is more conducive to ensuring uniform stress on the battery cell. If the thickness of the buffer layer is too small, the buffering effect will be poor; if the thickness of the buffer layer is too large, the buffer layer will be easily compressed, affecting the energy density of the battery cell.

[0032] In a preferred embodiment, the cylindrical shell includes, but is not limited to, a cylindrical steel shell, and is more preferably a nickel-plated steel shell. The cylindrical shell made of nickel-plated steel has significantly better mechanical strength than an aluminum shell.

[0033] In a preferred embodiment, the thickness of the nickel-plated steel shell can be 0.05mm-3mm, for example, 0.05mm, 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, 1mm, 1.5mm, 2mm, 2.5mm, or 3mm, but is not limited thereto, and can be further preferably 1mm-2mm.

[0034] In a preferred embodiment, the distance between the inner wall of the housing and the outer periphery of the winding core under isostatic pressing can be 0.01mm-0.2mm, for example, 0.01mm, 0.02mm, 0.03mm, 0.04mm, 0.05mm, 0.1mm, or 0.2mm, but is not limited thereto. It is more preferably 0.01mm-0.1mm, which is more conducive to assembly. If the distance between the two is too small, it will be difficult to insert the core into the housing; if the distance between the two is too large, it will affect the energy density of the battery cell.

[0035] In a preferred embodiment, the pressure of the inert gas in the casing can be 3MPa-20MPa, for example, 3MPa, 5MPa, 10MPa, 15MPa, or 20MPa, but is not limited to these values. This is more conducive to ensuring that the core is in an isostatic pressure state. If the pressure of the inert gas is too low, the solid-solid interface contact will be poor, the internal resistance will be high, and the capacity will be difficult to achieve. If the pressure of the inert gas is too high, the casing needs to be thicker to ensure that the casing does not leak, which will affect the battery energy density.

[0036] In a preferred embodiment, the hard rod includes, but is not limited to, a lightweight alloy, which is more conducive to preventing the collapse of the core center hole during isostatic pressing and / or charging and discharging.

[0037] The diameter of the rigid rod is customized according to the flexibility of the electrode sheet. The diameter can be 2mm-10mm, for example, 2mm, 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, but is not limited to these. It is more preferably 5mm-7mm.

[0038] According to a second aspect of the present invention, a method for preparing an all-solid-state cylindrical battery as described in any one of the preceding claims is provided, comprising the following steps: The core is subjected to isostatic pressing to obtain a core in an isostatic pressing state. The winding core, which is in an isostatic state, is inserted into a cylindrical shell, inert gas is introduced into the shell, and it is sealed to obtain an all-solid-state cylindrical battery.

[0039] In a preferred embodiment, the method for preparing the winding core includes the following steps: The composite negative electrode and positive electrode are wound onto a rigid rod to obtain a core.

[0040] In this invention, the electrolyte layer is transferred onto the negative electrode sheet to form a composite negative electrode, which is then wound together with the positive electrode onto a rigid rod to obtain a core.

[0041] It should be noted that a ceramic edge can be applied to the positive electrode tab; the height of the ceramic edge coating can be between 2mm and 7mm, and can be further preferably between 3mm and 5mm; the thickness of the ceramic edge after rolling can be between 2um and 10um, and can be further preferably between 4um and 6um.

[0042] In a preferred embodiment, the outermost layer of the core can be wrapped with a high-strength foil such as stainless steel foil extended from the negative electrode sheet. After wrapping, an elastic mold is applied, and then isostatic pressing is performed to obtain a core in an isostatic pressing state.

[0043] In this invention, the core needs to be welded to the current collector. After the tabs are welded to the current collector, the current collector is connected to the cylindrical shell, which carries a negative charge. The core is then inserted into the cylindrical shell, filled with inert gas, and sealed to obtain a fully solid-state cylindrical battery.

[0044] In a preferred embodiment, the pressure of the isostatic pressing process can be 100MPa-630MPa, for example, 100MPa, 200MPa, 300MPa, 400MPa, 500MPa, 600MPa, or 630MPa, but is not limited thereto. It is more preferably 250MPa-500MPa, which is more conducive to ensuring that the core is in an isostatic pressing state. If the pressure of the isostatic pressing process is too low, the solid-solid interface contact will be poor and the internal resistance will be high. If the pressure of the isostatic pressing process is too high, the processing will be difficult.

[0045] In a preferred embodiment, the isostatic pressing temperature can be 30℃-100℃, for example, 30℃, 40℃, 50℃, 60℃, 70℃, 80℃, 90℃, or 100℃, but is not limited thereto. It is more preferably 70℃-90℃, which is more conducive to ensuring that the core is in an isostatic pressing state. If the isostatic pressing temperature is too low, the core will be subjected to greater stress during densification. If the isostatic pressing temperature is too high, it will affect the stability of the material.

[0046] In a preferred embodiment, the isostatic pressing time can be 3 min to 10 min, for example, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, or 10 min, but is not limited to this. It is more preferably 5 min to 8 min, which is more conducive to ensuring that the core is in an isostatic pressing state. If the isostatic pressing time is too short, the density will be low and the solid-solid interface contact will be poor. If the isostatic pressing time is too long, the processing efficiency will be low.

[0047] In a preferred embodiment, the preparation method of the present invention further includes the following steps: A fiber-reinforced silica aerogel pad is attached between the casing and the battery cell as a buffer layer.

[0048] According to a third aspect of the present invention, an electrical device is provided, comprising an all-solid-state cylindrical battery as described in any of the preceding claims, wherein the all-solid-state cylindrical battery can be used as a power source for the electrical device or as an energy storage unit for the electrical device.

[0049] In this invention, the electrical device can be a mobile device (typically such as a mobile phone, a laptop computer, etc.), an electric vehicle (typically such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, or an energy storage system, etc.

[0050] Figure 2 This is an example of an electrical device, which can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc.

[0051] The present invention will be further illustrated below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or purchased directly from the market.

[0052] Example 1 A solid-state cylindrical battery includes a cylindrical casing and a wound core in an isostatic pressure state located within the casing. The shell is filled with inert gas (nitrogen) at a pressure of 3 MPa to keep the core in an isostatic pressure state. The casing is made of nickel-plated steel with a thickness of 1.5mm; The distance between the inner wall of the housing and the outer periphery of the winding core under isostatic pressure is 0.05 mm; The negative electrode foil of the all-solid-state cylindrical battery is made of high-strength stainless steel foil; The inner ring of the core is filled with a rigid rod with a diameter of 6mm. The rigid rod is made of aluminum alloy and is used to prevent the core from collapsing under isostatic pressure and / or during charging and discharging. A buffer layer with a thickness of 0.5mm is set between the casing and the battery cell to ensure that the battery cell is subjected to uniform force. The buffer layer is a fiber-reinforced silica aerogel pad, and the fiber material is ceramic fiber. The fiber material content in the silica aerogel pad is 80%.

[0053] Example 2 The difference between this embodiment and Embodiment 1 is that the pressure of the inert gas in the shell is 1 MPa; Everything else is the same as in Example 1.

[0054] Example 3 The difference between this embodiment and Embodiment 1 is that the pressure of the inert gas in the shell is 5 MPa; Everything else is the same as in Example 1.

[0055] Example 4 The difference between this embodiment and Embodiment 1 is that the pressure of the inert gas in the shell is 10 MPa; Everything else is the same as in Example 1.

[0056] Example 5 The difference between this embodiment and Embodiment 1 is that the pressure of the inert gas in the shell is 20 MPa; Everything else is the same as in Example 1.

[0057] Example 6 The difference between this embodiment and Embodiment 1 is that the fiber material of the fiber-reinforced silica aerogel pad is pre-oxidized fiber. Everything else is the same as in Example 1.

[0058] Example 7 The difference between this embodiment and Embodiment 1 is that the fiber material of the fiber-reinforced silica aerogel pad is glass fiber; Everything else is the same as in Example 1.

[0059] Example 8 The difference between this embodiment and Embodiment 1 is that the amount of fiber material in the silica aerogel pad is 30%. Everything else is the same as in Example 1.

[0060] Example 9 The difference between this embodiment and Embodiment 1 is that the amount of fiber material in the silica aerogel pad is 40%. Everything else is the same as in Example 1.

[0061] Example 10 The difference between this embodiment and Embodiment 1 is that the amount of fiber material in the silica aerogel pad is 60%. Everything else is the same as in Example 1.

[0062] Example 11 The difference between this embodiment and Embodiment 1 is that the amount of fiber material in the silica aerogel pad is 90%. Everything else is the same as in Example 1.

[0063] Example 12 The difference between this embodiment and Embodiment 1 is that the thickness of the buffer layer between the casing and the battery cell is 0.02 mm; Everything else is the same as in Example 1.

[0064] Example 13 The difference between this embodiment and Embodiment 1 is that the thickness of the buffer layer between the casing and the battery cell is 0.05 mm; Everything else is the same as in Example 1.

[0065] Example 14 The difference between this embodiment and Embodiment 1 is that the thickness of the buffer layer between the casing and the battery cell is 0.1 mm; Everything else is the same as in Example 1.

[0066] Example 15 The difference between this embodiment and Embodiment 1 is that the thickness of the buffer layer between the casing and the battery cell is 1 mm; Everything else is the same as in Example 1.

[0067] Example 16 The difference between this embodiment and Embodiment 1 is that the buffer layer is a silica aerogel pad and does not contain fibrous materials; Everything else is the same as in Example 1.

[0068] Examples 17-32 Examples 17-32 describe the preparation methods of the all-solid-state cylindrical solar cells of Examples 1-16, including the following steps: (1) Formulation preparation: The positive electrode formulation is NCM: corresponding solid electrolyte: SP: corresponding binder = 65%: 32.5%: 1.5%: 1%, and the negative electrode formulation is SiC: corresponding solid electrolyte: SP: corresponding binder = 50%: 47.5%: 1.5%: 1%. The N / P ratio is 1.1, and the positive electrode material area capacity is 4 mAh / cm². 2 The solid electrolyte thickness is 50 micrometers, and the negative electrode material area has a capacity of 4.4 mAh / cm². 2 ; The formulation of the solid electrolyte layer is: corresponding solid electrolyte: corresponding binder = 97%: 3%; (2) Preparation of positive electrode: NCM811 cathode material, LPSC electrolyte powder, VGCF, and SEPS were added to butyl butyrate solvent in a certain proportion. The components were then uniformly dispersed using a high-speed disperser to form a stable slurry. After obtaining a uniform slurry, the slurry was uniformly coated onto a 12μm thick aluminum current collector using a grooved die coating machine to form a thin layer. Ceramic edges were coated at the cathode tabs, and the thickness after rolling was 5μm, with a ceramic edge tab coating height of 4mm. (3) Anode preparation: Silicon carbon material, LPSC electrolyte powder with a particle size of 2μm, VGCF and PAA binder are added to xylene solvent according to the mass fraction ratio. The components are uniformly dispersed using a high-speed disperser to form a stable slurry. After obtaining a uniform slurry, the slurry is uniformly coated onto a 10μm thick stainless steel current collector using a grooved die coating machine to form a thin layer. (4) Preparation of solid electrolyte layer: The electrolyte raw materials are placed in xylene and stirred. The stirred slurry is then coated onto a release film and dried to obtain the electrolyte layer. (5) Solid-state battery fabrication: The electrolyte layer is rolled and transferred onto the negative electrode sheet. The composite negative electrode and positive electrode are wound onto a 6mm diameter rigid rod. The outermost layer of the core is wrapped with a high-strength stainless steel foil extended from the negative electrode sheet. After wrapping, an elastic mold is put on. The core is subjected to isostatic pressing at 70℃ and 500MPa for 30 minutes. A buffer layer is attached between the cylindrical casing and the battery cell; After isostatic pressing, the compressed core is welded to the current collector. After the electrode tab is welded to the current collector, the current collector is connected to the cylindrical shell, and the cylindrical shell is negatively charged. After isostatic pressing, the core is inserted into a cylindrical casing, inert gas is introduced into the casing, and it is sealed to obtain a fully solid-state cylindrical battery.

[0069] Comparative Example 1 The difference between this comparative example and Example 1 is that the shell is not filled with inert gas; Everything else is the same as in Example 1.

[0070] Comparative Example 2 The difference between this comparative example and Example 1 is that no buffer layer is provided between the casing and the battery cell; Everything else is the same as in Example 1.

[0071] Test case The performance of the all-solid-state cylindrical batteries of Examples 1-16 and Comparative Examples 1-2 was tested, and the results are shown in Table 1.

[0072] Charge and discharge at an ambient temperature of 45℃:

[0073] 0.5C capacity: Charge and discharge at an ambient temperature of 45℃; step 6 generates a capacity of C. 放 .

[0074] Internal resistance test: The voltage internal resistance meter is used to test the connection between the positive and negative tabs of the large cylindrical tube.

[0075] Table 1

[0076] As shown in Table 1, on the one hand, the all-solid-state cylindrical batteries of Examples 1-16 of the present invention have good solid-solid interface contact and stability due to the inert gas filling in the casing, which puts the core in an isostatic pressure state. As a result, the solid-solid interface is stable, the internal resistance is low, and the capacity is well utilized. In contrast, the all-solid-state cylindrical battery of Comparative Example 1 does not fill the casing with inert gas, which directly leads to poor solid-solid interface contact, high internal resistance, and difficulty in capacity utilization. On the other hand, the all-solid-state cylindrical batteries of Examples 1-16 of the present invention have different internal resistances and different capacity utilizations due to the different pressures of inert gas filling in the casing, different fiber materials used in the buffer layer, different amounts of fiber materials used in the buffer layer, or different thicknesses of the buffer layer. This shows that the inert gas pressure and the buffer layer material both affect the stability of the solid-solid interface. In addition, compared with Example 1, the all-solid-state cylindrical battery of Comparative Example 2 does not have a buffer layer between the casing and the cell, which has an adverse effect on the stability of the solid-solid interface, resulting in high internal resistance and poor capacity utilization.

[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A fully solid-state cylindrical battery, characterized in that, It includes a cylindrical shell and a wound core in an isostatic state located within the shell; The housing is filled with inert gas to keep the winding core in an isostatic pressure state. The pressure of the inert gas is 1 MPa-20 MPa.

2. The all-solid-state cylindrical battery according to claim 1, characterized in that, The negative electrode foil of the all-solid-state cylindrical battery is a high-strength stainless steel foil; Preferably, the tensile strength of the high-strength stainless steel foil is between 400MPa and 2000MPa; Preferably, the inner ring of the core is filled with rigid rods to prevent the core from collapsing under isostatic pressure and / or during charging and discharging; Preferably, a buffer layer is provided between the housing and the core to ensure that the battery cell is subjected to uniform force.

3. The all-solid-state cylindrical battery according to claim 2, characterized in that, The buffer layer includes a fiber-reinforced silica aerogel pad. Preferably, the fiber material includes at least one of ceramic fiber, pre-oxidized fiber, and glass fiber; Preferably, the fiber material is incorporated into the silica aerogel pad at a concentration of 30%-90%. Preferably, the thickness of the buffer layer is 0.02mm-1mm.

4. The all-solid-state cylindrical battery according to any one of claims 1-3, characterized in that, The cylindrical shell includes a cylindrical steel shell, preferably a nickel-plated steel shell; Preferably, the thickness of the nickel-plated steel shell is 0.05mm-3mm, and more preferably 1mm-2mm.

5. The all-solid-state cylindrical battery according to claim 4, characterized in that, The distance between the inner wall of the housing and the outer periphery of the winding core under isostatic pressure is 0.01mm-0.2mm, preferably 0.01mm-0.1mm.

6. The all-solid-state cylindrical battery according to claim 4, characterized in that, The pressure of the inert gas in the shell is 3MPa-20MPa.

7. The all-solid-state cylindrical battery according to claim 4, characterized in that, The hard rod comprises a lightweight alloy; Preferably, the diameter of the hard rod is 2mm-10mm, and more preferably 5mm-7mm.

8. A method for preparing an all-solid-state cylindrical battery according to any one of claims 1-7, characterized in that, Includes the following steps: The core is subjected to isostatic pressing to obtain a core in an isostatic pressing state. The winding core, which is in an isostatic pressure state, is inserted into a cylindrical shell, an inert gas is introduced into the shell, and the shell is sealed to obtain the all-solid-state cylindrical battery.

9. The preparation method according to claim 8, characterized in that, The method for preparing the core includes the following steps: The composite negative electrode and positive electrode are wound onto a rigid rod to obtain the core. Preferably, the pressure of the isostatic pressing treatment is 100MPa-630MPa, more preferably 250MPa-500MPa; Preferably, the isostatic pressing temperature is 30℃-100℃, and more preferably 70℃-90℃; Preferably, the isostatic pressing treatment time is 3 min-10 min, more preferably 5 min-8 min; Preferably, the preparation method further includes the following steps: A fiber-reinforced silica aerogel pad is attached between the shell and the core as a buffer layer.

10. An electrical device, characterized in that, Includes the all-solid-state cylindrical battery as described in any one of claims 1-7.