Battery cell and method for producing the same, battery device, electric device, energy storage device

By coating the outer surface of the battery's aluminum casing with an insulating composition to form an insulating protective film, the problems of adaptability and disassembly of traditional film-applying processes are solved, achieving low-temperature rapid film formation and efficient insulation protection, which is suitable for irregularly shaped batteries.

CN123143607APending Publication Date: 2026-11-20JINKO SOLAR CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611303186.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing battery manufacturing processes, the insulation protection of the aluminum shell surface is difficult to adapt to irregularly shaped battery cells. Traditional film application processes are complex and difficult to disassemble, and spraying insulating paint presents challenges in terms of high-temperature damage and film thickness control.

Method used

An insulating composition coating method is used, comprising phosphoryl halogen organic compounds and polysiloxanes containing terminal hydroxyl groups as prepolymers, coupling agents and curing agents, to form an insulating protective film through chemical covalent bonding. The curing temperature is below 150°C, making it suitable for batteries with complex shapes.

Benefits of technology

It enables rapid film formation at low temperatures, providing excellent insulation, flame retardancy, and resistance to electrolyte corrosion, avoiding the defects of traditional film application processes. It is suitable for batteries with complex shapes, reducing production costs and environmental burden.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123143607A_ABST
    Figure CN123143607A_ABST
Patent Text Reader

Abstract

The application provides a battery monomer, a preparation method thereof, a battery device, a power utilization device and an energy storage device. The battery monomer comprises an electric core with a shell and an insulation protective film arranged on the outer surface of the shell, and the insulation protective film is prepared from an insulation composition, which comprises, in parts by weight, 30-60 parts of a prepolymer, 2-8 parts of a coupling agent and 1-5 parts of a curing agent; wherein the polymerized monomers of the prepolymer comprise a phosphorus oxyhalide organic compound and a hydroxyl-terminated polysiloxane. The insulation protective film prepared from the above insulation composition not only has good insulation protection performance and electrolyte corrosion resistance, but also has fast film forming speed, is not prone to aging and falling off, and can be applied to complex battery shapes. Therefore, the insulation protective film can better protect the electric core, so that the battery monomer has good safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more specifically, to a battery cell and its preparation method, a battery device, an electrical device, and an energy storage device. Background Technology

[0002] In battery manufacturing, insulating the outer surface of the aluminum casing is a crucial step to ensure safe battery operation and meet electrical isolation requirements. Currently, the common method for insulating the aluminum casing is to apply a blue film (PET-based pressure-sensitive adhesive tape). This process uses pressure-sensitive adhesive to bond the blue film to the surface of the aluminum casing, and it is intuitive and inexpensive. However, as battery structures become more integrated and irregularly shaped, the limitations of traditional film application methods in adapting to complex curved surfaces are becoming increasingly apparent.

[0003] To overcome the problems associated with film application, some studies have proposed alternatives such as spraying insulating varnish and powder coating. Liquid insulating varnish, applied by dip-coating or spraying, forms a continuous film layer, adaptable to irregularly shaped surfaces. However, the film thickness of a single spray application is difficult to control precisely, easily leading to defects such as pinholes and exposed substrate. Powder coating forms a protective layer through high-temperature melting and leveling, offering advantages such as thick coating and good chemical resistance. However, it typically requires high curing temperatures, limiting its application on pre-assembled battery cells.

[0004] Therefore, there is an urgent need to develop new aluminum shell insulation protection methods that can quickly form films at room temperature or mild conditions, adapt to complex shapes, have simple production processes, and produce films with good recyclability. Summary of the Invention

[0005] The main objective of this invention is to provide a battery cell and its preparation method, battery device, power consumption device, and energy storage device, in order to solve the problems in the prior art where the cell casing film application process is difficult to adapt to irregularly shaped cells and the blue film is difficult to dismantle for battery recycling.

[0006] To achieve the above objectives, according to one aspect of the present invention, a battery cell is provided, comprising a cell having a casing and an insulating protective film disposed on the outer surface of the casing. The insulating protective film is prepared from an insulating composition, which, by weight, comprises: 30 to 60 parts of a prepolymer, 2 to 8 parts of a coupling agent, and 1 to 5 parts of a curing agent; wherein the polymeric monomers of the prepolymer include phosphoryl halogen organic compounds and polysiloxanes containing terminal hydroxyl groups.

[0007] Furthermore, the molar ratio of the phosphoryl halide organic compound and the hydroxyl-terminated polysiloxane is 1:(1~1.2); the phosphoryl halide organic compound is selected from any one or more of phenyl dichlorophosphate, methyl dichlorophosphate, and ethyl dichlorophosphate; the hydroxyl-terminated polysiloxane is selected from any one or more of hydroxyl-terminated polydimethylsiloxane, hydroxyl-terminated polymethylphenylsiloxane, and hydroxyl-terminated polydiphenylsiloxane; the number average molecular weight of the prepolymer is 2000~5000 Da.

[0008] Further, the coupling agent is selected from any one or more of the following: a complex of aluminum acetylacetonate and silane coupling agent, a phosphate-modified silane coupling agent, and a zirconium aluminate coupling agent; wherein the mass ratio of aluminum acetylacetonate and silane coupling agent is (0.5~2):1; the phosphate-modified silane coupling agent is selected from any one or more of the following: triethoxysilylpropyl phosphate, diethoxyphosphorylethyltriethoxysilane, and trimethoxysilylpropyl phosphate; the zirconium aluminate coupling agent is selected from any one or more of the following: a complex of tetra(triethanolamine)zirconate and aluminate, isopropoxyzirconium aluminate, and n-butoxyzirconium aluminate.

[0009] Furthermore, the curing agent is a cationic photoinitiator and / or a latent curing agent; wherein the cationic photoinitiator is selected from any one or more of diphenyliodonium salt, triphenylsulfonium salt and dialkylbenzoylmethylsulfonium salt; and the latent curing agent is a blocked isocyanate and / or a microencapsulated amine curing agent.

[0010] Furthermore, the mass ratio of the prepolymer, coupling agent, and curing agent is 100:(3~15):(2~10).

[0011] Furthermore, the insulating composition also includes additives and solvents;

[0012] The additives are selected from one or more of the following components: leveling agent, defoamer, and colorant; leveling agent, defoamer, and colorant; defoamer, defoamer, and colorant; solvent, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl acetate, acetone, and butanone.

[0013] Furthermore, the housing is made of aluminum; and / or the thickness of the insulating protective film is 10~30μm.

[0014] According to another aspect of the present invention, a method for preparing a battery cell is provided, comprising stacking and assembling a positive electrode, a separator, and a negative electrode in sequence to obtain a battery cell, inserting the battery cell into a casing, injecting electrolyte, and then encapsulating it to obtain a battery cell. The method for processing the casing includes: mixing raw materials comprising 30-60 parts by weight of a prepolymer, 2-8 parts by weight of a coupling agent, and 1-5 parts by weight of a curing agent to obtain an insulating composition; coating the insulating composition onto the outer surface of the casing and then curing it to obtain a casing containing an insulating protective film; wherein the polymer monomers of the prepolymer include phosphoryl halogen organic compounds and polysiloxanes containing terminal hydroxyl groups; the curing process includes sequential drying and heating; the drying temperature is lower than the heating temperature; the heating temperature is 60-90°C.

[0015] Furthermore, the shell treatment method further includes: pre-treating the shell before coating the insulating composition onto the outer surface of the shell to obtain a pre-treated shell; coating the insulating composition onto the outer surface of the pre-treated shell and then curing it to obtain a shell containing an insulating protective film; wherein, the pre-treatment is degreasing and / or chemical conversion treatment; the shell is degreased and cleaned with a cleaning solution, the cleaning solution being an alkaline cleaning solution and / or a surfactant; the chemical conversion treatment is titanium-zirconium conversion treatment and / or silane modification treatment; and an active layer is formed on the outer surface of the shell through chemical conversion treatment, the thickness of the active layer being 5~50 nm.

[0016] Further, the preparation process of the insulating composition includes: first mixing raw materials including a prepolymer and a solvent to obtain a first mixture; second mixing raw materials including the first mixture, a coupling agent, and a curing agent to obtain a second mixture; and third mixing raw materials including the second mixture and an additive to obtain the insulating composition; wherein the first mixing time is 10-15 min; the second mixing time is 5-10 min; the third mixing time is 5-15 min; and / or, the prepolymer is obtained by polycondensation reaction of polymeric monomer raw materials including a phosphoryl halide organic compound and a polysiloxane containing terminal hydroxyl groups; the molar ratio of the phosphoryl halide organic compound and the polysiloxane containing terminal hydroxyl groups is 1:(1-1.2); the polycondensation reaction temperature is 20-80°C, and the polycondensation reaction time is 2-8 h.

[0017] Further, the insulating composition is coated on the outer surface of the shell to form a wet film, which is then cured to obtain a shell containing an insulating protective film; wherein the thickness of the wet film is 30~100μm; the coating method is selected from any one or more of spraying, dipping, rolling and spin coating.

[0018] Furthermore, the drying temperature is 20~30℃, the drying time is 1~5 min; and / or, the heating time is 10~20 min.

[0019] According to another aspect of the present invention, a battery device is provided, the battery device comprising the above-described battery cell, and the battery device comprising any one or more of a battery module, a battery pack, and an energy storage battery.

[0020] According to another aspect of the present invention, an electrical device is provided, which includes the battery device described above, the battery device being used to provide electrical energy.

[0021] According to another aspect of the present invention, an energy storage device is provided, which includes the battery device described above, the battery device being used to store electrical energy.

[0022] By applying the technical solution of this invention, the insulating composition of the above-mentioned components and weight proportions can form a film in situ on the surface of the battery cell casing, which not only provides good insulation protection but also fundamentally avoids the inherent defects of the film-applying process. Specifically, 1) the prepolymer formed by the above-mentioned polymer monomers serves as the film-forming body, providing good insulation and flexibility. Phosphoryl halide organic compounds and polysiloxanes containing terminal hydroxyl groups have a phosphorus-silicon synergistic flame-retardant and insulating effect. Utilizing the char-forming flame-retardant mechanism of phosphorus in phosphoryl halide organic compounds and the advantage of silicon in polysiloxanes containing terminal hydroxyl groups in improving the density of the protective layer, even in ultra-thin (around 20 μm) film layers, the requirements for 500V insulation and breakdown resistance can be met. 2) The coupling agent enables the insulating protective film to form a chemical covalent bond with the casing, thereby improving the bonding strength between the two, which far exceeds the physical adhesion of films such as blue films. It also improves the battery's aging resistance and electrolyte resistance. 3) The curing agent can control the curing speed and activation temperature of the insulating composition, promoting the cross-linking and curing of the above components, thereby achieving rapid film formation at lower temperatures and obtaining a dense insulating protective film, which in turn better protects the battery cell. In summary, the insulating protective film obtained from the above insulating composition not only has good insulation and protection properties, flame retardant properties, and electrolyte corrosion resistance, but also has a fast film formation speed, is not prone to aging and peeling, can be retained as a long-term protective layer, and is suitable for complex battery shapes. Attached Figure Description

[0023] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0024] Figure 1 A schematic flowchart of the method for preparing the battery cell of this application is shown. Detailed Implementation

[0025] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0026] As analyzed in the background section of this application, the application of blue film also has the following disadvantages: 1) Complex application process and limited yield. The blue film application process includes multiple steps such as cell loading, casing cleaning, application of the main surface, side wrapping, edge folding, hot pressing shaping, and insulation testing. On high-speed automated production lines, the yield of the application process is usually only 98-99.5%, which is one of the main sources of defects in cell manufacturing. Common defect patterns include: bubbles, wrinkles, edge lifting, misalignment, and edge breakage. 2) Difficulty in applying film to irregularly shaped and thin-walled cells. As cell design develops towards irregular shapes and ultra-thinness, traditional planar application methods are difficult to adapt to complex geometric features such as curved surfaces, steps, and grooves. Even with hot pressing blue film, its adhesion and edge wrapping ability are still not ideal. 3) Environmental burden and cost pressure. Blue film is a PET / adhesive composite film, which is a single-use petrochemical-based material. With the surge in battery production, the consumption of blue film is huge, resulting in a significant environmental burden. Meanwhile, fluctuations in the prices of raw materials such as PET film and acrylic pressure-sensitive adhesive have also increased manufacturing costs. 4) Difficulty in recycling and dismantling. In the battery recycling process, the blue film needs to be removed so that the aluminum casing can be recycled. Currently, pyrolysis or solvent immersion methods are mainly used to remove the blue film, which are energy-intensive, inefficient, and generate secondary pollution.

[0027] However, spraying insulating varnish and powder coating also have the following disadvantages: 1) They require independent spraying / baking equipment and baking processes, resulting in high production line modification costs. 2) The coating curing temperature is usually ≥150℃, which may damage the heat-sensitive materials of the already filled electrolyte cells. 3) The film thickness of a single spray is difficult to control precisely, easily leading to defects such as pinholes and exposed substrate. 4) The curing time is long, ranging from 30 to 60 minutes, significantly reducing production efficiency.

[0028] As analyzed above in this application, the prior art has the problem that the cell casing film application process is difficult to adapt to irregularly shaped cells and that the blue film is difficult to dismantle for battery recycling. In order to solve the above problems, this application provides a battery cell and its preparation method, a battery device, an electrical device, and an energy storage device.

[0029] In a typical embodiment of this application, a battery cell is provided, including a cell with a casing and an insulating protective film disposed on the outer surface of the casing. The insulating protective film is prepared by an insulating composition, which, by weight, includes: 30 to 60 parts of prepolymer, 2 to 8 parts of coupling agent and 1 to 5 parts of curing agent; wherein the polymer monomers of the prepolymer include phosphoryl halogen organic compounds and polysiloxanes containing terminal hydroxyl groups.

[0030] This application utilizes an insulating composition with the aforementioned components and weight proportions to form an in-situ film on the surface of the battery cell casing. This not only provides excellent insulation and protection but also fundamentally avoids the inherent defects of the lamination process. Specifically, 1) the prepolymer formed from the aforementioned polymer monomers serves as the film-forming body, providing excellent insulation and flexibility. Phosphoryl halide organic compounds and hydroxyl-terminated polysiloxanes exhibit a phosphorus-silicon synergistic flame-retardant and insulating effect. Utilizing the char-forming flame-retardant mechanism of phosphorus in phosphoryl halide organic compounds and the advantage of silicon in hydroxyl-terminated polysiloxanes in improving the density of the protective layer, even ultra-thin (approximately 20 μm) films can meet the requirements for 500V insulation and breakdown resistance. 2) The coupling agent enables the insulating protective film to form a chemical covalent bond with the casing, thereby increasing the bonding strength between the two, far exceeding the physical adhesion of films like blue films. It also improves the battery's aging resistance and electrolyte resistance. 3) The curing agent can control the curing speed and activation temperature of the insulating composition, promoting the cross-linking and curing of the above components, thereby achieving rapid film formation at lower temperatures and obtaining a dense insulating protective film, which in turn better protects the battery cell. In summary, the insulating protective film obtained from the above insulating composition not only has good insulation and protection properties, flame retardant properties, and electrolyte corrosion resistance, but also has a fast film formation speed, is not prone to aging and peeling, can be retained as a long-term protective layer, and is suitable for complex battery shapes.

[0031] Furthermore, the weight percentages of the prepolymer in the insulating composition can be 30, 35, 40, 45, 50, 55, or 60 parts, etc. The weight percentages of the coupling agent can be 2, 3, 4, 5, 6, 7, or 8 parts, etc. The weight percentages of the curing agent can be 1, 2, 3, 4, or 5 parts, etc.

[0032] In one embodiment of this application, the molar ratio of the phosphoryl halide organic compound and the hydroxyl-terminated polysiloxane is 1:(1~1.2); the phosphoryl halide organic compound is selected from any one or more of phenyl dichlorophosphate, methyl dichlorophosphate, and ethyl dichlorophosphate; the hydroxyl-terminated polysiloxane is selected from any one or more of hydroxyl-terminated polydimethylsiloxane, hydroxyl-terminated polymethylphenylsiloxane, and hydroxyl-terminated polydiphenylsiloxane; and the number average molecular weight of the prepolymer is 2000~5000 Da.

[0033] The preferred molar ratio of phosphoryl halides to hydroxyl-terminated polysiloxanes within the aforementioned range facilitates the formation of a prepolymer through polycondensation, containing both P=O bonds (flame retardancy, enhanced insulation) and a Si-O-Si backbone (flexibility, weather resistance), thereby improving the insulation, flexibility, and flame retardancy of the insulating protective film. The phosphorus element in the prepolymer can form a phosphoric acid / polyphosphoric acid layer at high temperatures, promoting char formation and isolating oxygen; the silicon element forms a dense silicon oxide protective layer. The synergistic effect of these two elements further enhances the flame retardancy and electrical insulation (dielectric strength ≥20kV / mm) of the insulating protective film.

[0034] Preferred phosphoryl halide organic compounds within the above-mentioned range contribute to improving the insulation and flame-retardant properties of the insulating protective film. Specifically, the benzene ring structure of phenyl dichlorophosphate contributes to improving the heat resistance and mechanical strength of the insulating protective film, while methyl dichlorophosphate and ethyl dichlorophosphate contribute to improving the reactivity and flexibility of the prepolymer. Preferred polysiloxanes containing terminal hydroxyl groups within the above-mentioned range contribute to improving the flexibility and weather resistance of the insulating protective film. Specifically, hydroxyl-terminated polydimethylsiloxane has low surface energy and good hydrophobicity, while hydroxyl-terminated polymethylphenylsiloxane and hydroxyl-terminated polydiphenylsiloxane, due to the presence of benzene rings in their side groups, contribute to improving the thermal stability of the insulating protective film. Preferred hydroxyl-terminated polysiloxanes have 2 to 10 terminal hydroxyl groups, and a hydroxyl value of 50 to 120 mg KOH / g, which helps promote their reaction with phosphoryl halide organic compounds to generate prepolymers within the above-mentioned molecular weight range. Preferred number-average molecular weight of the prepolymer within the above-mentioned range helps the insulating protective film achieve both good flexibility and mechanical strength.

[0035] In one embodiment of this application, the coupling agent is selected from any one or more of a complex of aluminum acetylacetonate and silane coupling agent, phosphate-modified silane coupling agent, and zirconium aluminate coupling agent; wherein the mass ratio of aluminum acetylacetonate and silane coupling agent is (0.5~2):1; the phosphate-modified silane coupling agent is selected from any one or more of triethoxysilylpropyl phosphate, diethoxyphosphorylethyltriethoxysilane, and trimethoxysilylpropyl phosphate; the zirconium aluminate coupling agent is selected from any one or more of a complex of tetra(triethanolamine)zirconate and aluminate, isopropoxyzirconium aluminate, and n-butoxyzirconium aluminate.

[0036] The preferred coupling agent, falling within the aforementioned range, facilitates the formation of a chemical covalent bond between the insulating protective film and the shell, thereby enhancing the bonding strength between them. Specifically, for the aluminum shell, its surface naturally possesses a nano-thick layer of alumina and surface hydroxyl groups. Aluminum atoms in aluminum acetylacetonate can coordinate with the hydroxyl groups or alumina on the aluminum shell surface, while the silane coupling agent can crosslink with the prepolymer. Silane coupling agents include, but are not limited to, γ-aminopropyltriethoxysilane (KH-550), γ-glycidoxypropyltrimethoxysilane (KH-560), and γ-methacryloyloxypropyltrimethoxysilane (KH-570).

[0037] The aforementioned phosphate-modified silane coupling agents react with the hydroxyl groups on the aluminum shell surface at room temperature through the phosphate groups, forming stable Al-OP covalent bonds. This firmly anchors the coupling agent to the aluminum shell surface, thereby improving the bonding strength between the insulating protective film and the shell. Preferably, the mass ratio of aluminum acetylacetonate to the silane coupling agent is within the aforementioned range, which helps to further improve the bonding strength between the insulating protective film and the shell, building upon the formation of a uniform and dense insulating protective film.

[0038] Preferably using zirconium aluminate coupling agents within the above-mentioned range helps to utilize their high reactivity to improve the bonding strength between the insulating protective film and the shell.

[0039] In one embodiment of this application, the curing agent is a cationic photoinitiator and / or a latent curing agent; wherein the cationic photoinitiator is selected from any one or more of diphenyliodonium salt, triphenylsulfonium salt and dialkylbenzoylmethylsulfonium salt; and the latent curing agent is a blocked isocyanate and / or a microencapsulated amine curing agent.

[0040] The preferred type of curing agent falls within the above-mentioned range, which helps to promote the rapid and controlled curing of the insulating composition into a film at a lower temperature, reducing the damage to the internal heat-sensitive materials of the battery cell caused by traditional high-temperature baking (≥150℃), while meeting the needs of high-speed production lines. Among them, latent curing agents have an activation temperature of 60~90℃, at which they rapidly release the curing components, thereby increasing the curing rate. Blocked isocyanates include, but are not limited to, Imprafix 2794XP (aqueous blocked isocyanate, curing temperature approximately 180℃) and MF-K60X (blocked isocyanate curing agent for lithium battery covers, curing temperature >120℃). Microencapsulated amine curing agents include, but are not limited to, polyetheramine D230@PMMA microcapsules (using polymethyl methacrylate as the shell material, with polyetheramine D230 coated on the outer surface), and microcapsule systems encapsulating amine curing agents.

[0041] In one embodiment of this application, the mass ratio of the prepolymer, coupling agent and curing agent is 100:(3~15):(2~10), preferably 100:(7~15):(3~10).

[0042] Optimizing the mass ratio of prepolymer, coupling agent, and curing agent within the aforementioned range helps to form a dense insulating protective film with certain flexibility and mechanical strength. Furthermore, the insulating protective film maintains good insulation properties, aging resistance, and corrosion resistance, thereby better meeting the insulation protection requirements of the battery cell casing.

[0043] In one embodiment of this application, the insulating composition further includes an additive and a solvent; wherein the additive is 0.1 to 5 parts by weight, and the additive is selected from any one or more of leveling agents, defoamers, and colorants; the leveling agent is 0.1 to 1 part by weight; the defoamer is 0.1 to 0.5 parts by weight; the colorant is 0.5 to 3 parts by weight; and the solvent is 20 to 50 parts by weight, and the solvent is selected from any one or more of isopropanol, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl acetate, acetone, and butanone.

[0044] Leveling agents include, but are not limited to, BYK-333. Adding the above-mentioned types and parts by weight of leveling agents helps improve film uniformity. Defoamers include, but are not limited to, BYK-024. Adding the above-mentioned types and parts by weight of defoamers helps reduce bubble formation, thereby improving the surface quality of the insulating protective film. Colorants include, but are not limited to, phthalocyanine blue pigment. Adding the above-mentioned types and parts by weight of colorants helps impart a blue appearance to the insulating protective film, thus facilitating visual inspection. Adding the above-mentioned types and parts by weight of solvents helps adjust the viscosity and workability of the insulating composition. The viscosity of the insulating composition is 10~2500 mPa·s (25°C), optionally 200~500 mPa·s.

[0045] In one embodiment of this application, the housing is an aluminum housing; and / or, the thickness of the insulating protective film is 10~30μm.

[0046] The aluminum casing, made of aluminum metal, combines lightweight, thermal conductivity, and mechanical strength, thus providing physical protection for the battery cell. The aforementioned thickness of the insulating protective film enhances its density and protective capabilities, ensuring dielectric strength, corrosion resistance, and resistance to electrolyte corrosion, reducing the risk of short circuits. Simultaneously, the insulating protective film at this thickness exhibits better toughness and lower brittleness, resulting in lower internal stress during battery charging and discharging, and a lower risk of cracking, peeling, or edge lifting. Therefore, optimizing the insulating protective film thickness within the aforementioned range helps it balance mechanical strength, flexibility, insulation performance, and protective performance.

[0047] In another typical embodiment of this application, a method for preparing a battery cell is provided, comprising stacking and assembling a positive electrode, a separator, and a negative electrode in sequence to obtain a battery cell, inserting the battery cell into a casing, injecting electrolyte, and then sealing it to obtain a battery cell. The casing processing method comprises: mixing raw materials comprising 30-60 parts by weight of a prepolymer, 2-8 parts by weight of a coupling agent, and 1-5 parts by weight of a curing agent to obtain an insulating composition; coating the insulating composition onto the outer surface of the casing and then curing it to obtain a casing containing an insulating protective film; wherein the polymer monomers of the prepolymer include phosphoryl halides and polysiloxanes containing terminal hydroxyl groups; the curing process includes sequential drying and heating; the drying temperature is lower than the heating temperature; the heating temperature is 60-90°C.

[0048] This application utilizes an insulating composition with the aforementioned components and weight proportions to form an in-situ film on the surface of the battery cell casing. This provides excellent insulation protection while perfectly adhering to irregularly shaped / thin-walled battery cells. The insulating protective film and the casing are chemically covalently bonded, resulting in a bond strength far exceeding that of physical adhesives like blue film. Furthermore, it improves the battery's aging resistance and electrolyte resistance. The curing temperature of this insulating composition is significantly lower than traditional baking paint temperatures (≥150℃), allowing direct application to subsequent processing of already-filled battery cells (short-term heating has virtually no impact on cell performance). The short curing time also significantly improves production efficiency. This application greatly simplifies the casing processing, is compatible with existing production lines, eliminates the need for expensive laminating machines, and allows for simple coating to form a film. It is easily integrated into existing casing cleaning or assembly processes, resulting in low investment costs and flexible process switching.

[0049] In one embodiment of this application, the shell processing method further includes: pre-treating the shell before coating the insulating composition onto the outer surface of the shell to obtain a pre-treated shell; coating the insulating composition onto the outer surface of the pre-treated shell and then curing it to obtain a shell containing an insulating protective film; wherein the pre-treatment is degreasing and / or chemical conversion treatment; the shell is degreased and cleaned with a cleaning solution, the cleaning solution being an alkaline cleaning solution and / or a surfactant; the chemical conversion treatment is titanium-zirconium conversion treatment and / or silane modification treatment; and an active layer is formed on the outer surface of the shell through chemical conversion treatment, the thickness of the active layer being 5~50 nm.

[0050] Pre-treating the housing as described above before applying the insulating composition to its outer surface helps improve the cleanliness of the housing surface and the adhesion between the housing and the insulating protective film. Specifically, degreasing the housing with the aforementioned cleaning solutions helps remove oil stains from the housing surface, thus facilitating the adhesion of the insulating composition. Alkaline cleaning solutions include, but are not limited to, sodium hydroxide and potassium hydroxide solutions, sodium carbonate, sodium metasilicate pentahydrate, trisodium phosphate, etc.; surfactants include, but are not limited to, sodium alkylbenzene sulfonate (sodium dodecylbenzene sulfonate (LAS), sodium dodecyl sulfonate (SDS)), sodium fatty alcohol polyoxyethylene ether sulfate, and other compoundable types of surfactants, such as nonionic surfactants: isomeric decayl alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene ether (AEO7, AEO9), coconut oil fatty acid diethanolamide, etc.; anionic surfactants: sodium secondary alkyl sulfonate (SAS-60), fatty alcohol polyoxyethylene ether sulfonate (MOASO-4), etc.

[0051] Chemical conversion treatment helps form a nanoscale active layer on the shell surface, thereby enhancing film adhesion. Preferably, the thickness of the active layer is within the aforementioned range, which helps improve the bonding strength between the insulating protective film and the pretreated shell. Specifically, the titanium-zirconium conversion treatment involves spraying a 1-5 wt% fluorozirconic acid solution onto the shell surface to form the active layer. The pH of the fluorozirconic acid solution is 4-6, the spraying temperature is 30-60℃, and the spraying time is 5-6 seconds. The silane modification treatment involves hydrolyzing a silane coupling agent (KH-550, KH-570) into a 5-7.5 wt% treatment solution, applying it via dip coating, treating at 40-90℃ for 1-30 minutes, and curing at 25-200℃.

[0052] In one embodiment of this application, the preparation process of the insulating composition includes: first mixing raw materials including a prepolymer and a solvent to obtain a first mixture; second mixing raw materials including the first mixture, a coupling agent, and a curing agent to obtain a second mixture; and third mixing raw materials including the second mixture and an additive to obtain the insulating composition; wherein the first mixing time is 10-15 min; the second mixing time is 5-10 min; the third mixing time is 5-15 min; and / or, the prepolymer is obtained by polycondensation reaction of polymeric monomer raw materials including a phosphoryl halide organic compound and a polysiloxane containing terminal hydroxyl groups; the molar ratio of the phosphoryl halide organic compound and the polysiloxane containing terminal hydroxyl groups is 1:(1-1.2); the polycondensation reaction temperature is 20-80°C, and the polycondensation reaction time is 2-8 h.

[0053] In the preparation of the insulating composition, the prepolymer and solvent are first mixed, and the mixing time is controlled within the aforementioned range to help the prepolymer be fully dispersed in the solvent, thereby obtaining a first mixture with uniform composition. The first mixture, coupling agent, and curing agent are then mixed a second time, and the mixing time is controlled within the aforementioned range to help the coupling agent and curing agent be uniformly distributed in the prepolymer, thus facilitating subsequent crosslinking and curing. The second mixture and additives are then mixed a third time, and the mixing time is controlled within the aforementioned range to help the additives be fully dispersed, thereby improving the compositional uniformity of the insulating composition.

[0054] The preferred molar ratio of phosphoryl halide organic compounds and hydroxyl-terminated polysiloxanes within the above-mentioned range helps to promote the polycondensation reaction, thereby improving the purity of the prepolymer. The preferred temperature and time of the polycondensation reaction within the above-mentioned range also help to promote the reaction between the phosphoryl halide organic compounds and hydroxyl-terminated polysiloxanes, improving reaction efficiency and thus increasing the yield and purity of the prepolymer. A catalyst may be added during the polycondensation reaction; catalysts include, but are not limited to, pyridine, triethylamine, and imidazole.

[0055] In one embodiment of this application, an insulating composition is coated onto the outer surface of the housing to form a wet film, which is then cured to obtain a housing containing an insulating protective film; wherein the thickness of the wet film is 30~100μm; the coating method is selected from any one or more of spraying, dipping, rolling and spin coating.

[0056] The preferred wet film thickness, within the aforementioned range, helps to accommodate solvent evaporation and volume shrinkage during curing, thereby improving the density of the dry film and achieving an insulation withstand voltage of ≥500V. The insulating protective film of this application can be prepared by coating the insulating composition using the above-described method, resulting in a simple process and low equipment investment costs.

[0057] Dip coating is suitable for processing large batches of irregularly shaped battery cell casings. Adjust the viscosity of the insulating composition to 50~150 mPa·s. Immerse the aluminum casing in the insulating composition, hold for 5~10s, and then pull it out at a constant speed (50~200 mm / min) to form a uniform wet film.

[0058] In one embodiment of this application, the drying temperature is 20~30°C, the drying time is 1~5 min; and / or, the heating time is 10~20 min.

[0059] The preferred drying temperature and time are within the above range, which helps to remove most of the solvent from the wet film. The preferred heating time is within the above range, which helps to promote the full cross-linking reaction of the above components and form a dense insulating protective film.

[0060] In another typical embodiment of this application, a battery device is provided, which includes the above-mentioned battery cell, and the battery device includes any one or more of battery modules, battery packs, and energy storage batteries.

[0061] Battery devices including the aforementioned battery cells have superior overall performance in terms of high power output, wide temperature range operation, and long cycle life, making them suitable for energy storage systems and power battery applications with high requirements for energy density, safety, and reliability.

[0062] In another typical embodiment of this application, an electrical device is provided, which includes the battery device described above, the battery device being used to provide electrical energy.

[0063] The aforementioned battery devices enable electrical devices to have higher energy efficiency, longer service life and more stable power output characteristics, making them suitable for applications such as energy storage systems and electric vehicles with stringent requirements for safety and cycle performance.

[0064] In another typical embodiment of this application, an energy storage device is provided, which includes the battery device described above, the battery device being used to store electrical energy.

[0065] Energy storage devices including the aforementioned battery devices can effectively reduce interface impedance, suppress dendrite growth, and improve the cycle life and rate performance of batteries in a wide temperature range environment. They are suitable for energy storage systems with comprehensive requirements for energy density, safety and low temperature adaptability, and are especially suitable for high-reliability energy storage application scenarios under solid-state battery architecture.

[0066] Furthermore, the battery cell using the casing containing the aforementioned insulating protective film, as described in this application, not only maintains high specific capacity but also achieves excellent long-cycle performance, making it more suitable for the needs of long-term energy storage systems. This battery cell possesses high volumetric energy density and excellent cycle stability, efficiently supporting the operation of large-scale energy storage power stations at 4-hour (4h) and 8-hour (8h) levels, meeting the stringent requirements for high-capacity batteries in application scenarios such as grid peak shaving and smooth output of renewable energy.

[0067] The beneficial effects of this application will be further illustrated below with reference to the embodiments.

[0068] Example 1

[0069] Adopting such Figure 1 The battery cell preparation method shown includes the following process for processing the casing:

[0070] Preparation of the prepolymer: In a 500 mL three-necked flask equipped with a stirrer and a condenser, 0.11 mol of hydroxyl-terminated polydimethylsiloxane (hydroxyl value 50 mg KOH / g) was added under a nitrogen atmosphere, dissolved in 50 mL of anhydrous toluene. Then, 0.1 mol of phenyl dichlorophosphate (dissolved in 20 mL of toluene) was slowly added dropwise, while simultaneously adding 0.22 mol of pyridine catalyst to initiate the polycondensation reaction. The polycondensation reaction was carried out by reacting at room temperature (25 °C) for 4 h, followed by a further reaction at 60 °C for 2 h. After the reaction was complete, pyridine hydrochloride was removed by filtration, and the solvent and low-boiling substances were removed by vacuum distillation, yielding a pale yellow viscous liquid, i.e., the prepolymer. The number average molecular weight of the prepolymer was 4000 Da, and the yield was 85%.

[0071] The insulating composition, by weight, comprises: 50 parts of prepolymer, 5 parts of coupling agent diethoxyphosphorylethyltriethoxysilane, 3 parts of curing agent blocked isocyanate (Desmodur BL 3175), 35 parts of solvent, and 1.5 parts of additives; wherein the solvent is 20 parts of isopropanol and 15 parts of propylene glycol methyl ether, and the additives are 0.3 parts of leveling agent BYK-333, 0.2 parts of defoamer BYK-024, and 1 part of phthalocyanine blue pigment.

[0072] Preparation of the insulating composition: Under light-proof and moisture-proof conditions, the prepolymer and solvent were first mixed for 12 min to obtain a first mixture. A coupling agent and a curing agent were added to the first mixture, and the mixture was second mixed for 5 min to obtain a second mixture. An additive was added to the second mixture, and the mixture was third mixed for 10 min to obtain the insulating composition, with the viscosity adjusted to 200 mPa·s (25°C).

[0073] Housing pretreatment: A 314Ah square aluminum battery cell (unencapsulated) was degreased and cleaned by ultrasonic cleaning with a 40℃ alkaline cleaning agent (sodium hydroxide solution) for 5 minutes, followed by rinsing with deionized water and drying at 60℃. A 1wt% fluorozirconic acid solution was then sprayed on for chemical conversion treatment, forming a 25nm thick active layer on the outer surface of the aluminum shell. After washing and drying, the pretreated aluminum shell was obtained.

[0074] In-situ film formation: The insulating composition was sprayed onto the pretreated aluminum shell outer surface using an automatic spray gun (1.0 mm nozzle, 0.3 MPa air pressure) to form a wet film with a thickness of 40 μm. After drying at room temperature (25 °C) for 3 min, it was then placed in an infrared drying tunnel and heated at 80 °C for 15 min for curing. After natural cooling, an aluminum shell containing an insulating protective film with a thickness of 25 μm was obtained.

[0075] Example 2

[0076] The difference from Example 1 is that only degreasing and cleaning are performed in the shell pretreatment, without chemical conversion treatment, to obtain a pretreated aluminum shell, and finally an aluminum shell containing an insulating protective film.

[0077] Example 3

[0078] The difference from Example 1 is that the curing agent in the insulating composition is replaced with a microencapsulated amine curing agent (polyetheramine D230@PMMA microcapsules), which ultimately yields an aluminum shell containing an insulating protective film.

[0079] Example 4

[0080] The difference from Example 1 is that, by weight, the insulating composition consists of: 50 parts of prepolymer, 3 parts of coupling agent, 3 parts of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0081] Example 5

[0082] The difference from Example 1 is that, by weight, the insulating composition consists of: 50 parts of prepolymer, 7 parts of coupling agent, 3 parts of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0083] Example 6

[0084] The difference from Example 1 is that, by weight, the insulating composition consists of: 50 parts of prepolymer, 5 parts of coupling agent, 1 part of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0085] Example 7

[0086] The difference from Example 1 is that, by weight, the insulating composition consists of 50 parts of prepolymer, 5 parts of coupling agent, 5 parts of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0087] Example 8

[0088] The difference from Example 1 is that, by weight, the insulating composition consists of: 30 parts of prepolymer, 5 parts of coupling agent, 3 parts of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0089] Example 9

[0090] The difference from Example 1 is that, by weight, the insulating composition consists of 60 parts of prepolymer, 5 parts of coupling agent, 3 parts of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0091] Example 10

[0092] The difference from Example 1 is that the coupling agent in the insulating composition is replaced with aluminum acetylacetonate and silane coupling agent KH-560 (γ-glycidyl etheroxypropyltrimethoxysilane) in a mass ratio of 1:1, and an aluminum shell containing an insulating protective film is finally obtained.

[0093] Example 11

[0094] The difference from Example 1 is that the coupling agent in the insulating composition is replaced with a zirconium aluminate coupling agent (isopropoxyzirconium aluminate), and an aluminum shell containing an insulating protective film is finally obtained.

[0095] Example 12

[0096] The difference from Example 1 is that the curing agent in the insulating composition is replaced with a cationic photoinitiator (diphenyl iodonium salt), and an aluminum shell containing an insulating protective film is finally obtained.

[0097] Example 13

[0098] The difference from Example 1 is that the thickness of the active layer on the surface of the aluminum shell after pretreatment is 50nm, and the final result is an aluminum shell containing an insulating protective film.

[0099] Example 14

[0100] The difference from Example 1 is that the thickness of the active layer on the surface of the aluminum shell after pretreatment is 5nm, and the final result is an aluminum shell containing an insulating protective film.

[0101] Example 15

[0102] The difference from Example 1 is that the chemical conversion treatment in the shell pretreatment is replaced by silane modification treatment, that is, silane coupling agent KH-550 is used to carry out silane modification treatment at 180°C for 40 minutes, and finally an aluminum shell containing an insulating protective film is obtained.

[0103] Example 16

[0104] The difference from Example 1 is that no pretreatment is performed on the aluminum shell, and the final product is an aluminum shell containing an insulating protective film.

[0105] Example 17

[0106] The difference from Example 1 is that, by weight, the insulating composition consists of: 40 parts of prepolymer, 4 parts of coupling agent, 2 parts of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0107] Example 18

[0108] The difference from Example 1 is that, by weight, the insulating composition consists of: 55 parts of prepolymer, 6 parts of coupling agent, 4 parts of curing agent, 35 parts of solvent and 1.5 parts of additives; wherein, the curing agent is a microencapsulated amine curing agent (polyetheramine D230@PMMA microcapsules), and an aluminum shell containing an insulating protective film is finally obtained.

[0109] Example 19

[0110] The difference from Example 1 is that, by weight, the insulating composition consists of: 45 parts of prepolymer, 7 parts of coupling agent, 2 parts of curing agent, 35 parts of solvent and 1.5 parts of additives, ultimately yielding an aluminum shell containing an insulating protective film.

[0111] Example 20

[0112] The difference from Example 1 is that the coating method was changed from spraying to dip coating, and the viscosity of the insulating composition was adjusted to 100 mPa·s. The pretreated aluminum shell was immersed in the insulating composition, held for 8 seconds, and then pulled up at a constant speed (150 mm / min) to form a wet film, which was then cured to obtain an aluminum shell containing an insulating protective film.

[0113] Example 21

[0114] The difference from Example 3 is that the coating method was changed from spraying to dip coating, and the viscosity of the insulating composition was adjusted to 100 mPa·s. The pretreated aluminum shell was immersed in the insulating composition, held for 8 seconds, and then pulled up at a constant speed (150 mm / min) to form a wet film, which was then cured to obtain an aluminum shell containing an insulating protective film.

[0115] Example 22

[0116] The difference from Example 1 lies in the preparation of the prepolymer: hydroxyl-terminated polymethylphenylsiloxane and methyl dichlorophosphate were subjected to a polycondensation reaction. The polycondensation reaction process was as follows: the reaction was first carried out at room temperature (25°C) for 4 hours, and then continued at 80°C for another 4 hours to obtain the prepolymer with a molecular weight of 5000 Da, ultimately yielding an aluminum shell containing an insulating protective film.

[0117] Example 23

[0118] The difference from Example 1 lies in the preparation of the prepolymer: hydroxyl-terminated polymethylphenylsiloxane and methyl dichlorophosphate were subjected to a polycondensation reaction. The polycondensation reaction process was as follows: the reaction was first carried out at room temperature (25°C) for 4 hours, and then continued at 90°C for 9 hours to obtain the prepolymer with a molecular weight of 8000 Da, ultimately yielding an aluminum shell containing an insulating protective film.

[0119] Example 24

[0120] The difference from Example 1 is that in-situ film formation was used: the insulating composition was sprayed onto the pretreated outer surface of the aluminum shell to form a wet film with a thickness of 100 μm. It was dried at 20°C for 5 min, then cured by heating at 60°C for 20 min, and allowed to cool naturally to obtain an aluminum shell containing an insulating protective film with a thickness of 30 μm.

[0121] Example 25

[0122] The difference from Example 1 is that in-situ film formation was used: the insulating composition was sprayed onto the pretreated outer surface of the aluminum shell to form a wet film with a thickness of 30 μm. It was dried at 30°C for 1 min, then cured by heating at 90°C for 10 min, and allowed to cool naturally to obtain an aluminum shell containing an insulating protective film with a thickness of 10 μm.

[0123] Comparative Example 1

[0124] The difference from Example 1 is that a blue film (PET substrate pressure-sensitive tape) is used to insulate the outer surface of the aluminum shell.

[0125] Comparative Example 2

[0126] The difference from Example 1 is that, by weight, the insulating composition consists of: 50 parts of prepolymer, 1 part of coupling agent, 3 parts of curing agent, 35 parts of solvent and 0.5 parts of additives, without the addition of phthalocyanine blue pigment, and finally an aluminum shell containing an insulating protective film is obtained.

[0127] Test method:

[0128] The properties of the insulating protective film were tested using the following methods:

[0129] Adhesion: Tested according to the method specified in GB / T 9286-2021 "Paints and Varnishes - Cross-cut Test". The coating is cut into a grid pattern using a cross-cutting tool, and then peeled off using pressure-sensitive adhesive tape. The grade is determined based on the area of ​​coating peeling. Requirement: ≤ Grade 1.

[0130] Insulation resistance: Tested according to the method specified in GB / T 31838.2-2019 "Test Methods for Volume Resistivity and Surface Resistivity of Solid Insulating Materials". Test voltage 500V, electrochemical time 1 minute, requirement ≥5×10 11 Ω.

[0131] Dielectric strength: Tested according to the short-time method specified in ASTM D149. A 60Hz AC voltage is used, and the voltage is increased at a uniform rate until breakdown. The ratio of breakdown voltage to film thickness is calculated, and it is required to be ≥60kV / mm.

[0132] Flexibility: Tested according to the method specified in GB / T 1731-2020 "Determination of Flexibility of Paint Film and Putty Film". Bend the test piece 180° on a 2mm diameter shaft and check for cracks in the coating.

[0133] Salt spray corrosion resistance: The test was conducted according to the neutral salt spray test (NSS) method in GB / T 10125-2021 "Artificial Atmosphere Corrosion Test - Salt Spray Test". The test temperature was 35±2℃, and a 5% (w / w) NaCl solution was sprayed continuously for 72 hours. No abnormalities were observed in the test results.

[0134] Electrolyte resistance test: The test piece with the insulating protective film was completely immersed in lithium-ion battery electrolyte (1M LiPF6, ethylene carbonate EC, ethyl methyl carbonate EMC, and dimethyl carbonate DMC in a volume ratio of 1:1:1) and left to stand in a 60℃ constant temperature oven for 7 days. After removal, it was cleaned and dried, and the changes in the appearance of the film were observed and the adhesion retention was tested.

[0135] Overall yield: 500 irregularly shaped aluminum shells are processed in batches according to the above shell processing method. Those that pass the performance test are recorded as qualified aluminum shells. Overall yield = number of qualified aluminum shells / total number of tested aluminum shells.

[0136] The test results are shown in Table 1.

[0137] Table 1

[0138]

[0139] In the flexibility test, slight cracks indicate that small cracks or fissures appear in the bending test, but there is no breakage or peeling.

[0140] No abnormalities in the salt spray corrosion test indicates that the sample's appearance, adhesion, and insulation properties showed no observable deterioration or failure after the test. Slight corrosion indicates that the sample showed a small amount of pitting or discoloration after the test, but the corrosion area did not expand significantly.

[0141] No abnormalities in the electrolyte resistance test indicate that the insulating protective film did not expand in volume after immersion in the electrolyte, and no observable deterioration or failure was observed in the appearance, adhesion, and insulation performance of the sample after the test. Slight swelling indicates that the insulating protective film expanded to a certain extent after immersion in the electrolyte, but without cracking, peeling, or a significant decrease in insulation performance. Peeling indicates that the insulating protective film partially or completely peeled off from the shell surface, losing its protective function.

[0142] "Not applicable" means that the test cannot be performed on the current sample or the test results are not relevant.

[0143] The insulating protective film of this application has good insulating protection and can protect the battery cell, thereby giving the battery with the aluminum shell good safety.

[0144] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:

[0145] This application utilizes an insulating composition with the aforementioned components and weight proportions to form an in-situ film on the surface of the battery cell casing. This not only provides excellent insulation and protection but also fundamentally avoids the inherent defects of the lamination process. Specifically, 1) the prepolymer formed from the aforementioned polymer monomers serves as the film-forming body, providing excellent insulation and flexibility. Phosphoryl halide organic compounds and hydroxyl-terminated polysiloxanes exhibit a phosphorus-silicon synergistic flame-retardant and insulating effect. Utilizing the char-forming flame-retardant mechanism of phosphorus in phosphoryl halide organic compounds and the advantage of silicon in hydroxyl-terminated polysiloxanes in improving the density of the protective layer, even ultra-thin (approximately 20 μm) films can meet the requirements for 500V insulation and breakdown resistance. 2) The coupling agent enables the insulating protective film to form a chemical covalent bond with the casing, thereby increasing the bonding strength between them, far exceeding the physical adhesion of films like blue films. It also improves the battery's aging resistance and electrolyte resistance. 3) The curing agent can control the curing speed and activation temperature of the insulating composition, promoting the cross-linking and curing of the above components, thereby achieving rapid film formation at a lower temperature and obtaining a dense insulating protective film, thus better protecting the battery cell. In summary, the insulating protective film obtained from the above insulating composition not only has good insulation and protection properties, flame retardant properties, and electrolyte corrosion resistance, but also has a fast film formation speed, is not prone to aging and peeling, can be retained as a permanent protective layer, and is suitable for complex battery shapes.

[0146] The above are merely embodiments of the present invention and are not intended to limit the invention. Those skilled in the art will recognize that the present invention can have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A battery cell comprising a cell having a casing and an insulating protective film disposed on the outer surface of the casing, the insulating protective film being prepared from an insulating composition, characterized in that, The insulating composition comprises, by weight, 30 to 60 parts of prepolymer, 2 to 8 parts of coupling agent and 1 to 5 parts of curing agent; The monomers of the prepolymer include phosphoryl halides and polysiloxanes containing terminal hydroxyl groups.

2. The battery cell according to claim 1, characterized in that, The molar ratio of the phosphoryl halide organic compound to the hydroxyl-terminated polysiloxane is 1:(1~1.2); the phosphoryl halide organic compound is selected from any one or more of phenyl dichlorophosphate, methyl dichlorophosphate, and ethyl dichlorophosphate; the hydroxyl-terminated polysiloxane is selected from any one or more of hydroxyl-terminated polydimethylsiloxane, hydroxyl-terminated polymethylphenylsiloxane, and hydroxyl-terminated polydiphenylsiloxane; the number average molecular weight of the prepolymer is 2000~5000 Da.

3. The battery cell according to claim 1, characterized in that, The coupling agent is selected from any one or more of the following: a complex of aluminum acetylacetonate and a silane coupling agent, a phosphate-modified silane coupling agent, and a zirconium aluminate coupling agent; wherein the mass ratio of aluminum acetylacetonate to the silane coupling agent is (0.5~2):1; the phosphate-modified silane coupling agent is selected from any one or more of the following: triethoxysilylpropyl phosphate, diethoxyphosphorylethyltriethoxysilane, and trimethoxysilylpropyl phosphate; the zirconium aluminate coupling agent is selected from any one or more of the following: a complex of tetra(triethanolamine)zirconate and aluminate, isopropoxyzirconium aluminate, and n-butoxyzirconium aluminate.

4. The battery cell according to claim 1, characterized in that, The curing agent is a cationic photoinitiator and / or a latent curing agent; wherein the cationic photoinitiator is selected from any one or more of diphenyliodonium salt, triphenylsulfonium salt and dialkylbenzoylmethylsulfonium salt; and the latent curing agent is a blocked isocyanate and / or a microencapsulated amine curing agent.

5. The battery cell according to any one of claims 1 to 4, characterized in that, The mass ratio of the prepolymer, the coupling agent and the curing agent is 100:(3~15):(2~10).

6. The battery cell according to any one of claims 1 to 4, characterized in that, The insulating composition further includes additives and solvents; The additive is selected from any one or more of leveling agents, defoamers, and colorants, with the leveling agent comprising 0.1 to 1 part by weight; the defoamer comprising 0.1 to 0.5 parts by weight; and the colorant comprising 0.5 to 3 parts by weight. The solvent is 20 to 50 parts by weight, and the solvent is selected from any one or more of isopropanol, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl acetate, acetone and butanone.

7. The battery cell according to any one of claims 1 to 4, characterized in that, The housing is made of aluminum; and / or the thickness of the insulating protective film is 10~30μm.

8. A method for preparing a battery cell, comprising sequentially stacking and assembling a positive electrode, a separator, and a negative electrode to obtain a battery cell, inserting the battery cell into a housing, injecting electrolyte, and then encapsulating it to obtain the battery cell, characterized in that, The method for processing the housing includes: By weight, raw materials comprising 30-60 parts of prepolymer, 2-8 parts of coupling agent and 1-5 parts of curing agent are mixed to obtain an insulating composition; the insulating composition is coated on the outer surface of the shell and then cured to obtain a shell containing an insulating protective film. The monomers of the prepolymer include phosphoryl halide organic compounds and polysiloxanes containing terminal hydroxyl groups; The curing process includes sequential drying and heating; the drying temperature is lower than the heating temperature; the heating temperature is 60~90℃.

9. The method for preparing a battery cell according to claim 8, characterized in that, The method for processing the housing further includes: pre-treating the housing before coating the insulating composition onto the outer surface of the housing to obtain a pre-treated housing; and curing the housing after coating the insulating composition onto the outer surface of the pre-treated housing to obtain the housing containing the insulating protective film. The pretreatment includes degreasing and / or chemical conversion treatment; the shell is degreased and cleaned with a cleaning solution, which is an alkaline cleaning solution and / or a surfactant; the chemical conversion treatment includes titanium-zirconium conversion treatment and / or silane modification treatment; an active layer is formed on the outer surface of the shell through the chemical conversion treatment, and the thickness of the active layer is 5~50 nm.

10. The method for preparing a single battery cell according to claim 8, characterized in that, The preparation process of the insulating composition includes: first mixing raw materials including the prepolymer and solvent to obtain a first mixture; second mixing raw materials including the first mixture, the coupling agent and the curing agent to obtain a second mixture; and third mixing raw materials including the second mixture and additives to obtain the insulating composition. The first mixing time is 10-15 minutes; the second mixing time is 5-10 minutes; and the third mixing time is 5-15 minutes. And / or, the prepolymer is obtained by polycondensation reaction of a polymeric monomer raw material comprising the phosphoryl halide organic compound and the polysiloxane containing terminal hydroxyl groups; the molar ratio of the phosphoryl halide organic compound and the polysiloxane containing terminal hydroxyl groups is 1:(1~1.2); the temperature of the polycondensation reaction is 20~80℃, and the time of the polycondensation reaction is 2~8h.

11. The method for preparing a battery cell according to any one of claims 8 to 10, characterized in that, The insulating composition is coated on the outer surface of the housing to form a wet film, and after curing, the housing containing the insulating protective film is obtained; The thickness of the wet film is 30~100μm; the coating method is selected from any one or more of spraying, dip coating, roller coating and spin coating.

12. The method for preparing a battery cell according to any one of claims 8 to 10, characterized in that, The drying temperature is 20~30℃, the drying time is 1~5min; and / or, the heating time is 10~20min.

13. A battery device, characterized in that, The battery device includes the battery cell according to any one of claims 1 to 7, and the battery device includes any one or more of the following: battery module, battery pack, and energy storage battery.

14. An electrical appliance, characterized in that, The electrical device includes the battery device of claim 13, the battery device being used to provide electrical energy.

15. An energy storage device, characterized in that, The energy storage device includes the battery device of claim 13, the battery device being used to store electrical energy.