Battery cell seal structure for bipolar current collector and method of manufacturing the same
By introducing a serrated trench structure and microencapsulation technology into the bipolar battery, efficient bonding and corrosion resistance of the aluminum and copper layers are achieved, solving the stability problem of the bipolar battery sealing structure and improving the volumetric energy density and safety of the battery.
Patent Information
- Application Number
- CN202611452679.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-20
AI Technical Summary
In existing technologies, the sealing structure of bipolar batteries cannot simultaneously achieve efficient bonding of aluminum and copper layers, resistance to electrolyte corrosion, and long-term stability, leading to sealing failure and affecting battery safety and lifespan.
By employing a synergistic enhancement effect of mechanical locking structure and chemical bonding, combined with microcapsule in-situ release technology, a copper layer is plated on an aluminum substrate to form a serrated groove. Modified hydrogenated nitrile rubber and microcapsule encapsulation active coupling agent are used to achieve "dry storage-wet activation" delayed bonding and construct a three-dimensional cross-linked network.
It improves the interfacial peel strength and bonding power, ensures the long-term stability of the sealant, reduces the space occupied by the sealant layer, and improves the volumetric energy density and safety of the battery.
Smart Images

Figure CN123143618A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bipolar current collector technology, specifically to a sealing structure for a bipolar current collector cell and its preparation method. Background Technology
[0002] Bipolar batteries represent a key development direction for future high-energy-density energy storage devices. This technology coats the positive and negative electrode active materials on opposite sides of the same current collector, eliminating the need for traditional inter-cell electrical connections and significantly improving the battery's volumetric energy density and power density. However, bipolar current collectors typically employ an aluminum / copper composite structure, presenting extremely stringent sealing challenges when assembling them into cell modules. The sealing material must simultaneously bond the aluminum and copper layers. The aluminum layer has a dense oxide film on its surface, resulting in low surface energy and difficulty in adhesion; the copper layer is prone to oxidation at the high potential of the positive electrode and exhibits poor adhesion to most polymer materials. Furthermore, the sealant comes into direct contact with the electrolyte and must withstand corrosion from organic carbonate solvents and lithium salts. In addition, the sealing structure requires high interlayer peel strength and a pressure resistance greater than 0.5 MPa. Any seal failure can lead to electrolyte leakage, severely impacting battery safety and lifespan.
[0003] To address the aforementioned sealing challenges, existing technologies often employ a single homogeneous sealant, such as fluororubber or acrylic adhesive, increasing the sealant layer thickness to over 500 μm to improve pressure resistance and sealing reliability. However, this solution has significant drawbacks: the thick sealant layer lacks cohesive strength, making it prone to seal failure under long-term creep; the excessively thick sealant layer occupies valuable battery stacking space, reducing the overall volumetric energy density of the battery; more critically, the single sealant only achieves physical adsorption with the metal surface, relying on van der Waals forces for adhesion, which weakens significantly under long-term immersion in electrolyte, failing to meet the long-term stable sealing requirements of bipolar batteries.
[0004] Therefore, how to develop a composite sealing structure that can achieve efficient bonding between aluminum and copper layers, withstand electrolyte corrosion, and maintain long-term stability has become a key technical problem that urgently needs to be solved in the industrialization process of bipolar battery technology. Summary of the Invention
[0005] The purpose of this invention is to provide a sealing structure for a bipolar current collector cell and its preparation method. The mechanical locking structure and chemical bonding work together to enhance the interfacial peel strength. Combined with microcapsule in-situ release technology, it addresses the weak points of delayed bonding during "dry storage-wet activation". In addition, the sealant occupies little space, which can meet the application requirements of high volumetric energy density of devices and solve the problems raised in the prior art.
[0006] To achieve the above objectives, the present invention provides the following technical solution: Step 1: A copper layer is plated on an aluminum substrate to obtain a bipolar current collector. A serrated groove is formed at the edge regions of the upper and lower ends of the bipolar current collector by femtosecond laser etching. Step 2: Pre-treat the sawtooth grooves on the surface of the aluminum substrate, immerse the sawtooth grooves on the surface of the copper layer in γ-mercaptopropyltrimethoxysilane solution, and dry to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: After plasticizing, hydrogenated nitrile rubber is mixed with fumed silica to obtain a compound; the microcapsules and the compound are mixed evenly, and peroxide vulcanizing agent, antioxidant, plasticizer and polytetrafluoroethylene micro powder are added and mixed evenly to obtain a sealant. Step 4: Apply sealant to the surface-treated serrated grooves on the bipolar current collector, apply negative electrode active slurry to the copper side and positive electrode active slurry to the aluminum side, dry and roll to obtain bipolar electrode sheets, stack and hot press bipolar electrode sheets, polypropylene diaphragm and bipolar electrode sheets in sequence to obtain the sealing structure of the bipolar current collector battery cell.
[0007] Furthermore, in step 2, the pretreatment is either atmospheric pressure plasma treatment or anodic oxidation followed by atmospheric pressure plasma treatment.
[0008] Furthermore, the specific steps of the anodizing process are as follows: The surface of the aluminum substrate with serrated grooves in the bipolar current collector is placed in an electrolyte solution, which is a mixture of oxalic acid, anhydrous ethanol and deionized water. The electrolysis temperature is 19~21℃, the voltage is 155~165V, and the mixture is magnetically vibrated and stirred for 30~60 minutes to form porous alumina on the inner wall of the grooves.
[0009] Furthermore, the porous alumina has the following parameters: pore size 50~100nm and depth 490~510nm.
[0010] Furthermore, the anhydrous ethanol and deionized water are mixed in a volume ratio of 1:1, and the oxalic acid concentration is 0.3 mol / L.
[0011] Furthermore, the preparation steps of the microcapsules are as follows: KH-792, dibutyltin dilaurate, propylene glycol methyl ether acetate, and polyimide short fibers were mixed and stirred to obtain an oil phase core. Span 80 was added and stirred evenly. Toluene diisocyanate, hexamethylene diisocyanate, and polycaprolactone diol were added dropwise and stirred evenly to obtain a total oil phase. Diethylenetriamine and deionized water were mixed and stirred to obtain an aqueous phase. The total oil phase was added dropwise to the aqueous phase at a speed of 3500~4000 r / min. After the addition was complete, shear emulsification was maintained for 2~4 min. The temperature was raised to 65~70℃ and the reaction was carried out at a constant temperature of 300~350 r / min for 2~3 h to form a polyurea-polyurethane wall material. The material was filtered, washed, and dried to obtain microcapsules.
[0012] Furthermore, the microcapsule particle size is 20~40μm.
[0013] Furthermore, the parameters of the sawtooth groove are: spacing 80~120μm, depth 4~15μm, opening width 20~40μm, tooth tip angle 40~50°, and surface roughness 1~5μm.
[0014] Furthermore, the sealant comprises, by mass percentage, 5-10% fumed silica, 8-15% microcapsules, 1-2% peroxide vulcanizing agent, 0.5-2% antioxidant, 1-2% plasticizer, 0-5% polytetrafluoroethylene micro powder, and the balance being hydrogenated nitrile rubber.
[0015] Furthermore, the antioxidant is a mixture of antioxidant BLE and antioxidant KY-405 in a weight ratio of 2:3, the plasticizer is dibutyl phthalate, and the peroxide vulcanizing agent is bis-tert-butylperoxyisopropylbenzene.
[0016] Furthermore, the working conditions for femtosecond laser etching in step 1 are: scanning speed 490~510 mm / s, wavelength 1000~1030 nm, pulse width 280~320 fs, frequency 190~210 kHz, and power 8~12 W; the working conditions for pretreatment in step 2, when it is atmospheric pressure plasma treatment, are: gas is one of argon, oxygen, or a mixture of argon and oxygen in a volume ratio of 9:1, power is 100~200 W, and time is 2~5 min. The mass concentration of the γ-mercaptopropyltrimethoxysilane solution is 1-3%, the immersion time is 25-35s, the drying temperature is 75-85℃, and the drying time is 3-7min; the thickness of the coated adhesive layer in step 4 is 160-200μm, and the hot pressing conditions are: first stage temperature 120-140℃, pressure 0.3-0.5MPa, time 8-12min, second stage temperature 145-155℃, pressure 0.5-0.7MPa, time 3-7min.
[0017] Furthermore, the hydrogenated nitrile butadiene rubber is a modified hydrogenated nitrile butadiene rubber, and the preparation steps are as follows: Hydrogenated nitrile butadiene rubber, glycidyl methacrylate, and diisopropylbenzene peroxide were mixed at a mass ratio of 10:1:0.15 at 165~175℃ for 2~6 min to obtain modified hydrogenated nitrile butadiene rubber.
[0018] Furthermore, the fumed silica is modified fumed silica, and the preparation steps are as follows: Xylene and pentamethylpiperidinol were mixed and stirred. 3-propyltrimethoxysilane 3-isocyanate was added while stirring continuously. The mixture was heated to 35-45°C and stirred for 2.5-3.5 hours to obtain a mixed solution. Fumed silica was dispersed in xylene and sonicated for 13-17 minutes. It was then added to the mixed solution, heated to 115-125°C, and stirred continuously for 11-13 hours. The mixture was cooled to 20-25°C, centrifuged, washed repeatedly with ethanol 3-5 times, dried at 55-65°C for 25-35 minutes, and then heated to 115-125°C and dried for 11-13 hours to obtain modified fumed silica.
[0019] Furthermore, the mass ratio of xylene, pentamethylpiperidinol, propyltrimethoxysilane 3-isocyanate and fumed silica is 45:0.2:0.22:0.1.
[0020] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention describes a sealing structure for a bipolar current collector cell and its preparation method. By introducing a sawtooth groove structure and microcapsule delayed release technology, the sealing problem of bipolar batteries is improved. Specifically, a femtosecond laser is used to form sawtooth grooves at the edge regions of the upper and lower ends of the metal current collector, creating a mechanical interlocking structure that enhances peel strength. This structure can be prepared using conventional laser equipment, demonstrating good industrial feasibility. Simultaneously, the active coupling agent is encapsulated in polyurea-polyurethane double-layer microcapsules, achieving "dry storage-wet activation" of the sealant, extending its shelf life significantly beyond that of traditional coupling agent-containing adhesives. Under the synergistic physical-chemical mechanism, the mechanical interlocking structure effectively prevents rapid crack propagation and increases fracture energy; chemical bonding inhibits interfacial separation and enhances adhesive work. The synergistic effect of both significantly enhances interfacial toughness. Based on this, the present invention ensures high reliability by enhancing the microstructure rather than thickening the macrostructure, and achieves ultra-thin adhesive layer with a thickness that can be controlled below 200μm. Compared with traditional adhesive layers with a thickness of more than 500μm, this design increases the number of cells stacked, thereby directly improving the overall volumetric energy density of the battery pack.
[0021] 2. The bipolar current collector cell sealing structure and its preparation method described in this invention construct a high-strength, high-durability three-dimensional cross-linked network based on a serrated microstructure through multi-level chemical synergy: the aluminum side is anodized and plasma activated to form porous alumina and introduce active hydroxyl groups; the copper side undergoes hydrolysis and condensation of γ-mercaptopropyltrimethoxysilane to form Cu-S coordination bonds with the copper surface through thiol groups; during hot pressing, the epoxy groups of the epoxy-modified hydrogenated nitrile rubber in the sealant undergo ring-opening etherification with the hydroxyl groups on the aluminum side, while the thiol groups participate in the coordination bonding of the copper interface and the rubber matrix, realizing the chemical anchoring of the heterogeneous interface and the construction of a gradient transition layer; the isocyanate and amine / alcohol interfacial polymerization in the sealant system... The reaction forms polyurea-polyurethane microcapsules coated with KH-792 repair agent and dibutyltin dilaurate catalyst. When cracks initiate, these microcapsules can release repair components in situ to achieve self-repair function. Hindered amine light stabilizer-modified fumed silica, through covalent grafting, inhibits nanoparticle aggregation and imparts free radical scavenging ability. Together with BLE / KY-405 composite antioxidant, it forms a system that synergistically enhances interfacial bonding strength and long-term durability. Finally, through the synergistic effect of peroxide-induced free radical cross-linking sulfurization and the above-mentioned coordination bonds, a three-dimensional cross-linked network with high interfacial bonding strength, crack self-repair ability, and long-term durability is formed on the basis of physical interlocking of serrated grooves etched by femtosecond laser. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the bipolar current collector of the present invention; Figure 2 This is a schematic diagram of the bipolar cell assembly structure of the present invention; Figure 3 This is a product diagram of the sealing structure of the bipolar current collector cell in Embodiment 1 of the present invention. Detailed Implementation
[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] In the following specific implementation, Bipolar current collector: 43μm aluminum foil, 1μm copper plating, with a width of 6mm at the top and bottom edge areas; γ-Mercaptopropyltrimethoxysilane: Industrial grade, 98% purity; Hydrogenated nitrile butadiene rubber: Acrylonitrile content 18~22%, Mooney viscosity 78~92; Fumed silica: specific surface area 175~225m² 2 / g, particle size 12nm; Anti-aging agent BLE: 99% purity; Anti-aging agent KY-405: 99% purity; Polytetrafluoroethylene (PTFE) micro powder: particle size 5μm, specific surface area 7.5m². 2 / g; N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane: KH-792, industrial grade, 99% purity; Polyimide short fibers: length 50~100μm, diameter 5μm; Emulsifier: Span 80, HLB value 8~10; 3-Propylisocyanatetrimethoxysilane: Industrial grade, 98% purity; Graphite: Specific surface area 1.5m² 2 / g, density 1.0g / cm³ 3 ; Conductive carbon black: total iron content 2ppm, specific surface area 62m² 2 / g, carbon content 99.5%; Carbon nanotubes: diameter 7~11nm, length 5~20μm; Conductive carbon: Super P, model number ENSACO, specific surface area 65m² 2 / g; Polyvinylidene fluoride: molecular weight 1,000,000, particle size 30 μm; Di-tert-butylperoxyisopropylbenzene, dibutyl phthalate, oxalic acid, anhydrous ethanol, dibutyltin dilaurate, propylene glycol methyl ether acetate, toluene diisocyanate, hexamethylene diisocyanate, diethylenetriamine, polycaprolactone diol, glycidyl methacrylate, dicumyl peroxide, xylene and pentamethylpiperidinol, carboxymethyl cellulose and lithium iron phosphate were all of analytical grade.
[0025] Example 1: A method for preparing a sealing structure for a bipolar current collector cell, comprising the following steps: Step 1: A copper layer is deposited on an aluminum substrate to obtain a bipolar current collector. The current collector is then etched by a femtosecond laser at a scanning speed of 500 mm / s, a wavelength of 1030 nm, a pulse width of 300 fs, a frequency of 200 kHz, and a power of 8 W. This forms a serrated groove with a spacing of 100 μm, a depth of 10 μm, an opening width of 30 μm, a tooth tip angle of 45°, and a surface roughness of 1 μm at the edge regions of the upper and lower ends of the bipolar current collector. Step 2: Perform atmospheric pressure plasma treatment on the sawtooth grooves on the surface of the aluminum substrate. The gas is argon, the power is 150W, and the time is 3min. Immerse the sawtooth grooves on the surface of the copper layer in a 2% γ-mercaptopropyltrimethoxysilane solution for 30s. Dry at 80℃ for 5min to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: Mix 65g KH-792, 5g dibutyltin dilaurate, 20g propylene glycol methyl ether acetate, and 10g polyimide short fibers to obtain the oil phase core. Add 5g Span 80 and stir until homogeneous. Dropwise add 18g toluene diisocyanate, 12g hexamethylene diisocyanate, and 6g polycaprolactone diol and stir until homogeneous to obtain the total oil phase. Mix 10g diethylenetriamine and 300mL deionized water to obtain the aqueous phase. Slowly add the total oil phase to the aqueous phase at 4000r / min. After the addition is complete, maintain shear emulsification for 4min. Heat to 70℃ and react at a constant temperature of 350r / min for 3h to form polyurea-polyurethane wall material. Filter, wash, and dry to obtain microcapsules. Step 4: By mass percentage, 80.5% hydrogenated nitrile rubber is plasticized on a two-roll mill, and 6% fumed silica is added and mixed evenly to obtain a compound; 10% microcapsules with a particle size of 30μm are mixed evenly with the compound in a vacuum kneader at a temperature of 45℃, and 2% peroxide vulcanizing agent, 0.5% antioxidant and 1% dibutyl phthalate are added and mixed evenly to obtain a sealant; Step 5: Apply sealant to the surface-treated serrated grooves of the bipolar current collector using slit coating. The sealant layer thickness is 180μm. Coat the copper surface with a negative electrode active slurry made of graphite, conductive carbon black, carbon nanotubes, and carboxymethyl cellulose in a mass ratio of 96:1:0.5:2.5. Coat the aluminum surface with a positive electrode active slurry made of lithium iron phosphate, conductive carbon, carbon nanotubes, and polyvinylidene fluoride in a mass ratio of 96:1.6:0.7:1.7. After drying, roll press to obtain bipolar electrodes. Stack the bipolar electrodes, a 20μm thick polypropylene separator, and the bipolar electrodes in that order. Place the stack in a hot press and hot press at 130℃ and 0.4MPa for 10 minutes. Then raise the temperature to 150℃ and the pressure to 0.6MPa and hot press for 5 minutes to obtain the sealing structure of the bipolar current collector cell.
[0026] Example 2: A method for preparing a sealing structure for a bipolar current collector cell, comprising the following steps: Step 1: A copper layer is deposited on an aluminum substrate to obtain a bipolar current collector. The current collector is then etched by a femtosecond laser at a scanning speed of 500 mm / s, a wavelength of 1030 nm, a pulse width of 300 fs, a frequency of 200 kHz, and a power of 10 W. This forms a serrated groove with a spacing of 100 μm, a depth of 12 μm, an opening width of 30 μm, a tooth tip angle of 40°, and a surface roughness of 2 μm at the edge regions of the upper and lower ends of the bipolar current collector. Step 2: Perform atmospheric pressure plasma treatment on the sawtooth grooves on the surface of the aluminum substrate. The gas is argon, the power is 150W, and the time is 3min. Immerse the sawtooth grooves on the surface of the copper layer in a 2% γ-mercaptopropyltrimethoxysilane solution for 30s. Dry at 80℃ for 5min to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: Mix 65g KH-792, 5g dibutyltin dilaurate, 20g propylene glycol methyl ether acetate, and 10g polyimide short fibers to obtain the oil phase core. Add 5g Span 80 and stir until homogeneous. Dropwise add 18g toluene diisocyanate, 12g hexamethylene diisocyanate, and 6g polycaprolactone diol and stir until homogeneous to obtain the total oil phase. Mix 10g diethylenetriamine and 300mL deionized water to obtain the aqueous phase. Slowly add the total oil phase to the aqueous phase at 4000r / min. After the addition is complete, maintain shear emulsification for 4min. Heat to 70℃ and react at a constant temperature of 350r / min for 3h to form polyurea-polyurethane wall material. Filter, wash, and dry to obtain microcapsules. Step 4: By mass percentage, 69.5% hydrogenated nitrile rubber is plasticized on a two-roll mill, and 6% fumed silica is added and mixed evenly to obtain a compound; 15% microcapsules with a particle size of 30μm are mixed evenly with the compound in a vacuum kneader at a temperature of 50℃, and 2% peroxide vulcanizing agent, 1% antioxidant, 1.5% dibutyl phthalate and 5% polytetrafluoroethylene micro powder are added and mixed evenly to obtain a sealant; Step 5: Apply sealant to the surface-treated serrated grooves of the bipolar current collector using a slit-type coating method. The sealant layer thickness is 180μm. Coat the copper surface with a negative electrode active slurry made of graphite, conductive carbon black, carbon nanotubes, and carboxymethyl cellulose in a mass ratio of 96:1:0.5:2.5. Coat the aluminum surface with a positive electrode active slurry made of lithium iron phosphate, conductive carbon, carbon nanotubes, and polyvinylidene fluoride in a mass ratio of 96:1.6:0.7:1.7. After drying, roll press to obtain bipolar electrodes. Stack the bipolar electrodes, a 20μm thick polypropylene separator, and the bipolar electrodes in that order. Place the stack in a hot press and hot press at 140℃ and 0.5MPa for 12 minutes. Then raise the temperature to 155℃ and the pressure to 0.7MPa and hot press for 7 minutes to obtain the sealing structure of the bipolar current collector cell.
[0027] Example 3: A method for preparing a sealing structure for a bipolar current collector cell, comprising the following steps: Step 1: A copper layer is deposited on an aluminum substrate to obtain a bipolar current collector. The current collector is then etched by a femtosecond laser at a scanning speed of 500 mm / s, a wavelength of 1030 nm, a pulse width of 300 fs, a frequency of 200 kHz, and a power of 12 W. This forms a serrated groove with a spacing of 100 μm, a depth of 15 μm, an opening width of 30 μm, a tooth tip angle of 45°, and a surface roughness of 3 μm at the edge regions of the upper and lower ends of the bipolar current collector. Step 2: The surface of the aluminum substrate with serrated grooves of the bipolar current collector is placed in an electrolyte with a concentration of 0.3 mol / L, which is obtained by mixing 2.7 g oxalic acid, 50 mL anhydrous ethanol and 50 mL deionized water. The electrolyte temperature is 20℃, the voltage is 160 V, and the mixture is magnetically stirred for 60 min to form porous alumina with a pore size of 50 nm and a depth of 500 nm on the inner wall of the grooves. Then, it is treated with atmospheric pressure plasma at 150 W for 3 min using argon gas. The copper layer surface is then coated with a 2% γ-mercaptopropyltrimethoxysilane solution for 30 s. The mixture is then dried at 80℃ for 5 min to obtain a surface-treated bipolar current collector with serrated grooves. Step 3: Mix 65g KH-792, 5g dibutyltin dilaurate, 20g propylene glycol methyl ether acetate, and 10g polyimide short fibers to obtain the oil phase core. Add 5g Span 80 and stir until homogeneous. Dropwise add 18g toluene diisocyanate, 12g hexamethylene diisocyanate, and 6g polycaprolactone diol and stir until homogeneous to obtain the total oil phase. Mix 10g diethylenetriamine and 300mL deionized water to obtain the aqueous phase. Slowly add the total oil phase to the aqueous phase at 4000r / min. After the addition is complete, maintain shear emulsification for 4min. Heat to 70℃ and react at a constant temperature of 350r / min for 3h to form polyurea-polyurethane wall material. Filter, wash, and dry to obtain microcapsules. Step 4: By mass percentage, 78% hydrogenated nitrile rubber is plasticized on a two-roll mill, and 6% fumed silica is added and mixed evenly to obtain a compound; 10% microcapsules with a particle size of 30μm are mixed evenly with the compound in a vacuum kneader at a temperature of 55℃, and 2% peroxide vulcanizing agent, 2% antioxidant and 2% dibutyl phthalate are added and mixed evenly to obtain a sealant; Step 5: Apply sealant to the surface-treated serrated grooves of the bipolar current collector using slit coating. The sealant layer thickness is 180μm. Coat the copper surface with a negative electrode active slurry made of graphite, conductive carbon black, carbon nanotubes, and carboxymethyl cellulose in a mass ratio of 96:1:0.5:2.5. Coat the aluminum surface with a positive electrode active slurry made of lithium iron phosphate, conductive carbon, carbon nanotubes, and polyvinylidene fluoride in a mass ratio of 96:1.6:0.7:1.7. After drying, roll press to obtain bipolar electrodes. Stack the bipolar electrodes, a 20μm thick polypropylene separator, and the bipolar electrodes in that order. Place the stack in a hot press and hot press at 130℃ and 0.4MPa for 10 minutes. Then raise the temperature to 150℃ and the pressure to 0.6MPa and hot press for 5 minutes to obtain the sealing structure of the bipolar current collector cell.
[0028] Example 4: Compared with Example 1, modified hydrogenated nitrile butadiene rubber was used instead of hydrogenated nitrile butadiene rubber, and modified fumed silica was used instead of fumed silica. Step 1: A copper layer is deposited on an aluminum substrate to obtain a bipolar current collector. The current collector is then etched by a femtosecond laser at a scanning speed of 500 mm / s, a wavelength of 1030 nm, a pulse width of 300 fs, a frequency of 200 kHz, and a power of 8 W. This forms a serrated groove with a spacing of 100 μm, a depth of 10 μm, an opening width of 30 μm, a tooth tip angle of 45°, and a surface roughness of 1 μm at the edge regions of the upper and lower ends of the bipolar current collector. Step 2: Perform atmospheric pressure plasma treatment on the sawtooth grooves on the surface of the aluminum substrate. The gas is argon, the power is 150W, and the time is 3min. Immerse the sawtooth grooves on the surface of the copper layer in a 2% γ-mercaptopropyltrimethoxysilane solution for 30s. Dry at 80℃ for 5min to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: Mix 65g KH-792, 5g dibutyltin dilaurate, 20g propylene glycol methyl ether acetate, and 10g polyimide short fibers to obtain the oil phase core. Add 5g Span 80 and stir until homogeneous. Dropwise add 18g toluene diisocyanate, 12g hexamethylene diisocyanate, and 6g polycaprolactone diol and stir until homogeneous to obtain the total oil phase. Mix 10g diethylenetriamine and 300mL deionized water to obtain the aqueous phase. Slowly add the total oil phase to the aqueous phase at 4000r / min. After the addition is complete, maintain shear emulsification for 4min. Heat to 70℃ and react at a constant temperature of 350r / min for 3h to form polyurea-polyurethane wall material. Filter, wash, and dry to obtain microcapsules. Step 4: Place 50g of hydrogenated nitrile rubber, 5g of glycidyl methacrylate and 0.75g of dicumyl peroxide in a Hacker torque rheometer and mix at 165℃ for 2min to obtain modified hydrogenated nitrile rubber. Step 5: In a 250 mL round-bottom flask, mix 30 mL of xylene with 0.2 g of pentamethylpiperidinol and stir until completely dissolved. While stirring continuously, slowly add 0.22 mL of propyltrimethoxysilane 3-isocyanate to the solution. Transfer the flask to an oil bath, connect a reflux condenser, and slowly heat to 35 °C. Maintain stirring at this temperature for 2.5 h to obtain a mixed solution. Disperse 0.1 g of fumed silica in 15 mL of xylene, sonicate for 13 min, and then quickly add it to the mixed solution. Heat to 115 °C and stir continuously for 11 h. After the reaction is complete, cool to 20 °C, centrifuge, wash three times with ethanol, dry in a 55 °C oven for 25 min, and then transfer to a vacuum drying oven to dry at 115 °C for 11 h to obtain modified fumed silica. Step 6: By mass percentage, 80.5% of modified hydrogenated nitrile rubber is plasticized on a two-roll mill, and 6% of modified fumed silica is added and mixed evenly to obtain a compound; 10% of microcapsules with a particle size of 30μm and the compound are mixed evenly in a vacuum kneader at a temperature of 45℃, and 2% peroxide vulcanizing agent, 0.5% antioxidant and 1% dibutyl phthalate are added and mixed evenly to obtain a sealant; Step 7: Apply sealant to the surface-treated serrated grooves of the bipolar current collector using slit coating. The sealant layer thickness is 180μm. Coat the copper surface with a negative electrode active slurry made of graphite, conductive carbon black, carbon nanotubes, and carboxymethyl cellulose in a mass ratio of 96:1:0.5:2.5. Coat the aluminum surface with a positive electrode active slurry made of lithium iron phosphate, conductive carbon, carbon nanotubes, and polyvinylidene fluoride in a mass ratio of 96:1.6:0.7:1.7. After drying, roll press to obtain bipolar electrodes. Stack the bipolar electrodes, a 20μm thick polypropylene separator, and the bipolar electrodes in that order. Place the stack in a hot press and hot press at 130℃ and 0.4MPa for 10 minutes. Then raise the temperature to 150℃ and the pressure to 0.6MPa and hot press for 5 minutes to obtain the sealing structure of the bipolar current collector cell.
[0029] Example 5: Compared with Example 1, modified hydrogenated nitrile butadiene rubber was used instead of hydrogenated nitrile butadiene rubber, and modified fumed silica was used instead of fumed silica. The parameters that were changed were the experimental parameters in the hydrogenated nitrile butadiene rubber and fumed silica modification steps: Step 1: A copper layer is deposited on an aluminum substrate to obtain a bipolar current collector. The current collector is then etched by a femtosecond laser at a scanning speed of 500 mm / s, a wavelength of 1030 nm, a pulse width of 300 fs, a frequency of 200 kHz, and a power of 8 W. This forms a serrated groove with a spacing of 100 μm, a depth of 10 μm, an opening width of 30 μm, a tooth tip angle of 45°, and a surface roughness of 1 μm at the edge regions of the upper and lower ends of the bipolar current collector. Step 2: Perform atmospheric pressure plasma treatment on the sawtooth grooves on the surface of the aluminum substrate. The gas is argon, the power is 150W, and the time is 3min. Immerse the sawtooth grooves on the surface of the copper layer in a 2% γ-mercaptopropyltrimethoxysilane solution for 30s. Dry at 80℃ for 5min to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: Mix 65g KH-792, 5g dibutyltin dilaurate, 20g propylene glycol methyl ether acetate, and 10g polyimide short fibers to obtain the oil phase core. Add 5g Span 80 and stir until homogeneous. Dropwise add 18g toluene diisocyanate, 12g hexamethylene diisocyanate, and 6g polycaprolactone diol and stir until homogeneous to obtain the total oil phase. Mix 10g diethylenetriamine and 300mL deionized water to obtain the aqueous phase. Slowly add the total oil phase to the aqueous phase at 4000r / min. After the addition is complete, maintain shear emulsification for 4min. Heat to 70℃ and react at a constant temperature of 350r / min for 3h to form polyurea-polyurethane wall material. Filter, wash, and dry to obtain microcapsules. Step 4: Place 100g of hydrogenated nitrile butadiene rubber, 10g of glycidyl methacrylate and 1.5g of dicumyl peroxide in a Hacker torque rheometer and mix at 175℃ for 6min to obtain modified hydrogenated nitrile butadiene rubber. Step 5: In a 250 mL round-bottom flask, mix 60 mL of xylene with 0.4 g of pentamethylpiperidinol and stir until completely dissolved. While stirring continuously, slowly add 0.44 mL of propyltrimethoxysilane 3-isocyanate to the solution. Transfer the flask to an oil bath, connect a reflux condenser, and slowly heat to 45 °C. Maintain stirring at this temperature for 3.5 h to obtain a mixed solution. Disperse 0.2 g of fumed silica in 30 mL of xylene, sonicate for 17 min, and then quickly add it to the mixed solution. Heat to 125 °C and stir continuously for 13 h. After the reaction is complete, cool to 25 °C, centrifuge, wash repeatedly with ethanol 5 times, dry in a 65 °C oven for 35 min, and then transfer to a vacuum drying oven to dry at 125 °C for 13 h to obtain modified fumed silica. Step 6: By mass percentage, 80.5% of modified hydrogenated nitrile rubber is plasticized on a two-roll mill, and 6% of modified fumed silica is added and mixed evenly to obtain a compound; 10% of microcapsules with a particle size of 30μm and the compound are mixed evenly in a vacuum kneader at a temperature of 45℃, and 2% peroxide vulcanizing agent, 0.5% antioxidant and 1% dibutyl phthalate are added and mixed evenly to obtain a sealant; Step 7: Apply sealant to the surface-treated serrated grooves of the bipolar current collector using slit coating. The sealant layer thickness is 180μm. Coat the copper surface with a negative electrode active slurry made of graphite, conductive carbon black, carbon nanotubes, and carboxymethyl cellulose in a mass ratio of 96:1:0.5:2.5. Coat the aluminum surface with a positive electrode active slurry made of lithium iron phosphate, conductive carbon, carbon nanotubes, and polyvinylidene fluoride in a mass ratio of 96:1.6:0.7:1.7. After drying, roll press to obtain bipolar electrodes. Stack the bipolar electrodes, a 20μm thick polypropylene separator, and the bipolar electrodes in that order. Place the stack in a hot press and hot press at 130℃ and 0.4MPa for 10 minutes. Then raise the temperature to 150℃ and the pressure to 0.6MPa and hot press for 5 minutes to obtain the sealing structure of the bipolar current collector cell.
[0030] Comparative Example 1: Compared with Example 5, hydrogenated nitrile butadiene rubber was used instead of modified hydrogenated nitrile butadiene rubber; Step 1: A copper layer is deposited on an aluminum substrate to obtain a bipolar current collector. The current collector is then etched by a femtosecond laser at a scanning speed of 500 mm / s, a wavelength of 1030 nm, a pulse width of 300 fs, a frequency of 200 kHz, and a power of 8 W. This forms a serrated groove with a spacing of 100 μm, a depth of 10 μm, an opening width of 30 μm, a tooth tip angle of 45°, and a surface roughness of 1 μm at the edge regions of the upper and lower ends of the bipolar current collector. Step 2: Perform atmospheric pressure plasma treatment on the sawtooth grooves on the surface of the aluminum substrate. The gas is argon, the power is 150W, and the time is 3min. Immerse the sawtooth grooves on the surface of the copper layer in a 2% γ-mercaptopropyltrimethoxysilane solution for 30s. Dry at 80℃ for 5min to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: Mix 65g KH-792, 5g dibutyltin dilaurate, 20g propylene glycol methyl ether acetate, and 10g polyimide short fibers to obtain the oil phase core. Add 5g Span 80 and stir until homogeneous. Dropwise add 18g toluene diisocyanate, 12g hexamethylene diisocyanate, and 6g polycaprolactone diol and stir until homogeneous to obtain the total oil phase. Mix 10g diethylenetriamine and 300mL deionized water to obtain the aqueous phase. Slowly add the total oil phase to the aqueous phase at 4000r / min. After the addition is complete, maintain shear emulsification for 4min. Heat to 70℃ and react at a constant temperature of 350r / min for 3h to form polyurea-polyurethane wall material. Filter, wash, and dry to obtain microcapsules. Step 4: In a 250 mL round-bottom flask, mix 60 mL of xylene with 0.4 g of pentamethylpiperidinol and stir until completely dissolved. While stirring continuously, slowly add 0.44 mL of propyltrimethoxysilane 3-isocyanate to the solution. Transfer the flask to an oil bath, connect a reflux condenser, and slowly heat to 45 °C. Maintain stirring at this temperature for 3.5 h to obtain a mixed solution. Disperse 0.2 g of fumed silica in 30 mL of xylene, sonicate for 17 min, and then quickly add it to the mixed solution. Heat to 125 °C and stir continuously for 13 h. After the reaction is complete, cool to 25 °C, centrifuge, wash repeatedly with ethanol 5 times, dry in a 65 °C oven for 35 min, and then transfer to a vacuum drying oven to dry at 125 °C for 13 h to obtain modified fumed silica. Step 5: By mass percentage, 80.5% hydrogenated nitrile rubber is plasticized on a two-roll mill, and 6% modified fumed silica is added and mixed evenly to obtain a compound; 10% microcapsules with a particle size of 30μm are mixed evenly with the compound in a vacuum kneader at a temperature of 45℃, and 2% peroxide vulcanizing agent, 0.5% antioxidant and 1% dibutyl phthalate are added and mixed evenly to obtain a sealant; Step 6: Apply sealant to the surface-treated serrated grooves of the bipolar current collector using slit coating. The sealant layer thickness is 180μm. Coat the copper surface with a negative electrode active slurry made of graphite, conductive carbon black, carbon nanotubes, and carboxymethyl cellulose in a mass ratio of 96:1:0.5:2.5. Coat the aluminum surface with a positive electrode active slurry made of lithium iron phosphate, conductive carbon, carbon nanotubes, and polyvinylidene fluoride in a mass ratio of 96:1.6:0.7:1.7. After drying, roll press to obtain bipolar electrodes. Stack the bipolar electrodes, a 20μm thick polypropylene separator, and the bipolar electrodes in that order. Place the stack in a hot press and hot press at 130℃ and 0.4MPa for 10 minutes. Then raise the temperature to 150℃ and the pressure to 0.6MPa and hot press for 5 minutes to obtain the sealing structure of the bipolar current collector cell.
[0031] Comparative Example 2: Compared with Example 5, fumed silica was used instead of modified fumed silica; Step 1: A copper layer is deposited on an aluminum substrate to obtain a bipolar current collector. The current collector is then etched by a femtosecond laser at a scanning speed of 500 mm / s, a wavelength of 1030 nm, a pulse width of 300 fs, a frequency of 200 kHz, and a power of 8 W. This forms a serrated groove with a spacing of 100 μm, a depth of 10 μm, an opening width of 30 μm, a tooth tip angle of 45°, and a surface roughness of 1 μm at the edge regions of the upper and lower ends of the bipolar current collector. Step 2: Perform atmospheric pressure plasma treatment on the sawtooth grooves on the surface of the aluminum substrate. The gas is argon, the power is 150W, and the time is 3min. Immerse the sawtooth grooves on the surface of the copper layer in a 2% γ-mercaptopropyltrimethoxysilane solution for 30s. Dry at 80℃ for 5min to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: Mix 65g KH-792, 5g dibutyltin dilaurate, 20g propylene glycol methyl ether acetate, and 10g polyimide short fibers to obtain the oil phase core. Add 5g Span 80 and stir until homogeneous. Dropwise add 18g toluene diisocyanate, 12g hexamethylene diisocyanate, and 6g polycaprolactone diol and stir until homogeneous to obtain the total oil phase. Mix 10g diethylenetriamine and 300mL deionized water to obtain the aqueous phase. Slowly add the total oil phase to the aqueous phase at 4000r / min. After the addition is complete, maintain shear emulsification for 4min. Heat to 70℃ and react at a constant temperature of 350r / min for 3h to form polyurea-polyurethane wall material. Filter, wash, and dry to obtain microcapsules. Step 4: Place 100g of hydrogenated nitrile butadiene rubber, 10g of glycidyl methacrylate and 1.5g of dicumyl peroxide in a Hacker torque rheometer and mix at 175℃ for 6min to obtain modified hydrogenated nitrile butadiene rubber. Step 5: By mass percentage, 80.5% of modified hydrogenated nitrile butadiene rubber is plasticized on a two-roll mill, and 6% fumed silica is added and mixed evenly to obtain a compound; 10% microcapsules with a particle size of 30μm are mixed evenly with the compound in a vacuum kneader at a temperature of 45℃, and 2% peroxide vulcanizing agent, 0.5% antioxidant and 1% dibutyl phthalate are added and mixed evenly to obtain a sealant; Step 6: Apply sealant to the surface-treated serrated grooves of the bipolar current collector using slit coating. The sealant layer thickness is 180μm. Coat the copper surface with a negative electrode active slurry made of graphite, conductive carbon black, carbon nanotubes, and carboxymethyl cellulose in a mass ratio of 96:1:0.5:2.5. Coat the aluminum surface with a positive electrode active slurry made of lithium iron phosphate, conductive carbon, carbon nanotubes, and polyvinylidene fluoride in a mass ratio of 96:1.6:0.7:1.7. After drying, roll press to obtain bipolar electrodes. Stack the bipolar electrodes, a 20μm thick polypropylene separator, and the bipolar electrodes in that order. Place the stack in a hot press and hot press at 130℃ and 0.4MPa for 10 minutes. Then raise the temperature to 150℃ and the pressure to 0.6MPa and hot press for 5 minutes to obtain the sealing structure of the bipolar current collector cell.
[0032] Experiment: The bipolar current collector sealing structures prepared in Examples 1-5 and Comparative Examples 1 and 2 were used to make samples and their performance was tested. Peel strength test: GB / T 2790-1995 was used as the reference standard. The sample size was 25 mm wide, 200 mm long, and 1.5 mm thick. The tensile speed of the testing machine was 100 mm / min. Electrolyte peel strength test: After immersing the sample in an electrolyte at 85℃ for 1000h, remove it, clean and dry it with anhydrous ethanol, and then test it according to the peel strength test method. The electrolyte is prepared by dissolving LiPF6 in a mixed solvent of ethylene carbonate and diethyl carbonate in a volume ratio of 1:1, with a concentration of 1M. Withstand pressure test: Using the packaged housing as a base, negative terminal plates are placed in sequence, and multiple bipolar cell units are stacked in sequence. Each unit consists of a bipolar current collector cell sealing structure. The units are separated by a diaphragm, and electrolyte is dripped on both sides of the diaphragm. Positive terminal plates are placed, and gaskets, springs, and the packaged housing are placed. After hot pressing and sealing, a bipolar current collector cell module is obtained. The bipolar current collector cell module is filled with helium to the test pressure. There is no leakage within 30 minutes. Bursting test: The prepared bipolar current collector cell sealing structure is placed in the test fixture and pressurized by filling with gas at 0.5MPa / min until the structure is destroyed. The location of the failure surface is observed. If the failure mode is cohesive failure of the adhesive layer rather than interfacial debonding, the test result is qualified, proving that the interfacial strength exceeds the strength of the adhesive itself. All test results are shown in Table 1.
[0033] Table 1
[0034] According to the data in Table 1, the peel strength of Examples 1-5 was 450-534 N / m, and after immersion in electrolyte at 85℃ for 1000 h, it still maintained 385-451 N / m. This proves that the ring-opening etherification reaction of the hydroxyl groups of the aluminum-side anodic oxide layer and the epoxy groups of the modified hydrogenated nitrile rubber, the Cu-S coordination bonding of the γ-mercaptopropyltrimethoxysilane on the copper side, and the hydrolysis condensation repair mechanism of the KH-792 silane coupling agent released by the microcapsules under the catalysis of dibutyltin dilaurate jointly constructed a covalent / coordination bond network resistant to electrolyte corrosion. The pressure resistance test showed that the porous alumina interface layer constructed by anodization in Example 3 and the toughening synergy of the polyimide short fibers in the microcapsules resulted in a pressure resistance value of 1.2 MPa. In Comparative Example 1, the hydrogenated nitrile rubber without epoxy modification resulted in a decrease in peel strength and electrolyte resistance compared to Example 5, confirming that the rubber grafting ring... The key contribution of oxygen groups to interfacial chemical bonding; in Comparative Example 2, unmodified fumed silica was used instead of the modified fumed silica covalently grafted with hindered amine light stabilizer. The peel strength and electrolyte peel strength were lower than those in Example 5, indicating that the surface-grafted hindered amine groups not only inhibited nanoparticle aggregation and improved dispersion reinforcement, but also significantly improved the sealant's anti-peeling ability in high-temperature electrolyte environments by capturing free radicals and forming a synergistic enhancement system with BLE / KY-405 antioxidant to enhance interfacial bonding strength and long-term durability. The burst failure mode in all examples was cohesive failure of the adhesive layer rather than interfacial debonding, confirming that the mechanical interlocking structure provided by the serrated grooves etched by femtosecond laser and the anti-aging effect of free radical capture by modified fumed silica synergistically enhanced the interfacial bonding work and fracture energy, ultimately achieving high-reliability sealing under ultra-thin adhesive layers.
[0035] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
Claims
1. A method for preparing a sealing structure for a bipolar current collector cell, characterized in that: Includes the following steps: Step 1: A copper layer is plated on an aluminum substrate to obtain a bipolar current collector. A serrated groove is formed at the edge regions of the upper and lower ends of the bipolar current collector by femtosecond laser etching. Step 2: Pre-treat the sawtooth grooves on the surface of the aluminum substrate, immerse the sawtooth grooves on the surface of the copper layer in γ-mercaptopropyltrimethoxysilane solution, and dry to obtain a bipolar current collector with sawtooth grooves after surface treatment. Step 3: After plasticizing, hydrogenated nitrile rubber is mixed with fumed silica to obtain a compound; the microcapsules and the compound are mixed evenly, and peroxide vulcanizing agent, antioxidant, plasticizer and polytetrafluoroethylene micro powder are added and mixed evenly to obtain a sealant. Step 4: Apply sealant to the surface-treated serrated grooves on the bipolar current collector, apply negative electrode active slurry to the copper side and positive electrode active slurry to the aluminum side, dry and roll to obtain bipolar electrode sheets, stack and hot press bipolar electrode sheets, polypropylene diaphragm and bipolar electrode sheets in sequence to obtain the sealing structure of the bipolar current collector battery cell.
2. The method for preparing a sealing structure for a bipolar current collector cell according to claim 1, characterized in that: In step 2, the pretreatment is either atmospheric pressure plasma treatment or anodic oxidation followed by atmospheric pressure plasma treatment.
3. The method for preparing a sealing structure for a bipolar current collector cell according to claim 2, characterized in that: The specific steps of the anodizing process are as follows: The surface of the aluminum substrate with serrated grooves in the bipolar current collector is placed in an electrolyte solution, which is a mixture of oxalic acid, anhydrous ethanol and deionized water. The electrolysis temperature is 19~21℃, the voltage is 155~165V, and the mixture is magnetically vibrated and stirred for 30~60 minutes to form porous alumina on the inner wall of the grooves.
4. The method for preparing a sealing structure for a bipolar current collector cell according to claim 1, characterized in that: The preparation steps of the microcapsules are as follows: KH-792, dibutyltin dilaurate, propylene glycol methyl ether acetate, and polyimide short fibers were mixed and stirred to obtain an oil phase core. Span 80 was added and stirred evenly. Toluene diisocyanate, hexamethylene diisocyanate, and polycaprolactone diol were added dropwise and stirred evenly to obtain a total oil phase. Diethylenetriamine and deionized water were mixed and stirred to obtain an aqueous phase. The total oil phase was added dropwise to the aqueous phase at a speed of 3500~4000 r / min. After the addition was complete, shear emulsification was maintained for 2~4 min. The temperature was raised to 65~70℃ and the reaction was carried out at a constant temperature of 300~350 r / min for 2~3 h to form a polyurea-polyurethane wall material. The material was filtered, washed, and dried to obtain microcapsules.
5. The method for preparing a sealing structure for a bipolar current collector cell according to claim 1, characterized in that: The parameters of the sawtooth groove are: spacing 80~120μm, depth 4~15μm, opening width 20~40μm, tooth tip angle 40~50°, and surface roughness 1~5μm.
6. The method for preparing a sealing structure for a bipolar current collector cell according to claim 1, characterized in that: The sealant comprises, by mass percentage, 5-10% fumed silica, 8-15% microcapsules, 1-2% peroxide vulcanizing agent, 0.5-2% antioxidant, 1-2% plasticizer, 0-5% polytetrafluoroethylene micro powder, and the balance being hydrogenated nitrile rubber.
7. The method for preparing a sealing structure for a bipolar current collector cell according to claim 1, characterized in that: The working conditions for femtosecond laser etching in step 1 are: scanning speed 490~510 mm / s, wavelength 1000~1030 nm, pulse width 280~320 fs, frequency 190~210 kHz, and power 8~12 W; When the pretreatment in step 2 is atmospheric pressure plasma treatment, the working conditions are: gas is one of argon, oxygen, or a mixture of argon and oxygen in a volume ratio of 9:1; power is 100~200 W; time is 2~5 min; γ- The mass concentration of the mercaptopropyltrimethoxysilane solution is 1-3%, the immersion time is 25-35s, the drying temperature is 75-85℃, and the drying time is 3-7min; the thickness of the coated adhesive layer in step 4 is 160-200μm, and the hot pressing conditions are: first stage temperature 120-140℃, pressure 0.3-0.5MPa, time 8-12min, second stage temperature 145-155℃, pressure 0.5-0.7MPa, time 3-7min.
8. The method for preparing a sealing structure for a bipolar current collector cell according to claim 1, characterized in that: The hydrogenated nitrile butadiene rubber is a modified hydrogenated nitrile butadiene rubber, and the preparation steps are as follows: Hydrogenated nitrile butadiene rubber, glycidyl methacrylate, and diisopropylbenzene peroxide were mixed at a mass ratio of 10:1:0.15 at 165~175℃ for 2~6 min to obtain modified hydrogenated nitrile butadiene rubber.
9. The method for preparing a sealing structure for a bipolar current collector cell according to claim 1, characterized in that: The fumed silica is modified fumed silica, and the preparation steps are as follows: Xylene and pentamethylpiperidinol were mixed and stirred. 3-propyltrimethoxysilane 3-isocyanate was added while stirring continuously. The mixture was heated to 35-45°C and stirred for 2.5-3.5 hours to obtain a mixed solution. Fumed silica was dispersed in xylene and sonicated for 13-17 minutes. It was then added to the mixed solution, heated to 115-125°C, and stirred continuously for 11-13 hours. The mixture was cooled to 20-25°C, centrifuged, washed repeatedly with ethanol 3-5 times, dried at 55-65°C for 25-35 minutes, and then heated to 115-125°C and dried for 11-13 hours to obtain modified fumed silica.
10. A sealing structure for a bipolar current collector cell prepared by the preparation method according to any one of claims 1-9.