Gallium nitride semiconductor laser and method for manufacturing the same
By employing mask layer patterning and two-stage MOCVD epitaxial growth to form a void structure in a gallium nitride semiconductor laser, the problems of optical field confinement and crystal quality were solved, achieving effective optical field confinement and improved crystal quality, thereby enhancing the performance and reliability of the laser.
Patent Information
- Application Number
- CN202611516334.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-20
AI Technical Summary
In gallium nitride semiconductor lasers, how can we effectively confine the optical field while ensuring crystal quality, avoid dislocations and cracks caused by lattice mismatch between high-Al content AlGaN and GaN, and solve the problem of optical field tunneling and leakage towards the substrate?
A central growth window and a patterned window are formed by patterning a mask layer. The lower light confinement layer fills the central growth window and forms voids on both sides to form a micro/nano refractive index structure. This reduces the lateral equivalent refractive index of the lower light confinement layer. The micro/nano structure formed by the voids laterally raises the light field confinement potential well, preventing the light field from tunneling and leaking into the substrate. The formation of voids is controlled by two-stage MOCVD epitaxial growth.
This technology effectively confines the optical field while ensuring crystal quality, reduces the optical confinement factor and threshold current, improves the far-field beam quality and reliability of the laser, is compatible with existing mass production processes, and enhances process consistency and controllability.
Smart Images

Figure CN123143809A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor technology, and in particular to a gallium nitride semiconductor laser and its fabrication method. Background Technology
[0002] With the continuous development of semiconductor technology, gallium nitride (GaN) semiconductor lasers have been widely used in laser processing, display lighting, information storage, and biochemistry. In GaN semiconductor laser design, optical field confinement capability is one of the key factors determining laser performance. Good optical field confinement can improve the optical confinement factor, reduce the lasing threshold current, and improve the far-field beam quality.
[0003] Gallium nitride semiconductor lasers typically use AlGaN material to fabricate the lower optical confinement layer. In order to improve the optical field confinement capability, the Al composition of the lower optical confinement layer is increased to increase the refractive index difference between AlGaN and GaN waveguide layers, thereby confining the optical field to the waveguide region near the active layer.
[0004] However, the high Al content of AlGaN results in a large lattice mismatch between AlGaN and GaN, making it highly susceptible to dislocations and cracks during epitaxy. This leads to a significant deterioration in crystal quality, increased leakage current, and a marked decrease in device reliability. While using a GaN homogeneous substrate to circumvent the lattice mismatch problem between AlGaN and GaN can significantly reduce dislocation density and improve thermal conductivity and reliability, the small refractive index difference between the GaN homogeneous substrate and the upper epitaxial layer means that the optical field cannot be effectively confined. This results in easy tunneling leakage towards the substrate, leading to a decrease in the optical confinement factor and an increase in the optical threshold.
[0005] Therefore, how to effectively constrain the light field while ensuring crystal quality has become an urgent technical problem to be solved. Summary of the Invention
[0006] The purpose of this invention is to overcome at least the above-mentioned technical problem of not being able to ensure crystal quality while effectively constraining the optical field, and to provide a gallium nitride semiconductor laser and its fabrication method.
[0007] The first aspect of the technical solution of the present invention is: A gallium nitride semiconductor laser includes a gallium nitride substrate, a mask layer, a lower light confinement layer, a lower waveguide layer, an active layer, and a p-type structure layer stacked sequentially from bottom to top. The mask layer has a central growth window extending along the resonant cavity direction and a plurality of patterned windows located on both sides of the central growth window. The central growth window and the plurality of patterned windows divide the mask layer into a plurality of patterned mask retention portions located on both sides of the central growth window. The lower light confinement layer fills the central growth window and the plurality of patterned windows, and extends above the plurality of patterned mask retention portions. A void is formed between the side of the plurality of patterned mask retention portions facing away from the gallium nitride substrate and the upper lower light confinement layer. The p-type structure layer has a ridge structure extending along the direction of the resonant cavity on the side away from the gallium nitride substrate, and the orthogonal projection of the ridge structure on the surface of the gallium nitride substrate is located within the central growth window. The voids are located on both sides of the central growth window perpendicular to the direction of the resonant cavity, and the voids on each side are arranged in at least two columns, with each column of voids arranged along the direction of the resonant cavity.
[0008] Optionally, each column of the voids is a continuous strip-shaped void extending along the direction of the resonant cavity; or, each column of the voids includes a plurality of discrete voids spaced apart along the direction of the resonant cavity.
[0009] Optionally, the lasing wavelength of the gallium nitride semiconductor laser is λ, and the width of the plurality of patterned mask retention portions in the direction perpendicular to the resonant cavity is 1 / 10 to 1 / 8 of the lasing wavelength of the gallium nitride semiconductor laser.
[0010] Furthermore, the width of the plurality of patterned mask retention portions in the direction perpendicular to the resonant cavity is 1 / 9 of the lasing wavelength of the gallium nitride semiconductor laser.
[0011] Optionally, the distance between the side of the orthographic projection and the side of the central growth window in the direction perpendicular to the resonant cavity is greater than zero.
[0012] The second aspect of the technical solution of the present invention is: A method for fabricating a gallium nitride semiconductor laser includes the following steps: S1. Provide a gallium nitride substrate and form a common mask layer on the surface of the gallium nitride substrate; S2. Pattern the common mask layer to form multiple mask units. Each mask unit includes a mask layer, a central growth window extending along the resonant cavity direction, and multiple patterned windows. The multiple patterned windows of each mask unit are located on both sides of the central growth window. The central growth window and the multiple patterned windows divide the mask layer of each mask unit into multiple patterned mask retention portions located on both sides of the central growth window. S3. Vertical growth of the lower light confinement layer is performed in the central growth window and the plurality of patterned windows of each mask unit, and a cavity is reserved above the plurality of patterned mask retention portions; lateral growth of the lower light confinement layer is performed, so that the crystals grown from the central growth window and the plurality of patterned windows grow laterally toward the plurality of patterned mask retention portions and close together, forming a cavity located between the plurality of patterned mask retention portions and the lower light confinement layer; S4. A lower waveguide layer, an active layer, and a p-type structure layer are epitaxially grown sequentially on the lower optical confinement layer. S5. Etch the p-type structure layer to form a plurality of ridge structures corresponding to the plurality of mask units, wherein the orthographic projection of each ridge structure on the surface of the gallium nitride substrate is located within the central growth window of the corresponding mask unit; S6. P electrodes and N electrodes are formed on the top surface of the ridge structure and the bottom surface of the gallium nitride substrate, respectively, and multiple gallium nitride semiconductor lasers are obtained by cleaving.
[0013] Optionally, in step S2, the plurality of patterned mask retention portions located on each side of the central growth window include at least two continuous strip mask strips extending along the resonant cavity direction and divided by the patterned window; or, the plurality of patterned mask retention portions located on each side of the central growth window include at least two rows of island-shaped mask blocks arranged along the resonant cavity direction and divided by the patterned window.
[0014] Optionally, the width of the continuous strip mask or the island mask block in the direction perpendicular to the ridge structure is 1 / 10 to 1 / 8 of the lasing wavelength of the gallium nitride semiconductor laser.
[0015] Furthermore, the width of the continuous strip mask or the island mask block in the direction perpendicular to the ridge structure is 1 / 9 of the lasing wavelength of the gallium nitride semiconductor laser.
[0016] Optionally, during the longitudinal growth of the lower light confinement layer in step S3, the ratio of the longitudinal growth rate to the lateral growth rate of the lower light confinement layer is greater than or equal to 3:1, and during the lateral growth of the lower light confinement layer in step S3, the ratio of the lateral growth rate to the longitudinal growth rate of the lower light confinement layer is greater than or equal to 2:1.
[0017] The gallium nitride semiconductor laser and its fabrication method provided by this invention utilize a lower light confinement layer to fill the central growth window region corresponding to the orthographic projection of the ridge structure, and form a continuously filled, void-free lower light confinement layer in this region, constituting a complete core waveguide optical path to ensure stable transmission of the fundamental mode. Simultaneously, micro-nano refractive index structures composed of voids are formed on both sides of the central growth window perpendicular to the resonant cavity direction, reducing the lateral equivalent refractive index of the lower light confinement layer. This laterally raises the optical field confinement potential well, confining the optical field to the central waveguide region, while mechanistically cutting off the tunneling leakage of the optical field to the GaN substrate, solving the problem of optical leakage in homogeneous substrates. Moreover, the reduction of the refractive index of the lower light confinement layer does not require the use of AlGaN with a high Al content, thus ensuring crystal quality while achieving effective optical field confinement. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 This is a schematic diagram of the structure of a gallium nitride semiconductor laser provided in an embodiment of the present invention; Figure 2 This is a flowchart of the method for fabricating a gallium nitride semiconductor laser provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of a gallium nitride substrate with a shared mask layer provided in an embodiment of the present invention; Figure 4 Yes Figure 3 A schematic diagram of the structure after the shared mask layer of the structure shown has been patterned. Figure 5 Is Figure 4 A schematic diagram of the structure after longitudinal and lateral growth of the lower light confinement layer is shown. Figure 6 Is Figure 5 A schematic diagram of the structure after growing the lower waveguide layer, active layer, and p-type structure layer on the structure shown; Figure 7 Is Figure 6 A schematic diagram of the ridge structure etched on the structure shown. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0021] It should be noted that the terms "setup" and "connection" should be interpreted broadly. For example, they can refer to direct setup or connection, or indirect setup or connection through centered components or centered structures.
[0022] Furthermore, in embodiments of this invention, terms such as "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer" are used to indicate orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, or in a conventional placement or usage state. These terms are merely for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the structures, features, devices, or elements referred to must have a specific orientation or positional relationship, nor that they must be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.
[0023] The various specific technical features and embodiments described in the detailed embodiments can be combined in any suitable manner without contradiction. For example, different implementation methods can be formed by combining different specific technical features / embodiments. In order to avoid unnecessary repetition, the various possible combinations of the various specific technical features / embodiments in this invention will not be described separately.
[0024] like Figure 1 As shown, an embodiment of the present invention provides a gallium nitride semiconductor laser 10, which includes a gallium nitride substrate 11, a mask layer 12, a lower light confinement layer 13, a lower waveguide layer 14, an active layer 15, and a p-type structure layer 16 stacked sequentially from bottom to top.
[0025] The gallium nitride substrate 11 is used to provide support and a conductive substrate for the device. In one embodiment, the gallium nitride substrate is an n-type conductive gallium nitride (GaN) homogeneous substrate, which has low dislocation density, high thermal conductivity and high electrical conductivity, and can provide excellent substrate conditions for the device.
[0026] Mask layer 12 is deposited on the surface of gallium nitride substrate 11 and patterned. See also Figure 1 The mask layer 12 has a shape formed along the resonant cavity direction (perpendicular to) Figure 1The mask layer 12 extends from a central growth window 121 (in the direction shown in the image) and includes multiple patterned windows 122 on either side of the central growth window 121. The central growth window 121 and the multiple patterned windows 122 divide the mask layer 12 into multiple patterned mask retention portions 123 located on either side of the central growth window 121. The central growth window 121 corresponds to the light-emitting region directly below the subsequent laser ridge structure, and the exposed substrate within it is available for crystal nucleation and growth. The patterned mask retention portions 123 provide a structural basis for the formation of air voids (hereinafter referred to as voids 124). In some feasible embodiments, the material of the mask layer 12 may be SiN or SiO2.
[0027] The lower light confinement layer 13 is selectively epitaxially grown above the mask layer 12 by metal-organic chemical vapor deposition (MOCVD). The lower light confinement layer 13 is made of GaN and fills the central growth window 121 and multiple patterned windows 122, extending above multiple patterned mask retention portions 123. Since the patterned mask retention portions 123 are mask materials and do not provide crystal nucleation, voids 124 are formed between the side of the multiple patterned mask retention portions 123 facing away from the gallium nitride substrate 11 and the upper lower light confinement layer 13. The voids 124 are located on both sides of the central growth window 121 perpendicular to the resonant cavity direction, and the voids 124 on each side are arranged in at least two rows, with each row of voids 124 arranged along the resonant cavity direction.
[0028] It should be noted that the void 124 can be formed by two-stage selective epitaxy: the first stage mainly grows vertically within the central growth window 121 and multiple patterned windows 122, causing the crystal to rise vertically within the windows and leaving a cavity above the multiple patterned mask retention portions 123; the second stage mainly grows laterally, causing the crystal grown within the windows to spread laterally from the top towards the multiple patterned mask retention portions 123, bridge, and close to seal the cavity. Therefore, the bottom wall of the void 124 is a flat surface of the multiple patterned mask retention portions 123 facing away from the gallium nitride substrate 11, the top wall is a curved surface formed by the lateral closure of the epitaxial layer and tilted or bent towards the center, and the two side walls are upright crystal surfaces formed by the vertical growth of the first stage (since the vertical growth process also has a lateral growth component, the upright crystal surfaces here will be slightly tilted). The cross-section of the void 124 in the direction perpendicular to the resonant cavity is roughly triangular, trapezoidal, or arched (dome) in shape, and the specific shape depends on the growth rate ratio of the two stages and the closure position.
[0029] In this embodiment, the cross-section of the cavity 124 in the direction perpendicular to the resonant cavity is triangular, the planar dimensions of the cavity 124 are consistent with the corresponding patterned mask retention portion 123, the width W of the cavity 124 in the direction perpendicular to the resonant cavity is 1 / 9 of the lasing wavelength of the gallium nitride semiconductor laser, and the cross-sectional height of the cavity 124 in the direction perpendicular to the resonant cavity is equal to the thickness of the mask layer 12.
[0030] It is understood that by setting the voids 124 on both sides of the central growth window 121 perpendicular to the direction of the resonant cavity, and arranging at least two columns on each side along the direction of the resonant cavity, periodic air (n≈1, n is the refractive index) refractive index micro-nano structures can be formed on both sides of the core waveguide optical path below the ridge structure, thereby reducing the lateral equivalent refractive index of the lower light confinement layer 13, and forming a high-contrast equivalent refractive index waveguide with the central high refractive index dense GaN.
[0031] It should be noted that the central growth window 121 is on each side ( Figure 1 The voids 124 (left and right of the central growth window 121 shown in the figure) are not limited to two columns, but can also be three, four, five or more columns. Specifically, periodic patterned windows 122 can be set on the mask layer 12 to divide the mask layer 12 into periodically arranged patterned mask retention parts 123, thereby facilitating the subsequent formation of multiple columns of periodically arranged voids 124.
[0032] In one embodiment, each row of voids 124 is a continuous strip-shaped void extending along the direction of the resonant cavity. In another embodiment, each row of voids 124 includes a plurality of discrete voids spaced apart along the direction of the resonant cavity. It is understood that both continuous strip-shaped voids and discrete voids can form low-refractive-index micro / nano structures in the direction perpendicular to the resonant cavity, and those skilled in the art can choose according to the mode field size, process conditions, and output power requirements.
[0033] In one embodiment, the gallium nitride semiconductor laser 10 has a lasing wavelength of λ, and multiple patterned mask retention portions 123 are located in a direction perpendicular to the resonant cavity ( Figure 1 The width W in the horizontal direction (indicated by the X-axis) is 1 / 10 to 1 / 8 of the lasing wavelength. The lateral penetration depth of the evanescent wave of the mode field of the gallium nitride laser 10 falls exactly in the range of λ / 8 to λ / 10. The hole 124 formed on the patterned mask retention portion 123 of this size can match the lateral attenuation penetration depth of the evanescent wave of the mode field of the gallium nitride laser 10, covering the evanescent wave region where the optical field leaks energy, producing a refractive index step attenuation effect on the diffused evanescent wave, and suppressing the lateral dispersion of the optical field and the tunneling leakage on the substrate side. Correspondingly, the width W of the hole 124 in the direction perpendicular to the resonant cavity can also be set to 1 / 10 to 1 / 8 of the lasing wavelength of the gallium nitride semiconductor laser.
[0034] Furthermore, the width W of the multiple patterned mask retention portions 123 in the direction perpendicular to the resonant cavity is 1 / 9 of the lasing wavelength. The voids 124 above the patterned mask retention portions 123 of this characteristic size can cover the evanescent wave region where the light field leakage energy is strongest, generating the strongest refractive index step attenuation effect on the diffuse evanescent wave, constructing a steep transverse refractive index barrier, adapting to the laser mode field matching requirements of different lasing wavelengths, and achieving the effect of "suppressing leakage light without damaging the main mode field".
[0035] Of course, those skilled in the art will understand that the structural configuration of the mask layer 12 and the lower light confinement layer 13 is not limited to the above embodiments. For example, the material of the mask layer 12 can be replaced with various high-temperature stable dielectric materials for MOCVD, and the thickness of the mask layer can be flexibly adjusted within the range of 100-500 nm to correspondingly change the height of the void 124 and achieve control of the equivalent refractive index. For example, the thickness of the mask layer 12 can be 100 nm, 250 nm, 300 nm, 400 nm, 450 nm, or 500 nm, etc. In addition, the width of the central growth window 121 and the patterned window 122 on the mask layer 12, as well as the width of the patterned mask retention portion 123 in the direction perpendicular to the resonant cavity, can be adapted and adjusted according to the laser ridge width, mode field size, and output power requirements. In addition, in some other embodiments, the lower light confinement layer 13 may be doped with trace amounts of Al to form low-content AlGaN, so as to slightly adjust the basic refractive index and further optimize the light field confinement effect without using high-Al content materials. This avoids the lattice mismatch problem between high-Al content AlGaN and GaN from the root, thereby significantly improving crystal quality and long-term device reliability.
[0036] The lower waveguide layer 14 is grown above the lower light confinement layer 13. In one embodiment, the material of the lower waveguide layer 14 is n-type GaN or InGaN. The active layer 15 is an InGaN / GaN multi-quantum-well structure, which can be adapted to different lasing bands such as blue light, violet light, and green light. A ridge structure 160 extending along the resonant cavity direction is formed on the side of the p-type structure layer 16 away from the gallium nitride substrate 11. The orthographic projection of the ridge structure 160 on the surface of the gallium nitride substrate 11 is located within the central growth window 121.
[0037] Specifically, in some embodiments, the p-type structure layer 16 includes an upper waveguide, an AlGaN electron blocking layer, and a p-type GaN contact layer, which can subsequently be etched to form a conventional ridge-shaped mesa structure 160. In one embodiment, the distance D between the side of the orthographic projection of the ridge structure 160 onto the surface of the gallium nitride substrate 11 and the side of the central growth window 121 in the direction perpendicular to the resonant cavity is greater than zero. This distance range allows the lateral dimension (perpendicular to the resonant cavity direction, i.e., the X-axis direction) of the central growth window 121 to be slightly larger than the lateral dimension of the ridge structure 160, further reducing dislocations in the active layer 15 below the ridge structure 160.
[0038] The gallium nitride semiconductor laser 10 provided by the present invention utilizes a lower light confinement layer 13 to fill the central growth window 121 corresponding to the orthographic projection of the ridge structure 160, and forms a continuously filled lower light confinement layer 13 without voids in this region, constituting a complete core waveguide optical path to ensure stable transmission of the fundamental mode. At the same time, micro-nano refractive index structures composed of voids 124 are formed on both sides of the central growth window 121 perpendicular to the direction of the resonant cavity, reducing the lateral equivalent refractive index of the lower light confinement layer 13, laterally raising the optical field confinement potential well, confining the optical field to the central waveguide region, and mechanistically cutting off the tunneling leakage of the optical field to the GaN substrate 11, solving the problem of optical leakage in homogeneous substrates. Moreover, the reduction of the refractive index of the lower light confinement layer 13 does not need to be achieved by using AlGaN with a high Al composition, thus ensuring crystal quality while achieving effective optical field confinement.
[0039] Additionally, the void 124 is directly epitaxially formed during the MOCVD process, without the need for additional processes such as sacrificial layers and electrochemical etching. It can be achieved through only one patterning photolithography and conventional epitaxy, making it compatible with existing gallium nitride laser mass production lines with strong process consistency and controllability. At the same time, the lower light confinement layer 13 in the central growth window 121 region can also retain the vertical conductive and thermally conductive channels of the central dense GaN, which greatly improves the laser's light confinement capability and overall performance while ensuring the electrical and thermal performance of the device and crystal quality.
[0040] See Figure 2 The present invention also provides a method for fabricating a gallium nitride semiconductor laser, comprising the following steps S1-S6.
[0041] S1. Provide a gallium nitride substrate 11 and form a common mask layer 20 on the surface of the gallium nitride substrate 11.
[0042] See Figure 3 Specifically, in this embodiment, an n-type conductive GaN homogeneous substrate can be selected. In this step, the n-type conductive GaN homogeneous substrate is first subjected to standard cleaning treatment to remove surface impurities and oxide layers to ensure the cleanliness of the substrate surface; then, a SiN or SiO2 dielectric layer is deposited on the substrate surface as a common mask layer 20.
[0043] S2. Patterned shared mask layer 20 forms multiple mask units.
[0044] Please see also Figure 4Specifically, each mask unit includes a mask layer 12, a central growth window 121 penetrating the mask layer 12, and multiple patterned windows 122. The central growth window 121 of each mask unit extends along a pre-defined resonant cavity direction. The multiple patterned windows 122 of each mask unit are located on both sides of the central growth window 121. The central growth window 121 and the multiple patterned windows 122 divide the mask layer 12 of each mask unit into multiple patterned mask retention portions 123 located on both sides of the central growth window 121. In step S2, the patterned mask can be fabricated through photolithography and etching processes to form the central growth window 121, the patterned windows 122, and the patterned mask retention portions 123 located on both sides of the central growth window 121.
[0045] In one embodiment, in each mask unit formed in step S2, a plurality of patterned mask retention portions 123 located on each side of the central growth window 121 include at least two continuous strip mask strips 1230 extending along the resonant cavity direction and divided by the patterned window 122. Furthermore, in another feasible embodiment, the plurality of patterned mask retention portions 123 located on each side of the central growth window 121 include at least two rows of island-shaped mask blocks 1230' arranged along the resonant cavity direction and divided by the patterned window.
[0046] Optionally, in some embodiments, the width of the continuous strip mask 1230 or island mask block 1230' in the direction perpendicular to the resonant cavity is 1 / 10 to 1 / 8 of the lasing wavelength of the gallium nitride semiconductor laser 10. Further, in some embodiments, preferably, the width of the continuous strip mask 1230 or island mask block 1230' in the direction perpendicular to the resonant cavity is 1 / 9 of the lasing wavelength of the gallium nitride semiconductor laser 10.
[0047] S3. Vertical and horizontal growth of the lower light confinement layer 13 is performed in the central growth window 121 and multiple patterned windows 122 of each mask unit.
[0048] Specifically, firstly, the lower light confinement layer 13 is grown vertically within the central growth window 121 and multiple patterned windows 122 of each mask unit, reserving cavities 124' above the multiple patterned mask retention portions 123; then, the lower light confinement layer 13 is grown laterally, causing the crystals grown from the central growth window 121 and multiple patterned windows 122 to grow laterally upwards towards the multiple patterned mask retention portions 123 and converge, forming a cavity 124 located between the multiple patterned mask retention portions 123 and the lower light confinement layer 13, such as... Figure 5 As shown.
[0049] This step employs a two-stage variable-parameter MOCVD epitaxial growth of the lower light-confining layer 13, enabling controllable formation of the voids 124. Simply put, the lower light-confining layer undergoes longitudinal growth under a first growth condition (first growth stage), and lateral growth under a second growth condition (second growth stage). The reaction pressure under the first growth condition is greater than that under the second growth condition, the growth temperature under the first growth condition is lower than that under the second growth condition, and the molar ratio of ammonia to trimethylgallium in the first growth condition is lower than that in the second growth condition.
[0050] Taking GaN growth as the lower light confinement layer 13 as an example: The first stage is the vertical growth stage: After GaN nucleation and emergence within the central growth window 121 and patterned window 122, growth is carried out under high pressure, low temperature, and low ammonia flow rate conditions. Under these conditions, the surface mobility of Ga atoms is significantly reduced, greatly suppressing the lateral spread of GaN crystals. This results in a much higher vertical growth rate than the lateral growth rate, enabling the GaN crystal at the window position to grow vertically and rapidly without prematurely spreading above the patterned mask retention area 123, thus reserving a complete and regular cavity space for the subsequent formation of the void 124. The process parameters for this stage can be executed under the following conditions: growth temperature 900–980℃, reaction pressure 300–600 mbar, V / III molar ratio (NH3 / TMGa, the molar ratio of ammonia to trimethylgallium) 500–1500, growth time 5–15 min, vertical growth thickness 300–800 nm, and the ratio of vertical growth rate to lateral growth rate greater than or equal to 3:1. Among them, high pressure suppresses the lateral diffusion of gaseous precursors, low temperature limits the migration distance of Ga atoms on the surface, and low V / III molar ratio reduces the density of nitrogen active sites. The three factors work together to ensure that GaN crystals are mainly grown in a vertical columnar manner, and the area above the patterned mask retention part 123 is not covered by GaN crystals in advance.
[0051] The second stage is the rapid lateral closure and sealing stage: After the GaN crystal is grown longitudinally to the set thickness, the process conditions are switched to low pressure, high temperature, and high ammonia flow rate. Under this condition, the surface migration and lateral diffusion capabilities of Ga atoms are significantly enhanced, causing the lateral growth rate of the GaN crystal to surpass the longitudinal growth rate. The GaN crystal rapidly spreads, bridges, and closes from the central growth window 121 and patterned window 122 to the top of the patterned mask retention parts 123 on both sides, and finally completely seals above the patterned mask retention parts 123. The patterned mask retention parts 123 form a structurally stable and uniformly sized sealed cavity 124 between the GaN crystal (i.e., the lower light confinement layer 13). The process parameters for this stage can be executed under the following conditions: growth temperature 1000–1080℃, reaction pressure 50–150 mbar, molar ratio of ammonia to trimethylgallium 3000–5000, growth time 3–10 min, until the epitaxial layer of the GaN crystal above the patterned mask retention part 123 is completely bridged and joined, and the ratio of lateral growth rate to longitudinal growth rate is greater than or equal to 2:1. Among these, high temperature significantly enhances the surface migration and lateral diffusion ability of Ga atoms, low pressure reduces gas phase collisions, making it easier for the precursor to reach the top surface of the patterned mask retention part 123, and high V / III ratio provides sufficient nitrogen active sites to promote rapid lateral crystal plane growth. These three factors work together to achieve rapid lateral cavity sealing, sealing the air in situ above the patterned mask retention part 123 to form a stable and sealed cavity 124.
[0052] It should be noted that the above-mentioned two-stage parameter switching growth logic is different from the traditional heteroepitaxial lateral overgrowth (ELOG): the traditional heteroepitaxial ELOG strengthens lateral growth throughout the process and deliberately eliminates unwanted air voids, only improving crystal quality, without any optical waveguide design and without optical field confinement function; while the embodiment of the present invention controls the process in stages, first strengthening the longitudinal growth with high pressure, low temperature and low ammonia to reserve the cavity, and then accelerating the lateral closing and sealing of the cavity with low pressure, high temperature and high ammonia, actively, controllably and repeatedly creating functional voids 124, so that the size and morphology of voids 124 are highly controllable.
[0053] S4. A lower waveguide layer 14, an active layer 15, and a p-type structure layer 16 are epitaxially grown sequentially on the lower light confinement layer 13.
[0054] See Figure 6 Specifically, an n-type GaN or InGaN lower waveguide layer, an InGaN / GaN multi-quantum-well active layer, and a p-type structure layer 16 containing an upper waveguide, an AlGaN electron blocking layer, and a p-type GaN contact layer can be grown sequentially to complete the fabrication of a complete epitaxial wafer.
[0055] S5. Etch the p-type structure layer 16 to form multiple ridge structures 160 corresponding to multiple mask units.
[0056] Please see also Figure 7 In this step, the ridge structure 160 is formed on the p-type structure layer 16 by photolithography and etching processes, and the ridge structure 160 is aligned with the central growth window 121. Specifically, each ridge structure 160 extends along the resonant cavity direction, and its orthographic projection on the surface of the gallium nitride substrate 11 is located within the central growth window 121 of the corresponding mask unit.
[0057] S6. P-electrodes and N-electrodes are formed on the top surface of the ridge structure 160 and the bottom surface of the gallium nitride substrate 11, respectively, and multiple gallium nitride semiconductor lasers 10 are obtained by cleaving.
[0058] Specifically, electrodes can be deposited on the top surface of the ridge structure 160 and the bottom surface of the gallium nitride substrate 11 using a deposition process. It should be noted that a substrate thinning process can be performed before electrode deposition, and cavity cleaving coating and die cleaving (along the...) can be performed after electrode deposition. Figure 7 The process involves subsequent steps such as cleaving the die at the location indicated by the dashed line, ultimately resulting in multiple gallium nitride semiconductor lasers 10 (gallium nitride semiconductor laser dies).
[0059] The method for fabricating the gallium nitride semiconductor laser provided by this invention produces a gallium nitride semiconductor laser structure by filling the central growth window 121 corresponding to the orthographic projection of the ridge structure 160 with a lower light confinement layer 13, forming a continuously filled, void-free lower light confinement layer 13 in this region, constituting a complete core waveguide optical path to ensure stable transmission of the fundamental mode. Simultaneously, micro-nano refractive index structures composed of voids 124 are formed on both sides of the central growth window 121 perpendicular to the resonant cavity direction, reducing the lateral equivalent refractive index of the lower light confinement layer 13 and forming a high-contrast equivalent refractive index waveguide. This laterally raises the optical field confinement potential well, confining the optical field to the central waveguide region, while mechanistically cutting off the tunneling leakage of the optical field to the GaN substrate 11, solving the problem of light leakage from the homogeneous substrate. Furthermore, the reduction in the refractive index of the lower light confinement layer 13 does not require the use of AlGaN with a high Al content, thus ensuring crystal quality while achieving effective optical field confinement.
[0060] Additionally, the void 124 is directly epitaxially formed during the MOCVD process, without the need for additional processes such as sacrificial layers and electrochemical etching. It can be achieved through only one patterning photolithography and conventional epitaxy, which is compatible with existing gallium nitride laser mass production lines and has strong process consistency and controllability. At the same time, the lower light confinement layer 13 in the central growth window 121 region can also retain the vertical conductive and thermal conduction channels of the central dense GaN, which greatly improves the laser's light confinement capability and overall performance while ensuring the electrical and thermal performance of the device and crystal quality.
[0061] It should be noted that different process parameters can be used in the above preparation method to prepare epitaxial structures with different lasing wavelengths to suit different application requirements. For example: 450nm blue gallium nitride edge-emitting laser.
[0062] Using an n-type GaN homogeneous substrate, a 220nm thick SiN layer is deposited on the surface as a mask layer. After photolithography patterning, a central growth window with a width of 5μm is formed. The patterned mask retention areas on both sides of the central growth window are strip-shaped mask strips. The width of the strip-shaped mask strips is designed based on a 450nm wavelength, and the theoretically optimal subwavelength width is 50nm (450nm / 9). The strip-shaped mask strip width is designed to be 50nm, which can match the evanescent wave penetration depth of the blue laser and achieve better refractive index modulation. In order to adapt to mass production photolithography process, the size can be appropriately widened while retaining the optical mechanism. The central growth window corresponds to the area directly below the ridge of the subsequent laser.
[0063] The light confinement layer is grown using a two-stage variable-parameter MOCVD epitaxial growth method: The first stage is vertical growth, with a growth temperature of 940℃, a reaction pressure of 450mbar, a V / III molar ratio of 1000, and a growth time of 8min. The GaN crystal grows to a thickness of about 500nm in the vertical direction, and the vertical / horizontal growth rate ratio is about 4:1. The crystal in the central growth window and the patterned window is vertically raised, and a complete cavity is reserved above the patterned mask retention area. The second stage involves lateral closure and sealing of the cavity. The growth temperature is set to 1040℃, the reaction pressure to 100mbar, the V / III molar ratio to 4000, the growth time to 5min, and the lateral / vertical growth rate ratio to approximately 3:1. The GaN crystal rapidly spreads and bridges above the patterned mask retention areas on both sides, forming a closed air cavity with a height of 220nm. A dense GaN conductive layer is formed in the central growth window region.
[0064] A 120 nm thick n-GaN lower waveguide layer, a 450 nm InGaN / GaN multi-quantum-well active layer, a P-type GaN upper waveguide, an AlGaN electron blocking layer, and a P-type GaN contact layer are sequentially epitaxially grown. Subsequent etching forms a 4 μm wide ridge-shaped mesa, and P and N electrodes are fabricated. Cavity surface coating and die cleaving are then completed to finally obtain a blue laser.
[0065] 405nm violet gallium nitride edge-emitting laser Using an n-type GaN homogeneous substrate, a 180nm thick SiO2 layer is deposited on the surface as a mask layer. After photolithography patterning, a central growth window with a width of 4μm is formed. The patterned mask retention areas on both sides of the central growth window are strip-shaped mask strips. The width of the strip-shaped mask strips is designed based on a wavelength of 405nm. The theoretically optimal subwavelength width is 45nm (405nm / 9). This size can match the evanescent wave leakage characteristic scale of short-wavelength lasers, solving the industry problem of more serious light field leakage in the violet band. The engineering value can be adapted to fine-tuning of process precision.
[0066] The light confinement layer is grown using a two-stage variable-parameter MOCVD epitaxial growth method: The first stage is vertical longitudinal growth, with a growth temperature of 920℃, a reaction pressure of 500mbar, a V / III molar ratio of 800, and a growth time of 10min. The GaN crystal has a longitudinal growth thickness of about 600nm and a longitudinal / transverse growth rate ratio of about 5:1. The crystal in the central growth window and the patterned window is vertically raised, and a regular cavity is reserved above the patterned mask retention area for short-wavelength devices. The second stage involves lateral closure and sealing of the cavity. The growth temperature is set to 1030℃, the reaction pressure to 80mbar, the V / III molar ratio to 4200, the growth time to 6min, and the lateral / vertical growth rate ratio to approximately 2.5:1. The GaN crystal rapidly spreads and bridges above the patterned mask retention areas on both sides, forming a closed air cavity with a height of 180nm. Dense GaN conductivity is formed in the central growth window region.
[0067] An n-GaN lower waveguide layer, a 405nm short-wavelength InGaN multi-quantum-well active layer, a P-type GaN upper waveguide, an AlGaN electron blocking layer, and a P-type GaN contact layer are sequentially epitaxially grown. Subsequent etching forms ridge-shaped mesa surfaces, P and N electrodes are fabricated, and cavity surface coating and die cleaving are completed to finally obtain a violet laser.
[0068] This example addresses the challenges of severe light field leakage and difficult light confinement in the violet band. By employing a λ / 9 subwavelength evanescent wave matching design, the light field confinement is precisely enhanced, significantly reducing the threshold current of short-wavelength lasers and improving beam quality and device efficiency.
[0069] 520nm green gallium nitride edge-emitting laser Using an n-type GaN homogeneous substrate, a 200nm thick SiN layer is deposited on the surface as a mask layer. After photolithography patterning, a 6μm wide central growth window is formed to ensure the integrity of the vertical conductivity and thermal conductivity pathways of the device. The patterned mask retention areas on both sides of the central growth window are strip-shaped mask strips or island-shaped mask blocks. Their width is designed based on the 520nm green laser wavelength matching, with a theoretically optimal subwavelength width of 58nm (520nm / 9). The strip-shaped mask strips or island-shaped mask blocks are designed with a width of 58nm. This size can be adapted to the lateral penetration depth of the evanescent wave of the green laser mode field, matching the characteristic scale of optical field leakage in the green light band. This solves the industry problems of large mode field dispersion, weak optical confinement, and high threshold of green GaN lasers. The engineering size can be finely adjusted to adapt to mass production photolithography processes while retaining the core optical mechanism.
[0070] A two-stage variable-parameter MOCVD epitaxial growth method is used to grow the lower light confinement layer, which is compatible with green light epitaxial processes. The first stage is vertical growth, with a growth temperature of 950℃, a reaction pressure of 400mbar, a V / III molar ratio of 1200, and a growth time of 7min. The GaN crystal grows to a thickness of about 450nm vertically, and the vertical / horizontal growth rate ratio is about 3.5:1. The vertical elevation in the central growth window and patterned window, and the complete cavity space above the patterned mask retention area are reserved. The second stage involves lateral closure and sealing, switching to a growth temperature of 1050℃, a reaction pressure of 120mbar, a V / III molar ratio of 3800, a growth time of 4min, and a lateral / vertical growth rate ratio of approximately 2.5:1. The GaN crystal rapidly spreads, bridges, and closes from the central growth window and patterned window to the area above the patterned mask retention areas on both sides, forming a closed air cavity with a height of 200nm in situ above the area above the patterned mask retention areas on both sides. The central growth window area maintains a dense and defect-free GaN crystal structure throughout the process, ensuring stable optoelectronic and thermal performance of the device.
[0071] A 150 nm thick n-GaN lower waveguide layer, a 520 nm high-indium composition InGaN / GaN multiple quantum well active layer, a P-type GaN upper waveguide, an AlGaN electron blocking layer, and a P-type GaN contact layer were sequentially epitaxially grown. Subsequent etching formed a 5 μm wide ridge-shaped mesa to match the green light mode field size. P and N electrode deposition, cavity surface coating, and die cleaving were then completed to fabricate a high-performance green gallium nitride edge-emitting laser.
[0072] Compared to blue and violet light, green light exhibits greater mode field penetration depth, leading to more pronounced transverse and substrate-side leakage issues, and conventional waveguide structures suffer from extremely low optical confinement factors. This example utilizes evanescent wave matching modulation of λ / 9 subwavelength air holes to effectively construct a high-contrast equivalent refractive index barrier, significantly suppressing green light mode field dispersion and substrate tunneling leakage. This dramatically improves the optical confinement efficiency of the green laser, reduces the threshold current, and enhances far-field beam quality. Furthermore, leveraging the low dislocation characteristics of the homogeneous substrate, it also improves the luminous efficiency and long-term reliability of the green light device.
[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A gallium nitride semiconductor laser, characterized in that, It includes, in order from bottom to top, a gallium nitride substrate, a mask layer, a lower light confinement layer, a lower waveguide layer, an active layer, and a p-type structure layer. The mask layer has a central growth window extending along the resonant cavity direction and a plurality of patterned windows located on both sides of the central growth window. The central growth window and the plurality of patterned windows divide the mask layer into a plurality of patterned mask retention portions located on both sides of the central growth window. The lower light confinement layer fills the central growth window and the plurality of patterned windows, and extends above the plurality of patterned mask retention portions. A void is formed between the side of the plurality of patterned mask retention portions facing away from the gallium nitride substrate and the upper lower light confinement layer. The p-type structure layer has a ridge structure extending along the direction of the resonant cavity on the side away from the gallium nitride substrate, and the orthogonal projection of the ridge structure on the surface of the gallium nitride substrate is located within the central growth window. The voids are located on both sides of the central growth window perpendicular to the direction of the resonant cavity, and the voids on each side are arranged in at least two columns, with each column of voids arranged along the direction of the resonant cavity.
2. The gallium nitride semiconductor laser as described in claim 1, characterized in that, Each column of voids is a continuous strip-shaped void extending along the direction of the resonant cavity; or, each column of voids comprises a plurality of discrete voids spaced apart along the direction of the resonant cavity.
3. The gallium nitride semiconductor laser as described in claim 1, characterized in that, The lasing wavelength of the gallium nitride semiconductor laser is λ, and the width of the plurality of patterned mask retention portions in the direction perpendicular to the resonant cavity is 1 / 10 to 1 / 8 of the lasing wavelength of the gallium nitride semiconductor laser.
4. The gallium nitride semiconductor laser as described in claim 3, characterized in that, The width of the plurality of patterned mask retention portions in the direction perpendicular to the resonant cavity is 1 / 9 of the lasing wavelength of the gallium nitride semiconductor laser.
5. The gallium nitride semiconductor laser as described in claim 1, characterized in that, The distance between the side of the orthographic projection and the side of the central growth window in the direction perpendicular to the resonant cavity is greater than zero.
6. A method for fabricating a gallium nitride semiconductor laser, characterized in that, Includes the following steps: S1. Provide a gallium nitride substrate and form a common mask layer on the surface of the gallium nitride substrate; S2. Pattern the common mask layer to form multiple mask units. Each mask unit includes a mask layer, a central growth window extending along the resonant cavity direction, and multiple patterned windows. The multiple patterned windows of each mask unit are located on both sides of the central growth window. The central growth window and the multiple patterned windows divide the mask layer of each mask unit into multiple patterned mask retention portions located on both sides of the central growth window. S3. Vertical growth of the lower light confinement layer is performed in the central growth window and the plurality of patterned windows of each mask unit, and a cavity is reserved above the plurality of patterned mask retention portions; lateral growth of the lower light confinement layer is performed, so that the crystals grown from the central growth window and the plurality of patterned windows grow laterally toward the plurality of patterned mask retention portions and close together, forming a cavity located between the plurality of patterned mask retention portions and the lower light confinement layer; S4. A lower waveguide layer, an active layer, and a p-type structure layer are epitaxially grown sequentially on the lower optical confinement layer. S5. Etch the p-type structure layer to form multiple ridge structures corresponding to the multiple mask units, wherein the orthographic projection of each ridge structure on the surface of the gallium nitride substrate is located within the central growth window of the corresponding mask unit; S6. P electrodes and N electrodes are formed on the top surface of the ridge structure and the bottom surface of the gallium nitride substrate, respectively, and a plurality of gallium nitride semiconductor lasers are obtained by cleaving.
7. The method for fabricating a gallium nitride semiconductor laser as described in claim 6, characterized in that, In step S2, the plurality of patterned mask retention portions located on each side of the central growth window include at least two continuous strip mask strips extending along the resonant cavity direction and divided by the patterned window; or, the plurality of patterned mask retention portions located on each side of the central growth window include at least two rows of island-shaped mask blocks arranged along the resonant cavity direction and divided by the patterned window.
8. The method for fabricating a gallium nitride semiconductor laser as described in claim 7, characterized in that, The width of the continuous strip mask or the island mask block in the direction perpendicular to the ridge structure is 1 / 10 to 1 / 8 of the lasing wavelength of the gallium nitride semiconductor laser.
9. The method for fabricating a gallium nitride semiconductor laser as described in claim 8, characterized in that, The width of the continuous strip mask or the island mask block in the direction perpendicular to the ridge structure is 1 / 9 of the lasing wavelength of the gallium nitride semiconductor laser.
10. The method for fabricating a gallium nitride semiconductor laser as described in claim 6, characterized in that, In step S3, during the longitudinal growth of the lower light confinement layer, the ratio of the longitudinal growth rate to the lateral growth rate of the lower light confinement layer is greater than or equal to 3:1, and in step S3, during the lateral growth of the lower light confinement layer, the ratio of the lateral growth rate to the longitudinal growth rate of the lower light confinement layer is greater than or equal to 2:1.