Method for manufacturing a prepreg window and printed circuit board

By alternately stacking prepreg and release film and fixing them with a pressure plate, combined with laser cutting, the problem of warping of prepreg during window opening was solved, improving the processing quality and electrical connection reliability of printed circuit boards.

CN123145802APending Publication Date: 2026-11-20AIFANG INTELLIGENT MANUFACTURING (THAILAND) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611435518.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Prepregs are prone to warping when laser-cut, which affects their use.

Method used

Prepreg and release film are stacked alternately and covered with a pressure plate on top to form a multi-layer structure. The pressure plate is used to fix the prepreg, and laser cutting is used to ensure cutting accuracy and stability.

Benefits of technology

It reduces the risk of thermal warpage of prepreg, improves the quality and precision of windowed edges, and enhances the finished product quality and electrical connection reliability of printed circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123145802A_ABST
    Figure CN123145802A_ABST
Patent Text Reader

Abstract

The embodiment of the application provides a manufacturing method of a prepreg window and a printed circuit board, and relates to the technical field of circuit board manufacturing. The manufacturing method comprises the following steps: alternately stacking at least one prepreg and at least two release films, and each prepreg is provided with a release film on both sides; pressing a cover plate on the top release film to fix the prepreg, the release film and the cover plate into an integrated body to form a multilayer structure; wherein the cover plate in the multilayer structure is provided with a window with the same position and shape as a preset window area on the prepreg; performing laser cutting on the preset window area on each prepreg through the window; and separating the prepreg from the multilayer structure. The manufacturing method can improve the warping problem of the prepreg during the manufacturing of the window, improve the shape quality of the window on the prepreg, and thus is beneficial to improving the finished product quality of the printed circuit board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to circuit board manufacturing technology, and more particularly to a method for manufacturing a windowed prepreg and a printed circuit board. Background Technology

[0002] Printed circuit boards (PCBs) are the basic carriers of various electronic devices. They use an insulating substrate as the base and form patterned conductive lines on the substrate to carry various electronic components and realize electrical connections between different electronic components.

[0003] Multilayer printed circuit boards (PCBs) are mainly composed of alternating layers of conductive lines and insulating adhesive media (prepregs). Electrical interconnection between layers is achieved through vias. They are widely used in various electronic products such as communications, industrial control, and consumer electronics. The prepreg acts as insulation and adhesion between adjacent inner core layers. In some applications, the prepreg needs to be windowed to meet requirements for localized heat dissipation, insulation clearance, or structural assembly.

[0004] Prepreg windows can be made using laser cutting; however, laser cutting involves high temperatures, which can cause the prepreg to warp after cutting, affecting its usability. Summary of the Invention

[0005] This application provides a method for manufacturing a windowed prepreg to improve the problem of warping when manufacturing a windowed prepreg.

[0006] In a first aspect, embodiments of this application provide a method for manufacturing a windowed prepreg, comprising:

[0007] At least one prepreg and at least two release films are stacked alternately, with the release film on both sides of each prepreg;

[0008] A pressure plate is pressed onto the release film at the top to fix the prepreg, the release film, and the pressure plate into a single unit, forming a multi-layer structure; wherein, the pressure plate in the multi-layer structure has a window with the same position and shape as the preset window area on the prepreg;

[0009] The preset window area on each of the prepreg sheets is laser-cut through the window;

[0010] The semi-cured sheet is separated from the multilayer structure.

[0011] In one possible implementation, before laser cutting the preset windowed area on each of the prepreg sheets through the window, the method further includes:

[0012] The thickness of the prepreg is divided into multiple preset levels, and each preset level is matched with the corresponding laser cutting single pulse energy and laser pulse width.

[0013] In one possible implementation, the preset gear includes:

[0014] In the first gear position, the thickness of the prepreg in the first gear position is greater than or equal to 0.04 mm and less than or equal to 0.08 mm, the laser cutting single pulse energy is greater than or equal to 0.08 mJ and less than or equal to 0.12 mJ, and the laser pulse width is greater than or equal to 75 ns and less than or equal to 85 ns.

[0015] In the second gear, the thickness of the prepreg in the second gear is greater than or equal to 0.1 mm and less than or equal to 0.15 mm, the laser cutting single pulse energy is greater than or equal to 0.15 mJ and less than or equal to 0.2 mJ, and the laser pulse width is greater than or equal to 95 ns and less than or equal to 105 ns.

[0016] In the third gear, the thickness of the prepreg in the third gear is greater than or equal to 0.18 mm, the laser cutting single pulse energy is greater than or equal to 0.22 mJ and less than or equal to 0.28 mJ, and the laser pulse width is greater than or equal to 115 ns and less than or equal to 125 ns.

[0017] In one possible implementation, when the thickness of the prepreg is at the first or second level, the preset cutting method of the prepreg is unidirectional single-pass cutting.

[0018] When the thickness of the prepreg is at the third level, the preset cutting method of the prepreg is bidirectional reciprocating cutting.

[0019] In one possible implementation, before alternatingly stacking at least one prepreg sheet and at least two release films, the method further includes:

[0020] The prepreg and the release film are cut to the same shape and size, and the edges of the prepreg and the release film are provided with a preset allowance.

[0021] In one possible implementation, before cutting the prepreg and the release film to the same shape and size, the method further includes:

[0022] The semi-cured sheet with a thickness of 0.08 mm or less is subjected to constant temperature drying treatment, and the semi-cured sheet is supported by a cutting table with a soft pad.

[0023] In one possible implementation, before laser cutting the preset windowed area on each of the prepreg sheets through the window, the method further includes:

[0024] Obtain the outline of the preset window area, and offset the outline of the preset window area inward by half the laser spot diameter based on the laser cutting spot diameter to obtain the preset cutting trajectory.

[0025] In one possible implementation, the edge of the pressure plate in the multilayer structure is flush with the edge of the prepreg.

[0026] In one possible implementation, the pressure plate is an aluminum alloy plate with a thickness greater than or equal to 0.15 mm and less than or equal to 0.2 mm.

[0027] The method for fabricating a windowed prepreg provided in this application involves alternately stacking at least one prepreg and at least two release films. Each prepreg has a release film on both sides, allowing for easy peeling after cutting to separate the prepreg. A pressure plate is placed on the top release film, with windows in the same position and shape as the prepreg's prepreg window area. This fixes the prepreg, release film, and pressure plate together, forming a multi-layer structure. The pressure plate maintains pressure on the prepreg below and also holds the prepreg at the window edges after cutting, providing stable pressure and limiting the prepreg, reducing the risk of thermal warping. Laser cutting is performed on the prepreg's prepreg area through the windows. The windows are flush with the boundaries of the prepreg areas, preventing laser ablation beyond the prepreg area and improving edge quality. The prepreg is then separated from the multi-layer structure, completing the prepreg window fabrication.

[0028] Secondly, embodiments of this application provide a printed circuit board, wherein the dielectric layer of the printed circuit board is made of a prepreg, and the openings on the prepreg are made using the manufacturing method described in any of the above possible embodiments.

[0029] The printed circuit board provided in this application embodiment uses the above-described manufacturing method to fabricate the prepreg for the dielectric layer. During the windowing process, the prepreg can be fixed as a whole by alternately stacking release films and using pressure plates with corresponding windows. This makes it less likely for the edges of the prepreg to lift, and the laser ablation only acts on the preset window area, thereby reducing the stress deformation of the prepreg. This improves the accuracy of the window outline and the consistency of dimensions, thereby improving the subsequent printed circuit board lamination quality, component assembly accuracy, and electrical connection reliability, which is beneficial to improving the finished quality of the printed circuit board.

[0030] In addition to the technical problems solved by the embodiments of this application, the technical features constituting the technical solutions, and the beneficial effects brought about by the technical features of these technical solutions described above, other technical problems that can be solved by the technical solutions provided by this application, other technical features contained in the technical solutions, and the beneficial effects brought about by these technical features will be further explained in detail in the specific embodiments. Attached Figure Description

[0031] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0032] Figure 1 A flowchart illustrating a method for manufacturing a windowed prepreg according to this application;

[0033] Figure 2 A schematic diagram of a multi-layer structure provided in this application;

[0034] Figure 3 for Figure 2 A schematic diagram of the structure of the prepreg.

[0035] Explanation of reference numerals in the attached figures:

[0036] 100. Pre-cured sheet; 110. Preset window area; 120. Preset cutting trajectory;

[0037] 200. Release film;

[0038] 300, pressure plate; 310, window.

[0039] The accompanying drawings illustrate specific embodiments of this application, which will be described in more detail below. These drawings and descriptions are not intended to limit the scope of the concept in any way, but rather to illustrate the concept of this application to those skilled in the art through reference to particular embodiments. Detailed Implementation

[0040] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be described in more detail below with reference to the accompanying drawings. In the drawings, the same or similar reference numerals denote the same or similar components or components having the same or similar functions throughout. The described embodiments are some, but not all, embodiments of this application. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application. Other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are all within the scope of protection of this application. The embodiments of this application will be described in detail below with reference to the accompanying drawings.

[0041] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, an indirect connection through an intermediate medium, or the internal communication between two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0042] In the description of this application, it should be understood that the terms "upper", "lower", "front", "rear", "left", "right", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0043] The terms "first," "second," "third," "fourth," etc., used in the specification and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented, for example, in a sequence other than those illustrated or described herein.

[0044] Furthermore, the terms “comprising” and “having”, and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or components is not necessarily limited to those steps or components that are explicitly listed, but may include other steps or components that are not explicitly listed or that are inherent to those processes, methods, products, or apparatuses.

[0045] Printed circuit boards (PCBs) are the basic carriers of various electronic devices. They use an insulating substrate as the base and form patterned conductive lines on the substrate to carry various electronic components and realize electrical connections between different electronic components.

[0046] Multilayer printed circuit boards (PCBs) are mainly composed of alternating layers of conductive lines and insulating adhesive media (prepregs). Electrical interconnection between layers is achieved through vias. They are widely used in various electronic products such as communications, industrial control, and consumer electronics. The prepreg acts as insulation and adhesion between adjacent inner core layers. In some applications, the prepreg needs to be windowed to meet requirements for localized heat dissipation, insulation clearance, or structural assembly.

[0047] Prepreg windows can be made using laser cutting; however, laser cutting involves high temperatures, which can cause the prepreg to warp after cutting, affecting its usability.

[0048] Based on this, this application proposes a method for fabricating windows on prepreg sheets. This involves alternately stacking at least one prepreg sheet and at least two release films. Each prepreg sheet has release films on both sides, allowing for easy peeling of the release films after cutting, thus separating the prepreg sheet. A pressure plate is placed on top of the release film, with windows in the same position and shape as the prepreg sheet's prepreg opening areas. This fixes the prepreg sheet, release films, and pressure plate into a multi-layer structure. The pressure plate maintains pressure on the prepreg sheet below and also holds the prepreg sheet at the window edges after cutting, providing stable pressure and limiting the prepreg sheet, reducing the risk of thermal warping. The prepreg opening areas on each prepreg sheet are then laser-cut through the windows. The windows are flush with the boundaries of the prepreg opening areas, preventing laser ablation of the prepreg sheet beyond the prepreg opening areas and improving the edge quality of the openings. The prepreg sheet is then separated from the multi-layer structure, completing the prepreg sheet window fabrication.

[0049] The technical solution of this application and how the technical solution of this application solves the above-mentioned technical problems are described in detail below with specific embodiments. These specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described again in some embodiments. The embodiments of this application will now be described with reference to the accompanying drawings.

[0050] Firstly, referring to Figure 1 , Figure 2 and Figure 3 This embodiment provides a method for manufacturing a windowed prepreg, which may include the following steps:

[0051] S101. At least one semi-cured sheet 100 and at least two release films 200 are stacked alternately, and each semi-cured sheet 100 has a release film 200 on both sides.

[0052] In this step, the prepreg 100 and release film 200 are stacked alternately so that the upper and lower surfaces of each prepreg 100 are covered by the release film 200. This can provide interface isolation and support for the prepreg 100 during subsequent pressing and laser cutting, while reducing the chance of cutting debris coming into direct contact with the prepreg 100.

[0053] In some embodiments, before alternatingly stacking at least one prepreg 100 and at least two release films 200, the following may also be done:

[0054] The prepreg 100 and release film 200 are cut to the same shape and size, and the edges of the prepreg 100 and release film 200 are provided with a preset allowance.

[0055] The preset allowance refers to the portion of the outer edges of the prepreg 100 and release film 200 that extend beyond the outer edge of the core board of the adapted printed circuit board. The purpose of setting the preset allowance on the prepreg 100 is to allow for the necessary dimensions for alignment during subsequent pressing, serving as a positioning structure or clamping area. Simultaneously, the preset allowance of the prepreg 100 and release film 200 also provides clamping areas during subsequent laser cutting of the prepreg 100, thereby improving positional stability.

[0056] In practical implementation, the prepreg 100 and release film 200 can be uniformly cut according to the outline of the prepreg 100, the location of the target window area, and the size of the window 310 of the pressure plate 300, so that their dimensions are consistent and the same preset allowance is retained at the edges. The preset allowance is not less than 5mm on each side to ensure that the preset allowance is sufficient for use. For example, it can be 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, etc.

[0057] For example, the prepreg 100 and the release film 200 can be cut simultaneously. The cutting head for cutting the prepreg 100 and the cutting head for cutting the release film 200 are set on the same movable cutter seat, so as to achieve the same size cutting of the prepreg 100 and the release film 200.

[0058] Since the prepreg 100 and release film 200 are the same size, the materials of each layer are not prone to misalignment after being stacked alternately. With the reserved space at the edge, the stress concentration and edge lifting phenomenon can be reduced, thereby enabling the multi-layer structure to maintain high positioning stability and processing consistency during fixing, cutting and separation.

[0059] The release film 200 can be made of high-temperature modified polyethylene terephthalate (PET), with a short-term temperature resistance of ≥180℃, isolating it from the instantaneous high temperature of the laser to prevent interlayer adhesion after the resin of the prepreg 100 melts. After the prepreg 100 is laser-cut, the release film 200 can be directly peeled off layer by layer. The open edges of the prepreg 100 are free of stringing and adhesive buildup, making the peeling of the prepreg 100 easier during subsequent lamination and layout of the printed circuit board.

[0060] In some embodiments, before cutting the prepreg 100 and release film 200 to the same shape and size, the following may also be done:

[0061] Precursor sheets 100 with a thickness of 0.08 mm or less are subjected to constant temperature drying treatment, and the precursor sheets 100 are supported by a cutting table with a soft pad.

[0062] The constant temperature drying process refers to removing moisture and stabilizing volatile components from the prepreg 100 under constant temperature conditions, ensuring that the ultra-thin prepreg 100 with a thickness of 0.08 mm or less maintains a relatively stable moisture content and flatness before cutting. The padded cutting table refers to setting an elastic buffer layer on the cutting table surface to disperse local contact stress when supporting the prepreg 100, thus reducing the rigid support effect of the table on the thin material.

[0063] In practice, a prepreg sheet 100 with a thickness of 0.08 mm or less is first dried in a constant-temperature environment. This allows for the uniform release of residual moisture and reduces localized differences in moisture absorption. The temperature is controlled within a range that matches the thermal stability of the resin system to prevent warping, shrinkage, or edge undulations in the prepreg sheet 100 due to uneven moisture content during subsequent cutting and alternating stacking. For prepreg sheets 100 within this thickness range, the material rigidity is relatively low. If cut directly without drying, dimensional drift is easily caused by the coupling effect of moisture and heat, affecting the conformal cutting accuracy with the release film 200 and the consistency of interlayer bonding after subsequent alternating stacking. Stabilizing the material state through constant-temperature drying allows for a more stable profile after cutting and reduces deformation before window opening.

[0064] For example, a prepreg 100 with a thickness of less than or equal to 0.08 mm can be placed in a constant temperature drying cabinet at 25±2℃ and left to stand for at least 2 hours to fully release the internal stress in the prepreg 100.

[0065] When cutting the prepreg 100, the prepreg 100 is placed on a cutting table covered with a soft pad for support. The soft pad can be made of an elastic material layer with a certain degree of resilience. Its thickness and hardness are matched with the load-bearing requirements of the cutting equipment, so that the prepreg 100 is in a flexible support state during cutting, positioning and handling. Because the thin prepreg 100 has a small self-weight and weak bending resistance, stress concentration can easily occur when the flat and rigid table surface does not provide sufficient support for it locally. The soft pad can compensate for small thickness differences and buffer contact impact, thereby maintaining the flatness of the sheet and reducing edge warping and surface indentation.

[0066] For example, the pad can be made of silicone material, which can reduce the cutting speed by 30% when cutting a prepreg 100 with a thickness of less than or equal to 0.08 mm compared to prepregs 100 of other thicknesses, further reducing the risk of edge warping or curling of the prepreg 100.

[0067] S102. Press the pressure plate 300 onto the release film 200 at the top to fix the prepreg 100, release film 200 and pressure plate 300 into a whole, forming a multi-layer structure. The pressure plate 300 in the multi-layer structure is provided with a window 310 with the same position and shape as the preset window area 110 on the prepreg 100.

[0068] The pressure plate 300 is used to rigidly support and hold the prepreg 100 and the release film 200, making the prepreg 100 flat and not easy to curl, which is beneficial to improving the accuracy of subsequent laser cutting.

[0069] In some embodiments, the pressure plate 300 is a hard aluminum alloy plate with a thickness greater than or equal to 0.15 mm and less than or equal to 0.2 mm.

[0070] By controlling the thickness of the aluminum alloy pressure plate 300 between 0.15mm and 0.2mm, the pressure plate 300 possesses sufficient structural strength to maintain the boundary stability of the area corresponding to the window 310, while also avoiding excessive local compressive stress due to excessive plate thickness, thereby reducing the possibility of indentations or deformation on the surface of the prepreg 100. This thickness range also facilitates the prefabrication of the window 310 corresponding to the preset window opening area 110 on the pressure plate 300, and maintains the stability of the edge shape of the window 310 during laser cutting, thus ensuring that the laser only acts on the target area and reduces damage to surrounding materials.

[0071] In some embodiments, the edge of the pressure plate 300 in the multilayer structure is flush with the edge of the prepreg 100.

[0072] The pressure plate 300 can be made by conventional rolling or cutting of aluminum alloy sheet. Its size is the same as the outer size of the prepreg 100 to be made into a window, which facilitates the alignment of the window 310 on the pressure plate 300 with the preset window area 110 on the prepreg 100. After pressing, the pressure plate 300 and the prepreg 100 together define the overall boundary of the multi-layer structure, making the relative position between the processing area of ​​the window 310 and the surrounding fixed area more stable. Since the outer edge of the pressure plate 300 does not exceed the outer edge of the prepreg 100, the stress on the outer periphery after lamination is more balanced.

[0073] The prepreg 100, release film 200 and pressure plate 300 can be bonded and fixed together with masking tape. In the multi-layer structure formed by the prepreg 100, release film 200 and pressure plate 300, the number of prepregs 100 is the same as the number required when the final printed circuit board is laminated and arranged. In the subsequent lamination process, there is no need to count them and they can be used directly, which improves efficiency.

[0074] For example, the pressure plate 300 can be made of 0.15mm hard aluminum alloy. It can be cut and shaped once and reused. Before each use, wipe the surface oil and resin debris with a lint-free cloth. If scratches or dents appear, it should be scrapped and replaced immediately to prevent uneven support of the pressure plate 300 from causing the window size deviation on the prepreg 100.

[0075] S103, Laser cutting is performed on the preset window area 110 on each semi-cured sheet 100 through window 310.

[0076] In some embodiments, the prepreg 100 is cut using an ultraviolet laser cutting machine. The ultraviolet laser cutting machine is a precision processing equipment that uses high-energy photons to directly break the molecular bonds of materials to achieve cold processing. Its advantages are small focused spot, high cutting accuracy, small heat-affected zone, and the ability to achieve automated processing.

[0077] In some embodiments, before laser cutting the preset windowed area 110 on each prepreg 100 through window 310, the following may also be performed:

[0078] The thickness of the prepreg 100 is divided into multiple preset levels, and each preset level is matched with the corresponding laser cutting single pulse energy and laser pulse width.

[0079] In practical implementation, the thickness range of the semi-cured sheet of conventional processing can be determined first, the range can be divided into multiple preset levels, and the correspondence between the levels and the laser cutting single pulse energy and laser pulse width can be established in the control system in advance.

[0080] For thinner prepreg 100, a lower laser cutting single-pulse energy and a shorter laser pulse width can be used to ensure stable removal within the window 310 while avoiding excessive heat input. For thicker prepreg 100, a relatively higher laser cutting single-pulse energy and a longer laser pulse width can be used to ensure sufficient cutting depth and continuous cutting.

[0081] By matching prepregs 100 of different thicknesses to the corresponding settings, the laser irradiation depth, heat-affected zone, and material removal rate can be kept within a controllable range. This reduces edge ablation, resin carbonization, and incomplete cutting during window cutting (310), and ensures that the windowing effect of prepregs 100 of different batches and thicknesses is more consistent.

[0082] Furthermore, in some embodiments, the preset gear position includes:

[0083] In the first gear, the thickness of the prepreg 100 is greater than or equal to 0.04 mm and less than or equal to 0.08 mm, the laser cutting single pulse energy is greater than or equal to 0.08 mJ and less than or equal to 0.12 mJ, and the laser pulse width is greater than or equal to 75 ns and less than or equal to 85 ns.

[0084] In the second gear, the thickness of the prepreg 100 is greater than or equal to 0.1 mm and less than or equal to 0.15 mm, the laser cutting single pulse energy is greater than or equal to 0.15 mJ and less than or equal to 0.2 mJ, and the laser pulse width is greater than or equal to 95 ns and less than or equal to 105 ns.

[0085] In the third gear, the thickness of the prepreg 100 is greater than or equal to 0.18 mm, the laser cutting single pulse energy is greater than or equal to 0.22 mJ and less than or equal to 0.28 mJ, and the laser pulse width is greater than or equal to 115 ns and less than or equal to 125 ns.

[0086] Prepreg 100 with a thickness between 0.04 mm and 0.08 mm corresponds to a laser cutting single-pulse energy of 0.08 mJ to 0.12 mJ and a laser pulse width of 75 ns to 85 ns. This ensures that the laser energy is controlled within a range that allows penetration of the ultra-thin prepreg 100 without excessive heat accumulation, thereby reducing the possibility of edge ablation and resin charring. Prepreg 100 with a standard thickness of 0.1 mm to 0.15 mm corresponds to a laser cutting single-pulse energy of 0.15 mJ to 0.2 mJ and a laser pulse width of 95 ns to 105 ns. This ensures cutting stability while suppressing cutting discontinuities caused by insufficient energy. Prepreg 100 with a thickness of not less than 0.18 mm corresponds to a laser cutting single-pulse energy of 0.22 mJ to 0.28 mJ and a laser pulse width of 115 ns to 125 ns. This compensates for the effects of thicker materials on laser attenuation and heat diffusion, resulting in a more consistent cutting depth.

[0087] By adjusting the laser output energy and matching the corresponding pulse width, the window size and tolerance of the prepreg can be stably controlled to meet the precision requirements of different customers. After the window is processed, a three-dimensional measuring device is used to carry out full-item inspection, collecting the coordinates of the four corners of the window, the length and width dimensions, the radius of the rounded corners, and the offset of the rivet positioning holes. Five sets of data are collected and stored for each window point. At the same time, the four sides of the window 310 are visually inspected with a 10x magnifying glass. The acceptance criteria are: the cut is straight and smooth, there are no fiberglass burrs, no resin adhesion, and no melt overflow.

[0088] In some embodiments, the linear cutting speed is uniformly set to 800mm / s-1200mm / s. When it reaches the corner of the preset window area 110, the laser cutting equipment automatically reduces its speed to 400mm / s-600mm / s to prevent dimensional deviations in the arc contour caused by high-speed cutting. The entire laser cutting process runs continuously without interruption or repeated overlapping scans, which helps reduce resin carbonization and gelling defects caused by local heat accumulation.

[0089] In some embodiments, when the thickness of the prepreg 100 is at the first or second level, the preset cutting method of the prepreg 100 is unidirectional single-pass cutting; when the thickness of the prepreg 100 is at the third level, the preset cutting method of the prepreg 100 is bidirectional reciprocating cutting.

[0090] In practice, when the thickness of the prepreg 100 is in the first or second range, corresponding to the ultra-thin and standard thickness ranges, a single unidirectional laser scan is sufficient to complete the cut. The scanning path aligns with the boundary of the window 310 of the pressure plate 300, ensuring that the laser energy forms a continuous and concentrated removal zone within the material. Because thinner materials have shorter thermal penetration distances and lower melt discharge resistance, a single unidirectional, single-pass cut is sufficient to penetrate the prepreg 100, thus reducing processing time.

[0091] When the prepreg 100 thickness is at the third level, corresponding to a thicker material range, the laser is controlled to perform bidirectional reciprocating cutting along the same cutting path. The forward cutting is used to form the initial kerf, while the reverse cutting is used to supplement the energy input to areas that are not fully penetrated, ensuring the stable removal of residual connecting parts inside the thicker material. Because the thicker prepreg 100 has a greater laser absorption depth and heat conduction path, a single unidirectional scan may result in localized incomplete cuts or edge slag. Using bidirectional reciprocating cutting can improve the consistency of kerf penetration and reduce the risk of localized incomplete cuts.

[0092] In some embodiments, before laser cutting the preset window area 110 on each prepreg 100 through window 310, a negative pressure vacuum adsorption platform can be used to support the multi-layer structure. The negative pressure value is 0.07MPa-0.09MPa, the flatness of the processing area of ​​the platform used to support the multi-layer structure is no greater than 0.01mm, and the laser is incident perpendicularly to improve the cutting accuracy.

[0093] In some embodiments, during laser cutting, an air intake channel or the device's built-in synchronous air intake duct is required to remove fine carbon powder and resin debris generated by laser ablation in real time. This ensures dust-free operation during laser cutting and reduces the likelihood of dust adhering to the surface of the prepreg 100. After cutting, the prepreg 100 is removed and placed in a closed waste collection box. It is gently shaken to remove ablation waste from the window. Then, a handheld low-pressure vacuum cleaner is used to thoroughly clean the inner wall of the window and the front and back surfaces of the prepreg 100, removing any remaining fine debris. Cleaning acceptance criteria: The prepreg 100 is visually free of dust and resin particle residue, and the surface is free of black stains when wiped with a white lint-free cotton swab.

[0094] In some embodiments, before laser cutting the preset windowed area 110 on each prepreg 100 through window 310, the following may also be performed:

[0095] Obtain the outline of the preset window area 110, and offset the outline of the preset window area 110 inward by half the spot diameter based on the laser cutting spot diameter to obtain the preset cutting trajectory 120.

[0096] The laser cutting spot diameter refers to the effective width of the laser beam on the surface of the prepreg 100. This parameter indicates the actual coverage of the laser energy on the prepreg 100 and directly affects the consistency between the kerf boundary and the final window size. The preset cutting trajectory 120 is the actual motion path calculated based on the contour. It has a preset compensation relationship with the target boundary of the preset window area 110 and is used to guide the laser along the compensated path to complete the cutting shape.

[0097] Specifically, the offset is set according to half the spot diameter, which is determined based on the energy distribution and material removal mechanism of laser cutting. When the preset cutting trajectory 120 is located at half the spot width inside the target boundary, the edge of the laser action just covers the boundary position of the preset window area 110, thereby making the actual window boundary match the preset window area 110. Combined with the window 310 structure of the pressure plate 300, it suppresses the overcutting of the window edge caused by the spot diameter, thereby improving the contour accuracy, edge cleanliness and processing consistency of the window of the prepreg 100.

[0098] For example, if the laser cutting spot diameter is 0.03mm, the boundary of the preset window area 110 is offset inward by 0.015mm to offset the laser ablation damage to the prepreg 100, thus controlling the window size tolerance of the prepreg 100 within ±0.05mm. When the design end creates the laser-cut prepreg 100 data, it outputs two types of DXF format files: one is the rivet positioning hole layer file, and the other is the laser window cutting path layer file. The layers distinguish different line widths and preset levels, and the laser cutting equipment can directly read the layers without secondary conversion, avoiding graphic offset.

[0099] S104. Separate the prepreg 100 from the multilayer structure.

[0100] During the separation process of the prepreg 100, the release film 200 can be easily separated from the prepreg 100 due to its release properties. The edges of the prepreg 100 opening are not easily damaged by peeling, thus maintaining the integrity of the opening outline.

[0101] Secondly, this application provides a printed circuit board, the dielectric layer of which is made of a prepreg 100, and the openings on the prepreg 100 are made using the manufacturing method described in the above embodiments.

[0102] In the printed circuit board of this application embodiment, the prepreg 100 for making the dielectric layer is manufactured using the above-described manufacturing method. During the windowing process, the prepreg 100 can be alternately stacked with release film 200 and fixed as a whole with pressure plate 300 with corresponding window 310. This makes it less likely for the edge of the prepreg 100 to lift up, and the laser ablation only acts on the preset windowing area 110, thereby reducing the stress deformation of the prepreg 100, improving the windowing contour accuracy and dimensional consistency, and thus improving the subsequent printed circuit board lamination quality, component assembly accuracy and electrical connection reliability, which is beneficial to improving the finished quality of the printed circuit board.

[0103] Other embodiments of this application will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This application is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary techniques in the art not disclosed herein. The specification and embodiments are to be considered exemplary only.

[0104] It should be understood that this application is not limited to the precise structure described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope.

Claims

1. A method for manufacturing a prepreg with windows, characterized in that, include: At least one prepreg and at least two release films are stacked alternately, with the release film on both sides of each prepreg; A pressure plate is pressed onto the release film at the top to fix the prepreg, the release film, and the pressure plate into a single unit, forming a multi-layer structure; wherein, the pressure plate in the multi-layer structure has a window with the same position and shape as the preset window area on the prepreg; The preset window area on each of the prepreg sheets is laser-cut through the window; The semi-cured sheet is separated from the multilayer structure.

2. The method for manufacturing a windowed prepreg according to claim 1, characterized in that, Before laser cutting the preset windowed area on each of the prepreg sheets through the window, the method further includes: The thickness of the prepreg is divided into multiple preset levels, and each preset level is matched with the corresponding laser cutting single pulse energy and laser pulse width.

3. The method for manufacturing a windowed prepreg according to claim 2, characterized in that, The preset gears include: In the first gear position, the thickness of the prepreg in the first gear position is greater than or equal to 0.04 mm and less than or equal to 0.08 mm, the laser cutting single pulse energy is greater than or equal to 0.08 mJ and less than or equal to 0.12 mJ, and the laser pulse width is greater than or equal to 75 ns and less than or equal to 85 ns. In the second gear, the thickness of the prepreg in the second gear is greater than or equal to 0.1 mm and less than or equal to 0.15 mm, the laser cutting single pulse energy is greater than or equal to 0.15 mJ and less than or equal to 0.2 mJ, and the laser pulse width is greater than or equal to 95 ns and less than or equal to 105 ns. In the third gear, the thickness of the prepreg in the third gear is greater than or equal to 0.18 mm, the laser cutting single pulse energy is greater than or equal to 0.22 mJ and less than or equal to 0.28 mJ, and the laser pulse width is greater than or equal to 115 ns and less than or equal to 125 ns.

4. The method for manufacturing a windowed prepreg according to claim 3, characterized in that, When the thickness of the prepreg is at the first or second level, the preset cutting method of the prepreg is unidirectional single-pass cutting. When the thickness of the prepreg is at the third level, the preset cutting method of the prepreg is bidirectional reciprocating cutting.

5. The method for manufacturing a windowed prepreg according to claim 1, characterized in that, Before alternatingly stacking at least one prepreg and at least two release films, the process also includes: The prepreg and the release film are cut to the same shape and size, and the edges of the prepreg and the release film are provided with a preset allowance.

6. The method for manufacturing a windowed prepreg according to claim 5, characterized in that, Before cutting the prepreg and the release film to the same shape and size, the process further includes: The semi-cured sheet with a thickness of 0.08 mm or less is subjected to constant temperature drying treatment, and the semi-cured sheet is supported by a cutting table with a soft pad.

7. The method for manufacturing a windowed prepreg according to claim 1, characterized in that, Before laser cutting the preset windowed area on each of the prepreg sheets through the window, the method further includes: Obtain the outline of the preset window area, and offset the outline of the preset window area inward by half the laser spot diameter based on the laser cutting spot diameter to obtain the preset cutting trajectory.

8. The method for manufacturing a windowed prepreg according to claim 1, characterized in that, In the multi-layer structure, the edge of the pressure plate is flush with the edge of the prepreg.

9. The method for manufacturing a prepreg with windows according to any one of claims 1-8, characterized in that, The pressure plate is an aluminum alloy plate with a thickness greater than or equal to 0.15 mm and less than or equal to 0.2 mm.