PCB anti-soldering process technology and system for improving adhesion and chemical resistance

By improving the process of graded composite pretreatment and segmented gradient pre-baking and curing, the problems of unstable adhesion and insufficient chemical corrosion resistance in the traditional PCB solder resist process have been solved, achieving stable adhesion of solder resist ink to the PCB board surface and improving chemical resistance.

CN123145808APending Publication Date: 2026-11-20TRUSTECH ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611213577.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In traditional PCB solder mask processes, the adhesion between the solder mask ink and the PCB board surface is unstable, and the chemical corrosion resistance is insufficient, which can easily lead to problems such as blistering, peeling, and discoloration.

Method used

A graded composite pretreatment process is adopted, including alkaline chemical degreasing, micro-etching chemical roughening, and ultrasonic cleaning with ultrapure water to form a micro-interlocking surface; two thin-layer coatings of solder resist ink are applied; segmented gradient pre-baking and segmented progressive post-curing are combined with CCD vision automatic alignment exposure and segmented pressure spray development.

Benefits of technology

It significantly improves the adhesion and chemical corrosion resistance of solder resist ink to the PCB board surface, avoids problems such as blistering, peeling, and discoloration, and improves the yield and reliability of PCB production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123145808A_ABST
    Figure CN123145808A_ABST
Patent Text Reader

Abstract

The application discloses a PCB anti-soldering process technology for improving adhesion and chemical resistance, which adopts hierarchical composite pretreatment to replace traditional grinding process, builds micro occlusal surface on the copper surface through alkaline oil removal and micro-etching roughening, removes impurities through ultrasonic cleaning, and strengthens ink adhesion effect. The ink is coated in two thin layers, the first layer fills the micro gap of the board surface, and the second layer is thickened to a certain thickness, so that the defects of solvent residue and uneven film thickness caused by single thick coating are solved. The process is set to be segmented gradient pre-baking and three-stage progressive post-curing, the stepwise temperature rise makes the solvent stratified volatilization and the crosslinking reaction sufficient, and the slow cooling after curing eliminates the internal stress of the ink. The scheme can make the anti-soldering layer crosslink completely, effectively improve the adhesion and chemical corrosion resistance of the anti-soldering layer, avoid the defects of blistering, falling off and discoloration in production, and improve the yield of PCB finished products and long-term use reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of PCB manufacturing technology, and in particular to a PCB solder mask process and system for improving adhesion and chemical resistance. Background Technology

[0002] The current traditional PCB solder mask process typically involves: pre-treatment grinding of the board → coating the entire board with solder mask ink → pre-baking → exposure → development → post-curing. Industry-standard processes often employ a single physical brushing process combined with conventional degreasing pre-treatment, where the solder mask ink adheres solely to the copper and substrate surfaces through physical adhesion. This single pre-treatment results in poor uniformity of copper surface roughness, easily leading to localized areas of excessive or insufficient roughness. Excessive roughness results in poor ink coverage and residual gaps, while insufficient roughness fails to create sufficient adhesion, leading to unstable overall adhesion between the solder mask ink and the board surface. Furthermore, conventional coating often uses a single, thick-coat application, resulting in poor ink thickness uniformity. Thick areas have difficulty evaporating solvent, while thin areas are prone to exposed copper defects. Subsequent curing can leave residual stress, leading to blistering and peeling issues during subsequent soldering and chemical treatment processes.

[0003] In addition, conventional pre-baking and post-curing often use constant temperature direct heating, which results in incomplete evaporation of the solvent inside the ink and uneven cross-linking and curing reaction. The resulting solder resist layer has insufficient chemical corrosion resistance and is prone to discoloration, wrinkling and peeling during acid plating, cleaning and other processes.

[0004] In response to the shortcomings of these existing processes, there is an urgent need for a process that can improve the adhesion of solder resist ink to the PCB board surface, while allowing the ink to crosslink more fully and evenly, and effectively improve the chemical corrosion resistance of the solder resist layer. Summary of the Invention

[0005] To address the shortcomings of the aforementioned technologies, this invention provides a PCB solder mask manufacturing process and system that enhances adhesion and chemical resistance.

[0006] To achieve the above objectives, the present invention provides a PCB solder mask process that improves adhesion and chemical resistance. S1, the PCB board surface is subjected to graded composite pretreatment, which includes alkaline chemical degreasing, micro-etching chemical roughening, ultrapure water ultrasonic cleaning and hot air drying in sequence, forming a micro-interlocking surface on the copper surface of the PCB board.

[0007] S2 uses semi-automatic screen printing and electrostatic spraying to apply solder resist ink to the PCB board in two thin layers. The first layer is a thin base coat of solder resist ink, and the second layer is a thicker, fixed-thickness coating of solder resist ink, controlling the total ink thickness to be 18-25μm.

[0008] S3 involves segmented gradient pre-baking of the coated PCB board, using a stepped heating method. The low-temperature section evaporates the ink solvent, while the high-temperature section performs preliminary curing.

[0009] S4 uses a CCD vision automatic alignment exposure machine to expose the pre-baked PCB board, and adjusts the exposure energy according to the PCB line density in different zones.

[0010] S5, develops the exposed PCB board to remove solder resist ink from the unexposed areas;

[0011] S6 involves segmented progressive curing of the developed PCB board. After being heated and held at a multi-stage temperature gradient in the curing oven, the temperature is slowly lowered to ensure complete cross-linking and curing of the solder resist ink.

[0012] As an improvement of the present invention, in step S1, the alkaline chemical degreasing uses an alkaline chemical degreasing agent to soak and spray the PCB board surface at 50°C for a treatment time of 1.5-3 minutes; the micro-etching chemical roughening uses a micro-etching agent to treat for 1-2.5 minutes to form a micro-interlocking surface on the copper surface; the ultrapure water ultrasonic cleaning uses low-pressure ultrapure water in conjunction with ultrasonic cleaning, and finally is dried with hot air.

[0013] As an improvement of the present invention, in step S1, a water washing process is further included between the alkaline chemical degreasing and the micro-etching chemical roughening, and a water washing process is further included between the micro-etching chemical roughening and the ultrapure water ultrasonic cleaning.

[0014] As an improvement of the present invention, in step S2, the thickness of the first layer of solder resist ink thin coating is 8-12μm, the thickness of the second layer of solder resist ink thickening coating is 10-15μm, and the total ink thickness is controlled to be 18-25μm.

[0015] As an improvement of the present invention, in step S3, the segmented gradient pre-baking is kept at 75°C for 20-30 minutes, and then heated to 85°C and kept at 85°C for 15-25 minutes.

[0016] As an improvement of the present invention, in step S4, for the fine line area on the PCB board, the exposure energy deviation range is reduced so that the exposure energy deviation is controlled within ±5%; for the non-fine line area, conventional exposure energy is used.

[0017] As an improvement of the present invention, in step S5, the developing process adopts segmented pressure spray developing, wherein the segmented pressure spray includes a high-pressure spray section and a low-pressure spray section, and the spray pressure of the high-pressure spray section is higher than that of the low-pressure spray section.

[0018] As an improvement of the present invention, in step S6, the segmented progressive post-curing includes: heating to a first curing temperature in a first temperature zone and holding at that temperature for a first time period in a curing oven, then heating to a second curing temperature in a second temperature zone and holding at that temperature for a second time period, then heating to a third curing temperature in a third temperature zone and holding at that temperature for a third time period, wherein the third curing temperature is higher than the second curing temperature, and the second curing temperature is higher than the first curing temperature; after the holding period, the temperature is slowly reduced to room temperature at a cooling rate of 0.5-2℃ / min.

[0019] As an improvement of the present invention, the first curing temperature is 100-120℃ and the first time period is 20-40min, the second curing temperature is 120-140℃ and the second time period is 20-40min, and the third curing temperature is 145-160℃ and the third time period is 50-70min.

[0020] The present invention also provides a PCB solder resist process system for a PCB solder resist process for improving adhesion and chemical resistance as described in any of the above claims, comprising:

[0021] The composite pretreatment equipment includes an alkaline chemical degreasing tank, a micro-etching roughening tank, an ultrapure water ultrasonic cleaning tank, and a hot air drying device connected in sequence.

[0022] The ink coating equipment includes a semi-automatic screen printing machine and an electrostatic spraying device. The semi-automatic screen printing machine is used to screen print a first thin layer of solder resist ink on the PCB board surface, and the electrostatic spraying device is used to electrostatically spray a second layer of solder resist ink on the PCB board surface.

[0023] The segmented pre-baking oven is used to perform segmented gradient pre-baking on coated PCB boards.

[0024] The CCD vision automatic alignment exposure machine is used to perform zoned exposure processing on the pre-baked PCB board.

[0025] A developing device, comprising a segmented pressure spraying device for segmented pressure spraying development of an exposed PCB board;

[0026] The segmented post-curing oven is used to perform segmented progressive post-curing on the developed PCB board.

[0027] The beneficial effects of this invention are as follows: Compared with the prior art, this invention provides a PCB solder resist process and system that improves adhesion and chemical resistance. It replaces the traditional single physical abrasive pretreatment with a graded composite pretreatment. First, alkaline chemical degreasing thoroughly removes oxidation and oil stains from the board surface. Then, micro-etching chemical roughening uniformly forms a stable microscopic interlocking surface on the copper surface. Combined with ultrasonic cleaning to remove residual impurities, this allows the solder resist ink to fully adhere to the board surface, significantly improving the bonding force between the ink and the board surface. The use of a two-layer thin-coating method ensures that the first thin base coat fully fills the microscopic gaps on the board surface, improving the bonding tightness. The second thicker layer ensures uniform ink thickness, avoiding the problems of incomplete solvent evaporation and uneven thickness caused by a single thick coating, and reducing residual internal stress after curing. By using segmented gradient pre-baking and segmented progressive post-curing, the step-by-step heating method allows the solvent inside the ink to evaporate completely layer by layer, ensuring that the cross-linking and curing reaction proceeds gradually and evenly. Combined with slow cooling to reduce internal stress generation, the solder resist ink cross-links more fully, resulting in a more stable solder resist layer with significantly improved chemical corrosion resistance. This effectively avoids problems such as blistering, peeling, and discoloration of the solder resist layer in subsequent processes, thereby improving the yield and reliability of PCB production. Attached Figure Description

[0028] Figure 1 This is a flowchart of the process steps of the present invention;

[0029] Figure 2 This is an architecture diagram of the PCB solder mask process system in this invention;

[0030] Figure 3 This is a structural connection block diagram of the PCB solder mask process system in this invention. Detailed Implementation

[0031] To more clearly illustrate the present invention, the invention will be further described below with reference to the accompanying drawings.

[0032] In the following description, specific examples are given to provide a more in-depth understanding of the invention. It is obvious that the described embodiments are merely some, not all, of the embodiments of the invention. It should be understood that the specific embodiments described are for illustrative purposes only and are not intended to limit the scope of the invention.

[0033] It should be understood that when the terms “comprising” and / or “including” are used in this specification, they indicate the presence of the said feature, integral, step, operation, element, or component, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components, or combinations thereof.

[0034] Please see Figures 1-3 The present invention provides a PCB solder mask manufacturing process for improving adhesion and chemical resistance, comprising the following steps:

[0035] S1, graded pretreatment of the PCB board surface, including alkaline chemical degreasing, micro-etching chemical roughening, ultrapure water ultrasonic cleaning and hot air drying, to form a micro-interlocking surface on the copper surface of the PCB board.

[0036] S2 uses semi-automatic screen printing and electrostatic spraying to apply solder resist ink to the PCB board in two thin layers. The first layer is a thin base coat of solder resist ink, and the second layer is a thicker, fixed-thickness coating of solder resist ink, controlling the total ink thickness to be 18-25μm.

[0037] S3 involves segmented gradient pre-baking of the coated PCB board, using a stepped heating method. The low-temperature section evaporates the ink solvent, while the high-temperature section performs preliminary curing.

[0038] S4 uses a CCD vision automatic alignment exposure machine to expose the pre-baked PCB board, and adjusts the exposure energy according to the PCB line density in different zones.

[0039] S5, develops the exposed PCB board to remove solder resist ink from the unexposed areas;

[0040] S6 involves segmented progressive curing of the developed PCB board. After being heated and held at a multi-stage temperature gradient in the curing oven, the temperature is slowly lowered to ensure complete cross-linking and curing of the solder resist ink.

[0041] This process creates a nanoscale uneven structure on the copper surface through pretreatment, increasing the mechanical bonding area between the solder resist ink and the copper surface. Combined with two thin-layer coatings, it reduces solvent residue and sagging issues caused by a single thick coating. Furthermore, the gradient temperature control process of segmented gradient pre-baking and segmented progressive post-curing allows the ink solvent to gradually evaporate and the cross-linking reaction to proceed slowly and evenly, avoiding uneven internal stress and incomplete curing caused by rapid heating. At the same time, the zoned adjustment of exposure energy can adapt to the exposure requirements of different density circuits, avoiding overexposure or underexposure. Ultimately, the adhesion between the solder resist layer and the PCB board surface is improved compared to traditional processes, and the chemical resistance properties such as acid and alkali resistance and solvent resistance are also significantly improved, meeting the long-term reliability requirements of high-precision PCBs.

[0042] In this embodiment, in step S1, alkaline chemical degreasing involves immersing and spraying the PCB board surface with an alkaline chemical degreasing agent at 50°C for 1.5-3 minutes. Micro-etching chemical roughening uses a micro-etching agent for 1-2.5 minutes, which helps to uniformly form a micro-interlocking surface on the copper surface, increasing the contact area and adhesion between the ink and the copper surface. Ultrapure water ultrasonic cleaning uses low-pressure ultrapure water combined with ultrasonic cleaning to thoroughly remove residual micro-etching agent and impurity particles from the copper surface. Finally, hot air drying completes the pretreatment process. Furthermore, counter-current water rinsing processes are incorporated between alkaline chemical degreasing and micro-etching chemical roughening, and between micro-etching chemical roughening and ultrapure water ultrasonic cleaning, effectively preventing cross-contamination of chemicals from different processes and ensuring stable pretreatment results.

[0043] In step S2, the first layer is coated with solder resist ink by semi-automatic screen printing, with a thin coating thickness controlled at 8-12μm, which can evenly cover the line gaps on the PCB board surface and complete the base coat; the second layer is coated with solder resist ink by electrostatic spraying to thicken and fix the thickness, with the thickness controlled at 10-15μm, and the final total ink thickness is stably controlled at 18-25μm, which meets the solder resist thickness requirements of different PCB specifications, while avoiding the problems of uneven ink leveling and solvent residue caused by single thick coating.

[0044] In step S3, the segmented gradient pre-baking is specifically as follows: first, keep the temperature at 75℃ for 20-30 minutes to allow the solvent in the ink to evaporate slowly and fully, avoiding rapid evaporation of the solvent and leaving pinhole defects in the ink layer; then, raise the temperature to 85℃ and keep the temperature for 15-25 minutes to allow the ink to complete the initial curing and shaping, which is convenient for the subsequent alignment and exposure process.

[0045] In step S4, after high-precision alignment is completed using a CCD vision automatic alignment exposure machine, the exposure parameters are adjusted according to the line density of different areas of the PCB: for fine line areas on the PCB with line width spacing ≤ [threshold], the exposure energy deviation range is reduced, and the exposure energy deviation is controlled within ±5% to ensure the exposure accuracy of fine line positions and avoid problems such as blurred line edges and ink peeling after development; for non-fine line areas, conventional exposure energy can be used to balance production efficiency and processing quality.

[0046] In step S5, the developing process adopts segmented pressure spray developing, which is divided into a high-pressure spray section and a low-pressure spray section. The spray pressure of the high-pressure spray section is higher than that of the low-pressure spray section: first, the loose and uncured ink in the unexposed area is quickly removed by high-pressure spray, and then the residual ink is removed by low-pressure spray while avoiding impact damage to the exposed and cured solder resist pattern, so as to ensure clean and uniform developing and reduce developing defects.

[0047] In step S6, the specific process of segmented progressive post-curing is as follows: In the segmented post-curing oven, the ink is first heated to 100-120℃ in the first temperature zone and held for 20-40 minutes, then heated to 120-140℃ in the second temperature zone and held for 20-40 minutes, and then heated to 145-160℃ in the third temperature zone and held for 50-70 minutes. The gradient heating allows the ink to gradually undergo cross-linking reaction, avoiding excessive internal stress caused by rapid heating. After all the holding processes are completed, the ink is slowly cooled to room temperature at a cooling rate of 0.5-2℃ / min to further release the internal stress of the ink and avoid cracking and reduced adhesion of the solder resist ink. Finally, the solder resist ink achieves complete and sufficient cross-linking and curing, resulting in a uniform and stable solder resist layer.

[0048] The present invention also provides a PCB solder resist process system for a PCB solder resist process for improving adhesion and chemical resistance as described in any of the above claims, comprising:

[0049] The composite pretreatment equipment includes an alkaline chemical degreasing tank, a micro-etching roughening tank, an ultrapure water ultrasonic cleaning tank, and a hot air drying device connected in sequence.

[0050] The ink coating equipment includes a semi-automatic screen printing machine and an electrostatic spraying device. The semi-automatic screen printing machine is used to screen print a first thin layer of solder resist ink on the PCB board surface, and the electrostatic spraying device is used to electrostatically spray a second layer of solder resist ink on the PCB board surface.

[0051] The segmented pre-baking oven is used to perform segmented gradient pre-baking on coated PCB boards.

[0052] The CCD vision automatic alignment exposure machine is used to perform zoned exposure processing on the pre-baked PCB board.

[0053] A developing device, comprising a segmented pressure spraying device for segmented pressure spraying development of an exposed PCB board;

[0054] The segmented post-curing oven is used to perform segmented progressive post-curing on the developed PCB board.

[0055] The process of this invention, based on a PCB solder mask manufacturing system, is implemented in the following specific steps:

[0056] The first step is to send the PCB board to be processed into the composite pretreatment equipment. First, it is sent to the alkaline chemical degreasing tank to remove oil stains and oxidation impurities from the board surface. Then, it is sent to the micro-etching roughening tank to micro-etch the copper surface to form a uniform and rough micro-concave-convex structure. Next, it is sent to the ultrapure water ultrasonic cleaning tank to remove residual micro-etching agent and copper fragments from the board surface through ultrasonic oscillation. Finally, it is dried by the hot air drying device to obtain a clean surface and uniform roughness of the PCB board to be processed.

[0057] The second step is to send the pre-processed PCB board into the ink coating equipment. First, a thin layer of solder resist ink with a thickness of 8~12μm is evenly printed on the PCB board surface by a semi-automatic screen printing machine, so that the ink can fully fill the gaps between PCB lines. Then, a second layer of solder resist ink with a thickness of 15~20μm is sprayed on the surface of the first layer of ink by an electrostatic spraying device to form a solder resist coating with a total thickness that meets the requirements.

[0058] The third step is to send the coated PCB board into a segmented pre-baking oven and pre-bake it in segments according to a gradient program of 60℃ for 10 minutes, 75℃ for 10 minutes, and 90℃ for 15 minutes. This process gradually evaporates the solvent in the coating and prevents the ink from heating up too quickly and causing pinholes or blistering defects.

[0059] The fourth step is to send the pre-baked PCB board into a CCD vision automatic alignment exposure machine. After the CCD automatically recognizes the alignment marks and completes the precise alignment, the board is exposed in sections according to the design file, so that the solder resist ink that needs to be cured undergoes a photopolymerization reaction.

[0060] The fifth step is to send the exposed PCB board into the developing equipment. Through the segmented pressure spraying device, sodium carbonate solution is first sprayed at a pressure of 0.10~0.12MPa to dissolve and remove excess ink that has not been exposed. Then, ultrapure water is sprayed at a pressure of 0.15~0.18MPa to rinse the board surface of residual developing agents, thus completing the developing process.

[0061] The sixth step is to send the developed PCB board into a segmented post-curing oven and perform segmented progressive post-curing according to the procedure of holding at 100℃ for 20 minutes, 130℃ for 20 minutes, and 150℃ for 30 minutes, so that the solder resist ink can be fully cross-linked and cured, and finally a finished PCB with qualified adhesion and chemical resistance is obtained.

[0062] The advantages of this invention are:

[0063] 1. This invention forms a uniform micro-interlocking structure on the copper surface through graded composite pretreatment, which greatly improves the bonding area and interlocking strength between the solder resist ink and the copper surface, and fundamentally improves the problem of insufficient adhesion of the solder resist layer.

[0064] 2. Two thin-layer coatings are used instead of the traditional single thick coating. The first thin coating can fully fill the gaps in the circuit to ensure uniform coverage, and the second layer is of fixed thickness to meet the total thickness requirements. This avoids the problems of sagging and solvent residue that are easy to occur with single thick coating, and improves the forming quality of the solder resist layer.

[0065] 3. The gradient temperature control process of segmented gradient pre-baking and segmented progressive post-curing allows the ink solvent to gradually evaporate and the cross-linking reaction to proceed evenly. Combined with the final slow cooling to release internal stress, it avoids the problems of uneven stress, incomplete curing, and coating cracking caused by traditional one-time temperature rise curing. This allows the solder resist ink to cross-link more fully and significantly improves its acid and alkali resistance and solvent resistance.

[0066] 4. Exposure parameters are adjusted for different density lines, and exposure energy deviation is strictly controlled in fine line areas to ensure the exposure accuracy of fine lines and avoid problems such as line edge defects and ink peeling after development, thus adapting to the processing requirements of high-precision PCBs.

[0067] The above-disclosed embodiments are merely a few specific examples of the present invention, but the present invention is not limited thereto. Any variations that can be conceived by those skilled in the art should fall within the protection scope of the present invention.

Claims

1. A PCB solder mask manufacturing process that improves adhesion and chemical resistance, characterized in that, Includes the following steps: S1, graded pretreatment of the PCB board surface, including alkaline chemical degreasing, micro-etching chemical roughening, ultrapure water ultrasonic cleaning and hot air drying, to form a micro-interlocking surface on the copper surface of the PCB board. S2 uses semi-automatic screen printing and electrostatic spraying to apply solder resist ink to the PCB board in two thin layers. The first layer is a thin base coat of solder resist ink, and the second layer is a thicker, fixed-thickness coating of solder resist ink, controlling the total ink thickness to be 18-25μm. S3 involves segmented gradient pre-baking of the coated PCB board, using a stepped heating method. The low-temperature section evaporates the ink solvent, while the high-temperature section performs preliminary curing. S4 uses a CCD vision automatic alignment exposure machine to expose the pre-baked PCB board, and adjusts the exposure energy according to the PCB line density in different zones. S5, develops the exposed PCB board to remove solder resist ink from the unexposed areas; S6 involves segmented progressive curing of the developed PCB board. After being heated and held at a multi-stage temperature gradient in the curing oven, the temperature is slowly lowered to ensure complete cross-linking and curing of the solder resist ink.

2. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 1, characterized in that, In step S1, the alkaline chemical degreasing uses an alkaline chemical degreasing agent to soak and spray the PCB board surface at 50°C for 1.5-3 minutes; the micro-etching chemical roughening uses a micro-etching agent to treat for 1-2.5 minutes to form a micro-interlocking surface on the copper surface; the ultrapure water ultrasonic cleaning uses low-pressure ultrapure water in conjunction with ultrasonic cleaning, and finally is dried with hot air.

3. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 2, characterized in that, In step S1, a water washing process is further included between the alkaline chemical degreasing and the micro-etching chemical roughening, and a water washing process is further included between the micro-etching chemical roughening and the ultrapure water ultrasonic cleaning.

4. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 1, characterized in that, In step S2, the thickness of the first layer of solder resist ink is 8-12 μm, the thickness of the second layer of solder resist ink is 10-15 μm, and the total ink thickness is controlled to be 18-25 μm.

5. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 1, characterized in that, In step S3, the segmented gradient pre-baking is carried out at 75°C for 20-30 minutes, and then heated to 85°C for 15-25 minutes.

6. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 1, characterized in that, In step S4, for fine circuit areas on the PCB, the exposure energy deviation range is reduced to keep the exposure energy deviation within ±5%; for non-fine circuit areas, conventional exposure energy is used.

7. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 1, characterized in that, In step S5, the developing process employs segmented pressure spray developing, which includes a high-pressure spray section and a low-pressure spray section, wherein the spray pressure of the high-pressure spray section is higher than that of the low-pressure spray section.

8. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 1, characterized in that, In step S6, the segmented progressive post-curing includes: heating to a first curing temperature in a curing oven via a first temperature zone and holding at that temperature for a first time period; then heating to a second curing temperature in a second temperature zone and holding at that temperature for a second time period; then heating to a third curing temperature in a third temperature zone and holding at that temperature for a third time period, wherein the third curing temperature is higher than the second curing temperature, and the second curing temperature is higher than the first curing temperature; after the holding period, the temperature is slowly reduced to room temperature at a cooling rate of 0.5-2℃ / min.

9. The PCB solder mask manufacturing process for improving adhesion and chemical resistance according to claim 8, characterized in that, The first curing temperature is 100-120℃ and the first time period is 20-40min; the second curing temperature is 120-140℃ and the second time period is 20-40min; and the third curing temperature is 145-160℃ and the third time period is 50-70min.

10. A PCB solder resist process system for implementing the PCB solder resist process of any one of claims 1-9 to improve adhesion and chemical resistance, characterized in that, include: The composite pretreatment equipment includes an alkaline chemical degreasing tank, a micro-etching roughening tank, an ultrapure water ultrasonic cleaning tank, and a hot air drying device connected in sequence. The ink coating equipment includes a semi-automatic screen printing machine and an electrostatic spraying device. The semi-automatic screen printing machine is used to screen print a first thin layer of solder resist ink on the PCB board surface, and the electrostatic spraying device is used to electrostatically spray a second layer of solder resist ink on the PCB board surface. The segmented pre-baking oven is used to perform segmented gradient pre-baking on coated PCB boards. The CCD vision automatic alignment exposure machine is used to perform zoned exposure processing on the pre-baked PCB board. A developing device, comprising a segmented pressure spraying device for segmented pressure spraying development of an exposed PCB board; The segmented post-curing oven is used to perform segmented progressive post-curing on the developed PCB board.