A method for manufacturing a semiconductor structure
By forming a multilayer sidewall structure on the surface of the bit line structure and selectively oxidizing to remove the layer with the lowest mass density, the problem of sidewall voids or pinholes in the bit line is solved, thereby improving the density and reliability of the semiconductor structure.
Patent Information
- Application Number
- CN202611327695.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-20
AI Technical Summary
In dynamic random access memory with recessed gate structure, voids or pinholes are prone to appear on the sidewalls of the bit lines, affecting device density and reliability.
A first sidewall, a second sidewall, and a third sidewall are formed on the surface of the bitline structure in a sequentially stacked manner from the inside out. The second sidewall, which has the lowest mass density, is removed by selective oxidation treatment, while the first sidewall on the inner side is retained, thereby improving the density of the sidewall structure.
This effectively avoids voids or pinholes in the sidewall structure, improving the performance and reliability of the semiconductor structure.
Smart Images

Figure CN123145901A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor technology, and in particular to a method for fabricating a semiconductor structure. Background Technology
[0002] With the trend towards miniaturization in various electronic products, the design of semiconductor devices must also meet the requirements of high integration and high density. For Dynamic Random Access Memory (DRAM) with a recessed gate structure, it can achieve a longer carrier channel length within the same semiconductor substrate, reducing leakage current caused by capacitor structures. Therefore, under the current mainstream development trend, it has gradually replaced DRAM with only a planar gate structure. Generally, DRAM with a recessed gate structure consists of a large number of memory cells arranged in an array to store information. Each memory cell can be composed of transistor components and capacitor components connected in series to receive voltage information from the word line (WL) and bit line (BL). To improve device density, the increasingly thin sidewall layers on the bit line sidewalls are prone to voids or pinholes. Summary of the Invention
[0003] One objective of this application is to provide a method for fabricating a semiconductor structure to improve the mass density of the sidewall structure, avoid the formation of voids or pinholes inside, and thereby improve the performance and reliability of the semiconductor structure.
[0004] To achieve the above objectives, one embodiment of this application provides a method for fabricating a semiconductor structure, comprising:
[0005] Provide substrate;
[0006] Multiple bit line structures that are horizontally spaced apart are formed on the substrate;
[0007] A sidewall structure is formed on the surface of the bit line structure. The sidewall structure includes a first sidewall, a second sidewall, and a third sidewall that are stacked sequentially from the inside to the outside and have a first oxidation rate, a second oxidation rate, and a third oxidation rate, respectively. The first oxidation rate and the third oxidation rate are less than the second oxidation rate. The first sidewall, the second sidewall, and the third sidewall are made of the same material.
[0008] The second sidewall of the sidewall structure is selectively oxidized;
[0009] Remove the third sidewall and the oxidized second sidewall of the sidewall structure.
[0010] Optionally, the sidewall structure comprises silicon nitride.
[0011] Optionally, the Si / N atomic ratio of the first sidewall and the third sidewall is smaller than the Si / N atomic ratio of the second sidewall.
[0012] Optionally, the porosity of the first sidewall and the third sidewall is less than that of the second sidewall.
[0013] Optionally, the mass density of the first sidewall and the third sidewall is greater than the mass density of the second sidewall.
[0014] Optionally, the hydrogen content of the first sidewall and the third sidewall is less than the hydrogen content of the second sidewall.
[0015] Optionally, the dielectric constants of the first sidewall and the third sidewall are greater than the dielectric constant of the second sidewall.
[0016] Optionally, the step of forming the sidewall structure includes:
[0017] Provides a mixture of silicon source gas and nitrogen source gas;
[0018] The gas flow ratio of the silicon source gas and the nitrogen source gas is adjusted during different reaction time periods to sequentially form the first sidewall, the second sidewall, and the third sidewall on the surface of the bit line structure.
[0019] Optionally, the gas flow rate ratio forming the second sidewall is less than the gas flow rate ratio forming the first sidewall and the third sidewall.
[0020] Optionally, the step of forming the sidewall structure includes:
[0021] A mixture of silicon source gas and nitrogen source gas is provided to form a silicon nitride layer on the surface of the bit line structure;
[0022] Ion implantation is performed on the middle region of the silicon nitride layer to form the second sidewall of the sidewall structure;
[0023] The portion of the silicon nitride layer that is in direct contact with the bit line structure is designated as the first sidewall, and the portion of the silicon nitride layer that is in direct contact with the second sidewall along a direction away from the bit line structure is designated as the third sidewall.
[0024] Optionally, the first sidewall has a first thickness, the second sidewall has a second thickness, and the third sidewall has a third thickness, wherein the first thickness is less than the second thickness, and the second thickness is less than the third thickness.
[0025] To achieve the above objectives, another embodiment of this application provides a method for fabricating a semiconductor structure, comprising:
[0026] Provide substrate;
[0027] Multiple bit line structures that are horizontally spaced apart are formed on the substrate;
[0028] Provides a mixture of silicon source gas and nitrogen source gas;
[0029] The gas flow rate ratio of the silicon source gas and the nitrogen source gas is adjusted during different reaction time periods to form a sidewall structure on the surface of the bit line structure, comprising a first sidewall, a second sidewall, and a third sidewall stacked sequentially from the inside out; the first sidewall has a first oxidation rate, the second sidewall has a second oxidation rate, and the third sidewall has a third oxidation rate, wherein the first oxidation rate and the third oxidation rate are less than the second oxidation rate, and the first sidewall, the second sidewall, and the third sidewall are made of the same material;
[0030] The second sidewall of the sidewall structure is selectively oxidized;
[0031] Remove the third sidewall and the oxidized second sidewall of the sidewall structure.
[0032] Optionally, the gas flow rate ratio forming the second sidewall is less than the gas flow rate ratio forming the first sidewall and the third sidewall.
[0033] Optionally, the sidewall structure comprises silicon nitride.
[0034] Optionally, the Si / N atomic ratio of the first sidewall and the third sidewall is smaller than the Si / N atomic ratio of the second sidewall.
[0035] Optionally, the porosity of the first sidewall and the third sidewall is less than that of the second sidewall.
[0036] Optionally, the mass density of the first sidewall and the third sidewall is greater than the mass density of the second sidewall.
[0037] Optionally, the hydrogen content of the first sidewall and the third sidewall is less than the hydrogen content of the second sidewall.
[0038] Optionally, the dielectric constants of the first sidewall and the third sidewall are greater than the dielectric constant of the second sidewall.
[0039] As described above, the fabrication method in this application includes forming a bit line structure on a substrate; forming a sidewall structure on the surface of the bit line structure, wherein the sidewall structure includes a first sidewall, a second sidewall, and a third sidewall stacked sequentially from the inside to the outside; selectively oxidizing the second sidewall of the sidewall structure; and removing the third sidewall and the oxidized second sidewall of the sidewall structure. Because this application embodiment performs additional processing on the middle portion during the formation of a thicker silicon nitride layer, the oxidation rate of the silicon nitride layer in the middle portion (i.e., the second sidewall) is greater than that of the remaining portions. Thus, during the oxidation process of the sidewall structure, the second sidewall is more easily selectively oxidized. This oxidation process alters the characteristics of the second sidewall, which has the lowest mass density in the sidewall structure, making the etch selectivity of the second sidewall different from the other two layers. Subsequently, the outer silicon nitride layer is removed, leaving only the innermost silicon nitride layer, thereby obtaining a thin silicon nitride layer without voids, improving the performance and reliability of the semiconductor structure. Attached Figure Description
[0040] The accompanying drawings provide a more in-depth understanding of embodiments of this application and are incorporated herein by reference as a whole. These drawings and descriptions are used to illustrate the principles of some embodiments. It should be noted that all drawings are schematic diagrams and are for illustrative and drawing convenience, and relative sizes and proportions have been adjusted. The same symbols represent corresponding or similar features in different embodiments.
[0041] Figure 1 This is a flowchart illustrating the method for fabricating a semiconductor structure in an embodiment of this application.
[0042] Figure 2 This is a partial cross-sectional view of the semiconductor structure after the bit line structure is formed in the embodiments of this application;
[0043] Figure 3 This is a partial cross-sectional view of the semiconductor structure after the sidewall structure is formed in the embodiments of this application;
[0044] Figure 4 for Figure 2 A partially enlarged view of the semiconductor structure shown;
[0045] Figure 5 This is a partial cross-sectional view of the semiconductor structure after selectively processing the sidewall structure in an embodiment of this application;
[0046] The attached figures are labeled as follows:
[0047] 100 - Substrate, D1 - First direction, D2 - Second direction, 101 - Shallow trench isolation, 110 - Insulating layer, OP - Bit line plug hole, 121a - Bit line plug, 120 - Bit line structure, 121 - Semiconductor layer, 122 - Barrier layer, 123 - Metal layer, 124 - Cap layer, 130 - Sidewall structure, 131 - First sidewall, 132 - Second sidewall, 133 - Third sidewall, H1 - First thickness, H2 - Second thickness, H3 - Third thickness.
[0048] In the accompanying drawings, the same parts are referred to by the same reference numerals, and the drawings are not drawn to scale. Detailed Implementation
[0049] To enable those skilled in the art to further understand this application, preferred embodiments of the application are described below, along with accompanying drawings, to explain in detail the composition and desired effects of the application. It should be understood that the following embodiments can be modified by substituting, recombining, or mixing features from several different embodiments to achieve other embodiments without departing from the spirit of this application.
[0050] Please see Figure 1 , Figure 1 This is a method for fabricating a semiconductor structure in the first embodiment of this application.
[0051] like Figure 1 As shown, the method for fabricating the semiconductor structure in the first embodiment of this application includes:
[0052] Step S101: Provide a substrate;
[0053] Step S102: A plurality of bit line structures that are horizontally separated from each other are formed on the substrate;
[0054] Step S103: A sidewall structure is formed on the surface of the bit line structure. The sidewall structure includes a first sidewall, a second sidewall, and a third sidewall that are stacked sequentially from the inside to the outside and have a first oxidation rate, a second oxidation rate, and a third oxidation rate, respectively. The first oxidation rate and the third oxidation rate are less than the second oxidation rate. The first sidewall, the second sidewall, and the third sidewall are made of the same material.
[0055] Step S104: Selective oxidation of the second sidewall of the sidewall structure;
[0056] Step S105: Remove the third sidewall and the oxidized second sidewall of the sidewall structure.
[0057] To enable those skilled in the art to easily understand the method for fabricating the semiconductor structure in the embodiments of this application, the following will further explain the method for fabricating the semiconductor structure proposed in this application with reference to various structural schematic diagrams during the fabrication process. Among them, Figures 2-5 This is a schematic diagram of the fabrication process of the semiconductor structure provided in the first embodiment of this application.
[0058] For ease of understanding, the horizontal and vertical directions are defined below, and the X and Y directions are defined in the accompanying drawings. The horizontal direction is parallel to the surface of the substrate 100 and corresponds to the X direction; the vertical direction is perpendicular to the surface of the substrate 100 and corresponds to the Y direction. Furthermore, the horizontal X direction and the vertical Y direction are perpendicular to each other.
[0059] Please see Figure 2 , Figure 2 This is a partial cross-sectional view of the semiconductor structure after the bit line structure is formed in the first embodiment of this application; as shown... Figure 2 As shown, in performing step S101, a substrate 100 is first provided, and then multiple trenches (not shown) are formed in the substrate 100 by etching. One or more layers of insulating / dielectric material are then filled into the trenches to form multiple shallow trench isolations 101 (STIs) within the substrate 100, and an active area (not shown) defined by the multiple shallow trench isolations 101. For example, the shallow trench isolation 101 may be elongated with its long axis extending in the vertical direction Y. In one embodiment, the substrate 100 is any suitable substrate material known in the art, such as a silicon substrate, a silicon-containing substrate (e.g., SiC, SiGe), or a silicon-on-insulator substrate, or a substrate made of other suitable materials, but is not limited thereto. Shallow trench isolation 101 may include a single layer or multiple layers of insulating / dielectric materials. Suitable dielectric materials may include, for example, silicon oxide (SiO2), silicon nitride (SiN), silicon oxynitride (SiON), silicon carbide (SiCN), nitrogen-doped silicon carbide (NDC), low-k dielectric materials such as fluorinated silica glass (FSG), silicon carbide oxide (SiCOH), spin-on glass, porous low-k dielectric material, organic polymer dielectric materials, or combinations of the above materials, but are not limited thereto.
[0060] Continue reading Figure 2Perform the above step S102, using at least one of the deposition processes such as physical vapor deposition, chemical vapor deposition, and atomic layer deposition to form an insulating layer 110 on the surface of the substrate 100, and etch the insulating layer 110 and a portion of the substrate 100 along the vertical direction Y, so as to form a plurality of bit line plug holes OP in the insulating layer 110 and the substrate 100. The bit line plug holes OP are the corresponding positions of the bit line plugs 121a formed later in the substrate 100. Next, a material layer (e.g., polycrystalline silicon) for bit line plug 121a can be formed within the bit line plug hole OP using the above deposition process. Then, a bit line material layer consisting of a semiconductor layer 121, a barrier layer 122, a metal layer 123, and a capping layer 124, stacked sequentially from bottom to top, is formed on most of the substrate 100 and on the material layer of the bit line plug 121a. A portion of the bit line material layer is removed downward along the vertical direction Y to form a plurality of bit line structures 120 extending in the vertical direction Y and spaced apart from each other in the horizontal direction X on the substrate 100. In one embodiment, the insulating layer 110 may include a single layer or multiple layers of insulating / dielectric materials. Suitable dielectric materials may include, for example, silicon oxide (SiO2), silicon nitride (SiN), etc., but are not limited thereto. The material of the semiconductor layer 121 may include crystalline silicon, polycrystalline silicon, amorphous silicon, doped silicon, silicon germanium (SiGe), or other suitable semiconductor materials, but is not limited thereto. The barrier layer 122 may be made of metal, metal silicide, or metal nitride, such as titanium (Ti), titanium nitride (TiN), tungsten silicide (WSi), cobalt silicide (CoSi), or tungsten nitride (WN), but is not limited thereto. The metal layer 123 may be made of tungsten (W), copper (Cu), aluminum (Al), titanium (Ti), tantalum (Ta), or compounds, alloys, and / or composite layers of the aforementioned metal materials, but is not limited thereto. The capping layer 124 may be made of a dielectric material, such as silicon oxide (SiO2), silicon nitride (SiN), silicon oxynitride (SiON), silicon carbide nitride (SiCN), or combinations thereof, but is not limited thereto. Preferably, the semiconductor layer 121 is made of polycrystalline silicon, the barrier layer 122 is made of cobalt silicide (CoSi), the metal layer 123 is made of tungsten (W), and the capping layer 124 is made of silicon nitride (SiN).
[0061] Please see Figure 3 and Figure 4 , Figure 3 This is a partial cross-sectional view of the semiconductor structure after the sidewall structure is formed in the embodiments of this application; Figure 4 for Figure 2 A partially enlarged view of the semiconductor structure shown. Figure 3As shown, by performing step S103 above, a sidewall structure 130 is formed on the surface of the bit line structure 120, the insulating layer 110 exposed on both sides of the bit line structure 120, and the bit line plug hole OP using the chemical vapor deposition process in the above deposition process.
[0062] like Figure 4 As shown, the sidewall structure 130 includes a first sidewall 131, a second sidewall 132, and a third sidewall 133 stacked sequentially from the inside out. In this embodiment, the sidewall structure 130 is made of silicon nitride; therefore, the first sidewall 131, the second sidewall 132, and the third sidewall 133 are all made of the same material, and are all silicon nitride. Furthermore, the first oxidation rate of the first sidewall 131 and the third oxidation rate of the third sidewall 133 are less than the second oxidation rate of the second sidewall 132. The oxidation rate of the sidewall structure may depend on the Si / N atomic ratio, porosity, mass density, hydrogen content, or dielectric constant, but is not limited thereto. In one embodiment, the Si / N atomic ratio of the first sidewall 131 and the third sidewall 133 is less than the Si / N atomic ratio of the second sidewall 132. In another embodiment, the porosity of the first sidewall 131 and the third sidewall 133 is less than the porosity of the second sidewall 132, such that the mass density of the first sidewall 131 and the third sidewall 133 is greater than the mass density of the second sidewall. In another embodiment, the hydrogen content of the first sidewall 131 and the third sidewall 133 is less than the hydrogen content of the second sidewall 132. In another embodiment, the dielectric constant of the first sidewall 131 and the third sidewall 133 is greater than the dielectric constant of the second sidewall 132.
[0063] In this embodiment, the specific process of forming the sidewall structure 130 including the first sidewall 131 to the third sidewall 133 using chemical vapor deposition can be as follows: a mixture of silicon source gas and nitrogen source gas is introduced into the process chamber carrying the substrate 100, and then the gas flow ratio of silicon source gas and nitrogen source gas is adjusted in different reaction time periods; for example, the duration of forming the sidewall structure 130 is roughly divided into three time periods, namely the first to the third time periods, and then the gas flow ratio of silicon source gas and nitrogen source gas introduced into the process chamber in the first time period and the third time period is the same, and the gas flow ratio of silicon source gas and nitrogen source gas introduced into the process chamber in the second time period is increased. The gas flow rate ratio of the nitrogen source gas (increasing the silicon atom content in the second time period), that is, the gas flow rate ratio of the silicon source gas to the nitrogen source gas in the second time period is greater than the gas flow rate ratio of the silicon source gas to the nitrogen source gas in the first time period and the third time period; thus, the silicon content in the silicon nitride in the second sidewall 132 formed in the second time period increases, thereby making the porosity, Si / N atomic ratio or hydrogen content of the first sidewall 131 formed in the first time period and the third sidewall 132 formed in the third time period less than the porosity, Si / N atomic ratio or hydrogen content of the second sidewall 132 formed in the second time period.
[0064] In an embodiment, the porosity and hydrogen content may depend on the Si / N atomic ratio. The closer the Si / N ratio is to 3 / 4 (i.e., the standard stoichiometric ratio of silicon nitride), the lower the porosity and hydrogen content, and the smaller the oxidation rate. In another embodiment, the Si / N atomic ratio of the first sidewall 131 and the Si / N atomic ratio of the third sidewall 133 are closer to 3 / 4 than the Si / N atomic ratio of the second sidewall 132.
[0065] Exemplarily, after the sidewall structure 130 is formed, different positions of the sidewall structure 130 may be subjected to area scanning or line scanning by electron beam laser, for example, performing area scanning or line scanning on corresponding positions of the first sidewall 131, the second sidewall 132, and the third sidewall 133, and exciting the silicon nitride at the first sidewall 131, the second sidewall 132, and the third sidewall 133 to generate X-rays, then collecting and analyzing the X-rays generated at different positions, so as to obtain the N / Si atomic ratio of the first sidewall 131 to the third sidewall 133; in other embodiments, other detection methods such as an ellipsometer, a profilometer and the like may also be used to determine the N / Si atomic ratio of the first sidewall 131 to the third sidewall 133. Similarly, a transmission electron microscope (TEM), X-ray reflectivity (XRR), Rutherford backscattering spectrometry (RBS), ellipsometer or profilometer may also be used to further determine the porosity, mass density and hydrogen content of the first sidewall 131 to the third sidewall 133.
[0066] Further, since the hydrogen content in the second sidewall 132 is higher than that in the first sidewall 131 and the third sidewall 133, the silicon nitride material of the second sidewall 132 is relatively loose, resulting in a significantly increased porosity and a decreased mass density, and the increase of the porosity in the film layer will inevitably cause a decrease in the dielectric constant. Therefore, the dielectric constant of the second sidewall 132 in the embodiment of the present application is smaller than the dielectric constants of the first sidewall 131 and the third sidewall 133. In addition, in the embodiment of the present application, the durations of the first to third time periods may also be adjusted to change the thicknesses of the first sidewall 131, the second sidewall 132 and the third sidewall 133. For example, the first sidewall 131 has a first thickness H1, the second sidewall 132 has a second thickness H2, and the third sidewall 133 has a third thickness H3, then the first thickness H1 is smaller than the second thickness H2, and the second thickness H2 is smaller than the third thickness H3, that is, H1<H2<H3.
[0067] Continuing to refer to Figure 4In step S104, the second sidewall 132 in the sidewall structure 130 is selectively oxidized to oxidize the silicon nitride material of the second sidewall 132, which has low mass density and high porosity, into silicon oxide material. The high mass density and low porosity of silicon oxide material are then used to improve the density of the sidewall structure 130 and avoid voids or pinholes in some areas of the sidewall structure 130, such as the area where the second sidewall 132 is located. This improves the efficiency and reliability of the sidewall structure 130 that is finally covered on the sidewall of the bit line structure 120.
[0068] Please see Figure 5 , Figure 5 This is a partial cross-sectional view of the semiconductor structure after selectively processing the sidewall structure in the first embodiment of this application. (See image below.) Figure 5 As shown, in step S105, the third sidewall 133 and the oxidized second sidewall 132 in the sidewall structure 130 are removed by using an etching process such as dry etching or wet etching, that is, only the first sidewall 131 with a thickness of the first thickness H1 remains / covers the surface of the bit line structure 120.
[0069] Those skilled in the art to which this application pertains will readily understand that, to meet actual product requirements, the method for fabricating the semiconductor structure of this application may have other forms and is not limited to those described above. Further embodiments or variations of the method for fabricating the semiconductor structure of this application will be described below. For the sake of simplicity, identical components in the various embodiments of this application are designated with the same reference numerals to facilitate comparison between embodiments.
[0070] Continue reading Figures 2-5 , Figures 2-5 This is a schematic diagram of the fabrication process of the semiconductor structure provided in the second embodiment of this application.
[0071] like Figures 2-5 As shown, the method for fabricating the semiconductor structure in the second embodiment of this application is largely the same as the method for fabricating the semiconductor structure in the first embodiment described above. For example, a substrate 100 is first provided, and multiple shallow trench isolations 101 are formed within the substrate 100, as well as an active region (not shown) defined by the multiple shallow trench isolations 101; then the bit line structure 120 is formed, and so on, which will not be described again here. The main difference between the method for fabricating the semiconductor structure in the second embodiment of this application and the method for fabricating the first embodiment described above is that a silicon nitride layer 130 is first formed on the surface of the bit line structure 120 using a chemical vapor deposition process, such as... Figure 3As shown; at this time, the silicon nitride layer 130 does not have a first sidewall, a second sidewall, and a third sidewall, that is, the film material and its properties at different positions of the silicon nitride layer 130 are uniform; then, ion implantation is performed on the middle part of the silicon nitride layer 130 (corresponding to the position of the first sidewall 132). In this way, the Si-N chemical bonds in the middle part of the silicon nitride layer 130 will be broken during the ion implantation process, thereby reducing the mass density and increasing the porosity of the middle part of the silicon nitride layer 130, thus forming the second sidewall 132 of the sidewall structure in the first embodiment; then, the part of the silicon nitride layer 130 that is in direct contact with the bit line structure 120 is taken as the first sidewall 131 of the sidewall structure in the first embodiment, and the part of the silicon nitride layer 130 that is in direct contact with the second sidewall 132 in the direction away from the bit line structure 120 is taken as the third sidewall 133 of the sidewall structure in the first embodiment.
[0072] Therefore, the main difference between the second embodiment of this application and the aforementioned first embodiment is that the process of forming the first sidewall 131 to the third sidewall 133 in the sidewall structure is different. That is, the first embodiment is achieved by adjusting the gas flow ratio of silicon source gas and nitrogen source gas (mixed gas of silicon source gas and nitrogen source gas) in the chemical vapor deposition process during different reaction time periods, while the second embodiment is achieved by using ion implantation to destroy / break the chemical bonds in the film material.
[0073] In summary, the fabrication method in this application includes forming a bit line structure on a substrate; forming a sidewall structure on the surface of the bit line structure, wherein the sidewall structure includes a first sidewall, a second sidewall, and a third sidewall stacked sequentially from the inside out; selectively oxidizing the second sidewall of the sidewall structure; and removing the third sidewall and the oxidized second sidewall of the sidewall structure. Because this application performs additional processing on the middle portion during the formation of a thicker silicon nitride layer, the oxidation rate of the silicon nitride layer in the middle portion (i.e., the second sidewall) is greater than that of the remaining portions. Therefore, during the oxidation process of the sidewall structure, the second sidewall is more easily selectively oxidized. This oxidation process alters the characteristics of the second sidewall, which has the lowest mass density in the sidewall structure, making the etch selectivity of the second sidewall different from the other two layers. Subsequently, the outer silicon nitride layer is removed, leaving only the innermost silicon nitride layer, resulting in a thin silicon nitride layer without voids, thus improving the performance and reliability of the semiconductor structure.
[0074] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for fabricating a semiconductor structure, characterized in that, include: Provide substrate; Multiple bit line structures that are horizontally spaced apart are formed on the substrate; A sidewall structure is formed on the surface of the bit line structure. The sidewall structure includes a first sidewall, a second sidewall, and a third sidewall that are stacked sequentially from the inside to the outside and have a first oxidation rate, a second oxidation rate, and a third oxidation rate, respectively. The first oxidation rate and the third oxidation rate are less than the second oxidation rate. The first sidewall, the second sidewall, and the third sidewall are made of the same material. The second sidewall of the sidewall structure is selectively oxidized; Remove the third sidewall and the oxidized second sidewall of the sidewall structure.
2. The manufacturing method as described in claim 1, characterized in that, The sidewall structure comprises silicon nitride.
3. The manufacturing method as described in claim 2, characterized in that, The Si / N atomic ratio of the first sidewall and the third sidewall is less than that of the second sidewall.
4. The manufacturing method as described in claim 2, characterized in that, The porosity of the first sidewall and the third sidewall is less than that of the second sidewall.
5. The manufacturing method as described in claim 2, characterized in that, The mass density of the first sidewall and the third sidewall is greater than the mass density of the second sidewall.
6. The manufacturing method as described in claim 2, characterized in that, The hydrogen content of the first sidewall and the third sidewall is less than that of the second sidewall.
7. The manufacturing method as described in claim 2, characterized in that, The dielectric constants of the first sidewall and the third sidewall are greater than the dielectric constant of the second sidewall.
8. The manufacturing method as described in claim 2, characterized in that, The steps of forming the sidewall structure include: Provides a mixture of silicon source gas and nitrogen source gas; The gas flow ratio of the silicon source gas and the nitrogen source gas is adjusted during different reaction time periods to sequentially form the first sidewall, the second sidewall, and the third sidewall on the surface of the bit line structure.
9. The manufacturing method as described in claim 8, characterized in that, The gas flow rate ratio forming the second sidewall is less than the gas flow rate ratio forming the first sidewall and the third sidewall.
10. The manufacturing method as described in claim 2, characterized in that, The steps of forming the sidewall structure include: A mixture of silicon source gas and nitrogen source gas is provided to form a silicon nitride layer on the surface of the bit line structure; Ion implantation is performed on the middle region of the silicon nitride layer to form the second sidewall of the sidewall structure; The portion of the silicon nitride layer that is in direct contact with the bit line structure is designated as the first sidewall, and the portion of the silicon nitride layer that is in direct contact with the second sidewall along a direction away from the bit line structure is designated as the third sidewall.
11. The manufacturing method as described in claim 1, characterized in that, The first sidewall has a first thickness, the second sidewall has a second thickness, and the third sidewall has a third thickness, wherein the first thickness is less than the second thickness, and the second thickness is less than the third thickness.
12. A method for fabricating a semiconductor structure, characterized in that, include: Provide substrate; Multiple bit line structures that are horizontally spaced apart are formed on the substrate; Provides a mixture of silicon source gas and nitrogen source gas; The gas flow rate ratio of the silicon source gas and the nitrogen source gas is adjusted during different reaction time periods to form a sidewall structure on the surface of the bit line structure, comprising a first sidewall, a second sidewall, and a third sidewall stacked sequentially from the inside out; the first sidewall has a first oxidation rate, the second sidewall has a second oxidation rate, and the third sidewall has a third oxidation rate, wherein the first oxidation rate and the third oxidation rate are less than the second oxidation rate, and the first sidewall, the second sidewall, and the third sidewall are made of the same material; The second sidewall of the sidewall structure is selectively oxidized; Remove the third sidewall and the oxidized second sidewall of the sidewall structure.
13. The manufacturing method as described in claim 12, characterized in that, The gas flow rate ratio forming the second sidewall is less than the gas flow rate ratio forming the first sidewall and the third sidewall.
14. The manufacturing method as described in claim 12, characterized in that, The sidewall structure comprises silicon nitride.
15. The manufacturing method as described in claim 14, characterized in that, The Si / N atomic ratio of the first sidewall and the third sidewall is less than that of the second sidewall.
16. The manufacturing method as described in claim 14, characterized in that, The porosity of the first sidewall and the third sidewall is less than that of the second sidewall.
17. The manufacturing method as described in claim 14, characterized in that, The mass density of the first sidewall and the third sidewall is greater than the mass density of the second sidewall.
18. The manufacturing method as described in claim 14, characterized in that, The hydrogen content of the first sidewall and the third sidewall is less than that of the second sidewall.
19. The manufacturing method as described in claim 14, characterized in that, The dielectric constants of the first sidewall and the third sidewall are greater than the dielectric constant of the second sidewall.