Solar cell and method of manufacturing the same
By introducing a thin-layer doped amorphous silicon oxide layer into silicon-based heterojunction solar cells and depositing a doped microcrystalline silicon layer under high power and high pressure, the problem of balancing film deposition rate and cell performance was solved, thereby improving cell yield and efficiency.
Patent Information
- Application Number
- CN202510602272.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-12
- Publication Date
- 2026-11-20
AI Technical Summary
In the mass production of silicon-based heterojunction solar cells, existing technologies struggle to increase the film deposition rate while maintaining cell performance, thus limiting the increase in cell yield.
An intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer are sequentially deposited on the surface of a silicon substrate. The thickness of the doped amorphous silicon oxide layer is less than 3 nm. The deposition is carried out under high power and high pressure, combined with a high silane hydrogen dilution ratio to reduce ion bombardment damage.
While maintaining battery performance, the film deposition time is significantly reduced, increasing battery production output on mass production lines and improving battery photoelectric efficiency.
Smart Images

Figure CN123145991A_ABST
Abstract
Description
Technical Field
[0001] This invention relates primarily to the field of solar energy technology, and more particularly to a solar cell and its preparation method. Background Technology
[0002] A solar cell (or photovoltaic cell) is a component that converts solar energy into electrical energy. When sunlight shines on the semiconductor material on the surface of a solar cell, the semiconductor material absorbs the energy of photons, allowing electrons in the semiconductor atoms to gain enough energy to be excited from their covalent bonds, forming free electrons. These free electrons separate under the influence of the electric field of the PN junction, forming a current that can drive a load.
[0003] Solar cells come in many varieties and can be classified into various types based on the materials used, structures, and working principles. Among them, silicon-based heterojunction solar cells have technological advantages such as good low-light performance, high cell efficiency, fewer production processes, and high bifaciality, attracting much attention from the research and industry sectors since their introduction. For example, by optimizing the front structure of silicon-based heterojunction solar cells, the front side, which is generally the light-facing side, is N-type doped (also known as the N-side). In particular, the N-side electron transport layer, after upgrading N-type doped amorphous silicon to N-type doped microcrystalline silicon or doped microcrystalline silicon oxide, has achieved a laboratory R&D efficiency of 26.81%, and some companies have already begun GW-level mass production of silicon-based heterojunction solar cells, with mass production efficiencies exceeding 25.5%.
[0004] In the mass production of heterojunction solar cells, a large silane hydrogen dilution ratio is typically required to deposit the doped microcrystalline layer. This significantly reduces the deposition rate of the thin film, hindering the increase in cell yield on the mass production line. Conventional methods to improve the thin film deposition rate include increasing the deposition power and decreasing the hydrogen dilution ratio. However, increasing the deposition power may lead to increased bombardment damage during deposition, resulting in a decrease in the cell's open-circuit voltage. Conversely, decreasing the hydrogen dilution ratio may lead to a decrease in the crystallinity of the film layer, thereby increasing the cell's series resistance. These deposition methods struggle to simultaneously improve the film deposition rate without compromising cell performance. Summary of the Invention
[0005] The technical problem to be solved by the present invention is to provide a solar cell and a method for its preparation, which reduces the film deposition time while maintaining the performance of the cell, thereby improving the cell yield on the mass production line.
[0006] To address the aforementioned technical problems, in a first aspect, the present invention provides a solar cell comprising: a silicon substrate; wherein a surface of the silicon substrate has, sequentially along a direction away from the silicon substrate, an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer, wherein the thickness of the doped amorphous silicon oxide layer is less than 3 nm, and the doped amorphous silicon oxide layer, the doped microcrystalline silicon oxide layer, and the doped microcrystalline silicon layer have the same doping conductivity type.
[0007] Optionally, the intrinsic passivation layer is an intrinsic amorphous silicon layer or an intrinsic amorphous silicon oxide layer.
[0008] Optionally, the doped microcrystalline silicon oxide layer includes a seed layer and a main layer sequentially connected along a direction away from the silicon substrate, wherein the crystallinity of the seed layer is higher than that of the main layer, and the doping concentration of the doped microcrystalline silicon layer is higher than that of the main layer.
[0009] Optionally, the surface of the silicon substrate is the front side of the silicon substrate, wherein the thickness of the intrinsic passivation layer is 5nm to 8nm, the thickness of the seed layer is less than 3nm, the thickness of the main layer is 10nm to 20nm, and the thickness of the doped microcrystalline silicon layer is less than 5nm.
[0010] Optionally, the crystallization rate of the seed layer is greater than 50%.
[0011] Optionally, the surface of the silicon substrate is the back side of the silicon substrate, the thickness of the intrinsic passivation layer is 9nm to 12nm, the thickness of the seed layer is less than 3nm, the thickness of the main layer is 20nm to 40nm, and the thickness of the doped microcrystalline silicon layer is less than 5nm.
[0012] Optionally, the crystallinity of the seed layer, the host layer, and the doped microcrystalline silicon layer is all greater than 20%.
[0013] Optionally, the surface of the doped microcrystalline silicon layer further has a transparent conductive oxide layer, and the refractive index of the transparent conductive oxide layer is less than 2.
[0014] Optionally, the transparent conductive oxide layer is made of one or more of the following materials: ITO, AZO, GAZO, SnO2, ATO, FTO, ICO, and IWO.
[0015] In a second aspect, the present invention provides a method for fabricating a solar cell, comprising: providing a silicon substrate; and sequentially depositing an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer on a surface of the silicon substrate, wherein the thickness of the doped amorphous silicon oxide layer is less than 3 nm, and the doped amorphous silicon oxide layer, the doped microcrystalline silicon oxide layer, and the doped microcrystalline silicon layer have the same doping conductivity type.
[0016] Optionally, depositing the doped microcrystalline silicon oxide layer includes: sequentially depositing a seed layer and a host layer on the surface of the doped amorphous silicon oxide layer, wherein the crystallinity of the seed layer is higher than that of the host layer, and the doping concentration of the doped microcrystalline silicon oxide layer is higher than that of the host layer.
[0017] Optionally, one surface of the silicon substrate is the front side of the silicon substrate, and during the deposition of the host layer and / or the doped microcrystalline silicon layer, the hydrogen dilution ratio is greater than 150, the gas pressure is greater than 4 mbar, and the deposition power is 350-450 mW / cm². 2 .
[0018] Optionally, one surface of the silicon substrate is the back surface of the silicon substrate, and the gas pressure during the deposition process is 1 mbar to 4 mbar when depositing the seed layer and / or the main layer and / or the doped microcrystalline silicon layer.
[0019] Compared with the prior art, the present invention has the following advantages: an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer are sequentially provided on one surface of a silicon substrate along a direction away from the silicon substrate. The thickness of the doped amorphous silicon oxide layer is less than 3 nm. Because of the presence of a doped amorphous silicon oxide layer, it is beneficial for subsequent film layers to be prepared under high power and high pressure. While maintaining battery performance, the film deposition time is reduced, which is conducive to increasing battery production on the mass production line. Attached Figure Description
[0020] The accompanying drawings are included to provide a further understanding of this application; they are incorporated into and constitute a part of this application. The drawings illustrate embodiments of this application and, together with this specification, serve to explain the principles of this application. In the drawings:
[0021] Figure 1 This is a schematic diagram of the structure of a solar cell according to an embodiment of the present invention;
[0022] Figure 2 This is a schematic diagram of the structure of a solar cell according to another embodiment of the present invention;
[0023] Figure 3 This is a schematic flowchart of a method for preparing a solar cell according to an embodiment of the present invention.
[0024] In the picture:
[0025] 110 - Silicon substrate, 120 - Intrinsic passivation layer, 130 - Doped amorphous silicon oxide layer, 140 - Functional layer; 141 - Seed layer, 142 - Main layer, 143 - Contact layer, 150 - Transparent conductive oxide layer, 160 - Metal electrode.
[0026] 221-First intrinsic passivation layer, 222-Second intrinsic passivation layer, 231-First doped amorphous silicon oxide layer, 232-Second doped amorphous silicon oxide layer, 241-First functional layer, 242-Second functional layer; 251-First transparent conductive oxide layer, 252-Second transparent conductive oxide layer, 261-First metal electrode, 262-Second metal electrode.
[0027] 2411 - First seed layer, 2412 - First main body layer, 2413 - First contact layer; 2421 - Second seed layer, 2422 - Second main body layer, 2423 - Second contact layer. Detailed Implementation
[0028] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are merely some examples or embodiments of this application. For those skilled in the art, these drawings can be applied to other similar scenarios without creative effort. Unless obvious from the context or otherwise specified, the same reference numerals in the drawings represent the same structures or operations.
[0029] As indicated in this application and claims, unless the context clearly indicates otherwise, the words "a," "an," "an," and / or "the" are not specifically singular and may include plural forms. Generally speaking, the terms "comprising" and "including" only indicate the inclusion of explicitly identified steps and elements, which do not constitute an exclusive list, and the method or apparatus may also include other steps or elements.
[0030] Furthermore, it should be noted that the use of terms such as "first" and "second" to define components is merely for the purpose of distinguishing the corresponding components. Unless otherwise stated, these terms have no special meaning and therefore should not be construed as limiting the scope of protection of this application. In addition, although the terminology used in this application is selected from commonly known and used terms, some terms mentioned in this application's specification may have been chosen by the applicant according to his or her judgment, and their detailed meanings are explained in the relevant sections of this description. Moreover, this application should be understood not only through the actual terms used, but also through the meaning implied by each term.
[0031] Flowcharts are used in this application to illustrate the operations performed according to embodiments of this application. It should be understood that the preceding or following operations are not necessarily performed in exact order. Instead, various steps can be processed in reverse order or simultaneously. Furthermore, other operations may be added to these processes, or one or more steps may be removed from them.
[0032] Figure 1This is a schematic diagram of the structure of a solar cell according to an embodiment of the present invention, for reference. Figure 1 As shown, it includes: a silicon substrate 110, one surface of which (the upper surface of the figure) has an intrinsic passivation layer 120, a doped amorphous silicon oxide layer 130, a doped microcrystalline silicon oxide layer and a doped microcrystalline silicon layer in sequence along a direction away from the silicon substrate 110, wherein the thickness of the doped amorphous silicon oxide layer 130 is less than 3 nm, and the doping conductivity types of the doped amorphous silicon oxide layer 130, the doped microcrystalline silicon oxide layer and the doped microcrystalline silicon layer are the same.
[0033] To improve the thin film deposition rate, high-power, high-pressure deposition methods are often used. However, this method results in higher ion bombardment, leading to a decrease in passivation effectiveness. For example, on the light-receiving surface (or sun-facing surface) of a solar cell, to reduce parasitic absorption in the passivation layer, the passivation layer thickness needs to be reduced. Therefore, the light-receiving surface in high-efficiency heterojunction cells is usually unsaturated passivation. Subsequent deposition of doped microcrystalline silicon oxide layers and doped microcrystalline silicon layers using high power will result in higher ion bombardment, causing a decrease in passivation effectiveness.
[0034] Without the doped amorphous silicon oxide layer 130, the doped microcrystalline silicon oxide layer and the doped microcrystalline silicon layer are directly deposited on the surface of the intrinsic passivation layer 120. Under high power and high pressure deposition conditions, this can easily damage other film layers, such as the intrinsic passivation layer 120, and even the silicon substrate 110. In this embodiment, the solar cell has a doped amorphous silicon oxide layer 130 between the intrinsic passivation layer 120 and the doped microcrystalline silicon oxide layer. With this structure, a high silane hydrogen dilution ratio can be maintained during the deposition of the doped microcrystalline silicon oxide layer and the doped microcrystalline silicon layer, while also maintaining the high power and high pressure deposition method. The high silane hydrogen dilution ratio and high deposition power can also give the film a high crystallinity, while the high pressure can reduce the mean free path of the plasma, reducing the bombardment damage to the film caused by the plasma under high power. Ultimately, while maintaining the performance of the solar cell, the film deposition time is significantly reduced, and the cell yield is increased.
[0035] In this embodiment, if the doped amorphous silicon oxide layer 130 is too thick, the parasitic absorption of the solar cell will increase significantly, leading to a decrease in cell current. Simultaneously, an excessively thick doped amorphous silicon oxide layer 130 will also increase the cell's series resistance. Therefore, in this embodiment, the thickness of the doped amorphous silicon oxide layer 130 is less than 3 nm. Furthermore, the wider bandgap of the doped amorphous silicon oxide layer 130 allows more sunlight to enter the solar cell, resulting in a higher current output.
[0036] In one implementation, the intrinsic passivation layer 120 is an intrinsic amorphous silicon layer or an intrinsic amorphous silicon oxide layer.
[0037] In this embodiment, the doped amorphous silicon oxide layer 130, the doped microcrystalline silicon oxide layer, and the doped microcrystalline silicon layer have the same doping conductivity type. For example, the doped amorphous silicon oxide layer 130, the doped microcrystalline silicon oxide layer, and the doped microcrystalline silicon layer are all N-type doped, which can be achieved by phosphorus doping.
[0038] In one example, the doped microcrystalline silicon oxide layer includes a seed layer 141 (the inner doped microcrystalline silicon oxide layer) and a host layer 142 (the outer doped microcrystalline silicon oxide layer) sequentially connected along a direction away from the silicon substrate 110. The doped microcrystalline silicon layer can be referred to as the contact layer 143, and the seed layer 141, host layer 142, and contact layer 143 are collectively referred to as the functional layer 140. The crystallinity of the seed layer 141 is higher than that of the host layer 142, and the doping concentration of the contact layer 143 is higher than that of the host layer 142.
[0039] In this embodiment, the doped microcrystalline silicon oxide layer is not deposited in a single step, but rather its performance is improved through a two-layer deposition process. The seed layer 141 is mainly used to improve the crystallinity of the main layer 142. The contact layer 143 is generally located between the transparent conductive oxide layer and the main layer 142, mainly to achieve good ohmic contact between the transparent conductive oxide layer and the main layer 142, reduce contact resistance, and improve carrier collection efficiency. Therefore, in this embodiment, the functional layer 140 includes the seed layer 141, the main layer 142, and the contact layer 143. When preparing the functional layer 140, a high crystallinity seed layer 141 can be deposited on the intrinsic passivation layer 120 to guide the crystal growth of the main layer 142, followed by the sequential deposition of the main layer 142 and the contact layer 143, thereby improving the performance of the functional layer 140.
[0040] In this embodiment, the seed layer 141 is a highly crystallized doped microcrystalline silicon with a very thin thickness. The crystallization rate of the main layer 142 is lower than that of the seed layer 141. The contact layer 143 is a highly doped microcrystalline silicon with the highest doping content. Through the cooperation between the four layers of doped amorphous silicon oxide layer 130, seed layer 141, main layer 142 and contact layer 143, it is beneficial to the efficient extraction and transport of electrons in the battery, forming better field-effect passivation, thereby improving the photoelectric efficiency of the battery.
[0041] In one example, the surface of the silicon substrate 110 is the front side of the silicon substrate 110, wherein the thickness of the intrinsic passivation layer 120 is 5 nm to 8 nm, the thickness of the seed layer 141 is less than 3 nm, the thickness of the main layer 142 is 10 nm to 20 nm, and the thickness of the contact layer 143 is less than 5 nm. Preferably, the crystallinity of the seed layer 141 is greater than 50%. A high crystallinity seed layer 141 is beneficial to improving the crystallinity of the main layer 142.
[0042] In one example, the surface of the silicon substrate 110 is the back side of the silicon substrate 110, the intrinsic passivation layer 120 has a thickness of 9 nm to 12 nm, the seed layer 141 has a thickness of less than 3 nm, the main layer 142 has a thickness of 20 nm to 40 nm, and the contact layer 143 has a thickness of less than 5 nm. Preferably, the crystallinity of the seed layer 141, the main layer 142, and the contact layer 143 is all greater than 20%.
[0043] In this embodiment, if the intrinsic passivation layer 120 is too thin, the battery passivation performance will be insufficient; if it is too thick, the battery series resistance will increase, especially on the front side of the battery. An excessively thick intrinsic passivation layer 120 will also reduce the battery current. For the seed layer 141 on both the front and back sides of the battery, if the seed layer 141 is too thin, it will not have a crystal-inducing effect; if it is too thick, the crystallinity at the interface between the intrinsic passivation layer 120 and the main layer 142 will be too high, leading to a decrease in the battery open-circuit voltage. For the front side of the battery, if the main layer 142 is too thin, the field effect will be weakened, which is not conducive to carrier transport; if the main layer 142 is too thick, the battery current will decrease. For the back side of the battery, if the main layer 142 is too thin, the built-in electric field strength of the PN junction will be insufficient, resulting in a lower battery open-circuit voltage; if the main layer 142 is too thick, the battery series resistance will increase. For both the front and back sides of the battery, if the contact layer 143 is too thin, it will not effectively reduce the contact resistance with the transparent conductive oxide layer 150; if the contact layer 143 is too thick, the battery series resistance will increase. Therefore, in this embodiment, the thicknesses of the seed layer 141, the main body layer 142, and the contact layer 143 should all be controlled within a reasonable range.
[0044] In one example, the surface of contact layer 143 also has a transparent conductive oxide layer 150, and the refractive index of the transparent conductive oxide layer 150 is less than 2. Transparent conductive oxide (TCO) is a thin film material with high transmittance and low resistivity in the visible light spectrum. It mainly includes oxides of In, Sb, Zn, and Cd, and their composite multi-element oxide thin film materials. Its high conductivity and transparency allow it to effectively allow most of the light to enter the absorption layer, collecting and transmitting the current generated by the solar cell, thus improving the light absorption efficiency of the cell. The low refractive index of the transparent conductive oxide is beneficial for reducing light reflection. Preferably, the texture thickness of the transparent conductive oxide layer 150 is less than 80 nm. An 80 nm thickness is the thickness that best reduces light reflection according to the Lambert-Beer law.
[0045] In one example, the transparent conductive oxide layer 150 is made of one or more of the following materials: ITO (indium tin oxide), AZO (aluminum-doped zinc oxide), GAZO (gallium aluminum co-doped zinc oxide), SnO2 (tin dioxide), ATO (antimony-doped tin dioxide), FTO (fluorine-doped tin oxide), ICO (indium cerium oxide), and IWO (indium tungsten oxide).
[0046] Figure 2 This is a schematic diagram of the structure of a solar cell according to another embodiment of the present invention, for reference. Figure 2 As shown, its structure mainly includes: on the front side (light incident surface) of the silicon substrate 110, there are sequentially a first intrinsic passivation layer 221, a first doped amorphous silicon oxide layer 231, a first functional layer 241, a first transparent conductive oxide layer 251 and a first metal electrode 261, wherein the first functional layer 241 can be composed of a first seed layer 2411 (the inner doped microcrystalline silicon oxide layer), a first host layer 2412 (the outer doped microcrystalline silicon oxide layer) and a first contact layer 2413 (the doped microcrystalline silicon layer). On the back side of the silicon substrate 110, a second intrinsic passivation layer 222, a second doped amorphous silicon oxide layer 232, a second functional layer 242, a second transparent conductive oxide layer 252, and a second metal electrode 262 are sequentially provided. The second functional layer 242 may be composed of a second seed layer 2421 (an inner doped microcrystalline silicon oxide layer), a second host layer 2422 (an outer doped microcrystalline silicon oxide layer or a doped microcrystalline silicon layer), and a second contact layer 2423 (a doped microcrystalline silicon layer). Preferably, the gate line density of the second metal electrode 262 is greater than the gate line density of the first metal electrode 261.
[0047] In this embodiment, the solar cell may have an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer structure on its front side, or it may have the same structure on its back side. Alternatively, the solar cell may have this structure on both its front and back sides. Further details regarding the doped amorphous silicon oxide layer, doped microcrystalline silicon oxide layer, and doped microcrystalline silicon layer structure in this embodiment can be found in the foregoing embodiments and will not be elaborated upon here.
[0048] In this embodiment, the solar cell has an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer sequentially on one surface (front and / or back) of the silicon substrate along the direction away from the silicon substrate. The thickness of the doped amorphous silicon oxide layer is less than 3 nm. Because of the presence of a doped amorphous silicon oxide layer, it is beneficial for subsequent film layers to be prepared under high power and high pressure. While maintaining the battery performance, the film deposition time is reduced, which is conducive to increasing the battery yield on the mass production line.
[0049] refer to Figure 3As shown, another embodiment of the present invention provides a method for preparing a solar cell, which can be used to prepare solar cells as shown in the foregoing embodiments, but is not limited to the above-mentioned solar cells. Method 300 mainly includes: S310, providing a silicon substrate; S320, sequentially depositing an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer and a doped microcrystalline silicon layer on a surface of the silicon substrate, wherein the thickness of the doped amorphous silicon oxide layer is less than 3 nm, and the doping conductivity types of the doped amorphous silicon oxide layer, the doped microcrystalline silicon oxide layer and the doped microcrystalline silicon layer are the same.
[0050] In one example, depositing a doped microcrystalline silicon oxide layer can be achieved by sequentially depositing a seed layer and a host layer on the surface of a doped amorphous silicon oxide layer, wherein the crystallinity of the seed layer is higher than that of the host layer, and the doping concentration of the doped microcrystalline silicon layer is higher than that of the host layer.
[0051] In one example, one surface of the silicon substrate is the front side of the silicon substrate. During the deposition of the host layer and / or the doped microcrystalline silicon layer, the hydrogen dilution ratio is greater than 150, the gas pressure is greater than 4 mbar, and the deposition power is 350-450 mW / cm². 2 These deposition parameters facilitate rapid deposition of the host layer and / or doped microcrystalline silicon layer, significantly reducing the deposition time of the host layer and / or doped microcrystalline silicon layer. Furthermore, the high gas pressure helps reduce the bombardment damage to the passivation layer caused by high-power processes.
[0052] Taking phosphorus doping as an example, the molar ratio of gas flow rates among the reactive gas raw materials H2, SiH4, CO2, and PH3 for forming the N-type amorphous silicon-oxygen layer is (10-200):1:(0.1-2):(0.01-0.1), and the pressure of the reactive gas is 1 mbar to 4 mbar; the molar ratio of gas flow rates among the reactive gas raw materials H2, SiH4, CO2, and PH3 for forming the seed layer is (200-400):1:(0.1-2):(0.01-0.1), and the reaction... The gas pressure is 1 mbar to 4 mbar; the molar ratio of the gas flow rates of the reactant raw materials H2, SiH4, CO2, and PH3 forming the N-type host layer is (150-250):1:(0.3-2):(0.01-0.1), and the gas pressure is 4 mbar to 6 mbar; the molar ratio of the gas flow rates of the reactant raw materials H2, SiH4, and PH3 forming the N-type doped microcrystalline silicon layer is (150-250):1:(0.02-0.1), and the gas pressure is 4 mbar to 6 mbar.
[0053] In one example, one surface of the silicon substrate is the back side of the silicon substrate, and the gas pressure during the deposition process is 1 mbar to 4 mbar when depositing the seed layer and / or the host layer and / or the doped microcrystalline silicon layer.
[0054] For example, the molar ratio of gas flow rates among the reactant gas raw materials H2, SiH4 and CO2 forming the P-type seed layer is (300-600):1:(0.3-2), and the pressure of the reactant gas is 1 mbar to 4 mbar; the molar ratio of gas flow rates among the reactant gas raw materials H2, SiH4 and B2H6 forming the P-type host layer is (300-600):1:(0.005-0.02), and the pressure of the reactant gas is 1 mbar to 4 mbar; the molar ratio of gas flow rates among the reactant gas raw materials H2, SiH4 and B2H6 forming the P-type doped microcrystalline silicon layer is (300-600):1:(0.02-0.1), and the pressure of the reactant gas is 1 mbar to 4 mbar.
[0055] It should be noted that the method of this embodiment may also include other conventional processes involved in the fabrication of solar cells. For example, in the cleaning or texturing process of the silicon substrate, before film deposition, the 100-phase monocrystalline silicon substrate needs to be cleaned and damaged, then texturized to form a uniform pyramid textured surface structure, then RCA cleaning is used to remove surface organic matter and metal ions, and the surface pyramids are smoothed, and finally the oxide layer is removed with HF solution.
[0056] Method 300 of this embodiment can prepare an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer structure on the front side of the solar cell, or prepare an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer structure on the back side of the solar cell, or prepare an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer structure on both the front and back sides of the solar cell.
[0057] For example, an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer structure are fabricated on both the front and back sides of a solar cell. The main steps include: fabricating a P-side intrinsic amorphous silicon passivation layer on the back side of an (N-type) monocrystalline silicon substrate using an RF-PECVD device; fabricating an N-side intrinsic amorphous silicon passivation layer on the light-facing side after flipping the silicon substrate; subsequently fabricating an N-type seed layer (the inner doped microcrystalline silicon oxide layer) sequentially using VHF-PECVD; fabricating an N-type host layer (the outer doped microcrystalline silicon oxide layer) under high pressure and high power conditions; depositing an N-type contact layer (doped microcrystalline silicon layer); fabricating a P-side seed layer (the inner doped microcrystalline silicon oxide layer) again after flipping the silicon substrate; fabricating a P-type host layer (the outer doped microcrystalline silicon oxide layer) under high pressure and high power conditions; and depositing a P-type contact layer (doped microcrystalline silicon layer). After completing the silicon-based thin film preparation stage, transparent conductive oxides are prepared on double-sided silicon substrates using PVD / RPD equipment. The thickness of the N-sided transparent conductive oxide is 68 nm, and the thickness of the P-sided transparent conductive oxide is 77 nm. Finally, metal electrodes are prepared by means of screen printing / laser transfer / copper electroplating, followed by curing / annealing of the metal electrodes.
[0058] In this embodiment, after depositing the intrinsic passivation layer, a doped amorphous silicon oxide layer (e.g., 1 nm thick) less than 2 nm can be deposited first. Then, a high crystallinity seed layer is deposited on this doped amorphous silicon oxide layer to guide the crystal growth of the main layer. Subsequently, the main layer and the contact layer are deposited sequentially. This preparation method can balance high silane hydrogen dilution ratio, high power, and high gas pressure during the deposition process. The high silane hydrogen dilution ratio and high deposition power can give the film a high crystallinity, while the high gas pressure can reduce the mean free path of the plasma and reduce the bombardment damage to the film caused by the plasma under high power. Ultimately, the deposition time is significantly reduced without affecting the battery performance, thereby increasing the battery yield.
[0059] Table 1 compares the effects of conventional solar cell fabrication methods with the solar cell fabrication method of this embodiment. Under the high-power, high-pressure deposition method, the film deposition time is reduced by 40% compared to the conventional method, and the performance of the solar cell does not decrease.
[0060] Table 1 Comparison of battery performance between conventional methods and the method of this embodiment.
[0061] Isc_(A) Voc_(V) FF_(%) Eta_(%) Rs_(Ω) pFF_(%) conventional methods 1.0000 1.0000 1.0000 1.0000 1.0000 1.0000 Method of this embodiment 0.9934 1.0014 1.0086 1.0027 1.1396 1.0118
[0062] The solar cell fabrication method of this embodiment produces a solar cell with an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer structure. Because it has a doped amorphous silicon oxide layer, it is beneficial for subsequent film layers to be fabricated under high power and high pressure. While maintaining the performance of the cell, the film deposition time is reduced, which is conducive to increasing the cell yield on the mass production line.
[0063] The basic concepts have been described above. Obviously, for those skilled in the art, the above disclosure is merely illustrative and does not constitute a limitation of this application. Although not explicitly stated herein, those skilled in the art may make various modifications, improvements, and corrections to this application. Such modifications, improvements, and corrections are suggested in this application, and therefore remain within the spirit and scope of the exemplary embodiments of this application.
[0064] In some embodiments, numbers describing the quantity of components and attributes are used. It should be understood that such numbers used in the description of embodiments are modified in some examples with the terms "approximately," "approximately," or "generally." Unless otherwise stated, "approximately," "approximately," or "generally" indicates that the numbers are allowed to vary by ±20%. Accordingly, in some embodiments, the numerical parameters used in the specification and claims are approximate values, which may be changed depending on the characteristics required by individual embodiments. In some embodiments, numerical parameters should take into account specified significant digits and employ a general method of digit reservation. Although the numerical ranges and parameters used to confirm their breadth of scope in some embodiments of this application are approximate values, in specific embodiments, such values are set as precisely as feasible.
[0065] Although this application has been described with reference to specific embodiments, those skilled in the art should recognize that the above embodiments are only used to illustrate this application, and various equivalent changes or substitutions can be made without departing from the spirit of this application. Therefore, any changes or modifications to the above embodiments within the essential spirit of this application will fall within the scope of the claims of this application.
Claims
1. A solar cell, characterized in that, include: silicon substrate; One surface of the silicon substrate has, in sequence along a direction away from the silicon substrate, an intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer, wherein the thickness of the doped amorphous silicon oxide layer is less than 3 nm, and the doped amorphous silicon oxide layer, the doped microcrystalline silicon oxide layer, and the doped microcrystalline silicon layer have the same doping conductivity type.
2. The solar cell as described in claim 1, characterized in that, The intrinsic passivation layer is an intrinsic amorphous silicon layer or an intrinsic amorphous silicon oxide layer.
3. The solar cell as described in claim 1, characterized in that, The doped microcrystalline silicon oxide layer includes a seed layer and a main layer sequentially connected in a direction away from the silicon substrate, wherein the crystallinity of the seed layer is higher than that of the main layer, and the doping concentration of the doped microcrystalline silicon layer is higher than that of the main layer.
4. The solar cell as described in claim 3, characterized in that, The surface of the silicon substrate is the front side of the silicon substrate, wherein the thickness of the intrinsic passivation layer is 5nm to 8nm, the thickness of the seed layer is less than 3nm, the thickness of the main layer is 10nm to 20nm, and the thickness of the doped microcrystalline silicon layer is less than 5nm.
5. The solar cell as described in claim 4, characterized in that, The crystallization rate of the seed layer is greater than 50%.
6. The solar cell as described in claim 3, characterized in that, The surface of the silicon substrate is the back side of the silicon substrate, the intrinsic passivation layer has a thickness of 9nm to 12nm, the seed layer has a thickness of less than 3nm, the main layer has a thickness of 20nm to 40nm, and the doped microcrystalline silicon layer has a thickness of less than 5nm.
7. The solar cell as claimed in claim 6, characterized in that, The crystallinity of the seed layer, the main layer, and the doped microcrystalline silicon layer is all greater than 20%.
8. The solar cell as claimed in claim 1, characterized in that, The surface of the doped microcrystalline silicon layer also has a transparent conductive oxide layer, and the refractive index of the transparent conductive oxide layer is less than 2.
9. The solar cell as claimed in claim 8, characterized in that, The transparent conductive oxide layer is made of one or more of the following materials: ITO, AZO, GAZO, SnO2, ATO, FTO, ICO, and IWO.
10. A method for preparing a solar cell, characterized in that, include: Provide a silicon substrate; An intrinsic passivation layer, a doped amorphous silicon oxide layer, a doped microcrystalline silicon oxide layer, and a doped microcrystalline silicon layer are sequentially deposited on one surface of the silicon substrate. The thickness of the doped amorphous silicon oxide layer is less than 3 nm, and the doped amorphous silicon oxide layer, the doped microcrystalline silicon oxide layer, and the doped microcrystalline silicon layer have the same doping conductivity type.
11. The method for preparing a solar cell as described in claim 10, characterized in that, Depositing the doped microcrystalline silicon oxide layer includes: sequentially depositing a seed layer and a host layer on the surface of the doped amorphous silicon oxide layer, wherein the crystallinity of the seed layer is higher than that of the host layer, and the doping concentration of the doped microcrystalline silicon layer is higher than that of the host layer.
12. The method for preparing a solar cell as described in claim 11, characterized in that, One surface of the silicon substrate is the front side of the silicon substrate. During the deposition of the host layer and / or the doped microcrystalline silicon layer, the hydrogen dilution ratio is greater than 150, the gas pressure is greater than 4 mbar, and the deposition power is 350-450 mW / cm². 2 .
13. The method for preparing a solar cell as described in claim 11, characterized in that, One surface of the silicon substrate is the back surface of the silicon substrate. When depositing the seed layer and / or the main layer and / or the doped microcrystalline silicon layer, the gas pressure during the deposition process is 1 mbar to 4 mbar.