Photovoltaic cell and method of manufacture

By incorporating a phase change material layer into the photovoltaic cell, the problem of hot spot effect in photovoltaic cells is solved, achieving insulation and isolation under normal operating conditions and bypass protection when hot spots occur, reducing leakage current and safety hazards, and extending the service life of photovoltaic cells.

CN123145992APending Publication Date: 2026-11-20ZHEJIANG AIKO SOLAR ENERGY TECH CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611407678.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Photovoltaic cells are prone to hot spot effects when partially shaded or when there is current mismatch, which can cause a sharp rise in temperature, resulting in a decrease in output power and safety hazards.

Method used

A phase change material layer is placed between the P-type and N-type regions of a photovoltaic cell. The phase change material layer is in an insulating state below the phase change temperature and transforms into a conductive state above the phase change temperature, forming a bypass protection path to isolate or connect the P-type and N-type regions.

Benefits of technology

It effectively avoids leakage current, suppresses the temperature rise in hot spot areas, reduces safety hazards, and extends the service life of photovoltaic cells and modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123145992A_ABST
    Figure CN123145992A_ABST
Patent Text Reader

Abstract

The application relates to the photovoltaic technology field, in particular to a photovoltaic cell and a preparation method. The photovoltaic cell comprises a silicon substrate, a P-type region, an N-type region, a phase change material layer and a metal electrode. The P-type region and the N-type region are arranged on the same surface of the silicon substrate, and a gap region is arranged between the P-type region and the N-type region. The phase change material layer is arranged in the gap region, and the two sides of the phase change material layer are connected to the P-type region and the N-type region respectively. The metal electrode is arranged on the P-type region and the N-type region respectively. The phase change material layer is in an insulating state when being lower than a phase change temperature, so as to insulate and separate the P-type region and the N-type region; the phase change material layer is converted into a conductor state when reaching or exceeding the phase change temperature, so as to make the P-type region and the N-type region electrically conductive to form a bypass protection path. The photovoltaic cell can reduce the hot spot effect, reduce the safety hidden danger and prolong the service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of photovoltaic technology, and in particular to a photovoltaic cell and its preparation method. Background Technology

[0002] Back-contact (BC) solar cells have become an important development direction in the photovoltaic field due to their advantages such as no metal grid lines obstructing the front side, high photoelectric conversion efficiency, and aesthetically pleasing appearance. However, in practical applications, when photovoltaic modules experience localized shading, cell defects, or current mismatch, some cell units may switch from power generation to energy consumption, leading to a sharp increase in local temperature and the formation of hot spots. Hot spots not only cause a significant decrease in the output power of photovoltaic modules and long-term performance degradation, but in severe cases, excessively high local temperatures can also lead to safety hazards such as aging of encapsulation materials, backsheet burnout, and even fire.

[0003] Therefore, there is an urgent need to design a photovoltaic cell and its fabrication method to solve the above technical problems. Summary of the Invention

[0004] The purpose of this application is to propose a photovoltaic cell and its preparation method, which can reduce the hot spot effect of photovoltaic cells and reduce safety hazards.

[0005] To achieve this objective, the following technical solution is adopted in this application: In a first aspect, this application provides a photovoltaic cell, comprising: Silicon substrate; P-type regions and N-type regions are disposed on the same surface of the silicon substrate, and a gap region is disposed between the P-type regions and the N-type regions; A phase change material layer is disposed in the gap region, and the two sides of the phase change material layer are respectively connected to the P-type region and the N-type region; Metal electrodes are respectively disposed on the P-type region and the N-type region; Wherein, the phase change material layer is in an insulating state below the phase change temperature to insulate and isolate the P-type region from the N-type region; the phase change material layer transforms into a conductive state when the phase change temperature is reached or exceeded, so that the P-type region and the N-type region are electrically connected to form a bypass protection path. As an optional technical solution for photovoltaic cells, the phase change material layer has a phase change temperature of not less than 70°C.

[0006] As an optional technology solution for photovoltaic cells, the phase change material layer is a VO2 thin film, and the VO2 thin film is doped with Sn element.

[0007] As an optional technology for photovoltaic cells, the phase transition temperature of the phase change material layer is controlled by adjusting the Sn element doping concentration.

[0008] As an optional technology solution for photovoltaic cells, a buffer layer is further provided between the surface of the silicon substrate and the phase change material layer; the buffer layer is disposed on the bottom surface of the gap region and extends to the surface of the silicon substrate, the phase change material layer is formed on the buffer layer, and the buffer layer is configured to isolate the silicon substrate and the phase change material layer to prevent interface reaction.

[0009] As an optional technical solution for photovoltaic cells, the buffer layer includes at least one of Al2O3, SiO2, or TiO2.

[0010] As an optional technology for photovoltaic cells, a phase change material layer is disposed in a portion of the gap region between the P-type region and the N-type region.

[0011] As an optional technology for photovoltaic cells, the phase change material layer is disposed in all gap regions between the P-type region and the N-type region.

[0012] As an optional technology for photovoltaic cells, the thickness of the phase change material layer is 150nm-400nm.

[0013] Secondly, this application provides a method for preparing a photovoltaic cell, used to prepare the photovoltaic cell described in any of the above optional technical solutions, the method for preparing the photovoltaic cell comprising the following steps: Provide silicon substrate; A P-type region and an N-type region are formed on the same surface of the silicon substrate, with a gap region between the P-type region and the N-type region; A phase change material layer is formed in the gap region, and the phase change material layer is in contact with the P-type region and the N-type region respectively; the phase change material layer is in an insulating state below the phase change temperature to insulate and isolate the P-type region from the N-type region; the phase change material layer transforms into a conductive state when the phase change temperature is reached or exceeded to form a conductive path between the P-type region and the N-type region. Metal electrodes are formed on the P-type region and the N-type region.

[0014] As an optional technical solution for the fabrication of photovoltaic cells, the step of forming a phase change material layer in the gap region includes: Using VO2 ceramic target and SnO2 ceramic target as dual sputtering sources, magnetron sputtering is performed in a mixed gas of Ar and O2 to deposit a tin-doped VO2 phase change material layer in the gap region. After sputtering is completed, the VO2 ceramic target, SnO2 ceramic target and O2 are turned off, while Ar gas is retained, and the mixture is cooled to room temperature at a rate of 5℃-10℃ / min. The tin-doped VO2 phase change material layer cooled to room temperature was subjected to high-temperature annealing in a nitrogen atmosphere. The phase transition temperature of the phase transition material layer is controlled by adjusting the sputtering power of the SnO2 ceramic target to change the doping concentration of the Sn element.

[0015] As an optional technical solution for the fabrication of photovoltaic cells, after forming the phase change material layer, the fabrication method of the photovoltaic cell further includes: Based on a preset reverse voltage start-up threshold, the number and position of the phase change material layers are adjusted by laser or etching to remove unwanted phase change material layers, so that the P-type region and the N-type region can achieve selective conduction through the retained phase change material layers.

[0016] As an optional technical solution for the fabrication of photovoltaic cells, before forming the P-type and N-type regions, the fabrication method of the photovoltaic cell further includes: A buffer layer is prepared on the surface of the silicon substrate, the buffer layer being configured as an isolation layer between the silicon substrate and the phase change material layer; the buffer layer includes at least one of Al2O3, SiO2, or TiO2.

[0017] The beneficial effects of this application include at least the following: This application provides a photovoltaic cell, which includes a silicon substrate, a P-type region, an N-type region, a phase change material layer, and metal electrodes. The P-type and N-type regions are both disposed on the same surface of the silicon substrate, with a gap region between them. The phase change material layer is disposed in the gap region, and its two sides are connected to the P-type and N-type regions, respectively. Metal electrodes are disposed on the P-type and N-type regions. Below the phase change temperature, the phase change material layer is in an insulating state to isolate the P-type and N-type regions; when the phase change temperature is reached or exceeded, the phase change material layer transforms into a conductive state, electrically connecting the P-type and N-type regions to form a bypass protection path.

[0018] In summary, when the photovoltaic module is operating normally, the phase change material layer is at its normal operating temperature. At this time, the phase change material layer is in an insulating state, completely blocking the leakage current path between the P-type and N-type regions. This eliminates the direct conductive path between the P-type and N-type regions, effectively avoiding leakage current problems and reducing conversion efficiency loss. When a photovoltaic cell in the module switches from power generation to energy consumption due to partial shading, a reverse bias voltage is generated across the terminals of that photovoltaic cell. Simultaneously, the local temperature in the shaded area rises sharply due to Joule heat accumulation. As the temperature rises to the phase change threshold of the phase change material layer, the phase change material layer abruptly changes from an insulating state to a conductive state. The P-type region and the N-type region instantly become conductive, forming a low-resistance bypass path connected in parallel across the photovoltaic cell. The on-resistance of this bypass path is much lower than the reverse impedance of the shaded cell, allowing the current of the photovoltaic module to flow mainly through the bypass path. This clamps the reverse voltage across the shaded cell at a low level, suppressing the temperature of the hot spot area from continuing to rise. This avoids safety hazards such as yellowing of the encapsulation film, solder joint detachment, or even photovoltaic cell fire caused by local overheating, thus extending the service life of the photovoltaic cell and photovoltaic module.

[0019] This application provides a method for preparing photovoltaic cells, which has simple process steps, can reduce the hot spot effect of photovoltaic cells, and reduce safety hazards. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments of this application will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the content of the embodiments of this application and these drawings without creative effort.

[0021] Figure 1 This is a schematic diagram of the structure of the photovoltaic cell provided in the embodiments of this application; Figure 2 This is a schematic diagram of the structure between the P-type region, the phase change material layer, and the N-type region provided in the embodiments of this application. Figure 1 ; Figure 3 This is a schematic diagram of the structure between the P-type region, the phase change material layer, and the N-type region provided in the embodiments of this application. Figure 2 ; Figure 4 This is a schematic flowchart of the photovoltaic cell fabrication method provided in the embodiments of this application. Figure 1 ; Figure 5 This is a schematic diagram of the process for forming a phase change material layer provided in the embodiments of this application; Figure 6This is a schematic flowchart of the photovoltaic cell fabrication method provided in the embodiments of this application. Figure 2 .

[0022] Figure Labels 10. Silicon substrate; 20. P-type region; 30. N-type region; 40. Interstitial region; 50. Phase change material layer; 60. Metal electrode; 70. Buffer layer; 80. AlO x Layer; 90, SiN x Layer; 101, SiO x layer. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. The components of the embodiments of this application described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.

[0024] Therefore, the following detailed description of the embodiments of this application provided in the accompanying drawings is not intended to limit the scope of the claimed application, but merely to illustrate selected embodiments of the application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0025] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.

[0026] In the description of this application, it should be noted that the terms "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product is in use. They are used only for the convenience of describing this application and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application. Furthermore, the terms "first," "second," and "third," etc., are used only to distinguish descriptions and should not be construed as indicating or implying relative importance. In the description of this application, unless otherwise stated, "a plurality of" means two or more.

[0027] In the description of this application, it should also be noted that, unless otherwise expressly specified and limited, the terms "set" and "connection" should be interpreted broadly, for example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0028] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature being directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0029] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.

[0030] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments.

[0031] This embodiment provides a photovoltaic cell that can reduce the hot spot effect of photovoltaic cells and reduce safety hazards.

[0032] like Figures 1-3 As shown, the photovoltaic cell mainly includes a silicon substrate 10, a P-type region 20, an N-type region 30, a phase change material layer 50, and a metal electrode 60. The P-type region 20 and the N-type region 30 are both disposed on the same surface of the silicon substrate 10, and a gap region 40 is provided between the P-type region 20 and the N-type region 30. The phase change material layer 50 is disposed in the gap region 40, and its two sides are connected to the P-type region 20 and the N-type region 30, respectively. The metal electrode 60 is disposed on the P-type region 20 and the N-type region 30, respectively. The phase change material layer 50 is in an insulating state below the phase change temperature (<70℃) to isolate the P-type region 20 from the N-type region 30; when the phase change temperature is reached or exceeded (≥70℃), the phase change material layer 50 transforms into a conductive state, allowing the P-type region 20 and the N-type region 30 to be electrically connected, forming a bypass protection path.

[0033] Based on the above design, in this embodiment, when the photovoltaic module is operating normally, the phase change material layer 50 is at its normal operating temperature. At this time, the phase change material layer 50 is in an insulating state, completely blocking the leakage current path between the P-type region 20 and the N-type region 30. This ensures that there is no direct conductive path between the P-type region 20 and the N-type region 30, effectively avoiding leakage current problems and reducing conversion efficiency loss. When a photovoltaic cell in the photovoltaic module switches from a power generation state to an energy consumption state due to partial shading, a reverse bias voltage is generated at both ends of the photovoltaic cell. At the same time, the local temperature in the shaded area rises sharply due to the accumulation of Joule heat. As the temperature rises to the phase change threshold of the phase change material layer 50, the phase change material layer 50 abruptly changes from an insulating state to a conductive state. The P-type region 20 and the N-type region 30 are instantly connected, forming a low-resistance bypass path connected in parallel across the photovoltaic cell. The on-resistance of this bypass path is much lower than the reverse impedance of the shaded cell, so that the current of the photovoltaic module mainly flows through the bypass path. This clamps the reverse voltage across the shaded cell at a low level, suppressing the temperature of the hot spot area from continuing to rise. This avoids safety hazards such as yellowing of the encapsulation film, solder joint detachment, or even photovoltaic cell fire caused by local overheating, and extends the service life of the photovoltaic cell and photovoltaic module.

[0034] In some optional embodiments, the phase change material layer 50 is a VO2 thin film doped with Sn. Specifically, a magnetron sputtering process is used, employing a VO2 ceramic target and a SnO2 ceramic target as dual sputtering sources, in a mixed atmosphere of argon and oxygen to co-sputter, thereby depositing a Sn-doped VO2 thin film on the interstitial region 40. Sn enters the V sites in the VO2 lattice in a substitutional manner, and the atomic percentage concentration of Sn in the film is approximately 4%. This tin-doped VO2 thin film is light brown at room temperature and exhibits typical semiconductor properties; when the temperature is raised to approximately 80°C, a reversible phase transition occurs, accompanied by a sharp decrease in resistivity.

[0035] For example, the phase change temperature of the phase change material layer 50 in this embodiment is not less than 70°C.

[0036] Furthermore, in this embodiment, the phase transition temperature of the phase transition material layer 50 is controlled by adjusting the Sn doping concentration. The specific relationships are as follows: when the Sn doping concentration is 2 at.% to 3 at.%, the phase transition temperature is controlled at 70°C to 75°C; when the Sn doping concentration is 4 at.% to 5 at.%, the phase transition temperature is controlled at 75°C to 85°C; when the Sn doping concentration is 6 at.% to 7 at.%, the phase transition temperature is controlled at 85°C to 95°C; and when the Sn doping concentration is 7 at.% to 8 at.%, the phase transition temperature can reach above 95°C. The above-mentioned Sn doping concentration adjustment is achieved by changing the sputtering power of the SnO2 ceramic target. For example, gradually increasing the SnO2 target power from 10W to 40W can correspondingly increase the Sn doping concentration in the thin film.

[0037] As shown in Table 1, Table 1 shows the relationship between the phase transition temperature of the phase change material layer 50, the Sn doping concentration, and the sputtering power of the SnO2 ceramic target.

[0038] Table 1 By leveraging the continuously adjustable Sn doping concentration, customized design of the phase transition temperature is achieved. This allows the same battery fabrication process to be adapted to hot spot protection requirements in different regions and under different operating conditions by adjusting a single process parameter (SnO2 target power), significantly improving the product's applicability and process flexibility. Furthermore, adjusting the Sn doping concentration requires no changes to the deposition equipment or additional process steps; it can be achieved simply by adjusting the sputtering power, resulting in extremely low modification costs to existing production lines.

[0039] In some optional embodiments, the thickness of the phase change material layer 50 is 150 nm-400 nm. In specific implementations, the thickness of the phase change material layer 50 is precisely controlled by adjusting the deposition time of the PVD magnetron sputtering. Based on a deposition rate of 1 nm / min-3 nm / min, the deposition time for a target film thickness of 150 nm is approximately 50-150 minutes, and the deposition time for a target film thickness of 400 nm is approximately 133-400 minutes. After deposition, the film thickness is monitored online using an ellipsometry or profilometer to ensure that the thickness deviation is within ±10%.

[0040] Specifically, the impact of the phase change material layer thickness 50 on photovoltaic cell performance is reflected in the following three aspects. First, in terms of insulation performance: when the thickness is less than 150nm, the insulation resistivity of the VO2 film is insufficient, the isolation resistance between the P-type region 20 and the N-type region 30 is low, and a non-negligible leakage current may occur under normal operating conditions, leading to a decrease in conversion efficiency; when the thickness is above 150nm, the VO2 film can form a continuous and dense insulating layer, and the insulation resistivity reaches 10. 6 Above Ω•cm, it effectively isolates the P-type region 20 and the N-type region 30. Secondly, regarding phase transition response: when the thickness exceeds 400nm, although the resistivity of the insulating state further increases, the internal stress of the film increases significantly, posing a risk of cracking and peeling. Simultaneously, the heat transfer time within the thick film during the phase transition is prolonged, leading to a slower phase transition response speed—that is, a longer lag time from the insulating state to the conducting state—which is detrimental to a rapid protective response when hot spots occur. Thirdly, regarding process cost: the greater the thickness, the longer the deposition time, the lower the yield, and the higher the cost.

[0041] Therefore, the thickness of the phase change material layer 50 is controlled within the range of 150nm-400nm to ensure that the photovoltaic cell has sufficient insulation capability to suppress leakage under normal operating conditions, while also having a rapid phase change response capability to achieve timely bypass protection when hot spots occur. This thickness range balances photovoltaic cell performance and process feasibility, ensuring that the phase change material layer 50 exhibits stable and reliable electrical characteristics in both insulating and conductive states.

[0042] like Figure 1 As shown, in this embodiment, a buffer layer 70 is also provided between the surface of the silicon substrate 10 and the phase change material layer 50; the buffer layer 70 is provided on the bottom surface of the gap region 40 and extends to the entire surface of the silicon substrate 10. The phase change material layer 50, the P-type region 20 and the N-type region 30 are all formed on the buffer layer 70. The buffer layer 70 is configured to isolate the silicon substrate 10 and the phase change material layer 50 to prevent interface reaction.

[0043] In the specific implementation process, the buffer layer 70 is deposited on the surface of the silicon substrate 10 and the bottom surface of the interstitial region 40 using PVD (physical vapor deposition), ALD (atomic layer deposition), or CVD (chemical vapor deposition) processes, with a thickness ranging from 5nm to 50nm. The material of the buffer layer 70 can be a wide bandgap insulating material such as Al2O3, SiO2, or TiO2. These materials are chemically stable under high-temperature conditions and can effectively isolate the silicon element in the silicon substrate 10 from the vanadium element in the phase change material layer 50, preventing the formation of vanadium-silicon compounds from the interface reaction between V and Si during high-temperature annealing. Furthermore, the coefficient of thermal expansion of the buffer layer 70 is between that of the silicon substrate 10 and the phase change material layer 50, which can play a role in thermal stress transition, alleviating the stress concentration problem in the film layer caused by the difference in thermal expansion coefficients between the two.

[0044] like Figure 2 As shown, in some optional embodiments, a phase change material layer 50 is disposed in a portion of the gap region 40 between the P-type region 20 and the N-type region 30. In specific implementations, after the phase change material layer 50 is deposited, a portion of the phase change material layer 50 in the gap region 40 is removed by laser ablation or photolithography, so that only a portion of the gap region 40 retains the phase change material layer 50, while the remaining gap regions 40 have the P-type region 20 and N-type region 30 directly exposed or filled with other insulating media. By designing different patterned layouts, the coverage ratio (i.e., coverage rate) of the phase change material layer 50 in the gap region 40 can be controlled, thereby adjusting the effective area of ​​bypass conduction between the P-type region 20 and the N-type region 30.

[0045] By incorporating a phase change material layer 50 within a partial gap region 40, the bypass conduction area between the P-type region 20 and the N-type region 30 is flexibly adjustable, enabling the photovoltaic cell to achieve an optimal balance between bypass conduction capability and normal operating leakage current. For different application environments and safety requirements, the coverage of the phase change material layer 50 can be adjusted through a simple patterning process without changing the core materials and deposition process, reducing the process development costs for product series. Simultaneously, it also reduces the total amount of phase change material layer 50 used, which helps lower raw material costs.

[0046] In some embodiments, in the gap region 40 with a length of 100 μm, the phase change material layer 50 is distributed in multiple parallel strip structures, each strip structure having a length of approximately 10 μm and a spacing of approximately 15 μm between adjacent strip structures. The phase change material layer 50 covers an area of ​​approximately 40% of the total area of ​​the gap region 40, and the remaining 60% of the area is filled and covered by a silicon nitride passivation layer.

[0047] In some embodiments, the coverage of the phase change material layer 50 can be flexibly designed according to the power specifications and hot spot risk level of the photovoltaic cell. For example, one or more phase change material layers 50 can be provided in each gap region 40.

[0048] like Figure 3 As shown, in some optional embodiments, a phase change material layer 50 is disposed throughout the entire gap region 40 between the P-type region 20 and the N-type region 30. In a specific implementation, after the buffer layer 70 is prepared, the phase change material layer 50 is deposited throughout the entire gap region 40, so that the P-type region 20 and the N-type region 30 are separated by the phase change material layer 50 throughout the entire gap region 40. Thus, there is no direct contact area between the P-type region 20 and the N-type region 30; they are indirectly connected throughout the entire gap region 40 via the phase change material layer 50.

[0049] The fully covered phase change material layer 50 creates uniform insulation between the P-type region 20 and the N-type region 30 throughout the entire gap region 40, providing maximum leakage resistance protection under normal photovoltaic cell operating conditions. Simultaneously, it provides a maximum bypass conduction path when hot spots occur, ensuring sufficient reverse current shunting and rapid, uniform temperature suppression in the hot spot region. This solution features a simple process, requires no patterning steps, and is particularly suitable for photovoltaic cell structures with a narrow gap region 40 between the P-type region 20 and the N-type region 30.

[0050] like Figure 4 As shown, this embodiment also provides a method for preparing a photovoltaic cell, which includes the following steps: A silicon substrate 10 is provided. Specifically, an N-type monocrystalline silicon wafer is provided as the silicon substrate 10, and the silicon substrate 10 is cleaned to remove surface damage layers, organic contaminants, and metal ions.

[0051] A P-type region 20 and an N-type region 30 are formed on the same surface of a silicon substrate 10, with a gap region 40 between them. Specifically, an intrinsic amorphous silicon or polycrystalline silicon passivation layer is deposited on the back side of the silicon substrate 10, and a P-type region 20 is formed in a designated area by boron diffusion, while borosilicate glass is deposited simultaneously. Next, a portion of the borosilicate glass is selectively removed using a laser to define the boundary of the P-type region 20 and expose the silicon surface of the subsequent gap region 40. The laser-treated surface is then polished and cleaned to remove laser ablation residues, retaining the passivation layer above the gap region 40 and the N-type region 30, or selectively removing only the passivation layer of the gap region 40 to expose the surface of the silicon substrate 10.

[0052] A phase change material layer 50 is formed in the gap region 40, and the phase change material layer 50 is in contact with the P-type region 20 and the N-type region 30, respectively. The phase change material layer 50 is in an insulating state below the phase change temperature to insulate the P-type region 20 from the N-type region 30. When the phase change temperature is reached or exceeded, the phase change material layer 50 transforms into a conductive state to form a conductive path between the P-type region 20 and the N-type region 30. Specifically, a tin-doped VO2-based thin film is deposited in the gap region 40 using a PVD magnetron sputtering process, and the composition and properties of the phase change material layer 50 are controlled by adjusting the sputtering power and atmosphere.

[0053] Metal electrodes 60 are formed on the P-type region 20 and the N-type region 30. Specifically, metal electrodes 60 are formed on the surfaces of the P-type region 20 and the N-type region 30 respectively using silver paste printing and sintering or copper electroplating processes. Furthermore, the material of the metal electrodes 60 can be one or more alloys of metals such as gold, silver, copper, tin, and nickel.

[0054] The method for preparing this photovoltaic cell is highly compatible with existing back-contact cell production lines. It does not require large-scale modifications to the production line. Only the addition of a phase change material layer 50 deposition equipment is needed to achieve mass production of high-efficiency back-contact photovoltaic cells with adaptive hot spot protection function. The process steps are simple, which can reduce the hot spot effect of photovoltaic cells and reduce safety hazards.

[0055] Furthermore, such as Figure 5 As shown, in this embodiment, the step of forming a phase change material layer 50 in the gap region 40 specifically includes: Using VO2 ceramic target and SnO2 ceramic target as dual sputtering sources, magnetron sputtering is performed in a mixed gas of argon and oxygen to deposit a tin-doped VO2 phase change material layer 50 in the interstitial region 40.

[0056] Specifically, the pretreated silicon substrate 10 is first placed into the magnetron sputtering vacuum chamber, and a molecular pump is used to evacuate the chamber. Then, the silicon substrate 10 is heated to 400℃-500℃ and held for 10-20 minutes to remove adsorbed water vapor and volatile organic compounds from its surface. After degassing, a VO2 ceramic target (RF power set to 80W–120W) and a SnO2 ceramic target (RF power set to 10W–40W) are used as dual sputtering sources. Reactive magnetron sputtering is performed in a mixed atmosphere of Ar (flow rate 30sccm–50sccm) and O2 (flow rate 2sccm–6sccm). During sputtering, the working pressure is controlled at 3sccm–8mTorr, the substrate temperature is maintained at 400℃–500℃, and the substrate is rotated at 10rpm–20rpm to ensure uniform film thickness. Under these conditions, the deposition rate is approximately 1 nm / min–3 nm / min, and deposition continues for 125 minutes to obtain a tin-doped VO2 thin film phase change material layer 50 with a thickness of approximately 250 nm.

[0057] Tin-doped VO2 thin film phase change material layer 50 was prepared by PVD reactive magnetron co-sputtering process. The dual-target co-sputtering method achieved simultaneous deposition of VO2 main phase and Sn dopant. The process parameters were well controllable, the film composition was uniform, and the Sn doping concentration could be precisely controlled by the target power.

[0058] After sputtering, the VO2 ceramic target, SnO2 ceramic target and O2 are turned off, while Ar gas is retained. The film is cooled to room temperature at a rate of 5℃ / min-10℃ / min. This slow cooling process after sputtering can release the internal stress of the film, prevent the film from cracking, and maintain the stoichiometry of VO2.

[0059] The tin-doped VO2 phase change material layer 50, cooled to room temperature, was subjected to high-temperature annealing in a nitrogen atmosphere. Specifically, after cooling, the silicon wafer was transferred to a tube annealing furnace and annealed at 450°C–500°C for 1–2 hours in a nitrogen atmosphere (nitrogen flow rate 5 L / min) to eliminate residual stress in the tin-doped VO2 film and stabilize the crystal structure.

[0060] The phase transition temperature of the phase transition material layer 50 is controlled by adjusting the sputtering power of the SnO2 ceramic target to change the Sn doping concentration.

[0061] like Figure 6 As shown, in this embodiment, after forming the phase change material layer 50, the photovoltaic cell fabrication method further includes adjusting the number and position of the phase change material layer 50 by laser or etching according to a preset reverse voltage start-up threshold, removing unwanted phase change material layers 50, so that the P-type region 20 and the N-type region 30 can achieve selective conduction through the retained phase change material layer 50, that is, forming Figure 2 The structure of photovoltaic cells in the image.

[0062] Specifically, the reverse voltage start-up threshold refers to the voltage at which the bypass diode of a photovoltaic cell begins to conduct under reverse bias conditions. This threshold is directly related to the amount and positional distribution of the phase change material layer 50 in the gap region 40: the more phase change material layers 50 are covered and the larger the coverage area, the greater the equivalent insulation resistance between the P-type region 20 and the N-type region 30, and the higher the breakdown voltage of the bypass diode under reverse bias; conversely, the fewer the layers, the lower the breakdown voltage. Through circuit simulation or experimental calibration, the target reverse breakdown voltage under different hot spot risk scenarios can be determined, and a corresponding graphical layout scheme for the phase change material layer 50 can be designed. Then, pulsed laser ablation or photolithography mask etching processes are used to precisely remove the unwanted phase change material layer 50 in the gap region 40, exposing the underlying buffer layer 70.

[0063] This selective conduction layout allows for fine-tuning of the equivalent turn-on voltage and on-resistance of the bypass diodes according to design requirements. This enables photovoltaic cells with a phase change material layer 50 set in a partial gap region 40, achieving flexible adjustment of the bypass conduction area between the P-type region 20 and the N-type region 30. This allows the photovoltaic cells to achieve an optimal balance between bypass conduction capability and normal operation leakage current. For different application environments and safety requirements, the coverage of the phase change material layer 50 can be adjusted through a simple patterning process without changing the core materials and deposition process, reducing the process development cost for product series. At the same time, it also reduces the total amount of phase change material layer 50 used, which helps to reduce raw material costs.

[0064] like Figure 6 As shown, in this embodiment, before forming the P-type region 20 and the N-type region 30, the method for preparing a photovoltaic cell further includes preparing a buffer layer 70 on the surface of a silicon substrate 10. The buffer layer 70 is configured as an isolation layer between the silicon substrate 10 and the phase change material layer 50. The buffer layer 70 includes at least one of Al2O3, SiO2, or TiO2.

[0065] Specifically, the buffer layer 70 is prepared before the formation of the P-type region 20 and the N-type region 30, first forming a chemically inert isolation barrier on the surface of the silicon substrate 10. During the subsequent deposition and annealing of the phase change material layer 50 at temperatures up to 500°C, the buffer layer 70 effectively blocks the diffusion of vanadium atoms into the silicon substrate 10 and the diffusion of silicon atoms into the phase change material layer 50, suppressing the V-Si interface reaction and the formation of vanadium-silicon compounds.

[0066] For example, the thickness of the buffer layer 70 in this embodiment can be set to 5nm-50nm.

[0067] like Figure 6As shown, in this embodiment, after adjusting the number and position of the phase change material layer 50 by laser or etching and removing unwanted phase change material layers 50, the photovoltaic cell fabrication method further includes the following steps: An anti-reflective textured surface and an AlO2 layer are sequentially fabricated on the front side of the silicon substrate 10. x Layer 80, SiN x Layer 90 and SiO x Layer 101, a three-layer stacked structure (AlO x / SiN x / SiO x Together, they form a composite passivation and anti-reflection stack, enabling the photovoltaic cell surface to simultaneously possess excellent surface passivation effects and extremely low reflectivity, thereby maximizing the photoelectric conversion efficiency of the photovoltaic cell.

[0068] Obviously, the above are merely preferred embodiments and technical principles applied in this application. Those skilled in the art will understand that this application is not limited to the specific embodiments described herein, and various obvious changes, readjustments, and substitutions can be made without departing from the scope of protection of this application. Therefore, although this application has been described in detail through the above embodiments, this application is not limited to the above embodiments, and may include many other equivalent embodiments without departing from the concept of this application, the scope of which is determined by the scope of the appended claims.

[0069] Note that in the description of this specification, the references to terms such as "some embodiments," "other embodiments," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

Claims

1. A photovoltaic cell, characterized in that, include: Silicon substrate (10); P-type region (20) and N-type region (30) are disposed on the same surface of the silicon substrate (10), and a gap region (40) is disposed between the P-type region (20) and the N-type region (30). A phase change material layer (50) is disposed in the gap region (40), and the two sides of the phase change material layer (50) are respectively connected to the P-type region (20) and the N-type region (30). Metal electrodes (60) are respectively disposed on the P-type region (20) and the N-type region (30); The phase change material layer (50) is in an insulating state when it is below the phase change temperature, so as to isolate the P-type region (20) from the N-type region (30); the phase change material layer (50) transforms into a conductive state when it reaches or exceeds the phase change temperature, so that the P-type region (20) and the N-type region (30) are electrically connected to form a bypass protection path.

2. The photovoltaic cell according to claim 1, characterized in that, The phase change temperature of the phase change material layer (50) is not less than 70°C.

3. The photovoltaic cell according to claim 1, characterized in that, The phase change material layer (50) is a VO2 thin film, and the VO2 thin film is doped with Sn element.

4. The photovoltaic cell according to claim 3, characterized in that, The phase transition temperature of the phase change material layer (50) is controlled by adjusting the doping concentration of Sn element.

5. The photovoltaic cell according to claim 1, characterized in that, A buffer layer (70) is further provided between the surface of the silicon substrate (10) and the phase change material layer (50); the buffer layer (70) is disposed on the bottom surface of the gap region (40) and extends to the surface of the silicon substrate (10), the phase change material layer (50) is formed on the buffer layer (70), and the buffer layer (70) is configured to isolate the silicon substrate (10) and the phase change material layer (50) to prevent interface reaction.

6. The photovoltaic cell according to claim 5, characterized in that, The buffer layer (70) includes at least one of Al2O3, SiO2 or TiO2.

7. The photovoltaic cell according to claim 1, characterized in that, The phase change material layer (50) is disposed in the gap region (40) between the P-type region (20) and the N-type region (30).

8. The photovoltaic cell according to claim 1, characterized in that, The phase change material layer (50) is provided in all the gap regions (40) between the P-type region (20) and the N-type region (30).

9. The photovoltaic cell according to claim 1, characterized in that, The thickness of the phase change material layer (50) is 150nm-400nm.

10. A method for preparing a photovoltaic cell, characterized in that, The method for preparing the photovoltaic cell according to any one of claims 1-9 includes the following steps: Provide a silicon substrate (10); A P-type region (20) and an N-type region (30) are formed on the same surface of the silicon substrate (10), with a gap region (40) between the P-type region (20) and the N-type region (30). A phase change material layer (50) is formed in the gap region (40), and the phase change material layer (50) is in contact with the P-type region (20) and the N-type region (30) respectively; the phase change material layer (50) is in an insulating state below the phase change temperature to insulate the P-type region (20) from the N-type region (30); the phase change material layer (50) transforms into a conductive state when the phase change temperature is reached or exceeded to form a conductive path between the P-type region (20) and the N-type region (30); Metal electrodes (60) are formed on the P-type region (20) and the N-type region (30).

11. The method for preparing a photovoltaic cell according to claim 10, characterized in that, The step of forming the phase change material layer (50) in the gap region (40) includes: Using a VO2 ceramic target and a SnO2 ceramic target as dual sputtering sources, magnetron sputtering is performed in a mixed gas of argon and oxygen to deposit a tin-doped VO2 phase change material layer (50) in the gap region (40). After sputtering is completed, the VO2 ceramic target, SnO2 ceramic target and O2 are turned off, while Ar gas is retained, and the mixture is cooled to room temperature at a rate of 5℃-10℃ / min. The tin-doped VO2 phase change material layer (50) cooled to room temperature was subjected to high-temperature annealing in a nitrogen atmosphere; The phase transition temperature of the phase transition material layer (50) is controlled by adjusting the sputtering power of the SnO2 ceramic target to change the Sn element doping concentration.

12. The method for preparing a photovoltaic cell according to claim 10, characterized in that, After forming the phase change material layer (50), the method for preparing the photovoltaic cell further includes: According to the preset reverse voltage start threshold, the number and position of the phase change material layer (50) are adjusted by laser or etching, and the unwanted phase change material layer (50) is removed so that the P-type region (20) and the N-type region (30) can be selectively connected through the retained phase change material layer (50).

13. The method for preparing a photovoltaic cell according to claim 10, characterized in that, Before forming the P-type region (20) and the N-type region (30), the method for preparing the photovoltaic cell further includes: A buffer layer (70) is prepared on the surface of the silicon substrate (10), the buffer layer (70) being configured as an isolation layer between the silicon substrate (10) and the phase change material layer (50); the buffer layer (70) includes at least one of Al2O3, SiO2 or TiO2.