Method for manufacturing an image sensor and image sensor

By employing a single-fill process and adjusting deposition parameters, the uniformity and white spot performance issues of the isolation structure in CMOS image sensors were resolved, enabling more efficient image sensor fabrication.

CN123146002APending Publication Date: 2026-11-20SMARTSENS TECH (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510652084.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-20
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing CMOS image sensors suffer from problems such as poor trench uniformity, metal ion contamination of the reaction chamber due to repeated etching, and poor performance due to white spots when fabricating isolation structures.

Method used

A single-fill process is used to deposit filler oxides through HDP deposition. The deposition-etch ratio and RF power are adjusted to avoid trench opening blockage, reduce fluoride ion corrosion during etching, and use a filler auxiliary layer to improve deposition uniformity.

Benefits of technology

It effectively avoids metal ion contamination, reduces white spot performance defects, simplifies the process flow, and improves the uniformity and stability of the isolation structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146002A_ABST
    Figure CN123146002A_ABST
Patent Text Reader

Abstract

A manufacturing method of an image sensor and the image sensor, the manufacturing method comprising: providing a semiconductor substrate comprising a device functional layer; preparing a first trench in the device functional layer from a first surface of the semiconductor substrate; forming a filling auxiliary layer on the sidewall and bottom of the first trench; depositing a filling oxide in the first trench by using a HDP process, depositing the filling oxide to obtain an initial material layer based on the filling auxiliary layer by using a single filling process, and forming a first isolation structure based on the initial material layer; preparing a semiconductor device in the device functional layer from the first surface; wherein, in the process of forming the first isolation structure, the method further comprises adjusting the deposition of the filling oxide at the opening of the first trench based on a deposition etching ratio. The manufacturing method of the image sensor can effectively avoid the filling oxide from blocking the opening of the first trench in the deposition process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of image sensing technology, and in particular to a method for manufacturing an image sensor and an image sensor itself. Background Technology

[0002] Image sensors are a crucial component of digital cameras. Based on the different components, they can be divided into two main categories: CCD (Charge Coupled Device) and CMOS (Complementary Metal-Oxide Semiconductor).

[0003] With the continuous development of CMOS integrated circuit manufacturing processes, especially the design and manufacturing processes of CMOS image sensors (CIS), CMOS image sensors have gradually replaced CCD image sensors as the mainstream. Compared with CCD, CMOS image sensors have advantages such as low voltage, low power consumption, low cost, and high integration, and have important application value in fields such as machine vision, consumer electronics, high-definition surveillance, and medical imaging.

[0004] However, existing CMOS image sensors use STI (Sedimentation-Isolation Technology) to fabricate isolation structures, which involves multiple cycles (deposition + etching) to create the oxide filling within the STI. After creating trenches on the semiconductor substrate, multiple layers of material are deposited and filled. The trench openings gradually accumulate filler layers, causing the trenches to close prematurely. When the trenches are closed or about to close, nitrogen trifluoride (NF3) is used to etch the blocked trenches to reopen the openings. This process is repeated multiple times to complete the trench filling. During the deposition of multiple material layers in different types of trenches, there is a problem of poor uniformity. The deposition of each material layer varies in uniformity due to the different trench types. The design of multiple types of trenches in the image sensor layout is limited and difficult to arrange effectively. Since nitrogen trifluoride gas is used in the etching process, the fluoride ions generated by dissociation can etch the inner wall of the reaction chamber of the instrument, causing metal ions to be exposed in the reaction chamber. This allows metal ions to enter the oxide medium and / or the filler layer, resulting in poor white spot performance. Multiple etching processes are more likely to generate defects on the surface of the isolation structure.

[0005] The above background information is provided solely for the purpose of clearly and completely explaining the technical solutions of this invention and facilitating understanding by those skilled in the art. It should not be assumed that these solutions are known to those skilled in the art simply because they have been described in the background section of this invention. Summary of the Invention

[0006] In view of this, the present invention provides a method for manufacturing an image sensor that can effectively avoid the filling oxide during the deposition process from blocking the opening of the first trench.

[0007] A method for manufacturing an image sensor, the method comprising:

[0008] A semiconductor substrate is provided, the semiconductor substrate including a device functional layer;

[0009] A first trench is formed in the functional layer of the device from a first surface of the semiconductor substrate;

[0010] A filling auxiliary layer is formed on the sidewalls and bottom of the first trench;

[0011] Oxides were deposited and filled in the first trench using a deposition process.

[0012] Based on the filling auxiliary layer, the filling oxide is deposited in a single fill using the HDP deposition process to obtain an initial material layer, and a first isolation structure is formed based on the initial material layer;

[0013] Semiconductor devices are fabricated from the first surface in the device functional layer;

[0014] The formation of the first isolation structure also includes adjusting the deposition of the filling oxide at the opening of the first trench based on the deposition-etch ratio.

[0015] Optionally, the method for adjusting the deposition of the filling oxide at the opening of the first trench based on the deposition-etch ratio includes:

[0016] During the formation of the first isolation structure, the radio frequency power is adjusted to increase the sputtering rate.

[0017] Optionally, the radio frequency power is greater than 4000W; the deposition-etch ratio is less than 9.

[0018] Optionally, during the formation of the first isolation structure, the filling oxide is prevented from depositing and sealing at the opening of the first trench by adjusting the flow rate of the reactive gas forming the filling oxide; and / or by adjusting the flow rate of high-energy ions sputtering the filling oxide.

[0019] Optionally, the flow rate of the reactant gas is greater than 150 sccm; the flow rate of the high-energy ions is greater than or equal to 300 sccm.

[0020] Optionally, the filling auxiliary layer at the bottom of the first trench can be prevented from being sputtered through by adjusting the thickness of the filling auxiliary layer; the thickness of the filling auxiliary layer is greater than or equal to 400 Å.

[0021] Optionally, the thickness of the initial material layer is between 2 and 3 times the depth of the first trench; and / or, the first trench is formed based on the first mask layer, and the initial material layer is formed based on the first mask layer.

[0022] Optionally, after forming the semiconductor device, the process further includes the following steps:

[0023] An interconnect structure layer is formed on the first surface of the semiconductor substrate. The interconnect structure layer includes a dielectric layer and multiple interconnect layers. Each interconnect layer is used to realize electrical interconnection and lead-out between the semiconductor devices. And / or, a passivation layer is prepared on the second surface of the semiconductor substrate. Color filters and grids are prepared on the passivation layer. Lens arrays are prepared on or between the color filters.

[0024] Optionally, the semiconductor device includes a photoelectric conversion region, and after forming the photoelectric conversion region, the process further includes the following steps:

[0025] An isolation region is prepared in the functional layer of the device from the first surface to achieve isolation between the photoelectric conversion regions, and the isolation region corresponds to the preparation of the first trench.

[0026] Optionally, after forming the isolation area, the method further includes the following steps:

[0027] A second trench is prepared from the second surface of the semiconductor substrate opposite to the first surface, and a second isolation structure is prepared based on the second trench, the second isolation structure corresponding to the first trench.

[0028] Optionally, the first trench includes a plurality of first-type trenches and a plurality of second-type trenches, wherein the extension direction of the first-type trenches and the extension direction of the second-type trenches form an angle, wherein each of the first-type trenches and each of the second-type trenches is formed simultaneously based on the initial material layer, and the top of the lowest position of the initial material layer extends beyond the plane containing the upper surface of the semiconductor substrate.

[0029] Optionally, the semiconductor substrate includes a plurality of pixel units arranged in an array, each pixel unit including a photoelectric conversion region and a transmission control gate corresponding to the photoelectric conversion region, wherein:

[0030] Each of the transmission control gates is arranged facing each other to form a central opening region. The pixel unit also includes an output transistor located in the central opening region, a first floating diffusion node and a second floating diffusion node located on both sides of the output transistor and connected to the corresponding transmission control gate, and a device gate connected to at least one floating diffusion node.

[0031] The output transistor is located in the first type of trench region, the device gate is located in the second type of trench region, and the output transistor corresponds to the intersection region of the first type of trench and the second type of trench, and the pixel unit is formed with the output transistor as the center.

[0032] Optionally, when forming a second isolation structure from the second surface of the semiconductor substrate, the second isolation structure is disposed at least around the pixel unit and spans the first type trench and / or the second type trench;

[0033] And / or, each of the pixel units is arranged in an array in rows and columns, and the arrangement of the first type of trench and the second type of trench includes: the first type of trench connects and penetrates the pixel units of each corresponding column, and the second type of trench is arranged at intervals in the row direction between each of the pixel unit columns.

[0034] This application also relates to an image sensor, which is manufactured by the above-described method for manufacturing an image sensor, and the image sensor includes:

[0035] A semiconductor substrate, the semiconductor substrate including a device functional layer;

[0036] The first trench extends from the first surface of the semiconductor substrate into the functional layer of the device;

[0037] A filling auxiliary layer is formed on the sidewalls and bottom of the first trench;

[0038] The first isolation structure is formed in the first trench.

[0039] The first isolation structure includes a filled oxide and is an integral structure;

[0040] A semiconductor device extending from the first surface into the functional layer of the device.

[0041] Optionally, the first trench includes a plurality of first-type trenches and a plurality of second-type trenches, and the extension direction of the first-type trenches and the extension direction of the second-type trenches form an angle. The semiconductor substrate includes a plurality of pixel units arranged in an array, each pixel unit including a photoelectric conversion region and a transmission control gate corresponding to the photoelectric conversion region, wherein:

[0042] Each of the transmission control gates is arranged facing each other to form a central opening region. The pixel unit also includes an output transistor located in the central opening region, a first floating diffusion node and a second floating diffusion node located on both sides of the output transistor and connected to the corresponding transmission control gate, and a device gate connected to at least one floating diffusion node.

[0043] The output transistor is located in the first type of trench region, the device gate is located in the second type of trench region, and the output transistor corresponds to the intersection region of the first type of trench and the second type of trench, and the pixel unit is formed with the output transistor as the center.

[0044] Optionally, when forming a second isolation structure from the second surface of the semiconductor substrate, the second isolation structure is disposed at least around the pixel unit and spans the first type trench and / or the second type trench;

[0045] And / or, each of the pixel units is arranged in an array in rows and columns, and the arrangement of the first type of trench and the second type of trench includes: the first type of trench connects to and passes through the pixel units of each corresponding column, and the second type of trench is arranged at intervals in the row direction between each column of pixel units.

[0046] The image sensor fabrication method of the present invention employs a single-pass filling process to deposit filling oxide in the first trench, thereby forming the first isolation structure in one step. This effectively avoids the filling oxide from blocking the opening of the first trench during the deposition process, thus eliminating the need for subsequent etching of the blocked first trench with nitrogen trifluoride (NF3). This effectively prevents fluoride ion corrosion of the metal cavity wall of the HDP device, not only preventing damage to the components of the HDP device but also preventing the metal ions from diffusing with the high-energy plasma gas into the filling auxiliary layer and / or filling oxide. This significantly optimizes white point performance and greatly reduces the problem of defects on the surface of the first isolation structure. The design of this application also facilitates the design of different types of isolation and the formation of different types of isolation combinations to meet imaging requirements. Attached Figure Description

[0047] Figures 1 to 12 This is a flowchart illustrating the method for manufacturing the image sensor of this application.

[0048] Figure 13 This is a partial schematic diagram of the formation of the initial material layer in the first trench of this application.

[0049] Figure 14 This is a partial pixel diagram of the semiconductor substrate of this application.

[0050] Figure 15 yes Figure 14 The diagram shows a schematic of the pixel circuit corresponding to the pixel unit.

[0051] Figures 16a to 16c This is a schematic diagram of the deposition and etching process using existing HDP equipment.

[0052] Figure 17This is a coordinate graph comparing the temperature curves of the semiconductor deposition process in this application with those in the comparative example.

[0053] Figure 18 This is a basic structural block diagram of the image sensor of this application.

[0054] Figure 19 This is a schematic diagram of another pixel unit in the image sensor of this application. Detailed Implementation

[0055] The following specific embodiments illustrate the implementation of this application. Those skilled in the art can easily understand other advantages and effects of this application from the content disclosed in this specification.

[0056] In the following description, reference is made to the accompanying drawings, which illustrate several embodiments of the present application. It should be understood that other embodiments may also be used, and changes in mechanical composition, structure, electrical and operational aspects may be made without departing from the spirit and scope of the present application. The following detailed description should not be considered limiting, and the terminology used herein is for describing particular embodiments only and is not intended to limit the present application.

[0057] Although the terms first, second, etc., are used in some instances to describe various elements herein, these elements should not be limited by these terms. They are used only to distinguish one element from another.

[0058] Furthermore, as used herein, the singular forms “a,” “an,” and “the” are intended to include the plural forms as well, unless the context indicates otherwise. It should be further understood that the terms “comprising,” “including,” indicate the presence of a feature, step, operation, element, component, item, kind, and / or group, but do not exclude the presence, occurrence, or addition of one or more other features, steps, operations, elements, components, items, kinds, and / or groups. The terms “or” and “and / or” as used herein are interpreted as inclusive, or mean any one or any combination thereof. Thus, “A, B, or C” or “A, B, and / or C” means “any one of: A; B; C; A and B; A and C; B and C; A, B, and C.” Exceptions to this definition arise only when combinations of elements, functions, steps, or operations are inherently mutually exclusive in some way.

[0059] Figures 1 to 12 This is a flowchart illustrating the method for fabricating the image sensor of this application. Please refer to it. Figures 1 to 12 The method for manufacturing the image sensor in this application includes:

[0060] A semiconductor substrate 10 is provided, the semiconductor substrate 10 including a device functional layer, such as... Figure 1 As shown;

[0061] A first trench 101 is fabricated in the device functional layer from the first surface 111 of the semiconductor substrate 10, such as Figure 3 As shown; wherein, the semiconductor substrate 10 has a first surface 111 and a second surface 112 opposite to each other;

[0062] A filling auxiliary layer 12 is formed on the sidewalls and bottom of the first trench 101, such as Figure 4 As shown;

[0063] Oxide 131 was deposited and filled in the first trench 101 using a deposition process.

[0064] An initial material layer is obtained by depositing a filled oxide 131 based on the filler layer 12 using a single-fill process, and a first isolation structure 13 is formed based on the initial material layer, such as... Figure 5 and Figure 6 As shown, the deposition process is HDP (high-density plasma-assisted chemical vapor deposition).

[0065] Semiconductor devices are fabricated in the device functional layer from the first surface 111;

[0066] The formation of the first isolation structure 13 includes a step of adjusting the deposition of the filling oxide 131 at the opening of the first trench 101 based on the deposition-etch ratio. In this embodiment, the deposition-etch ratio = total deposition rate / sputtering rate = (net deposition rate + sputtering rate) / sputtering rate.

[0067] The image sensor fabrication method of this application employs a single-fill process to deposit filling oxide 131 in the first trench 101, thereby forming the first isolation structure 13 in one step. This effectively prevents the filling oxide 131 from blocking the opening of the first trench 101 during the deposition process, eliminating the need for subsequent etching of the blocked first trench 101 with nitrogen trifluoride (NF3). This effectively prevents fluoride ion corrosion of the metal cavity wall of the HDP device, not only avoiding damage to the components of the HDP device but also preventing the metal ions from diffusing with the high-energy plasma gas into the filling auxiliary layer 12 and / or the filling oxide 131, thus mitigating the entry of metal ions into the substrate (wafer) and significantly optimizing white spot performance. At the same time, the problem of defects on the surface of the first isolation structure 13 is greatly reduced. The deposition state of the filling oxide at the opening of the first trench is adjusted based on the deposition-etch ratio, promoting the formation of the initial material layer in a single-fill process.

[0068] Optionally, the method for adjusting the deposition state of the filling oxide 131 at the opening of the first trench 101 based on the deposition-etch ratio includes: adjusting the radio frequency power and increasing the sputtering rate during the formation of the first isolation structure 13. In one implementation, increasing the radio frequency power increases the sputtering rate and reduces the deposition-etch ratio. The high power of the HDP process not only reduces the porosity of the first isolation structure 13, but also lowers the overall deposition temperature compared to existing processes, further reducing the diffusion of metal ions in the first isolation structure 13.

[0069] Optionally, the radio frequency power can be controlled to be greater than 4000W, for example, 4200W, 4400W, 4500W, 4600W, 4700W, or 4800W, but is not limited to this.

[0070] Optionally, the deposition-etch ratio can be controlled to be less than 9, for example, 7.5, 8.2, 8.5, 8.7, or 8.9. This facilitates the preparation of the initial material layer through a single-pass filling process.

[0071] Optionally, during the formation of the first isolation structure 13, the deposition and sealing of the filling oxide 131 at the opening of the first trench 101 can be avoided by adjusting the flow rate of the reactive gas forming the filling oxide 131 and / or adjusting the flow rate of the high-energy ions sputtering the filling oxide 131. In one implementation, increasing the flow rate of the reactive gas forming the filling oxide 131 and / or increasing the flow rate of the high-energy ions sputtering the filling oxide 131 facilitates the preparation of the initial material layer through a single filling process.

[0072] In this embodiment, the reaction gas is SiH4 and / or O2; the high-energy ions used for sputtering are H2.

[0073] Optionally, the flow rate of the reactant gas is greater than 150 sccm, for example 152 sccm, 155 sccm, 157 sccm, or 160 sccm; and the flow rate of the high-energy ions is greater than or equal to 300 sccm, for example 310 sccm, 315 sccm, or 320 sccm.

[0074] Optionally, the filling auxiliary layer 12 at the bottom of the first trench 101 can be prevented from being sputtered through by adjusting the thickness of the filling auxiliary layer 12; the thickness of the filling auxiliary layer 12 is greater than or equal to 400 Å, for example, it can be 420 Å, 450 Å, 480 Å, 500 Å, or 520 Å.

[0075] In this application, based on the formation of the filler layer 12, an initial material layer is formed by a single-fill process. The filler layer 12 includes, but is not limited to, a silicon oxide layer, which can be formed on the inner surface of the trench using processes such as thermal oxidation. Since the HDP process of this application increases the RF power, reactive gas flow rate, and sputtering high-energy ion flow rate, the filler layer 12 is beneficial for the implementation of the single-fill process. Furthermore, in order to avoid sputtering through the filler layer 12, the thickness of the filler layer 12 is adjusted.

[0076] Optionally, Figure 13 This is a partial schematic diagram of the formation of the initial material layer in the first trench of this application, as shown below. Figure 13 As shown, the thickness h of the initial material layer is between 2 and 3 times the depth D of the first trench 101. In a specific example, the depth D of the first trench 101 is 2000 Å, 2200 Å, 2500 Å, 2800 Å, etc., and correspondingly, the thickness h of the initial material layer is 5200 Å, 5500 Å, 5800 Å, 6000 Å, etc. In this application, a single-fill process is used to form the initial material layer, and then the first isolation structure 13 is further formed. The single-fill process means that the initial material layer is formed in one step after adjusting the deposition parameters. The initial material layer fills the first trench 101 and extends to the upper surface (first surface 111) of the semiconductor substrate surrounding the first trench 101. Using the method of this application, the single trench filling can improve the problem of unevenness of the material layers when multiple material layers are formed to fill each first trench 101, which is beneficial to improving the performance of the isolation structure. Furthermore, setting the thickness h of the initial material layer to be between 2 and 3 times the depth D of the first trench 101 is beneficial to improving the structural stability.

[0077] In one example, the method for forming the first trench 101 may be:

[0078] First, a first mask layer 21 is formed on the first surface 111 of the semiconductor substrate 10, such as Figure 2 As shown; then etching is performed based on the first mask layer 21 to form the first trench 101, as follows. Figure 3 As shown.

[0079] Optionally, the material of the first mask layer 21 includes, but is not limited to, a hard mask layer, such as silicon nitride.

[0080] Optionally, when forming the filling auxiliary layer 12 in the first trench 101, the filling auxiliary layer 12 may be formed on the sidewalls and bottom of the first trench 101 based on the first mask layer 21 while retaining the first mask layer 21.

[0081] Optionally, the filler layer 12 may include, but is not limited to, a silicon oxide layer on the surface of the trench formed by a thermal oxidation process, and may also facilitate subsequent ion implantation processes based on the filler layer 12.

[0082] Optionally, the step of forming the first isolation structure 13 after forming the filling auxiliary layer 12 includes:

[0083] First, the filling auxiliary layer 12 of the inner wall of the first trench 101 is exposed;

[0084] Next, an initial material layer is deposited on the first trench 101 and the surrounding semiconductor substrate 10, i.e., a filling oxide 131 is deposited, including but not limited to a silicon oxide layer, such as... Figure 5 As shown;

[0085] Finally, the initial material layer is subjected to chemical mechanical polishing (CMP) to obtain the first isolation structure 13. In this embodiment, the first isolation structure 13 can be a shallow trench isolation structure (STI).

[0086] Optionally, a first trench 101 is formed based on the first mask layer 21, and an initial material layer is formed based on the first mask layer 21. The initial material layer is formed while retaining the first mask layer 21; that is, a first mask layer 12 exists before the first isolation structure 13 is formed by chemical mechanical polishing. The first isolation structure 13 can be further formed based on the first mask layer 12 after the first trench 101 is formed based on the first mask layer 12. The first mask layer 12 can serve as a stop layer for chemical mechanical polishing, which helps improve the stability of the process and the quality of the final obtained first isolation structure 13.

[0087] Optionally, after forming the semiconductor device, the following steps are also included:

[0088] An interconnect structure layer 16 is formed on the first surface 111 of the semiconductor substrate 10. The interconnect structure layer 16 includes a dielectric layer 161 and multiple interconnect layers 162. Each interconnect layer 162 is used to realize electrical interconnection and lead-out between semiconductor devices, such as... Figure 9 As shown.

[0089] Optionally, the semiconductor device includes the photoelectric conversion region 14 and the corresponding transistors of the pixel circuit of the image sensor. The photoelectric conversion region 14 realizes photoelectric conversion and is a component of the photoelectric conversion element. Of course, it may also include other CIS pixel circuit devices in the prior art to realize the functions of image acquisition and subsequent imaging. For example, the pixel circuit may include transmission transistors, etc.

[0090] Optionally, the steps for forming the photoelectric conversion region 14 include:

[0091] First, a second mask layer 22 is formed on the first surface 111 of the semiconductor substrate 10 where the first isolation structure 13 is formed. Then, ion implantation is performed based on the second mask layer 22 to form an initial doped region. The doping type is described using N-type as an example. Figure 7 As shown;

[0092] Next, the initial doped region is heat-treated to form the photoelectric conversion region 14. Specifically, the heat treatment annealing temperature is between 900℃ and 1200℃, such as 1050℃, 1100℃, or 1150℃ for heat treatment of the initial doped region.

[0093] Optionally, after forming the photoelectric conversion region 14, the following steps are also included:

[0094] An isolation region 15 is fabricated in the functional layer of the device from the first surface 111 to achieve isolation between the photoelectric conversion regions 14. The isolation region 15 is fabricated corresponding to the first trench 101, such as... Figure 8 As shown.

[0095] Optionally, the isolation region 15 can be an ion-doped isolation region, with the doping type being opposite to that of the photoelectric conversion region 14, to achieve the isolation function. In this embodiment, it is a P-type doped ion.

[0096] In one example, the isolation region 15 can be formed by ion doping. For example, the steps for forming the isolation region 15 may be: first, forming a third mask layer 23 on the first surface 111 of the semiconductor substrate 10, and then performing ion implantation based on the third mask layer 23 to form the isolation region 15. It should be noted that the materials of the various mask layers in this embodiment can be selected with reference to existing CIS fabrication processes.

[0097] In one example, the semiconductor substrate 10 includes a semiconductor substrate and an epitaxial layer, which serves as a functional layer of the device. Additionally, the isolation region 15 extends through the functional layer. Of course, in other implementations, the depth of the isolation region 15 can be set according to the location of the photoelectric conversion region 14 or actual needs for isolation, such as the bottom of the isolation region 15 being closer to the first surface 111 than the photoelectric conversion region 14.

[0098] Optionally, after forming the isolation zone 15, the following steps are also included:

[0099] A second trench 102 is fabricated from the second surface 112 of the semiconductor substrate 10, which is opposite to the first surface 111, and a second isolation structure 17 is fabricated based on the second trench 102. The second isolation structure 17 corresponds to the first trench 101, such as... Figure 10 and Figure 11 As shown.

[0100] Specifically, the aforementioned fabricated structure is flipped over, and subsequent processes are performed from the second surface 112 of the semiconductor substrate 10. This may involve thinning the semiconductor substrate 10 after flipping, for example, thinning it to the location with the photoelectric conversion region 14. In one implementation, it may involve thinning it to the epitaxial layer.

[0101] In one implementation of forming the second trench 102, firstly, a patterned mask for the deep trench isolation structure is formed using a photolithography process; then, an etching process is performed to fabricate the deep trench isolation structure in the back-side deep trench isolation structure region defined by the photolithography process, resulting in the second trench 102; next, a filling material layer, including but not limited to silicon oxide, is prepared in the second trench 102 to obtain the second isolation structure 17. The second isolation structure 17 can be a back-side deep trench isolation structure (BDTI), and the material can be silicon oxide, and may further include a negative charge layer on the inner wall of the trench.

[0102] Optionally, the structure formed by the combination of the first isolation structure 13, the isolation region 15, and the second isolation structure 17 can achieve the function of device isolation as required. For example, the position of the first trench 101 corresponding to the isolation region 15 can mean that the first trench 101 is completely located within the range of the isolation region 15, that is, the periphery of the first trench 101 is the isolation region 15, or the edge of the first trench 101 is aligned with the edge of the isolation region 15.

[0103] Optionally, after forming the second isolation structure 17, the following steps are also included:

[0104] A passivation layer 18 is prepared on the second surface 112 of the semiconductor substrate 10. The material of the passivation layer 18 includes, but is not limited to, HK materials, such as hydroxyl oxide. Based on the passivation layer 18, it is beneficial to achieve material layer planarization and repair of process damage on the second surface 112.

[0105] A color filter 19 and a grid are fabricated on the passivation layer 18; the color filter can be an RGGB Bayer array, or an RGBIR array, etc.

[0106] A lens array 20 is prepared on or between color filters 19.

[0107] Optionally, Figure 14 This is a partial pixel schematic diagram of the semiconductor substrate of this application, as shown below. Figure 14As shown, the first trench 101 includes multiple first-type trenches 1011 and multiple second-type trenches 1012, with an angle between the extension directions of the first-type trenches 1011 and the extension directions of the second-type trenches 1012. Each first-type trench 1011 and each second-type trench 1012 is formed simultaneously based on an initial material layer, and the top of the lowest position of the initial material layer extends beyond the plane containing the upper surface (first surface 111) of the semiconductor substrate. The angle between the first-type trenches 1011 and the second-type trenches 1012 indicates a directional difference during their internal filling process. Using a single-pass filling method during deposition improves the overall uniformity of the trench filling, resulting in better uniformity compared to multiple-pass deposition using multiple material layers, thus optimizing the performance of the filling structure.

[0108] Optionally, Figure 15 This is a schematic diagram of the pixel circuit corresponding to the pixel unit of this application. Figure 13 The pixel units within the dashed box, such as Figure 12 , Figure 14 and Figure 15 As shown, the semiconductor substrate 10 includes a plurality of pixel units arranged in an array. Each pixel unit includes at least one photoelectric conversion region 14 (corresponding to PD1 to PD4) and a transmission control gate (corresponding to Tx1 to Tx4) corresponding to the photoelectric conversion region 14.

[0109] In one example, the pixel unit includes four photoelectric conversion regions 14 (corresponding to PD1 to PD4) and four transmission control gates (corresponding to Tx1 to Tx4) corresponding to the photoelectric conversion regions 14 (corresponding to PD1 to PD4).

[0110] The transmission control gates (corresponding to Tx1 to Tx4) are arranged facing each other to form a central opening region. The pixel unit also includes an output transistor SF located in the central opening region, a first floating diffusion node FD1 and a second floating diffusion node FD2 located on both sides of the output transistor SF and connected to the corresponding transmission control gates, and a device gate connected to at least one floating diffusion node. Figure 14 , Figure 15 The image shows the gate RST of the reset transistor connected to FD1. The output transistor SF is located in the first type trench 1011 region, the device gate is located in the second type trench 1012 region, and the output transistor SF corresponds to the intersection region of the first type trench 1011 and the second type trench 1012. The pixel unit is formed with the output transistor SF as the center. Figure 14(The area defined by the dashed line). The layout of the first type of trench 1011 and the second type of trench 1012 can be flexibly designed, thereby optimizing the pixel layout design of the image sensor and forming a symmetrical pixel unit. With the output transistor SF as the center, the symmetry of the signal can be improved, and the quality of the acquired image can be enhanced.

[0111] Optionally, when the second isolation structure 17 is formed from the second surface 112 of the semiconductor substrate, the second isolation structure 17 is arranged at least around the pixel unit and spans the first type trench 1011 and / or the second type trench 1012. That is, in this example, the second isolation structure 17 is at least disposed around the pixel unit, effectively preventing crosstalk between pixel units. Furthermore, the second isolation structure 17 has columns at the gaps that correspond vertically with the first isolation structure 13 formed by the first type trench 1011 and the second type trench 1012. The formation of different types of isolation is beneficial for the acquisition of different signals by the image sensor. For example, effective isolation between pixels is formed based on the periphery, while signal overflow can occur within the pixel unit.

[0112] Optionally, the pixel units are arranged in an array in rows and columns. The arrangement of the first type of trench 1011 and the second type of trench 1012 includes: the first type of trench 1011 connects to and passes through the pixel units in each corresponding column, and the second type of trench 1012 is spaced apart in the row direction between the columns of pixel units. In this example, the first type of trench 1011 and the second type of trench 1012 are perpendicular to each other, forming a corresponding pixel array.

[0113] To further illustrate the effectiveness of this application, a comparative example based on the prior art and a specific embodiment based on the technical solution of this application are provided. The parameters of the comparative example are: RF power 1890W, SiH4 flow rate 55sccm, high-energy ion H2 flow rate 130sccm, initial material layer of the first isolation structure formed by a five-stage deposition and etching process with a single deposition depo thickness of 730Å, deposition-etch ratio 18, and silicon oxide thickness of the auxiliary filling layer 240Å. Correspondingly, the specific embodiment provided according to the method of this application has the following parameters: RF bias power 4600W, SiH4 flow rate 155sccm, H2 flow rate 300sccm, deposition thickness 4050Å, deposition-etch ratio 8.9, and silicon oxide thickness of the auxiliary filling layer 400Å.

[0114] in, Figures 16a to 16c This is a schematic diagram of the deposition and etching process using existing HDP equipment. Please refer to it. Figures 16a to 16cIn the comparative example, a five-cycle (Depo and Sputter+Eeth) process was used to fabricate the filling oxide within the STI. After fabricating trenches on the semiconductor substrate, an oxide dielectric layer was formed at the bottom and sidewalls of the trench using the HDP process with an applied RF power of 1830W. Then, a filler layer was deposited on the oxide dielectric. Due to the applied RF power of 1890W, the filler layer gradually accumulated at the opening of the trench, causing the trench to close prematurely. When the trench was closed or about to close, nitrogen trifluoride (NF3) was used to etch the blocked trench to open the trench opening. Then, the Depo+Eth process was repeated multiple times (e.g., five times) to complete the trench filling. Finally, the filler layer outside the trench was removed to form an isolation structure.

[0115] Please refer to Figures 16a to 16c Because the etching process uses nitrogen trifluoride (NF3) gas, the resulting fluoride ions F... - It will etch the inner wall of the reaction chamber of the machine, causing metal ions M + Exposed to the reaction chamber, thus allowing metal ions M + Infiltration into the oxide medium and / or filler layer leads to poor white spot performance, and repeated etching makes it easier to generate defects on the surface of the isolation structure. To address these drawbacks, the image sensor fabrication method of this application eliminates the need to etch the first sealing trench 101 with nitrogen trifluoride (NF3), effectively preventing fluoride ion corrosion of the metal cavity wall of the HDP device. This not only avoids damage to HDP device components but also prevents corrosion from metal ions. + As high-energy plasma gas diffuses into the filler layer 12 and / or filler oxide 131, the metal ion M is relieved. + By penetrating into the interior of the substrate (wafer), white spot performance is significantly optimized, while the problem of defects on the surface of the first isolation structure 13 is greatly reduced.

[0116] It is worth mentioning that, compared with the design of this application which controls the RF power to be greater than 4000W, such as RF power of 4200W, 4400W, 4500W, 4600W, 4700W, and 4800W, but is not limited to this, in the comparative example, the RF power applied by the HDP process is 1890W. During the Depo (semiconductor deposition process), the first trench 101 will be sealed prematurely. Therefore, after the opening of the first trench 101 is blocked, nitrogen trifluoride (NF3) is used to etch the blocked first trench 101 to open the opening of the first trench 101. Then, the Depo+Etch process is repeated multiple times (a total of five times) to complete the filling of the first trench 101. Compared to the design in this application where the controlled deposition-etch ratio is less than 9 (e.g., 7.5, 8.2, 8.5, 8.7, 8.9), the HDP process in the comparative example has a deposition-etch ratio of 18, requiring five depo+etch cycles to fill the first trench 101, resulting in a complex process and high manufacturing cost. In contrast, the flow rate of the reactive gas in this application is greater than 150 (e.g., 152, 155, 157, 160), and the flow rate of the high-energy ions is greater than or equal to 300 (e.g., 310, 315, 320). In the comparative example, the HDP process provides a SiH4 reactive gas flow rate of 55, which is much lower than the reactive gas flow rate in this example, and a H2 high-energy ion flow rate of 130, which is much lower than the high-energy ion flow rate in this example. Therefore, the above designs are difficult to fill the first trench 101 in a single deposition. Furthermore, based on the formation of the filler layer 12, this application uses a single-fill process to form the initial material layer. The filler layer 12 includes, but is not limited to, a silicon oxide layer, which can be formed on the inner surface of the trench using processes such as thermal oxidation. Since the HDP process of this application increases the radio frequency power, the reactive gas flow rate, and the sputtering high-energy ion flow rate, the filler layer 12 is beneficial for the implementation of the single-fill process. Furthermore, in order to avoid sputtering through the filler layer 12, the thickness of the filler layer 12 is increased from the original 240 Å (the above comparative example) to greater than or equal to 400 Å.

[0117] Further, see Figure 17 , Figure 17 This is a coordinate graph comparing the temperature curves of the semiconductor deposition process in this application with those in the comparative example. The horizontal axis represents the process time, and the vertical axis represents the wafer temperature. Reference numeral ① indicates the temperature curve of the semiconductor deposition process in this application, and reference numeral ② indicates the temperature curve of the semiconductor deposition process in the comparative example. The graph shows that the semiconductor deposition process in this application operates at a lower temperature when fabricating the isolation structure than the semiconductor deposition process in the comparative example, which helps to reduce the amount of metal ions (M). + It diffuses into the interior of the substrate (wafer).

[0118] like Figure 12As shown, this application also relates to an image sensor, which is manufactured using the above-described image sensor manufacturing method. The corresponding structural description can be found above and will not be repeated here.

[0119] The image sensor includes:

[0120] Semiconductor substrate 10, semiconductor substrate 10 includes a device functional layer;

[0121] The first trench 101 extends from the first surface 111 of the semiconductor substrate 10 into the device functional layer;

[0122] A filling auxiliary layer 12 is formed on the sidewalls and bottom of the first trench 101;

[0123] The first isolation structure 13 is formed in the first trench 101.

[0124] The first isolation structure 13 includes a filling oxide 131 and is an integral structure;

[0125] A semiconductor device extends from the first surface 111 into the device functional layer.

[0126] Optionally, such as Figure 12 , Figure 14 and Figure 15 As shown, the first trench 101 includes a plurality of first-type trenches 1011 and a plurality of second-type trenches 1012, and the extension direction of the first-type trenches 1011 and the extension direction of the second-type trenches 1012 form an angle. The semiconductor substrate 10 includes a plurality of pixel units arranged in an array. Each pixel unit includes a photoelectric conversion region 14 and a transmission control gate (corresponding to Tx1 to Tx4) corresponding to the photoelectric conversion region 14, wherein:

[0127] Each transmission control gate (corresponding to Tx1 to Tx4) is arranged facing each other to form a central opening region. The pixel unit also includes an output transistor SF located in the central opening region, a first floating diffusion node FD1 and a second floating diffusion node FD2 located on both sides of the output transistor SF and connected to the corresponding transmission control gates, and a device gate connected to at least one floating diffusion node. Figure 14 , Figure 15 The image shows the gate (RST) of the reset transistor connected to FD1;

[0128] Furthermore, the output transistor SF is located in the first type trench 1011 region, the device gate is located in the second type trench 1012 region, and the output transistor SF corresponds to the intersection region of the first type trench 1011 and the second type trench 1012, and the pixel unit is formed with the output transistor SF as the center. Figure 14 (The area defined by the dashed line).

[0129] Optionally, when the second isolation structure 17 is formed from the second surface 112 of the semiconductor substrate 10, the second isolation structure 17 is arranged at least around the pixel unit and spans the first type trench 1011 and / or the second type trench 1012.

[0130] And / or, each pixel unit is arranged in an array in rows and columns. The arrangement of the first type of trench 1011 and the second type of trench 1012 includes: the first type of trench 1011 connects and penetrates the pixel units of each corresponding column, and the second type of trench 1012 is arranged at intervals in the row direction between each column of pixel units.

[0131] Optionally, Figure 18 This is a basic structural block diagram of the image sensor of this application, as shown below. Figure 18 As shown, the image sensor includes a readout circuit and a control circuit connected to the pixel array. A functional logic unit is connected to the readout circuit, and the readout circuit and control circuit are connected to a status register to control the pixel array. The pixel array includes multiple pixels (P1, P2, P3) arranged in rows (R1, R2, R3…Ry) and columns (C1, C2, C3…Cx). The pixel signals output by the pixel array are output to the readout circuit via column lines. In a specific implementation, the readout circuit may include an analog-to-digital converter (ADC) and other circuits. In some applications, after the pixels acquire image data, they are read out using the readout mode specified by the status register and then transmitted to the functional logic unit.

[0132] In some applications, the status register may contain a programmed selection system to determine whether the readout system uses rolling shutter or global shutter exposure. The functional logic unit may store raw image data or image data after image processing. In some implementations, the readout circuitry may read one row of image data at a time along the readout column lines; other methods may also be used. The operation of the control circuitry can be determined by the current settings in the status register. For example, the control circuitry generates a shutter signal to control image acquisition. In some applications, this shutter signal may be a global shutter signal, allowing all pixels in the pixel array to acquire their image data simultaneously through a single acquisition window. In other applications, this shutter signal may be a rolling shutter signal, allowing pixels in each row of the pixel array to be continuously exposed and read through the acquisition window.

[0133] Figure 19 This is a schematic diagram of another pixel unit in the image sensor of this application, as shown below. Figure 19As shown, each pixel unit includes a photoelectric conversion region 14 (e.g., a photodiode) and pixel circuitry (as shown by the transistor within the dashed box in the figure). The photodiode can be a buried photodiode (PPD) used in current image sensors. In one application example, the pixel circuitry includes a reset transistor (RST), a source follower transistor (SF), and a pixel select transistor (RS), connected to, for example... Figure 19 The diagram shows a transfer transistor (TX) and a photodiode. In some applications, the pixel circuitry is stacked, including a reset transistor, a source follower transistor, and a pixel select transistor on a first circuit chip, and a transfer transistor on a second circuit chip, where the photodiode is connected to other transistors on the first circuit chip via the transfer transistor. In further applications, the pixel circuitry may also include a gain control transistor (DCG) connected between the floating diffusion region (FD) and the reset transistor. During operation, the photoelectric conversion element generates photocharge in response to incident light during exposure. The transfer transistor is connected to a transfer signal that controls the transfer transistor to transfer the accumulated charge in the photoelectric conversion element to the floating diffusion region. The reset transistor is connected between the power supply voltage and the floating diffusion region, and in response to a reset signal, resets the sensor pixel circuitry (e.g., discharges or charges the floating diffusion region and the photodiode to the current voltage). The floating diffusion region is connected to the gate of the source follower transistor, which is connected between the power supply voltage and the pixel select transistor, responding to and outputting the potential of the floating diffusion region. The pixel select transistor is connected to the source follower transistor and the bit line, and in response to a pixel select control signal, performs pixel selection readout and outputs it to the readout column.

[0134] The above embodiments are merely illustrative of the principles and effects of this application and are not intended to limit this application. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in this application should still be covered by the claims of this application.

Claims

1. A method for manufacturing an image sensor, characterized in that, The manufacturing method includes: A semiconductor substrate is provided, the semiconductor substrate including a device functional layer; A first trench is formed in the functional layer of the device from a first surface of the semiconductor substrate; A filling auxiliary layer is formed on the sidewalls and bottom of the first trench; Oxides were deposited and filled in the first trench using a deposition process. Based on the filling auxiliary layer, the filling oxide is deposited in a single fill using the HDP deposition process to obtain an initial material layer, and a first isolation structure is formed based on the initial material layer; Semiconductor devices are fabricated from the first surface in the device functional layer; The formation of the first isolation structure also includes adjusting the deposition of the filling oxide at the opening of the first trench based on the deposition-etch ratio.

2. The method for manufacturing an image sensor as described in claim 1, characterized in that, The method for adjusting the deposition of the filling oxide at the opening of the first trench based on the deposition-etch ratio includes: During the formation of the first isolation structure, the radio frequency power is adjusted to increase the sputtering rate.

3. The method for manufacturing an image sensor as described in claim 2, characterized in that, The radio frequency power is greater than 4000W; the deposition-etch ratio is less than 9.

4. The method for manufacturing an image sensor as described in claim 1, characterized in that, During the formation of the first isolation structure, the filling oxide is prevented from depositing and sealing at the opening of the first trench by adjusting the flow rate of the reactive gas forming the filling oxide and / or adjusting the flow rate of high-energy ions sputtering the filling oxide.

5. The method for manufacturing an image sensor as described in claim 4, characterized in that, The flow rate of the reactant gas is greater than 150 sccm; the flow rate of the high-energy ions is greater than or equal to 300 sccm.

6. The method for manufacturing an image sensor as described in claim 1, characterized in that, The filling auxiliary layer at the bottom of the first trench is prevented from being sputtered through by adjusting its thickness; the thickness of the filling auxiliary layer is greater than or equal to 400 Å.

7. The method for fabricating an image sensor as described in claim 1, characterized in that, The thickness of the initial material layer is between 2 and 3 times the depth of the first trench; and / or, the first trench is formed based on the first mask layer, and the initial material layer is formed based on the first mask layer.

8. The method for fabricating an image sensor as described in claim 1, characterized in that, The process after forming the semiconductor device further includes the following steps: An interconnect structure layer is formed on the first surface of the semiconductor substrate. The interconnect structure layer includes a dielectric layer and multiple interconnect layers. Each interconnect layer is used to realize electrical interconnection and lead-out between the semiconductor devices. And / or, a passivation layer is formed on the second surface of the semiconductor substrate, color filters and grids are formed on the passivation layer, and a lens array is formed on or between the color filters.

9. The method for fabricating an image sensor as described in claim 1, characterized in that, The semiconductor device includes a photoelectric conversion region, and after forming the photoelectric conversion region, the following steps are further included: An isolation region is prepared in the functional layer of the device from the first surface to achieve isolation between the photoelectric conversion regions, and the isolation region corresponds to the preparation of the first trench.

10. The method for manufacturing an image sensor as described in claim 9, characterized in that, After the isolation area is formed, the following steps are also included: A second trench is prepared from the second surface of the semiconductor substrate opposite to the first surface, and a second isolation structure is prepared based on the second trench, the second isolation structure corresponding to the first trench.

11. The method for manufacturing an image sensor as described in any one of claims 1 to 10, characterized in that, The first trench includes a plurality of first-type trenches and a plurality of second-type trenches, wherein the extension direction of the first-type trenches and the extension direction of the second-type trenches form an angle, wherein: Based on the initial material layer, both the first type of trench and the second type of trench are formed simultaneously, and the top of the lowest position of the initial material layer corresponds to the plane where the upper surface of the semiconductor substrate is located.

12. The method for manufacturing an image sensor as described in claim 11, characterized in that, The semiconductor substrate includes a plurality of pixel units arranged in an array, each pixel unit including a photoelectric conversion region and a transmission control gate corresponding to the photoelectric conversion region, wherein: Each of the transmission control gates is arranged facing each other to form a central opening region. The pixel unit also includes an output transistor located in the central opening region, a first floating diffusion node and a second floating diffusion node located on both sides of the output transistor and connected to the corresponding transmission control gate, and a device gate connected to at least one floating diffusion node. The output transistor is located in the first type of trench region, the device gate is located in the second type of trench region, and the output transistor corresponds to the intersection region of the first type of trench and the second type of trench, and the pixel unit is formed with the output transistor as the center.

13. The method for manufacturing an image sensor as described in claim 12, characterized in that, When a second isolation structure is formed from the second surface of the semiconductor substrate, the second isolation structure is disposed at least around the pixel unit and spans the first type trench and / or the second type trench. And / or, each of the pixel units is arranged in an array in rows and columns, and the arrangement of the first type of trench and the second type of trench includes: the first type of trench connects to and passes through the pixel units of each corresponding column, and the second type of trench is arranged at intervals in the row direction between the columns of the pixel units.

14. An image sensor, characterized in that, The image sensor is manufactured by the method of any one of claims 1 to 13, and the image sensor comprises: A semiconductor substrate, the semiconductor substrate including a device functional layer; The first trench extends from the first surface of the semiconductor substrate into the functional layer of the device; A filling auxiliary layer is formed on the sidewalls and bottom of the first trench; The first isolation structure is formed in the first trench. The first isolation structure includes a filled oxide and is an integral structure; A semiconductor device extending from the first surface into the functional layer of the device.

15. The image sensor as claimed in claim 14, characterized in that, The first trench includes a plurality of first-type trenches and a plurality of second-type trenches, and the extension direction of the first-type trenches and the extension direction of the second-type trenches form an angle. The semiconductor substrate includes a plurality of pixel units arranged in an array, each pixel unit including a photoelectric conversion region and a transmission control gate corresponding to the photoelectric conversion region, wherein: Each of the transmission control gates is arranged facing each other to form a central opening region. The pixel unit also includes an output transistor located in the central opening region, a first floating diffusion node and a second floating diffusion node located on both sides of the output transistor and connected to the corresponding transmission control gate, and a device gate connected to at least one floating diffusion node. The output transistor is located in the first type of trench region, the device gate is located in the second type of trench region, and the output transistor corresponds to the intersection region of the first type of trench and the second type of trench, and the pixel unit is formed with the output transistor as the center.

16. The image sensor as claimed in claim 15, characterized in that, When a second isolation structure is formed from the second surface of the semiconductor substrate, the second isolation structure is disposed at least around the pixel unit and spans the first type trench and / or the second type trench. And / or, each of the pixel units is arranged in an array in rows and columns, and the arrangement of the first type of trench and the second type of trench includes: the first type of trench connects to and passes through the pixel units of each corresponding column, and the second type of trench is spaced apart in the row direction between each column of pixel units.