A polycrystalline silicon layer and a preparation process thereof, a photovoltaic cell and a preparation method thereof
By using the POPAID technique to prepare polycrystalline silicon layers with gradient doping concentrations, the problem of tunnel oxide penetration under high doping concentrations was solved, achieving good ohmic contact and carrier suppression in the polycrystalline silicon layer, and improving the photoelectric conversion efficiency of photovoltaic cells.
Patent Information
- Application Number
- CN202611324895.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies struggle to balance reducing metal-semiconductor contact resistance with maintaining the passivation performance of the tunnel oxide layer at high doping concentrations, leading to increased carrier recombination and limiting the improvement of photovoltaic cell photoelectric conversion efficiency.
A polycrystalline silicon layer with gradient doping concentration was prepared using POPAID technology. A doped amorphous silicon layer was formed by plasma oxidation and plasma-assisted in-situ doping deposition, and then a short-time annealing was performed in an oxygen atmosphere to form a doped polycrystalline silicon layer. This ensured that the doping concentration gradually increased from the contact tunneling layer to the metal electrode surface. A special annealing process was also used to avoid the diffusion of doped atoms and the phenomenon of film bursting.
A continuous doping concentration gradient in the polycrystalline silicon layer was achieved, reducing series resistance, increasing fill factor and open-circuit voltage, and synergistically improving photoelectric conversion efficiency, while avoiding recombination increase and polycrystalline silicon layer delamination caused by dopant atom diffusion at high temperatures.
Smart Images

Figure CN123146013A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic technology, specifically to a polycrystalline silicon layer and its preparation process, and a photovoltaic cell and its preparation method. Background Technology
[0002] The photoelectric conversion efficiency of crystalline silicon solar cells (such as back contact cells and passivated contact cells) is limited by the recombination loss of photogenerated carriers and the resistive loss inside the device. Taking back contact (BC) cells and Tunnel Back Contact (TBC) cells that integrate tunnel oxide passivated contact (TOPCon) technology as examples, the back of the cell is provided with several alternating P-type doped regions and N-type doped regions. Each doped region is usually composed of a passivated contact structure of a tunnel oxide layer + a doped polycrystalline silicon layer. The metal electrode is disposed on the back of the cell and makes ohmic contact with the corresponding doped region.
[0003] In an ideal passivated contact structure, an ultrathin tunneling oxide layer (typically 0.5–2 nm thick) reduces recombination centers by saturating the silicon substrate surface with chemical bonds. Simultaneously, it allows majority carriers to tunnel through the oxide barrier into the doped polycrystalline silicon layer via quantum tunneling, while minority carriers are blocked. This achieves selective carrier transport and reduces the surface recombination rate. The doped polycrystalline silicon layer then functions as the lateral carrier transport interface for ohmic contact with the metal electrode.
[0004] However, in practical devices, battery efficiency is constrained by both carrier recombination and series resistance, and these two factors create a fundamental contradiction in their requirements for doping concentration: On the one hand, in order to improve the ohmic contact characteristics between the metal electrode and the silicon substrate and reduce the contact resistance to increase the fill factor (FF), the polycrystalline silicon layer needs to be highly doped (the doping concentration usually needs to reach 1×10^19 atoms / cm³ or higher). High-concentration doping can increase the majority carrier concentration and reduce the bulk resistance of the polycrystalline silicon layer, thereby significantly reducing the contact resistivity between the metal electrode and the silicon substrate.
[0005] On the other hand, high doping concentrations can lead to serious negative effects under high-temperature processes (such as doping-activated annealing and metallization sintering). Dopant atoms (especially phosphorus atoms) diffuse into the silicon substrate at high temperatures. When the phosphorus doping concentration is high, as the annealing time increases, dopant atoms diffuse through the ultrathin tunneling oxide layer into the silicon substrate, significantly aggravating Auger recombination. This results in a decrease in the implied open-circuit voltage (iVoc), an increase in the recombination current density, and severe deterioration of the passivation quality of the tunneling oxide layer. Meanwhile, although thinning the polycrystalline silicon layer is beneficial for increasing the short-circuit current density, the metal electrode paste is prone to burn-through of the polycrystalline silicon layer during high-temperature sintering, leading to direct contact between the metal electrode and the silicon substrate, and a sharp increase in the metal-induced recombination current density.
[0006] Therefore, in the existing BC / TBC battery fabrication process, there is a process bottleneck that makes it difficult to achieve both "reducing the metal-semiconductor contact resistance" and "maintaining the excellent passivation performance of the tunnel oxide layer and suppressing carrier recombination": simply increasing the doping concentration uniformly can reduce the contact resistance, but at high temperatures, the penetration of doped atoms into the tunnel oxide layer will destroy the passivation contact structure, induce severe interfacial recombination, and ultimately restrict the further improvement of the battery's photoelectric conversion efficiency.
[0007] To address the aforementioned issues, several attempts have been made in the prior art. For example, CN118213440A discloses a method for fabricating an N-type BC battery, employing a stacked structure of a first tunneling oxide layer + intrinsic amorphous silicon layer + second tunneling oxide layer + boron-doped amorphous silicon layer + silicon oxide layer, and utilizing laser film opening and printed phosphorus sources to achieve regional doping, aiming to simplify the process. Another example is CN122094237A, which proposes introducing richly doped polycrystalline silicon particles into the tunneling oxide passivation contact structure to promote carrier collection and reduce the carrier transport resistance in the tunneling layer; by controlling the size of the doped polycrystalline silicon particles, it is beneficial to optimize the enrichment effect of doped atoms, enhance the selective collection of carriers, and reduce recombination.
[0008] Nevertheless, existing technical solutions have not fundamentally solved the technical problem of carrier recombination caused by the penetration of the tunneling oxide layer and the degradation of passivation performance under conditions of high doping concentration and series resistance. Summary of the Invention
[0009] The purpose of this invention is to overcome the shortcomings of the prior art and provide a polycrystalline silicon layer and its preparation process, a photovoltaic cell and its preparation method, so as to obtain a polycrystalline silicon layer with a gradient doping concentration, thereby solving the contradiction between series resistance and carrier recombination caused by high doping concentration, and avoiding the film explosion phenomenon of the doped polycrystalline silicon layer during annealing, thereby synergistically improving the fill factor and open circuit voltage, and achieving higher photoelectric conversion efficiency.
[0010] Based on this, the present invention discloses a process for preparing a polycrystalline silicon layer, comprising the following preparation steps: Step 1: Using plasma oxidation and plasma-assisted in-situ doping deposition (POPAID) technology, a tunneling layer and a doped amorphous silicon layer are sequentially prepared on the surface of a silicon wafer. The POPAID device includes a PO cavity for preparing a tunneling layer and a PAID cavity for preparing a doped amorphous silicon layer. The PAID cavity includes three chambers arranged sequentially, which are respectively connected to doping gas path U1, doping gas path U2, and doping gas path U3. The silicon wafer with the tunneling layer is passed sequentially through the three chambers in the PAID cavity that are respectively connected to doping gas path U1, doping gas path U2, and doping gas path U3. The doping gas flow rate of the three chambers is controlled by adjusting the doping gas flow rate of doping gas path U1, U2, and U3 to form a gradient doping concentration. The doping gas flow rate of doping gas path U1, U2, and U3 satisfies the following relationship: flow rate of U3 > flow rate of U2 > flow rate of U1. Step 2: Anneal the silicon wafer with the doped amorphous silicon layer prepared in an oxygen atmosphere. The initial annealing temperature is 350~650℃, the heating rate is ≤5℃ / min, and the holding time after heating is 200~650s. Annealing causes the doped amorphous silicon layer to crystallize and activates the doped atoms in the doped amorphous silicon layer to form a doped polycrystalline silicon layer with a gradient doping concentration. The doping concentration of the doped polycrystalline silicon layer gradually increases from the interface of the contact tunneling layer to the surface of the contact metal electrode.
[0011] Preferably, in step 1, the power of the PO cavity is 90~130W, the oxygen flow rate is 450~550sccm, and the belt speed is 120~260cm / min; the tunneling layer is a tunneling oxide layer with a thickness of 0.5~2nm.
[0012] Preferably, in step 1, the power of the PAID cavity is 20~65kW, the belt speed is 80~170 cm / min, and the thickness of the doped amorphous silicon layer is 100~200nm.
[0013] More preferably, in step 1, when the doped amorphous silicon layer is a phosphorus-doped amorphous silicon layer, the doping gas includes phosphine and argon, and the volume concentration of phosphine in the doping gas is ≤20%. The flow rate of the doped gas in the doped gas path U1 is 0~40 sccm, the flow rate of the doped gas in the doped gas path U2 is 150~200 sccm, the flow rate of the doped gas in the doped gas path U3 is 180~230 sccm, and the total flow rate of the doped gas is 330~440 sccm.
[0014] More preferably, in step 1, the volume concentration of phosphine in the doping gas is 5%; The flow rate of the doped gas in doped gas path U1 is 10~40 sccm, the flow rate of the doped gas in doped gas path U2 is 150~170 sccm, and the flow rate of the doped gas in doped gas path U3 is 180~230 sccm.
[0015] Preferably, in step 2, after heating to 840~875℃, the temperature is held and annealed in an atmosphere with an oxygen flow rate of 20000~100000 sccm; after annealing, a 30~100nm thick doped silicon glass is formed on the surface of the doped polycrystalline silicon layer. The doping concentration of the polycrystalline silicon layer near the interface of the contact tunneling layer is 5E19~2E20 cm⁻¹. 3 The doping concentration of the polycrystalline silicon layer near the contact metal electrode is 3E20~6E20 cm⁻¹. 3 .
[0016] More preferably, in step 2, the initial annealing temperature is 600℃, the heating rate is 5℃ / min, after heating to 875℃, the holding time is 300~600s, and the annealing treatment is carried out in an atmosphere with an oxygen flow rate of 50000sccm.
[0017] The present invention also discloses a polycrystalline silicon layer, which is prepared by the polycrystalline silicon layer preparation process described above in the present invention; the polycrystalline silicon layer has a gradient doping concentration, the doping concentration on the surface of the contact metal electrode is higher than the doping concentration at the interface of the contact tunneling layer, and the doping concentration in the polycrystalline silicon layer is distributed continuously without abrupt changes.
[0018] This invention also discloses a method for preparing a photovoltaic cell, which includes the following preparation steps: Step 1: Using the polycrystalline silicon layer fabrication process described above in this invention, a tunneling layer and a doped polycrystalline silicon layer with gradient doping concentration are sequentially fabricated on the surface of a silicon wafer. Step 2: Metallize the silicon wafer processed in Step 1 to obtain a metal electrode that contacts the doped polycrystalline silicon layer.
[0019] The present invention also discloses a photovoltaic cell, which is prepared by the photovoltaic cell preparation method described above in the present invention; The photovoltaic cell includes: a silicon wafer, on the surface of which a tunneling layer and a doped polycrystalline silicon layer with a gradient doping concentration are sequentially disposed; the doping concentration of the doped polycrystalline silicon layer gradually increases from the interface in contact with the tunneling layer to the surface in contact with the metal electrode; the doped polycrystalline silicon layer is in contact with the metal electrode.
[0020] The main innovative technologies of this invention are as follows: 1. This invention shortens the high-temperature annealing time to 200-650 seconds. This has the following advantages: shortening the high-temperature annealing time can protect the tunneling oxide layer and avoid the increase in recombination caused by excessive diffusion of doped atoms such as phosphorus due to damage to the tunneling oxide layer, thereby helping to improve the open-circuit voltage and other electrical properties of the battery; this advantage is especially obvious when the polycrystalline silicon layer (such as the N-poly layer, also known as the N-type doped polycrystalline silicon layer) has a high doping concentration. Meanwhile, shortening the high-temperature holding time during annealing makes it easier to achieve a better, continuous, and abrupt doping gradient in the polycrystalline silicon layer and simplifies the process. Doped atoms (such as phosphorus doped atoms) in the polycrystalline silicon layer diffuse continuously and gradually from the high doping concentration side (i.e., the surface of the polycrystalline silicon layer contacting the metal electrode) to the low doping concentration side (i.e., the interface of the polycrystalline silicon layer contacting the tunneling oxide layer) until the doping concentration is balanced. In this way, maintaining a high doping concentration on the surface of the polycrystalline silicon layer contacting the metal electrode ensures a good ohmic contact between the metal electrode and the polycrystalline silicon layer, thereby reducing the series resistance and improving the fill factor. At the same time, maintaining a low doping concentration at the interface of the polycrystalline silicon layer contacting the tunneling oxide layer effectively suppresses carrier recombination, thereby increasing the open-circuit voltage and thus improving the photoelectric conversion efficiency and other electrical performance of the battery. However, if the high-temperature holding time during annealing is too long, the doping concentration at various locations in the polycrystalline silicon layer tends to be uniform, losing the structural advantages of the gradient concentration doping of the polycrystalline silicon layer.
[0021] 2. Regarding the annealing process, amorphous silicon materials release hydrogen gas at temperatures around 300-400℃. Excessively high initial annealing temperatures cause the doped amorphous silicon layer to release a large amount of hydrogen gas, thus exacerbating the film-bursting phenomenon. Therefore, this invention reduces the initial annealing temperature and heating rate to slow down the hydrogen release rate, thereby minimizing the occurrence of film-bursting in the polycrystalline silicon layer.
[0022] 3. In the process of preparing a doped amorphous silicon layer using POPAID technology (plasma oxidation and plasma-assisted in-situ doping deposition), the carrier plate supporting the silicon wafer sequentially passes through three chambers (U1, U2, and U3) within the PAID cavity. By adjusting the doping gas flow rates of each of the doping gas paths U1, U2, and U3 within the PAID cavity, and in conjunction with subsequent special annealing processes (such as shortening the high-temperature holding time during annealing), a better doping concentration gradient in the polycrystalline silicon layer (such as an N-poly layer) can be achieved. Experimental results show that when the doping gas flow rates of U1, U2, and U3 are the same, a gradient doping concentration cannot be formed in the polycrystalline silicon layer. Furthermore, if the doping gas flow rate of U1 is too high, it can cause phosphorus atoms to diffuse inward and tunnel through the oxide layer and the silicon wafer, which is detrimental to the improvement of the battery's electrical performance. When the doping gas flow rate of U2 is too high and the doping gas flow rate of U3 is too low, the magnitude of the doping concentration gradient in the polycrystalline silicon layer will decrease, which is also detrimental to the improvement of the battery's electrical performance. When the flow rate of doped gas U2 is too low and the flow rate of doped gas U3 is too high, coupled with a short annealing time, the doping concentration in the middle position of the polycrystalline silicon layer will be too low, the electronic lateral resistance will be high, and the fill factor will be reduced, which is not conducive to improving the battery's electrical performance.
[0023] Therefore, compared with the prior art, the present invention has at least the following beneficial effects: This invention discloses a polycrystalline silicon layer fabrication process. During the fabrication of a doped amorphous silicon layer using POPAID technology, the flow rates of doped gases in the PAID cavity's doping gas paths U1, U2, and U3 are controlled, along with subsequent special annealing processes (such as reducing the initial annealing temperature and heating rate, and shortening the annealing holding time). This allows doped atoms to diffuse from the high-concentration surface of the polycrystalline silicon layer into the polycrystalline silicon layer, spontaneously forming a doped polycrystalline silicon layer (such as an N-poly layer) with a continuous and abrupt doping concentration gradient. Maintaining a high doping concentration on the surface of the polycrystalline silicon layer contacting the metal electrode ensures good ohmic contact between the metal electrode and the polycrystalline silicon layer, thereby reducing contact resistance and series resistance, and improving the fill factor. Simultaneously, maintaining a low doping concentration at the interface of the polycrystalline silicon layer with the contact tunneling oxide layer effectively suppresses carrier recombination, thereby increasing the open-circuit voltage. This effectively resolves the contradiction between series resistance and carrier recombination caused by high doping concentration, thus improving the photoelectric conversion efficiency and other electrical performance of the battery. On the other hand, it can also effectively suppress the phenomenon of film bursting of doped polycrystalline silicon layer caused by excessive accumulation of interface stress and concentrated release of hydrogen, improve the quality of doped polycrystalline silicon layer, and thus synergistically improve fill factor and open circuit voltage, achieving higher photoelectric conversion efficiency. Attached Figure Description
[0024] Figure 1This is a schematic diagram of the cross-sectional structure of a back-contact photovoltaic cell according to the present invention.
[0025] Figure 2 This is a 3D microscope image of the back side of the silicon wafer after annealing in step S7 of Example 1. Figure 2 In the image, a) is a 3D microscope image magnified 20 times, and b) is a 3D microscope image magnified 50 times.
[0026] Figure 3 This is a 3D microscope image of the back side of the silicon wafer after annealing in step S7, Comparative Example 2. Figure 3 In the image, a) is a 3D microscope image magnified 20 times, and b) is a 3D microscope image magnified 50 times.
[0027] Figure 4 The phosphorus doping concentration distribution on the back side of the silicon wafers after annealing in step S7 is shown in Example 1 and Comparative Example 1.
[0028] Figure 5 The phosphorus doping concentration distribution on the back side of the silicon wafers after annealing in step S7 is shown in Examples 1 and Comparative Examples 3-5.
[0029] Reference numerals: 1. Silicon wafer; 2. First tunneling oxide layer; 3. P-poly layer; 4. Second tunneling oxide layer; 5. N-poly layer; 6. GAP region; 7. Alumina passivation layer; 8. Silicon nitride antireflective coating; 9. P-type metal electrode; 10. N-type metal electrode. Detailed Implementation
[0030] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Example 1 This embodiment describes a method for fabricating a back-contact photovoltaic cell with a gradient doped N-poly layer. See [link to relevant documentation]. Figure 1 It includes the following preparation steps: S1. A clean, pre-existing silicon wafer 1 is provided, polished on both sides (i.e., the front and back sides). The back side of the silicon wafer 1 includes an N-region, a P-region, and a gap region (GAP region 6) that isolates adjacent N-regions and P-regions.
[0032] S2. A first tunneling oxide layer 2, a P-type doped polysilicon layer (boron doped polysilicon layer, i.e., P-poly layer 3) and a mask layer are sequentially prepared on the back side of silicon wafer 1.
[0033] In step S2, the thickness of the first tunneling oxide layer 2 is 1.5 nm; the thickness of the P-poly layer 3 is 170 nm, and its boron doping concentration is 7e19cm. -3The mask layer is borosilicate glass (BSG) with a thickness of 80 nm. In practice, boron doping is performed using a boron diffusion process, and BSG is formed on the back side of the P-poly layer 3 as a mask layer.
[0034] S3. Perform a laser patterning process on the back N-region and GAP region 6 of the silicon wafer processed in step S2 to etch away the mask layer (BSG) and P-poly layer 3 of the N-region and GAP region 6. At this time, the P-poly layers 3 on the back are arranged at intervals.
[0035] S4. The silicon wafer processed in step S3 is wet-cleaned using a chain machine (using HF aqueous solution for acid washing) to remove the BSG plating on the front and side surfaces of silicon wafer 1.
[0036] S5. The silicon wafer processed in step S4 is subjected to alkaline polishing using a tank-type machine to remove residual film layers (such as the first tunneling oxide layer 2 and residual P-poly layer 3 in the first laser area (i.e., N area and GAP area 6) on the front and back sides.
[0037] S6. Using POPAID technology (plasma oxidation and plasma-assisted in-situ doping deposition), a second tunneling oxide layer 4 and an N-type doped amorphous silicon layer (phosphorus-doped amorphous silicon layer) are sequentially fabricated on the entire back side of the silicon wafer after the treatment in step S5. In practice, for the P-region on the back side of silicon wafer 1, the second tunneling oxide layer 4 and the N-type doped amorphous silicon layer are sequentially fabricated on the back side of the BSG. The specific fabrication process of step S6 is as follows: S61. First, a second tunneling oxide layer 4 is prepared in the PO cavity (plasma oxidation process cavity) of the POPAID equipment. The power of the PO cavity is 110W, the oxygen flow rate is 450sccm, the belt speed is 120 cm / min, and the thickness of the second tunneling oxide layer 4 is 1nm.
[0038] S62. Then, a phosphorus-doped amorphous silicon layer is grown in the PAID cavity (plasma-assisted in-situ doping deposition process cavity) of the POPAID equipment: The PAID cavity includes three chambers arranged in sequence; after the silicon wafer 1 carried by the carrier board enters the PAID cavity, it passes through the three chambers in sequence. These three chambers are respectively connected to the doping gas paths U1, U2 and U3. The doping gas flow rate of the three chambers is controlled by adjusting the doping gas flow rate of U1, U2 and U3, thereby achieving the gradient doping concentration of the N-type doped amorphous silicon layer.
[0039] In step S62, the doping gas includes phosphine and argon. The volume concentration of phosphine in the doping gas is 5%. The flow rate of the doping gas for U1 is 20 sccm, the flow rate of the doping gas for U2 is 170 sccm, the flow rate of the doping gas for U3 is 200 sccm, and the total flow rate of the doping gas is 390 sccm. The power of the PAID cavity is 44 kW, the band speed is 125 cm / min, and the thickness of the N-type doped amorphous silicon layer is 130 nm.
[0040] S7. The silicon wafer processed in step S6 is subjected to high-temperature annealing in an oxygen atmosphere to crystallize the N-type doped amorphous silicon layer at high temperature to form an N-type doped polycrystalline silicon layer (i.e., N-poly layer 5), and phosphorus doping atoms are activated to obtain an N-poly layer 5 with a gradient doping concentration. PSG (phosphosilicate glass) is generated on the back side of the N-poly layer 5 to protect the N-poly.
[0041] In the high-temperature annealing process of step S7, the problem of N-poly film bursting is solved by lowering the initial annealing temperature and slowing down the heating rate: the initial annealing temperature is 600℃, the heating rate is 5℃ / min, and after heating to 875℃, the holding time is 300s, which is carried out in an atmosphere with an oxygen injection rate of 50000 sccm; the thickness of the formed PSG is 40nm, and the phosphorus doping concentration on the surface of the N-poly layer 5 contacting the metal electrode is 4E20cm. -3 The phosphorus doping concentration at the interface between the N-poly layer 5 and the second tunneling oxide layer 4 is 2E20cm⁻¹. -3 .
[0042] S8. The GAP region 6 and the PSG and N-poly layer 5 of the P region on the back side of the silicon wafer after step S7 are removed by laser patterning. At this time, the N region on the back side of the silicon wafer 1 has a second tunneling oxide layer 4 and an N-poly layer 5 with a gradient doping concentration formed sequentially, while the P region on the back side of the silicon wafer 1 has a first tunneling oxide layer 2 and a P-poly layer 3 formed sequentially, and the N region and the P region are isolated by the GAP region 6; thus, a pattern of N-poly layer 5, GAP region 6 and P-poly layer 3 arranged in sequence is formed on the back side of the silicon wafer 1.
[0043] S9. The silicon wafer processed in step S8 is wet-cleaned using a chain machine (using HF aqueous solution for acid washing) to remove the PSG plating on the front and side surfaces of silicon wafer 1.
[0044] S10. The silicon wafer processed in step S9 is subjected to alkaline texturing using a tank-type machine to remove residual film layers (such as the second tunneling oxide layer 4 and residual N-poly layer 5 in the second laser region 6 and P region 6) on the front and back sides. Alkaline texturing is used to form a textured surface with a pyramid structure on the front side of the silicon wafer 1. Then, acid washing in an acid tank is used to remove BSG in the P region and PSG in the N region.
[0045] S11. Using an atomic layer deposition equipment, an aluminum oxide passivation layer 7 is deposited on both the front and back sides of the silicon wafer after the process in step S10 (specifically, the aluminum oxide passivation layer 7 on the back side is deposited on the back side of the silicon wafer 1 with N-poly layer 5, GAP area 6 and P-poly layer 3).
[0046] S12. Using a plasma-enhanced chemical deposition system, silicon nitride antireflection films 8 are deposited on the surfaces of the alumina passivation layers 7 on both the front and back sides to reduce light reflection.
[0047] S13. Metallization: Using screen printing equipment, P-type metal electrode paste and N-type metal electrode paste are respectively applied to the P-region and N-region of the back side of the silicon wafer after the treatment in step S12. The mixture is then sintered in a sintering furnace to allow the metal electrode paste to bond with the silicon substrate, forming an alloy to extract photogenerated carriers. This process yields the P-type metal electrode 9 contacting the P-poly layer 3 and the N-type metal electrode 10 contacting the N-poly layer 5, thus completing the fabrication of the back-contact photovoltaic cell. The structure of this back-contact photovoltaic cell is as follows: Figure 1 As shown.
[0048] Steps S6-S7 described above constitute a polycrystalline silicon layer fabrication process according to this embodiment. The remaining steps in this embodiment follow the existing fabrication methods for back-contact photovoltaic cells, and therefore will not be elaborated upon here.
[0049] Furthermore, it should be noted that the P-poly layer 3 can also be prepared using the polycrystalline silicon layer preparation process of this invention. However, in practice, the mainstream preparation method for the P-poly layer 3 is tubular boron diffusion. The polycrystalline silicon layer preparation process of this invention can also be used to prepare other types of photovoltaic cells containing doped polycrystalline silicon layers, and is not limited to back-contact photovoltaic cells.
[0050] Example 2 This embodiment describes a method for fabricating a back-contact photovoltaic cell with a gradient doped N-poly layer. The specific fabrication steps are the same as in Example 1, but the difference between Example 1 and Example 1 is as follows: In step S62 of this embodiment, the doping gas flow rate of U1 in the PAID cavity is 10 sccm, the doping gas flow rate of U2 is 150 sccm, and the doping gas flow rate of U3 is 230 sccm, while the remaining process parameters remain unchanged.
[0051] Example 3 This embodiment describes a method for fabricating a back-contact photovoltaic cell with a gradient doped N-poly layer. The specific fabrication steps are the same as in Example 1, but the difference between Example 1 and Example 1 is as follows: In step S62 of this embodiment, the doping gas flow rate of U1 in the PAID cavity is 40 sccm, the doping gas flow rate of U2 is 170 sccm, and the doping gas flow rate of U3 is 180 sccm, while the remaining process parameters remain unchanged.
[0052] Example 4 This embodiment describes a method for fabricating a back-contact photovoltaic cell with a gradient doped N-poly layer. The specific fabrication steps are the same as in Example 1, but the difference between Example 1 and Example 1 is as follows: In the high-temperature annealing process of step S7 in this embodiment, after the temperature is raised to 875°C, the holding time is 600s, and the other process parameters remain unchanged.
[0053] Comparative Example 1 The preparation method of the back-contact photovoltaic cell in this comparative example is the same as that in Example 1, except that: In the high-temperature annealing process of step S7 in this comparative example, after the temperature is raised to 875℃, the holding time is 1800s, and the other process parameters remain unchanged.
[0054] Comparative Example 2 The preparation method of the back-contact photovoltaic cell in this comparative example is the same as that in Example 1, except that: In the high-temperature annealing process of step S7 in this comparative example, the initial annealing temperature was set to 800℃, and the other process parameters remained unchanged.
[0055] Comparative Example 3 The preparation method of the back-contact photovoltaic cell in this comparative example is the same as that in Example 1, except that: In step S62 of this comparative example, the doping gas flow rate of U1 in the PAID cavity is 130 sccm, the doping gas flow rate of U2 is 130 sccm, the doping gas flow rate of U3 is 130 sccm, and the total doping gas flow rate is 390 sccm. The remaining process parameters remain unchanged.
[0056] Comparative Example 4 The preparation method of the back-contact photovoltaic cell in this comparative example is the same as that in Example 1, except that: In step S62 of this comparative example, the doping gas flow rate of U1 in the PAID cavity is 20 sccm, the doping gas flow rate of U2 is 220 sccm, the doping gas flow rate of U3 is 150 sccm, and the total doping gas flow rate is 390 sccm. The remaining process parameters remain unchanged.
[0057] Comparative Example 5 The preparation method of the back-contact photovoltaic cell in this comparative example is the same as that in Example 1, except that: In step S62 of this comparative example, the doping gas flow rate of U1 in the PAID cavity is 20 sccm, the doping gas flow rate of U2 is 130 sccm, the doping gas flow rate of U3 is 240 sccm, and the total doping gas flow rate is 390 sccm. The remaining process parameters remain unchanged.
[0058] Performance testing 1. 3D microscopic images of the back side of silicon wafers after high-temperature annealing in step S7, using Examples 1 and Comparative Example 2, are shown in the image. Figure 2-3 As shown.
[0059] The process conditions for depositing phosphorus-doped amorphous silicon layers using POPAID in Example 1 and Comparative Example 2 were the same, except that the initial annealing temperature in step S7 of Example 1 was 600°C, while the initial annealing temperature in step S7 of Comparative Example 2 was 800°C. All other annealing conditions were the same. See also... Figure 2-3 As can be seen, in Example 1, the N-poly layer on the back side of the silicon wafer after annealing in step S7 did not exhibit any film bursting, while in Comparative Example 2, the N-poly layer on the back side of the silicon wafer after annealing in step S7 showed obvious film bursting. This proves that excessively high initial annealing temperatures cause the N-poly layer to release a large amount of hydrogen gas, thereby exacerbating the film bursting phenomenon and affecting the quality of the N-poly layer and the electrical performance of the battery (see Table 1 below). Therefore, lowering the initial annealing temperature can effectively solve the film bursting problem.
[0060] 2. The phosphorus doping concentration distribution in the N-region on the back side of the silicon wafers after the high-temperature annealing treatment in step S7 of Examples 1 and Comparative Examples 2-5 was detected. The detection results are as follows: Figure 4-5 As shown.
[0061] It should be noted that, Figure 4-5 In the phosphorus doping concentration distribution diagram, the horizontal axis represents the phosphorus doping depth, and the vertical axis represents the phosphorus doping concentration. In this Example 1, the thickness of the N-poly layer is approximately 130 nm, meaning that the layer is essentially an N-poly layer up to a depth of 0.13 μm on the horizontal axis, and after 0.13 μm, it consists of the second tunneling oxide layer and the silicon wafer. That is, the gradient doping concentration of the N-poly layer is... Figure 4-5 Within the 0-0.13μm depth region of the middle horizontal axis.
[0062] (1) The annealing and holding time in step S7 of Example 1 is 300s, and the annealing and holding time in step S7 of Comparative Example 1 is 1800s. Figure 4 The results show that excessive phosphorus diffusion occurred after annealing in Comparative Example 1, indicating that the phosphorus doping concentration in the second tunneling oxide layer and the silicon wafer was too high. This was due to the excessively long annealing time, which prevented the second tunneling oxide layer from blocking phosphorus atoms, resulting in excessive diffusion. Therefore, in the preparation of gradient doped N-Poly layers, the annealing time needs to be shortened to avoid damaging the tunneling oxide layer, causing excessive phosphorus diffusion and increasing recombination, which in turn affects the battery's open-circuit voltage, short-circuit current density, battery performance, and other electrical properties (see Table 1 below).
[0063] See Figure 5 Therefore, we can conclude that: (2) The doping gas flow rates of U1, U2, and U3 in the PAID cavity of Comparative Example 3 in step S62 are all the same. Compared with Example 1, the N-poly layer of Comparative Example 3 does not form a gradient doping concentration, that is, the phosphorus doping concentration in the N-poly layer with a depth of 0-0.13 μm is basically the same; and because the doping gas flow rate of the cavity corresponding to the doping gas path U1 is too large, it also leads to the problem of excessive phosphorus diffusion (that is, phosphorus doping atoms diffuse into the second tunneling oxide layer and the silicon wafer), which in turn affects the electrical performance of the battery (see Table 1 below).
[0064] (3) The flow rate of doped gas in the PAID cavity U1 and the total flow rate of doped gas in Comparative Example 4 are the same as those in Example 1 in step S62. However, the flow rate of doped gas in the doped gas path U2 in Comparative Example 4 is too large and the flow rate of doped gas in the doped gas path U3 is too small. This results in the phosphorus doping concentration gradient of the N-poly layer in Comparative Example 4 being too low, which is also not conducive to the improvement of the battery's electrical performance to some extent (see Table 1 below).
[0065] (4) The flow rate of doped gas U1 in the PAID cavity and the total flow rate of doped gas in Comparative Example 5 are the same as those in Example 1 in step S62. However, the flow rate of doped gas U2 in Comparative Example 5 is too small and the flow rate of doped gas in doped gas path U3 is too large. Combined with the use of a shorter annealing and holding time, the phosphorus doping concentration in the middle position of the N-poly layer of Comparative Example 5 is too low. The N-poly layer does not form a good continuous and abrupt phosphorus doping concentration gradient, which will lead to a higher electronic transverse resistance and thus reduce the fill factor and other electrical properties (as shown in Table 1 below).
[0066] 3. The back-contact photovoltaic cell samples prepared in Examples 1-4 and Comparative Examples 1-5 were subjected to IV (current-voltage) electrical performance tests (IV test median, 500 cells for each sample). The test results are shown in Table 1 below. In Table 1, Voc is the open-circuit voltage, FF is the fill factor, Jsc is the short-circuit current density, and Eta is the photoelectric conversion efficiency (i.e., cell efficiency) of the cell.
[0067] Table 1
[0068] Although preferred embodiments of the present invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present invention.
[0069] The technical solution provided by the present invention has been described in detail above. Specific examples have been used to illustrate the principle and implementation of the present invention. The description of the above embodiments is only for the purpose of helping to understand the method and core idea of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation and application scope based on the idea of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A process for preparing a polycrystalline silicon layer, characterized in that, The preparation steps include the following: Step 1: Using plasma oxidation and plasma-assisted in-situ doping deposition (POPAID) technology, a tunneling layer and a doped amorphous silicon layer are sequentially prepared on the surface of a silicon wafer. The POPAID device includes a PO cavity for preparing a tunneling layer and a PAID cavity for preparing a doped amorphous silicon layer. The PAID cavity includes three chambers arranged in sequence. The silicon wafer with the tunneling layer is passed through the three chambers of the PAID cavity, which are respectively connected to the doping gas path U1, doping gas path U2 and doping gas path U3. The flow rates of the doping gas in the doping gas paths U1, U2 and U3 satisfy the following relationship: flow rate of U3 > flow rate of U2 > flow rate of U1. Step 2: Anneal the silicon wafer with the doped amorphous silicon layer prepared in an oxygen atmosphere. The initial annealing temperature is 350~650℃, the heating rate is ≤5℃ / min, and the holding time after heating is 200~650s. Annealing causes the doped amorphous silicon layer to crystallize and activates the doped atoms in the doped amorphous silicon layer to form a doped polycrystalline silicon layer with a gradient doping concentration. The doping concentration of the doped polycrystalline silicon layer gradually increases from the interface of the contact tunneling layer to the surface of the contact metal electrode.
2. The process for preparing a polycrystalline silicon layer according to claim 1, characterized in that, In step 1, the power of the PO cavity is 90~130W, the oxygen flow rate is 450~550sccm, and the belt speed is 120~260cm / min; the tunneling layer is a tunneling oxide layer with a thickness of 0.5~2nm.
3. The process for preparing a polycrystalline silicon layer according to claim 1, characterized in that, In step 1, the power of the PAID cavity is 20~65kW, the belt speed is 80~170cm / min, and the thickness of the doped amorphous silicon layer is 100~200nm.
4. The process for preparing a polycrystalline silicon layer according to claim 1 or 3, characterized in that, In step 1, when the doped amorphous silicon layer is a phosphorus-doped amorphous silicon layer, the doping gas includes phosphine and argon, and the volume concentration of phosphine in the doping gas is ≤20%. The flow rate of the doped gas in the doped gas path U1 is 0~40 sccm, the flow rate of the doped gas in the doped gas path U2 is 150~200 sccm, the flow rate of the doped gas in the doped gas path U3 is 180~230 sccm, and the total flow rate of the doped gas is 330~440 sccm.
5. The process for preparing a polycrystalline silicon layer according to claim 4, characterized in that, In step 1, the volume concentration of phosphine in the doping gas is 5%; The flow rate of the doped gas in doped gas path U1 is 10~40 sccm, the flow rate of the doped gas in doped gas path U2 is 150~170 sccm, and the flow rate of the doped gas in doped gas path U3 is 180~230 sccm.
6. The process for preparing a polycrystalline silicon layer according to claim 1, characterized in that, In step 2, after heating to 840~875℃, the temperature is held and annealed in an atmosphere with an oxygen flow rate of 20000~100000 sccm; after annealing, a 30~100nm thick doped silicon glass is formed on the surface of the doped polycrystalline silicon layer. The doping concentration of the polycrystalline silicon layer near the interface of the contact tunneling layer is 5E19~2E20 cm⁻¹. 3 The doping concentration of the polycrystalline silicon layer near the contact metal electrode is 3E20~6E20 cm⁻¹. 3 .
7. The process for preparing a polycrystalline silicon layer according to claim 6, characterized in that, In step 2, the initial annealing temperature is 600℃, the heating rate is 5℃ / min, and after heating to 875℃, the holding time is 300~600s, and the annealing treatment is carried out in an atmosphere with an oxygen flow rate of 50000sccm.
8. A polycrystalline silicon layer, characterized in that, It is prepared by a polycrystalline silicon layer fabrication process according to any one of claims 1-7; the polycrystalline silicon layer has a gradient doping concentration, the doping concentration on the surface of the contact metal electrode is higher than the doping concentration at the interface of the contact tunneling layer, and the doping concentration in the polycrystalline silicon layer is distributed continuously without abrupt changes.
9. A method for preparing a photovoltaic cell, characterized in that, It includes the following preparation steps: Step 1: Using the polycrystalline silicon layer fabrication process described in any one of claims 1-7, a tunneling layer and a doped polycrystalline silicon layer with gradient doping concentration are sequentially fabricated on the surface of a silicon wafer. Step 2: Metallize the silicon wafer processed in Step 1 to obtain a metal electrode that contacts the doped polycrystalline silicon layer.
10. A photovoltaic cell, characterized in that, It is prepared using the photovoltaic cell preparation method described in claim 9; The photovoltaic cell includes: a silicon wafer, on the surface of which a tunneling layer and a doped polycrystalline silicon layer with a gradient doping concentration are sequentially disposed; the doping concentration of the doped polycrystalline silicon layer gradually increases from the interface in contact with the tunneling layer to the surface in contact with the metal electrode; the doped polycrystalline silicon layer is in contact with the metal electrode.
Citation Information
Patent Citations
Preparation method of N-type BC battery
CN118213440A
Tunneling oxide layer passivation contact structure, preparation method thereof and solar cell