An artificial optoelectronic synapse device, a preparation method and application thereof
By constructing a multi-level trap system in TiO₂ nanorod-based artificial optoelectronic synaptic devices, the problems of easy recombination of photogenerated carriers and insufficient storage capacity were solved, improving the photoresponse performance and conductivity retention of the devices, and realizing learning, memory and neuromorphic computing functions.
Patent Information
- Application Number
- CN202611335996.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-20
AI Technical Summary
In TiO₂ nanorod-based artificial optoelectronic synaptic devices, the photogenerated carrier recombination rate is fast and the lifetime is short. The trap energy level distribution is uniform, resulting in insufficient photoresponse sensitivity, limited conductivity retention and synaptic plasticity. Furthermore, the existing heterojunction interface bonding mode is simple, and the carriers are easy to recombine, resulting in insufficient long-term performance retention.
Nitrogen-doped TiO₂ nanorod arrays were grown in situ on the surface of FTO conductive glass using a hydrothermal method. Shallow and deep level defects were constructed by repeatedly spin-coating ZnO quantum dots and performing low-temperature annealing. Ultraviolet light irradiation was carried out simultaneously during the last low-temperature annealing process to form a multi-level trap system and optimize the heterojunction interface state.
It improves the lifetime and storage capacity of photogenerated carriers, enhances the photoresponse performance and conductivity retention of the device, realizes learning and memory, optical information encoding and storage and neuromorphic computing functions, and improves the stability and plasticity of the device.
Smart Images

Figure CN123146014A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the fields of semiconductor optoelectronic devices and neuromorphic devices, and in particular to an artificial optoelectronic synapse device, its fabrication method, and its application. Background Technology
[0002] Artificial opto-synaptic devices can simultaneously perform optical information sensing, storage, and processing functions, serving as an important hardware foundation for neuromorphic computing and artificial visual perception systems. TiO2 nanorod arrays, with their good ultraviolet light response, chemical stability, and controllable growth characteristics, are often used as photosensitive functional materials for artificial opto-synaptic devices.
[0003] However, TiO2 nanorods exhibit a high recombination rate and short lifetime for photogenerated carriers, and their internal trap energy level distribution is relatively homogeneous, limiting their ability to capture and store photogenerated carriers. This restricts the photoresponse sensitivity, conductivity retention, and synaptic plasticity of TiO2 nanorod-based devices. To address these limitations, a scheme has emerged that modifies TiO2 nanorods with ZnO quantum dots to construct heterojunctions, aiming to utilize the heterojunction to promote the separation of photogenerated carriers.
[0004] However, the related technologies mainly focus on the construction of the heterojunction itself, and give less consideration to the defect state, trap energy level distribution and interface charge transport behavior of the heterojunction interface. The interface bonding mode is relatively simple, and charge carriers are still prone to recombination at the interface. The devices still have shortcomings in maintaining performance over a long period of time and simulating complex neuromorphic behavior. Summary of the Invention
[0005] To address the issues of easy recombination and insufficient capture and storage capacity of photogenerated carriers in artificial optoelectronic synaptic devices, and to improve the device's photoresponse performance, conductivity retention capability, and synaptic plasticity, this application provides an artificial optoelectronic synaptic device, its fabrication method, and its application.
[0006] To achieve the above objectives, the technical solution adopted in this application is as follows: A method for fabricating an artificial photoelectric synapse device is provided, comprising the following steps: S1: Nitrogen-doped TiO2 nanorod arrays are grown in situ on the surface of FTO conductive glass using a hydrothermal method, and the nitrogen-doped TiO2 nanorod arrays are annealed to construct shallow level defects in the nitrogen-doped TiO2 nanorod arrays as carrier trapping and storage centers. S2: Spin-coat a ZnO quantum dot suspension onto the surface of the nitrogen-doped TiO2 nanorod array. The spin-coating is performed at least twice, and a low-temperature annealing treatment is performed after each spin-coating. This allows ZnO quantum dots to be deposited layer by layer and cover the surface of the nitrogen-doped TiO2 nanorod array, forming a ZnO quantum dot heterolayer. The ZnO quantum dot heterolayer and the nitrogen-doped TiO2 nanorod array form a heterojunction and introduce deep-level defects. S3: During the last low-temperature annealing process, the interface of the heterojunction is simultaneously subjected to ultraviolet light irradiation to form interface defects at the interface of the heterojunction. S4: Deposit a metal top electrode on the surface of the ZnO quantum dot heterolayer. The metal top electrode and the FTO conductive glass, which serves as the bottom electrode, form a two-end structure to obtain an artificial photoelectric synapse device. The shallow level defects, deep level defects, and interface defects together constitute a multi-level trap system, which is used to capture and store photogenerated carriers step by step under the action of the built-in electric field of the heterojunction.
[0007] Further, in step S1, the in-situ growth of nitrogen-doped TiO2 nanorod arrays on the surface of FTO conductive glass using a hydrothermal method includes: S101: Tetrabutyl titanate, urea, hydrochloric acid and water are mixed and magnetically stirred to obtain a hydrothermal reaction solution, wherein the volume ratio of water to hydrochloric acid in the hydrothermal reaction solution is 1:1. S102: The FTO conductive glass is placed in the hydrothermal reaction solution to carry out a hydrothermal reaction, and the nitrogen-doped TiO2 nanorod array is grown in situ on the surface of the FTO conductive glass.
[0008] Furthermore, in step S1, the annealing process is carried out under a nitrogen atmosphere at a temperature of 400 °C.
[0009] Further, step S2 includes: S201: Spin-coat the surface of the nitrogen-doped TiO2 nanorod array with ZnO quantum dot suspension and perform a first low-temperature annealing treatment; S202: After the first low-temperature annealing treatment, the ZnO quantum dot suspension is spin-coated again onto the surface of the nitrogen-doped TiO2 nanorod array, and a second low-temperature annealing treatment is performed to allow ZnO quantum dots to be deposited layer by layer and cover the surface of the nitrogen-doped TiO2 nanorod array, forming the ZnO quantum dot heterolayer.
[0010] Furthermore, the annealing temperature for both the first and second low-temperature annealing treatments is 150 °C.
[0011] Furthermore, in step S3, the final low-temperature annealing process is the second low-temperature annealing process, and the wavelength of the ultraviolet light is 405 nm.
[0012] Furthermore, the shallow energy level defects are formed by nitrogen being doped into the TiO2 lattice in the form of interstitial doping; the interface defects are oxygen vacancies at the interface of the heterojunction.
[0013] Furthermore, in step S4, the metal top electrode is an Au electrode, which is deposited on the surface of the ZnO quantum dot heterolayer by sputtering.
[0014] This application also provides an artificial photoelectric synapse device, which is prepared by the preparation method described above; the artificial photoelectric synapse device includes an FTO conductive glass as a bottom electrode, a nitrogen-doped TiO2 nanorod array located on the surface of the FTO conductive glass, a ZnO quantum dot heterolayer covering the surface of the nitrogen-doped TiO2 nanorod array, and a metal top electrode located on the surface of the ZnO quantum dot heterolayer.
[0015] This application also provides the application of the artificial opto-synaptic device as described above in optical information encoding and storage or neuromorphic computing.
[0016] In summary, the beneficial effects of this application are as follows: 1. By using a hydrothermal method to grow nitrogen-doped TiO2 nanorod arrays in situ on the surface of FTO conductive glass and annealing to construct shallow energy level defects, ZnO quantum dots are repeatedly spin-coated on the surface of the nanorod array and stepwise low-temperature annealing is performed to form a ZnO quantum dot heterolayer to form a heterojunction and introduce deep energy level defects. During the final low-temperature annealing process, ultraviolet light irradiation is performed simultaneously to form interface defects at the heterojunction interface. The shallow energy level defects, deep energy level defects and interface defects together form a multi-level trap system. Under the action of the built-in electric field of the heterojunction, photogenerated electrons and holes can be rapidly separated and directionally transported. Photogenerated charge carriers are captured and stored step by step by traps of different energy levels. Electron-hole recombination is suppressed, and the lifetime and storage capacity of photogenerated charge carriers are improved. This improves the photoresponse performance, conductivity retention and synaptic plasticity of the device, which is conducive to realizing functions such as learning and memory, optical information encoding and storage and neuromorphic computing.
[0017] 2. By spin-coating ZnO quantum dot suspension at least twice and performing low-temperature annealing after each spin-coating, ZnO quantum dots are deposited layer by layer and cover the surface of nitrogen-doped TiO2 nanorod array. Compared with single deposition, this method is beneficial to improve the uniformity of ZnO quantum dots on the nanorod surface and their binding state with the nanorods, thereby improving the bonding quality and stability of the heterojunction interface and providing favorable conditions for the separation and transport of charge carriers at the interface.
[0018] 3. By simultaneously subjecting the heterojunction interface to ultraviolet light irradiation during the final low-temperature annealing process, the heterojunction interface is activated and interface defects are adjusted. This is beneficial for improving the bonding state of the heterojunction interface, optimizing the charge transport characteristics at the interface, and providing favorable conditions for the separation, transport, and storage of photogenerated carriers.
[0019] 4. In-situ nitrogen doping of TiO2 nanorods is achieved by introducing nitrogen-containing precursors into the reaction system and annealing under a nitrogen atmosphere to stabilize the doping state. Nitrogen is incorporated into the TiO2 lattice in the form of interstitial doping to form shallow energy level defects. While maintaining the orderly arrangement of the nanorod array, it provides storage centers for carrier capture, which is beneficial to improving the optical response and conductivity retention of the device. Attached Figure Description
[0020] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings: Figure 1 This is a flowchart illustrating the fabrication method of the artificial photoelectric synapse device in Example 1; Figure 2 This is a schematic diagram of the fabrication process of the artificial photoelectric synapse device in Example 1; Figure 3 The images show the morphology of the ZnO quantum dot heterolayer@nitrogen-doped TiO2 nanorod array heterostructure prepared in Example 1, where (a) is a top-view scanning electron microscope image, (b) is a cross-sectional scanning electron microscope image of the heterostructure grown on an FTO substrate, and (c) is a transmission electron microscope image of the heterostructure. Figure 4 The energy dispersive X-ray spectroscopy (EDS) elemental distribution diagrams of the heterostructure prepared in Example 1 are shown, where (a) is a top view of the elemental distribution diagrams of Ti, O, N and Zn, and (b) is a cross-sectional elemental distribution diagram of the heterostructure. Figure 5 High-resolution X-ray photoelectron spectroscopy (XPS) spectra of TiO2 nanorods, nitrogen-doped TiO2 nanorods, and heterostructures prepared in Example 1, where (a) is the Ti 2p spectrum, (b) is the O 1s spectrum, (c) is the N 1s spectrum, and (d) is the Zn 2p spectrum. Figure 6 The simulated resistive switching characteristics and corresponding current-time (It) response curves of the artificial photoelectric synapse device prepared in Example 1 under continuous positive and negative voltage scans; Figure 7The image shows the continuous photoconductivity response of the artificial photoelectric synapse device prepared in Example 1 under 405 nm illumination, where (a) is the continuous photoconductivity response curve of the device under different illumination intensities, and (b) is the photocurrent response curve of the device under different illumination times at a fixed light power density. Figure 8 The photocurrent response diagrams of the devices fabricated in Comparative Example 1 and Comparative Example 2 under 405 nm illumination are shown, where (a) shows the Au / TiO2 / FTO device of Comparative Example 1 under different illumination intensities (30–100 mW·cm). - (a) shows the photocurrent response and attenuation curves under a fixed illumination intensity of 30 mW·cm² (reading voltage is 0.1 V). (b) shows the photocurrent response and attenuation curves of the device in Comparative Example 1 under a fixed illumination intensity of 30 mW·cm². - Photocurrent response curves under different illumination times (5–25 s) are shown in Figure 2. (c) shows the Au / N-TiO2 / FTO device of Comparative Example 2 under different illumination intensities (30–100 mW·cm²). - ²) shows the photocurrent response and attenuation curves (reading voltage 0.1 V), and (d) shows the device of Comparative Example 2 at a fixed illumination intensity of 30 mW·cm². - Photocurrent response curves under different illumination times (5–25 s); Figure 9 The artificial photoelectric synapse device prepared in Example 1 was subjected to continuous light stimulation (20→50→20 mW·cm). - ²) Overthreshold sensitization response plot; Figure 10 The image shows the optical information encoding and two-dimensional pattern reconstruction of the artificial photoelectric synapse device prepared in Example 1. (a)-(d) are the photocurrent response diagrams corresponding to the 4-bit binary optical pulse signals (1000, 1010, 1011, 1111), (e) is the steady-state photocurrent statistical result diagram corresponding to different binary pulse sequences, and (f) is a schematic diagram of two-dimensional binary pattern reconstruction based on optical modulation of synaptic conductance. Detailed Implementation
[0021] To enable those skilled in the art to better understand the technical solutions of this application, the technical solutions of this application will be further described below in conjunction with the accompanying drawings and embodiments.
[0022] TiO2 nanorod arrays possess excellent ultraviolet light response, good chemical stability, and controllable growth characteristics, making them widely used in artificial optoelectronic synaptic devices. However, TiO2 nanorods suffer from problems such as rapid carrier recombination rates, short photogenerated carrier lifetimes, a single trap energy level distribution, and insufficient photoresponse sensitivity, which limit the synaptic plasticity and long-term retention performance of the devices. The scheme of constructing heterojunctions using ZnO quantum dots to modify TiO2 nanorods mainly focuses on the heterojunction itself, lacking control over the interface defect states, trap energy level distribution, and interface charge transport behavior. Furthermore, the interface bonding is relatively simple, and carrier recombination remains easy, resulting in shortcomings in long-term retention, continuous learning, and simulation of complex neuromorphic behaviors.
[0023] To address the aforementioned issues, the technical concept of this application is as follows: A nitrogen-doped TiO2 nanorod array is grown in situ on the surface of FTO conductive glass using a hydrothermal method, followed by annealing in a nitrogen atmosphere to stabilize the nitrogen doping state. This process maintains the ordered arrangement of the nanorod array while constructing stable shallow-level defects, providing carrier trapping and storage centers for interfacial charge capture. A ZnO quantum dot heterolayer is constructed on the surface of the nitrogen-doped TiO2 nanorod array using a multi-spin-coating-stepwise low-temperature annealing process. This allows ZnO quantum dots to uniformly cover the nanorod array surface layer by layer, forming a tightly bonded and uniformly covered heterojunction. This improves the bonding quality and stability of the heterojunction interface and introduces deep-level defects. During the final low-temperature annealing process, the heterojunction interface is simultaneously subjected to ultraviolet light irradiation to activate the interface, improve the bonding state of the heterojunction interface, and regulate interfacial defects. This creates interfacial defects at the heterojunction interface, optimizing the charge transport characteristics of the heterojunction interface. Shallow-level defects, deep-level defects, and interface defects together constitute a multi-level trap system. Under the influence of the built-in electric field of the heterojunction, photogenerated electrons and holes can be rapidly separated and directionally transported. Electrons are preferentially captured and stored by traps of different energy levels, effectively suppressing electron-hole recombination and improving the lifetime and storage capacity of photogenerated carriers. At the same time, the uniform and dense heterolayer enhances the interface contact quality and carrier transport efficiency, giving the device excellent photoresponse performance, long-term retention performance, and synaptic plasticity, enabling functions such as learning and memory, associative learning, and complex neuromorphic computing.
[0024] The raw materials, reagents, and instruments used in the embodiments of this application are described below: FTO conductive glass: Fluorine-doped tin oxide conductive glass, commercially available, used as both a growth substrate and bottom electrode.
[0025] Tetrabutyl titanate, urea, and hydrochloric acid: all are commercially available analytical grade reagents and require no further purification.
[0026] ZnO quantum dot suspension: Zinc oxide quantum dots (ZnO QDs) were synthesized using a solvothermal method. The specific steps are as follows: 0.33 g of zinc acetate dihydrate was dissolved in 14 mL of ethanol by magnetic stirring at 60 °C to obtain a zinc acetate ethanol solution. Separately, 0.16 g of potassium hydroxide (KOH) was added to 7.7 mL of ethanol and sonicated to prepare a potassium hydroxide ethanol solution. Then, under vigorous stirring and while maintaining the reaction temperature at 60 °C, the potassium hydroxide ethanol solution was added dropwise to the zinc acetate ethanol solution. After the addition was complete, the mixture was stirred at 60 °C for 60 min. The system was allowed to cool naturally to room temperature to obtain a transparent zinc oxide quantum dot solution.
[0027] Nitrogen: Commercially available high-purity nitrogen.
[0028] Ultraviolet light source: an ultraviolet light source with an emission wavelength of 405 nm.
[0029] Instruments and equipment: magnetic stirrer, hydrothermal reactor, spin coater, tube furnace, magnetron sputtering equipment, scanning electron microscope (SEM), transmission electron microscope (TEM), X-ray energy dispersive spectrometer (EDS), X-ray photoelectron spectrometer (XPS), semiconductor parameter analyzer, etc., are all conventional instruments and equipment in this field.
[0030] Example 1 In this embodiment, an artificial photoelectric synapse device is fabricated. The device structure is an Au / ZnO quantum dot heterolayer@nitrogen-doped TiO2 nanorod array / FTO end structure. The fabrication process is as follows: Figure 1 and Figure 2 As shown, the specific steps are as follows.
[0031] S1: A nitrogen-doped TiO2 nanorod array is grown in situ on the surface of FTO conductive glass using a hydrothermal method, and the nitrogen-doped TiO2 nanorod array is annealed to construct shallow level defects in the nitrogen-doped TiO2 nanorod array as carrier trapping and storage centers.
[0032] Furthermore, step S1 is detailed as follows: S101: Tetrabutyl titanate, urea, hydrochloric acid and water are mixed and magnetically stirred to obtain a hydrothermal reaction solution; the volume ratio of water to hydrochloric acid in the hydrothermal reaction solution is 1:1, and in this example, 10 mL of water and 10 mL of hydrochloric acid are used.
[0033] S102: FTO conductive glass is placed in a hydrothermal reaction solution for hydrothermal reaction, and nitrogen-doped TiO2 nanorod arrays are grown in situ on the surface of FTO conductive glass; urea is introduced into the reaction system as a nitrogen-containing precursor to achieve in-situ nitrogen doping of TiO2 nanorods.
[0034] Annealing treatment: The nitrogen-doped TiO2 nanorod array was annealed in a nitrogen atmosphere at a temperature of 400℃ to stabilize the nitrogen doping state, improve crystal quality and optimize defect distribution. While maintaining the orderly arrangement of the nanorod array, shallow level defects as carrier trapping and storage centers were constructed in the nitrogen-doped TiO2 nanorod array. The shallow level defects were formed by nitrogen being incorporated into the TiO2 lattice in the form of interstitial doping.
[0035] S2: Spin-coat a ZnO quantum dot suspension onto the surface of the nitrogen-doped TiO2 nanorod array. The spin-coating is performed at least twice, and a low-temperature annealing treatment is performed after each spin-coating. This allows ZnO quantum dots to be deposited layer by layer and cover the surface of the nitrogen-doped TiO2 nanorod array, forming a ZnO quantum dot heterolayer. The ZnO quantum dot heterolayer and the nitrogen-doped TiO2 nanorod array form a heterojunction and introduce deep-level defects. Furthermore, step S2 is detailed as follows: S201: A ZnO quantum dot suspension was spin-coated onto the surface of a nitrogen-doped TiO2 nanorod array and subjected to a first low-temperature annealing treatment at a temperature of 150 °C.
[0036] S202: After the first low-temperature annealing treatment, ZnO quantum dot suspension is spin-coated again on the surface of the nitrogen-doped TiO2 nanorod array, and a second low-temperature annealing treatment is performed. The annealing temperature of the second low-temperature annealing treatment is 150 ℃, so that ZnO quantum dots are deposited layer by layer and cover the surface of the nitrogen-doped TiO2 nanorod array to form a ZnO quantum dot heterolayer. The ZnO quantum dot heterolayer and the nitrogen-doped TiO2 nanorod array form a heterojunction and introduce deep energy level defects.
[0037] S3: During the final low-temperature annealing process, the interface of the heterojunction is simultaneously subjected to ultraviolet light irradiation to form interface defects at the interface of the heterojunction.
[0038] Specifically, during the second low-temperature annealing process, the interface of the heterojunction is simultaneously subjected to ultraviolet light irradiation treatment with a wavelength of 405 nm to activate the interface and adjust the interface defects of the heterojunction, so as to form interface defects at the interface of the heterojunction; the interface defects are oxygen vacancies at the interface of the heterojunction.
[0039] S4: A metal top electrode is deposited on the surface of the ZnO quantum dot heterolayer. The metal top electrode and the FTO conductive glass, which serves as the bottom electrode, form a two-end structure to obtain an artificial photoelectric synapse device.
[0040] Specifically, an Au electrode is deposited on the surface of a ZnO quantum dot heterolayer by sputtering as a metal top electrode. The metal top electrode and the FTO conductive glass, which serves as the bottom electrode, form a two-end structure, thus obtaining an artificial photoelectric synapse device.
[0041] The shallow level defects, deep level defects, and interface defects together constitute a multi-level trap system, which is used to capture and store photogenerated carriers step by step under the action of the built-in electric field of the heterojunction.
[0042] Furthermore, the following two comparative examples are also provided.
[0043] Comparative Example 1 Devices with both ends were fabricated using undoped TiO2 nanorod arrays: except that urea was not added to the hydrothermal reaction solution, the ZnO quantum dot suspension spin-coating and low-temperature annealing treatment in step S2 were omitted, and the ultraviolet light irradiation treatment in step S3 was omitted, the remaining processes were the same as in Example 1, resulting in Au / TiO2NR / FTO devices (where NR stands for nanorod). This device does not undergo controllable interface construction or multi-level carrier modulation.
[0044] Comparative Example 2 A two-end device was fabricated using a nitrogen-doped TiO2 nanorod array: except for omitting the ZnO quantum dot suspension spin-coating and low-temperature annealing treatment in step S2 and the ultraviolet light irradiation treatment in step S3, the remaining processes were the same as in Example 1, yielding an Au / N-TiO2NR / FTO device. This device only underwent in-situ nitrogen doping, without further constructing an interface-controllable heterostructure, and lacked a multi-level carrier synergistic regulation mechanism.
[0045] Furthermore, the structure and components of Example 1 were characterized.
[0046] Detection method: (1) Morphological characterization: The top view and cross-sectional morphology of the sample were observed by scanning electron microscopy, and the microstructure of the single nanorod was observed by transmission electron microscopy.
[0047] (2) Elemental composition and distribution: The elemental composition and spatial distribution of the composite film were analyzed by combining energy dispersive X-ray spectroscopy (EDS) with elemental surface scanning and full-spectrum scanning.
[0048] (3) Valence state and defect state of elements: High-resolution spectra of Ti 2p, O 1s, N 1s and Zn 2p were measured by X-ray photoelectron spectroscopy (XPS).
[0049] Characterization results: (1) SEM and TEM characterization: Figure 3In the image 'a', we have a low-magnification top-view scanning electron microscope image of the ZnO quantum dot heterolayer@nitrogen-doped TiO2 nanorod array prepared in Example 1. The nanorods grow vertically and densely on the entire FTO substrate, exhibiting excellent overall structural uniformity. Neither nitrogen doping nor ZnO quantum dot modification has destroyed the intrinsic one-dimensional vertical growth structure of the rutile phase TiO2 nanorods. No structural collapse or severe particle aggregation was observed on the film surface. Figure 3 b in the image is a cross-sectional scanning electron microscope image. The thin film is vertically stacked on the FTO conductive glass. The nanorods are of uniform length and the interface between the substrate and the thin film is clear, which proves that the composite nanorod array has grown completely. Figure 3 In the image, c is a transmission electron microscope image, showing that monodisperse ZnO quantum dots are tightly attached to the outer wall of a single nitrogen-doped TiO2 nanorod, with no obvious aggregation.
[0050] (2) EDS characterization: Figure 4 The top-view EDS elemental surface scan results of a show that the Ti, O, and N elemental signals are uniformly distributed throughout the entire nanorod matrix, proving that nitrogen is uniformly incorporated into the TiO2 lattice; the Zn elemental signal is uniformly distributed across the entire sample surface, confirming that the ZnO quantum dots are uniformly coated and there is no phase separation or local agglomeration. Figure 4 The EDS elemental surface scan results of section b show that Ti and O signals are only distributed in the nanorod layer above the FTO glass, N element is uniformly distributed throughout the entire TiO2 nanorod matrix, and Zn element only appears on the outer surface of the nanorod, which is completely consistent with the designed heterostructure.
[0051] (3) XPS characterization: Figure 5 High-resolution XPS spectra of TiO2NR, N-TiO2NR, and the sample prepared in Example 1 are shown. The results indicate that Ti elemental retention... 4+ In the valence state, N exists stably in the TiO2 lattice as interstitial doping, and ZnO quantum dots were successfully loaded onto the surface of the nitrogen-doped TiO2 nanorod array. After the heterostructure was built, the Ti 2p peak shifted towards lower binding energy, and the O 1s defect peak was enhanced, indicating that the interface electronic environment and defect state were optimized. The above results demonstrate that the controllable construction of the heterojunction interface was achieved through in-situ nitrogen doping, heterolayer construction, and interface modulation, providing a structural basis for multi-level carrier modulation.
[0052] Furthermore, the electrical and photoelectric performance of the above embodiments and comparative examples were tested.
[0053] Detection method: The device was subjected to electrical and photoelectric tests using a semiconductor parameter analyzer. The device has a two-end structure, with the metal top electrode and bottom electrode connected to the test probes respectively. In the photoelectric test, ultraviolet light with a wavelength of 405 nm was used as the photostimulation signal, and the reading voltage was 0.1 V.
[0054] Electrical stimulation modulation performance: The device prepared in Example 1 was subjected to continuous positive and negative voltage scan modulation tests. The positive voltage scan range was 0~4V, the scan rate was 4V / s, and it was executed for 10 cycles. The negative voltage scan range was 0~-4V, the scan rate was 4V / s, and it was executed for 10 cycles. The results are as follows: Figure 6 As shown, the device exhibits stable analog resistance switching characteristics under continuous positive and negative voltage scans. Its conductance can be continuously and reversibly modulated, and it possesses good cyclic stability and repeatability. Thanks to the controllable interface construction and multi-level carrier modulation, the device can achieve stable conductance state regulation, providing support for the learning, memory, and neuromorphic computing functions of artificial photoelectric synapses.
[0055] Photoelectric response and continuous photoconductive properties: The photoelectric response of the device prepared in Example 1 was tested, and the results are as follows: Figure 7 As shown, under 405 nm ultraviolet light irradiation, the device exhibits a stable photoresponse: with increasing light intensity, the photocurrent gradually increases, demonstrating good light intensity-dependent characteristics; with prolonged illumination time, the photocurrent further increases, and it maintains a high conductivity state even after the light is removed, exhibiting significant continuous photoconductivity (PPC) characteristics. The device can achieve continuous control of its conductivity state by adjusting the light intensity and illumination time, thus simulating photosynaptic functions such as short-term and long-term memory.
[0056] Figure 8 The photocurrent response of devices in Comparative Example 1 and Comparative Example 2 under 405 nm illumination: Device in Comparative Example 1 under different illumination intensities (30–100 mW·cm²) - Photocurrent response and attenuation curves under 2) and at a fixed illumination intensity of 30 mW·cm² - The photocurrent response curves under different illumination times (5–25 s)² show that the TiO2 nanorod devices without controllable interface construction and multi-level carrier regulation have weak photoresponse, insignificant sustained photoconductivity, poor conductivity retention, and difficulty in achieving stable photosynaptic plasticity. The test results of the device in Comparative Example 2 show that in-situ nitrogen doping can improve the photoresponse performance of the device to a certain extent and achieve preliminary photoinduced memory function. However, due to the lack of further construction of controllable interface heterostructure and the absence of multi-level carrier synergistic regulation mechanism, the sustained photoconductivity, conductivity retention, and synaptic plasticity of the device are still limited.
[0057] Overthreshold sensitization characteristics: The device prepared in Example 1 was subjected to stimulation tests using light irradiation of different intensities, with the light intensity ranging from 20 to 50 to 20 mW·cm⁻¹. - The order of ² changes continuously, and the result is as follows: Figure 9As shown, after being subjected to strong light stimulation, the device exhibits an enhanced photoelectric response to subsequent weak light stimulation, demonstrating photostimulation sensitization and stimulation intensity recognition capabilities, which can simulate the response behavior of biological nociceptors. This performance is attributed to the improvement of heterojunction interface carrier transport and storage characteristics through controllable interface construction and multi-level carrier modulation strategies, enabling the device to possess photostimulation memory, adaptive response, and neuromorphic information processing capabilities.
[0058] Optical information encoding and two-dimensional pattern reconstruction: Based on the device's excellent continuous photoconductivity, 405 nm ultraviolet light was used as the photostimulation signal to perform optical information encoding and storage tests on the device prepared in Example 1. The results are as follows: Figure 10 As shown, when a 4-bit binary optical pulse signal (1000, 1010, 1011, 1111) is input, the device can generate a stable and distinguishable photocurrent response. Different binary pulse sequences correspond to different steady-state photocurrents, realizing the effective conversion of optical signals to electrical signals and information recognition. Furthermore, based on optical modulation synaptic conductance, two-dimensional binary pattern reconstruction is completed to realize the encoding and storage of optical information.
[0059] Furthermore, based on performance testing, the artificial photoelectric synapse device prepared in Example 1 can be used for optical information encoding and storage or neuromorphic computing: In terms of optical information encoding and storage, the device generates a distinguishable steady-state photocurrent response to a 4-bit binary optical pulse sequence based on its continuous photoconductive properties, and can complete two-dimensional optical information reconstruction (see...). Figure 10 In neuromorphic computing, the device possesses synaptic plasticity functions such as continuous reversible modulation of conductance, switching between short-term and long-term memory, photostimulation sensitization, and stimulation intensity recognition (see...). Figure 6 , Figure 7 , Figure 9 It can be used for learning and memory, associative learning and complex neuromorphic computing, and has good application prospects in fields such as artificial visual perception, intelligent information processing and neuromorphic computing.
[0060] In summary, by Figures 3 to 5 As can be seen, Example 1 obtained a ZnO quantum dot heterostructure @ nitrogen-doped TiO2 nanorod array heterostructure with complete structure, uniform coverage, and tight interface bonding through hydrothermal in-situ nitrogen doping, multiple spin coating-stepwise low-temperature annealing and simultaneous ultraviolet light irradiation treatment. Nitrogen was uniformly incorporated into the TiO2 lattice in the form of interstitial doping, and ZnO quantum dots were only distributed on the outer surface of the nanorods. The electronic environment and defect state of the heterojunction interface were optimized, providing a structural basis for a multi-level trap system composed of shallow energy level defects, deep energy level defects and interface defects.
[0061] Depend on Figure 7 and Figure 8The comparison shows that: the TiO2 nanorod device in Comparative Example 1 has a single trap level distribution, fast recombination of photogenerated carriers, weak photoresponse, and insignificant sustained photoconductivity; the photoresponse of Comparative Example 2 is improved after the introduction of nitrogen-doped shallow level defects, but it lacks the synergistic effect of the heterojunction built-in electric field, deep level defects, and interface defects, and the carrier storage capacity is still limited; the device in Example 1, under the action of the built-in electric field, rapidly separates and directionally transports photogenerated electrons and holes. Electrons are captured and stored step by step by shallow level defects, deep level defects, and interface defects, effectively suppressing electron-hole recombination. The lifetime and storage capacity of photogenerated carriers are significantly improved, thus exhibiting excellent photoresponse performance, sustained photoconductivity characteristics, and conductivity retention ability.
[0062] Depend on Figure 6 , Figure 9 , Figure 10 It can be seen that the multi-level trap system and controllable interface construction enable the device to have stable continuous conductance modulation capability, over-threshold sensitization capability and optical information encoding and storage capability. The overall performance of the device is better than that of the device without controllable interface construction and multi-level carrier regulation.
[0063] The foregoing has shown and described the basic principles, main features, and advantages of this application. Those skilled in the art should understand that this application is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of this application. Various changes and modifications can be made to this application without departing from the spirit and scope thereof, and all such changes and modifications fall within the scope of this application as claimed. The scope of protection of this application is defined by the appended claims and their equivalents.
Claims
1. A method for fabricating an artificial photoelectric synapse device, characterized in that, Includes the following steps: S1: Nitrogen-doped TiO2 nanorod arrays are grown in situ on the surface of FTO conductive glass using a hydrothermal method, and the nitrogen-doped TiO2 nanorod arrays are annealed to construct shallow level defects in the nitrogen-doped TiO2 nanorod arrays as carrier trapping and storage centers. S2: Spin-coat a ZnO quantum dot suspension onto the surface of the nitrogen-doped TiO2 nanorod array. The spin-coating is performed at least twice, and a low-temperature annealing treatment is performed after each spin-coating. This allows ZnO quantum dots to be deposited layer by layer and cover the surface of the nitrogen-doped TiO2 nanorod array, forming a ZnO quantum dot heterolayer. The ZnO quantum dot heterolayer and the nitrogen-doped TiO2 nanorod array form a heterojunction and introduce deep-level defects. S3: During the last low-temperature annealing process, the interface of the heterojunction is simultaneously subjected to ultraviolet light irradiation to form interface defects at the interface of the heterojunction. S4: Deposit a metal top electrode on the surface of the ZnO quantum dot heterolayer. The metal top electrode and the FTO conductive glass, which serves as the bottom electrode, form a two-end structure to obtain an artificial photoelectric synapse device. The shallow level defects, deep level defects, and interface defects together constitute a multi-level trap system, which is used to capture and store photogenerated carriers step by step under the action of the built-in electric field of the heterojunction.
2. The preparation method according to claim 1, characterized in that, In step S1, the in-situ growth of nitrogen-doped TiO2 nanorod arrays on the surface of FTO conductive glass using a hydrothermal method includes: S101: Tetrabutyl titanate, urea, hydrochloric acid and water are mixed and stirred to obtain a hydrothermal reaction solution, wherein the volume ratio of water to hydrochloric acid in the hydrothermal reaction solution is 1:
1. S102: The FTO conductive glass is placed in the hydrothermal reaction solution to carry out a hydrothermal reaction, and the nitrogen-doped TiO2 nanorod array is grown in situ on the surface of the FTO conductive glass.
3. The preparation method according to claim 1 or 2, characterized in that, In step S1, the annealing process is carried out under a nitrogen atmosphere at a temperature of 400 °C.
4. The preparation method according to claim 1, characterized in that, Step S2 includes: S201: Spin-coat the surface of the nitrogen-doped TiO2 nanorod array with ZnO quantum dot suspension and perform a first low-temperature annealing treatment; S202: After the first low-temperature annealing treatment, the ZnO quantum dot suspension is spin-coated again onto the surface of the nitrogen-doped TiO2 nanorod array, and a second low-temperature annealing treatment is performed to allow ZnO quantum dots to be deposited layer by layer and cover the surface of the nitrogen-doped TiO2 nanorod array, forming the ZnO quantum dot heterolayer.
5. The preparation method according to claim 4, characterized in that, The annealing temperature for both the first and second low-temperature annealing processes is 150 °C.
6. The preparation method according to claim 4 or 5, characterized in that, In step S3, the last low-temperature annealing process is the second low-temperature annealing process, and the wavelength of the ultraviolet light is 405 nm.
7. The preparation method according to claim 1, characterized in that, The shallow energy level defects are formed by nitrogen being doped into the TiO2 lattice in the form of interstitial doping; the interface defects are oxygen vacancies at the interface of the heterojunction.
8. The preparation method according to claim 1, characterized in that, In step S4, the metal top electrode is an Au electrode, which is deposited on the surface of the ZnO quantum dot heterolayer by sputtering.
9. An artificial photoelectric synapse device, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 8; The artificial photoelectric synapse device includes an FTO conductive glass as a bottom electrode, a nitrogen-doped TiO2 nanorod array on the surface of the FTO conductive glass, a ZnO quantum dot heterolayer covering the surface of the nitrogen-doped TiO2 nanorod array, and a metal top electrode on the surface of the ZnO quantum dot heterolayer.
10. The application of the artificial opto-synaptic device as described in claim 9 in optical information encoding and storage or neuromorphic computing.