Liquid phase confined annealing and orientation-induced preparation method of selenium thin film solar cell
By employing liquid-phase confined annealing and orientation-induced methods, the problems of selenium sublimation loss and crystal orientation in selenium thin film preparation were solved, resulting in the preparation of high-quality selenium thin films and improving the photoelectric conversion performance and industrial application potential of selenium-based solar cells.
Patent Information
- Application Number
- CN202611454290.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-20
AI Technical Summary
In existing selenium thin film preparation processes, selenium sublimation loss is severe, leading to reduced film density and continuity. At the same time, crystal orientation has a significant impact on carrier transport, making it difficult to achieve the preparation of high-quality selenium thin films.
By employing liquid-phase confined annealing and orientation-inducing methods, an interface orientation-inducing layer is constructed on the surface of a selenium thin film to regulate selenium crystal growth and form a preferred orientation. Combined with a chemically inert liquid annealing environment, selenium sublimation loss is reduced and crystal orientation is optimized.
A selenium thin film with low defects, high density and preferred orientation was achieved, which improved the photoelectric conversion performance of selenium-based solar cells. The process is simple and suitable for large-area production.
Smart Images

Figure CN123146019A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of selenium thin-film solar cell technology, specifically to a method for preparing selenium thin-film solar cells using liquid-phase confined annealing and orientation-induced processes. Background Technology
[0002] Currently, silicon, copper indium gallium selenide (CIGS), and perovskite solar cells have achieved high photoelectric conversion efficiencies, but they still face challenges such as high manufacturing costs and insufficient stability of some materials. Therefore, developing new low-cost, environmentally friendly thin-film photovoltaic materials remains of great significance. Elemental selenium (Se) possesses advantages such as a wide bandgap (approximately 1.8–1.9 eV), high absorption coefficient, non-toxicity, and abundant resources, making it a promising candidate for indoor photovoltaics and wide-bandgap top-cell tandem solar cells. The controllable preparation of high-quality selenium thin films has become an important research direction in this field.
[0003] Currently, in the preparation of selenium thin films, amorphous selenium precursor layers are typically prepared by vacuum evaporation, followed by thermal annealing to achieve crystallization. Due to the high saturated vapor pressure of elemental selenium, it is prone to sublimation during annealing, leading to defects such as pinholes, vacancies, and component loss in the film, reducing its density and continuity. To mitigate selenium sublimation, studies have employed methods such as enclosed-space annealing and high-selenium partial pressure annealing to improve the annealing environment. However, there is still room for optimization in further reducing selenium loss and improving film integrity while achieving sufficient crystallization.
[0004] During the research process, the inventors discovered that using a high-boiling-point chemically inert liquid to construct a liquid-phase confined annealing environment can effectively reduce selenium sublimation loss during the annealing process, providing a new technical path for selenium thin film crystallization.
[0005] However, further research by the inventors revealed that while liquid-phase confined annealing can improve selenium sublimation and film integrity, the crystal orientation of the resulting selenium film has room for further control. Because selenium has a one-dimensional chain-like crystal structure, its carrier transport exhibits significant anisotropy, and crystal orientation has a crucial impact on carrier transport and device performance. Therefore, how to suppress selenium sublimation and improve film integrity while further controlling the crystal orientation of the selenium film to achieve a preferred orientation that facilitates longitudinal carrier transport is a technical problem that needs further resolution to obtain high-quality selenium films.
[0006] To address the aforementioned problems, this invention proposes a method for preparing selenium thin-film solar cells based on liquid-phase confined annealing and orientation-induced processes. Summary of the Invention
[0007] To address the aforementioned shortcomings of existing technologies, this invention provides a method for fabricating selenium thin-film solar cells using liquid-phase confined annealing and orientation-induced processes. This method utilizes a liquid-phase confined annealing environment to reduce selenium sublimation loss during annealing, thereby reducing sublimation defects. Simultaneously, by pre-constructing an interface orientation-inducing layer, the crystal growth and preferred orientation of the selenium thin film are controlled, promoting the formation of a favorable (101) preferred orientation. This achieves synergistic optimization of the defect state and crystal orientation of the selenium thin film, resulting in a low-defect, highly dense selenium thin film with preferred orientation, and improving the photoelectric conversion performance of selenium-based solar cells.
[0008] To achieve the above objectives, the present invention provides the following technical solution:
[0009] A method for fabricating selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced processes includes the following steps:
[0010] Step 1: Prepare an electron transport layer on the surface of a conductive substrate;
[0011] Step 2: Prepare an interface orientation induction layer with a thickness of 10~15 nm on the surface of the electron transport layer. The interface orientation induction layer provides an orientation induction interface for the selenium crystal and regulates its preferred orientation growth.
[0012] Step 3: Prepare an amorphous selenium precursor film on the surface of the interface orientation induction layer using vacuum evaporation;
[0013] Step 4: Immerse the substrate with the deposited amorphous selenium precursor film in a chemically inert liquid medium for heat preservation and annealing to obtain a crystalline selenium film with a preferred orientation of the (101) crystal plane; the boiling point of the chemically inert liquid medium is higher than the temperature of the heat preservation and annealing.
[0014] Step 5: Prepare a metal electrode on the surface of a crystalline selenium thin film to obtain a selenium-based solar cell device.
[0015] Furthermore, the conductive substrate is an FTO conductive glass substrate, and the electron transport layer is a dense TiO2 thin film.
[0016] Furthermore, dense TiO2 thin films were prepared on the surface of a conductive substrate using spraying, spin coating, and magnetron sputtering methods.
[0017] Furthermore, the interface orientation induction layer is a heterogeneous induction layer; the heterogeneous induction layer is made of chalcogenide or selenide.
[0018] Furthermore, the heterogeneous induction layer is made of Sb2Se3;
[0019] The heterogeneous induction layer is prepared by vacuum evaporation and then annealed at 250-350 °C for 25-30 min.
[0020] Furthermore, the thickness of the amorphous selenium precursor film is 500~800 nm.
[0021] Furthermore, the chemically inert liquid medium has a boiling point higher than the temperature of the heat preservation annealing, is chemically stable, does not react chemically with selenium and the functional layers of the selenium-based solar cell, and is capable of forming a continuous liquid-phase covering insulating liquid.
[0022] Furthermore, the chemically inert liquid medium is a perfluoropolyether with a boiling point or lower boiling range limit higher than 250 °C.
[0023] To better achieve the objectives of this invention, this invention also provides a selenium thin-film solar cell characterized by liquid-phase confined annealing and orientation-induced processes, comprising:
[0024] Conductive substrate;
[0025] An electron transport layer is disposed on the surface of the conductive substrate;
[0026] An interface orientation induction layer is disposed on the surface of the electron transport layer. The interface orientation induction layer is used to provide an orientation induction interface for the selenium crystal and regulate its preferred orientation growth.
[0027] A crystalline selenium film is disposed on the surface of the interface orientation induction layer, and the crystalline selenium film has a preferred crystal orientation.
[0028] A metal electrode is disposed on the surface of the crystalline selenium thin film.
[0029] Furthermore, the interface orientation induction layer has a thickness of 10~15 nm, which provides an orientation induction interface for the selenium crystal and regulates its preferred orientation growth on the (101) crystal plane; the thickness of the amorphous selenium precursor film is 500~800 nm.
[0030] Compared with the prior art, the beneficial effects of this invention are as follows:
[0031] (1) Liquid-phase confined annealing can reduce the sublimation loss of selenium during high-temperature annealing, reduce pinholes and local defects caused by selenium sublimation, and improve the density and crystal uniformity of selenium films.
[0032] (2) The interface orientation induction layer can regulate the crystal growth and preferred orientation of selenium thin films, and improve the preferred orientation degree that is conducive to the longitudinal transport of charge carriers.
[0033] (3) The synergistic effect of liquid-phase confined annealing and interface orientation-induced layer formation improves the crystal quality of the thin film and optimizes the crystal texture, thereby achieving simultaneous optimization of selenium thin film defect control and crystal orientation control, and improving the photoelectric conversion performance of selenium-based solar cells.
[0034] (4) The process of this invention is simple, has good compatibility with existing vacuum deposition processes, and the process parameters are easy to control. It is suitable for the preparation of large-area selenium thin films and selenium thin film solar cells and has good prospects for industrial application. Attached Figure Description
[0035] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.
[0036] Figure 1 The images shown are scanning electron microscope (SEM) images of the selenium thin films prepared in Example 1 and Comparative Examples 1-3. (a) corresponds to Example 1, (b) corresponds to Comparative Example 1, (c) corresponds to Comparative Example 2, and (d) corresponds to Comparative Example 3.
[0037] Figure 2 The figures show the X-ray diffraction (XRD) patterns of the selenium thin films prepared in Example 1 and Comparative Examples 1-3. The curves in the figures correspond to Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 from top to bottom.
[0038] Figure 3 This is a schematic diagram of the structure of the selenium-based solar cell device prepared according to the present invention.
[0039] Figure 4 The JV characteristic curve is shown for the selenium-based solar cell device prepared in Example 1 of this invention. Detailed Implementation
[0040] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0041] Example 1: A method for fabricating selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation, comprising the following steps:
[0042] Step 1, Substrate pretreatment and electron transport layer preparation: After ultrasonic cleaning of the FTO conductive glass substrate, a dense TiO2 film with a thickness of 30 nm is prepared on the surface of the FTO conductive glass substrate by spraying method as an electron transport layer.
[0043] Step 2: Prepare an ultrathin Sb2Se3 induced layer using vacuum evaporation: Place the substrate obtained in Step 1 in a vacuum evaporation apparatus and deposit an Sb2Se3 film on the surface of a dense TiO2 film. Monitor the thickness in real time using a film thickness gauge. Stop the deposition when the thickness reaches 15 nm. Then anneal on a hot stage at 300℃ for 30 min to form an ultrathin Sb2Se3 induced layer.
[0044] Step 3: Deposition of amorphous selenium precursor layer: An 800 nm thick amorphous selenium precursor film is prepared on the surface of the ultrathin Sb2Se3 induced layer using a vacuum evaporation equipment.
[0045] Step 4, Liquid-phase confined annealing and crystallization: Add 100 mL of perfluoropolyether (PFPE) to a beaker and preheat it to 200 °C in an oven; completely immerse the substrate with the amorphous selenium precursor film deposited in Step 3 in the preheated PFPE, anneal at 200 °C for 5 min, and then remove it. Preferably, use a low-boiling-point (boiling point less than 150 °C, preferably 55–135 °C) PFPE cleaning agent to remove the residual liquid phase medium on the surface and dry it to obtain a crystalline selenium film.
[0046] Since the annealing temperature of selenium films is not higher than 220 ℃, in order to ensure that the perfluoropolyether can maintain a stable liquid phase environment during the annealing process, perfluoropolyether with a boiling point or lower limit of boiling range higher than 250 ℃ is preferred as the liquid phase annealing medium.
[0047] like Figure 1 As shown, the selenium thin film prepared in this embodiment uniformly covers the substrate, without defects such as pores or shedding, and the maximum grain size can reach 3 μm.
[0048] like Figure 2 As shown, an ultrathin Sb₂Se₃ orientation-inducing layer was prepared by vacuum evaporation and then subjected to thermal annealing to promote its crystallization; subsequently, amorphous selenium was deposited on the surface of the Sb₂Se₃ orientation-inducing layer. After crystallization annealing, the resulting selenium film exhibited a significantly enhanced (101) preferred orientation, indicating that the introduction of the annealed Sb₂Se₃ inducing layer can effectively control the crystal orientation of the Se film and promote the formation of Se (101) preferred orientation.
[0049] Step 5, Device Fabrication and Performance Testing: A 100 nm thick gold back electrode was fabricated on the surface of a crystalline selenium thin film using vacuum evaporation to obtain a selenium-based solar cell device, the structure of which is shown below. Figure 3 As shown.
[0050] Under standard simulated sunlight (AM 1.5G, 100 mW·cm²) -2 The photoelectric performance of the prepared selenium thin-film solar cell device was tested under irradiation conditions. During the test, the effective area of the device was 0.09 cm². 2 .like Figure 4 As shown, the J-V curve of this device exhibits typical photovoltaic response characteristics, with an open-circuit voltage of 901 mV and a short-circuit current density of 11.93 mA·cm⁻¹. -2 With a fill factor of 56.8% and a photoelectric conversion efficiency of 6.11%, the selenium thin-film solar cell based on liquid-phase confined annealing and orientation-induced conversion exhibits superior photoelectric conversion performance.
[0051] Example 2: A method for fabricating selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation, comprising the following steps:
[0052] Step 1, Substrate pretreatment and electron transport layer preparation: After ultrasonic cleaning of the FTO conductive glass substrate, a dense TiO2 film with a thickness of 30 nm was prepared on the surface of the FTO conductive glass substrate by spin coating as an electron transport layer.
[0053] Step 2: Prepare an ultrathin Sb2Se3 induced layer using vacuum evaporation: Place the substrate obtained in Step 1 in a vacuum evaporation apparatus and deposit an Sb2Se3 film on the surface of a dense TiO2 film. Monitor the thickness in real time using a film thickness gauge. Stop the deposition when the thickness reaches 10 nm. Then anneal on a hot stage at 350℃ for 25 min to form an ultrathin Sb2Se3 induced layer.
[0054] Step 3: Deposition of amorphous selenium precursor layer: A 500 nm thick amorphous selenium precursor film is prepared on the surface of the ultrathin Sb2Se3 induced layer using a vacuum evaporation equipment.
[0055] Step 4, Liquid-phase confined annealing and crystallization: Add 300 ml of perfluoropolyether (PFPE) to a beaker and preheat it to 180 °C in an oven; completely immerse the substrate with the amorphous selenium precursor film deposited in Step 3 in the preheated PFPE, anneal at 180 °C for 10 min, and then remove it. Preferably, use a low-boiling-point (boiling point less than 150 °C, preferably 55–135 °C) PFPE cleaning agent to remove the residual liquid phase medium on the surface and dry it to obtain a crystalline selenium film.
[0056] Since the annealing temperature of selenium films is not higher than 220 ℃, in order to ensure that the perfluoropolyether can maintain a stable liquid phase environment during the annealing process, perfluoropolyether with a boiling point or lower limit of boiling range higher than 250 ℃ is preferred as the liquid phase annealing medium.
[0057] Step 5, Device fabrication and performance testing: A gold back electrode with a thickness of 80 nm was fabricated on the surface of a crystalline selenium thin film using vacuum evaporation to obtain a selenium-based solar cell device.
[0058] The photoelectric performance of the prepared selenium thin-film solar cell device was tested under standard simulated sunlight irradiation conditions. The effective area of the device was 0.09 cm².2 Its open-circuit voltage is 899 mV, and its short-circuit current density is 11.91 mA·cm⁻¹. -2 The fill factor is 56.5%, and the device photoelectric conversion efficiency is 6.05%.
[0059] Example 3: A method for fabricating selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced processes, comprising the following steps:
[0060] Step 1, Substrate pretreatment and electron transport layer preparation: After ultrasonic cleaning of the FTO conductive glass substrate, a dense TiO2 film with a thickness of 30 nm was prepared on the surface of the FTO conductive glass substrate by spin coating as an electron transport layer.
[0061] Step 2: Prepare an ultrathin Sb2Se3 induced layer using vacuum evaporation: Place the substrate obtained in Step 1 in a vacuum evaporation apparatus and deposit an Sb2Se3 film on the surface of a dense TiO2 film. Monitor the thickness in real time using a film thickness gauge. Stop the deposition when the thickness reaches 10 nm. Then anneal on a hot stage at 250°C for 25 min to form an ultrathin Sb2Se3 induced layer.
[0062] Step 3: Deposit amorphous selenium precursor layer: A 600 nm thick amorphous selenium precursor film is prepared on the surface of the ultrathin Sb2Se3 induced layer using a vacuum evaporation equipment.
[0063] Step 4, Liquid-phase confined annealing and crystallization: Add 200 ml of perfluoropolyether (PFPE) to a beaker and preheat it to 180 °C in an oven; completely immerse the substrate with the amorphous selenium precursor film deposited in Step 3 in the preheated PFPE, anneal at 180 °C for 10 min, and then remove it. Preferably, use a low-boiling-point (boiling point less than 150 °C, preferably 55-135 °C) PFPE cleaning agent to remove the residual liquid phase medium on the surface and dry it to obtain a crystalline selenium film.
[0064] Since the annealing temperature of selenium films is not higher than 220 ℃, in order to ensure that the perfluoropolyether can maintain a stable liquid phase environment during the annealing process, perfluoropolyether with a boiling point or lower limit of boiling range higher than 250 ℃ is preferred as the liquid phase annealing medium.
[0065] Step 5, Device fabrication and performance testing: A gold back electrode with a thickness of 80 nm was fabricated on the surface of a crystalline selenium thin film using vacuum evaporation to obtain a selenium-based solar cell device.
[0066] The photoelectric performance of the prepared selenium thin-film solar cell device was tested under standard simulated sunlight irradiation conditions. The effective area of the device was 0.09 cm². 2 Its open-circuit voltage is 900 mV, and its short-circuit current density is 11.94 mA·cm⁻¹. -2The fill factor is 56.7%, and the device photoelectric conversion efficiency is 6.09%.
[0067] Comparative Example 1: Air annealing was used. The method for preparing a selenium thin-film solar cell includes the following steps:
[0068] Step 1, Substrate pretreatment and electron transport layer preparation: After ultrasonic cleaning of the FTO conductive glass substrate, a dense TiO2 film with a thickness of 30 nm is prepared on the surface of the FTO conductive glass substrate by spraying method as an electron transport layer.
[0069] Step 2: Prepare an ultrathin Sb2Se3 induced layer using vacuum evaporation: Place the substrate obtained in Step 1 in a vacuum evaporation apparatus and deposit an Sb2Se3 film on the surface of a dense TiO2 film. Monitor the thickness in real time using a film thickness gauge. Stop the deposition when the thickness reaches 15 nm. Then anneal on a hot stage at 300℃ for 30 min to form an ultrathin Sb2Se3 induced layer.
[0070] Step 3: Deposit amorphous selenium precursor layer: A 600 nm thick amorphous selenium precursor film is prepared on the surface of the ultrathin Sb2Se3 induced layer using a vacuum evaporation equipment.
[0071] Step 4, Air Annealing and Crystallization: The substrate with the amorphous selenium precursor film deposited in Step 3 is annealed in air at 200°C for 5 min to obtain a crystalline selenium film.
[0072] like Figure 1 As shown in Figure b, the Se film prepared in Comparative Example 1 has pores on its surface and relatively small grains. Figure 2 As shown, the Se thin film prepared in Comparative Example 1 exhibits a preferred orientation dominated by the (101) crystal plane.
[0073] Step 5, Device fabrication and performance testing: A gold back electrode with a thickness of 100 nm was fabricated on the surface of a crystalline selenium thin film using vacuum evaporation to obtain a selenium-based solar cell device.
[0074] The photoelectric performance of the prepared selenium thin-film solar cell device was tested under standard simulated sunlight irradiation conditions. The effective area of the device was 0.09 cm². 2 The device has a photoelectric conversion efficiency of 5.23%.
[0075] Compared to Example 1, Comparative Example 1 uses a liquid-phase confined annealing process, while Comparative Example 1 uses an air-heated stage annealing process. The photoelectric conversion efficiency of the device in Comparative Example 1 is significantly lower than that in Example 1. In the liquid-phase confined annealing process of Example 1, the liquid medium covers the surface of the selenium thin film, which helps to suppress the sublimation loss of selenium during the annealing process, reduce local material loss, and reduce the formation of defects such as pinholes, voids, and vacancies caused by selenium sublimation. At the same time, the liquid medium can provide a more uniform and stable thermal environment, which is conducive to the full growth of selenium grains, improves the compactness, continuity, and crystal quality of the film, thereby reducing defect-assisted recombination and improving carrier transport performance.
[0076] Comparative Example 2: No Sb₂Se₃ inducing layer was provided. The method for preparing a selenium thin-film solar cell includes the following steps:
[0077] Step 1, Substrate pretreatment and electron transport layer preparation: After ultrasonic cleaning of the FTO conductive glass substrate, a dense TiO2 film with a thickness of 30 nm is prepared on the surface of the FTO conductive glass substrate by spraying method as an electron transport layer.
[0078] Step 2, Deposition of amorphous selenium precursor layer: An 800 nm thick amorphous selenium precursor film is prepared on the surface of a dense TiO2 film using a vacuum evaporation device.
[0079] Step 3, Liquid-phase confined annealing and crystallization: Add 100 mL of perfluoropolyether (PFPE) to a beaker and preheat it to 200 °C in an oven; completely immerse the substrate with the amorphous selenium precursor film deposited in Step 2 into the preheated perfluoropolyether, anneal at 200 °C for 5 min, remove it, clean it to remove the residual liquid phase medium on the surface and dry it to obtain a crystalline selenium film.
[0080] like Figure 2 As shown, the selenium thin film prepared in Comparative Example 2 has a preferred orientation of the (100) crystal plane and parallel orientation of the selenium chains, resulting in a lower carrier transport efficiency. Figure 1 As shown in Figure c, the selenium thin film uniformly covers the substrate, without defects such as pores or shedding, and the maximum grain size can reach 3 μm.
[0081] Step 4, Device fabrication and performance testing: A gold back electrode with a thickness of 100 nm was fabricated on the surface of a crystalline selenium thin film using vacuum evaporation to obtain a selenium-based solar cell device.
[0082] The photoelectric performance of the prepared selenium thin-film solar cell device was tested under standard simulated sunlight irradiation conditions. The effective area of the device was 0.09 cm². 2 The device has a photoelectric conversion efficiency of 5.5%.
[0083] In Comparative Example 2, without the Sb₂Se₃ inducing layer, the selenium thin film crystal is mainly controlled by its own crystallization kinetics, and it usually tends to form a preferred orientation dominated by the (100) crystal plane. At this time, the selenium atom chains tend to be aligned parallel to the substrate, which is not conducive to the transport of charge carriers along the thickness direction of the film and easily increases the carrier recombination loss. In Example 1, after setting the Sb₂Se₃ inducing layer between the electron transport layer and the Se thin film, the resulting Se thin film exhibits a significantly enhanced (101) preferred orientation. The above comparative results show that the Sb₂Se₃ inducing layer can regulate the crystallization orientation of the Se thin film and promote the transformation of the Se thin film from a preferred orientation dominated by the (100) crystal plane to a preferred orientation dominated by the (101) crystal plane. Its function may be that the Sb2Se3 induced layer provides a heterogeneous nucleation interface with orientation selection for Se. By changing the interface formation energy and nucleation barrier of selenium nuclei with different orientations, the target orientation nuclei are preferentially formed and gradually form a preferred orientation during the subsequent competitive growth of grains. This promotes the transformation of the selenium film from a preferred orientation dominated by the (100) crystal plane to a preferred orientation dominated by the (101) crystal plane, thereby improving the transport and collection efficiency of charge carriers along the thickness direction of the film.
[0084] Comparative Example 3: No ultrathin Sb₂Se₃ inducing layer was provided, and air annealing was used. The method for fabricating a selenium thin-film solar cell includes the following steps:
[0085] Step 1, Substrate pretreatment and electron transport layer preparation: After ultrasonic cleaning of the FTO conductive glass substrate, a dense TiO2 film with a thickness of 30 nm is prepared on the surface of the FTO conductive glass substrate by spraying method as an electron transport layer.
[0086] Step 2, Deposition of amorphous selenium precursor layer: An 800 nm thick amorphous selenium precursor film is prepared on the surface of a dense TiO2 film using a vacuum evaporation device.
[0087] Step 3, Air Annealing and Crystallization: The substrate with the amorphous selenium precursor film deposited in Step 2 is annealed in air at 200°C for 5 min to obtain a crystalline selenium film.
[0088] like Figure 1 As shown in Figure d, the selenium film prepared in Comparative Example 3 has pores on its surface. Figure 2 As shown, the selenium thin film prepared in Comparative Example 3 has the (100) crystal plane as the preferred orientation.
[0089] Step 4, Device fabrication and performance testing: A gold back electrode with a thickness of 100 nm was fabricated on the surface of a crystalline selenium thin film using vacuum evaporation to obtain a selenium-based solar cell device.
[0090] The photoelectric performance of the prepared selenium thin-film solar cell device was tested under standard simulated sunlight irradiation conditions. The effective area of the device was 0.09 cm².2 The device has a photoelectric conversion efficiency of 5.02%.
[0091] This invention employs a combination of liquid-phase confined annealing and an interface orientation-inducing layer to synergistically regulate the crystallinity and orientation of selenium thin films. Liquid-phase confined annealing primarily suppresses selenium sublimation, reduces defect density, and improves film crystallinity, while the interface orientation-inducing layer mainly regulates the crystal orientation of the selenium thin film. Through the synergy of these two methods, the quality and orientation of the selenium thin film are simultaneously optimized, ultimately reducing carrier recombination losses and improving the photoelectric conversion performance of selenium thin-film solar cells.
[0092] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation, characterized in that, Includes the following steps: Step 1: Prepare an electron transport layer on the surface of a conductive substrate; Step 2: Prepare an interface orientation induction layer with a thickness of 10~15 nm on the surface of the electron transport layer. The interface orientation induction layer provides an orientation induction interface for the selenium crystal and regulates its preferred orientation growth. Step 3: Prepare an amorphous selenium precursor film on the surface of the interface orientation induction layer using vacuum evaporation; Step 4: Immerse the substrate with the deposited amorphous selenium precursor film in a chemically inert liquid medium for heat preservation and annealing to obtain a crystalline selenium film with a preferred orientation of the (101) crystal plane; the boiling point of the chemically inert liquid medium is higher than the temperature of the heat preservation and annealing. Step 5: Prepare a metal electrode on the surface of a crystalline selenium thin film to obtain a selenium-based solar cell device.
2. The method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation according to claim 1, characterized in that, The conductive substrate is an FTO conductive glass substrate, and the electron transport layer is a dense TiO2 thin film.
3. The method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation according to claim 1, characterized in that, Dense TiO2 thin films were prepared on the surface of conductive substrates using spraying, spin coating, and magnetron sputtering methods.
4. The method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation according to claim 3, characterized in that, The interface orientation induction layer is a heterogeneous induction layer; the heterogeneous induction layer is made of chalcogenide.
5. The method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation according to claim 4, characterized in that, The heterogeneous induction layer is made of Sb2Se3; The heterogeneous induction layer is prepared by vacuum evaporation and then annealed at 250-350 °C for 25-30 min.
6. The method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation according to claim 5, characterized in that, The thickness of the amorphous selenium precursor film is 500~800 nm.
7. The method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation according to claim 6, characterized in that, The chemically inert liquid medium is a liquid with a boiling point higher than the temperature of the heat preservation annealing, stable chemical properties, and does not react chemically with selenium or the functional layers of the selenium-based solar cell, and can form a continuous liquid phase covering insulating liquid.
8. The method for preparing selenium thin-film solar cells by liquid-phase confined annealing and orientation-induced oxidation according to claim 7, characterized in that, The chemically inert liquid medium is a perfluoropolyether with a boiling point or lower boiling range limit higher than 250°C.
9. A selenium thin-film solar cell subjected to liquid-phase confined annealing and orientation-induced polymerization, characterized in that, include: Conductive substrate; An electron transport layer is disposed on the surface of the conductive substrate; An interface orientation induction layer is disposed on the surface of the electron transport layer. The interface orientation induction layer is used to provide an orientation induction interface for the selenium crystal and regulate its preferred orientation growth. A crystalline selenium film is disposed on the surface of the interface orientation induction layer, and the crystalline selenium film has a preferred crystal orientation. A metal electrode is disposed on the surface of the crystalline selenium thin film.
10. The selenium thin-film solar cell according to claim 9, characterized in that, The interface orientation induction layer has a thickness of 10~15 nm. The interface orientation induction layer provides an orientation induction interface for the selenium crystal and regulates its preferential orientation growth on the (101) crystal plane. The thickness of the amorphous selenium precursor film is 500~800 nm.