Semiconductor structure and method of manufacturing the same

The high-temperature silicon ion implantation process solves the problems of reduced critical opening size and sidewall damage caused by room-temperature silicon ion implantation, improving the morphological uniformity and processing convenience of semiconductor structures, especially addressing the recess problem in the core logic region and input/output region.

CN123146145APending Publication Date: 2026-11-20SHANGHAI HUALI INTEGRATED CIRCUIT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611330143.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, the reduction in critical aperture size and sidewall implantation damage caused by room temperature silicon ion implantation processes are particularly severe in the core logic region, affecting device design performance.

Method used

High-temperature silicon ion implantation is used to treat the front-end devices on the semiconductor substrate at high temperatures of 200℃ to 500℃. This process involves comprehensive ion implantation to repair lattice defects, reduce sidewall deformation, and improve the reduction of aperture and the depression of the interlayer dielectric layer.

Benefits of technology

High-temperature silicon ion implantation significantly reduces the shrinkage of critical opening dimensions and sidewall deformation, improves the pitting problem of interlayer dielectric layers, and enhances the morphological uniformity and fabrication ease of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146145A_ABST
    Figure CN123146145A_ABST
Patent Text Reader

Abstract

The application provides a semiconductor structure and a preparation method thereof, wherein the preparation method of the semiconductor structure comprises the following steps: providing a semiconductor substrate, and forming a front-end device containing a dummy gate, a sidewall and an interlayer dielectric layer successively on the side of the dummy gate on the semiconductor substrate; performing a high-temperature silicon ion implantation process on the front-end device, wherein the temperature of the high-temperature silicon ion implantation process is 200-500 DEG C; and removing the dummy gate to form an opening. The application can repair implantation damage, reduce compressive stress, and further improve the phenomenon of opening reduction and the recess of the interlayer dielectric layer by means of the high-temperature silicon ion implantation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing, and more particularly to a semiconductor structure and its preparation method. Background Technology

[0002] See Figures 1-3 Existing techniques, when removing dummy gates, cause depressions 014 (dishing) to form on the interlayer dielectric layer 010 in the input / output (I / O) region 015 and the core logic region 016. Furthermore, during the etching process of the gate oxide layer 013 on the semiconductor substrate 017, the photoresist patterned windows only cover the core logic region 016, while the I / O region 015 has no photoresist windows and remains completely masked by the photoresist. Therefore, during the etching process of the gate oxide layer 013, the oxide of the interlayer dielectric layer 010 in the core logic region 016 is further consumed, resulting in severe depressions.

[0003] The core logic region 016 integrates short-channel (SC) and / or long-channel (LC) devices, and the longer the channel, the more severe the recess. Differences in recess cause variations in the chemical mechanical polishing (MG) patterning loading effect of the metal gate 019 within the gate recess 018, thus affecting design specifications. Therefore, it is particularly necessary to improve the recess 014 of the core logic region 016. Currently, after performing chemical mechanical polishing (CMP) on the interlayer dielectric layer 010, room-temperature silicon ion implantation (Si IMP) can be used to improve the recess of the interlayer dielectric layer 010.

[0004] However, during room-temperature silicon ion implantation, the sidewalls 011 on the dummy gate side undergo pre-amorphization implantation, transforming them into an amorphous layer structure. This implantation damage causes volume expansion and lattice distortion of the sidewalls 011, generating compressive stress. During subsequent etching to remove the dummy gate, this compressive stress leads to a reduction in the critical dimension of the opening 012. The higher the implantation energy, the greater the degree of implantation damage, the greater the compressive stress, and the more severe the reduction in the critical dimension of the opening 012. Therefore, how to suppress the reduction in the critical dimension of the opening 012 has become a pressing technical challenge in this field. Summary of the Invention

[0005] The purpose of this invention is to provide a semiconductor structure and its fabrication method to solve the problem of reduced critical size of the opening caused by implantation damage.

[0006] To address the aforementioned technical problems, this invention provides a method for fabricating a semiconductor structure, comprising the following steps:

[0007] A semiconductor substrate is provided, and a front-end device comprising a dummy gate and a sidewall and an interlayer dielectric layer sequentially located on the side of the dummy gate is formed on the semiconductor substrate;

[0008] The front-end device is subjected to a high-temperature silicon ion implantation process, wherein the temperature of the high-temperature silicon ion implantation process is 200℃~500℃.

[0009] Remove the dummy gate to form an opening.

[0010] Optionally, the sidewall includes a first sidewall and a second sidewall sequentially covering the dummy gate sidewall, wherein the first sidewall is made of silicon nitride and the second sidewall is made of a low-k material.

[0011] Optionally, the process for removing the dummy gate includes a polysilicon removal process.

[0012] Optionally, the polysilicon removal process includes performing a dry etching process and a wet etching process sequentially on the dummy gate.

[0013] Optionally, the front-end device further includes a gate oxide layer located between the dummy gate and the semiconductor substrate.

[0014] Optionally, the semiconductor substrate is made of silicon, the dummy gate is made of polycrystalline silicon, and the gate oxide layer is made of silicon dioxide.

[0015] Optionally, after the step of removing the dummy gate, the method for fabricating the semiconductor structure further includes: etching the gate oxide layer to remove the gate oxide layer and increase the depth of the opening to form a gate trench.

[0016] Optionally, after etching the gate oxide layer, the method for fabricating the semiconductor structure further includes: fabricating a metal gate within the gate recess.

[0017] Optionally, after the step of fabricating the metal gate in the gate recess, the method for fabricating the semiconductor structure further includes: observing the morphology of the metal gate using a transmission electron microscope.

[0018] Optionally, the energy of the high-temperature silicon ion implantation process is 1Kev to 5Kev.

[0019] Optionally, the implantation dose of the high-temperature silicon ion implantation process is 5 × 10⁻⁶. 15 atom / cm 2 ~2×10 16 atom / cm 2 .

[0020] Optionally, the high-temperature silicon ion implantation process includes a comprehensive ion implantation process.

[0021] To address the aforementioned technical problems, the present invention also provides a semiconductor structure, which is prepared by the semiconductor structure preparation method described above.

[0022] The semiconductor structure and its fabrication method provided by this invention perform a high-temperature silicon ion implantation process on the front-end device on the semiconductor substrate. The high-temperature silicon ion implantation process can maintain a stable high temperature. During the implantation process, lattice defects generated by ion implantation are quickly repaired, and implantation damage to the sidewalls is repaired, thereby reducing the deformation of the sidewalls and thus improving the problem of reduced opening size.

[0023] In addition to improving the reduction of the opening, the semiconductor structure and its fabrication method provided by this invention further improve the problem of interlayer dielectric layer depression by accelerating the formation of silicon-rich materials. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of the semiconductor structure after removing the dummy gate in the prior art;

[0025] Figure 2 This is a schematic diagram of a semiconductor structure after etching the gate oxide layer in the prior art;

[0026] Figure 3 This is a schematic diagram of the semiconductor structure after the metal gate is fabricated in the prior art;

[0027] Figure 4 This is a schematic flowchart of a method for preparing a semiconductor structure according to an embodiment of the present invention;

[0028] Figure 5 This is a schematic diagram of the semiconductor structure of the front-end device before the high-temperature silicon ion implantation process is performed in one embodiment of the present invention;

[0029] Figure 6 This is a schematic diagram of the semiconductor structure before the opening is improved in one embodiment of the present invention;

[0030] Figure 7 This is a schematic diagram of the semiconductor structure with improved opening in one embodiment of the present invention;

[0031] in, Figures 1-3 middle:

[0032] 010-Interlayer dielectric layer, 011-Sidewall, 012-Opening, 013-Gate oxide layer, 014-Recess, 015-Input / output area, 016-Core logic area, 017-Semiconductor substrate, 018-Gate groove, 019-Metal gate;

[0033] Figures 5-7 middle:

[0034] 100 - Interlayer dielectric layer, 110 - Sidewall, 1101 - First sidewall, 1102 - Second sidewall, 120 - Pseudo-gate, 130 - Gate oxide layer, 140 - Input / output region, 150 - Core logic region, 160 - Semiconductor substrate, 170 - Opening. Detailed Implementation

[0035] The semiconductor structure and its fabrication method proposed in this invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. The advantages and features of this invention will become clearer from the following description and claims. It should be noted that the drawings are all in a very simplified form and use non-precise proportions, and are only used to facilitate and clarify the illustration of the embodiments of this invention.

[0036] In the description of embodiments of this disclosure, the term "comprising" and similar terms should be understood as open-ended inclusion, i.e. "including but not limited to", and the terms "first", "second", and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0037] Existing room-temperature silicon ion implantation processes tend to generate amorphous layers and cause aperture shrinkage, a defect particularly pronounced in the core logic region. This invention aims to improve the aperture shrinkage and abnormal depth issues in the core logic region. Based on this, Figure 4 This is a schematic flowchart of a method for fabricating a semiconductor structure according to an embodiment of the present invention. The method for fabricating the semiconductor structure may include the following steps:

[0038] Step S1: Provide a semiconductor substrate 160, and form a front-end device on the semiconductor substrate 160 including a dummy gate 120 and a sidewall 110 and an interlayer dielectric layer 100 sequentially located on the side of the dummy gate 120.

[0039] Step S2: Perform a high-temperature silicon ion implantation process on the front-end device, wherein the temperature of the high-temperature silicon ion implantation process is 200℃~500℃;

[0040] Step S3: Remove the dummy gate 120 to form an opening.

[0041] Please see Figure 5The semiconductor substrate 160 may include an input / output region 140 and a core logic region 150. The figure shows the input / output region 140 and the core logic region 150. The input / output region 140 is used to form input / output devices, and the core logic region 150 is used to form core logic devices. In step S1, the material of the semiconductor substrate 160 may be silicon, silicon carbide, or silicon-germanium, but is not limited to these. The front-end device may also include a gate oxide layer 130, located between the dummy gate 120 and the semiconductor substrate 160, with the dummy gate 120 stacked on top of the gate oxide layer 130. The dummy gate 120 is preferably made of polysilicon, and the gate oxide layer 130 is preferably made of silicon dioxide. Furthermore, the sidewall 110 may include a first sidewall 1101 and a second sidewall 1102 sequentially covering the side of the dummy gate 120. The first sidewall 1101 is preferably made of silicon nitride, and the second sidewall 1102 is preferably made of a low-k material.

[0042] In this embodiment, to facilitate the high-temperature silicon ion implantation process for the front-end device, the interlayer dielectric layer 100 extending over the upper surface of the dummy gate 120 can be chemically mechanically polished during the fabrication of the front-end device to remove the portion of the interlayer dielectric layer 100 extending over the upper surface of the dummy gate 120, thereby exposing the upper surface of the dummy gate 120. The thickness of the removed interlayer dielectric layer 100 extending over the upper surface of the dummy gate 120 can be 500 Å to 1000 Å.

[0043] In step S2, the high-temperature silicon ion implantation process is preferably a blanket implantation process. This blanket implantation process not only saves one mask layer but also reduces process steps and costs. The preferred temperature for the high-temperature silicon ion implantation process is 200℃~500℃, the preferred energy is 1Kev~5Kev, and the preferred dose is 5×10⁻⁶. 15 atom / cm 2 ~2×10 16 atom / cm 2Compared to room-temperature silicon ion implantation, this embodiment uses a higher temperature to heat the front-end device, ensuring that the front-end device maintains a stable higher temperature. The high-temperature environment not only provides the energy for immediate repair of displaced lattice atoms but also dynamically repairs some damage, reducing the generation of pre-amorphization implantation. The underlying physical mechanism is that ion implantation forms pairs of vacancies and interstitial atoms, and high-temperature implantation increases the recombination probability of these atoms, thereby improving implantation damage. Therefore, under high-temperature conditions, lattice defects generated by silicon ion implantation are rapidly repaired, significantly reducing implantation damage.

[0044] Meanwhile, the high-temperature silicon ion implantation process generates a "dynamic annealing" effect. Due to the heat generated by the continuous bombardment of the high-temperature ion beam, lattice damage can be repaired to a certain extent during the manufacturing process. Therefore, the high-temperature silicon ion implantation process can effectively suppress the accumulation of damage and inhibit the formation of pre-amorphization implantation.

[0045] The high-temperature silicon ion implantation further repairs the sidewalls 110, reducing damage caused by ion implantation, thereby reducing lattice distortion and reducing compressive stress. Furthermore, the first sidewalls 1101 and 1102 can even reform stable chemical bonds with surrounding lattice atoms, reducing deformation of the first sidewalls 1101 and 1102, thus suppressing their expansion into the dummy gate 120 and improving the issue of reduced opening size.

[0046] In step S3, the process for removing the dummy gate 120 is preferably a polysilicon removal process (DPR). Further, the polysilicon removal process is preferably performed by sequentially performing a dry etching process and a wet etching process on the dummy gate 120. In this embodiment, by removing the dummy gate 120 to form an opening 170, and by adjusting the parameters of the dry etching process to expand the top of the dummy gate 120 and etching the sidewalls 110 into an inclined shape, the problem of reduced opening size is further improved, facilitating subsequent fabrication of the metal gate. The specific parameters of the dry etching process can be flexibly adjusted according to the actual product specifications. Please refer to [link to relevant documentation]. Figure 6 and Figure 7 In this embodiment, the size of the opening 170 has been significantly improved to facilitate subsequent fabrication of the metal gate. Figure 6 and Figure 7 All are simplified schematic diagrams of the core logic area 150. To highlight the improved key size optimization structure of the opening in this invention, the input / output area 140 has been omitted.

[0047] While improving the size of the opening 170, the high-temperature silicon ion implantation process can further alter the etching rate of the interlayer dielectric layer 100 oxide, reducing the depressions caused to the interlayer dielectric layer 100 oxide during subsequent etching. In this embodiment, after employing the high-temperature silicon ion implantation process, strong Si-Si bonds are introduced while Si-O bonds break. The reduction of Si-O bonds leads to a decrease in the reaction sites of hydrofluoric acid (HF) during etching, thereby reducing the etching rate of the interlayer dielectric layer 100 oxide by the Certas vapor phase chemical etching process. The introduction of silicon ions can also accelerate the formation of silicon-rich materials (e.g., silicon-rich silicon oxide, SiO₂). x (x<2) This reduces the activation of silicon dioxide, and the silicon-rich material is denser than pure silicon dioxide, making it more difficult for gas molecules to penetrate into the deep lattice of the material. Etching is limited to the outermost few atomic layers. If the etching uses a mixture of hydrogen fluoride and ammonia (HF-NH3), the silicon-rich material formed will reduce the activation of silicon dioxide due to the strong selectivity of the hydrogen fluoride and ammonia mixture for pure silicon dioxide. This reduces the reaction between the hydrogen fluoride and ammonia mixture and silicon dioxide, thereby reducing the depression of the interlayer dielectric layer 100.

[0048] In this embodiment, after step S3, i.e., after the step of removing the dummy gate 120, the method for fabricating the semiconductor structure may further include: etching the gate oxide layer 130 to remove the gate oxide layer 130 and increase the depth of the opening, thereby forming a gate trench. Since the gate oxide layer 130 in the input / output region has no photoresist window, and the photoresist patterned window only covers the core logic region 150, this embodiment only etches the gate oxide layer 130 in the core logic region 150. This embodiment etches the gate oxide layer 130 to remove it, thereby increasing the depth of the opening 170 and forming a gate trench, so that a metal gate can be subsequently fabricated within the gate trench.

[0049] After etching the gate oxide layer 130, the method for fabricating the semiconductor structure further includes: fabricating a metal gate within the gate trench. Specifically, a high-k hafnium dioxide gate dielectric layer is deposited within the gate trench, followed by the sequential deposition of a work function metal layer and a gate metal filling layer to form a high-k metal gate. In this embodiment, after fabricating the metal gate within the gate trench, input / output devices can be obtained in the input / output region 140, and core logic devices can be obtained in the core logic region 150.

[0050] Following the step of fabricating the metal gate within the gate recess, the semiconductor structure fabrication method further includes observing the morphology of the metal gate using a transmission electron microscope (TEM). The observation results show that, due to the significantly improved lateral dimensional uniformity of the opening 170 within the core logic region 150, the opening shrinkage phenomenon is significantly suppressed, resulting in better fabrication of the metal gate and greater convenience in fabricating the metal gate within the gate recess. The longitudinal depth of the recess in the interlayer dielectric layer 100 is also significantly improved, especially the dimensional deviation of the core logic region 150 integrating short-channel and / or long-channel devices is effectively improved, and the overall morphological uniformity of the device is superior to devices fabricated using existing technologies. Furthermore, the opening shrinkage and recess phenomena in the input / output region 140 are also well improved. The above-mentioned morphological improvement effects can be reproduced and verified using conventional transmission electron microscopy detection methods in the art.

[0051] This embodiment uses the core logic region 150 and the input / output region 140, which include short-channel devices SC and / or long-channel devices LC, as the processing objects, but it is not limited to this. The present invention can be adapted to various device regions. For the core logic region 150, which has particularly significant defects, it can significantly suppress the shrinkage problem of the opening 170 and alleviate the depression problem of the interlayer dielectric layer 100.

[0052] This embodiment also provides a semiconductor structure, which is fabricated using the semiconductor structure fabrication method described above, i.e., fabricated using at least steps S1 to S3. Specifically, the semiconductor structure may include: a semiconductor substrate 160, sidewalls 110, an interlayer dielectric layer 100, and an opening 170. The opening 170 in the semiconductor structure is obtained by removing a dummy gate 120, and the dummy gate 120, sidewalls 110, and interlayer dielectric layer 100 can be integrated into a front-end device. The sidewalls 110 and interlayer dielectric layer 100 are located on the side of the dummy gate 120, and the sidewalls 110 include a first sidewall 1101 and a second sidewall 1102 sequentially covering the side of the dummy gate 120. Furthermore, the front-end device may also include a gate oxide layer 130, which is located between the dummy gate 120 and the semiconductor substrate 160, with the dummy gate 120 stacked on top of the gate oxide layer 130. In this embodiment, a metal gate may also be further fabricated on the semiconductor structure. The critical size reduction problem of the opening 170 in the semiconductor structure provided in this embodiment has been significantly improved, and the depression problem of the interlayer dielectric layer 100 has also been further alleviated.

[0053] In summary, the semiconductor structure and its fabrication method provided in this invention repair the sidewalls on the dummy gate side by performing a high-temperature silicon ion implantation process on the semiconductor substrate, thereby reducing compressive stress and improving the problem of reduced opening size. Furthermore, while improving the opening size, this embodiment also further reduces the depression of the interlayer dielectric oxide layer. Ultimately, this embodiment successfully expands the openings in the input / output region and the core logic region while reducing the degree of depression in the interlayer dielectric layer.

[0054] The above description is merely a description of preferred embodiments of the present invention and is not intended to limit the scope of the present invention in any way. Any changes or modifications made by those skilled in the art based on the above disclosure shall fall within the protection scope of the claims.

Claims

1. A method for fabricating a semiconductor structure, characterized in that, Includes the following steps: A semiconductor substrate is provided, and a front-end device comprising a dummy gate and a sidewall and an interlayer dielectric layer sequentially located on the side of the dummy gate is formed on the semiconductor substrate; The front-end device is subjected to a high-temperature silicon ion implantation process, wherein the temperature of the high-temperature silicon ion implantation process is 200℃~500℃. Remove the dummy gate to form an opening.

2. The method for preparing the semiconductor structure according to claim 1, characterized in that, The sidewalls include a first sidewall and a second sidewall sequentially covering the sidewall of the dummy gate. The first sidewall is made of silicon nitride, and the second sidewall is made of a low-k material.

3. The method for preparing the semiconductor structure as described in claim 1, characterized in that, The process for removing the dummy gate includes a polysilicon removal process.

4. The method for preparing the semiconductor structure as described in claim 3, characterized in that, The polysilicon removal process includes performing dry etching and wet etching processes sequentially on the dummy gate.

5. The method for preparing a semiconductor structure as described in claim 1, characterized in that, The front-end device further includes a gate oxide layer located between the dummy gate and the semiconductor substrate.

6. The method for preparing a semiconductor structure as described in claim 5, characterized in that, The semiconductor substrate is made of silicon, the dummy gate is made of polycrystalline silicon, and the gate oxide layer is made of silicon dioxide.

7. The method for preparing a semiconductor structure as described in claim 5, characterized in that, After the step of removing the dummy gate, the method for fabricating the semiconductor structure further includes: etching the gate oxide layer to remove the gate oxide layer and increase the depth of the opening to form a gate trench.

8. The method for preparing a semiconductor structure as described in claim 7, characterized in that, After etching the gate oxide layer, the method for fabricating the semiconductor structure further includes: fabricating a metal gate within the gate recess.

9. The method for preparing a semiconductor structure as described in claim 8, characterized in that, After the step of fabricating the metal gate in the gate recess, the method for fabricating the semiconductor structure further includes: observing the morphology of the metal gate using a transmission electron microscope.

10. The method for preparing a semiconductor structure as described in claim 1, characterized in that, The energy of the high-temperature silicon ion implantation process is 1Kev to 5Kev.

11. The method for preparing a semiconductor structure as described in claim 1, characterized in that, The implantation dose of the high-temperature silicon ion implantation process is 5 × 10⁻⁶. 15 atom / cm 2 ~2×10 16 atom / cm 2 .

12. The method for preparing a semiconductor structure as described in claim 1, characterized in that, The high-temperature silicon ion implantation process includes a comprehensive ion implantation process.

13. A semiconductor structure, characterized in that, The semiconductor structure was prepared using any one of claims 1 to 12.