Method for laterally thinning a silicon-containing structure, silicon-containing structure and semiconductor device

By performing self-limiting oxidation on the silicon sidewalls in an oxygen-containing fluid environment and selectively removing the silicon oxide layer using vapor phase etching, the problems of inaccurate control of silicon structure cavity size and uneven processing inside the hollow structure in the prior art are solved, achieving nanoscale precise silicon thinning and cavity expansion.

CN123146151APending Publication Date: 2026-11-20WESTLAKE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611630592.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve precise nanoscale control over the size of silicon structure cavities and effective treatment of the silicon surface inside lateral hollow structures, leading to deviations in thinning and uneven processing.

Method used

Self-limiting oxidation of silicon-containing sidewalls is performed in an oxygen-containing fluid environment to form an atomic-layer-scale silicon oxide layer. The silicon oxide layer is then selectively removed in a vapor phase etching apparatus. A specific fluorine-containing gas reacts only with silicon oxide and not with silicon. By cyclically controlling the amount of silicon oxide layer removed, nanoscale precise thinning is achieved.

Benefits of technology

It achieves nanoscale precise and controllable thinning of silicon material in the lateral recessed area, solving the problem of uncontrollable removal amount in the prior art, expanding the cavity size and improving the uniformity of processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146151A_ABST
    Figure CN123146151A_ABST
Patent Text Reader

Abstract

The application provides a method for laterally thinning a silicon-containing structure, a silicon-containing structure and a semiconductor device. The method comprises the following steps: step 100: providing a silicon-containing structure with at least one lateral recessed region, the lateral recessed region having an exposed silicon-containing sidewall surface; step 200: placing the silicon-containing structure in an oxygen-containing fluid environment, and performing a self-limiting oxidation treatment on the silicon-containing sidewall surface to form an atomic layer of silicon oxide on the surface of the silicon-containing sidewall surface; and step 300: placing the silicon-containing structure with the atomic layer of silicon oxide in a gas phase etching device, and selectively removing the silicon oxide layer to expose a new silicon-containing sidewall surface. The application effectively processes the silicon-containing sidewall surface of the lateral recessed region and controls the removal amount of the surface layer silicon material of the silicon-containing sidewall surface to reach the nanometer scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the technical field of integrated circuit manufacturing, and in particular relates to a method for lateral thinning of a silicon-containing structure, a silicon-containing structure, and a semiconductor device. Background Technology

[0002] In the field of integrated circuit manufacturing, as device feature sizes continue to shrink and chip structures become increasingly complex, there is a need for lateral thinning of silicon structures in some advanced node devices. For example, in the manufacturing process of devices such as Gate-All-Around (GAA) transistors, it may be necessary to thin the inner walls of the silicon cutout structure to increase the size of the corresponding cavity. This type of processing not only requires the thinning process to be able to operate inside the lateral cutout structure, but also requires precise control over the amount of silicon material removed.

[0003] Existing processes for expanding the cavity size of silicon structures mainly include xenon fluoride vapor phase etching. Xenon fluoride can chemically react with silicon, producing silicon tetrafluoride and xenon, both of which are gaseous, thus making it suitable for vapor phase etching of silicon materials. However, the reaction rate between xenon fluoride and silicon is relatively fast, typically reaching 1–10 μm / min. When removing extremely thin silicon layers, even with shortened reaction times, it remains difficult to precisely control the amount of silicon material removed at the nanoscale, easily leading to deviations in the thinning amount and failing to meet the requirements for fine-tuning the cavity size of silicon structures.

[0004] In addition, grinding, polishing, chemical mechanical polishing, and conventional surface etching processes can also be used to thin silicon materials. However, these processes are mainly suitable for processing the surface layer of the substrate material. For the silicon surface inside the lateral hollow structure, due to the limitations of the processing position and structural shape, it is usually difficult to carry out effective and uniform thinning. Therefore, it is not suitable to expand the cavity size by thinning the inner sidewall. Summary of the Invention

[0005] The purpose of this application is to provide a method for lateral thinning of silicon-containing structures, silicon-containing structures, and semiconductor devices, in order to solve the problems of the prior art in achieving precise nanoscale control of the amount of silicon material removed and in effectively treating the silicon surface inside the laterally hollowed-out structure.

[0006] In a first aspect, this application provides a method for lateral thinning of a silicon-containing structure, the method comprising:

[0007] Step 100: Provide a silicon-containing structure having at least one laterally recessed region, the laterally recessed region having exposed silicon-containing sidewalls;

[0008] Step 200: Place the silicon-containing structure in an oxygen-containing fluid environment and perform a self-limiting oxidation treatment on the silicon-containing sidewall to form an atomic-layer-level silicon oxide layer on the surface of the silicon-containing sidewall.

[0009] Step 300: Place the silicon-containing structure with an atomic-layer-level silicon oxide layer in a vapor phase etching apparatus and selectively remove the silicon oxide layer to expose new silicon-containing sidewalls.

[0010] In one embodiment, the self-limiting oxidation treatment includes:

[0011] An oxygen-containing fluid is flowed into a heat treatment chamber at a preset oxidizing gas flow rate, and the silicon-containing sidewall is subjected to surface oxidation at a first preset temperature for a first preset time to obtain an initially oxidized silicon-containing sidewall.

[0012] The silicon-containing sidewall after initial oxidation is placed in a first preset vacuum environment, and the silicon-containing sidewall after initial oxidation is annealed at a second preset temperature for a second preset time to obtain an annealed silicon-containing sidewall.

[0013] The annealed silicon-containing sidewall is placed in a second preset vacuum environment for a third preset time of natural cooling, so that the temperature of the annealed silicon-containing sidewall drops to a temperature range suitable for the vapor phase etching equipment to selectively remove the silicon oxide layer.

[0014] In one embodiment, the preset oxidizing gas flow rate is 10~500 sccm, the first preset temperature is 200℃~800℃, and the first preset time is 1s~600s; the vacuum degree of the first preset vacuum environment is less than 0.01Pa, the second preset temperature is 200℃~800℃, and the second preset time is 1s~600s; the vacuum degree of the second preset vacuum environment is less than 0.01Pa, and the third preset time is 1s~600s.

[0015] Furthermore, the preset oxidizing gas flow rate is 100 sccm, the first preset temperature is 400℃, the first preset time is 120s, the second preset temperature is 400℃, the second preset time is 120s, and the third preset time is 300s.

[0016] In one embodiment, the process conditions in the vapor phase etching equipment are: reaction pressure of 60~150 Torr, reaction temperature of 35℃~60℃, flow rate of fluorine-containing gas of 50~1000 sccm, flow rate of organic alcohol catalyst gas of 50~1000 sccm, flow rate of inert carrier gas of 800~2000 sccm, and deoxidation time of 10s~1000s.

[0017] Furthermore, the process conditions in the vapor phase etching equipment are as follows: reaction pressure of 75 Torr, reaction temperature of 50°C, flow rate of fluorine-containing gas of 300 sccm, flow rate of organic alcohol catalyst gas of 350 sccm, flow rate of inert carrier gas of 1200 sccm, and deoxidation time of 300 s.

[0018] In one embodiment, the method further includes steps 100 to 300, which are performed alternately and repeated n times, where n is an integer greater than 1.

[0019] In one embodiment, after performing steps 100 to 300, the method further includes step 400: placing the new silicon-containing sidewall in a third vacuum environment and holding the new silicon-containing sidewall at a third preset temperature for a fourth preset time.

[0020] In one embodiment, the vacuum degree of the third vacuum environment is less than 0.01 Pa, the third preset temperature is 200℃~600℃, and the fourth preset time is 1~3000s.

[0021] Furthermore, the third preset temperature is 310℃, and the fourth preset time is 1200s.

[0022] In one embodiment, the silicon-containing structure is a silicon channel structure or a silicon layer structure in a gate-ring transistor, and the lateral recessed region is the gap between the silicon channel structure or the silicon layer structure.

[0023] Secondly, this application provides a silicon-containing structure having at least one laterally recessed region, wherein the laterally recessed region of the silicon-containing structure is expanded by the method described above.

[0024] Thirdly, this application provides a semiconductor device comprising a silicon-containing structure having at least one laterally recessed region.

[0025] As described above, the lateral thinning method for silicon-containing structures, the silicon-containing structures, and the semiconductor devices described in this application have the following beneficial effects:

[0026] This application achieves self-limiting oxidation of the silicon-containing sidewalls in an oxygen-containing fluid environment, restricting the oxidation thickness to the atomic layer level and preventing it from increasing indefinitely over time. Then, a specific fluorine-containing gas environment in a vapor phase etching device selectively removes the silicon oxide layer by reacting only with silicon oxide and not with silicon itself. This allows each cycle to remove only atomic-layer-level silicon material, overcoming the uncontrollable removal rate issue caused by excessively fast reaction rates in xenon fluoride vapor phase etching. Simultaneously, since both the oxygen-containing fluid and the fluorine-containing gas can directly enter the laterally recessed region to perform lateral thinning of the exposed silicon-containing sidewalls, it overcomes the limitations of planar processes such as grinding, polishing, and chemical mechanical polishing in effectively handling the interior of laterally hollowed-out structures. Furthermore, by setting the number of cycles n, it achieves nanometer-level precision, controllability, and repeatable and stable thinning of the silicon material removal from the exposed silicon-containing sidewall surface in the laterally recessed region, thereby precisely expanding the size of the laterally recessed region. Attached Figure Description

[0027] Figure 1 The diagram shown is a flowchart of a lateral thinning method for a silicon-containing structure provided in an embodiment of this application.

[0028] Figure 2 The diagram shows a process flow diagram of a lateral thinning method for a silicon-containing structure provided as an exemplary embodiment of this application;

[0029] Figure 3 The diagram shows a flowchart of a self-limiting oxidation treatment method provided in an exemplary embodiment of this application.

[0030] Figure 4 The diagram shows a microscopic flow chart at the atomic level of the lateral thinning method for a silicon-containing structure provided in an exemplary embodiment of this application.

[0031] Figure 5 The diagram shows a flowchart of a lateral thinning method for a silicon-containing structure provided as another exemplary embodiment of this application;

[0032] Figure 6 The diagram shown is a schematic representation of a thinned SOI wafer structure provided in an exemplary embodiment of this application.

[0033] Figure 7 The diagram shown is a schematic representation of a thinned silicon-germanium stacked structure provided in an exemplary embodiment of this application. Detailed Implementation

[0034] The following specific examples illustrate the implementation of this application. Those skilled in the art can easily understand other advantages and effects of this application from the content disclosed in this specification. This application can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of this application. It should be noted that, unless otherwise specified, the following embodiments and features in the embodiments can be combined with each other.

[0035] It should be noted that the illustrations provided in the following embodiments are only schematic representations of the basic concept of this application. Therefore, the drawings only show the components related to this application and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.

[0036] To address the aforementioned technical problems, this application proposes a method for lateral thinning of silicon-containing structures, a silicon-containing structure, and a semiconductor device. By performing self-limiting oxidation on the silicon-containing sidewalls in an oxygen-containing fluid environment, the oxidation thickness is limited to the atomic layer level and does not increase indefinitely over time. Then, the silicon oxide layer is selectively removed using a specific fluorine-containing gas environment in a vapor phase etching device, which reacts only with silicon oxide and not with silicon itself. Thus, each cycle removes only an atomic layer of silicon material, overcoming the drawback of uncontrollable removal due to the excessively fast reaction rate of xenon fluoride vapor phase etching. Simultaneously, since both the oxygen-containing fluid and the fluorine-containing gas can directly enter the laterally recessed region to perform lateral thinning on the exposed silicon-containing sidewalls, the limitations of planar processes such as grinding, polishing, and chemical mechanical polishing in effectively handling the interior of laterally hollowed-out structures are overcome. Furthermore, by setting the number of cycles n, nanometer-level precise, controllable, and repeatable thinning of the silicon material removal from the exposed silicon-containing sidewall surface in the laterally recessed region is achieved, thereby precisely expanding the size of the laterally recessed region.

[0037] The technical solutions in the embodiments of this application will be described in detail below with reference to the accompanying drawings.

[0038] like Figures 1 to 3 As shown, this embodiment provides a method for lateral thinning of a silicon-containing structure, the method comprising:

[0039] Step 100: Provide a silicon-containing structure having at least one laterally recessed region 1, the laterally recessed region 1 having an exposed silicon-containing sidewall 11.

[0040] In some embodiments, the silicon-containing structure is a silicon channel structure or a silicon layer structure in a gate-ring transistor, and the lateral recessed region 1 is the gap between the silicon channel structure or the silicon layer structure.

[0041] In this embodiment, as Figure 2 As shown, a silicon-containing structure with two lateral recessed regions 1 is provided.

[0042] Step 200: Place the silicon-containing structure in an oxygen-containing fluid environment and perform a self-limiting oxidation treatment on the silicon-containing sidewall 11 to form an atomic-layer-level silicon oxide layer 12 on the surface of the silicon-containing sidewall 11.

[0043] Specifically, such as Figure 2 and Figure 3 As shown, the self-limiting oxidation treatment includes:

[0044] Step 201: Flow oxygen-containing fluid into the heat treatment chamber at a preset oxidizing gas flow rate, and perform surface oxidation on the silicon-containing sidewall 11 at a first preset temperature for a first preset time to obtain the initially oxidized silicon-containing sidewall 11.

[0045] In some embodiments, the heat treatment chamber is a high-temperature rapid annealing furnace. The oxygen-containing fluid is an oxygen-containing gas selected from at least one of oxygen, ozone, water vapor, nitrous oxide, and air. The oxygen-containing gas reacts with the silicon-containing sidewall 11 at a temperature range of 200°C to 800°C to form a silicon oxide layer 12 with a thickness on the order of atomic layers.

[0046] Furthermore, the preset oxidizing gas flow rate is 10~500 sccm, the first preset temperature is 200℃~800℃, and the first preset time is 1s~600s.

[0047] In this embodiment, the preset oxidizing gas flow rate is 100 sccm, the first preset temperature is 400℃, and the first preset time is 120s.

[0048] Step 202: Place the initially oxidized silicon-containing sidewall 11 in a first preset vacuum environment, and anneal the initially oxidized silicon-containing sidewall 11 at a second preset temperature for a second preset time to obtain the annealed silicon-containing sidewall 11.

[0049] Furthermore, the vacuum degree of the first preset vacuum environment is less than 0.01 Pa, the second preset temperature is 200℃~800℃, and the second preset time is 1s~600s.

[0050] In this embodiment, the second preset temperature is 400°C. The second preset time is 120 seconds.

[0051] Step 203: Place the annealed silicon-containing sidewall 11 in a second preset vacuum environment for a third preset time of natural cooling, so that the temperature of the annealed silicon-containing sidewall 11 drops to a temperature range suitable for selective removal of the silicon oxide layer 12 by a vapor phase etching device.

[0052] Furthermore, the vacuum level of the second preset vacuum environment is less than 0.01 Pa, and the third preset time is 1 s to 600 s.

[0053] In this embodiment, the third preset time is 300s.

[0054] It should be noted that the vacuum level of the first preset vacuum environment and the vacuum level of the second preset vacuum environment can be the same or different, and those skilled in the art can adjust them according to the actual operating conditions.

[0055] It should be noted that steps 201 to 203 above can all be completed in a high-temperature rapid annealing furnace. After step 201, the oxygen-containing fluid is stopped from being introduced into the high-temperature rapid annealing furnace, and the high-temperature rapid annealing furnace is directly evacuated to a vacuum degree of less than 0.01 Pa using a vacuum pump group or other vacuum system. Alternatively, after step 201, the silicon-containing structure after initial oxidation can be transferred to another independent vacuum annealing furnace or vacuum insulation chamber through a vacuum transfer device or atmospheric transfer.

[0056] In this embodiment, the oxidation reaction of the silicon-containing structure under certain process conditions is limited to the surface atomic layer level of the silicon-containing sidewall 11 through a self-limiting oxidation process. After the formation of the silicon oxide layer 12 with a thickness of atomic layer level, the oxidation reaction will not continue to oxidize indefinitely over time, that is, it will no longer continue to extend to the deep silicon below the silicon oxide layer 12, thus avoiding the deviation in thinning amount caused by the difficulty in controlling the thinning amount.

[0057] Step 300: Place the silicon-containing structure with an atomic-layer-scale silicon oxide layer 12 in a vapor phase etching apparatus and selectively remove the silicon oxide layer 12 to expose new silicon-containing sidewalls 13.

[0058] Specifically, the process conditions in this vapor phase etching equipment are as follows: reaction pressure is 60~150 Torr, reaction temperature is 35℃~60℃, flow rate of fluorine-containing gas is 50~1000 sccm, flow rate of organic alcohol catalyst gas is 50~1000 sccm, flow rate of inert carrier gas is 800~2000 sccm, and deoxidation time is 10s~1000s.

[0059] In this embodiment, the process conditions in the vapor phase etching equipment are: reaction pressure of 75 Torr, reaction temperature of 50°C, flow rate of fluorine-containing gas of 300 sccm, flow rate of organic alcohol catalyst gas of 350 sccm, flow rate of inert carrier gas of 1200 sccm, and deoxidation time of 300 s.

[0060] In some embodiments, the fluorine-containing gas can be any one of hydrogen fluoride, nitrogen trifluoride, and ammonia.

[0061] In some embodiments, the organic alcohol catalytic gas can be a low-carbon alcohol vapor with no more than four carbon atoms, such as methanol, anhydrous ethanol, isopropanol, n-propanol, or tert-butanol.

[0062] In some embodiments, the inert carrier gas may be one or more of argon, nitrogen, helium, neon, or other rare gases.

[0063] In this embodiment, the vapor phase etching equipment is a hydrogen fluoride vapor phase etching machine, the fluorine-containing gas is hydrogen fluoride, the organic alcohol catalyst gas is anhydrous ethanol, and the inert carrier gas is nitrogen.

[0064] For example, a silicon-containing structure with an atomic-layer-level silicon oxide layer 12 is placed in the reaction chamber of a hydrogen fluoride vapor phase etching machine. After closing the reaction chamber door, the vacuum pump group is started to remove air and water vapor to a vacuum state. Then, hydrogen fluoride gas at a flow rate of 300 sccm, anhydrous ethanol vapor at a flow rate of 350 sccm, and nitrogen gas at a flow rate of 1200 sccm are introduced into the reaction chamber to stabilize the pressure in the reaction chamber at 75 Torr and the reaction temperature at 50°C. The silicon-containing structure is treated in the existing gas atmosphere for 300 s, allowing hydrogen fluoride to react with the atomic-layer-level silicon oxide layer 12 to generate gaseous byproducts (silicon fluoride gas and water vapor), which are then removed by the vacuum pump group, thereby selectively removing the silicon oxide layer 12 and exposing new silicon-containing sidewalls 13. After etching, the gas supply to the reaction chamber is stopped, and the vacuum pump group is started again to remove residual gas and reaction byproducts. After the reaction chamber returns to a background vacuum, the vacuum is broken, the reaction chamber is opened, and the silicon-containing structure is removed.

[0065] It should be noted that the vacuum level of this vapor phase etching equipment is different from the vacuum level of the reactions in steps 201 to 203 above.

[0066] Specifically, the methods in steps 100 to 300 are transformed into, for example: Figure 4 The diagram shows a microscopic flow chart at the atomic level for the lateral thinning method of silicon-containing structures. ① represents the atomic stacking state of the unthinned silicon material (chemical formula Si); ② represents the oxidation reaction of the surface Si atoms of the stacked Si material to generate silicon dioxide (chemical formula SiO2). The generated SiO2, located on the surface of the stacked Si material, protects the lower Si atoms from further oxidation; ③ represents placing the stacked Si material with the SiO2 surface layer generated in ② into a vapor phase etching machine purged with hydrogen fluoride gas (chemical formula HF); ④ represents the chemical reaction between HF and the surface SiO2 to generate silicon tetrafluoride gas (chemical formula SiF4) and water vapor (chemical formula H2O); ⑤ represents the exposure of new surface Si atoms after the surface SiO2 undergoes a chemical reaction. This completes one cycle of steps 100 to 300.

[0067] This embodiment utilizes the characteristic that a specific fluorine-containing gas can only react with silicon oxide and cannot react with silicon. By chemically reacting the fluorine-containing gas with silicon oxide, the purpose of removing the silicon oxide layer 12 is achieved, thereby thinning the silicon and expanding the lateral recessed region 1.

[0068] In some embodiments, the method further includes steps 100 to 300, which are performed alternately and repeated n times, where n is an integer greater than 1.

[0069] This embodiment consumes an atomic-layer-scale silicon oxide layer in each cycle of steps 100 to 300 to retain the unoxidized silicon covered by this silicon oxide layer. Since the silicon thinning size obtained after each cycle is controlled at the atomic-layer level, this embodiment can control the silicon thinning size of the lateral recessed region 1 by controlling the number of cycles of steps 100 to 300. This allows the silicon thinning size to be accurate to the nanometer scale, obtaining the silicon-containing structure of the lateral recessed region 1 that actually needs to be enlarged. This solves the problem of thinning deviation caused by the difficulty in controlling the silicon thinning size using existing xenon fluoride gas phase etching technology.

[0070] In another exemplary embodiment, such as Figure 5 As shown, after performing steps 100 to 300, the method further includes step 400: placing the new silicon-containing sidewall 13 in a third vacuum environment and holding the new silicon-containing sidewall 13 at a third preset temperature for a fourth preset time.

[0071] Specifically, the vacuum level of the third vacuum environment is less than 0.01 Pa, the third preset temperature is 200℃~600℃, and the fourth preset time is 1~3000s.

[0072] In this embodiment, the third preset temperature is 310°C and the fourth preset time is 1200s.

[0073] In some embodiments, the third vacuum environment is obtained by evacuating a high-temperature rapid annealing furnace.

[0074] For example, the silicon-containing structure with the new silicon-containing sidewall 13 is transferred to a high-temperature rapid annealing furnace. After the reaction chamber door of the high-temperature rapid annealing furnace is closed, the vacuum pump group is started to remove air and water vapor to a third vacuum environment with a vacuum degree of less than 0.01 Pa. The silicon-containing structure with the new silicon-containing sidewall 13 is then held at 310°C for 1200 seconds to remove surface adsorption residues of the new silicon-containing sidewall 13 or repair surface defects.

[0075] In a specific exemplary embodiment, the silicon channel structure is formed in the silicon layer of an SOI (Silicon-On-Insulator) wafer. Three sets of SOI wafers are provided, each consisting of a silicon substrate, an intermediate silicon oxide layer, and a top silicon layer. In this SOI wafer, a laterally recessed region is located between the top silicon layer and the silicon substrate and is formed by partially removing the intermediate silicon oxide layer through a window in the top silicon layer. Figure 6 As shown, the three sets of SOI wafers were placed in a high-temperature rapid annealing furnace. Oxygen was introduced into the furnace at a flow rate of 100 sccm, and the silicon-containing sidewall 11 was subjected to surface oxidation treatment at 400°C for 120 seconds, forming a silicon oxide layer 12 with a thickness on the atomic layer level on the surface of the silicon-containing sidewall 11, resulting in the initially oxidized silicon-containing sidewall 11. The thickness of the silicon oxide layer 12 can be controlled within the range of 0.1 nanometers to several nanometers. The high-temperature rapid annealing furnace was evacuated to obtain a first preset vacuum environment with a vacuum degree of less than 0.01 Pa; then, the initially oxidized silicon-containing sidewall 11 was held at 400°C for 120 seconds to obtain the annealed silicon-containing sidewall 11. This holding process helps to repair microscopic defects in the silicon oxide layer 12, improve the density and uniformity of the silicon oxide layer 12, and stabilize the interface state between the silicon oxide layer 12 and the silicon substrate. The annealed silicon-containing structure is placed in a second preset vacuum environment, the vacuum level of which is also maintained at less than 0.01 Pa. Natural cooling is then performed in this second preset vacuum environment for 300 seconds, allowing the temperature of the silicon-containing sidewall 11 to slowly decrease to a temperature range suitable for selective removal of the silicon oxide layer 12 using a hydrogen fluoride vapor phase etching machine. This natural cooling process effectively prevents structural thermal stress damage caused by rapid temperature changes and avoids surface contamination due to vacuum environment disruption. The SOI wafer is transferred to a hydrogen fluoride vapor phase etching (CVT) machine, where the reaction pressure is controlled at 75 Torr and the reaction temperature at 50°C. Hydrogen fluoride gas at a flow rate of 300 sccm, anhydrous ethanol catalyst gas at a flow rate of 350 sccm, and nitrogen carrier gas at a flow rate of 1200 sccm are introduced into the CVT machine. The silicon oxide layer 12 on the surface of the silicon-containing sidewall 11 is etched for 300 seconds to selectively remove atomic-level silicon oxide layers 12, exposing new silicon-containing sidewalls 13. This process is repeated five times, alternating layers, to gradually thin the silicon-containing sidewall 11 of the SOI wafer until the predetermined lateral recessed region 1 is reached. After completing five cycles of thinning, the silicon-containing structure with the new silicon-containing sidewall 13 is placed in a vacuum environment with a vacuum degree of less than 0.01 Pa, and the new silicon-containing sidewall 13 is subjected to a heat treatment at 310°C for 1200 s to repair surface defects that may occur during the removal of the silicon oxide layer 12 and stabilize the surface state of the silicon-containing sidewall 11.

[0076] The thickness of the top silicon layer of each SOI wafer was measured at two random locations using TEM (transmission electron microscopy). The data for the thickness of the top silicon layer of the three SOI wafers are recorded in Table 1 below:

[0077]

[0078] Table 1

[0079] Measurements were taken at two random locations on the top silicon layer of each SOI wafer. The thinning amount at the two random locations was calculated based on the difference in thickness before and after thinning. The average of the thinning amounts at the two random locations was taken as the thinning amount of the top silicon layer of the SOI wafer. Therefore, the average thinning amount of the top silicon layer of the three SOI wafers after 5 cycles was (2.03+3.73+2.99) / 3≈2.91nm. The average thinning amount per cycle was then calculated to be 2.91 / 5≈0.58nm.

[0080] The surface roughness of the top silicon layer of the thinned SOI wafer generated by the above method can reach 0.0988 nm by AFM (atomic force microscopy) testing, and the thinned silicon surface is flat and smooth.

[0081] In another specific exemplary embodiment, such as Figure 7 As shown, the silicon-germanium laminate structure is formed by selective etching of a silicon-germanium stack structure. Specifically, the silicon-germanium stack structure consists of silicon layers and silicon-germanium alloy layers in sequence, wherein the germanium content in the silicon-germanium alloy layers varies. From top to bottom, the first silicon-germanium alloy layer has a germanium content of 50%, the second silicon-germanium alloy layer has a germanium content of 40%, the third silicon-germanium alloy layer has a germanium content of 30%, and the fourth silicon-germanium alloy layer has a germanium content of 20%. By wet etching, a portion of the silicon-germanium alloy is removed from the side to form four laterally recessed regions 1 with exposed silicon-containing sidewalls 11 (the reaction rates of silicon-germanium layers with different germanium contents are different, resulting in different sizes of the laterally recessed regions). The silicon-germanium stack structure is then subjected to a thinning step under the same process conditions as the SOI wafer described above.

[0082] In another exemplary embodiment, this application also provides a silicon-containing structure having at least one laterally recessed region, the laterally recessed region of which is enlarged by the method described above.

[0083] In another exemplary embodiment, this application also provides a semiconductor device comprising a silicon-containing structure having at least one laterally recessed region.

[0084] The above embodiments are merely illustrative of the principles and effects of this application and are not intended to limit this application. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in this application should still be covered by the claims of this application.

Claims

1. A method for lateral thinning of a silicon-containing structure, characterized in that, The method includes: Step 100: Provide a silicon-containing structure having at least one laterally recessed region, the laterally recessed region having exposed silicon-containing sidewalls; Step 200: Place the silicon-containing structure in an oxygen-containing fluid environment and perform a self-limiting oxidation treatment on the silicon-containing sidewall to form an atomic-layer-level silicon oxide layer on the surface of the silicon-containing sidewall. Step 300: Place the silicon-containing structure with an atomic-layer-level silicon oxide layer in a vapor phase etching apparatus and selectively remove the silicon oxide layer to expose new silicon-containing sidewalls.

2. The method according to claim 1, characterized in that, The self-limiting oxidation treatment includes: An oxygen-containing fluid is flowed into a heat treatment chamber at a preset oxidizing gas flow rate, and the silicon-containing sidewall is subjected to surface oxidation at a first preset temperature for a first preset time to obtain an initially oxidized silicon-containing sidewall. The silicon-containing sidewall after initial oxidation is placed in a first preset vacuum environment, and the silicon-containing sidewall after initial oxidation is annealed at a second preset temperature for a second preset time to obtain an annealed silicon-containing sidewall. The annealed silicon-containing sidewall is placed in a second preset vacuum environment for a third preset time of natural cooling, so that the temperature of the annealed silicon-containing sidewall drops to a temperature range suitable for the vapor phase etching equipment to selectively remove the silicon oxide layer.

3. The method according to claim 2, characterized in that, The preset oxidizing gas flow rate is 10~500 sccm, the first preset temperature is 200℃~800℃, and the first preset time is 1s~600s; the vacuum degree of the first preset vacuum environment is less than 0.01Pa, the second preset temperature is 200℃~800℃, and the second preset time is 1s~600s; the vacuum degree of the second preset vacuum environment is less than 0.01Pa, and the third preset time is 1s~600s.

4. The method according to claim 3, characterized in that, The preset oxidizing gas flow rate is 100 sccm, the first preset temperature is 400℃, the first preset time is 120s, the second preset temperature is 400℃, the second preset time is 120s, and the third preset time is 300s.

5. The method according to claim 1, characterized in that, The process conditions in the vapor phase etching equipment are as follows: reaction pressure of 60~150 Torr, reaction temperature of 35℃~60℃, flow rate of fluorine-containing gas of 50~1000 sccm, flow rate of organic alcohol catalyst gas of 50~1000 sccm, flow rate of inert carrier gas of 800~2000 sccm, and deoxidation time of 10s~1000s.

6. The method according to claim 5, characterized in that, The reaction pressure is 75 Torr, the reaction temperature is 50°C, the flow rate of the fluorine-containing gas is 300 sccm, the flow rate of the organic alcohol catalyst gas is 350 sccm, the flow rate of the inert carrier gas is 1200 sccm, and the deoxidation time is 300 s.

7. The method according to claim 1, characterized in that, The method further includes steps 100 to 300, which are performed alternately and repeated n times, where n is an integer greater than 1.

8. The method according to claim 1, characterized in that, After completing steps 100 to 300, the method further includes step 400: placing the new silicon-containing sidewall in a third vacuum environment and holding the new silicon-containing sidewall at a third preset temperature for a fourth preset time.

9. The method according to claim 8, characterized in that, The vacuum level of the third vacuum environment is less than 0.01 Pa, the third preset temperature is 200℃~600℃, and the fourth preset time is 1~3000s.

10. The method according to claim 9, characterized in that, The third preset temperature is 310℃, and the fourth preset time is 1200s.

11. The method according to claim 1, characterized in that, The silicon-containing structure is a silicon channel structure or a silicon layer structure in a gate-ring transistor, and the lateral recessed region is the gap between the silicon channel structure or the silicon layer structure.

12. A silicon-containing structure having at least one laterally recessed region, characterized in that, The lateral recessed region of the silicon-containing structure is enlarged by the method described in any one of claims 1 to 11.

13. A semiconductor device, characterized in that, The semiconductor device includes a silicon-containing structure having at least one laterally recessed region.