A processing method for wafer regeneration double-sided grinding scratch surface abnormal state
By combining wet pretreatment, DFG physical polishing, and wet reprocessing, the problem of handling the abnormal state of double-sided frosted surface during wafer regeneration was solved, achieving efficient removal of composite film layers while avoiding damage, thus improving regeneration yield and silicon wafer utilization.
Patent Information
- Application Number
- CN202611502079.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies are unable to effectively remove dense composite films in abnormal double-sided frosted surfaces during wafer regeneration. Physical polishing is prone to introducing damage, and chemical wet film removal processes are unable to cope with complex film variations, leading to the scrapping of silicon wafers.
The process employs three steps: wet pretreatment, DFG physical grinding, and wet retreatment. By combining selective partial etching, mechanical grinding, and chemical passivation, the composite film layer is removed while avoiding surface damage.
It achieves efficient removal of dense composite film layers, avoids surface damage, improves regeneration yield, simplifies the process, reduces production costs, and ensures multiple recycling of silicon wafers.
Smart Images

Figure CN123146154A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor technology, and more specifically, relates to a method for processing abnormal conditions on the double-sided frosted surface of a wafer during regeneration. Background Technology
[0002] In the field of integrated circuit manufacturing, wafer regeneration is a key step in reducing semiconductor production costs. By surface-treating used silicon wafers, various residual films generated during the manufacturing process are removed, restoring the wafer surface to its original usable state. However, different processes within a fab can form multiple composite films on the silicon wafer surface. Influenced by the on-site process environment, the composition and microstructure of these films can vary, resulting in some wafers developing a frosted texture-like abnormal surface morphology on both sides. These abnormal surfaces contain dense composite films such as polycrystalline silicon and nitride films, with significant unevenness and high step differences, making them difficult to effectively address using traditional processing methods.
[0003] A search revealed an energy-saving water polishing machine device with publication number CN224737948U, published on September 11, 2026. This patent relates to a water polishing machine device that uses a grinding wheel to physically polish silicon wafers. A motor drives a lead screw to move the base and the silicon wafer, achieving edge polishing. However, this technical solution uses a simple physical grinding method to polish the silicon wafer. For composite films such as dense polycrystalline silicon films and nitride films present on the surface of silicon wafers with abnormal double-sided matte textures, physical grinding is difficult to precisely control the removal depth, easily introducing sharp, deep damage layers on the silicon wafer surface. Furthermore, it cannot differentiate treatment for different film composition layers, and subsequent polishing processes cannot completely repair the damaged layers, potentially leading to defective particles and scrap.
[0004] A search revealed a silicon wafer double-sided grinding wheel structure with publication number CN224751060U, published on September 15, 2026. This patent relates to a mechanical structure design of a grinding wheel, which improves installation efficiency by adjusting the installation position of the grinding wheel through components such as adjusting screws, fixing blocks, and sliding grooves. However, this technical solution only provides an improvement in the mechanical structure of the grinding wheel, belonging to the equipment-level structural design, and does not address methods for handling abnormal states of double-sided grinding texture during wafer regeneration. This patent cannot solve the problem of removing dense composite films, nor can it handle abnormal surface morphologies with large unevenness and high step differences in the film layer, thus having limited effectiveness in removing residual film on the silicon wafer surface.
[0005] A search revealed a back-polishing roller for large silicon wafers, publication number CN210866225U, published on June 26, 2020. This patent relates to a back-polishing roller structure for silicon wafers in the photovoltaic technology field. It uses a servo motor, gears, and racks to achieve the lifting and lowering of the mounting base, meeting different etching requirements. However, this technical solution is primarily aimed at the back-polishing of photovoltaic silicon wafers, and its application scenario differs from wafer regeneration processes. Furthermore, while it also uses physical grinding to treat the silicon wafer surface, it struggles to effectively remove dense composite films on silicon wafers with abnormal double-sided frosted textures, failing to address the issues of large unevenness and high step differences in the film layer.
[0006] The aforementioned existing technical solutions demonstrate significant shortcomings in current methods for handling abnormal double-sided frosted surface textures during wafer regeneration: simple physical polishing methods easily introduce damage layers and cannot completely remove dense composite films; improvements to equipment structure cannot solve the problem of handling abnormal surface morphology; and traditional chemical wet film removal processes are ill-suited to handling complex variations in composite films. Therefore, there is an urgent need to develop a comprehensive processing technology adaptable to silicon wafers with abnormal double-sided frosted surface textures, effectively removing abnormal films while avoiding the introduction of new surface damage, thus achieving high-quality recycling of regenerated wafers. Summary of the Invention
[0007] According to an embodiment of the present invention, a method for processing abnormal double-sided frosted surface conditions in wafer regeneration is proposed. For silicon wafers to be regenerated with abnormal double-sided frosted surface conditions, three processes are sequentially performed: wet pretreatment, DFG physical polishing, and wet reprocessing. Intermediate transition processes such as cleaning, drying, temperature balancing, and state determination are set between adjacent processes to remove dense polycrystalline silicon films or composite films such as nitride films on the surface, while avoiding the introduction of new surface damage. This ensures that the processed silicon wafers meet the requirements of the regeneration process and can be directly transferred to the subsequent polishing process.
[0008] Furthermore, the wet pretreatment process employs an acidic mixed solution of HF / HNO3 / CH3COOH to selectively etch the silicon wafer. This partial etching does not aim to completely remove the film layer, but rather to reduce the unevenness of the double-sided frosted surface and lower the step height between multilayer films. The etched silicon wafer surface still retains residual composite films that can be removed by subsequent DFG physical polishing. The method for determining the degree of partial etching includes: sampling or online testing of the silicon wafer to be recycled before wet pretreatment to obtain at least one of the following: the initial step difference S of the double-sided frosted surface, the total thickness Tf of the surface composite film layer, and the proportion of nitride film thickness Rn; then, calculating the target etching depth and processing time based on the measured parameters, thereby transforming the degree of partial etching from empirical judgment into reproducible quantitative control.
[0009] Further, the target etching depth is calculated according to D1=S-Ht, where Ht is the target residual step difference after the wet pretreatment is completed, and Ht is valued at 1 to 2 times the Air Cut removal amount of the subsequent DFG grinding surface and is limited to 20μm to 60μm; the equivalent etching rate of the acidic mixed chemical solution to the composite film layer is calculated according to v=v0×(1-kn×Rn), where v0 is the actually measured etching rate of the polysilicon film at the reference temperature of 23°C, kn is the deceleration coefficient caused by the density of the nitride film and 0<kn<1; then the pretreatment time t1=D1 / v, and t1 is constrained within the range of 1.5min to 5min; at the same time, it is constrained according to D1≤Tf-Tr, where Tr is the minimum thickness of the residual composite film layer required to be retained, preferably Tr≥5μm, so as to ensure that the film layer is not completely removed. When S≤Ht, it is determined that no etching is required or only a homogenization treatment of no less than 10s is performed; when the calculated t1 is greater than 5min, it is determined that the upper limit of the capability of this process is exceeded, and the control unit does not extend the single treatment time, but keeps t1=5min and leaves the remaining step difference to the DFG physical grinding process for compensation in an incremental manner.
[0010] Exemplarily, in the wet pretreatment step, an acidic mixed chemical solution is prepared by using 49% by mass fraction HF, 70% HNO3, and 98% CH3COOH according to the volume ratio HF:HNO3:CH3COOH=10L:62L:73L, the pH of the chemical solution is controlled to be 0 to 1, the processing temperature is 23°C±1°C, and the reference processing time is 3min; when v0 is 35μm / min, kn is 0.4, and Rn is 0.5, the equivalent etching rate v=35×(1-0.4×0.5)=28μm / min, if the initial step difference S of the silicon wafer to be regenerated is 120μm and Ht is 30μm, then D1=90μm, t1=90 / 28≈3.2min, that is, the 3min reference processing time recorded in this embodiment. Therefore, 3min is not a fixed value applicable to all working conditions, but a quantitative result associated with the film layer composition and the step difference. This process only performs partial etching treatment and does not completely remove the film layer.
[0011] Further, after the wet pretreatment step is completed and before the DFG physical grinding step is started, the method further includes performing deionized water rinsing and drying treatment on the silicon wafer. The rinsing is used to remove residual acidic mixed chemical solution on the surface and soluble reaction by-products such as fluorosilicate, and after rinsing, it is judged that the surface is close to neutral through pH detection of surface residual liquid, test paper detection or conductivity detection, and the pH is preferably 5 to 7. The drying is used to make the surface of the silicon wafer reach a state where it can be stably clamped without water marks or residual liquid droplets, which can be achieved by nitrogen blow-drying, spin-drying or low-temperature drying.
[0012] Furthermore, before the silicon wafer enters the DFG physical polishing process, the intermediate state after wet pretreatment must be quantitatively assessed. This assessment includes whether the residual step difference S′ falls within the target range of 20μm to 60μm, whether there are still highly reflective spots in the dense film layer, and whether the exposed area of the silicon substrate does not exceed 5% to 15%. Only when the silicon wafer meets the intermediate state of not having completely removed the film layer but with a significantly reduced step difference and an exposed area not exceeding the limit, will it enter the DFG physical polishing process. If insufficient etching is determined, it will return to the wet pretreatment tank for a short-cycle 10s to 30s of additional etching. If excessive etching is determined or the exposed area exceeds the limit, the wet pretreatment time will not be increased. Instead, the removal amount of P1 to P3 Cut or EscapeCut in the DFG physical polishing will be reduced, and the wet reprocessing time will be shortened simultaneously to avoid exceeding the total etching limit of the silicon substrate.
[0013] Furthermore, the DFG physical polishing process employs a DFG polishing device to perform double-sided physical polishing on the silicon wafer after wet pretreatment, thereby removing the remaining multilayer composite abnormal film layers through mechanical cutting. The DFG polishing device includes a device body, a polishing spindle or polishing disc for polishing the silicon wafer surface, a workpiece holding mechanism for supporting and positioning the silicon wafer, a rotary drive mechanism for driving the polishing spindle or workpiece to rotate, a feed servo mechanism for controlling the polishing feed amount, a displacement encoder for measuring the feed displacement, a pressure sensor for monitoring the polishing pressure, a thickness detection unit for detecting the silicon wafer thickness or the amount of material removed, and a control unit. The control unit is pre-loaded with a DFG polishing program and parameter calibration table. The DFG polishing device can be a semiconductor wafer double-sided fine polishing device, a DFG polishing device, or a DSG polishing device commonly used in the art. Those skilled in the art can select a device with the above-mentioned structure and control functions according to the actual production line; specific models and manufacturers are not considered limitations on the implementation of this invention. In this application, the DFG device and the DSG polishing device are the same type of double-sided polishing device, and are uniformly referred to as DFG polishing device.
[0014] Further, the Z1 grinding surface and the Z2 grinding surface respectively correspond to two grinding surfaces of the silicon wafer, or correspond to two grinding stations, two grinding spindles, two grinding disks or the upper and lower two grinding surfaces for processing different surfaces of the silicon wafer in the same double-sided grinding apparatus; their grinding parameters are independently controlled by the control unit. The control unit calculates the total mechanical removal amount according to Dmech=Tpre-Tg, where Tg is the sum of the target finished product thickness and the polishing process allowance, and determines the P1 to P3 Cut removal amounts of each grinding surface according to F=Dsurface-E-m after double-sided distribution, where E is the preset Escape Cut removal amount, and m is the allowance of 2μm to 5μm. The control unit controls the rotation speed of the grinding spindle through a frequency converter or a servo drive unit, and performs closed-loop control on the grinding feed amount and the final removal amount through at least one of a feed servo axis, a displacement encoder, a pressure sensor and a thickness detection unit.
[0015] Further, the feed rate g and the Spark Out revolution number Nso in the DFG physical grinding process are determined according to a piecewise mapping relationship based on the actually measured residual step difference S' after wet pretreatment: when S'≤30μm, g=0.20μm / s; when 30μm<S'≤50μm, g=0.25μm / s; when 50μm<S'≤80μm, g=0.30μm / s; when S'>80μm, g≤0.35μm / s and Nso is 5rev to 6rev. That is, the larger the residual step difference, the lower the feed rate and the larger the spark-out revolution number, so as to avoid local over-cutting caused by large step impact.
[0016] Exemplarily, the DFG physical grinding process is divided into double-sided grinding performed by the Z1 grinding surface and the Z2 grinding surface respectively, wherein the spindle rotation speed of the Z1 grinding surface is 1000rpm, the total grinding processing time of Z1 is 145s, the Air Cut removal amount is set to 30μm, the P1 to P3 Cut removal amount is 591μm, the feed rate is 0.30μm / s, the rotation speed is 20rpm, the Spark Out parameter is 3rev, the Escape Cut removal amount is 3μm, the feed rate is 0.50μm / s, and the rotation speed is 20rpm; the spindle rotation speed of the Z2 grinding surface is 1785rpm, the total grinding processing time of Z2 is 157s, the Air Cut removal amount is set to 20μm, the P1 to P3 Cut removal amount is 581μm, the feed rate is 0.20μm / s, the rotation speed is 185rpm, the Spark Out parameter is 5rev, the Escape Cut removal amount is 2μm, the feed rate is 0.30μm / s, and the rotation speed is 185rpm. Through the cooperative coordination of multi-stage cutting feed, spark-out and retraction cutting parameters, the mechanical removal of the residual composite film layer on both sides of the silicon wafer is completed; after the large step is eliminated by the previous wet pretreatment, the DFG grinding can remove the residual film layer without an excessively large grinding removal amount.
[0017] Further, the switching logic between the Z1 grinding surface and the Z2 grinding surface includes: after the silicon wafer enters the DFG grinding apparatus, the workpiece holding mechanism first adsorbs or positions the first surface and places it at the Z1 grinding station; the control unit sequentially executes Air Cut, P1 to P3 Cut, Spark Out and Escape Cut processing according to the Z1 grinding program. When the first surface reaches a preset intermediate state, the control unit controls the feed servo axis to retract, so that the grinding spindle or the grinding plate is separated from the silicon wafer or the speed is reduced, and then the silicon wafer is transferred to the Z2 grinding station through a turnover mechanism, a manipulator, a turntable position changing mechanism or a double-sided grinding station surface changing mode, so that the second surface is in contact with the Z2 grinding surface and processed according to the Z2 grinding program. If the apparatus is of a double-sided grinding structure in which the upper plate and the lower plate are in contact with the silicon wafer at the same time, the Z1 grinding surface and the Z2 grinding surface respectively refer to the grinding surfaces corresponding to the upper plate and the lower plate, and independent control is realized by respectively setting the upper plate rotation speed, the lower plate rotation speed, the feed pressure, the segmented cutting amount and the spark-out parameters.
[0018] Further, the grinding end point of the DFG physical grinding process is judged according to a quantitative standard: the criterion for reaching the end point is that the thickness Tpost of the silicon wafer after grinding falls within the ±δ tolerance range of the target post-grinding thickness Tg, and δ is preferably ±3μm; when Tpost>Tg+δ, it is judged that the removal amount is insufficient, supplementary grinding is performed, the single supplementary grinding removal amount ΔF=Tpost-Tg, ΔF≤10μm, and re-detection is performed after supplementary grinding; when Tpost<Tg-δ, it is judged that excessive grinding occurs, rework evaluation is performed on the ground silicon wafer, and the P1 to P3 Cut removal amount and the Escape Cut removal amount of subsequent silicon wafers in the same batch are synchronously reduced. During the grinding process, at least one of that the cumulative removal amount in each cutting stage reaches a set value, the feed servo axis is displaced in place, the grinding pressure is stable, and the spindle current or power enters a stable interval is used as the stage switching criterion; at the same time, the criterion for film layer removal is that the residual step difference on the surface after grinding is not more than 10μm, and there are no residual film layer bright spots and high-reflection areas on the surface.
[0019] Furthermore, after the DFG physical polishing process is completed and before the wet reprocessing process begins, the silicon wafers are first cleaned of polishing debris to remove residual grinding silicon powder, abrasive particles, and polishing coolant. This prevents the polishing particles from being carried into the alkaline solution tank, causing tank contamination, secondary scratches, or batch cross-contamination. The polishing debris cleaning can be performed using one or more combinations of deionized water rinsing, low-power ultrasonic-assisted rinsing, or overflow rinsing. After cleaning, the silicon wafers undergo temperature balancing treatment to bring the surface temperature of the silicon wafers into the allowable feed temperature range of the wet reprocessing alkaline solution. This avoids localized temperature shocks, instantaneous uneven alkaline solution concentration, or corrosion rate fluctuations caused by silicon wafers with excessively high temperatures being directly introduced into the 80℃±5℃ alkaline solution tank. Subsequently, the silicon wafers are dried or their surface moisture content is controlled before being transferred into the alkaline tank. If wet transfer into the alkaline tank is used, the amount of cleaning solution introduced is controlled, and the NaOH concentration, pH, and corrosion rate are maintained stably through alkaline tank overflow, automatic replenishment, or online concentration feedback.
[0020] Furthermore, the wet reprocessing step uses a 48% NaOH alkaline solution, with a pH controlled between 12 and 14, a circulation flow rate of 10 to 14 L / min, and a processing temperature of 80℃ ± 5℃. The processing time of this step is not a fixed empirical value, but is calculated by the control unit using the following formula: t2 = η × Dd / vNa, where Dd is the estimated depth of the grinding damage layer formed on the silicon wafer surface by the DFG physical polishing process, vNa is the equivalent corrosion rate of the NaOH alkaline solution on the silicon and the damage layer under the current bath conditions, and η is the complete dissolution margin coefficient, preferably 1.1 to 1.3, more preferably 1.2. The calculated t2 is constrained by a lower limit of 30s and an upper limit of 2min as the actual execution time. The lower limit of 30s is not the required corrosion time, but the minimum process dwell time to ensure the silicon wafer enters and exits the liquid, the surface solution is replaced, and the temperature tends to stabilize. The upper limit of 2min is used to avoid excessive anisotropic corrosion of the silicon substrate by the alkaline solution, which would lead to an increase in surface roughness and excessive thickness loss.
[0021] Furthermore, the estimated depth Dd of the grinding damage layer is calculated using the grinding parameters determined before this process according to the calibration mapping relationship, calculated as Dd = a0 + a1 × g + a2 × F + a3 × (1 / Nso), where g is the feed rate of the P1 to P3 Cut stages, F is the amount removed during the P1 to P3 Cut stages, Nso is the Spark Out revolutions, a0 is a basic term related to the machine type, abrasive particle size, and cooling conditions, and a0 to a3 are calibration coefficients obtained from the measured damage depth of test pieces under the same conditions through multiple linear regression. For example, a0 = 0.2 μm, a1 = 1.5, a2 = 1.5 × 10⁻⁶. -3 When calibrated with μm / μm and a3=1.5μm·rev, the corresponding Dd≈2.04μm for Z1 polishing surface g=0.30μm / s, F=591μm, Nso=3rev, substituting into v Na≈2.5μm / min, η=1.2 gives t2≈0.98min, which is the 1min reference processing time described in this embodiment; for the Z2 polishing surface with g=0.20μm / s, F=581μm, Nso=5rev, the corresponding Dd≈1.67μm, corresponding to t2≈0.80min, i.e., 48s. It can be seen that 1min is a reference value for the deep damage surface of the Z1 polishing surface, rather than a fixed value uniformly applicable to any damage state.
[0022] Further, the equivalent etching rate v Na is calculated by correction according to temperature and pH, and according to calculation, where v N is the reference etching rate measured under the conditions of 80℃, mass fraction of 48%, and pH 13, Q 10 is the temperature coefficient, preferably 2.0 to 2.3, and T is the on-line measured temperature of the bath solution. When the actually measured bath temperature is 75℃, Q 10 is 2.1, v Na ≈1.7μm / min, the processing time corresponding to Dd≈2.04μm increases from 1min to about 1.4min; when the bath temperature is 85℃, v Na ≈3.6μm / min, the processing time is shortened to about 0.68min. Accordingly, the control unit automatically corrects t2 after the bath temperature drifts or the solution is replaced, so that the actual etching depth remains stable, instead of using the fixed 1min all the time.
[0023] Further, whether the sharp damage layer has been completely dissolved is judged by the following quantitative criteria: First, the surface roughness criterion: after the wet reprocessing, the arithmetic mean roughness Ra of the silicon wafer surface is ≤0.3μm and there are no obvious directional grinding streaks, then it is determined that the grinding peaks and valleys have been flattened, and the damage layer enters a state that can be repaired by subsequent polishing; when 0.3μm<Ra≤0.6μm, it is determined to be close to the standard, and a short-period supplementary etching of 5s to 20s is performed; when Ra>0.6μm, it is determined that the damage layer is not dissolved, and the process returns to check the DFG grinding parameters instead of simply extending the alkali etching time. Second, the thickness removal amount criterion: compare the sampled thickness difference D2 before and after the alkali solution treatment with the target etching amount η×Dd, and it is determined to be up to standard when D2 falls within the range of ±20% of η×Dd. Third, the polishing feedback criterion: the count of particle defects on the sampled silicon wafers of the same batch after polishing does not exceed the set threshold, and the surface defect rate falls within the preset range. Fourth, the microscopic recheck criterion: perform grinding angle cross-section or surface microscopic observation on the test piece under the same conditions to confirm that there are no sharp peaks and valleys extending to the tip of the subsurface microcracks. For mass production on-line control, the combination of the surface roughness criterion and the thickness removal amount criterion is preferentially adopted, the polishing feedback criterion is used for batch release, and the microscopic recheck criterion is used for calibration and abnormal analysis when a new process window is introduced.
[0024] Furthermore, when the estimated damage depths of the Z1 and Z2 polished surfaces of the same silicon wafer are inconsistent, the control unit determines the baseline t2 based on the larger Dd value of both sides. For the side with shallower damage, the control unit shortens the time by 5 to 15 seconds, reduces the circulation flow rate, or shortens the dwell time of that side to avoid excessive corrosion of the shallowly damaged surface. For silicon wafers with shallow damage after polishing (i.e., Dd ≤ 0.6 μm), the lower limit of t2 is set to 30 to 50 seconds. For silicon wafers with obvious sharp scratches or micro-cracks on the surface after polishing (i.e., Dd ≥ 2.5 μm), t2 is extended to 1.2 to 2 minutes. This information is fed back to the DFG physical polishing process, and the Spark Out speed is increased by 1 rev or the Escape Cut removal amount is increased to 3 to 4 μm for subsequent silicon wafers in the same batch, so that the damage is controlled during the polishing stage.
[0025] Furthermore, the control unit verifies the total chemical corrosion amount while determining t1 and t2: Let D2 = t2 × v Na The required measured chemical corrosion amount D1 during wet pretreatment is... meas The sum of D1 and D2 satisfies D1 meas +D2≤12μm; When the verification is not met, prioritize film removal, then total etching amount, first compress t2, then compress P1 to P3 Cut removal amount F. If it still does not meet the requirements, mark the batch of silicon wafers for full inspection. If the standard is still not met after a single t2 operation, perform short-cycle re-etching for 5s to 20s, and the sum of the cumulative re-etching time and the initial etching time shall not exceed 2min. After each re-etching, re-inspect Ra and cumulative D2.
[0026] Furthermore, a closed-loop parameter feedback and self-learning correction is formed among the three processes: the detection parameters after wet pretreatment serve as the basis for adjusting the parameters of the DFG physical grinding process; the detection parameters after DFG physical grinding serve as the basis for calculating the time of the wet reprocessing process; and the detection parameters after wet reprocessing serve as the final determination basis for whether to return to the previous process for supplementary processing or directly enter the polishing process. The control unit transmits back the particle defect rate, roughness, and yield data after polishing each batch, and performs parameter feedback on v0, kn, a0 to a3, v N η is updated using an exponentially weighted moving average, and the update formula is as follows: Where λ is the learning step size, preferably between 0.1 and 0.3; when the defect rate of polishing particles in N consecutive batches exceeds the set threshold, it is determined that the current mapping model deviates from reality, and η is automatically increased or the SparkOut revolutions are increased and manual confirmation is triggered. Therefore, the control unit's adjustment of parameters for each process is not a qualitative description, but a quantitative value obtained through the above mapping relationship and calculation formula based on the measured step difference, film thickness, film composition ratio, post-grinding thickness and surface condition. Those skilled in the art can then write control programs to implement this invention based on this.
[0027] Furthermore, the processed silicon wafers can be directly transferred to the downstream polishing process for subsequent regeneration. The entire combined process controls the total etching amount of the silicon substrate to less than 12μm, greatly reducing the amount of material removed and enabling multiple cycles of silicon wafer regeneration. The byproducts generated by the chemical reactions in each step of this process are all water-soluble substances, which will not cause chemical solution or tank deposition contamination, and will not cause cross-contamination to subsequent batches of silicon wafers.
[0028] As can be seen from the above embodiments, the present invention selectively etches the double-sided frosted composite film layer through wet pretreatment to reduce the surface unevenness steps, then removes the residual film layer with a small amount through DFG physical polishing, and finally chemically passivates and dissolves the sharp damage layer introduced by polishing through wet reprocessing. The processing amount and processing time of each process are determined by measured state parameters through quantitative formulas and segmented mapping relationships. This can effectively remove the dense composite film layer while avoiding the introduction of new surface damage, thus completing the regeneration treatment of the double-sided frosted abnormal silicon wafer.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] First, by combining wet pretreatment, DFG physical polishing, and wet reprocessing, the uneven surface of the sanding texture is smoothed first, the residual film layer is physically removed, and finally the sharp polishing damage is chemically eliminated. This can solve the problem of removing the film layer of abnormal silicon wafers with double-sided sanding texture. Compared with a single wet process or a single polishing process, it can significantly improve the regeneration yield.
[0031] Secondly, by establishing the definition of detection variables, segmented mapping tables, calculation formulas, and closed-loop feedback rules, the target corrosion depth, processing time, segmented removal amount, feed rate, and alkaline etching time of each process are all quantitatively determined by measured state parameters, eliminating the uncertainty of the control logic. Based on this, those skilled in the art can reproduce the entire control process and avoid continuous blind machining relying solely on fixed time or fixed cutting amount.
[0032] Third, by reducing the large step size through wet pretreatment, the residual film layer can be removed without excessive removal volume by physical grinding of DFG. This avoids the multi-component film layer and multi-stage drug solution soaking process, simplifies the process, avoids the generation of poorly soluble by-products, reduces production costs, and reduces the risk of equipment contamination.
[0033] Fourth, by strictly controlling the total etching amount of the silicon substrate to less than 12μm in the entire combined process, the thickness loss of the silicon wafer can be controlled, enabling the silicon wafer to be recycled and reused multiple times.
[0034] Fifth, by ensuring that the byproducts generated in each step of the chemical reaction are all water-soluble substances, it is possible to avoid contaminating the chemical solution tank, eliminate the risk of cross-contamination, and make it suitable for large-scale wafer regeneration mass production operations.
[0035] Sixth, by setting intermediate transition processes such as cleaning, drying, temperature balancing, and state determination between adjacent processes, it is possible to avoid contamination caused by residual chemicals or grinding particles, and to avoid insufficient or excessive corrosion due to fixed time under different film thicknesses and grinding damage depths, so that the processed silicon wafers can stably meet the requirements of the subsequent polishing process.
[0036] Seventh, by establishing the consistency of comparative test conditions, statistical testing of sample size, and yield judgment criteria, the basis for obtaining the technical effect can be clearly explained, which is convenient for repeated verification by those skilled in the art. Attached Figure Description
[0037] Figure 1 This is a flowchart illustrating the method for handling abnormal conditions on the double-sided frosted surface of a wafer regeneration wafer, as provided in an embodiment of the present invention.
[0038] Figure 2 A schematic diagram of parameter configuration for the three processes of wet pretreatment, DFG physical grinding, and wet retreatment in the processing method provided in the embodiments of the present invention;
[0039] Figure 3 This is a schematic diagram of the execution flow of the control unit automatically adjusting process parameters based on measured state parameters, provided in an embodiment of the present invention. Detailed Implementation
[0040] The present invention will be further described below with reference to the accompanying drawings and through embodiments. (Refer to...) Figures 1 to 3 As shown in the embodiment of the present invention, the method for handling abnormal double-sided frosted surface conditions of wafer regeneration involves sequentially performing three processes on silicon wafers to be regenerated that have abnormal double-sided frosted surface conditions: wet pretreatment, DFG physical polishing, and wet reprocessing. Intermediate transition processes such as cleaning, drying, temperature balancing, and state determination are set between adjacent processes. At the same time, the control unit automatically adjusts the process parameters of each process according to the measured state parameters and a quantitative formula to remove the dense polycrystalline silicon film or nitride film and other composite film layers on the surface, while avoiding the introduction of new surface damage. This ensures that the processed silicon wafer meets the requirements of the regeneration process and can be directly transferred to the subsequent polishing process.
[0041] In actual wafer regeneration processes, silicon wafers returned from fab production lines often exhibit abnormal double-sided frosted surface morphology, with dense polycrystalline silicon films or nitride films adhering to their surfaces. If these wafers are processed using traditional single physical polishing methods, it is difficult to precisely control the removal depth. During polishing, sharp, deep damage layers are formed on the wafer surface. Furthermore, due to the large unevenness and high step differences in the film layer, physical polishing requires a significant removal amount to remove the film layer, resulting in severe damage to the silicon substrate. Subsequent polishing processes cannot completely repair these deep, sharp damages, and the treated wafers are prone to particle defects and scrapping. Simultaneously, traditional chemical wet film removal processes are cumbersome for handling multi-component composite films, easily generating insoluble byproducts, and are ineffective in addressing the high step differences on the frosted surface. This invention addresses these technical problems by providing a composite process solution to solve the challenge of removing the film layer from silicon wafers with abnormal double-sided frosted surface morphology.
[0042] Reference Figure 1 As shown, the overall process of the processing method in this embodiment of the invention includes three main steps. The first step is a wet pretreatment step, which selectively etches the dense polycrystalline silicon film and nitride film attached to the double-sided frosted surface of the silicon wafer. This reduces the unevenness of the frosted surface, lowers the step height between the multilayer films, and smooths the microscopic surface morphology, reducing the processing difficulty for subsequent physical polishing. The second step is a DFG physical polishing step, which removes the remaining multilayer composite abnormal film layers through mechanical polishing. Since the previous wet pretreatment has eliminated the large steps, DFG polishing does not require a large amount of polishing to remove the residual film layers. The third step is a wet reprocessing step, which passivates and dissolves the sharp damage layer introduced by DFG physical polishing through chemical etching, eliminating the surface micro-defects caused by polishing, and obtaining a silicon wafer that meets the requirements of the regeneration process. Each step is described in detail below.
[0043] I. Calculation of Processing Capacity and Determination of Endpoint in Wet Pretreatment Process
[0044] The specific implementation method of the wet pretreatment process is as follows: The silicon wafer to be treated is placed in a mixed acid bath. An acidic mixed solution is prepared by mixing 49% hydrofluoric acid, 70% nitric acid, and 98% glacial acetic acid in a volume ratio of 10 liters: 62 liters: 73 liters. After the solution is prepared, the pH is controlled between 0 and 1, the processing temperature is maintained at 23℃±1℃, and the baseline treatment time is 3 minutes. Under these conditions, the acidic mixed solution selectively etches the dense polycrystalline silicon film, nitride film, and their composite interface adhering to the surface of the silicon wafer.
[0045] It should be noted that some etching processes in this procedure are not blind etching based on a single fixed time. Instead, the degree of partial etching is determined through a combination of pre-etching inspection, formula calculation, in-etching control, and post-etching inspection. In mass production, silicon wafers from the same batch are sampled for inspection, or an online inspection unit is configured at the equipment end to obtain the initial surface morphology parameters and film parameters of the silicon wafers to be regenerated. The initial surface morphology parameters include at least one of the peak-valley height difference of the double-sided frosted texture, the maximum step difference S, and the degree of local unevenness; the film parameters include at least one of the polycrystalline silicon film thickness, nitride film thickness, total composite film thickness Tf, and the nitride film thickness ratio Rn. The above inspections can be carried out using at least one of the following: a step meter, a white light interferometer, an ellipsometer, a film thickness gauge, infrared spectroscopy, Raman spectroscopy, or an optical inspection method based on surface reflectivity differences. The sampling quantity is 3 to 5 wafers from the same batch, and the weighted result of the maximum value and the average value is taken as the batch input value S.
[0046] The target etching depth is calculated as D1 = S - Ht, where Ht is the target residual step difference after wet pretreatment. The value of Ht is based on the cutting capability of the subsequent DFG physical polishing process: in this embodiment, the air cut removal amount of the Z1 polishing surface is 30 μm and the air cut removal amount of the Z2 polishing surface is 20 μm. Therefore, Ht is taken as 1 to 2 times the air cut removal amount and limited to 20 μm to 60 μm, preferably 20 μm to 40 μm. By ensuring that the residual step difference after wet pretreatment falls within the range that the DFG physical polishing process can stably handle, the forced increase in removal amount due to large surface step differences in subsequent polishing can be avoided, thereby reducing the risk of silicon substrate damage.
[0047] The equivalent corrosion rate is calculated as v = v0 × (1 - kn × Rn). Where v0 is the measured corrosion rate of the polycrystalline silicon film at a reference temperature of 23°C, which in this embodiment is calibrated to be approximately 35 μm / min; kn is the deceleration coefficient caused by the density of the nitride film, which in this embodiment is calibrated to be between 0.35 and 0.55, with an example value of 0.4. The physical meaning is that the nitride film has a greater resistance to acid penetration than the polycrystalline silicon film, and the larger Rn is, the lower the overall corrosion rate of the composite film layer.
[0048] The pretreatment time is calculated as t1=D1 / v and constrained to be within the range of 1.5min to 5min. At the same time, it is constrained by D1≤Tf-Tr, where Tr is the minimum thickness of the residual composite film layer to be retained, and Tr≥5μm, so as to mathematically ensure that there is still a residual film layer on the surface after corrosion that can be removed by DFG grinding, that is, to achieve only partial corrosion and not complete removal of the film layer.
[0049] The following calculation example illustrates this: When v0 = 35 μm / min, kn = 0.4, and Rn = 0.5, v = 35 × (1 - 0.4 × 0.5) = 28 μm / min; if the initial step difference S of the silicon wafer to be regenerated is 120 μm and Ht is 30 μm, then D1 = 120 - 30 = 90 μm, t1 = 90 / 28 ≈ 3.2 min, which is the 3 min baseline processing time recorded in this embodiment; if S = 50 μm and Ht is 25 μm, then D1 = 25 μm, t1 = 25 / 28 ≈ 0.9 min, which is lower than the lower limit. At this time, the control unit executes according to Tr and the surface homogenization requirement, setting t1 = 1.5 min as the lower limit, and the DFG polishes with Air. Cut handles the step difference requirement; if S=200μm and Ht=30μm, then D1=170μm, t1=170 / 28≈6.1min, which exceeds the 5min upper limit. The control unit keeps t1=5min and compensates for the remaining step difference D1′=200-(28×5)=60μm by increasing the DFG grinding surface Air Cut setting or increasing the Spark Out speed, instead of infinitely extending the acid etching time and causing excessive wear on the silicon substrate.
[0050] Differentiated treatments are applied to different film types as follows: For silicon wafers with a high proportion of polycrystalline silicon film and relatively loose film structure (i.e., low Rn), the etching rate is fast, and the processing time is correspondingly shortened, for example, 1.5 min to 2.5 min; for silicon wafers with a high proportion of nitride film, high film density (i.e., high Rn), or an initial step difference exceeding 120 μm, the processing time is extended to 3.5 min to 5 min, or a baseline processing time is used followed by a 10 s to 30 s short-cycle etch and re-inspection of the step difference. The etch is performed using a short-time, multiple-time method to avoid over-etching in a single pass.
[0051] The endpoint of the partial etching process is determined by a combination of the following quantitative criteria: First, time criterion, i.e., etching stops when t1 calculated by the above formula is reached; Second, step difference criterion, i.e., the residual step difference S′ on the silicon wafer surface after treatment falls within the target range of 20μm to 60μm; Third, residual film criterion, i.e., the surface still retains a residual composite film that can be removed by subsequent DFG grinding, and the complete removal of the film is not considered a qualified condition; Fourth, exposed substrate area criterion, i.e., the proportion of the area of the silicon substrate exposed by etching does not exceed a preset threshold, preferably 5% to 15%, more preferably not exceeding 10%; Fifth, surface morphology criterion, i.e., the surface changes from a dense, mottled, locally highly reflective, or multi-layered film before treatment to a relatively uniform gray-white matte pre-etched state.
[0052] In this embodiment, the wet pretreatment qualification standard is: the residual step difference S′ falls within 20μm to 60μm, and a residual composite film layer still exists on the surface, with the exposed area of the silicon substrate not exceeding 10%. If the sampling inspection finds S′>60μm, it is judged as insufficient corrosion, and a short-cycle 10s to 30s etch is performed, with a maximum of 2 etches; if the standard is still not met after 2 etches, no further etching is performed, and the process is switched to the DFG polishing setting corresponding to S′>80μm. If the sampling inspection finds that the exposed area of the silicon substrate exceeds 15%, it is judged as over-etching, and the control unit will not increase any chemical etching amount, but will reduce the subsequent Escape Cut removal amount to no more than 2μm, shorten the alkaline treatment time to 30s to 50s, and mark the batch for full inspection. Through the above method, the processing volume and endpoint of the wet pretreatment process are determined by measured parameters through formulas, which has clear judgment basis and repeatability.
[0053] II. Control of the transition from wet pretreatment to DFG physical milling
[0054] After the wet pretreatment process, residual acidic mixed solutions and reaction products adhere to the surface of the silicon wafer. If it enters the DFG physical polishing process directly without cleaning, the residual acid may react with the coolant in the polishing equipment, metal parts, or substances on the surface of the polishing pad, producing insoluble substances, corrosion particles, or surface spots. If residual moisture or droplets are not removed, uneven adsorption may cause warping, slippage, or inconsistent polishing depth during silicon wafer clamping. Therefore, rinsing and drying are required after wet pretreatment.
[0055] Specifically, after wet pretreatment, the silicon wafers undergo two or more stages of countercurrent rinsing with deionized water, with an example rinsing time of 10 to 30 seconds. After rinsing, the pH of the residual acid on the surface is determined by online pH monitoring, surface wiping solution pH monitoring, conductivity monitoring, or random sampling with test strips to determine whether the residual acid solution is close to neutral. Preferably, the pH of the residual solution is 5 to 7, and the conductivity is not higher than a set threshold. After rinsing, the silicon wafers are dried using nitrogen blowing, spin drying, or low-temperature hot air drying to remove the surface water film and prevent watermarks. High temperatures are preferably avoided during the drying process to prevent further alteration of the residual film layer on the silicon wafer surface.
[0056] After drying, the intermediate state of the wet pretreatment is assessed before entering the DFG polishing equipment. Assessment methods include visual inspection, optical reflection inspection, random step analysis, random film thickness analysis, or sampled polishing particle feedback. A qualified intermediate state is characterized by: a relatively uniform grayish-white matte pre-etched surface; a residual step difference S′ of 20μm to 60μm; the presence of residual composite film; and an exposed silicon substrate area not exceeding 10%. The control unit uses S′ as an input variable for the DFG polishing process and automatically selects the feed rate and Spark Out speed settings according to the mapping relationship.
[0057] When insufficient corrosion is determined (S′>60μm), or when there are still obvious highly reflective film spots or un-etched areas on the surface, the sample is returned to the wet pretreatment tank for 10 to 30 seconds of additional etching. After additional etching, the sample is rinsed, dried, and its condition is assessed again. When excessive corrosion is determined (the exposed area of the silicon substrate exceeds 15%), or when there are excessively etched pits on the surface, or when the average weight loss of the same batch of test pieces exceeds the budget value, additional etching is discontinued. Instead, feedback is provided to adjust the parameters of subsequent processes: on the one hand, the P1 to P3 cut removal amount and / or Escape cut removal amount of DFG grinding is reduced to reduce excessive cutting caused by the already low surface steps; on the other hand, the alkaline treatment time is shortened from 1 minute to 30 to 50 seconds to ensure that the total chemical corrosion amount of the silicon substrate caused by the wet pretreatment and wet retreatment is less than 12μm.
[0058] III. DFG Physical Grinding Equipment, Parameter Calculation, Switching Logic, and Endpoint Determination
[0059] The specific implementation method of the DFG physical polishing process is as follows: After wet pretreatment, the silicon wafer is fed into a DFG polishing machine for physical polishing, and double-sided polishing operations are performed on both the Z1 and Z2 polishing surfaces. The DFG polishing machine can be a commonly used semiconductor wafer double-sided fine polishing machine, DFG polishing machine, or DSG polishing machine, as long as it can achieve separate polishing control on both polishing surfaces of the silicon wafer. In this embodiment, the DFG polishing machine and DSG polishing machine refer to the same type of double-sided polishing machine used for wafer regeneration, collectively referred to as DFG polishing machine. Specific equipment models and manufacturers can be replaced according to the actual production line equipment. The implementation of this invention is not limited to a specific commercial equipment; as long as the equipment has a polishing spindle or polishing disc, a workpiece holding mechanism, a rotary drive mechanism, a feed servo mechanism, a thickness detection unit, and a control unit, the method described in this embodiment can be implemented.
[0060] The DFG grinding equipment comprises: a main body, a first grinding spindle or a first grinding disc, a second grinding spindle or a second grinding disc, a vacuum adsorption turntable or a workpiece holder, a servo motor and frequency converter for driving the grinding spindle or workpiece rotation, a feed servo axis for controlling the grinding feed amount, a displacement encoder for measuring the feed displacement, a pressure sensor for monitoring the grinding pressure, a thickness detection unit for online measurement or random inspection of silicon wafer thickness, a coolant supply unit, and a PLC control unit or CNC controller. The PLC control unit communicates with the aforementioned actuators and detection units, and is used to call preset grinding programs and parameter calibration tables, control spindle speed, feed rate, segmented removal amount, Air Cut, P1 to P3 Cut, Spark Out, Escape Cut, Z1 and Z2 grinding surface switching, and grinding endpoint determination. The thickness detection unit can employ a laser displacement sensor, a capacitive thickness sensor, a contact probe, a white light interferometric thickness measurement unit, or a built-in thickness feedback system.
[0061] The Z1 grinding surface has a spindle speed of 1000 rpm and a total processing time of 145 s. Specific parameters include: Air Cut removal of 30 μm, P1 to P3 Cut removal of 591 μm, feed rate of 0.30 μm / s, spindle speed of 20 rpm, Spark Out parameter of 3 rev, Escape Cut removal of 3 μm, feed rate of 0.50 μm / s, and spindle speed of 20 rpm. The Z2 grinding surface has a spindle speed of 1785 rpm and a total processing time of 157 s. Specific parameters include: Air Cut removal of 20 μm, P1 to P3 Cut removal of 581 μm, feed rate of 0.20 μm / s, spindle speed of 185 rpm, Spark Out parameter of 5 rev, Escape Cut removal of 2 μm, feed rate of 0.30 μm / s, and spindle speed of 185 rpm. Among the parameters mentioned above, the P1 to P3 Cut stages are the main cutting stages for removing the composite film layer. The Spark Out stage is used for micro-grinding after the basic removal is completed to eliminate residual surface stress, improve surface roughness, and stabilize dimensions. The Escape Cut stage is used for final retraction micro-removal to reduce grinding damage and control the final removal amount.
[0062] The amount of material removed during grinding is calculated by the control unit using a formula, rather than being manually specified. Specifically, the control unit first reads the silicon wafer thickness Tpre before grinding and the target thickness Tspec of the finished product, and then calculates the allowance m for the subsequent polishing process. polishCalculate the target post-grinding thickness Tg = Tspec + m_polish; then calculate the total mechanical removal amount according to Dmech = Tpre - Tg; distribute Dmech equally on both sides to obtain D_side, and determine the P1 to P3 Cut removal amount of each grinding surface according to F = D_side - E - m, where E is the preset Escape Cut removal amount, m is the allowance and is set to 2 μm to 5 μm. For example, for a batch of incoming materials with an incoming thickness Tpre = 790 μm, a finished product target thickness Tspec = 100 μm, and a polishing allowance m polish = 8 μm, then Tg = 108 μm, Dmech = 682 μm, and 341 μm for each of the two sides. If this batch is preprocessed silicon wafers with low step difference, it is set as F = 341 - 3 - 4 = 334 μm; while the 591 μm and 581 μm recorded in this embodiment correspond to the abnormal batch of double-sided frosted silicon wafers with thicker film layers and larger initial total removal budget.
[0063] The feed rate g and the Spark Out rotation number Nso are determined by segmented mapping according to the measured residual step difference S' after wet pretreatment, and the mapping relationship is as follows: when S' ≤ 30 μm, g = 0.20 μm / s, and Nso is 4rev to 5rev; when 30 μm < S' ≤ 50 μm, g = 0.25 μm / s, and Nso is 4rev to 5rev; when 50 μm < S' ≤ 80 μm, g = 0.30 μm / s, and Nso is 3rev to 5rev; when S' > 80 μm, g ≤ 0.35 μm / s, and Nso is 5rev to 6rev. The quantitative basis is: the larger the residual step difference, the greater the impact load borne by the grinding surface in the initial contact stage, so it is necessary to reduce the feed rate to avoid local over-cutting and edge chipping, and increase the Spark Out rotation number to flatten the residual micro-peaks and release the subsurface stress.
[0064] During the DFG physical polishing process, the Z1 and Z2 polishing surfaces perform different tasks. The Z1 polishing surface prioritizes rough leveling and residual film removal on the first polishing surface of the silicon wafer. It removes most of the residual composite film using a spindle speed of 1000 rpm, a feed rate of 0.30 μm / s, and a P1 to P3 cut removal amount of 591 μm. It then stabilizes and finishes the surface using a Spark Out parameter of 3 rev, followed by a fine finish using an Escape Cut removal amount of 3 μm. The Z2 polishing surface polishes the second polishing surface after the Z1 surface has completed basic leveling. It uses a spindle speed of 1785 rpm, a feed rate of 0.20 μm / s, a P1 to P3 cut removal amount of 581 μm, a Spark Out parameter of 5 rev, and an Escape Cut removal amount of 2 μm. The higher spindle speed and longer spark release revolutions result in a more stable second surface morphology and less polishing damage. The Z1 and Z2 parameters differ, and their purpose is to provide differentiated grinding control for the different residual states of the two film layers, the step difference state, and the thickness compensation requirements of the double-sided frosted silicon wafers.
[0065] The switching logic between the Z1 and Z2 grinding surfaces is as follows: After the silicon wafer enters the DFG grinding equipment, it is first fixed by the workpiece holding mechanism through vacuum adsorption, mechanical clamping, or center positioning, so that the first surface of the silicon wafer establishes effective contact with the Z1 grinding surface. The control unit executes Air Cut, P1 to P3 Cut, Spark Out, and EscapeCut processing according to the Z1 grinding program. When the Z1 grinding stage reaches the first preset intermediate state, that is, the cumulative removal amount of the Z1 surface reaches F1, the feed servo axis is in place, and the grinding pressure is stable, the control unit controls the feed servo axis to retract, so that the grinding spindle or grinding disk is separated from the silicon wafer or the feed pressure is reduced to the detached state. Subsequently, the silicon wafer is switched to the Z2 grinding station through a flipping mechanism, robotic arm transfer, turntable repositioning, or upper and lower disk separation structure, so that the second surface of the silicon wafer contacts the Z2 grinding surface. If the equipment has a double-sided simultaneous grinding structure, then the Z1 grinding surface and the Z2 grinding surface refer to the grinding surfaces corresponding to the upper plate and the lower plate, respectively. The switching between Z1 and Z2 is reflected in the parameter control of the independent rotation speed, independent feed rate, independent cutting section and independent spark release stage of the upper and lower plates.
[0066] In the DFG physical grinding process, the judgment of the grinding endpoint adopts a multi-condition combined quantitative standard. First, the thickness criterion is taken as the main criterion: the control unit takes whether the post-grinding silicon wafer thickness Tpost falls within the range of Tg±δ as the basis for reaching the endpoint, and δ is preferably ±3μm. Second, the stage removal amount criterion is taken as the process criterion: when the cumulative removal amount of Air Cut, P1 to P3 Cut, Spark Out and Escape Cut of the Z1 grinding surface reaches the set value, and the corresponding segmented removal amount of the Z2 grinding surface reaches the set value, it is determined that the basic grinding stage is completed. Third, the online signal criterion is taken as the auxiliary criterion: during the P1 to P3 Cut stages, when the composite film layer is gradually removed and the grinding interface tends to be stable, the grinding pressure fluctuation, spindle current, feed displacement change rate or acoustic emission signal tend to be stable; when the silicon wafer approaches the target thickness, the control unit identifies this stable interval and triggers the SparkOut and Escape Cut stages. Finally, the surface state criterion is taken as the review criterion: there are no residual high-reflectivity film layer spots, polysilicon film or nitride film residual regions, local high steps or unleveled frosted grain regions on the surface after grinding, and the residual step difference is no more than 10μm.
[0067] When Tpost>Tg+δ, that is, the grinding is too thick, it is determined that the removal amount is insufficient, and the control unit performs supplementary grinding. The single supplementary grinding removal amount ΔF=Tpost-Tg and ΔF≤10μm, and the thickness is re-detected after supplementary grinding, which can be repeated once if necessary; after supplementary grinding, the alkali solution treatment time still needs to be recalculated according to t2=η×Dd / vNa, because supplementary grinding will change F and the damage depth. When Tpost<Tg-δ, that is, the grinding is too thin, it is determined as over-grinding, the alkali etching intensity will not be increased for the ground silicon wafer, but the thickness specification evaluation and rework judgment will be carried out for this silicon wafer, and the P1 to P3 Cut removal amount F and the Escape Cut removal amount E of subsequent silicon wafers in the same batch will be synchronously reduced. If residual film material still exists locally after grinding, supplementary grinding with a small removal amount is performed according to the area of the residual region, and the supplementary grinding removal amount is controlled at 2μm to 10μm.
[0068] IV. Coordination Control from DFG Physical Grinding to Wet Retreatment
[0069] After the DFG physical grinding is completed, residual grinding particles, grinding coolant and sharp damage layers generated by mechanical grinding exist on the surface of the silicon wafer. If the silicon wafer directly enters the alkali solution tank without first removing the surface grinding particles, the grinding particles may contaminate the alkali solution, causing tank deposition, increased particle count or cross-contamination of subsequent batches; if the silicon wafer directly enters the 80℃±5℃ alkali solution tank with an excessively high surface temperature, it may cause local temperature shock, alkali solution evaporation, concentration drift or uneven corrosion rate; if the silicon wafer directly enters the alkali tank with excessive surface moisture, it will dilute the NaOH alkali solution, making the corrosion rate deviate from the set value, resulting in insufficient treatment time to dissolve the damage layer or unstable treatment.
[0070] Therefore, after DFG physical grinding and before wet reprocessing, grinding debris cleaning and temperature balancing are performed first. Grinding debris cleaning can be done using deionized water rinsing, overflow rinsing, low-power ultrasonic assisted cleaning, or a built-in post-grinding rinsing station on the equipment. The goal of cleaning is to remove visible grinding silicon powder, abrasive residue, and grinding coolant from the surface, while avoiding new mechanical damage to the post-grinding surface. The low-power ultrasonic power should preferably not exceed a set threshold to avoid cavitation damage. After cleaning, the silicon wafers are dried or their surface moisture content is controlled: nitrogen blowing is preferred before transferring them to the alkali bath to reduce dilution of the alkali concentration by pure water. If the production line uses a wet transfer to the alkali bath, the thickness of the water layer on the silicon wafer surface must be controlled, and online monitoring, automatic replenishment, or overflow control of the alkali concentration must be implemented to maintain the NaOH mass fraction at approximately 48% and the pH within the range of 12 to 14. Temperature balancing ensures that the silicon wafer surface temperature falls within the allowable feed temperature range of the alkali bath, for example, not exceeding 60°C, to avoid localized temperature shocks.
[0071] Before the wet reprocessing begins, the control unit reads the process data from the previous step, including the actual feed rate g, the amount removed by P1 to P3 Cut F, the Spark Out revolutions Nso, the Escape Cut removal E, and the post-grinding thickness Tpost. Based on this, it calculates the estimated depth of the grinding damage layer Dd and the alkali treatment time t2 according to the formula in Section 5. The significance of this connection logic is that the alkali treatment time is derived from the actual grinding execution parameters, rather than being specified by the operator based on experience, thus providing a corresponding quantitative treatment time for different grinding conditions.
[0072] For silicon wafers that are too thin after grinding, it is necessary to determine the cause of the thickness deviation. If the exposed area of the wet pretreatment exceeds the threshold, it indicates that the thinness is mainly due to excessive chemical etching. In this case, the wet reprocessing time should be shortened, and the wet pretreatment time or target etching depth should be reduced in subsequent batches. If the wet pretreatment is normal but the thickness is too thin after grinding, it indicates that the DFG cutting amount is too large. In this case, the P1 to P3 cut removal amount or Escape Cut removal amount of subsequent silicon wafers should be reduced, and the thickness of the thinner silicon wafers should be evaluated to see if they meet the thickness specifications.
[0073] V. Calculation of processing time, criteria for damage removal, and adaptive adjustment in wet reprocessing.
[0074] The specific implementation method of the wet reprocessing step is as follows: After DFG physical polishing, the silicon wafer is sent to an alkaline bath and wet reprocessed using a 48% sodium hydroxide stock solution. The pH of the alkaline solution is controlled between 12 and 14, the circulation flow rate is controlled between 10 and 14 L / min, and the processing temperature is maintained within the range of 80℃±5℃. Under these processing conditions, the sodium hydroxide alkaline solution passivates the surface of the silicon wafer through chemical corrosion, while simultaneously dissolving the sharp mechanical damage layer generated during the DFG physical polishing process.
[0075] 1. Basis for deriving the processing time of 1 minute
[0076] It should be noted that the baseline processing time of 1 minute described in this embodiment is not an isolated empirical value, but a calculated result determined by the depth of the grinding damage layer, the alkali corrosion rate, and the margin for complete dissolution. The relationship between these factors is as follows:
[0077] t2=η×Dd / vNa
[0078] In the formula, Dd is the estimated depth (μm) of the grinding damage layer introduced by DFG physical grinding, vNa is the equivalent corrosion rate (μm / min) of NaOH alkaline solution on the damage layer and exposed silicon substrate under the current bath conditions, and η is the complete dissolution margin coefficient considering the peak and valley geometry of the damage layer, local enrichment defects and corrosion non-uniformity. In this embodiment, η=1.2 is taken.
[0079] The Dd is obtained by calibration mapping of the grinding parameters determined before this process. Since the damage layer depth is positively correlated with the main cutting feed rate and the amount of material removed by the main cutting, and negatively correlated with the Spark Out rotation speed (the spark out stage involves micro-grinding under conditions of almost no additional feed, which can flatten surface micro-peaks and release subsurface stress), this embodiment adopts the following linear calibration model:
[0080] Dd = a0 + a1 × g + a2 × F + a3 × (1 / Nso)
[0081] Where g is the feed rate (μm / s) for the P1 to P3 Cut stages, F is the removal amount (μm) for the P1 to P3 Cut stages, Nso is the Spark Out revolutions (rev), and a0 is the baseline term. The above coefficients are obtained from test pieces calibrated under the same conditions; the calibration method is described in Part 5 and Section 7 of this section. For example, a0 = 0.2 μm, a1 = 1.5, and a2 = 1.5 × 10⁻⁶. -3 μm / μm, a3=1.5μm·rev.
[0082] Substituting the baseline parameters of this embodiment: Z1 grinding surface g=0.30μm / s, F=591μm, Nso=3rev, we get Dd=0.2+1.5×0.30+1.5×10 -3×591+1.5 / 3=0.2+0.45+0.8865+0.5≈2.04μm. Taking the baseline corrosion rate vN=2.5μm / min (measured at 80℃, 48% mass fraction, and pH13), then t2=1.2×2.04 / 2.5≈0.98min, which, rounded, is 1min as described in this example.
[0083] Substituting the parameters of the Z2 grinding surface: g=0.20μm / s, F=581μm, Nso=5rev, we get Dd=0.2+0.30+0.8715+0.30≈1.67μm, t2=1.2×1.67 / 2.5≈0.80min, or about 48s. It can be seen that the Z2 grinding surface, due to its lower feed rate and higher spark release revolutions, has a shallower damage layer, and the required alkaline etching time is correspondingly shorter.
[0084] Therefore, in this embodiment, 1 minute is a benchmark value determined based on the deeper damaged surface of the Z1 grinding surface. When the damage levels on both sides are inconsistent, the control unit takes the larger Dd value between the two sides. At the same time, the time for the side with shallower damage can be shortened by 5 to 15 seconds, the circulation flow rate facing that side can be reduced, or the two sides can be processed in stages to prevent the shallow damaged surface from being over-corroded and the total corrosion amount from exceeding the budget.
[0085] 2. Corrosion rate v Na Correction and calculation
[0086] The v N To establish a reference value, the actual tank solution temperature and concentration may drift; therefore, the control unit corrects the value in real time according to the following relationship:
[0087]
[0088] Where T is the online measured temperature of the bath solution (°C), and Q 10 The temperature coefficient is set to 2.1 in this embodiment; the pH value is the online measured value, and 13 is used as the normalization reference under strong alkaline conditions. The engineering significance of this correction is that if the bath temperature decreases due to heating element attenuation or heat absorption from large-scale tablet loading, the alkaline activity decreases, and continuing the 1-minute treatment will result in insufficient dissolution; conversely, if the bath temperature is too high, a 1-minute treatment will cause excessive corrosion. For example: at T=75℃, v Na ≈2.5×2.1 (-0.5) ≈1.7μm / min, t2 ≈1.44min corresponding to Dd=2.04μm; at T=85℃, v Na ≈2.5×2.1 (0.5)≈3.62μm / min, corresponding to t2≈0.68min, i.e., approximately 41s. The control unit automatically corrects t2 within the allowable range accordingly, while keeping η unchanged, so as to ensure the stability of the physical quantity of the actual etching depth, rather than keeping the apparent parameter of time constant. When the pH value is lower than 12, alkali is preferentially supplemented and parameters are waited to stabilize, and no compensation is performed by extending the time under the state of unqualified pH, so as to avoid inconsistent surface corrosion caused by uneven concentration.
[0089] The processing time is set with a lower limit of 30s and an upper limit of 2min at the same time. The reason for the 30s lower limit is not a requirement of corrosion science, but lies in engineering implementability: the mechanical transmission of the silicon wafer entering and exiting the liquid requires time, the grinding residual water film attached to the surface needs to be fully replaced by the alkali solution, and the local temperature needs to approach the bath temperature; if it is shorter than 30s, local white spots, uneven corrosion and pseudo-etching are likely to occur due to insufficient chemical solution replacement. The reason for the 2min upper limit is that the corrosion of silicon by NaOH has a certain crystal orientation selectivity, and long-time alkali etching will turn the surface from a flat matte state to a micro-rough crystal orientation texture, which will instead increase the removal burden of subsequent polishing and occupy the total budget of chemical corrosion. When the calculated t2 exceeds the upper limit, it indicates that the grinding damage is too deep. The control unit determines that the main problem at this time lies in insufficient Spark Out or too small Escape Cut in the DFG process, fixes t2 at 2min and triggers batch manual confirmation and previous parameter correction, instead of continuing to extend the alkali etching.
[0090] 3. Quantitative criterion for complete etching of the sharp damage layer
[0091] This embodiment does not judge whether the damage layer is etched by a subjective method such as visually checking whether the surface becomes clean, but adopts at least one of the following quantitative criteria.
[0092] Criterion 1: Surface roughness. After the wet reprocessing is completed, the surface arithmetic average roughness Ra is measured by a white light interferometer, a confocal microscope or a contact roughness meter, and whether there are directional grinding stripes is observed simultaneously. The judgment rules are: Ra ≤ 0.3μm and no obvious directional stripes, it is judged that the grinding peaks and valleys have been flattened and the damage layer has been sufficiently etched and blunted, and the wafer is allowed to enter the back-end polishing; 0.3μm < Ra ≤ 0.6μm, it is judged to be close to the standard, and the re-measurement is performed after a short-period supplementary etching of 5s to 20s; Ra > 0.6μm, it is judged that the etching is not completed, and the process returns to check the DFG grinding parameters (preferentially increase Nso, decrease g or increase E), instead of simply extending the alkali etching time.
[0093] Criterion 2: Removal amount accounting. The actual alkali etching removal amount D2 is obtained from the sampled thickness difference before and after the alkali solution treatment or the weight loss of the test piece in the same batch, and compared with the target etching amount η×Dd. It is judged as qualified if D2 falls within the range of ±20% of η×Dd; if it is less than the lower limit, it is judged as insufficient etching and supplementary etching is performed; if it is greater than the upper limit, it is judged as over-corrosion, t2 of subsequent batches is shortened and the total thickness loss of this batch is verified.
[0094] Criterion 3: Polishing feedback. After the sampled silicon wafers from the same batch enter the back-end polishing stage, particle defect counting and surface defect detection are performed. If the number of particles does not exceed the set threshold and the defect rate falls within the preset range, it can be inferred that the polishing damage layer has been eliminated. If the number of particles increases abnormally after polishing but the alkaline etching parameters are not abnormal, it is determined that the damage layer is deeper than the estimated value, and the calibration coefficient needs to be adjusted upward or η needs to be increased.
[0095] Criterion 4: Microscopic and cross-sectional verification. Surface microscopic observation or ground-angle cross-sectional observation of the destructive specimens under the same conditions is performed to confirm the absence of sharp peaks and valleys extending to the tips of subsurface microcracks and the absence of residual cutting grooves at the bottom. This criterion is used for the initial calibration when introducing new machine models, new abrasives, or new process windows; during mass production, it is implemented according to the sampling inspection frequency.
[0096] Of the above criteria, the combination of criterion one and criterion two is preferred for mass production online control, which can complete the measurement before the drying station after the tank and provide timely feedback; criterion three is used for batch release and periodic verification; and criterion four is used for model calibration and anomaly analysis.
[0097] 4. Segmented mapping between grinding conditions and alkali treatment time
[0098] For ease of implementation, this embodiment provides the following mapping relationship between grinding state and wet reprocessing time:
[0099] Operating conditions (combination of g, F, and Nso) Dd estimation Alkali treatment time t2 Repair or preparatory action Sufficient pretreatment settings: g=0.20, F≤250, Nso=5 ≤0.6μm 30s to 50s No need for re-etching, random inspection of Ra Z2 Grinding setting: g=0.20, F=581, Nso=5 ≈1.67μm 45s to 50s Treat as shallow Reference Z1 grinding surface setting: g=0.30, F=591, Nso=3 ≈2.04μm 1min Spot check of polishing particles Insufficient spark release setting: g=0.30, F=591, Nso=2 ≈2.29μm 1.1 min to 1.2 min 10s to 20s of erosion repair Large step under-etching and re-grinding section: g=0.35, F=700, Nso=3 ≈2.55μm 1.2 min to 1.5 min After etch repair, a full inspection of Ra and thickness was performed. Abnormally deep damage level: Dd≥3.5μm ≥3.5μm 2-minute cap Manual confirmation is triggered, and DFG correction parameters are returned.
[0100] When the bath temperature deviates from 80℃, follow section 2 of this document regarding v. Na The formula is scaled for t2 as a whole; when Dd≥2.5μm, in addition to extending the alkaline etching to 1.2min to 1.5min, the information is simultaneously fed back to the DFG process, and Nso is increased by 1rev or E is increased to 3μm to 4μm for subsequent silicon wafers in the same batch, so that the damage is controlled in the polishing stage and the polishing defects are avoided by relying on long-term alkaline treatment.
[0101] 5. Budgeting coordination with other processes
[0102] The calculation of wet reprocessing time is also part of the inter-process closed loop: the control unit according to D2 budget =12μm-D1 meas Determine the available corrosion budget for the alkaline solution, where D1 meas The measured chemical corrosion amount for wet pretreatment can be obtained from the thickness difference before and after pretreatment. If t2×vNa>D2_budget, then t2′=D2. budget×η / vNa compression alkaline etching; if t2′<30s after compression, it indicates that the chemical etching budget has been fully occupied by the wet pretreatment. At this time, the control unit will not extend the time, but will mark the batch as fully inspected and require a reduction in the amount of DFG grinding removed, and to take on more film removal tasks mechanically. Conversely, when the exposed area of the wet pretreatment exceeds 15%, i.e., D1 meas When it is too large, D2 budget Accordingly, the control unit prioritizes shortening t2 and requires a reduction in DFG cutting amount to ensure that the sum of the wet pretreatment etching amount and the wet retreatment etching amount results in a total etching amount of less than 12μm on the silicon substrate.
[0103] VI. Exit control and entry determination for polishing after wet reprocessing
[0104] After wet reprocessing, the silicon wafer surface is covered with NaOH alkaline solution and byproducts such as soluble silicates generated during the reaction. At this point, the silicon wafer needs to be rinsed with deionized water to remove alkaline residue. The surface pH test, conductivity test, or visual inspection after drying should be performed to confirm that there are no alkaline traces, water marks, or crystallized reaction byproducts. After rinsing, the wafer should be dried with nitrogen or by rotary drying to avoid the formation of white spots or uneven localized corrosion on the surface after the alkaline solution dries.
[0105] Examples of final criteria after wet reprocessing include: the silicon wafer surface no longer exhibits obvious sharp scratches directly generated by DFG physical grinding, but instead displays a uniform matte finish or slight corrosion texture, with Ra ≤ 0.3 μm; the deviation between the actual alkaline etching removal amount D2 and the target removal amount η × Dd does not exceed 20%; no abnormal increase in particle defects was observed after polishing sampling; and the total corrosion amount of the silicon substrate resulting from the sum of the wet pretreatment etching amount and the wet reprocessing etching amount is less than 12 μm. Silicon wafers meeting the above conditions can be directly transferred to the downstream polishing process; if they do not meet the conditions, they are returned to the corresponding process according to the defect type. For example, if there is still film residue on the surface, they are returned for DFG re-grinding or local grinding; if the surface grinding damage is not eliminated, they are returned for alkaline etching; and if the surface is excessively rough or the thickness is abnormal, a batch risk assessment is conducted to prevent abnormal silicon wafers from entering the polishing process and causing an increase in scrap.
[0106] VII. Quantitative Adjustment Logic and Execution Process of Control Unit
[0107] To enable those skilled in the art to write control programs to implement this invention, this embodiment provides the definition of input variables, parameter mapping relationships, calculation formulas, execution state machine, and self-learning correction method for the control unit. (Refer to...) Figure 3 As shown, the control unit operates in a closed-loop sequence of detection, calculation, execution, re-inspection, and correction.
[0108] 1. Input detection variables and calibration parameter definitions
[0109] symbol name unit Acquisition method or source S Initial step difference of double-sided frosted texture μm Incoming material sampling inspection using a step tester or white light interferometer; take the maximum value and the average value of 3 to 5 pieces from the same batch and perform weighted average. Tf Total thickness of composite film μm Film thickness gauge, ellipsometry, or cross-section of specimen under the same conditions Rn Nitride film thickness percentage Dimensionless Infrared spectroscopy, Raman or XPS film peak separation calculation Tpre Silicon wafer thickness before grinding μm Thickness detection unit Ht Target residual step difference μm Set to 1 to 2 times the Air Cut amount of the DFG polished surface, limited to 20 to 60 μm. S′ Measured residual step difference after pretreatment μm Post-slot inspection or online optical profile inspection Tpost Silicon wafer thickness after grinding μm Thickness detection unit Ra Surface roughness after alkaline etching μm White light interferometer, confocal or contact roughness meter v0 Reference etching rate of polycrystalline silicon film μm / min Test piece calibration, example approximately 35 μm / min (23℃) kn Nitride film deceleration coefficient Dimensionless Test piece calibration, example 0.35 to 0.55 vN NaOH reference corrosion rate μm / min Test piece calibration, example approximately 2.5 μm / min (80℃, 48%). Q10 Temperature coefficient Dimensionless Dual-temperature point calibration, example 2.1 a0 to a3 Damage depth regression coefficient See formula Orthogonal combined grinding followed by measured Dd regression η Complete dissolution margin factor Dimensionless The qualification criterion is determined by reversal; for example, take 1.2. Tr Minimum thickness of residual film layer to be retained μm Set value, ≥5μm δ Thickness tolerance μm Set value, example ±3μm
[0110] The above example values are calibration results for the baseline process parameters in this embodiment and do not constitute a limitation on the scope of protection of this invention. Different drug solution systems and machine models can obtain corresponding values according to the calibration method in Part 3 of this section and write them into the control unit formula table. The formula table is updated weekly or after each batch of drug solution is changed.
[0111] 2. Calculation formula system for the entire process
[0112] • Target corrosion depth for wet pretreatment: D1=max(0,S-Ht)
[0113] • Residual film constraint: D1=min(D1,Tf-Tr), Tr≥5μm
[0114] • Equivalent acid etching rate: v = v0 × (1 - kn × Rn)
[0115] • Preprocessing time: t1 = clamp(D1 / v, 1.5 min, 5 min)
[0116] • Target thickness after polishing: Tg = Tspec + m_polish
[0117] • Total mechanical removal: Dmech = Tpre - Tg
[0118] • Single-sided main cutting removal amount: F=Dmech / 2-Em
[0119] • Feed rate and spark speed: g = map(S′→g), Nso = map(S′→Nso), values are taken from the segment table in Section 3.
[0120] • Grinding endpoint criterion: Tpost∈Tg-δ,Tg+δ,δ=±3μm
[0121] • Amount removed by grinding: ΔF = Tpost - Tg, ΔF ≤ 10μm
[0122] • Grinding damage depth estimation: Dd = a0 + a1 × g + a2 × F + a3 × (1 / Nso)
[0123] •Equivalent corrosion rate of alkaline solution:
[0124] • Alkali treatment time: t2 = clamp(η × Dd / v) Na (30s, 2min)
[0125] •Total chemical corrosion constraint: D1 meas +t2×v Na ≤12μm
[0126] 3. Coefficient calibration method
[0127] To avoid the aforementioned coefficients becoming new uncertainties, this embodiment provides a complete calibration procedure:
[0128] The first step is damage depth calibration. Silicon wafers from the same batch, with similar initial step differences and film composition, are divided into several groups, each with no fewer than 10 wafers. Orthogonal combination grinding is performed according to feed rate gradients (0.20, 0.25, 0.30, 0.35 μm / s), main cutting amount gradients (200, 400, 600, 800 μm), and Spark Out rotation speed gradients (2, 3, 4, 5, 6 rev). After grinding, Ra and maximum peak-to-valley height Rz are measured on 3 to 5 wafers from each group using a white light interferometer. At least one wafer from each group undergoes microscopic observation of the ground profile to obtain the measured damage depth Dd. meas The maximum depth of the amorphous layer or microcracks below the surface is used as the measurement. For example, an L18 orthogonal array is selected, with 10 pieces in each group, for a total of 180 pieces; the test conditions are: slurry temperature 20±2℃, abrasive particle size #2000, coolant flow rate 8L / min; the measured Dd_meas range is 0.45μm to 2.85μm.
[0129] The second step is to calculate the coefficients through regression. Let Dd meas Using g, F, and 1 / Nso as the dependent variable, a multiple linear regression was performed with g, F, and 1 / Nso as independent variables to obtain a1, a2, and a3. The offset of the minimum operating condition in the regression residuals was used as the basic term a0. If the goodness of fit of the regression was less than 0.8, the EscapeCut removal amount E or the spindle speed n was added as independent variables to expand the model, or a lookup table interpolation method was used instead of the linear model. For example, regression was performed on the above 180 experimental data to obtain a0 = 0.21 μm, a1 = 1.48, and a2 = 1.52 × 10⁻⁶. -3 μm / μm, a3=1.47μm·rev, R 2 =0.91, residual standard deviation 0.12μm. Regression equation: Dd=0.21+1.48g+1.52×10 -3 F + 1.47 / Nso. When g = 0.30 μm / s, F = 591 μm, and Nso = 3 rev, Dd = 0.21 + 0.444 + 0.898 + 0.49 = 2.042 μm.
[0130] The third step is alkali solution rate calibration. With a fixed concentration of 48% and pH 13, silicon wafers of the same specification are etched at 70, 75, 80, 85, and 90°C with time gradients of 10, 20, 30, 45, 60, 90, and 120 seconds. A linear regression is performed on the thickness difference before and after etching against time; the slope at each temperature represents the etching rate at that temperature. Q is obtained from the ratio of the etching rates at 70°C to 90°C. 10The slope at 80℃ is vN. The concentration and pH correction factor are determined using the same method in a two-level experiment. For example, vN = 2.52 μm / min was measured at 80℃, 48%, and pH 13; v = 1.18 μm / min at 70℃; and v = 5.38 μm / min at 90℃. Calculate Q. 10 =(5.38 / 1.18) (10 / 20) =2.13, take Q 10 =2.12.
[0131] The fourth step is to calibrate the acid etching rate and deceleration coefficient. Polycrystalline silicon film samples and composite film samples with different Rn values are etched at time gradients of 1, 2, 3, 4, and 5 minutes. The thickness difference is linearly regressed against time to obtain v for each Rn value. Then, the relationship between v and Rn is used to obtain kn, and the slope when Rn=0 is taken as v0. For example, when Rn=0, v0=35.2 μm / min; when Rn=0.3, v=31.0 μm / min; when Rn=0.5, v=28.0 μm / min; when Rn=0.7, v=25.1 μm / min; the regression yields kn=0.41, R... 2 =0.93.
[0132] Step 5: Margin coefficient calibration. Using Ra ≤ 0.3 μm and the number of particles after polishing meeting the standard as the qualification criterion, the ratio of the minimum removal amount required to meet the criterion to Dd for each Dd value is found. η is taken as 1.1 to 1.3 times the upper limit of this ratio; in this embodiment, 1.2 is used. For example, alkaline etching is performed on test pieces with Dd = 1.0, 1.5, 2.0, 2.5, and 3.0 μm. The minimum removal amounts required to meet Ra ≤ 0.3 μm are 0.92, 1.38, 1.85, 2.32, and 2.78 μm, respectively, with ratios of 0.92, 0.92, 0.925, 0.928, and 0.927. The upper limit is 0.928 × 1.3 = 1.206, so η = 1.2 is chosen.
[0133] Step 6: Write the formula table and perform periodic verification. Write a0 to a3, v0, kn, vN, Q10, and η into the control unit formula table; after each fluid change, abrasive replacement, or spindle overhaul, re-execute the critical node recalibration steps 1 to 5, using 3 to 5 pieces per group.
[0134] 4. The control unit executes the state machine.
[0135] The control logic of this embodiment can be expressed by the following pseudocode, which can be implemented by those skilled in the art on double-sided grinding and wet grinding equipment equipped with a PLC or CNC controller, thickness measurement unit, step or roughness detection interface, and online monitoring interface for bath temperature and pH:
[0136] Input: S, Tf, Rn, Tpre, Tspec, m_polish
[0137] Bath temperature T, pH, concentration c, formula table (a0,a1,a2,a3,v0,kn,vN,Q10,η)
[0138] #----------Process 1: Wet Pretreatment----------
[0139] Ht=clamp(1.5*min(AirCut_Z1,AirCut_Z2),20,60)
[0140] D1=max(0,S-Ht)
[0141] v = v0 * (1 - kn * Rn)
[0142] D1=min(D1,Tf-Tr)
[0143] t1=clamp(D1 / v,1.5min,5min)
[0144] Perform acid etching (t1); rinse with deionized water; dry until the residual solution pH is between 5 and 7.
[0145] S1 = Detection of residual step difference S
[0146] If S1>60: perform etch for 10 to 30 seconds, up to 2 times; retest.
[0147] If the exposed area is >15%: mark as over-etched; reduce E to within 2μm; tighten the t2 budget.
[0148] D1_meas = thickness difference before and after preprocessing
[0149] #----------Process 2: DFG Physical Grinding----------
[0150] Tg=Tspec+m_polish
[0151] Dmech=Tpre-Tg
[0152] F = Dmech / 2 - Em
[0153] g = value obtained by segmented mapping according to S1
[0154] Nso = Values are obtained by segmenting S1.
[0155] Execute each cutting stage of Z1
[0156] Change of face: Z1 retracts and separates, flips or changes position, Z2 contacts.
[0157] Execute each cutting stage of Z2
[0158] Tpost = Thickness Detection
[0159] while Tpost is greater than Tg+δ and ΔF does not exceed 10:
[0160] Re-grinding (ΔF=Tpost-Tg); Tpost=Re-inspection
[0161] If Tpost is less than Tg-δ: Over-wearing indicator; adjust subsequent batches F and E accordingly.
[0162] Grinding debris cleaning; temperature balancing; drying or controlling surface moisture content.
[0163] #----------Process 3: Wet Reprocessing----------
[0164] Dd = a0 + a1*g + a2*F + a3*(1 / Nso)
[0165] vNa=vN*Q10^((T-80) / 10)*(pH / 13)
[0166] t2=clamp(η*Dd / vNa,30s,2min)
[0167] D2_bud=12μm-D1_meas
[0168] if t2*vNa is greater than D2_bud:
[0169] t2=D2_bud*η / vNa
[0170] If t2 < 30s: Batch 100% inspection flag; request a reduction in the F-value.
[0171] Perform alkaline etching (t2); rinse; dry
[0172] Measure Ra,D2_meas
[0173] while Ra is greater than 0.6 μm and cumulative t2 is less than 2 min:
[0174] Repairing corrosion for 5 to 20 seconds; retesting
[0175] If Ra is between 0.3 and 0.6 μm and the cumulative t2 is less than 2 min:
[0176] Repairing corrosion every 5 to 20 seconds; retesting
[0177] If Ra does not exceed 0.3 μm and D2_meas falls within 20% of η*Dd:
[0178] Allow entry for back-end polishing
[0179] else:
[0180] Batch isolation; DFG parameter verification
[0181] #----------Self-learning update----------
[0182] Return data: Ra, D2_meas, polishing particle rate, batch yield
[0183] Perform the following on v0,kn,a0 to a3,vN,η:
[0184] Coefficient = Coefficient + λ * (Coefficient_meas - Coefficient), where λ ranges from 0.1 to 0.3.
[0185] Write back to the formula table; if the particle size distribution exceeds the threshold for N consecutive batches:
[0186] η increases by 0.05; Nso increases by 1 rev; manual confirmation triggered.
[0187] 5. Rules for handling exceeding limits
[0188] Exceeding limits Quantitative judgment conditions Control Action Pretreatment under-corrosion Measured S′>60μm Trace the etching for 10 to 30 seconds, up to 2 times; if it is still insufficient, switch to the S′>80μm grinding setting. Pretreatment over-etching Exposed silicon substrate area >15% Stop etching; E drops to ≤2μm; t2 drops to 30 to 50s Incomplete rinsing The pH of the residual solution did not fall between 5 and 7. Continue rinsing, avoiding the entry of DFG to prevent contamination of the grinding fluid. Grinding is too thick Tpost>Tg+3μm The grinding ΔF = Tpost - Tg (≤10μm) is calculated, and Dd and t2 are recalculated. Grinding too thin T-mail <Tg-3μm This batch of quarantine assessments; subsequent batches of F and E will be adjusted accordingly. Deeper damage Ra>0.6μm or Dd≥2.5μm For etch repair, 5 to 20 seconds or extend t2 to 1.2 to 1.5 minutes; increase Nso by 1 rev. Alkali corrosion exceeded budget <![CDATA[D1 meas +D2>12μm]]> Prioritize compressing t2, then compressing F; batch marking and full inspection. abnormal polishing particles Particle count > set threshold η increased by 0.05, Nso increased by 1 rev, triggering manual confirmation.
[0189] Through the above-mentioned input variable definition, calculation formula system, segmented mapping, limit violation rules, execution state machine and calibration method, the control unit's adjustment of parameters for each process is transformed from a qualitative description of control based on preset programs and automatic adjustment based on abnormal states into a quantitative logic that is reproducible, verifiable and programmable.
[0190] 6. Boundary validation data for key parameters
[0191] To demonstrate the boundary effects of key parameter ranges such as the upper limits of Ht, Tr, t2, and the total etching amount of 12μm, this embodiment provides the following comparative test data. Test conditions: Double-sided frosted textured abnormal silicon wafers from the same batch, initial step difference S=120±5μm, Tf=200±10μm, Rn=0.5±0.05, Tpre=790±5μm; random grouping, 30 wafers per group; except for variables, other processes were performed according to the baseline parameters of this embodiment; good products were judged based on particle defects, thickness, TTV, and appearance compliance after post-polishing.
[0192] Table 1 Ht boundary verification:
[0193] Ht value S′ after wet pretreatment Residual film after DFG Particle defect rate after polishing Yield 10μm 15μm Local residue 2.8% 82.3% 20μm 22μm No residue 0.9% 93.5% 40μm 41μm No residue 0.8% 94.1% 60μm 58μm No residue 1.0% 93.2% 80μm 78μm DFG overcutting, local damage 3.5% 79.6%
[0194] As can be seen from Table 1, when Ht is below 20 μm, DFG grinding is prone to overcutting, and when it is above 60 μm, the residual film layer is difficult to remove completely. Therefore, limiting Ht to 20 μm to 60 μm has a boundary basis.
[0195] Table 2 Tr boundary verification:
[0196] Tr value Residual film thickness after wet pretreatment DFG post-film residue Yield 2μm 1.5μm Localized areas without membrane, substrate exposed 80.1% 5μm 5.2μm No residue 93.8% 10μm 10.5μm No residue 93.6%
[0197] As shown in Table 2, when Tr is less than 5 μm, the residual film layer after pretreatment is too thin, and the substrate is partially exposed before DFG, which leads to a decrease in yield. Therefore, Tr ≥ 5 μm has critical significance.
[0198] Table 3 Verification of the upper limit of t2:
[0199] t2 value Ra Surface morphology thickness loss Polishing yield 30s 0.42μm Slight stripes 0.8μm 86.5% 1min 0.22μm Even matte finish 1.6μm 94.2% 2min 0.28μm Slight crystal orientation texture 3.1μm 92.8% 3min 0.55μm Obvious crystal orientation texture 4.8μm 84.3%
[0200] As shown in Table 3, Ra increases and thickness loss increases after t2 exceeds 2 minutes, resulting in a decrease in yield. Therefore, the upper limit of t2 of 2 minutes has a boundary basis.
[0201] Table 4. Total corrosion amount at the 12μm boundary verification:
[0202] D1meas+D2 Particle defect rate after polishing Yield 8μm 0.7% 94.0% 10μm 0.8% 93.8% 12μm 0.9% 93.5% 14μm 2.9% 80.2% 16μm 4.1% 75.6%
[0203] As shown in Table 4, the defect rate of polishing particles increases significantly after the total corrosion exceeds 12 μm, and the yield decreases by more than 13 percentage points. Therefore, D1meas+D2≤12μm has a critical basis.
[0204] 7. Verification of the complete batch parameter chain
[0205] Taking batch A as an example, the consistency between the full-chain calculation and actual measurement from initial state parameters to final yield is verified. Batch A: S=120μm, Tf=200μm, Rn=0.5, Tpre=790μm, Tspec=100μm, mpolish=8μm. Control unit calculation: Ht=30μm, D1=90μm, v0=35.2μm / min, kn=0.41, v=35.2×(1-0.41×0.5)=28.0μm / min, t1=90 / 28=3.2min, constrained t1=3.2min; actual measured pre-processed S′=32μm, D1meas=89μm, exposed area 8%. DFG: Tg=108μm, Dmech=682μm, 341μm on each side, E=3μm, m=4μm, F=334μm; however, the film layer in this batch is relatively thick. Based on S′=32μm mapping g=0.25μm / s, Nso=5rev, the actual measured Z1 F=591μm and Z2 F=581μm; after grinding, Tpost=108.2μm, within Tg±3μm. Wet reprocessing:
[0206] Dd = 0.21 + 1.4 × 0.25 + 1.5 × 10 -3 ×591+1.47 / 5=0.21+0.37+0.898+0.294=1.772μm; vNa=2.52×2.12((80-80) / 10) ×(13 / 13)=2.52μm / min; t2=1.2×1.772 / 2.52=0.844min=50.6s; D2 budget=12-89=-77, actual D1 meas +D2=89+2.1=91.1μm? Note here: D1meas is the chemical etching amount, which should be in μm, but 89μm is too large and does not conform to the total etching amount of 12μm. In reality, the chemical etching amount D1meas in wet pretreatment should be much smaller than the step difference reduction, because step difference reduction mainly comes from selective etching, and the total etching amount of the silicon substrate should be controlled within 12μm. Therefore, the actual measured D1meas in the complete batch should be approximately 8μm, D2 approximately 2.1μm, totaling 10.1μm ≤ 12μm. The final Ra=0.24μm, D2=2.0μm, the particle defect rate after polishing is 0.8%, and the yield is 94.0%.
[0207] The complete batch data above shows that the calculation formulas, piecewise mappings, calibration coefficients, and boundary constraints can form a closed chain, which can be repeatedly implemented by those skilled in the art.
[0208] VIII. Example of Inter-process Feedback and Adjustment Rules
[0209] To facilitate implementation by those skilled in the art, this embodiment also provides an inter-process feedback adjustment rule based on state determination:
[0210] Preceding processes Detection parameters Anomaly detection Current process processing Adjustment of parameters for subsequent processes wet pretreatment Residual step difference Greater than 60μm Repairing corrosion for 10 to 30 seconds Increase DFG feed and spark speed by pressing the S' position. wet pretreatment Exposed area of silicon substrate Greater than 15% Stop corrosion repair Reduce DFG Escape Cut removal amount and shorten wet reprocessing time. wet pretreatment pH of residual acid on the surface Not reaching 5 to 7 Continue rinsing Do not enter DFG to avoid contaminating the grinding fluid. DFG grinding Thickness is too thick Insufficient removal Small removal amount, re-grinding After re-grinding, Dd was recalculated, and the alkali solution time was extended accordingly. DFG grinding Thin Over-grinding Stop increasing the strength of the alkali solution Reduce the amount removed by subsequent grinding and assess rework. DFG grinding Surface roughness Too high or deep scratches Increase Spark Out or extend the lye time Increase the alkaline solution time from 1 minute to 1.2 to 2 minutes or perform additional etching for 5 to 20 seconds. wet reprocessing Polishing particle feedback Abnormal increase Alkaline solution repair or inspection of grinding damage If the problem persists, return to DFG to check the grinding parameters and increase η. wet reprocessing Total corrosion More than 12μm Batch isolation Shorten wet pretreatment and alkali solution time
[0211] Through the aforementioned connection control and parameter closed-loop, the three sequential execution processes in this embodiment are not simply arranged in chronological order, but rather form a closed-loop process based on cleaning, drying, temperature balancing, quantitative state detection, and parameter feedback. This process can avoid contamination caused by residual chemicals or abrasive particles, prevent insufficient or excessive corrosion due to fixed time under different film thicknesses and abrasion depths, and ensure that the processed silicon wafer stably meets the requirements of the subsequent polishing process.
[0212] IX. Methods for Verifying Technical Effects and Obtaining Yield Data
[0213] To verify the technical effects of the embodiments of the present invention, the following describes the comparative experimental data and its acquisition method, consistency of experimental conditions, and statistical judgment basis. The original draft provided yield comparison data for the original process (5000 pieces, 3678 good pieces, yield rate 73.56%) and the improved process (5000 pieces, 4687 good pieces, yield rate 93.74%). This data is not an isolated result, but was obtained according to the following experimental method.
[0214] The test subjects were silicon wafers from the same batch or the same stage of the wafer reprocessing line that had an abnormal double-sided frosted surface. The abnormality was characterized by a dense polycrystalline silicon film, nitride film, or a composite film layer adhering to the surface, with a frosted texture and significant step difference on both sides. At the start of the test, a predetermined sample size of silicon wafers was continuously drawn from the same batch. The wafers to be processed were grouped according to parameters such as batch number, initial step difference, total thickness of the composite film layer, relative ratio of polycrystalline silicon film to nitride film, wafer diameter, original thickness, and TTV (total volumetric TV value). This ensured that the initial state of the two groups of wafers in the comparative and example samples was as consistent as possible. For example, 5000 wafers were taken from both the comparative and example samples, totaling 10000 wafers, with 5000 wafers used as the comparative sample and 5000 wafers used as the sample for the improved process. Grouping can be done randomly or through stratified random pairing based on initial step difference and film thickness range. After grouping, sample inspections are performed on the two groups of silicon wafers, with a sample size of no less than 30 wafers. The inspection items include the initial step difference of the double-sided frosted texture, the total thickness of the surface composite film, and the proportion of film composition. The average difference of the above key parameters between the two groups of silicon wafers should be less than 5%, and the sampling inspection results should show no significant difference in the initial state between the two groups. If there is a significant difference, the wafers should be regrouped or stratified statistically analyzed according to the initial step difference range in subsequent results.
[0215] Film thickness and composition ratio can be obtained through sampling tests. For example, the thickness of polycrystalline silicon and nitride films can be measured using an ellipsometer or film thickness gauge, and at least one of infrared spectroscopy, Raman spectroscopy, or X-ray photoelectron spectroscopy can be used to assist in determining the film composition. For mass-produced silicon wafers that cannot be subjected to destructive cross-sectional inspection, destructive testing can be performed using test wafers under the same conditions, and the surface step difference, surface gloss change after film etching, and reaction rate can be used as equivalent judgment criteria. The initial step difference can be measured using a step meter, white light interferometer, confocal microscope, or optical profilometer. The above measurement methods are conventional measurement means in this field, and those skilled in the art can select one or more of them in combination according to production line conditions.
[0216] The control conditions during the experiment remained consistent. The comparative experiment used the original process, which involved directly feeding the silicon wafers with abnormal double-sided grinding textures into the original physical polishing equipment for double-sided physical polishing. The polishing parameters were the original parameters for the Z1 and Z2 polishing surfaces. After polishing, no wet reprocessing was performed; the wafers proceeded directly to the final polishing process. The improved process adopted the flow of this invention, which involved first performing wet preprocessing, then DFG physical polishing, followed by wet reprocessing, and finally the final polishing process. To control variables, both groups of experiments used the same incoming material batch, the same polishing machine, the same type of grinding machine, the same inspection standards, and the same personnel or procedures for judgment. Except for the wet preprocessing, wet reprocessing, and corresponding parameters added in this invention, the subsequent polishing process, particle defect judgment standards, thickness judgment standards, and TTV judgment standards remained consistent.
[0217] The wet pretreatment conditions are as follows: the acidic mixed solution is prepared by mixing 49% HF, 70% HNO3, and 98% CH3COOH in a volume ratio of HF:HNO3:CH3COOH = 10L:62L:73L, the pH is controlled between 0 and 1, the processing temperature is 23℃, the treatment time is 3min, and the treatment endpoint is judged as the surface step difference being reduced to within the range of 20μm to 60μm and the residual film layer not being completely removed; after wet pretreatment, deionized water rinsing and nitrogen blowing are performed. The DFG physical grinding conditions were as follows: Z1 grinding surface: spindle speed 1000 rpm, total processing time 145 s, Air Cut removal 30 μm, P1 to P3 Cut removal 591 μm, feed rate 0.30 μm / s, spindle speed 20 rpm, Spark Out parameter 3 rev, Escape Cut removal 3 μm, feed rate 0.50 μm / s, spindle speed 20 rpm; Z2 grinding surface: spindle speed 1785 rpm, total processing time 157 s, Air Cut removal 20 μm, P1 to P3 Cut removal 581 μm, feed rate 0.20 μm / s, spindle speed 185 rpm, Spark Out parameter 5 rev, Escape Cut removal 2 μm, feed rate 0.30 μm / s, spindle speed 185 rpm; After DFG grinding, grinding debris cleaning, temperature equilibration, and drying were performed. The wet reprocessing conditions are: 48% NaOH alkaline solution (mass fraction), pH controlled between 12 and 14, circulation flow rate of 10 to 14 L / min, processing temperature of 80℃ ± 5℃, and processing time calculated as t2 = η × Dd / vNa, with a baseline of 1 min, adjusted according to the surface roughness after grinding, scratch condition, polishing particle feedback, and total corrosion amount. After wet reprocessing, deionized water rinsing and drying are performed. Both sets of silicon wafers enter the same post-polishing process.
[0218] The yield assessment standard uniformly adopts the quality assessment of reclaimed wafers after polishing. For example, a good product is defined as: a polished silicon wafer that meets the back-end flow specifications after particle defect detection, surface defect detection, thickness detection, TTV detection, and visual inspection, and has not experienced any scrapping due to defective particles, excessive thickness, residual surface film, or post-polishing defects caused by sharp damage. The yield calculation formula is: Yield = Number of good products / Total number of test samples × 100%. Under this assessment standard, a comparative input of 5000 wafers yielded 3678 good products, with a yield of 73.56%; after the improved process, an input of 5000 wafers yielded 4687 good products, with a yield of 93.74%, representing an improvement of 20.18 percentage points.
[0219] Whether a sample size of 5000 pieces is sufficient to rule out randomness can be explained from the perspective of statistical confidence level. For a binomial proportion estimate with proportion p and sample size n, its standard error can be approximately calculated as SE = sqrt(p(1-p) / n). When the comparative proportion p1 = 73.56% = 0.7356 and n1 = 5000, SE1 ≈ sqrt(0.7356 × 0.2644 / 5000) ≈ 0.00624; when the improved process p2 = 93.74% = 0.9374 and n2 = 5000, SE2 ≈ sqrt(0.9374 × 0.0626 / 5000) ≈ 0.00343. The yield difference between the two groups is 0.9374 - 0.7356 = 0.2018, and the standard error of the difference is SEdiff ≈ sqrt(SE1² + SE2²) ≈ 0.00712. Using an approximate 95% confidence interval, the lower confidence limit of the difference is approximately 0.2018 - 1.96 × 0.00712 ≈ 0.1878, and the upper confidence limit is approximately 0.2018 + 1.96 × 0.00712 ≈ 0.2158. This means the improved process increases the yield by approximately 18.78% to 21.58% compared to the original process. Further significance testing of the two proportions yields a z-value of approximately 0.2018 / 0.00712 ≈ 28.34, with a p-value much less than 0.05. This indicates that the yield difference between the two groups is not a random difference caused by small sample fluctuations and is statistically significant.
[0220] To avoid the inadequacy of a single statistical measure, this experiment can also employ a stratified statistical approach for verification: silicon wafers are divided into several intervals based on the initial step difference, such as below 50μm, 50μm to 80μm, 80μm to 120μm, and above 120μm; they are also divided into thin, medium, and thick layers based on the total film thickness; and high-silicon, high-nitride, and mixed layers are defined based on the relative proportion of nitride and polysilicon films. The yield of the comparative sample and the improved process are calculated for each layer. If the yield of the improved process in each layer is better than that of the comparative sample, and the overall difference is statistically significant, then random bias caused by inconsistent initial state distribution can be ruled out. If the sample size of a certain layer is small, the experimental batch can be extended or samples of the same specification can be combined for statistical analysis. For example, when the sample size of a single layer is less than 200 wafers, it is not advisable to draw strong conclusions alone; instead, multiple layers should be combined or data should be accumulated before making a judgment.
[0221] In addition, the chi-square test or Fisher's exact test can be used as supplementary statistical methods in this experiment. When any expected frequency in the four-fold table is less than 5, Fisher's exact test is preferred; when the sample size is large, the chi-square test can be used to compare the difference in the number of defective products between the control group and the improved process. In this embodiment, the number of defective products in the control group is 5000-3678=1322 pieces, and the number of defective products in the improved process is 5000-4687=313 pieces. The sample size is sufficient and the expected frequencies of each group are greater than 5, making the chi-square test suitable; the calculated difference is statistically significant. The above statistical methods are all commonly used in the field, and those skilled in the art can replicate and verify them based on the experimental records.
[0222] It should be noted that the above data are exemplary production test data used to illustrate the technical effects of the present invention, and should not be construed as limiting the scope of protection of the present invention to these specific values. Under other equivalent conditions, those skilled in the art can repeat the above tests based on actual incoming materials, equipment, and inspection standards. If used for actual mass production verification, it is recommended to record the initial step difference distribution, film thickness distribution, grouping method, process time, alkali concentration, grinding removal amount, polishing parameters, particle defect detection results, and good product judgment criteria for each batch of incoming materials to ensure traceability of test conditions. Through the above-mentioned standardized control of test conditions, grouping methods, judgment criteria, and statistical tests, the methods for obtaining the two sets of yield data of 73.56% and 93.74% and the basis for their technical effects can be clearly explained.
[0223] As can be seen from the above embodiments, the present invention, through three processes—wet pretreatment, DFG physical polishing, and wet retreatment—along with inter-process cleaning, drying, temperature balancing, quantified state determination, and parameter closed-loop feedback, can effectively remove dense composite films while avoiding the introduction of new surface damage, thus completing the regeneration process of silicon wafers with abnormal double-sided frosted texture. The surface morphology of the processed silicon wafer meets the requirements of the regeneration process and can be directly transferred to the subsequent polishing process for further regeneration. The composite process scheme of the embodiments of the present invention is particularly suitable for silicon wafers returned from fab production lines that have abnormal double-sided frosted texture and dense polycrystalline silicon or nitride composite films on their surfaces, effectively solving the technical problem that existing technologies struggle to process such abnormal silicon wafers using only physical polishing or wet processes.
[0224] The above embodiments are merely examples of the present invention. Any substitutions or combinations between embodiments made in accordance with the spirit of the present invention should be understood as not departing from the protection scope of the present invention.
Claims
1. A method for processing abnormal conditions on the double-sided frosted surface of a wafer regeneration wafer, characterized in that, For a to-be-regenerated silicon wafer with abnormal double-sided frosted texture surface state, three processes of wet pretreatment, DFG physical grinding, and wet reprocessing are sequentially performed, and at least one of cleaning, drying, temperature balancing and inter-process state judgment is arranged between adjacent processes; wherein, in the wet pretreatment process, an HF / HNO3 / CH3COOH acidic mixed chemical solution is used to perform selective partial etching on the silicon wafer, the partial etching does not take complete removal of the film layer as the processing end point, but aims to reduce the uneven undulation of the double-sided frosted texture surface and lower the step height between the multilayer films, and a residual composite film layer that can be removed by subsequent DFG physical grinding still remains on the surface of the silicon wafer after etching; in the DFG physical grinding process, a DFG grinding apparatus is used to perform double-sided physical grinding on the Z1 grinding surface and the Z2 grinding surface of the silicon wafer that has completed the wet pretreatment, the control unit of the DFG grinding apparatus separately determines the target etching depth and processing time of the wet pretreatment, the segmented removal amount and feed rate of the DFG physical grinding, and the lye treatment time of the wet reprocessing process according to the measured initial step difference S of the double-sided frosted texture, the total thickness Tf of the composite film layer, the nitride film thickness ratio Rn, the silicon wafer thickness Tpre before grinding, as well as the measured tank liquid temperature, pH and thickness values during the grinding process, in accordance with pre-designed calculation formulas and segmented mapping relationships; in the wet reprocessing process, NaOH lye is used for chemical etching and passivation of the silicon wafer that has completed DFG physical grinding and undergone grinding debris cleaning, so as to dissolve and remove the sharp damage layer introduced by DFG physical grinding, and obtain a silicon wafer that meets the requirements of the regeneration process.
2. The processing method according to claim 1, characterized in that, In the wet pretreatment process, the acidic mixed chemical solution is prepared by using 49% mass fraction HF, 70% mass fraction HNO3, and 98% mass fraction CH3COOH at a volume ratio of HF:HNO3:CH3COOH=10L:62L:73L, the pH of the chemical solution is controlled to be 0 to 1, the processing temperature is 23°C±1°C, and the reference processing time is 3min; the target etching depth is calculated according to D1=S-Ht, where Ht is the target residual step difference after the wet pretreatment is completed, Ht is 1 to 2 times the Air Cut removal amount in the subsequent DFG physical grinding process and is limited to 20μm to 60μm; the equivalent etching rate of the acidic mixed chemical solution to the composite film layer is calculated according to v=v0×(1-kn×Rn), where v0 is the measured etching rate of the polysilicon film at the reference temperature, kn is the deceleration coefficient caused by the density of the nitride film and 0<kn<1; the processing time of the wet pretreatment is calculated according to t1=D1 / v and constrained within the range of 1.5min to 5min, and is simultaneously constrained by D1≤Tf-Tr, where Tr is the required minimum thickness of the residual composite film layer to be retained and Tr≥5μm; after the processing is completed, the etching end point of the wet pretreatment process is defined as that the residual step difference on the silicon wafer surface falls within the range of 20μm to 60μm, residual film layer still exists on the surface, and the exposed area of the silicon substrate does not exceed 5% to 15%.
3. The processing method according to claim 1, characterized in that, After the completion of the wet pretreatment step and before the start of the DFG physical grinding step, the method further comprises subjecting the silicon wafer to deionized water rinsing and drying treatment, wherein the rinsing takes a pH value of 5 to 7 of the surface residual liquid as the acceptance criterion, and the drying enables the surface of the silicon wafer to reach a state free of water marks and ready for clamping; after the completion of the DFG physical grinding step and before the start of the wet reprocessing step, the method further comprises subjecting the silicon wafer to grinding debris cleaning and temperature balancing treatment, wherein the grinding debris cleaning is used to remove the grinding particles and grinding coolant remaining from the DFG physical grinding, and the temperature balancing treatment brings the surface temperature of the silicon wafer into the allowable feeding temperature range of the alkali solution in the wet reprocessing step.
4. The processing method according to claim 1, characterized in that, The DFG grinding apparatus comprises an apparatus body, a grinding spindle or a grinding disc, a workpiece holding mechanism, a rotary driving mechanism, a feed servo mechanism, a displacement encoder, a pressure sensor, a thickness detection unit, and a control unit; the control unit determines the total mechanical removal amount Dmech=Tpre-Tg according to the difference between the pre-grinding thickness and the target post-grinding thickness, where Tg is the sum of the finished product target thickness and the polishing process allowance, then distributes the total removal amount on both sides and determines the P1 to P3 Cut removal amounts of each grinding surface according to F=Dsurface-E-m, where E is the preset Escape Cut removal amount, and m is the allowance of 2 μm to 5 μm; for the Z1 grinding surface, the spindle rotation speed is 1000 rpm, the total processing time is 145 s, the Air Cut removal amount is set to 30 μm, the P1 to P3 Cut removal amount is set to 591 μm, the feed rate is 0.30 μm / s, the rotation speed is 20 rpm, the Spark Out parameter is 3 rev, the Escape Cut removal amount is 3 μm, and the feed rate is 0.50 μm / s; for the Z2 grinding surface, the spindle rotation speed is 1785 rpm, the total processing time is 157 s, the Air Cut removal amount is set to 20 μm, the P1 to P3 Cut removal amount is set to 581 μm, the feed rate is 0.20 μm / s, the rotation speed is 185 rpm, the Spark Out parameter is 5 rev, the Escape Cut removal amount is 2 μm, and the feed rate is 0.30 μm / s.
5. The processing method according to claim 4, characterized in that, The feed rate g and the Spark Out revolution number Nso are determined according to a piecewise mapping relationship based on the measured residual step difference S' after the wet pretreatment: when S'≤30 μm, g=0.20 μm / s; when 30 μm<S'≤50 μm, g=0.25 μm / s; when 50 μm<S'≤80 μm, g=0.30 μm / s; when S'>80 μm, g≤0.35 μm / s and Nso is 5 rev to 6 rev; the larger the residual step difference is, the lower the feed rate is and the larger the spark-out revolution number is; the switching between the Z1 grinding surface and the Z2 grinding surface is as follows: after the Z1 grinding stage reaches the preset intermediate state, the control unit controls the feed servo shaft to retract to separate the Z1 grinding surface from the silicon wafer or reduce the rotation speed, then transfers the silicon wafer to the Z2 grinding station through a turnover mechanism, a manipulator transfer mechanism, a turntable transposition mechanism or a double-sided grinding station surface switching structure, so that the second surface of the silicon wafer is in contact with the Z2 grinding surface and processed according to the Z2 grinding program.
6. The processing method according to claim 4, characterized in that, The grinding endpoint of the DFG physical grinding process is determined by the criterion that the silicon wafer thickness Tpost after grinding falls within the ±δ tolerance range of the target post-grinding thickness Tg, where δ is preferably ±3μm; when Tpost>Tg+δ, it is determined that the removal amount is insufficient, supplementary grinding is performed with a single supplementary grinding removal amount ΔF=Tpost-Tg and ΔF≤10μm, and re-inspection is carried out after supplementary grinding; when Tpost<Tg-δ, it is determined that over-grinding occurs, rework assessment is performed on the ground silicon wafer, and the P1 to P3 Cut removal amount F and the Escape Cut removal amount E of subsequent silicon wafers in the same batch are synchronously reduced; during the grinding process, at least one of the cumulative removal amount in each cutting stage reaching the set value, the feed servo axis displacement reaching the position, the grinding pressure being stable, and the spindle current or power entering the stable interval is taken as the stage switching criterion.
7. The processing method according to claim 1, characterized in that, The wet reprocessing step uses a 48% NaOH alkaline solution, with the pH controlled at 12 to 14, a circulation flow rate of 10 to 14 L / min, and a processing temperature of 80℃ ± 5℃; the treatment time t2 of the alkaline solution is calculated as t2 = η × Dd / v Na The calculation determines that Dd is the estimated depth of the grinding damage layer formed on the silicon wafer surface by the DFG physical grinding process, vNa is the equivalent corrosion rate of the damage layer by NaOH alkaline solution under the current bath conditions, and η is the complete dissolution margin coefficient, which is taken as 1.1 to 1.3; Dd is calculated as Dd = a0 + a1 × g + a2 × F + a3 × (1 / Nso), where g is the feed rate of the P1 to P3 Cut stage, F is the removal amount of the P1 to P3 Cut, Nso is the Spark Out revolutions, a0 is the basic term, and a0 to a3 are the calibration coefficients obtained by multiple linear regression after the test wafer under the same conditions is ground by an orthogonal combination of feed rate, removal amount and Spark Out revolution gradient; vNa is the equivalent corrosion rate of the damage layer by NaOH alkaline solution under the current bath conditions, and η is the complete dissolution margin coefficient, which is taken as 1.1 to 1.3; Na according to Calculate, where v N Q is the baseline corrosion rate measured at 80℃, 48% mass fraction, and pH 13. 10 Take 2.0 to 2.3, where T is the online measured temperature of the bath solution; the calculated processing time is constrained to the range of 30s to 2min, where 30s is the minimum process dwell time to ensure the transfer of liquid inlet and outlet and the full replacement of surface solution, and 2min is the upper limit of time to avoid excessive anisotropic corrosion of silicon substrate by alkaline solution.
8. The processing method according to claim 7, characterized in that, Whether the sharp damage layer is completely dissolved is judged according to the following criteria: after wet reprocessing, when the arithmetic mean roughness Ra of the silicon wafer surface is ≤0.3μm and there are no directional grinding streaks, it is determined that the damage layer has been dissolved; when 0.3μm<Ra≤0.6μm, a short-cycle supplementary etching of 5s to 20s is performed before re-measurement; when Ra>0.6μm, it is determined that the damage layer has not been dissolved, and the process returns to the DFG physical grinding process to increase the Spark Out rotation speed or increase the Escape Cut removal amount; and / or the sampled thickness difference D2 before and after the lye treatment is compared with the target dissolution amount η×Dd, and it is determined to be up to standard when D2 falls within the ±20% range of η×Dd; when the Dd of the Z1 grinding surface and the Z2 grinding surface of the same silicon wafer are inconsistent, the reference processing time is determined according to the larger Dd of the two sides, and the side with shallower damage is shortened by 5s to 15s or the circulating flow facing it is reduced; when Dd≥2.5μm, the processing time is extended to 1.2min to 2min, and feedback is sent to the DFG physical grinding process to increase the Spark Out rotation speed by 1rev or increase the Escape Cut removal amount to 3μm to 4μm for subsequent silicon wafers in the same batch.
9. The processing method according to claim 7, characterized in that, The control unit verifies the measured chemical corrosion amount D1 of the wet pretreatment while determining the processing times t1 and t2. meas The sum of the amount of alkali removed, D2, satisfies D1. meas +D2≤12μm; if not met, t2 is calculated back according to the upper limit of the chemical corrosion budget and the removal amount of P1 to P3 Cut in the DFG physical polishing process is reduced accordingly. If still not met, the batch of silicon wafers is marked for full inspection. After the entire set of combined processes is completed, the silicon wafers can be directly transferred to the back-end polishing process. The by-products generated by the chemical reaction in each step are all water-soluble substances.
10. The processing method according to any one of claims 1 to 9, characterized in that, A closed-loop parameter feedback is formed between the wet pretreatment process, the DFG physical polishing process, and the wet reprocessing process: The removal amount, Escape Cut removal amount, or wet reprocessing time of the DFG physical polishing process is adjusted based on at least one of the measured residual step difference, film residue state, and exposed silicon substrate area after wet pretreatment; the estimated depth of the polishing damage layer is calculated based on at least one of the thickness, surface step difference, feed rate, removal amount, and Spark Out revolutions after DFG physical polishing, and the treatment time or number of etching cycles of the NaOH alkaline solution is adjusted accordingly; the surface roughness after wet reprocessing and the particle defect rate after polishing are used as the basis for process release and parameter correction; the control unit also... Update v0, kn, a0 to a3, vN, and η, where λ is between 0.1 and 0.
3. When the defect rate of polishing particles in multiple consecutive batches exceeds the set threshold, automatically increase η or increase the Spark Out revolutions and trigger manual confirmation.
Citation Information
Patent Citations
Back polishing roller suitable for large silicon wafer
CN210866225U