A method of manufacturing a semiconductor device
By forming a conformal layer, a stop layer, and a HARP oxide layer during the semiconductor device fabrication process, and employing specific chemical mechanical polishing (CMP) steps, the problem of reduced semiconductor device reliability caused by CMP is solved, a smoother polished surface is achieved, metal residue is reduced, and device reliability is improved.
Patent Information
- Application Number
- CN202510623101.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2026-11-20
AI Technical Summary
The reliability degradation of semiconductor devices caused by chemical mechanical polishing (CMP) in the prior art is mainly due to the difference in polishing rate of film layers of different materials, which causes grooves to form in the softer material, thus affecting the reliability of the device.
In the semiconductor device fabrication process, a conformal layer, a first HARP oxide layer, a stop layer and a second HARP oxide layer are formed. Specific chemical mechanical polishing steps are adopted, including a first chemical mechanical polishing process that stops at a first stop portion, then etchs back to a second stop portion, and a second chemical mechanical polishing is performed to expose the top surface of the raised structure. The etching rate ratio of each layer is controlled to be 1:1 to gradually improve the surface flatness.
It improves the problem of inconsistent residual film height caused by CMP, reduces the risk of metal residue, and improves device reliability.
Smart Images

Figure CN123146155A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor technology and relates to a method for fabricating a semiconductor device. Background Technology
[0002] Chemical mechanical polishing (CMP) typically requires polishing a variety of different materials. However, due to the different polishing rates of the film layers on different materials, grooves often form in the softer material areas, leading to various reliability risks.
[0003] For example, please refer to Figures 1 to 4 The diagram shows the structural diagrams corresponding to each step in a semiconductor manufacturing process involving chemical mechanical polishing:
[0004] (1) As Figure 1 As shown, a TEOS layer 102 (TEOS is a tetraethoxysilane, an organosilicon compound, or a special type of silicon dioxide) is deposited on a silicon substrate 100 having a polycrystalline silicon bump structure 101.
[0005] (2) Figure 2 As shown, chemical mechanical polishing is performed to expose the top surface of the polycrystalline silicon bump structure 101. Since the TEOS material is softer than the polycrystalline silicon material, after CMP, a groove 103 will appear on the top surface of the TEOS layer 102 between adjacent polycrystalline silicon bump structures 101.
[0006] (3) Figure 3 As shown, a metal layer 104 is deposited to fill a specific area (not shown);
[0007] (4) Figure 4 As shown, chemical mechanical polishing is performed to remove excess metal layer 104. Due to the presence of groove 103 on the surface of TEOS layer 102, some metal will remain in the groove 103 to form metal residue 105. These metal residues 105 will bring defect risks and affect device reliability.
[0008] Therefore, how to provide a process method for improving CMP uniformity and a method for fabricating semiconductor devices to enhance device reliability has become an important technical problem that urgently needs to be solved by those skilled in the art.
[0009] It should be noted that the above introduction to the technical background is only for the purpose of providing a clear and complete explanation of the technical solutions of this application and facilitating understanding by those skilled in the art. It should not be assumed that these technical solutions are known to those skilled in the art simply because they have been described in the background section of this application. Summary of the Invention
[0010] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a method for fabricating semiconductor devices to solve the problem of reduced device reliability caused by poor CMP uniformity in the prior art.
[0011] To achieve the above and other related objectives, the present invention provides a method for fabricating a semiconductor device, comprising the following steps:
[0012] A substrate is provided, a protrusion structure is formed on the substrate, and a conformal layer covering the protrusion structure is formed on the substrate;
[0013] A first HARP oxide layer is formed on the surface of the conformal layer. The first HARP oxide layer includes a mound-shaped portion located above the protruding structure and flat portions located on both sides of the mound-shaped portion. The top surface of the flat portions is higher than the top surface of the conformal layer above the top surface of the protruding structure.
[0014] A stop layer is formed on the surface of the first HARP oxide layer, the stop layer comprising a first stop portion located on the surface of the mound portion and a second stop portion located on the surface of the flat portion;
[0015] A second HARP oxide layer is formed on the surface of the stop layer;
[0016] The first chemical mechanical polishing process is performed and stopped at the top of the first stopping part;
[0017] The second HARP oxide layer and the stop layer are etched back and stopped at the second stop portion. During the etch back process, the etching rate ratio of the second HARP oxide layer to the stop layer is 1:1.
[0018] A second chemical mechanical polishing process is performed to expose the top surface of the raised structure.
[0019] Optionally, the second chemical mechanical polishing process includes:
[0020] First polishing stage: Chemical mechanical polishing is performed on the second stop portion and the exposed first HARP oxide layer. The wear rate of the first HARP oxide layer is faster than the wear rate of the second stop portion. A first recessed portion is obtained above the protruding structure on the surface of the first HARP oxide layer.
[0021] Second polishing stage: Continue chemical mechanical polishing to expose the flat portion of the first HARP oxide layer and expose the conformal layer on the bottom surface of the first recessed portion, at which point the top surface of the flat portion is higher than the top surface of the first recessed portion.
[0022] Third polishing stage: Continue chemical mechanical polishing until the top surface of the protruding structure is exposed, the first HARP oxide layer is worn faster than the conformal layer.
[0023] Optionally, at the end of the third polishing stage, the lowest point of the top surface of the first HARP oxide layer on both sides of the protrusion structure is not lower than the top surface of the protrusion structure.
[0024] Optionally, at the end of the third polishing stage, the lowest point of the top surface of the first HARP oxide layer on both sides of the protrusion structure is lower than the top surface of the protrusion structure, and the height difference between the lowest point of the top surface of the first HARP oxide layer on both sides of the protrusion structure and the top surface of the protrusion structure is less than 5 nm.
[0025] Optionally, the stop layer includes a silicon nitride layer.
[0026] Optionally, the conformal layer includes a silicon oxide layer, and the density of the conformal layer is higher than that of the first HARP oxide layer.
[0027] Optionally, the bump structure includes a polysilicon-replaced gate.
[0028] Optionally, the protrusion structure may further include a protective layer located on the top surface of the polysilicon replacement gate.
[0029] Optionally, the protective layer includes a silicon nitride layer.
[0030] Optionally, the following steps are also included:
[0031] Remove the polysilicon to replace the gate to obtain a gate trench;
[0032] Deposit metallic gate material to fill the gate trench;
[0033] Chemical mechanical polishing is performed to remove the metal gate material outside the gate trench, resulting in a metal gate located in the gate trench.
[0034] As described above, the semiconductor device fabrication method of the present invention, after forming a bump structure on a substrate, sequentially forms a conformal layer, a first HARP oxide layer, a stop layer, and a second HARP oxide layer. The first HARP oxide layer includes a mound-like portion above the bump structure and flat portions on both sides of the mound-like portion. The top surface of the flat portions is higher than the top surface of the conformal layer above the top surface of the bump structure. The stop layer includes a first stop portion on the surface of the mound-like portion and a second stop portion on the surface of the flat portions. A first chemical mechanical polishing (CMP) process is then performed, stopping at the top of the first stop portion. The second HARP oxide layer and the stop layer are then etched back, stopping at the second stop portion. During the etch-back process, the etching rate ratio of the second HARP oxide layer to the stop layer is 1:1. Finally, a second CMP process is performed to expose the top surface of the bump structure. The semiconductor device fabrication method of the present invention can obtain a smoother polished surface, improving the problem of inconsistent residual film height caused by CMP, thereby reducing the risk of metal residue in subsequent processes and improving device reliability. Attached Figure Description
[0035] Figure 1 The diagram shows a structure obtained after depositing a TEOS layer on a silicon substrate with a polycrystalline silicon bump structure in a semiconductor manufacturing process involving chemical mechanical polishing.
[0036] Figure 2 The diagram shows a structure obtained after chemical mechanical polishing in a semiconductor manufacturing process involving chemical mechanical polishing to expose the top surface of a polycrystalline silicon bump structure.
[0037] Figure 3 The diagram shows a structure obtained after depositing a metal layer in a semiconductor manufacturing process involving chemical mechanical polishing.
[0038] Figure 4 The diagram shows a structure obtained after chemical mechanical polishing to remove excess metal layers in a semiconductor manufacturing process involving chemical mechanical polishing.
[0039] Figure 5 The diagram shown is a process flow chart of the method for fabricating the semiconductor device of the present invention.
[0040] Figure 6 The diagram shown illustrates the structure obtained after forming the protrusion structure and the conformal layer in the semiconductor device fabrication method of the present invention.
[0041] Figure 7 The diagram shows the structure obtained after forming the first HARP oxide layer according to the semiconductor device fabrication method of the present invention.
[0042] Figure 8The diagram shown is a schematic representation of the structure obtained after forming a stop layer in the semiconductor device fabrication method of the present invention.
[0043] Figure 9 The diagram shown illustrates the structure obtained after forming the second HARP oxide layer according to the semiconductor device fabrication method of the present invention.
[0044] Figure 10 The diagram shows the structure obtained after the first chemical mechanical polishing process of the semiconductor device fabrication method of the present invention.
[0045] Figure 11 The diagram shown illustrates the structure obtained after etching back the second HARP oxide layer and the stop layer, as per the semiconductor device fabrication method of the present invention.
[0046] Figure 12 The diagram shows the structure obtained after the first polishing stage of the second chemical mechanical polishing process in the semiconductor device fabrication method of the present invention.
[0047] Figure 13 The diagram shows the structure obtained after the second polishing stage of the second chemical mechanical polishing process in the semiconductor device fabrication method of the present invention.
[0048] Figure 14 The diagram shows the structure obtained after the third polishing stage of the second chemical mechanical polishing process in the semiconductor device fabrication method of the present invention.
[0049] Explanation of reference numerals in the attached figures
[0050] 100 Silicon substrate
[0051] 101 Polycrystalline silicon bump structure
[0052] 102 TEOS layer
[0053] 103 Grooves
[0054] 104 Metal Layer
[0055] 105 Metal Residue
[0056] Steps S1 to S7
[0057] 201 substrate
[0058] 202 Protruding Structure
[0059] 2021 Polysilicon Replacement Gate
[0060] 2022 Protective Layer
[0061] 203 Conformal Layer
[0062] 204 First HARP Oxide Layer
[0063] 2041 Hill-like region
[0064] 2042 Flat section
[0065] 205 Stop Layer
[0066] 2051 First Stop Section
[0067] 2052 Second Stop Section
[0068] 206 Second HARP Oxide Layer
[0069] 207 Depression Detailed Implementation
[0070] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0071] It should be emphasized that the term "including / comprises" as used herein refers to the presence of a feature, whole, step, or component, but does not exclude the presence or addition of one or more other features, wholes, steps, or components.
[0072] Features described and / or illustrated for one embodiment may be used in the same or similar manner in one or more other embodiments, combined with features in other embodiments, or substituted for features in other embodiments.
[0073] In the detailed description of embodiments of the present invention, for ease of explanation, the schematic diagrams illustrating the device structure may be partially enlarged without adhering to the general scale, and the schematic diagrams are merely examples and should not limit the scope of protection of the present invention. Furthermore, in actual manufacturing, the three-dimensional spatial dimensions of length, width, and depth should be included.
[0074] For ease of description, spatial relation terms such as “below,” “under,” “lower than,” “below,” “above,” and “upper” may be used herein to describe the relationship between one element or feature shown in the accompanying drawings and other elements or features. It will be understood that these spatial relation terms are intended to include directions other than those depicted in the drawings for devices in use or operation. Furthermore, when a layer is referred to as being “between” two layers, it may be the only layer between the two layers, or there may be one or more layers in between.
[0075] In the context of this application, the structure described above the first feature may include embodiments in which the first and second features are in direct contact, or embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.
[0076] It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the illustrations only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0077] This invention provides a method for fabricating a semiconductor device. Please refer to [link / reference]. Figure 5 The diagram shows the process flow of this method, which includes the following steps:
[0078] S1: A substrate is provided, a protrusion structure is formed on the substrate, and a conformal layer covering the protrusion structure is formed on the substrate;
[0079] S2: A first HARP oxide layer is formed on the surface of the conformal layer. The first HARP oxide layer includes a mound-shaped portion located above the protruding structure and a flat portion located on both sides of the mound-shaped portion. The top surface of the flat portion is higher than the top surface of the conformal layer above the top surface of the protruding structure.
[0080] S3: A stop layer is formed on the surface of the first HARP oxide layer, the stop layer including a first stop portion located on the surface of the mound portion and a second stop portion located on the surface of the flat portion;
[0081] S4: Form a second HARP oxide layer on the surface of the stop layer;
[0082] S5: Perform the first chemical mechanical polishing process and stop at the top of the first stopping part;
[0083] S6: The second HARP oxide layer and the stop layer are etched back and stopped at the second stop portion. During the etch back process, the etching rate ratio of the second HARP oxide layer to the stop layer is 1:1.
[0084] S7: Perform a second chemical mechanical polishing process to expose the top surface of the raised structure.
[0085] The following section details each of the above steps in conjunction with the structural diagram.
[0086] Please refer to the following first. Figure 6Perform step S1: Provide a substrate 201, form a protrusion structure 202 on the substrate 201, and form a conformal layer 203 covering the protrusion structure 202 on the substrate 201.
[0087] In some embodiments, the bump structure 202 includes a polysilicon replacement gate 2021 for subsequent replacement with a metal gate.
[0088] In some embodiments, the protrusion structure 202 further includes a protective layer 2022 located on the top surface of the polysilicon replacement gate 2021, the protective layer 2022 may include, for example, a silicon nitride layer.
[0089] It should be noted that, in other embodiments, the protrusion structure 202 may also be any other suitable structure, not limited to polysilicon-replaced gate.
[0090] Specifically, the conformal layer 203 conformally covers the surface of the substrate 201 and the surface of the protrusion structure 202. The thickness of the conformal layer 203 is less than the thickness of the protrusion structure 202, thereby forming recessed areas on both sides of the protrusion structure 202.
[0091] Specifically, the portion of the conformal layer 203 located on the sidewall of the protrusion structure 202 constitutes a sidewall. In embodiments where the protrusion structure 202 includes the polysilicon replacement gate 2021, the sidewall will be used subsequently to limit the gate trench.
[0092] In some embodiments, the conformal layer 203 includes a silicon oxide layer, such as a silicon oxide layer deposited using high-density plasma chemical vapor deposition (HDP-CVD) with relatively high density.
[0093] Please see again Figure 7 Step S2 is performed: a first HARP oxide layer 204 is formed on the surface of the conformal layer 203. The first HARP oxide layer 204 includes a mound portion 2041 located above the protruding structure 202 and a flat portion 2042 located on both sides of the mound portion 2041. The top surface of the flat portion 2042 is higher than the top surface of the conformal layer 203 above the top surface of the protruding structure 202.
[0094] Specifically, the High Aspect Ratio Process (HARP) uses a thermochemical reaction of ozone (O3) and tetraethoxysilane (TEOS) to form an oxide film, i.e., a HARP film. This process does not involve the use of plasma, thus avoiding damage to the semiconductor structure or substrate caused by plasma. Furthermore, the recessed regions on both sides of the protrusion structure 202 have a high aspect ratio, and the HARP process can effectively fill these high aspect ratio structural gaps and provide a pore-free thin film.
[0095] Specifically, the density of the conformal layer 203 is higher than that of the first HARP oxide layer 203.
[0096] Please see again Figure 8 Step S3 is performed: a stop layer 205 is formed on the surface of the first HARP oxide layer 204. The stop layer 205 includes a first stop portion 2051 located on the surface of the mound portion 2041 and a second stop portion 2052 located on the surface of the flat portion 2042.
[0097] Specifically, the stop portion 205 serves as a stop layer for subsequent chemical mechanical polishing processes.
[0098] In some embodiments, the stop layer 205 includes a silicon nitride layer, which can be formed on the surface of the first HARP oxide layer 204 by chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD) or other suitable methods.
[0099] Please see again Figure 9 Step S4 is performed: a second HARP oxide layer 206 is formed on the surface of the stop layer 205.
[0100] Specifically, the second HARP oxide layer 206 and the first HARP oxide layer 204 may be deposited under the same or substantially the same conditions.
[0101] Specifically, the thickness of the second HARP oxide layer 206 must satisfy the requirement that the lowest point of its surface is higher than the highest point of the surface of the stop layer 205.
[0102] Thus, a composite layer consisting of the first HARP oxide layer 204, the stop layer 205, and the second HARP oxide layer 206 is obtained on the substrate 201.
[0103] Please see again Figure 10 Execute step S5: Perform the first chemical mechanical polishing process and stop at the top of the first stop part 2051.
[0104] Specifically, at the end of the first chemical mechanical polishing process, the portion of the stop layer 205 located on the surface of the flat portion 2042 of the first HARP oxide layer 204 (i.e., the second stop portion 2052) still has an oxide layer of a certain thickness (i.e., the second HARP oxide layer 206), while the top of the portion of the stop layer 205 located on the surface of the mound portion 2041 of the first HARP oxide layer 204 (i.e., the first stop portion 2051) is exposed.
[0105] Please see again Figure 11 Step S6 is executed: the second HARP oxide layer 206 and the stop layer 205 are etched back and stopped at the second stop portion 2052. During the etch-back process, the etching rate ratio of the second HARP oxide layer 206 to the stop layer 205 is 1:1.
[0106] Specifically, the second HARP oxide layer 206 and the stop layer 205 can be etched back using dry etching, wet etching, or a combination thereof. By controlling the etching conditions, the etching rate ratio of the second HARP oxide layer 206 to the stop layer 205 is 1:1, so that the polished surface is basically flat when the etching is finished.
[0107] Please see again Figures 12 to 14 Then, perform step S7: perform a second chemical mechanical polishing process to expose the top surface of the protrusion structure 202.
[0108] As an example, the second chemical mechanical polishing process includes:
[0109] (1) First polishing stage: such as Figure 12 As shown, the second stop portion 2052 and the exposed first HARP oxide layer 204 are subjected to chemical mechanical polishing. The wear rate of the first HARP oxide layer 204 is faster than that of the second stop portion 2052. A first recess portion 207 is obtained above the protrusion structure 202 on the surface of the first HARP oxide layer 204.
[0110] (2) Second polishing stage: such as Figure 13 As shown, chemical mechanical polishing is continued to expose the flat portion 2042 of the first HARP oxide layer 204 and to expose the conformal layer 203 on the bottom surface of the first recessed portion 207. At this time, the top surface of the flat portion 2042 is higher than the top surface of the first recessed portion 207.
[0111] (3) Third polishing stage: such as Figure 14As shown, chemical mechanical polishing continues until the top surface of the protrusion structure 202 is exposed. The first HARP oxide layer 204 wears out faster than the conformal layer 203.
[0112] Specifically, in the first polishing stage, the first HARP oxide layer 204 is polished faster, while the second stop portion 2052 is polished slower. For example, when the second stop portion 2052 is made of silicon nitride, silicon nitride is harder and polishes slower, while the HARP deposited oxide layer is softer and wears out faster. As a result, during the polishing process, a concave shape will gradually form above the protruding structure 202, namely the first recessed portion 207.
[0113] Specifically, in the second polishing stage, since the first HARP oxide layer 204 is polished faster and the second stop portion 2052 is polished slower, the first recess 207 will gradually deepen and touch the conformal layer 203 on the top of the protrusion structure 202 more quickly. When the second stop portion 2052 is polished, the top surface of the first HARP oxide layer 204 on both sides of the protrusion structure 202 is higher than the top surface of the conformal layer 203 exposed on the top of the protrusion structure 202.
[0114] Specifically, in the third polishing stage, the grinding speed of the conformal layer 203 at the top of the protrusion structure 202 is slower, while the grinding speed of the first HARP oxide layer 204 on both sides of the protrusion structure 202 is faster. During the grinding process, the height difference will gradually decrease, and when the grinding stops, the height difference will be leveled, resulting in a smoother grinding surface. This can improve the problem of inconsistent height of the remaining film layer caused by CMP.
[0115] In some embodiments, at the end of the third polishing stage, the lowest point of the top surface of the first HARP oxide layer 204 on both sides of the protrusion structure 202 is not lower than the top surface of the protrusion structure 202.
[0116] In other embodiments, at the end of the third polishing stage, the lowest point of the top surface of the first HARP oxide layer 204 on both sides of the protrusion structure 202 may also be lower than the top surface of the protrusion structure 202. However, the height difference between the lowest point of the top surface of the first HARP oxide layer 204 on both sides of the protrusion structure 202 and the top surface of the protrusion structure 202 is less than 5nm, for example less than 4nm, 3nm or 2nm. Such a height difference makes it less likely for metal to remain in subsequent processes.
[0117] In some embodiments, when the bump structure 202 includes the polysilicon replacement gate 2021 and the structure to be fabricated includes a metal gate, the following steps are further included after performing the second chemical mechanical polishing process:
[0118] (1) Remove the polysilicon replacement gate 2021 to obtain a gate trench;
[0119] (2) Deposit metal gate material to fill the gate trench;
[0120] (3) Perform chemical mechanical polishing to remove the metal gate material outside the gate trench to obtain a metal gate located in the gate trench.
[0121] As an example, the polysilicon replacement gate 2021 can be removed using wet etching, dry etching, a combination thereof, or other suitable methods. For instance, in some embodiments, a mixture of HBr and O2 is used to dry-etch the polysilicon to remove the replacement gate 2021, wherein silicon reacts with bromine to generate a weakly volatile silicon bromide byproduct, thereby achieving a high polysilicon-to-silicon oxide selectivity. In other embodiments, CF4 or NF3 is used as the etching gas. In still other embodiments, a chemical solution such as tetramethylammonium hydroxide (TMAH) is used to wet-etch the polysilicon to remove the replacement gate 2021.
[0122] As an example, the metal grid material includes Al or other suitable materials.
[0123] Thus, a semiconductor device is obtained. Because the semiconductor device fabrication method of the present invention improves the surface uniformity of the dielectric layer after CMP, the structural surface before the deposition of metal material (e.g., but not limited to metal gate material) is relatively flat. After the subsequent deposition of metal material is chemically and mechanically polished to remove the metal material outside the trench (e.g., but not limited to gate trench), there is less metal residue on the dielectric surface outside the trench.
[0124] In summary, the semiconductor device fabrication method of the present invention, after forming a protrusion structure on a substrate, sequentially forms a conformal layer, a first HARP oxide layer, a stop layer, and a second HARP oxide layer. The first HARP oxide layer includes a mound-like portion above the protrusion structure and flat portions on both sides of the mound-like portion. The top surface of the flat portions is higher than the top surface of the conformal layer above the top surface of the protrusion structure. The stop layer includes a first stop portion on the surface of the mound-like portion and a second stop portion on the surface of the flat portions. A first chemical mechanical polishing (CMP) process is then performed, stopping at the top of the first stop portion. The second HARP oxide layer and the stop layer are then etched back, stopping at the second stop portion. During the etch-back process, the etching rate ratio of the second HARP oxide layer to the stop layer is 1:1. Finally, a second CMP process is performed to expose the top surface of the protrusion structure. The semiconductor device fabrication method of the present invention can obtain a smoother polished surface, improving the problem of inconsistent residual film height caused by CMP, thereby reducing the risk of metal residue in subsequent processes and improving device reliability. Therefore, the present invention effectively overcomes the various shortcomings of the prior art and has high industrial applicability.
[0125] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A method for fabricating a semiconductor device, characterized in that, Includes the following steps: A substrate is provided, a protrusion structure is formed on the substrate, and a conformal layer covering the protrusion structure is formed on the substrate; A first HARP oxide layer is formed on the surface of the conformal layer. The first HARP oxide layer includes a mound-shaped portion located above the protruding structure and flat portions located on both sides of the mound-shaped portion. The top surface of the flat portions is higher than the top surface of the conformal layer above the top surface of the protruding structure. A stop layer is formed on the surface of the first HARP oxide layer, the stop layer comprising a first stop portion located on the surface of the mound portion and a second stop portion located on the surface of the flat portion; A second HARP oxide layer is formed on the surface of the stop layer; The first chemical mechanical polishing process is performed and stopped at the top of the first stopping part; The second HARP oxide layer and the stop layer are etched back and stopped at the second stop portion. During the etch back process, the etching rate ratio of the second HARP oxide layer to the stop layer is 1:
1. A second chemical mechanical polishing process is performed to expose the top surface of the raised structure.
2. The method for fabricating a semiconductor device according to claim 1, characterized in that, The second chemical mechanical polishing process includes: First polishing stage: Chemical mechanical polishing is performed on the second stop portion and the exposed first HARP oxide layer. The wear rate of the first HARP oxide layer is faster than the wear rate of the second stop portion. A first recessed portion is obtained above the protruding structure on the surface of the first HARP oxide layer. Second polishing stage: Continue chemical mechanical polishing to expose the flat portion of the first HARP oxide layer and expose the conformal layer on the bottom surface of the first recessed portion, at which point the top surface of the flat portion is higher than the top surface of the first recessed portion. Third polishing stage: Continue chemical mechanical polishing until the top surface of the protruding structure is exposed, the first HARP oxide layer is worn faster than the conformal layer.
3. The method for fabricating a semiconductor device according to claim 2, characterized in that: At the end of the third polishing stage, the lowest point of the top surface of the first HARP oxide layer on both sides of the protrusion structure is not lower than the top surface of the protrusion structure.
4. The method for fabricating a semiconductor device according to claim 2, characterized in that: At the end of the third polishing stage, the lowest point of the top surface of the first HARP oxide layer on both sides of the protrusion structure is lower than the top surface of the protrusion structure, and the height difference between the lowest point of the top surface of the first HARP oxide layer on both sides of the protrusion structure and the top surface of the protrusion structure is less than 5 nm.
5. The method for fabricating a semiconductor device according to claim 1, characterized in that: The stop layer includes a silicon nitride layer.
6. The method for fabricating a semiconductor device according to claim 1, characterized in that: The conformal layer includes a silicon oxide layer, and the density of the conformal layer is higher than that of the first HARP oxide layer.
7. The method for fabricating a semiconductor device according to claim 1, characterized in that: The protrusion structure includes a polysilicon replacement gate.
8. The method for fabricating a semiconductor device according to claim 7, characterized in that: The protrusion structure also includes a protective layer located on the top surface of the polysilicon replacement gate.
9. The method for fabricating a semiconductor device according to claim 8, characterized in that: The protective layer includes a silicon nitride layer.
10. The method for fabricating a semiconductor device according to claim 7 or 8, characterized in that, It also includes the following steps: Remove the polysilicon to replace the gate to obtain a gate trench; Deposit metallic gate material to fill the gate trench; Chemical mechanical polishing is performed to remove the metal gate material outside the gate trench, resulting in a metal gate located in the gate trench.