Multi-temperature-zone graphene integrated electrostatic chuck and preparation method and application thereof

By printing multi-temperature zone heating electrodes on the electrostatic chuck and combining them with a graphene coating, the problem of temperature uniformity in highly integrated processes of electrostatic chucks was solved, achieving efficient temperature control and improved yield.

CN123146181APending Publication Date: 2026-11-20NINGBO JINGPAN ELECTRONIC MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611278618.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing electrostatic chucks have difficulty ensuring temperature uniformity in highly integrated and advanced processes. In particular, in multi-temperature zone designs, traditional methods lead to uneven internal stress distribution and enhanced thermal coupling, which affects product yield.

Method used

The preparation method of multi-temperature zone graphene integrated electrostatic chuck involves printing multi-temperature zone heating electrodes on alumina green ceramic sheet and printing a partitioned graphene coating on top of them. By utilizing the ultra-high thermal conductivity and uniform temperature characteristics of graphene, thermal crosstalk can be avoided, and extreme temperature uniformity can be achieved with a small number of temperature zones.

Benefits of technology

It achieves a wafer surface temperature non-uniformity as low as 1.6℃, surpassing the uniformity effect of densely heated temperature zones, thus improving the accuracy of temperature control and product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146181A_ABST
    Figure CN123146181A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of semiconductor manufacturing equipment, and relates to a multi-temperature-zone graphene integrated electrostatic chuck and a preparation method and application thereof. A multi-temperature-zone heating electrode with a temperature greater than or equal to 37 is integrated with a graphene partition, the in-plane super-high thermal conductivity and the uniform temperature characteristics of the graphene can be utilized to quickly smooth the local temperature difference caused by the annular heating electrode, the extreme temperature uniformity that needs to be achieved by using intensive heating temperature zones is broken, and the system only needs a relatively small number of temperature zones to achieve or even exceed the uniform temperature effect that needs to be achieved by using intensive temperature zones.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of semiconductor manufacturing equipment technology, and relates to a multi-temperature zone graphene integrated electrostatic chuck, its preparation method and application. Background Technology

[0002] Electrostatic chucks play an important role in semiconductor manufacturing processes, especially in core processes such as ion etching, ion implantation, physical vapor deposition, and chemical vapor deposition.

[0003] The ceramic structure of an electrostatic chuck mainly consists of a dielectric layer, an internal electrode layer, an internal heating layer, and a substrate layer. The core function of the internal electrode layer is to actively generate heat through the Joule heating effect, precisely controlling the wafer temperature to meet the specific temperature window requirements of processes such as etching and deposition. Traditional single-temperature zone designs can only provide a global heating temperature, making it difficult to ensure temperature uniformity on the wafer surface when facing challenges such as plasma bombardment and heat loss at the wafer edges. As integrated circuit process nodes evolve towards 7nm and below, the requirements for wafer surface temperature uniformity are extremely high. The number of temperature control zones has increased from the early 2 or 4 zones to more than 37 or even over 100 zones. However, precisely arranging 100 independent and mutually insulated heating circuits, sensor traces, and hundreds of corresponding leads within a ceramic substrate with a diameter of only 300mm means that the electrode pattern is extremely complex, exacerbating the problem of uneven internal stress distribution. Furthermore, when the heater density is too high, the thermal coupling between regions increases dramatically, leading to a significant decrease in product yield and an exponential increase in manufacturing difficulty.

[0004] Existing technologies have incorporated graphene to improve the structure of electrostatic chucks. CN221486472U discloses a heating electrostatic chuck mechanism that uses a graphite diffusion disk between the ceramic electrostatic chuck and an external single-temperature zone tungsten filament heating disk. This allows the heat from the tungsten filament to be evenly distributed across the electrostatic chuck, preventing uneven heating. CN119039056A discloses a semiconductor heating chuck, its preparation method, and its application. Graphene is directly coated onto the electrode as a built-in single-temperature heating layer, achieving an electrothermal conversion efficiency of over 99.2% and rapid heating within tens of seconds. CN107154377A discloses an electrostatic chuck device with graphene electrodes. Graphene is used to create a pure adsorption single electrode, replacing traditional metal electrodes. This avoids the high-temperature sintering process of traditional metal electrodes, prevents electrode deformation, and improves the uniformity of adsorption force. However, the graphene in these studies is mainly used in external single-temperature zone electrostatic chucks or as a pure adsorption single-electrode electrostatic chuck, resulting in limited functionality and certain limitations in highly integrated and advanced process technologies.

[0005] Therefore, there is an urgent need to develop an electrostatic chuck manufacturing process that can achieve good temperature uniformity without the need for a traditional Class 100 temperature zone system. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the purpose of this application is to provide a multi-temperature zone graphene integrated electrostatic chuck, its preparation method, and its application. This breaks through the requirement of using dense heating temperature zones to achieve extreme temperature uniformity, enabling the system to achieve or even surpass the uniform temperature effect that requires dense temperature zones with only a relatively small number of temperature zones.

[0007] To achieve the purpose of this application, the following technical solution is adopted: In a first aspect, this application provides a method for preparing a multi-temperature zone graphene integrated electrostatic chuck, comprising the following steps: (1) Provide 7-15 alumina green ceramic sheets, and print electrostatic electrodes, heating electrodes and graphene coatings on 3 of the alumina green ceramic sheets respectively. The heating electrodes contain ≥37 heating temperature zones, and the graphene coatings correspond to each heating temperature zone of the heating electrodes. Then dry them respectively. The remaining alumina green ceramic sheets serve as dielectric layer green ceramic sheets and substrate layer green ceramic sheets. (2) The dielectric layer green ceramic sheet, the green ceramic sheet containing electrostatic electrodes, the green ceramic sheet containing graphene coating, the green ceramic sheet containing heating electrodes and the base layer green ceramic sheet are stacked and hot-pressed. The resulting ceramic green body is sintered by HTCC and then processed to obtain the multi-temperature zone graphene integrated electrostatic chuck.

[0008] The method for fabricating a multi-temperature zone graphene integrated electrostatic chuck provided in this application integrates a multi-temperature zone heating electrode with a built-in area of ​​≥37 with graphene partitions. Specifically, a corresponding partitioned graphene coating is printed on a ceramic sheet above the heating electrode, which avoids "thermal crosstalk" during heating. At the same time, the ultra-high thermal conductivity of graphene (up to 5000 W / m·K) and its uniform temperature characteristics can be utilized to quickly smooth out the local temperature difference caused by the annular heating electrode. This breaks the requirement of using dense heating zones to achieve the ultimate temperature uniformity, allowing the system to achieve or even surpass the uniform temperature effect that requires a relatively small number of temperature zones.

[0009] The 7-15 alumina green ceramic tiles can be, for example, 7, 9, 10, 12 or 15 tiles, but are not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0010] The 7-15 alumina green ceramic sheets must be free of defects and foreign matter on their surfaces to ensure the subsequent stacking and hot pressing effect.

[0011] The heating electrode contains ≥37 heating temperature zones, for example, 37, 40, 42, 45 or 50, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0012] It should be noted that the HTCC sintering mentioned in step (2) refers to "high temperature co-fired ceramic sintering".

[0013] In some embodiments, the alumina green ceramic in step (1) is obtained by casting and slicing alumina ceramic slurry.

[0014] It should be noted that the casting and slicing are conventional techniques in the field. This application does not limit the specific process parameters of casting and slicing. Those skilled in the art can select appropriate casting and slicing process parameters according to the actual application scenario.

[0015] In some embodiments, the preparation steps of the alumina ceramic slurry include: ball milling alumina raw materials, auxiliary materials such as sintering aids, dispersants and solvents, and then adding plasticizers and binders to continue ball milling.

[0016] It should be noted that the alumina raw material can be alumina powder and / or alumina balls, and those skilled in the art can make an appropriate selection based on the actual application scenario.

[0017] In some embodiments, the auxiliary sintering agent includes silicon dioxide, calcium carbonate, and magnesium oxide.

[0018] In some embodiments, the dispersant comprises any one or a combination of at least two of triolein, polyacrylamide, or polyvinylpyrrolidone. Typical but non-limiting combinations include a combination of triolein and polyacrylamide, a combination of polyacrylamide and polyvinylpyrrolidone, or a combination of triolein, polyacrylamide, and polyvinylpyrrolidone.

[0019] In some embodiments, the solvent includes ethanol and / or toluene.

[0020] In some embodiments, the plasticizer includes polyethylene glycol and / or dibutyl phthalate.

[0021] In some embodiments, the adhesive includes PVB.

[0022] In some embodiments, the alumina ceramic slurry comprises, based on a total mass percentage of 100 wt%, 60-70 wt% alumina raw material, 0.1-0.5 wt% silica, 0.1-0.5 wt% calcium carbonate, 0.1-0.5 wt% magnesium oxide, 0.5-1 wt% dispersant, 20-30 wt% solvent, 2-5 wt% plasticizer, and 3-8 wt% binder.

[0023] The alumina ceramic slurry contains 60-70 wt% alumina raw material, for example, 60 wt%, 62 wt%, 65 wt%, 68 wt%, or 70 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0024] The mass percentage of silica in the alumina ceramic slurry is 0.1-0.5 wt%, for example, it can be 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt% or 0.5 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0025] The calcium carbonate content in the alumina ceramic slurry is 0.1-0.5 wt%, for example, it can be 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt% or 0.5 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0026] The magnesium oxide content in the alumina ceramic slurry is 0.1-0.5 wt%, for example, it can be 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt% or 0.5 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0027] The mass percentage of dispersant in the alumina ceramic slurry is 0.5-1 wt%, for example, it can be 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt% or 1 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0028] The solvent content in the alumina ceramic slurry is 20-30 wt%, for example, it can be 20 wt%, 22 wt%, 25 wt%, 28 wt% or 30 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0029] The plasticizer content in the alumina ceramic slurry is 2-5 wt%, for example, it can be 2 wt%, 2.5 wt%, 2.7 wt%, 4 wt% or 5 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0030] The mass percentage of binder in the alumina ceramic slurry is 3-8 wt%, for example, it can be 3 wt%, 4 wt%, 5 wt%, 6 wt% or 8 wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0031] In some embodiments, the ball mill rotates at a speed of 20-30 rpm for a total time of 20-36 hours.

[0032] The rotational speed of the ball mill is 20-30 rpm, for example, it can be 20 rpm, 22 rpm, 25 rpm, 28 rpm or 30 rpm, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0033] The total ball milling time is 20-36 hours, for example, it can be 20 hours, 24 hours, 28 hours, 32 hours or 36 hours, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0034] In some embodiments, the materials used for the electrostatic electrode and heating electrode in step (1) include tungsten paste or molybdenum paste.

[0035] In some embodiments, the drying temperature in step (1) is 40-70°C, for example, it can be 40°C, 45°C, 50°C, 60°C or 70°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0036] In some embodiments, the temperature of hot pressing the laminates in step (2) is 40-70°C, for example, it can be 40°C, 45°C, 50°C, 60°C or 70°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0037] In some embodiments, the pressure of hot pressing the stacked sheets in step (2) is 15-20 MPa, for example, it can be 15 MPa, 16 MPa, 18 MPa, 19 MPa or 20 MPa, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0038] In some embodiments, the holding time of the stacked hot pressing in step (2) is 3-5 min, for example, it can be 3 min, 3.5 min, 4 min, 4.5 min or 5 min, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0039] In some embodiments, the HTCC sintering temperature in step (2) is 1530-1580°C, for example, it can be 1530°C, 1540°C, 1550°C, 1560°C, 1570°C or 1580°C, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0040] In some embodiments, the HTCC sintering in step (2) is carried out in a hydrogen or nitrogen atmosphere.

[0041] In some implementations, the HTCC sintering time in step (2) is 2-6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0042] In some implementations, the post-processing in step (2) includes machining and assembly.

[0043] The assembly refers to the bonding of the ceramic obtained by HTCC sintering with a base using high-temperature adhesive.

[0044] Secondly, this application provides a multi-temperature zone graphene integrated electrostatic chuck, which is prepared by the preparation method of the multi-temperature zone graphene integrated electrostatic chuck described in the first aspect.

[0045] The multi-temperature zone graphene integrated electrostatic chuck provided in this application prints multi-temperature zone heating electrodes on alumina green ceramic sheets through a casting process. At the same time, a corresponding partitioned graphene coating is printed on the green ceramic sheet above the heating electrodes. After stacking the green ceramic sheets, debinding and sintering are performed to obtain multi-temperature zone graphene alumina ceramic. This can improve the temperature uniformity to the same level as traditional Class 100 temperature zone systems, achieving a performance breakthrough.

[0046] Thirdly, this application provides an application of the multi-temperature zone graphene integrated electrostatic chuck as described in the second aspect, wherein the multi-temperature zone graphene integrated electrostatic chuck is used in semiconductor manufacturing equipment.

[0047] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0048] Compared with the prior art, this application has the following advantages: The method for fabricating a multi-temperature zone graphene integrated electrostatic chuck provided in this application integrates a multi-temperature zone heating electrode with a built-in area of ​​≥37 with graphene partitions. Specifically, a corresponding partitioned graphene coating is printed on a ceramic sheet above the heating electrode, which avoids "thermal crosstalk" during heating. At the same time, the ultra-high thermal conductivity of graphene (up to 5000 W / m·K) and its uniform temperature characteristics can be utilized to quickly smooth out the local temperature difference caused by the annular heating electrode. This breaks through the requirement of using dense heating zones to achieve the ultimate temperature uniformity, enabling the system to achieve or even surpass the uniform temperature effect that requires dense heating zones with only a few temperature zones. The temperature non-uniformity of the wafer surface is as low as 1.6℃. Attached Figure Description

[0049] Figure 1 This is a schematic diagram of the structure of the ceramic green body provided in Embodiment 1 of this application.

[0050] Among them: 1, dielectric layer green ceramic sheet; 2, green ceramic sheet containing electrostatic electrodes; 3, green ceramic sheet containing graphene coating; 4, green ceramic sheet containing heating electrodes; 5, base layer green ceramic sheet. Detailed Implementation

[0051] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0052] Example 1 This embodiment provides a multi-temperature zone graphene integrated electrostatic chuck, and the preparation method of the multi-temperature zone graphene integrated electrostatic chuck includes the following steps: (1) Alumina powder, silicon dioxide, calcium carbonate, magnesium oxide, trioleic acid glyceride and ethanol are ball-milled, and then dibutyl phthalate and PVB are added and ball-milled again. The ball milling speed is 25 rpm and the total time is 28 h to obtain alumina ceramic slurry. The alumina ceramic slurry comprises: 65 wt% alumina powder, 0.3 wt% silicon dioxide, 0.2 wt% calcium carbonate, 0.2 wt% magnesium oxide, 0.8 wt% trioleic acid glyceride, 25 wt% ethanol, 2.5 wt% dibutyl phthalate and 6 wt% PVB. The obtained alumina ceramic slurry is cast and sliced ​​to obtain alumina green ceramic sheets.

[0053] Ten alumina green ceramic sheets are provided. Electrostatic electrodes, heating electrodes, and graphene coatings are printed on three of the alumina green ceramic sheets respectively. The electrostatic electrodes and heating electrodes are made of tungsten paste. The heating electrodes contain 37 heating temperature zones. The graphene coatings correspond to the heating temperature zones of the heating electrodes. Then, they are dried at 50°C. The remaining alumina green ceramic sheets serve as dielectric layer green ceramic sheet 1 and substrate layer green ceramic sheet 5.

[0054] (2) The dielectric layer green ceramic sheet 1, the green ceramic sheet 2 containing electrostatic electrodes, the green ceramic sheet 3 containing graphene coating, the green ceramic sheet 4 containing heating electrodes, and the base layer green ceramic sheet 5 are stacked and hot-pressed at a temperature of 50℃, a pressure of 18MPa, and a holding time of 4min. The structural diagram of the resulting ceramic green body is shown below. Figure 1 As shown, the obtained ceramic green body was sintered in a hydrogen atmosphere at a temperature of 1550℃ for 4 hours. After machining, the ceramic obtained by HTCC sintering was bonded to the base with high-temperature adhesive to obtain the multi-temperature zone graphene integrated electrostatic chuck.

[0055] Example 2 This embodiment provides a multi-temperature zone graphene integrated electrostatic chuck, and the preparation method of the multi-temperature zone graphene integrated electrostatic chuck includes the following steps: (1) Alumina powder, silicon dioxide, calcium carbonate, magnesium oxide, trioleic acid glyceride and ethanol are ball-milled, and then dibutyl phthalate and PVB are added and ball-milled again. The ball milling speed is 20 rpm and the total time is 36 h to obtain alumina ceramic slurry. The alumina ceramic slurry comprises: 60 wt% alumina powder, 0.5 wt% silicon dioxide, 0.5 wt% calcium carbonate, 0.5 wt% magnesium oxide, 0.5 wt% trioleic acid glyceride, 30 wt% ethanol, 5 wt% dibutyl phthalate and 3 wt% PVB. The obtained alumina ceramic slurry is cast and sliced ​​to obtain alumina green ceramic sheets.

[0056] Seven alumina green ceramic sheets are provided. Electrostatic electrodes, heating electrodes, and graphene coatings are printed on three of the alumina green ceramic sheets respectively. The electrostatic electrodes and heating electrodes are made of tungsten paste. The heating electrodes contain 40 heating temperature zones. The graphene coatings correspond to the heating temperature zones of the heating electrodes. Then, they are dried at 70°C. The remaining alumina green ceramic sheets serve as dielectric layer green ceramic sheet 1 and substrate layer green ceramic sheet 5.

[0057] (2) The dielectric layer green ceramic sheet 1, the green ceramic sheet 2 containing electrostatic electrodes, the green ceramic sheet 3 containing graphene coating, the green ceramic sheet 4 containing heating electrodes, and the base layer green ceramic sheet 5 are stacked and hot-pressed at a temperature of 70°C, a pressure of 15MPa, and a holding time of 3min to obtain a ceramic green body; the obtained ceramic green body is sintered in a hydrogen atmosphere at a temperature of 1580°C for 2h; after machining, the ceramic obtained by HTCC sintering is bonded to the base with high-temperature adhesive to obtain the multi-temperature zone graphene integrated electrostatic chuck.

[0058] Example 3 This embodiment provides a multi-temperature zone graphene integrated electrostatic chuck, and the preparation method of the multi-temperature zone graphene integrated electrostatic chuck includes the following steps: (1) Alumina powder, silicon dioxide, calcium carbonate, magnesium oxide, trioleic acid glyceride and toluene are ball-milled, and then dibutyl phthalate and PVB are added and ball-milled again. The ball milling speed is 30 rpm and the total time is 20 h to obtain alumina ceramic slurry. The alumina ceramic slurry comprises: 70 wt% alumina powder, 0.1 wt% silicon dioxide, 0.1 wt% calcium carbonate, 0.1 wt% magnesium oxide, 1 wt% trioleic acid glyceride, 20 wt% toluene, 2.7 wt% dibutyl phthalate and 6 wt% PVB. The obtained alumina ceramic slurry is then cast and sliced ​​to obtain alumina green ceramic sheets.

[0059] Fifteen alumina green ceramic sheets are provided. Electrostatic electrodes, heating electrodes, and graphene coatings are printed on three of the alumina green ceramic sheets respectively. The electrostatic electrodes and heating electrodes are made of molybdenum paste. The heating electrodes contain 45 heating temperature zones. The graphene coatings correspond to the heating temperature zones of the heating electrodes. Then, they are dried at 40-70℃ respectively. The remaining alumina green ceramic sheets serve as dielectric layer green ceramic sheet 1 and substrate layer green ceramic sheet 5.

[0060] (2) The dielectric layer green ceramic sheet 1, the green ceramic sheet 2 containing electrostatic electrodes, the green ceramic sheet 3 containing graphene coating, the green ceramic sheet 4 containing heating electrodes, and the base layer green ceramic sheet 5 are stacked and hot-pressed at a temperature of 40°C, a pressure of 20MPa, and a holding time of 5min to obtain a ceramic green body; the obtained ceramic green body is sintered in a hydrogen atmosphere at a temperature of 1530°C for 6h; after machining, the ceramic obtained by HTCC sintering is bonded to the base with high-temperature adhesive to obtain the multi-temperature zone graphene integrated electrostatic chuck.

[0061] Example 4 This embodiment provides a multi-temperature zone graphene integrated electrostatic chuck. The preparation method of the multi-temperature zone graphene integrated electrostatic chuck differs from that of Embodiment 1 in that the HTCC sintering temperature in step (2) is adjusted to 1500℃, while the rest is the same as in Embodiment 1.

[0062] Example 5 This embodiment provides a multi-temperature zone graphene integrated electrostatic chuck. The preparation method of the multi-temperature zone graphene integrated electrostatic chuck differs from that of Embodiment 1 in that the HTCC sintering temperature in step (2) is adjusted to 1600℃, while the rest is the same as in Embodiment 1.

[0063] Comparative Example 1 This comparative example provides an electrostatic chuck. The preparation method of the electrostatic chuck differs from that of Example 1 in that the graphene-coated raw ceramic sheet 3 described in step (2) is not set, and the heating temperature zone included in the heating electrode described in step (1) is adjusted to 100. The rest are the same as in Example 1.

[0064] Comparative Example 2 This comparative example provides a multi-temperature zone graphene integrated electrostatic chuck. The preparation method of the multi-temperature zone graphene integrated electrostatic chuck differs from that of Example 1 in that the heating temperature zone included in the heating electrode in step (1) is adjusted to 30, while the rest are the same as in Example 1.

[0065] After fixing the multi-temperature zone graphene integrated electrostatic chucks provided in Examples 1-5 and Comparative Example 2, as well as the electrostatic chuck provided in Comparative Example 1, a wafer surface temperature uniformity test was performed. The specific steps included: in a simulated chamber, evacuating the electrostatic chuck and heating it to a set temperature (60°C), using a TC-Wafer to detect the temperature at various points on the wafer, and obtaining the wafer surface temperature non-uniformity ΔT(T max -T min The results are shown in Table 1.

[0066] Table 1 As can be seen from Table 1, the multi-temperature zone graphene integrated electrostatic chuck provided in this application utilizes the ultra-high thermal conductivity and uniform temperature characteristics of graphene to quickly smooth out the local temperature difference caused by the annular heating electrode. This breaks the requirement of using dense heating temperature zones to achieve the ultimate temperature uniformity, enabling the system to achieve or even surpass the uniform temperature effect that requires dense temperature zones with only a few temperature zones.

[0067] Comparing Examples 1 with Examples 4 and 5, it can be seen that if the HTCC sintering temperature is too low, the green ceramic sheet will not be dense and uniform, resulting in uneven heat transfer of the heating wire of the heating electrode. If the HTCC sintering temperature is too high, the difference in thermal expansion coefficients between the electrode and the green ceramic sheet will cause the thermal stress to exceed the interfacial bonding force, resulting in cracking of the electrode and the green ceramic sheet. Comparing Example 1 with Comparative Example 1, it can be seen that without the green ceramic sheet containing graphene coating, the heating electrode contains 100 heating temperature zones. Compared with the multi-temperature zone graphene integrated electrostatic chuck structure in this application, the temperature uniformity is better, but the process design is more complex, and its temperature uniformity is not much different from the multi-temperature zone graphene integrated electrostatic chuck structure provided in this application. The introduction of graphene greatly reduces the impact of poor temperature uniformity in the low-temperature zone. Comparing Example 1 with Comparative Example 2, it can be seen that with the same multi-temperature zone + graphene structure, the electrostatic chuck with more temperature zones has better temperature uniformity than the electrostatic chuck with fewer temperature zones.

[0068] In summary, the method for fabricating a multi-temperature zone graphene integrated electrostatic chuck provided in this application integrates a multi-temperature zone heating electrode with a built-in area of ​​≥37 with graphene partitions. Specifically, corresponding partitioned graphene coatings are printed on a ceramic sheet above the heating electrodes, which avoids thermal crosstalk during heating. At the same time, the ultra-high thermal conductivity of graphene (up to 5000 W / m·K) and its uniform temperature characteristics can be utilized to quickly smooth out the local temperature difference caused by the annular heating electrode. This breaks through the requirement of using dense heating zones to achieve the ultimate temperature uniformity, enabling the system to achieve or even surpass the uniform temperature effect that requires dense heating zones with only a few temperature zones. The wafer surface temperature non-uniformity is as low as 1.6℃.

[0069] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for preparing a multi-temperature zone graphene integrated electrostatic chuck, characterized in that, Includes the following steps: (1) Provide 7-15 alumina green ceramic sheets, and print electrostatic electrodes, heating electrodes and graphene coatings on 3 of the alumina green ceramic sheets respectively. The heating electrodes contain ≥37 heating temperature zones, and the graphene coatings correspond to each heating temperature zone of the heating electrodes. Then dry them respectively. The remaining alumina green ceramic sheets are used as dielectric layer green ceramic sheets and substrate layer green ceramic sheets. (2) The dielectric layer green ceramic sheet, the green ceramic sheet containing electrostatic electrodes, the green ceramic sheet containing graphene coating, the green ceramic sheet containing heating electrodes and the base layer green ceramic sheet are stacked and hot-pressed. The resulting ceramic green body is sintered by HTCC and then processed to obtain the multi-temperature zone graphene integrated electrostatic chuck.

2. The preparation method according to claim 1, characterized in that, The alumina green ceramic in step (1) is obtained by casting and slicing alumina ceramic slurry.

3. The preparation method according to claim 2, characterized in that, The preparation steps of the alumina ceramic slurry include: ball milling alumina raw materials, auxiliary materials, sintering aids, dispersants and solvents, and then adding plasticizers and binders to continue ball milling.

4. The preparation method according to any one of claims 1-3, characterized in that, The materials used for the electrostatic electrode and heating electrode in step (1) include tungsten paste or molybdenum paste.

5. The preparation method according to any one of claims 1-4, characterized in that, The drying temperature in step (1) is 40-70℃.

6. The preparation method according to any one of claims 1-5, characterized in that, The temperature for hot pressing the laminated sheets in step (2) is 40-70℃; And / or, the pressure of hot pressing the laminates in step (2) is 15-20 MPa; And / or, the holding time for hot pressing of the stacked sheets in step (2) is 3-5 min.

7. The preparation method according to any one of claims 1-6, characterized in that, The sintering temperature of HTCC in step (2) is 1530-1580℃; And / or, the HTCC sintering in step (2) is carried out in a hydrogen or nitrogen atmosphere; And / or, the sintering time of HTCC in step (2) is 2-6 hours.

8. The preparation method according to any one of claims 1-7, characterized in that, The post-processing described in step (2) includes machining and assembly.

9. A multi-temperature zone graphene integrated electrostatic chuck, characterized in that, The multi-temperature zone graphene integrated electrostatic chuck is prepared by the preparation method of the multi-temperature zone graphene integrated electrostatic chuck according to any one of claims 1-8.

10. An application of the multi-temperature zone graphene integrated electrostatic chuck as described in claim 9, characterized in that, The multi-temperature zone graphene integrated electrostatic chuck is used in semiconductor manufacturing equipment.

Citation Information

Patent Citations

  • Electrostatic chuck device of graphene electrode

    CN107154377A

  • Semiconductor heating sucker and preparation method and application thereof

    CN119039056A

  • Electrostatic chuck mechanism for heating

    CN221486472U