Barrier layer penetration detection method, semiconductor structure formation method and apparatus
By performing an ion implantation process and growing an epitaxial layer after forming a barrier layer on the substrate surface, and using the change in the thickness of the epitaxial layer to determine ion penetration, the problem of long detection cycle, high cost or poor accuracy in the prior art is solved, and efficient and accurate barrier layer penetration detection is achieved.
Patent Information
- Application Number
- CN202611281310.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-20
AI Technical Summary
Existing barrier penetration detection solutions suffer from problems such as long detection cycles, high costs, or poor accuracy, making it difficult to balance detection efficiency, cost, and accuracy.
An ion implantation process is performed after a barrier layer is formed on the substrate surface. The barrier layer is then removed and an epitaxial layer is grown on the substrate surface. The thickness change of the epitaxial layer is used to determine whether ions have penetrated the barrier layer. Germanium-silicon material is used as the epitaxial layer, and the thickness of the epitaxial layer is detected by combining equipment such as an ellipsometry.
It achieves simple, fast, and low-cost barrier layer penetration detection with high accuracy. It is applicable to bare wafers and in-line process wafers, and suitable for online quality monitoring in the mass production stage.
Smart Images

Figure CN123146191A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and specifically to a barrier layer penetration detection method, a semiconductor structure formation method, and an apparatus. Background Technology
[0002] Ion implantation (IMP) is a core doping process in semiconductor chip manufacturing. It is mainly used to precisely introduce impurity ions into designated areas of a wafer to control the conductivity and resistivity of the semiconductor substrate, thereby constructing functional structures such as the active region and doped contact region of a transistor and achieving the intended electrical performance of the device.
[0003] In actual manufacturing processes, a barrier layer is usually formed on the substrate first. The barrier layer is used to cover non-target areas that do not require ion implantation and expose the target areas that require ion implantation. This can prevent impurities from being mistakenly doped into non-target areas and ensure that the device layout design and electrical parameters meet the specifications.
[0004] In this process chain, the thickness of the barrier layer is a critical process parameter. When introducing new ion implantation process parameters, it is necessary to first verify whether the barrier layer of the corresponding thickness can completely block the implanted ions and confirm that the ions will not penetrate the barrier layer.
[0005] However, existing barrier penetration detection solutions either have long detection cycles and high detection costs, or poor detection accuracy, making it difficult to balance detection efficiency, detection cost, and detection accuracy. Summary of the Invention
[0006] The problem this invention aims to solve is to balance detection efficiency, detection cost, and detection accuracy during the process of detecting barrier penetration.
[0007] To address the above problems, embodiments of the present invention provide a method for detecting barrier layer penetration, the method comprising: A wafer to be tested is provided, the wafer to be tested comprising: a substrate and a first barrier layer covering the surface of the substrate; An ion implantation process is performed on the wafer to be tested; Remove the first barrier layer and form an epitaxial layer on the substrate surface; The thickness of the epitaxial layer is detected to determine whether the implanted ions penetrate the first barrier layer during the ion implantation process.
[0008] In one possible embodiment, the implanted ions in the ion implantation process are heavy ions.
[0009] In one possible embodiment, the heavy ions include arsenic ions.
[0010] In one possible embodiment, the epitaxial layer is made of germanium-silicon.
[0011] In one possible embodiment, the material of the first barrier layer is photoresist.
[0012] In one possible embodiment, the substrate includes a substrate.
[0013] In one possible embodiment, the substrate further includes at least one film layer formed on the substrate and having a pattern.
[0014] In one possible embodiment, detecting the thickness of the epitaxial layer to determine whether implanted ions penetrate the first barrier layer during the ion implantation process includes: When the thickness of the epitaxial layer is less than the target thickness, it is determined that the implanted ions in the ion implantation process penetrate the first barrier layer; otherwise, it is determined that the implanted ions in the ion implantation process have not penetrated the first barrier layer.
[0015] This invention also provides a method for forming a semiconductor structure, the method comprising: Using any of the above-mentioned ion implantation processes, the thickness of the second barrier layer is determined and the second barrier layer is formed; the second barrier layer covers the non-target area of the substrate surface and exposes the target area; An ion implantation process is performed on the target region.
[0016] This invention also provides a barrier layer penetration detection method apparatus, the apparatus comprising: A receiving unit is adapted to receive a wafer under test, the wafer under test comprising: a substrate and a first barrier layer covering the surface of the substrate; An ion implantation unit is adapted to perform an ion implantation process on the wafer under test. An epitaxial unit is adapted to remove the first barrier layer and form an epitaxial layer on the surface of the substrate; And a detection unit, adapted to detect the thickness of the epitaxial layer, so as to determine whether the implanted ions penetrate the first barrier layer during the ion implantation process.
[0017] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages: The present invention utilizes an ion implantation process performed after forming a first barrier layer on the substrate surface, followed by removal of the first barrier layer and growth of an epitaxial layer on the substrate surface. By leveraging the principle that lattice damage caused by ions penetrating the first barrier layer affects the thickness of the epitaxial layer, the thickness of the epitaxial layer can be detected to determine whether ions have penetrated the first barrier layer. This method eliminates the need for secondary ion mass spectrometry (SIMS) profiling, avoiding the long detection cycle and high cost associated with offline destructive analysis. It also avoids the need for combined thermal wave detection and sheet resistance (TMW+Rs) monitoring, preventing interference from multiple process variables introduced by the annealing process on detection accuracy. The present invention offers a simple detection process, short detection cycle, low detection cost, and high detection accuracy, effectively balancing detection efficiency, cost, and accuracy. Furthermore, this method can be applied to both bare wafers with flat surfaces and process wafers in online production lines, making it suitable for online quality monitoring during mass production.
[0018] The semiconductor structure formation method of the present invention, based on the first barrier layer thickness determined by the above detection method, forms a second barrier layer on the substrate with a thickness not less than that thickness and then performs ion implantation, thereby ensuring that the barrier layer can effectively block implanted ions in the actual ion implantation process, preventing ions from penetrating to non-target areas, and improving the reliability and yield of the device fabrication process.
[0019] The barrier layer penetration detection device of the present invention achieves fully automated operation from wafer reception to penetration detection through the coordinated cooperation of various functional units, and is suitable for online inspection on production lines. Attached Figure Description
[0020] Figure 1 This is a flowchart illustrating a barrier layer penetration detection method according to an embodiment of the present invention; Figure 2 This is a schematic cross-sectional view of a wafer under test in an embodiment of the present invention; Figure 3 This is a schematic diagram of an ion implantation process performed on a wafer under test according to an embodiment of the present invention; Figure 4 This is a schematic cross-sectional view of the substrate after the first barrier layer has been removed, according to an embodiment of the present invention. Figure 5 This is a schematic diagram of epitaxial layer growth after implanted ions penetrate the first barrier layer in an embodiment of the present invention; Figure 6 This is a schematic diagram of epitaxial layer growth after implanted ions fail to penetrate the first barrier layer in an embodiment of the present invention; Figure 7 Comparison of the effects of different implanted elements on epitaxial layer thickness and germanium concentration in embodiments of the present invention; Figure 8A flowchart of a semiconductor structure formation method according to an embodiment of the present invention; Figure 9 This is a schematic diagram of the structure of a barrier layer penetration detection device according to an embodiment of the present invention. Detailed Implementation
[0021] In ion implantation, the thickness of the barrier layer is a critical process parameter. If the barrier layer is too thin, high-energy implanted ions will have sufficient penetration ability to directly break through the barrier layer and invade non-target areas that should be shielded from implantation, causing unexpected impurity doping, disrupting the internal doping distribution of the device, and leading to reliability and electrical problems such as leakage current, threshold voltage deviation, and device failure. Therefore, when introducing new ion implantation process parameters, it is essential to first verify whether the corresponding thickness of the barrier layer can completely block the implanted ions and confirm that the ions will not penetrate the barrier layer.
[0022] Currently, the mainstream detection methods used in the industry to determine whether implanted ions have penetrated the barrier layer and to verify the barrier layer's blocking ability fall into two categories: 1) Secondary ion mass spectrometry (SIMS) profiling detection method This method determines whether ions have penetrated the barrier layer by comparing the depth distribution curves of impurity elements inside the wafer before and after ion implantation. The standard procedure is as follows: deposit barrier layers of various thicknesses on the wafer surface, perform ion implantation for each thickness of barrier layer distribution, peel off the barrier layer after ion implantation, perform SIMS depth profiling on the wafer substrate, and infer whether ions have broken through the photoresist based on the content and vertical distribution of implanted impurities inside the substrate.
[0023] This testing method has several drawbacks: SIMS is an offline destructive analysis, with a cumbersome testing process, long experimental cycle, and high cost per batch. Furthermore, this test can only sample and analyze wafers with flat surfaces, and cannot perform in-situ, real-time penetration risk verification on wafers in the production line. It can only be used for preliminary process development and cannot be used for real-time quality monitoring in mass production.
[0024] 2) Combined monitoring method of thermal wave detection and sheet resistance (TMW+Rs)
[0025] This method indirectly determines the blocking effect of the barrier layer on implanted ions by using changes in the total wafer thickness and sheet resistance. However, this detection process requires a second sheet resistance measurement after annealing, introducing multiple process variables such as lattice damage, thermal budget fluctuations, and film thickness deviations into the entire process, resulting in numerous interference factors and low data accuracy in the detection results.
[0026] Meanwhile, this solution also targets wafers with flat surfaces for inspection, but it still cannot perform in-situ verification of ion penetration on online wafers that are currently in operation on the production line, making it difficult to meet the online quality control requirements of the mass production stage.
[0027] To address the aforementioned problems, this invention provides a barrier layer penetration detection method. This method utilizes the principle that implanted ions, after penetrating the barrier layer during ion implantation, cause lattice damage to the substrate surface, leading to a reduction in the thickness of the subsequent epitaxial layer. The method indirectly determines whether implanted ions have penetrated the barrier layer by detecting the thickness of the epitaxial layer. This approach eliminates the need for offline destructive detection methods such as SIMS, as well as indirect monitoring methods that introduce additional process variables, such as TMW+Rs. It achieves penetration determination solely using existing epitaxial growth processes and thickness detection methods in semiconductor manufacturing, offering advantages such as high detection efficiency, low detection cost, and good detection accuracy.
[0028] The technical solutions of the embodiments of the present invention will be described in detail below with reference to the accompanying drawings and specific implementation methods.
[0029] Reference Figure 1 This invention provides a method for detecting barrier layer penetration, which may include the following steps: Step S1, providing a wafer to be tested, the wafer to be tested comprising: a substrate and a first barrier layer covering the surface of the substrate; Step S2: Perform an ion implantation process on the wafer to be tested; Step S3: Remove the first barrier layer and form an epitaxial layer on the substrate surface; Step S4: Detect the thickness of the epitaxial layer to determine whether the implanted ions penetrate the first barrier layer during the ion implantation process.
[0030] The following is in conjunction with the appendix Figures 2 to 6 Steps S1 to S4 are described in detail below: Reference Figure 2 Provide the wafer to be tested.
[0031] Specifically, the wafer under test includes a substrate 11 and a first barrier layer 12 covering the surface of the substrate 11. The substrate 11 can be a bare wafer, i.e., a flat wafer on which no device structure has been formed, or it can be an inline wafer, i.e., a wafer on which several device structure films have been formed.
[0032] The material of the substrate 11 is typically a semiconductor material, such as silicon, silicon carbide, gallium nitride, etc., and this application does not limit it. The substrate 11 provides the physical basis for carrying functional structures such as transistors and device structures. A first barrier layer 12 is formed on the surface of the substrate 11 to cover the surface of the substrate 11.
[0033] In some embodiments, the substrate 11 may consist of only a substrate.
[0034] The substrate is the basic supporting structure of the wafer, and it is usually a semiconductor material substrate. The substrate material can be an elemental semiconductor material, such as a silicon substrate or a germanium substrate; or it can be a compound semiconductor material, such as a silicon carbide substrate, a nitride substrate, a gallium nitride substrate, or a gallium arsenide substrate.
[0035] In semiconductor manufacturing, silicon substrates are the most commonly used substrates. The crystal orientation of the substrate can be (100), (110), or (111), depending on the device requirements. When the substrate only includes the substrate itself and does not contain other film structures, this substrate 11 corresponds to a bare wafer, that is, a wafer with a flat surface and no device structure formed. Bare wafers are suitable for barrier layer penetration testing during the process development stage, which can simplify experimental conditions and eliminate interference from other structural factors. In specific implementations, the diameter of the substrate can be a standard specification such as 150mm (6 inches), 200mm (8 inches), or 300mm (12 inches).
[0036] By explicitly defining the substrate as including a substrate, the minimum constituent elements of the substrate 11 are defined, making the detection method of the present invention applicable to both bare wafer scenarios with simple structures and substrates containing more complex structures.
[0037] In other embodiments, the substrate 11 further includes at least one film layer formed on the substrate and having a pattern.
[0038] When the substrate, in addition to the substrate itself, includes at least one patterned film layer formed on the substrate, the substrate corresponds to an inline wafer, i.e., a wafer on which device structure film layers have already been formed. These film layers include, but are not limited to, silicon oxide (SiO2), silicon nitride (Si3N4), polysilicon, metal layers, and dielectric layers. These film layers are patterned using processes such as photolithography and etching to form the functional structure of the device. The film pattern on the inline wafer affects the ion implantation path and scattering characteristics, and also influences the growth morphology of the epitaxial layer.
[0039] The detection method of the present invention can be applied to process wafers, which means that the method is not limited to bare wafer detection under laboratory conditions, but can also be used for real-time penetration risk verification of process wafers in online production line, which is something that existing SIMS and TMW+Rs methods cannot achieve.
[0040] In practice, the first barrier layer 12 is formed on the topmost surface of the process wafer, covering the area to be protected and exposing the area to be implanted. During inspection, the epitaxial layer grows in the exposed area of the substrate 11 after the first barrier layer 12 is removed, and the thickness of the epitaxial layer is affected by the surface condition of the substrate in that area.
[0041] By defining the substrate, it may also include a patterned film layer, making the detection method of the present invention applicable to the online detection of process wafers, expanding the application scenarios of the detection method, realizing online penetration risk verification of the production line, and making up for the shortcomings of existing detection methods that cannot be used for online wafers.
[0042] In specific implementations, the first barrier layer 12 can be formed on the surface of the substrate 11 through processes such as spin coating or deposition. The thickness of the first barrier layer 12 is a key parameter to be verified by the detection method of this invention. Subsequent detection processes determine whether the barrier layer corresponding to this thickness can effectively block implanted ions.
[0043] It is understandable that the first barrier layer 12 can cover a portion of the substrate surface (i.e., a patterned barrier layer) or the entire substrate surface (i.e., an unpatterned, full-layer barrier layer), depending on the detection requirements and process design. When the first barrier layer 12 is a patterned barrier layer, the initial barrier layer can be patterned using processes such as photolithography and development to form a pattern of the first barrier layer 12 that exposes the target area and covers the non-target area.
[0044] In some embodiments, the material of the first barrier layer 12 may be photoresist.
[0045] In practical implementation, photoresist (PR) is a commonly used patterned mask material in semiconductor manufacturing. The photoresist is uniformly coated onto the surface of the substrate 11 through a spin coating process, and then a patterned photoresist layer is formed through exposure and development processes to define the ion implantation area.
[0046] The thickness of the photoresist layer can be adjusted by parameters such as spin coating speed and photoresist viscosity, with a common thickness range of 100nm to 3000nm. The advantages of using photoresist as a barrier layer are: firstly, the formation and removal processes of photoresist are mature, low-cost, and highly compatible with existing semiconductor manufacturing processes; secondly, the photoresist removal process (ashing and humidification cleaning) does not cause additional damage to the substrate surface, avoiding interference from the removal process itself with subsequent epitaxial layer growth.
[0047] It is understood that the material of the first barrier layer 12 is not limited to photoresist, but may also include other materials that can block ions and are easy to remove, such as organic barrier layers, inorganic barrier layers, etc.
[0048] By using photoresist as the material of the first barrier layer 12, the detection method is highly compatible with existing semiconductor manufacturing processes, and the removal of the photoresist does not introduce additional substrate damage, thus ensuring the accuracy of the detection results.
[0049] Reference Figure 3 Ion implantation is performed on the wafer to be tested.
[0050] Ion implantation is a process in which dopant ions are accelerated to a certain energy and then injected into a designated area on the surface of a wafer to change the conductivity and resistivity of that area. Parameters of the ion implantation process include the type of implanted ions, implantation energy, implantation dose, and implantation angle. The type of implanted ions is determined according to the doping requirements of the device, the implantation energy determines the penetration depth of the ions in the wafer, and the implantation dose determines the doping concentration.
[0051] In one embodiment, the implanted ions in the ion implantation process are heavy ions. Heavy ions refer to ions with a relatively large atomic mass, typically those with a relative atomic mass greater than 50.
[0052] In semiconductor manufacturing, commonly used heavy ions include, but are not limited to, germanium ions (Ge, relative atomic mass approximately 73), indium ions (In, relative atomic mass approximately 114), and antimony ions (Sb, relative atomic mass approximately 122).
[0053] Heavy ions, compared to light ions (such as boron ions B / 11 and phosphorus ions P / 31), have greater mass and momentum, resulting in a more significant collisional cascade effect on the crystal lattice and greater lattice damage at the same implantation energy. This physical characteristic makes the damage to the substrate surface more severe after heavy ions penetrate the barrier layer, thus having a more significant impact on the epitaxial layer thickness during subsequent epitaxial layer growth, which is beneficial for improving the sensitivity and reliability of detection. Furthermore, even if light ions (such as boron ions B / 11) penetrate the barrier layer, the damage to the crystal lattice is smaller, and the change in epitaxial layer thickness may be insignificant, making it difficult to accurately determine the penetration status. Therefore, the method of this invention is particularly suitable for barrier layer penetration detection in heavy ion implantation processes.
[0054] To verify the above principle, the inventors conducted the following experiment: Combined with Table 1 and Figure 7 As shown, the inventors deposited photoresist (PR) of the same thickness on multiple wafers as the first barrier layer, performed ion implantation processes using ions of different elements, removed the photoresist, and grew germanium-silicon epitaxial layers on the surface of each wafer. The epitaxial layer thickness (EPI CD) and germanium concentration (Ge%) of each group of wafers were measured.
[0055] Table 1
[0056] Table 1 summarizes the epitaxial layer thickness and germanium concentration distribution under multiple ion implantation conditions. This summary table includes five test wafers, all using the same baseline epitaxial process (BSL) conditions, differing only in the implanted elements: Group 1 (CCBMKE4-06) was a blank control group, without ion implantation; Group 2 (CCBMKE4-09) was implanted with carbon ions (C, relative atomic mass 12); Group 3 (CCBMKE4-10) was implanted with fluorine ions (F, relative atomic mass 19); Group 4 (CCBMKE4-12) was implanted with arsenic ions (As, relative atomic mass 75); and Group 5 (CCBMKE4-15) was implanted with boron ions (B, relative atomic mass 11).
[0057] As shown in Table 1, the average epitaxial layer thicknesses of each group were 287.2 nm, 289.7 nm, 290.4 nm, 275.3 nm, and 200.7 nm, respectively, and the average germanium concentrations were 36.4%, 36.4%, 36.3%, 35.7%, and 36.3%, respectively. Among them, the epitaxial layer thickness (245.3 nm) and germanium concentration (25.7%) of the arsenic ion implantation group (CCBMKE4-12) were significantly lower than those of the other four groups.
[0058] Figure 7 This is a comparison chart showing the effects of different implanted elements on epitaxial layer thickness and germanium concentration. The chart is a dual Y-axis composite plot. The horizontal axis represents the element and its relative atomic mass, including five categories: C / 12, F / 19, As / 75, B / 11, and Only EPI (the baseline control group with only epitaxy and no implantation). The left vertical axis represents the epitaxial layer thickness (EPI CD, nm), corresponding to the blue line data; the right vertical axis represents the germanium concentration (Ge%), corresponding to the orange bar data.
[0059] like Figure 7 As shown, after implantation of light elements such as carbon ions (C / 12), fluorine ions (F / 19), and boron ions (B / 11), the epitaxial layer thicknesses were approximately 287.8 nm, 292 nm, and 291.7 nm, respectively, with germanium concentrations of approximately 36.2%, 36.28%, and 36.25%, respectively. These thicknesses were very close to the baseline control group (Only EPI, thickness approximately 291.8 nm, Ge% approximately 36.22%). However, after implantation of heavy elements such as arsenic ions (As / 75), the epitaxial layer thickness plummeted to approximately 275.2 nm, and the germanium concentration dropped to approximately 35.75%, exhibiting a "double decrease" in both epitaxial layer thickness and germanium concentration.
[0060] The above experimental results directly verify the core principle of this invention: light elements (C, F, B), due to their relatively small atomic masses, cause only minor lattice damage to the silicon substrate surface even when penetrating the photoresist, and the epitaxial layer growth parameters are not significantly affected. However, heavy elements (As, relative atomic mass 75), due to their large mass and significant collisional cascade effect, cause severe lattice damage to the silicon substrate surface after penetrating the photoresist, leading to a decrease in the growth rate, thickness, and germanium concentration of the subsequent germanium-silicon epitaxial layer. Therefore, by detecting whether the epitaxial layer thickness is lower than the target thickness, it is possible to accurately determine whether heavy ions have penetrated the barrier layer.
[0061] In a preferred embodiment, the heavy ion includes arsenic ions (As, with a relative atomic mass of about 75).
[0062] Arsenic ions (As) are commonly used N-type dopant ions in semiconductor manufacturing, widely applied in source / drain region doping, polysilicon doping, and other processes. With a relative atomic mass of approximately 75, arsenic ions belong to the heavy ion category. Arsenic ion implantation causes significant damage to the silicon lattice. When arsenic ions penetrate the barrier layer and enter the silicon substrate surface, they form an amorphous damage layer. This damage layer affects the nucleation density and growth rate during subsequent epitaxial growth, leading to a significant reduction in epitaxial layer thickness.
[0063] In practice, the implantation energy range of arsenic ions is typically 5keV to 100keV, and the implantation dose range is typically 1E13 to 1E16 ions / cm². The specific parameters are determined according to the process requirements.
[0064] By limiting the implanted ions to heavy ions and utilizing the physical property that heavy ions cause greater lattice damage, the detectability of epitaxial layer thickness changes is improved, thereby enhancing the sensitivity and accuracy of barrier layer penetration detection.
[0065] It is understandable that heavy ions are not limited to arsenic ions, but can also include other ion types with a relative atomic mass greater than 50, such as germanium ions, indium ions, and antimony ions.
[0066] During the ion implantation process, implanted ions bombard the surface of the first barrier layer. If the thickness of the first barrier layer 12 is sufficient, the implanted ions will be absorbed or blocked by the first barrier layer 12 and will not reach the surface of the substrate 11. If the thickness of the first barrier layer 12 is insufficient, high-energy implanted ions will penetrate the first barrier layer 12 and enter the surface of the substrate 11, causing damage to the lattice structure of the substrate 11 surface.
[0067] Reference Figure 4 Remove the first blocking layer 12.
[0068] Specifically, the process for removing the first barrier layer 12 depends on the material type of the first barrier layer 12. For example, when the first barrier layer is photoresist, a plasma ashing process can be used to remove the photoresist, followed by wet chemical cleaning such as sulfuric acid-hydrogen peroxide mixture (SPM) or ammonia-hydrogen peroxide mixture (APM) to remove residues and ensure the surface of the substrate 11 is clean.
[0069] Reference Figure 5 and Figure 6 After removing the first barrier layer 12, an epitaxial layer growth process is performed on the surface of the substrate 11 to form an epitaxial layer 13.
[0070] The epitaxial layer 13 can be grown using chemical vapor deposition (CVD) methods, including but not limited to atmospheric pressure chemical vapor deposition (APCVD), reduced pressure chemical vapor deposition (RPCVD), and ultra-high vacuum chemical vapor deposition (UHVCVD). The material of the epitaxial layer 13 can be a homoepitaxial material (such as growing a silicon epitaxial layer on a silicon substrate) or a heteroepitaxial material (such as growing a germanium-silicon epitaxial layer on a silicon substrate).
[0071] The growth thickness of epitaxial layer 13 is affected by the surface condition of the substrate: if the lattice on the surface of substrate 11 is intact, epitaxial layer 13 will grow normally to the target thickness, such as... Figure 6 As shown; if lattice damage exists on the surface of substrate 11 due to ion penetration, the nucleation and growth rate in the damaged area will be affected, resulting in a reduction in the growth thickness of epitaxial layer 13, such as... Figure 5 As shown.
[0072] In some embodiments, the epitaxial layer 13 is made of silicon germanium (SiGe).
[0073] In a specific implementation, the epitaxial layer 13 of the germanium-silicon material can be formed by growing a silicon-germanium alloy layer containing germanium components on the substrate 11. Specifically, it can be formed by a reduced pressure chemical vapor deposition (RPCVD) process, using silicon source gas (such as dichlorosilane SiH2Cl2, silane SiH4, etc.) and germanium source gas (such as germanane GeH4) as precursors, and growing in a temperature range of 600℃ to 800℃.
[0074] The germanium-silicon epitaxial layer 13 exhibits high sensitivity to lattice damage on the substrate 11 surface: when lattice damage exists on the substrate surface, the growth rate of the germanium-silicon epitaxial layer in the damaged area decreases significantly, leading to a reduction in the epitaxial layer thickness. This sensitivity allows changes in the germanium-silicon epitaxial layer thickness to more readily reflect the degree of damage on the substrate surface. Furthermore, the thickness of the germanium-silicon epitaxial layer 13 can be precisely measured using optical measurement methods such as ellipsometers, achieving sub-nanometer accuracy, which is beneficial for realizing high-precision penetration detection.
[0075] In specific implementation, the germanium composition of the epitaxial layer 13 of the germanium-silicon material can be adjusted according to process requirements, for example, the germanium content is 10% to 30% atomic ratio, and the target thickness of the epitaxial layer 13 is 20nm to 200nm.
[0076] By using germanium-silicon material as the epitaxial layer 13, the high sensitivity of germanium-silicon epitaxial growth to surface damage of the substrate 11 is utilized to improve the detectable range of thickness changes in the epitaxial layer 13, thereby further enhancing the sensitivity and accuracy of penetration detection of the first barrier layer 12.
[0077] Finally, the thickness of the epitaxial layer 13 is measured to determine whether the implanted ions penetrate the first barrier layer 12 during the ion implantation process.
[0078] In some embodiments, detecting the thickness of the epitaxial layer 13 to determine whether implanted ions penetrate the first barrier layer 12 during the ion implantation process includes: determining that implanted ions penetrate the first barrier layer 12 during the ion implantation process when the thickness of the epitaxial layer 13 is less than the target thickness; otherwise, determining that implanted ions do not penetrate the first barrier layer 12 during the ion implantation process.
[0079] Specifically, refer to Figure 5 and Figure 6 The thickness of the epitaxial layer 13 can be detected by various methods, including but not limited to ellipsometry measurement, X-ray reflectance (XRR) measurement, scanning electron microscope (SEM) cross-sectional measurement, and transmission electron microscope (TEM) cross-sectional measurement.
[0080] The thickness of the epitaxial layer 13 is compared with the preset target thickness. If the thickness of the epitaxial layer 13 is less than the target thickness, it indicates that there is lattice damage on the surface of the substrate 11, that is, the implanted ions have penetrated the first barrier layer 12. If the thickness of the epitaxial layer 13 is equal to or close to the target thickness, it indicates that the surface of the substrate 11 is not damaged, that is, the implanted ions have not penetrated the first barrier layer 12.
[0081] In practice, the target thickness refers to the thickness that the epitaxial layer 13 should reach during normal growth when the surface of the substrate 11 is not damaged by ion penetration, which is also the baseline (BSL) thickness. The target thickness is determined as follows: under the same process conditions, the epitaxial layer 13 is grown on a reference wafer on the surface of the substrate 11 without ion implantation, and the measured thickness of the epitaxial layer 13 is the target thickness.
[0082] In practice, multiple reference wafers can be selected for measurement, and the average value can be taken as the target thickness to improve the reliability of the reference. When implanted ions penetrate the first barrier layer 12, the surface of the substrate 11 is damaged by ion bombardment, resulting in defects such as amorphization, vacancies, and interstitial atoms. These defects affect the nucleation and growth kinetics of the epitaxial layer 13, leading to a decrease in the growth rate of the epitaxial layer 13, and ultimately causing the thickness of the epitaxial layer 13 to be less than the target thickness.
[0083] When the implanted ions fail to penetrate the first barrier layer 12, the surface of the substrate 11 remains intact, and the epitaxial layer 13 grows normally to the target thickness. Therefore, by comparing the actual thickness of the epitaxial layer 13 with the target thickness, it is possible to accurately determine whether the ions have penetrated the first barrier layer 12.
[0084] In practice, a tolerance range can be set. When the difference between the thickness of the epitaxial layer 13 and the target thickness exceeds the tolerance range, it is determined to be penetration, so as to eliminate the influence of measurement error and process fluctuation.
[0085] The above technical solution achieves an objective and accurate determination of the penetration of the first barrier layer by quantitatively comparing the thickness of the epitaxial layer 13 with the target thickness, avoiding the uncertainty of subjective judgment and improving the reliability of the detection results.
[0086] By adopting the above technical solution, the present invention utilizes the physical mechanism that ions cause lattice damage to the surface of the substrate 11 after penetrating the barrier layer, thereby affecting the growth thickness of the epitaxial layer 13. Penetration determination is achieved by detecting the thickness of the epitaxial layer 13. The detection process is simple and does not require expensive offline detection equipment such as SIMS, nor does it require indirect monitoring methods such as TMW+Rs that introduce additional process variables. It effectively balances detection efficiency, detection cost and detection accuracy.
[0087] Reference Figure 8 The present invention also provides a method for forming a semiconductor structure, the method comprising: Step P1: Using the above-described barrier layer penetration detection method, determine the thickness of the second barrier layer and form the second barrier layer; the second barrier layer covers the non-target area of the substrate surface and exposes the target area; Step P2: Perform an ion implantation process on the target region.
[0088] Specifically, in step P1, the thickness of the second barrier layer can be determined using the aforementioned barrier layer penetration detection method. Specifically, first barrier layers of different thicknesses are formed on the surface of the wafer to be tested. The aforementioned detection process (ion implantation → barrier layer removal → epitaxial layer growth → thickness detection) is then performed to find the minimum first barrier layer thickness that allows the epitaxial layer thickness to reach the target thickness (i.e., ions do not penetrate), denoted as the critical thickness. This critical thickness is the minimum safe thickness to ensure that ions do not penetrate the barrier layer.
[0089] Then, based on the determined thickness of the first barrier layer (i.e., the critical thickness), a second barrier layer is formed on the substrate of the actual device fabrication process. The thickness of the second barrier layer is set to be greater than or equal to the critical thickness to ensure that the barrier layer can effectively block implanted ions during the actual ion implantation process. The material of the second barrier layer can be the same as that of the first barrier layer (e.g., both are photoresist), or other materials can be selected according to actual process requirements. The second barrier layer is patterned through processes such as photolithography and development to cover the non-target areas (i.e., areas that do not require ion implantation) on the substrate surface and expose the target areas (i.e., areas that require ion implantation).
[0090] Finally, ion implantation is performed on the target region. Since the thickness of the second barrier layer has been verified by the aforementioned detection method, it can be ensured that implanted ions will not penetrate the second barrier layer and enter non-target regions, thereby guaranteeing the accuracy of device doping distribution and the reliability of electrical performance.
[0091] By adopting the above technical solution, the detection results of the barrier layer penetration are applied to the actual ion implantation process, forming a complete technical closed loop from detection to application. This ensures that the barrier layer's blocking capability is fully verified in the actual process, effectively avoiding ion penetration problems caused by insufficient barrier layer thickness, and improving the reliability and yield of device fabrication.
[0092] Reference Figure 9 Embodiments of the present invention also provide a barrier layer penetration detection device 90. The device 90 includes: Receiving unit 91 is adapted to receive a wafer under test, the wafer under test comprising: a substrate and a first barrier layer covering the surface of the substrate; Ion implantation unit 92 is adapted to perform ion implantation process on the wafer under test; Epitaxial unit 93 is adapted to remove the first barrier layer and form an epitaxial layer on the substrate surface; And a detection unit 94, adapted to detect the thickness of the epitaxial layer, so as to determine whether the implanted ions penetrate the first barrier layer in the ion implantation process.
[0093] Specifically, receiving unit 91 is used to receive the wafer under test, which includes a substrate and a first barrier layer covering the surface of the substrate. The receiving unit can be a wafer transfer robot or a wafer loading port, capable of automatically or semi-automatically removing the wafer under test from the wafer cassette and transferring it to subsequent process units. The receiving unit may be equipped with an alignment mechanism to ensure accurate transfer and positioning of the wafer between process units.
[0094] The ion implantation unit 92 is used to perform ion implantation on the wafer under test. The ion implantation unit includes components such as an ion source, a mass analyzer, an accelerating tube, a scanning system, and a terminal chamber. The ion source generates the required ion beam, the mass analyzer (e.g., a magnetic analyzer) performs mass screening to select the target ion species, the accelerating tube accelerates the ions to the required energy, the scanning system uniformly scans the ion beam across the wafer surface, and the terminal chamber holds the wafer and maintains the vacuum environment required for implantation. The ion implantation unit can automatically execute the ion implantation process according to preset implantation parameters (ion species, energy, dose, etc.).
[0095] Epitaxial unit 93 is used to remove the first barrier layer and form an epitaxial layer on the substrate surface. Specifically, epitaxial unit 93 may include a photoresist removal subunit and an epitaxial growth subunit. The photoresist removal subunit performs barrier layer removal processes, such as plasma ashing chambers and wet cleaning tanks, to remove barrier layer materials such as photoresist and clean the substrate surface. The epitaxial growth subunit is an epitaxial deposition reaction chamber, such as a depressurized chemical vapor deposition (RPCVD) reaction chamber, equipped with subsystems for temperature control, pressure control, and gas flow control, and is capable of growing epitaxial layer materials such as germanium and silicon on the substrate surface. Parameters such as temperature, pressure, gas flow rate, and growth time for epitaxial growth can be set according to the epitaxial layer material and target thickness.
[0096] The detection unit 94 is used to detect the thickness of the epitaxial layer. The detection unit 94 can be a measuring device such as an ellipsometer, X-ray reflectometer, scanning electron microscope, or transmission electron microscope. The detection unit can accurately measure the thickness of the epitaxial layer, compare the measurement result with a preset target thickness, and output a penetration determination result. The detection unit can be equipped with a data processing module to automatically complete the thickness comparison and penetration determination, and generate a detection report.
[0097] The aforementioned functional units can achieve automatic transfer of wafers between units through a wafer transfer system, forming an automated inspection pipeline suitable for online inspection on production lines.
[0098] By employing the above technical solution, the barrier layer penetration detection device of the present invention achieves fully automated operation from wafer reception to penetration detection through the coordinated cooperation of various functional units. This device can be integrated into semiconductor production lines to perform real-time penetration risk verification on process wafers in online operation, eliminating the need to send wafers to offline laboratories for SIMS or other tests. This significantly shortens the detection cycle, reduces detection costs, and ensures the accuracy and reliability of the detection results.
[0099] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A method for detecting barrier layer penetration, characterized in that, include: A wafer to be tested is provided, the wafer to be tested comprising: a substrate and a first barrier layer covering the surface of the substrate; An ion implantation process is performed on the wafer to be tested; Remove the first barrier layer and form an epitaxial layer on the substrate surface; The thickness of the epitaxial layer is detected to determine whether the implanted ions penetrate the first barrier layer during the ion implantation process.
2. The barrier layer penetration detection method as described in claim 1, characterized in that, The ion implantation process uses heavy ions.
3. The barrier layer penetration detection method as described in claim 2, characterized in that, The heavy ions include arsenic ions.
4. The barrier layer penetration detection method as described in claim 1, characterized in that, The epitaxial layer is made of germanium-silicon.
5. The barrier layer penetration detection method as described in claim 1, characterized in that, The material of the first barrier layer is photoresist.
6. The barrier layer penetration detection method as described in claim 1, characterized in that, The substrate includes: a substrate.
7. The barrier layer penetration detection method as described in claim 6, characterized in that, The substrate further includes at least one film layer formed on the substrate and having a pattern.
8. The barrier layer penetration detection method according to any one of claims 1 to 7, characterized in that, Detecting the thickness of the epitaxial layer to determine whether implanted ions penetrate the first barrier layer during the ion implantation process includes: When the thickness of the epitaxial layer is less than the target thickness, it is determined that the implanted ions in the ion implantation process penetrate the first barrier layer; otherwise, it is determined that the implanted ions in the ion implantation process have not penetrated the first barrier layer.
9. A method for forming a semiconductor structure, characterized in that, include: The thickness of the second barrier layer is determined and the second barrier layer is formed by using the barrier layer penetration detection method in the ion implantation process according to any one of claims 1 to 8; The second barrier layer covers the non-target area of the substrate surface and exposes the target area; An ion implantation process is performed on the target region.
10. A barrier layer penetration detection method and apparatus, characterized in that, include: A receiving unit is adapted to receive a wafer under test, the wafer under test comprising: a substrate and a first barrier layer covering the surface of the substrate; An ion implantation unit is adapted to perform an ion implantation process on the wafer under test. An epitaxial unit is adapted to remove the first barrier layer and form an epitaxial layer on the surface of the substrate; And a detection unit, adapted to detect the thickness of the epitaxial layer, so as to determine whether the implanted ions penetrate the first barrier layer during the ion implantation process.