A test structure for aluminum gallium nitride barrier layer thickness and a method of manufacturing the same
By using a stacked structure design with a single capacitor and a double dielectric layer, the problems of large area occupation and complex process in aluminum gallium nitride barrier layer thickness testing are solved, enabling efficient and accurate online monitoring, reducing costs and improving the reliability of test results.
Patent Information
- Application Number
- CN202611291104.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-20
AI Technical Summary
Existing methods for measuring the thickness of aluminum gallium nitride barrier layers have problems such as large wafer area requirements, complex processes, and high costs. In particular, the four-capacitor testing scheme occupies too much area, affecting production efficiency, and the multi-step lithography process increases the risk of process fluctuations.
A stacked structure design with a single capacitor and two dielectric layers is adopted. By combining two capacitance measurements with the thickness parameters of the two dielectric layers, a simultaneous equation is established to solve for the thickness of the aluminum gallium nitride barrier layer, which simplifies the process flow and reduces photolithography steps, requiring only one capacitance test unit.
It significantly reduces the area occupied by the test structure on the wafer, lowers manufacturing costs, and improves the reliability and accuracy of test results, making it suitable for online batch testing and automated data processing.
Smart Images

Figure CN123146192A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor technology, and in particular to a test structure for measuring the thickness of an aluminum gallium nitride barrier layer and a method for manufacturing the same. Background Technology
[0002] Currently, methods for measuring the thickness of the aluminum gallium nitride (AGaN) barrier layer mainly include direct observation via transmission electron microscopy (TEM), X-ray diffraction (XRD), and indirect calculation based on capacitance-voltage testing. While TEM offers high precision, it is a destructive test with high costs and long processing times, making it unsuitable for online monitoring in mass production. XRD, although non-destructive, requires sophisticated equipment, and its results are significantly affected by fluctuations in aluminum composition, making it difficult to accurately extract thickness information independently. Capacitance-voltage testing offers a more economical and practical online monitoring solution. A typical existing approach involves fabricating a four-parallel-plate capacitor structure, measuring the capacitance values of different structures, and then using the parallel-plate capacitance formula to inversely calculate the thickness of the AGaN barrier layer.
[0003] However, existing four-capacitor testing schemes have significant shortcomings. Firstly, the four independent capacitor structures require a large wafer testing area. For wafers where space is extremely limited, an excessively large testing area means a corresponding reduction in the area available for producing usable chips, hindering cost reduction. Secondly, the fabrication of the four capacitors requires multiple photolithography and deposition processes, resulting in a relatively complex structure and a lengthy process flow. This not only increases the manufacturing cost of the testing structure but also introduces more process fluctuations, potentially affecting the accuracy of the test results. Summary of the Invention
[0004] Therefore, it is necessary to provide a test structure for measuring the thickness of the aluminum gallium nitride barrier layer and its manufacturing method to address the aforementioned technical problems.
[0005] In a first aspect, this application discloses a method for fabricating a test structure for the thickness of an aluminum gallium nitride barrier layer, the method comprising the following steps:
[0006] A first dielectric layer and a first metal electrode are sequentially deposited on an epitaxial substrate containing a gallium nitride layer and an aluminum gallium nitride barrier layer. The first dielectric layer, the first metal electrode, and the two-dimensional electron gas below together constitute a first capacitor.
[0007] The capacitance value of the first capacitor was measured.
[0008] A second dielectric layer is deposited on the first metal electrode, and a second metal electrode is fabricated. The second dielectric layer, the second metal electrode, and the first capacitor below are connected in series to form a second capacitor.
[0009] The capacitance value of the second capacitor was measured.
[0010] The thickness of the aluminum gallium nitride barrier layer was obtained based on the capacitance values measured twice and the thickness parameters of the two dielectric layers.
[0011] Furthermore, the first capacitor is composed of an aluminum gallium nitride barrier layer capacitor and a first dielectric layer capacitor connected in series, and the capacitance value of the first capacitor corresponds to the equivalent series capacitance of the aluminum gallium nitride barrier layer and the first dielectric layer acting together.
[0012] Furthermore, the second capacitor is composed of the first capacitor and the second dielectric layer capacitor connected in series, and the capacitance value of the second capacitor corresponds to the equivalent series capacitance of the aluminum gallium nitride barrier layer, the first dielectric layer and the second dielectric layer acting together.
[0013] Furthermore, before depositing the first dielectric layer, an ohmic contact electrode is first fabricated in the edge region of the aluminum gallium nitride barrier layer. The ohmic contact electrode penetrates the first dielectric layer and directly contacts the aluminum gallium nitride barrier layer.
[0014] Furthermore, obtaining the thickness of the aluminum gallium nitride barrier layer based on the capacitance values measured twice and the thickness parameters of the two dielectric layers includes: establishing a simultaneous equation to obtain the thickness of the aluminum gallium nitride barrier layer, wherein the thickness of the aluminum gallium nitride barrier layer is equal to the thickness of the second dielectric layer multiplied by the second capacitance value and then divided by the difference between the first capacitance value and the second capacitance value.
[0015] On the other hand, this application also discloses a test structure for the thickness of an aluminum gallium nitride barrier layer, including:
[0016] Semiconductor substrate;
[0017] A gallium nitride epitaxial layer is formed on the substrate;
[0018] An aluminum gallium nitride barrier layer is formed on the gallium nitride epitaxial layer, and a two-dimensional electron gas is formed at the heterojunction interface between the aluminum gallium nitride barrier layer and the gallium nitride layer.
[0019] A first dielectric layer, a first metal electrode, a second dielectric layer, and a second metal electrode are sequentially stacked on top of the aluminum gallium nitride barrier layer.
[0020] And an ohmic contact electrode, which is directly electrically connected to the aluminum gallium nitride barrier layer;
[0021] The first dielectric layer and the first metal electrode together with the two-dimensional electron gas below form a first capacitor, and the second dielectric layer and the second metal electrode together with the first capacitor below form a second capacitor.
[0022] Furthermore, the first and second dielectric layers are made of any one of silicon nitride, aluminum oxide, or hafnium oxide, and both dielectric layers use the same dielectric material.
[0023] Furthermore, the silicon-rich silicon oxide pad layer has a silicon-to-oxygen ratio greater than the stoichiometric ratio of silicon oxide and is in a compressive stress state, and the silicon-rich silicon oxide pad layer is a chemically deposited layer formed without applying bias voltage.
[0024] Furthermore, both the first and second metal electrodes are parallel plate electrode structures, with the upper and lower electrodes having the same area and being aligned vertically. The electrode material is any one or a combination of titanium, tungsten, molybdenum, or aluminum.
[0025] Furthermore, the ohmic contact electrode is disposed in the edge region of the test structure, and the ohmic contact electrode penetrates the first dielectric layer and directly contacts the surface of the aluminum gallium nitride barrier layer, serving as the bottom electrode lead-out terminal for capacitance testing.
[0026] Furthermore, it also includes an isolation structure arranged around the active region of the test structure, which electrically isolates the test capacitor region from other surrounding devices or the test structure.
[0027] The aforementioned test structure and manufacturing method for the aluminum gallium nitride (AGaN) barrier layer thickness achieve the following beneficial effects: This application adopts a stacked structure design with a single capacitor and dual dielectric layers. Only one capacitor test unit is needed to perform two capacitance measurements with different equivalent dielectric thicknesses. The thickness of the AGaN barrier layer is solved by simultaneously solving two equations. Compared with the traditional four-capacitor scheme, the test structure of this invention occupies a significantly reduced wafer area, only about one-quarter or even less of the original scheme, effectively saving valuable wafer area resources and reducing testing costs. In terms of process, this application adopts a stacked fabrication method, with two dielectric layers and two metal layers deposited sequentially. The process flow is simple, eliminating the need for multiple photolithography steps to fabricate four independent capacitors, significantly reducing process complexity and minimizing error accumulation caused by multiple photolithography alignments, thus improving the reliability of test results. Furthermore, the test principle of this application is clear, and the calculation method is simple and direct. The thickness of the AGaN barrier layer can be quickly calculated using only two capacitance measurements and the known thickness of the second dielectric layer, facilitating online batch testing and automatic data processing. Simulation results show that, under typical conditions of 17% aluminum content and 17 nm aluminum gallium nitride thickness, the capacitance value measured by the test structure of this invention is highly consistent with the theoretical calculation results, verifying the feasibility and accuracy of the structural scheme. Attached Figure Description
[0028] Figure 1 This is a schematic flowchart illustrating a method for fabricating a test structure for measuring the thickness of an aluminum gallium nitride barrier layer, as disclosed in one embodiment.
[0029] Figure 2 This is a side view of a test structure for the thickness of an aluminum gallium nitride barrier layer, as disclosed in one embodiment.
[0030] Figure 3 This is a top view schematic diagram of a test structure for the thickness of an aluminum gallium nitride barrier layer disclosed in one embodiment;
[0031] Figure 4 Capacitor for device simulation in one embodiment Voltage curve. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.
[0033] Example 1
[0034] In one embodiment, such as Figure 1 As shown, a method for fabricating a test structure for the thickness of an aluminum gallium nitride barrier layer is disclosed. The method includes the following steps:
[0035] S1: A first dielectric layer and a first metal electrode are sequentially deposited on an epitaxial substrate containing a gallium nitride layer and an aluminum gallium nitride barrier layer. The first dielectric layer, the first metal electrode, and the two-dimensional electron gas below together constitute a first capacitor.
[0036] S2: Measure the capacitance value of the first capacitor;
[0037] S3: Continue to deposit a second dielectric layer on the first metal electrode and fabricate a second metal electrode. The second dielectric layer, the second metal electrode and the first capacitor below are connected in series to form a second capacitor.
[0038] S4: Measure the capacitance value of the second capacitor;
[0039] S5: Based on the capacitance values measured twice and the thickness parameters of the two dielectric layers, the thickness of the aluminum gallium nitride barrier layer is obtained.
[0040] This embodiment details the method for testing the thickness of the aluminum gallium nitride barrier layer according to the present invention and its specific process steps. The fabrication process of the entire test structure mainly includes the following steps: epitaxial substrate preparation, isolation structure fabrication, ohmic contact formation, first dielectric deposition, first metal electrode fabrication, first capacitance test, second dielectric deposition, second metal electrode fabrication, second capacitance test, and solving simultaneous equations. Each step is explained below with reference to specific process parameters.
[0041] Before step S1, the epitaxial substrate is prepared. This step includes selecting silicon, silicon carbide, or sapphire as the semiconductor substrate; in this embodiment, a silicon substrate is preferred. First, a gallium nitride (GaN) epitaxial layer is grown on the substrate. The GaN layer has a thickness of approximately 1 to 3 micrometers and is typically grown using a metal-organic chemical vapor deposition (MOCVD) process. The GaN layer is unintentionally doped intrinsic GaN with a low carrier concentration. Above the GaN epitaxial layer, an aluminum gallium nitride (AGaN) barrier layer is grown. The AGaN barrier layer has an aluminum content of approximately 15% to 25%, and in this embodiment, an aluminum content of 17% is preferred. The thickness of the AGaN barrier layer is approximately 10 to 30 nanometers, and in this embodiment, the target thickness is approximately 17 nanometers. The AGaN barrier layer is also grown using a metal-organic chemical vapor deposition (MOCVD) process.
[0042] Due to lattice mismatch and piezoelectric polarization effects between gallium nitride (GaN) and aluminum gallium nitride (AlGaN), a highly concentrated two-dimensional electron gas forms at the heterojunction interface between the two, i.e., on the GaN side. The areal density of this two-dimensional electron gas is approximately 5 × 10¹² to 1.5 × 10¹³ electrons per square centimeter, and its mobility is approximately 1000 to 2000 square centimeters per volt-second. This two-dimensional electron gas is used as the bottom electrode of a parallel-plate capacitor in the test structure of this invention.
[0043] In this embodiment, before depositing the first dielectric layer, an isolation structure is fabricated, and ohmic contact electrodes are created at the edge region of the aluminum gallium nitride (AGaN) barrier layer. To electrically isolate the test capacitor area from other surrounding structures, an isolation structure is required. Ion implantation isolation or mesa etching isolation can be used. This embodiment employs a mesa etching scheme. The active region of the test structure is defined by photolithography, and then inductively coupled plasma etching (ICP-CPE) is used to etch away the AGaN and part of the gallium nitride surrounding the active region, forming an isolation trench of a certain depth. This cuts off the conductive path of the two-dimensional electron gas, thereby achieving electrical isolation. The depth of the isolation etching is approximately 100 nm to 300 nm, requiring complete penetration of the AGaN barrier layer and a certain depth into the gallium nitride layer to ensure reliable isolation. The isolation structure is arranged around the entire test capacitor area, forming a closed isolation ring.
[0044] In this embodiment, the fabrication of the ohmic contact electrode includes: fabricating an ohmic contact electrode in the edge region of the test structure, serving as the lead-out terminal for the two-dimensional electron gas, i.e., the bottom electrode, during capacitance testing. First, the window position of the ohmic contact is defined by photolithography, with the window located on the aluminum gallium nitride (AGL) surface region inside the isolation structure. Then, the ohmic contact metal is deposited, typically using a multilayer metal stack structure such as titanium / aluminum / nickel / gold or titanium / aluminum / titanium / gold, with a total thickness of approximately several hundred nanometers. After metal deposition, the photoresist is stripped, retaining the metal pattern in the window region. Next, a rapid thermal annealing process is performed at approximately 800°C to 900°C for approximately 30 to 60 seconds under a nitrogen atmosphere. The high-temperature annealing causes an alloying reaction between the metal and AGL, forming a low-resistance ohmic contact. The specific contact resistance of the ohmic contact should be controlled within ohms per square millimeter. The following is to ensure the accuracy of the test.
[0045] Step S1 includes the deposition of the first dielectric layer. After the ohmic contact is fabricated, the first dielectric layer is deposited on the entire wafer surface. The dielectric material can be silicon nitride, aluminum oxide, or hafnium oxide, etc., and silicon nitride is preferred in this embodiment. Silicon nitride is deposited using plasma-enhanced chemical vapor deposition at a temperature of approximately 300 to 400 degrees Celsius. The thickness of the first dielectric layer is set to approximately 500 nanometers. The thickness of the dielectric layer needs to be precisely controlled because its thickness is one of the known parameters for solving subsequent simultaneous equations, and the accuracy of the thickness directly affects the final calculation results. The dielectric layer thickness can be monitored and calibrated online using equipment such as an ellipsometry to ensure that the thickness error is controlled within 2%. The first dielectric layer covers the aluminum gallium nitride barrier layer and also covers the ohmic contact region. Subsequently, photolithography etching is needed to open the dielectric layer above the ohmic contact to expose the electrodes.
[0046] Step S1 also includes the fabrication of the first metal electrode layer. After the first dielectric layer is deposited, the first metal electrode layer is fabricated. First, the upper electrode pattern of the first capacitor is defined by photolithography. The electrode has a square structure, and the overall size of the first electrode layer and dielectric region is 200 micrometers by 200 micrometers. The effective electrode area is precisely calculated based on the actual pattern. The electrode area needs to be precisely known because the electrode area parameter is required in the parallel plate capacitor calculation formula. After photolithography, the first metal electrode material is deposited using sputtering or evaporation processes. The metal material can be titanium, aluminum, tungsten, molybdenum, etc. In this embodiment, a titanium / aluminum stacked structure is preferred, with a total thickness of approximately 200 nanometers to 500 nanometers. After metal deposition, the photoresist is stripped to form the first metal electrode pattern. The first metal electrode layer is located in the central region above the first dielectric layer, and together with the two-dimensional electron gas below, the first dielectric layer, and the aluminum gallium nitride barrier layer in the middle, constitutes the first capacitor. From the perspective of equivalent circuit analysis, the first capacitor is actually the equivalent capacitor of the aluminum gallium nitride barrier layer capacitor and the first dielectric layer capacitor connected in series. After the first metal layer is fabricated, photolithography etching is needed to open the dielectric layer of the ohmic contact region, exposing the ohmic contact metal for subsequent probe testing. Reactive ion etching (RIE) is used to selectively remove the silicon nitride dielectric. The distance between the ohmic contact region and the first electrode region is approximately 10 micrometers.
[0047] Step S2 includes the first capacitance test. After the first layer of metal electrodes is fabricated, the first capacitance measurement is performed. Testing. Using a capacitance-voltage tester or impedance analyzer, two probes are placed in contact with the first metal electrode and the ohmic contact electrode, respectively, and the capacitance between them is measured under a certain bias voltage. The test frequency is typically 1 MHz, and the test voltage range can be scanned from 0 volts to 10 volts to obtain a capacitance-voltage curve. Because the test structure operates near the flat band of the accumulation or depletion region, the capacitance value changes relatively smoothly with voltage; therefore, the capacitance value at zero bias is usually selected as the capacitance. The value of . Under the simulation conditions of this embodiment, the first capacitor . The typical value is approximately 3.56 picofarads. The first capacitance measurement corresponds to the equivalent capacitance of the two dielectric layers, namely the aluminum gallium nitride barrier layer and the first silicon nitride dielectric layer, connected in series. According to the series capacitance formula for parallel plates, the reciprocal of the first capacitance is equal to the reciprocal of the aluminum gallium nitride barrier layer capacitance plus the reciprocal of the first dielectric layer capacitance, that is:
[0048]
[0049] Where d_AlGaN is the thickness of the aluminum gallium nitride barrier layer, i.e., the unknown quantity to be determined, and ε_AlGaN is the relative permittivity of aluminum gallium nitride. The thickness of the first dielectric layer is a known quantity, ε_SiN is the relative permittivity of silicon nitride, and S is the electrode area.
[0050] Step S3 includes the deposition of a second dielectric layer. After the first capacitance test is completed, a second dielectric layer is deposited on the wafer surface. The material of the second dielectric layer can be the same as or different from the first dielectric layer. To simplify calculations, this embodiment uses the same silicon nitride material as the first layer. The deposition process also employs plasma-enhanced chemical vapor deposition. The thickness of the second dielectric layer is set to approximately 200 nanometers. This thickness also needs to be precisely controlled and measured, serving as another known parameter in the simultaneous equations. The second dielectric layer covers the dielectric surface above and around the first metal electrode.
[0051] Step S3 also includes the fabrication of a second metal electrode. After the second dielectric layer is deposited, the second metal electrode is fabricated. The upper electrode pattern of the second capacitor is defined by photolithography. The overall size of the second electrode and dielectric region is also 200 micrometers by 200 micrometers. The electrode shape and area are consistent with the first metal electrode, and they are strictly aligned vertically to ensure that the effective electrode area remains unchanged. The second metal material is deposited, and the material type is the same as or similar to the first metal layer. In this embodiment, a titanium / aluminum stack is also used. After the photoresist is stripped, the second metal electrode is formed. The second metal electrode is located above the second dielectric layer and is connected in series with the first capacitor structure below to form the second capacitor.
[0052] Step S4 includes a second capacitance test. After the second layer of metal electrodes is fabricated, a second capacitance measurement is performed. Test. The test method is the same as the first time. The probe is contacted with the second metal electrode and the ohmic contact electrode respectively, and the capacitance value under zero bias is read as... The second capacitance measurement corresponds to the equivalent capacitance of the three dielectric layers: the aluminum gallium nitride barrier layer, the first silicon nitride layer, and the second silicon nitride layer connected in series. The series connection formula is:
[0053]
[0054] Where Δd is the thickness of the second dielectric layer, that is, the increase in dielectric thickness between the two measurements, which is a known quantity.
[0055] Step S5 includes solving simultaneous equations to determine the aluminum gallium nitride thickness; specifically, obtaining... and After considering the two capacitance values, and combining them with the known thickness of the first dielectric layer... The thickness d_AlGaN of the aluminum gallium nitride barrier layer can be obtained by solving the above two equations simultaneously, given the thickness Δd of the second dielectric layer and the dielectric constant parameter of the dielectric.
[0056] Subtracting the two equations eliminates the part other than the aluminum gallium nitride term, and after simplification and derivation, we get:
[0057]
[0058] When both dielectric layers are made of the same material, the ratio of their dielectric constants is 1, and the formula further simplifies to:
[0059]
[0060] Substituting the simulation values from this embodiment: Δd equals 200 nanometers. Equals 3.56 picofarads. Equal to 2.45 picofarads, the aluminum gallium nitride thickness can be calculated to be approximately 17 nanometers. Figure 4 The publicly available simulation results, showing the capacitance-voltage curves, demonstrate that the thickness matches the target thickness obtained from epitaxial growth, validating the method's accuracy. The aforementioned calculations can be automated using testing software, enabling real-time output of test data. In actual mass production monitoring, only two capacitance values need to be obtained to quickly calculate the actual thickness of the aluminum gallium nitride barrier layer on the wafer, facilitating process monitoring and yield analysis.
[0061] It should be noted that the above embodiments are illustrated using a two-layer dielectric as an example. The principle of the present invention can also be extended to three-layer, four-layer, or even more-layer dielectrics. By depositing and testing layer by layer, multiple capacitance measurements can be obtained, more equations can be constructed, and multiple unknown parameters such as the aluminum gallium nitride thickness, the thickness of each dielectric layer, and the dielectric constant can be solved simultaneously, further improving the comprehensiveness and accuracy of the test.
[0062] Example 2
[0063] like Figure 2 and Figure 3 As shown, this embodiment describes in detail the test structure for the thickness of the aluminum gallium nitride barrier layer of the present invention from the perspective of product structure. The test structure described in this embodiment corresponds to the product structure prepared by the manufacturing method described in Embodiment 1, and the two correspond to each other in technical features.
[0064] The test structure for measuring the thickness of the aluminum gallium nitride (AGaN) barrier layer is a stacked structure with a single capacitor and two dielectric layers. It mainly comprises a semiconductor substrate, a gallium nitride epitaxial layer, an AGaN barrier layer, a two-dimensional electron gas, an isolation structure, a first dielectric layer, a first metal electrode, a second dielectric layer, a second metal electrode, and an ohmic contact electrode. The structure of each part and their interrelationships are described below.
[0065] I. Substrate and Epitaxial Layer Structure
[0066] The semiconductor substrate can be a silicon substrate, a silicon carbide substrate, or a sapphire substrate; in this embodiment, a silicon substrate is used. The substrate thickness is approximately 500 to 700 micrometers, serving a mechanical support function. A gallium nitride epitaxial layer is formed on top of the substrate, with a thickness of approximately 1 to 3 micrometers, and is an unintentionally doped intrinsic gallium nitride material. The crystal quality of the gallium nitride layer directly affects the two-dimensional electron gas characteristics of the heterojunction interface; therefore, it is necessary to control the dislocation density at a low level. An aluminum gallium nitride barrier layer is formed on the upper surface of the gallium nitride epitaxial layer, with a thickness of approximately 10 to 30 nanometers and an aluminum content of approximately 15% to 25%. The aluminum gallium nitride barrier layer is the target of testing in this invention, and its thickness is an unknown parameter to be measured.
[0067] At the heterojunction interface between the aluminum gallium nitride (AlGaN) barrier layer and the gallium nitride (GaN) layer, a highly mobile two-dimensional electron gas is formed in the triangular potential well on the GaN side due to the combined effects of piezoelectric polarization and spontaneous polarization. The areal density of the two-dimensional electron gas is approximately 5 × 10¹² to 1.5 × 10¹³ electrons per square centimeter, located in the range of a few nanometers below the heterojunction interface. This two-dimensional electron gas is used as the bottom electrode of a parallel-plate capacitor and exhibits good conductivity.
[0068] II. Isolation Structure
[0069] An isolation structure is positioned around the active capacitance region of the test structure, forming a closed isolation ring. This isolation structure is formed using mesa etching, with the etching depth penetrating the aluminum gallium nitride barrier layer and entering the gallium nitride layer at a depth of approximately tens to hundreds of nanometers. This completely severs the two-dimensional electron gas conduction path between the active region and the surrounding area, achieving excellent electrical isolation. The width of the isolation structure is approximately several micrometers to tens of micrometers, ensuring a sufficiently large isolation resistance and preventing leakage or parasitic capacitance between the test capacitor and other surrounding structures, thus guaranteeing the accuracy of capacitance testing.
[0070] III. First dielectric layer and first capacitor structure
[0071] The first dielectric layer is formed on the upper surface of the aluminum gallium nitride barrier layer, covering the entire active region. The dielectric material is any one of silicon nitride, aluminum oxide, or hafnium oxide; in this embodiment, silicon nitride is used. The thickness of the first dielectric layer is approximately 500 nanometers, with thickness uniformity deviation controlled within 2%. The first metal electrode is formed at the center of the upper surface of the first dielectric layer, forming a parallel plate electrode structure. The electrode shape can be square, circular, or interdigitated; in this embodiment, a square electrode is used, with a side length of approximately 100 to 200 micrometers. The electrode area is a known precise value and is an important parameter in the capacitance calculation formula. The material of the first metal electrode is any one of titanium, aluminum, tungsten, or molybdenum, or a combination thereof; in this embodiment, a titanium / aluminum bilayer metal structure is used, with a total thickness of approximately 200 to 500 nanometers. The surface of the metal electrode is smooth, with clear edge contours.
[0072] The first capacitor is composed of a first metal electrode layer, a first dielectric layer, an aluminum gallium nitride (AGaN) barrier layer, and a two-dimensional electron gas. Viewed vertically, the first capacitor is a parallel-plate capacitor structure with multiple dielectric layers connected in series, where the dielectric portion consists of a first silicon nitride dielectric layer and an AGaN barrier layer connected in series. The capacitance value of the first capacitor is denoted as [value missing]. Its size is determined by the electrode area, the thickness of the two dielectric layers, and the dielectric constant.
[0073] IV. Second dielectric layer and second capacitor structure
[0074] The first dielectric layer is formed on the upper surface of the aluminum gallium nitride (AlGaN) barrier layer, covering the entire active region. The dielectric material can be any one of silicon nitride, aluminum oxide, or hafnium oxide; in this embodiment, silicon nitride is used. The thickness of the first dielectric layer is approximately 500 nanometers, with thickness uniformity deviation controlled within 2%. From a planar layout perspective, the dimensions of the first electrode and dielectric region are 200 micrometers by 200 micrometers, forming the core region of the first capacitor. The first metal electrode is formed at the center of the upper surface of the first dielectric layer, forming a parallel plate electrode structure. The electrode shape is square, corresponding to the dimensions of the first dielectric region. The electrode area is a known precise value and is an important parameter in the capacitance calculation formula.
[0075] The first layer of the metal electrode is made of any one of titanium, aluminum, tungsten, or molybdenum, or a combination thereof. In this embodiment, a titanium / aluminum bilayer metal structure is used, with a total thickness of approximately 200 to 500 nanometers. The surface of the metal electrode is smooth, and the edge contours are clearly defined.
[0076] The first capacitor is composed of a first metal electrode layer, a first dielectric layer, an aluminum gallium nitride (AGaN) barrier layer, and a two-dimensional electron gas. Viewed vertically, the first capacitor is a parallel-plate capacitor structure with multiple dielectric layers connected in series, where the dielectric portion consists of a first silicon nitride dielectric layer and an AGaN barrier layer connected in series. The capacitance value of the first capacitor is denoted as [value missing]. Its size is determined by the electrode area, the thickness of the two dielectric layers, and the dielectric constant.
[0077] V. Ohmic Contact Electrode
[0078] The ohmic contact electrode is positioned at the edge of the test structure, inside the isolation structure, with a spacing of approximately 10 micrometers from the first electrode layer. The ohmic contact electrode penetrates both the first and second dielectric layers, directly forming an ohmic contact with the surface of the aluminum gallium nitride barrier layer. The ohmic contact metal employs a multilayer alloy structure of titanium / aluminum / nickel / gold, which undergoes high-temperature annealing to create a low-resistance contact. As the lead-out terminal of the two-dimensional electron gas (bottom electrode), during capacitance testing, one end of the test probe contacts the top metal electrode, while the other end contacts the ohmic contact electrode, thus forming a complete capacitance test circuit. The specific contact resistance of the ohmic contact is sufficiently low to significantly affect the capacitance test results.
[0079] VI. Equivalent Circuit and Working Principle
[0080] From the perspective of equivalent circuit analysis, the overall test structure presents as three capacitors connected in series. The three capacitors are: an aluminum gallium nitride (AGaN) barrier layer capacitor, with AGaN as its dielectric material and a thickness to be measured; a first dielectric layer capacitor, with silicon nitride as its dielectric material and a known thickness; and a second dielectric layer capacitor, also with silicon nitride as its dielectric material and a known thickness. The first test was conducted when only the first metal layer was fabricated; at this point, only the AGaN capacitor and the first dielectric layer capacitor were connected in series, and the total capacitance was measured. After the second metal layer was fabricated, a second test was conducted. This time, all three capacitors were connected in series, and the total capacitance was measured. Since the thicknesses of both dielectric layers are known precise values, two equations are established using the two capacitance measurements. After simultaneously solving these equations to eliminate common parameters such as dielectric constant and area, the thickness of the aluminum gallium nitride barrier layer can be calculated. The calculation principle is simple and direct, and the results are reliable.
[0081] VII. Advantages in Structural Dimensions and Area
[0082] This test structure is a single stacked capacitor unit, with its planar dimensions primarily determined by the electrode area. Using a square electrode with a side length of 100 micrometers as a baseline, plus the surrounding ohmic contacts and isolation areas, the overall planar dimensions of the test structure are approximately 150 micrometers by 150 micrometers. Compared to the traditional four-capacitor approach, this invention requires only one capacitor unit to complete the test, occupying only about one-third to one-quarter of the wafer area, significantly saving wafer area occupied by the test pattern and offering a clear cost advantage for mass production monitoring. Furthermore, the stacked structure has relatively simple fabrication steps, involving the sequential deposition of two dielectric and two metal layers, eliminating the need for multiple photomasks to fabricate multiple independent capacitors, thus reducing process costs.
[0083] The aluminum gallium nitride barrier layer thickness testing structure described in this embodiment adopts a stacked design with a single capacitor and two dielectric layers. It has a compact structure, simple process, and clear testing principle. It can accurately measure the thickness of the aluminum gallium nitride barrier layer and is suitable for online process monitoring on gallium nitride device production lines.
[0084] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0085] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A method for fabricating a structure for measuring the thickness of an aluminum gallium nitride barrier layer, characterized in that, Includes the following steps: A first dielectric layer and a first metal electrode are sequentially deposited on an epitaxial substrate containing a gallium nitride layer and an aluminum gallium nitride barrier layer. The first dielectric layer, the first metal electrode, and the two-dimensional electron gas below together constitute a first capacitor. The capacitance value of the first capacitor was measured. A second dielectric layer is deposited on the first metal electrode, and a second metal electrode is fabricated. The second dielectric layer, the second metal electrode, and the first capacitor below are connected in series to form a second capacitor. The capacitance value of the second capacitor was measured. The thickness of the aluminum gallium nitride barrier layer was obtained based on the capacitance values measured twice and the thickness parameters of the two dielectric layers.
2. The method for preparing the test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 1, characterized in that, The first capacitor is composed of an aluminum gallium nitride barrier layer capacitor and a first dielectric layer capacitor connected in series. The capacitance value of the first capacitor corresponds to the equivalent series capacitance of the aluminum gallium nitride barrier layer and the first dielectric layer working together.
3. The method for preparing the test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 1, characterized in that, The second capacitor is composed of the first capacitor and the second dielectric layer capacitor connected in series. The capacitance value of the second capacitor corresponds to the equivalent series capacitance of the aluminum gallium nitride barrier layer, the first dielectric layer and the second dielectric layer working together.
4. The method for preparing the test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 1, characterized in that, Before depositing the first dielectric layer, an ohmic contact electrode is fabricated in the edge region of the aluminum gallium nitride barrier layer. The ohmic contact electrode penetrates the first dielectric layer and makes direct contact with the aluminum gallium nitride barrier layer.
5. The method for preparing the test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 1, characterized in that, The process of obtaining the thickness of the aluminum gallium nitride barrier layer based on the capacitance values measured twice and the thickness parameters of the two dielectric layers includes: establishing a simultaneous equation to obtain the thickness of the aluminum gallium nitride barrier layer, wherein the thickness of the aluminum gallium nitride barrier layer is equal to the thickness of the second dielectric layer multiplied by the second capacitance value and then divided by the difference between the first capacitance value and the second capacitance value.
6. A test structure for the thickness of an aluminum gallium nitride barrier layer, characterized in that, include: Semiconductor substrate; A gallium nitride epitaxial layer is formed on the substrate; An aluminum gallium nitride barrier layer is formed on the gallium nitride epitaxial layer, and a two-dimensional electron gas is formed at the heterojunction interface between the aluminum gallium nitride barrier layer and the gallium nitride layer. A first dielectric layer, a first metal electrode, a second dielectric layer, and a second metal electrode are sequentially stacked on top of the aluminum gallium nitride barrier layer. And an ohmic contact electrode, which is directly electrically connected to the aluminum gallium nitride barrier layer; The first dielectric layer and the first metal electrode together with the two-dimensional electron gas below form a first capacitor, and the second dielectric layer and the second metal electrode together with the first capacitor below form a second capacitor.
7. The test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 6, characterized in that, The first and second dielectric layers are made of any one of silicon nitride, aluminum oxide, or hafnium oxide, and both dielectric layers use the same dielectric material.
8. The test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 6, characterized in that, Both the first and second metal electrodes are parallel plate electrode structures, with the upper and lower electrodes having the same area and being aligned vertically. The electrode material is any one or a combination of titanium, tungsten, molybdenum, or aluminum.
9. The test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 6, characterized in that, The ohmic contact electrode is disposed in the edge region of the test structure. The ohmic contact electrode penetrates the first dielectric layer and directly contacts the surface of the aluminum gallium nitride barrier layer, serving as the bottom electrode lead-out terminal for capacitance testing.
10. The test structure for the thickness of the aluminum gallium nitride barrier layer according to claim 11, characterized in that, It also includes an isolation structure that surrounds the active region of the test structure and electrically isolates the test capacitor region from other surrounding devices or the test structure.