Method and system for monitoring low to medium temperature thermal anneal temperature of wafers in a thermal anneal tool

By ion-implanted wafers with a non-metallic doped layer formed on the surface of silicon wafers, the problems of complex steps and uniformity in low-temperature rapid annealing processes in all-metal layer wafer monitoring have been solved. This enables sensitive and accurate monitoring of low-temperature thermal annealing temperatures, improving the applicability of product wafers and the safety of equipment.

CN123146201APending Publication Date: 2026-11-20SHENZHEN JINGWEI KAIWU INSTR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611646922.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In semiconductor manufacturing, existing technologies employing low-temperature rapid annealing processes for all-metal layer wafer monitoring suffer from complex steps, poor coating uniformity, and uneven heating due to non-uniform reflectivity, which affects wafer yield and damages equipment.

Method used

Ion-implanted wafers are used instead of all-metal wafers. By forming a non-metallic doped layer on the surface of the silicon wafer, the thermal annealing temperature is monitored, simplifying the monitoring process and improving uniformity. The annealing temperature is inversely calculated using the linear relationship between sheet resistance and temperature.

Benefits of technology

It enables sensitive and accurate monitoring of medium and low temperature thermal annealing temperatures, simplifies the monitoring process, improves the applicability of product wafers and equipment safety, and reduces production risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146201A_ABST
    Figure CN123146201A_ABST
Patent Text Reader

Abstract

The application discloses a kind of methods and systems for monitoring the medium-low temperature thermal annealing temperature of wafer in thermal annealing machine, it is related to semiconductor manufacturing technology field.The technical scheme in the application is by using ion implantation wafer instead of full metal layer wafer, monitoring process is more simplified, ion implantation uniformity is obviously superior to physical vapor deposition uniformity, and ion implantation wafer reflectivity is also close to product wafer, and the rapid annealing temperature field monitored by ion implantation wafer is more applicable to product wafer than full metal layer wafer.Based on this, the application develops a complete temperature monitoring method, the temperature sensitivity of wafer annealing process under 450 DEG C to 600 DEG C is excellent, the reflection to temperature is sensitive and accurate, and the stability of sheet resistance with time after annealing is high, the retest RS offset is less than 1.5% after 6 days interval, the interference of wafer storage time after annealing to the accuracy of monitoring data is smaller, with greater measurement window.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing technology, and in particular to a method and system for monitoring the medium- and low-temperature thermal annealing temperature of wafers in a thermal annealing machine. Background Technology

[0002] In semiconductor manufacturing, 450℃ to 600℃ is a critical medium-low temperature rapid annealing process window. The semiconductor industry typically uses offline monitoring of wafers to promptly assess the normality of the rapid annealing process and controls the monitoring timeline. This ensures the safe and efficient execution of the rapid annealing process for product wafers. Related technologies using all-metal layer wafers face several challenges. First, the process is complex, requiring the removal of unreacted metals. Second, the surface reflection of all-metal layer wafers differs significantly from that of product wafers. Furthermore, all-metal layers rely entirely on the uniformity of physical vapor deposition (PVD), and poor uniformity leads to poor sheet resistance uniformity. Ultimately, the rapid annealing temperature field monitored using all-metal layer wafers is unsuitable for product wafers, resulting in low product yield and impacting production capacity. Summary of the Invention

[0003] The main objective of this invention is to develop a temperature monitoring method and system suitable for medium- and low-temperature thermal annealing processes of ion-implanted wafers.

[0004] To achieve the above objectives, this invention proposes a method for monitoring the medium-low temperature thermal annealing temperature of wafers within a thermal annealing machine, comprising the following steps: S10 provides silicon wafers, as well as standard curves for thermal annealing process temperature and sheet resistance; S20. Perform an ion implantation process on the silicon wafer to form a non-metallic doped layer on the surface of the silicon wafer, thereby obtaining the wafer to be monitored. S30. The wafer to be monitored is sent into a thermal annealing machine and a thermal annealing process with a preset process temperature is performed. S40. Measure the sheet resistance of the non-metallic doped layer and determine whether the measured sheet resistance value conforms to the standard curve; if yes, determine that the process temperature of the hot annealing machine is normal; if no, determine that the process temperature of the hot annealing machine is abnormal; in step S20, the ion implantation depth is 50nm~300nm; in step S30, the preset process temperature is 450℃~600℃.

[0005] In one embodiment, the standard curve is specifically a standard curve of the thermal annealing process temperature and sheet resistance of a non-metallic doped layer within a preset process temperature range. The determination method includes the following steps: Multiple silicon wafers from step S10 are provided, and the ion implantation process in step S20 is performed on each of them. The non-metallic doped layer is formed on the surface of each silicon wafer to produce multiple test wafers. Within the preset process temperature range, thermal annealing processes at different temperatures are performed on multiple test wafers, and then the sheet resistance of the non-metallic doped layer of each test wafer is measured. The standard curve was obtained by plotting the corresponding relationship between different thermal annealing process temperatures and the sheet resistance values ​​of non-metallic doped layers.

[0006] In one embodiment, the standard curve satisfies the following condition: Within the preset process temperature range, with a temperature deviation of ±20℃, the sheet resistance of the non-metallic doped layer exhibits a linear relationship, with a linear correlation coefficient greater than or equal to 0.99.

[0007] In one embodiment, the ion implantation dose is 5 × 10⁻⁶. 14 atoms / cm 2 ~5×10 15 atoms / cm 2 .

[0008] In one embodiment, the ion implantation energy is 15keV to 30keV.

[0009] In one embodiment, the ions used for ion implantation include boron ions.

[0010] In one embodiment, the volume resistivity of the wafer substrate to be monitored is 3Ω. cm~5Ω cm.

[0011] In one embodiment, step S40 specifically includes the following steps: The sheet resistance measured in step S40 is substituted into the standard curve to calculate the annealing temperature. The annealing temperature is then compared with the preset process temperature of the hot annealing machine in step S30, and the temperature difference is calculated. If the temperature difference is less than or equal to the allowable temperature deviation, the process temperature of the hot annealing machine is normal; if the temperature difference is greater than the allowable temperature deviation, the process temperature of the hot annealing machine is abnormal.

[0012] In one embodiment, after a 6-day interval between performing the thermal annealing process at the preset process temperature, the sheet resistance value of the non-metallic doped layer measured is less than 1.5% of the value before the interval.

[0013] This invention also proposes a system for monitoring the medium-low temperature thermal annealing of wafers in a thermal annealing machine, comprising: a process execution unit, the process execution unit including an ion implantation device and a thermal annealing machine, the ion implantation device being used to perform an ion implantation process on the wafer to form a doped layer on the wafer surface; the thermal annealing machine being used to perform a thermal annealing process on the wafer at a preset process temperature; a data detection unit, the data detection unit measuring the sheet resistance value of the doped layer on the wafer surface using a four-probe resistivity meter and / or a sheet resistance meter; and a data judgment unit, the data judgment unit being used to compare the measured sheet resistance value with a standard curve, calculate the annealing temperature, and further determine whether it is consistent with the machine's set temperature.

[0014] The technical solution in this invention simplifies the monitoring process by using ion-implanted wafers instead of all-metal layer wafers. Ion implantation uniformity is significantly better than physical vapor deposition uniformity, and the reflectivity of ion-implanted wafers is close to that of product wafers. The rapid annealing temperature field monitored using ion-implanted wafers is more suitable for product wafers than that of all-metal layer wafers. Based on this, this invention develops a complete temperature monitoring method with excellent temperature sensitivity to wafer annealing processes from 450℃ to 600℃. It provides a sensitive and accurate temperature response, and the sheet resistance after annealing exhibits high stability over time. After a 6-day interval, the RS offset is less than 1.5%. The placement time of the wafer after annealing has minimal impact on the accuracy of the monitoring data, and it has a larger measurement window. Attached Figure Description

[0015] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0016] Figure 1 This is a schematic flowchart of a temperature monitoring method for a medium-low temperature annealing process according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the formation of a non-metallic doped layer in one embodiment of the present invention; Figure 3 This is a D-SIMS longitudinal B concentration distribution curve of the wafer to be monitored in one embodiment of the present invention; Figure 4 This is a standard curve of the thermal annealing process temperature and sheet resistance in Embodiment 1 of the present invention; Figure 5 This is a standard curve of the thermal annealing process temperature and sheet resistance in Embodiment 2 of the present invention; Figure 6This is a standard curve of the thermal annealing process temperature and sheet resistance in Embodiment 3 of the present invention.

[0017] Explanation of reference numerals in the attached figures: 100, silicon wafer; 200, non-metallic doped layer.

[0018] The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0020] It should be noted that if the embodiments of the present invention involve directional indicators (such as up, down, left, right, front, back, etc.), the directional indicators are only used to explain the relative positional relationship and movement of the components in a specific posture. If the specific posture changes, the directional indicators will also change accordingly.

[0021] Furthermore, if the embodiments of this invention involve descriptions such as "first" or "second," these descriptions are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the use of "and / or" or "and / or" throughout the text includes three parallel solutions. For example, "A and / or B" includes solution A, solution B, or a solution where both A and B are satisfied simultaneously. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.

[0022] In this invention, the product wafer refers to the actual wafer used to manufacture chips. The product wafer needs to undergo annealing during the manufacturing process. Directly using the product wafer to debug the temperature field of the thermal annealing machine is too costly and risky. Therefore, a simulation wafer is needed to represent the product wafer.

[0023] The wafer to be monitored in this invention is the simulation wafer mentioned above. By measuring the response of the simulation wafer to the annealing process, the temperature distribution inside the furnace cavity is deduced, and then the equipment parameters are adjusted to make the temperature field consistent with the annealing temperature field requirements of the product wafer. The simulation wafer should be as close as possible to the thermal and optical behavior of the product wafer, and the temperature field obtained by the adjustment should be closer to the requirements of the product wafer.

[0024] The all-metal layer wafer in this invention is a type of analog wafer, with the silicon wafer surface typically covered by a continuous all-metal layer. In contrast, product wafers are significantly different, with the silicon wafer surface of product wafers typically having only a small number of metal patterns such as gates and metal electrodes.

[0025] The ion-implanted wafer in this invention is another type of analog wafer. Instead of depositing metal on the silicon wafer surface, a doped layer is introduced near the surface of the silicon wafer through ion implantation, thereby altering the thermal / optical properties of the silicon wafer, such as absorption and emission of annealing lamp radiation. The surface of the ion-implanted wafer is still silicon, not a metal layer; therefore, the surface reflectivity of the ion-implanted wafer is closer to that of the product wafer.

[0026] The technical problem solved by this invention is that in semiconductor manufacturing, 450°C to 600°C is a critical medium-low temperature rapid annealing process window; the semiconductor industry generally uses offline monitoring to promptly assess whether the rapid annealing process is normal, while controlling the monitoring timeliness, so as to ensure that the rapid annealing process of product wafers is carried out safely and efficiently.

[0027] The offline monitoring solution in related technologies uses all-metal layer wafers, requiring at least three process steps: physical vapor deposition (PVD) coating, rapid annealing, wet etching to remove unreacted metal, and sheet resistance measurement. Because product wafers have photolithographic patterns, the metal area is very low after photolithography and etching, resulting in significant differences in surface reflection between all-metal layer wafers and product wafers. Furthermore, the all-metal layer relies entirely on the uniformity of the PVD coating; poor reflectivity and thickness uniformity will lead to poor sheet resistance uniformity during annealing. Adjusting the sheet resistance uniformity of all-metal layer wafers by adjusting the rapid annealing temperature field can easily lead to over-adjustment of the rapid annealing temperature field, ultimately causing the rapid annealing temperature field used for all-metal layer wafer monitoring to be unsuitable for product wafers. In severe cases, uneven reflectivity leading to uneven heating may ultimately cause wafer breakage and damage to components within the rapid annealing equipment chamber.

[0028] To address the aforementioned technical problems, this invention proposes a method for monitoring the medium-to-low temperature thermal annealing temperature of wafers within a thermal annealing machine, such as... Figure 1 and Figure 2 As shown, it includes the following steps: S10 provides silicon wafer 100, as well as standard curves for thermal annealing process temperature and sheet resistance; S20. Perform an ion implantation process on the silicon wafer 100 to form a non-metallic doped layer 200 on the surface of the silicon wafer 100, thereby obtaining the wafer to be monitored. S30. The wafer to be monitored is sent into a thermal annealing machine and a thermal annealing process with a preset process temperature is performed. S40. Measure the sheet resistance of the non-metallic doped layer 200 and determine whether the measured sheet resistance value conforms to the standard curve; if yes, determine that the process temperature of the hot annealing machine is normal; if no, determine that the process temperature of the hot annealing machine is abnormal. In step S20, the ion implantation depth is 50nm~300nm; In step S30, the preset process temperature is 450℃~600℃.

[0029] It should be noted that the wafer to be monitored in this invention is a simulation of the product wafer. This invention uses the wafer to be monitored instead of the product wafer to enter the hot annealing machine, measures the response of the wafer to be monitored to the annealing process, and deduces the temperature field in the furnace cavity to determine whether the temperature field in the existing hot annealing machine meets the requirements of the hot annealing temperature field of the product wafer.

[0030] The wafer to be monitored in this invention is an ion-implanted wafer. Ion implantation forms a non-metallic doped layer 200 on the surface of the silicon wafer 100. This doped layer undergoes activation of doped atoms and repair of lattice damage during thermal annealing. The annealing temperature directly determines the activation rate of doped atoms and the mobility of charge carriers, thereby determining the sheet resistance of the doped layer. By establishing a standard curve between annealing temperature and sheet resistance in advance, the annealing temperature can be inferred from the sheet resistance value during actual monitoring, thus determining whether the process temperature of the thermal annealing machine is abnormal.

[0031] Optionally, the silicon wafer 100 can be a bare die, a silicon wafer processed by epitaxial growth, or a circuit layer with devices already formed on it. Optionally, the silicon wafer 100 may include, but is not limited to, an SOI substrate, a bulk silicon substrate, a germanium substrate, a germanium-silicon substrate, an indium phosphide substrate, a gallium arsenide substrate, or a germanium-on-insulator substrate.

[0032] It should also be noted that, compared with all-metal layer wafers, the technical solution of this invention has the following significant advantages: First, the preparation of ion-implanted wafers only requires one ion implantation step, without the need for physical vapor deposition coating and wet etching to remove unreacted metals, making the monitoring process simpler; Second, the uniformity of ion implantation is significantly better than that of physical vapor deposition, because ion implantation is achieved by controlling the ion beam scanning with an electromagnetic field, and its dose uniformity can be controlled within ±1%, while the thickness uniformity of physical vapor deposition is usually ±3% to ±5%; Third, the surface reflectivity of ion-implanted wafers is close to that of product wafers. The surface of product wafers is a silicon substrate and a small amount of metal patterns, and the surface of ion-implanted wafers is also a silicon substrate. Therefore, the rapid annealing temperature field monitored by ion-implanted wafers can more accurately reflect the annealing conditions of product wafers compared to all-metal layer wafers.

[0033] When the ion implantation depth of the monitored wafer is 50nm to 300nm, the boron concentration exhibits a linear relationship with the depth, and the concentration gradient remains essentially constant. This ensures that the diffusion flux and redistribution of boron during annealing are primarily controlled by temperature. Furthermore, the preset process temperature for thermal annealing is 450℃ to 600℃. Within this temperature range, the activation process of boron ion implantation into silicon is highly sensitive to temperature. Under these dual conditions, the sheet resistance of the non-metallic doped layer 200 exhibits a strong linear relationship with the annealing temperature. By measuring the change in sheet resistance after annealing and comparing it with a standard curve, it is possible to sensitively and repeatedly determine whether the temperature of the thermal annealing machine is abnormal. Specific preset process temperatures for thermal annealing can be 450℃, 480℃, 510℃, 540℃, 570℃, 600℃, etc., as long as they fall within the above range.

[0034] In one embodiment, the standard curve is specifically a standard curve of the thermal annealing process temperature and sheet resistance of a non-metallic doped layer within a preset process temperature range; The method for determining the standard curve includes the following steps: Multiple silicon wafers 100 from step S10 are provided, and the ion implantation process in step S20 is performed on each of them, and the non-metallic doped layer is formed on the surface of each silicon wafer 100 to produce multiple test wafers. Within the preset process temperature range, thermal annealing processes at different temperatures are performed on multiple test wafers, and then the sheet resistance of the non-metallic doped layer of each test wafer is measured. Based on the correspondence between different thermal annealing process temperatures and the sheet resistance values ​​of non-metallic doped layers, the standard curve is plotted with annealing temperature as the abscissa and sheet resistance as the ordinate.

[0035] It should be noted that the test wafer and the wafer to be monitored in this embodiment are the same wafer. The purpose of the test wafer is to obtain an accurate standard curve through multiple tests; while the purpose of the wafer to be monitored is to serve as a simulation wafer to directly provide feedback on whether the temperature of the thermal annealing machine meets the requirements.

[0036] The surface of a silicon wafer after ion implantation contains numerous lattice damages and interstitial dopants. During thermal annealing, as the temperature increases, dopants migrate from interstitial sites to substitutional sites, while lattice damage is gradually repaired. Activated dopants provide free charge carriers, increasing the carrier concentration; simultaneously, the repair of lattice damage reduces carrier scattering and improves carrier mobility. The sheet resistance Rs is related to the carrier concentration n and mobility μ by the formula Rs = 1 / (q·μ·n·xj), where q is the elementary charge and xj is the doped junction depth. Therefore, the higher the annealing temperature, the higher the activation rate of dopants, the more complete the lattice damage repair, and the lower the sheet resistance. This temperature-sheet resistance correspondence exhibits good linearity within a certain temperature range, forming the physical basis of this monitoring method.

[0037] In one embodiment, when the preset process temperature difference is not less than 60°C, the temperature points corresponding to the test wafer are not less than 3, and can be 3, 4, 5 or more.

[0038] In one embodiment, the doped layers of the wafer under monitoring and the test wafer can be similar in properties by using the D-SIMS longitudinal B concentration distribution curve of the wafer.

[0039] In one embodiment, the D-SIMS longitudinal B concentration distribution curve of the wafer to be monitored is as follows: Figure 3 As shown. It can be understood that D-SIMS stands for Dynamic Secondary Ion Mass Spectrometry, specifically referring to the analysis of ion-implanted wafers using dynamic secondary ion mass spectrometry, obtaining a distribution curve of the implanted element concentration as a function of depth, also called a depth profile curve. This curve can directly measure the distribution of boron atom concentration with depth in a silicon wafer, allowing for the determination of whether significant boron atom diffusion has occurred. It can be used to confirm the quality of the implanted layer, i.e., the doped layer, providing physical mechanism support for the linear relationship of the standard curve and the reliability of temperature monitoring methods.

[0040] In one embodiment, such as Figure 3 As shown, when the ion implantation depth is 50nm~300nm, the boron concentration of the non-metallic doped layer of the wafer to be monitored is linearly related to the ion implantation depth.

[0041] It should be noted that in this embodiment, the boron concentration of the wafer under monitoring is linearly related to the depth in the range of 50nm to 300nm, and the concentration gradient is basically constant. This makes the diffusion flux and redistribution of boron during annealing mainly controlled by temperature. By measuring the change in sheet resistance after annealing and comparing it with the standard curve, it is possible to sensitively and repeatably determine whether the temperature of the hot annealing machine is abnormal.

[0042] In one embodiment, the standard curve satisfies the following condition: within the preset process temperature range, when the temperature is pulled by ±20°C, the sheet resistance of the non-metallic doped layer has a linear relationship.

[0043] In one embodiment, the linear correlation coefficient of the linear relationship is greater than or equal to 0.99.

[0044] Understandably, a linear correlation coefficient greater than or equal to 0.99 ensures that the sheet resistance has sufficiently high sensitivity and monotonicity to temperature changes, allowing the accuracy of temperature inference from the sheet resistance to meet the requirements of process monitoring. If the linear correlation coefficient is lower than 0.99, the correspondence between the sheet resistance and temperature is not accurate enough, the error in inferring temperature increases, and the probability of misjudgment increases significantly.

[0045] In one embodiment, the preset annealing time is 30 seconds.

[0046] In one embodiment, the ion implantation dose is 5 × 10⁻⁶. 14 atoms / cm 2 ~5×10 15 atoms / cm 2 It is important to note that the ion implantation dose determines the total number of doped atoms in the doped layer. If the dose is too low, the doped atom concentration is insufficient, resulting in excessively high sheet resistance and a decreased signal-to-noise ratio in the measurement signal. If the dose is too high, the doped atom concentration approaches or exceeds the solid solubility limit in silicon, and the excess doped atoms cannot be activated, leading to unintended cluster formation and affecting the linear relationship between sheet resistance and temperature. Controlling the implantation dose within the aforementioned range ensures that the sheet resistance of the doped layer remains within a suitable measurement range after annealing and maintains a good linear relationship with temperature.

[0047] In one embodiment, the ion implantation depth is 50 nm to 300 nm.

[0048] It should be noted that the implantation depth determines the junction depth (xj) of the doped layer. If the implantation depth is too shallow, the doped layer is too thin, and the sheet resistance is overly sensitive to surface conditions and interface scattering, resulting in poor measurement repeatability. If the implantation depth is too deep, the doped layer is far from the surface, making heat transfer and activation processes during annealing more complex, and the sheet resistance measurement may be affected by the substrate. Controlling the implantation depth within the range of 50nm to 300nm ensures that the doped layer is thin enough to be sensitive to changes in sheet resistance, yet thick enough to avoid surface and interface effects dominating the measurement results.

[0049] In one embodiment, the ion implantation energy is 15keV to 30keV.

[0050] It should be noted that the injection energy plays a decisive role in the injection depth. The injection energy should be controlled within the range of 15 keV to 30 keV to match the above-mentioned injection depth range.

[0051] In one embodiment, the ions used for ion implantation include boron ions.

[0052] It is understandable that boron ions are a commonly used p-type dopant with a suitable activation rate. Moreover, boron ions are relatively light in mass, causing relatively little damage to the silicon lattice during implantation, which is beneficial to the stability and repeatability of sheet resistance after annealing.

[0053] In one embodiment, the volume resistivity of the wafer substrate to be monitored is 3 Ω·cm to 5 Ω·cm.

[0054] Understandably, the volume resistivity of the substrate determines its conductivity. If the substrate resistivity is too low, the substrate's conductivity may mask the electrical signal of the doped layer, leading to distortion in the sheet resistance measurement. If the substrate resistivity is too high, the pn junction or Schottky contact between the substrate and the doped layer may affect the accuracy of the four-probe measurement. Controlling the substrate volume resistivity within the aforementioned range ensures that the electrical signal of the doped layer is clearly discernible while avoiding substrate interference with the measurement.

[0055] In one embodiment, step S40 specifically includes the following steps: The annealing temperature is calculated by substituting the measured sheet resistance into a standard curve. This annealing temperature is then compared with a preset process temperature to calculate the temperature difference. If the temperature difference is less than or equal to the allowable temperature deviation, the process temperature of the hot annealing machine is normal; if the temperature difference is greater than the allowable temperature deviation, the process temperature of the hot annealing machine is abnormal. Specifically, the allowable temperature deviation can be set according to actual process requirements.

[0056] In one embodiment, after a 6-day interval following the thermal annealing process at the preset process temperature, the sheet resistance value of the non-metallic doped layer measured showed a deviation of less than 1.5% compared to before the interval. This indicates that the annealed wafer exhibits good time stability, and the sheet resistance value does not change significantly with prolonged storage time. This allows the monitoring method to have a larger measurement window; the annealed wafer does not need to be measured immediately and can be retested after 6 days or even longer, providing convenience for flexible production line scheduling.

[0057] The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine according to the present invention can be applied to technical fields including but not limited to: monitoring the medium-low temperature annealing process window during the formation of metal silicides, monitoring the medium-low temperature annealing process window during the annealing and alloying process of metal thin films, monitoring the medium-low temperature annealing process window during the processing of dielectric layers and novel interconnect materials, and monitoring the medium-low temperature annealing process window during the formation of ohmic contacts of wide-bandgap semiconductor materials.

[0058] This invention also proposes a temperature monitoring system for medium- and low-temperature thermal annealing processes, comprising: a process execution unit, which includes an ion implantation device and a thermal annealing machine; the ion implantation device is used to perform an ion implantation process on a wafer to form a doped layer on the wafer surface; the thermal annealing machine is used to perform a thermal annealing process on the wafer at a preset process temperature; a data detection unit, which measures the sheet resistance value of the doped layer on the wafer surface using a four-probe resistivity meter and / or a sheet resistance meter; and a data judgment unit, which compares the measured sheet resistance value with a standard curve, calculates the annealing temperature, and further determines whether it is consistent with the machine's set temperature.

[0059] The technical solution of the present invention will be further described below through specific embodiments.

[0060] Example 1 The D-SIMS longitudinal B concentration distribution curve of the wafer to be monitored in Example 1 is shown below. Figure 3 As shown.

[0061] This embodiment provides a method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine, comprising the following steps: S10. Establishing the standard curve: Multiple test wafers of the same specifications as the wafer to be monitored are provided, with a substrate volume resistivity of 4 Ω·cm. Boron ion implantation is performed on each test wafer using an ion implantation device, with an implantation dose of 5 × 10⁻⁶. 14 atoms / cm 2 ~5×10 15 atoms / cm 2The implantation energy is 15keV~30keV, and the implantation depth is about 50nm~300nm, forming a non-metallic doped layer on the surface of each test wafer; Within a temperature range of 450℃ to 500℃, multiple test wafers were subjected to thermal annealing processes at different temperatures (specifically 450℃, 475℃, and 500℃) using a thermal annealing machine, with an annealing time of 30 seconds. Afterwards, the data detection unit used a four-probe resistivity meter to measure the sheet resistance of the non-metallic doped layer on each test wafer. The data judgment unit plots and stores a standard curve with annealing temperature as the x-axis and sheet resistance as the y-axis. Figure 4 As shown in the figure, within the temperature range of 450℃ to 500℃, the sheet resistance exhibits a good linear relationship with the annealing temperature, with a linear correlation coefficient R0. 2 =0.9941.

[0062] S20. Use an ion implantation device to perform a boron ion implantation process on the wafer to be monitored. The relevant process parameters are the same as those for the ion implantation process of the test wafer, and a non-metallic doped layer is formed on the surface of the wafer to be monitored. S30. The wafer to be monitored is fed into the hot annealing machine and a hot annealing process with a preset process temperature of 485℃ is performed. S40. The data detection unit uses a four-probe resistivity meter to measure the sheet resistance of the non-metallic doped layer and imports it into the data judgment unit. The data judgment unit substitutes the measured sheet resistance into the standard curve and calculates the annealing temperature to be 481℃. The temperature of 481℃ is compared with the machine's set temperature of 485℃. The temperature difference is 4℃, which is less than the allowable temperature deviation (±10℃), thus determining that the process temperature of the hot annealing machine is normal.

[0063] Example 2 The difference between this embodiment and Embodiment 1 is that in step S10 of Embodiment 2, multiple test wafers are subjected to thermal annealing processes at different temperatures (specifically 500℃, 520℃, and 545℃) within a temperature range of 500℃ to 545℃, with an annealing time of 30 seconds. Afterwards, the data detection unit uses a four-probe resistivity meter to measure the sheet resistance of the non-metallic doped layer of each test wafer and imports it into the data judgment unit; and the preset process temperature in step S30 of Embodiment 2 is changed to 540℃.

[0064] The data judgment unit plots a standard curve with annealing temperature on the x-axis and sheet resistance on the y-axis, such as... Figure 5 As shown in the figure, within the temperature range of 500℃ to 545℃, the sheet resistance exhibits a good linear relationship with the annealing temperature, with a linear correlation coefficient R0. 2 =0.9953.

[0065] The calculated annealing temperature is 538℃. Comparing 538℃ with the machine's set temperature of 540℃, the temperature difference is 2℃, which is less than the allowable temperature deviation (±10℃). Therefore, it is determined that the process temperature of the hot annealing machine is normal.

[0066] Example 3 The difference between this embodiment and Embodiment 1 is as follows: In step S10 of Embodiment 3, multiple test wafers are subjected to thermal annealing processes at different temperatures (specifically 545℃, 570℃, and 600℃) within a temperature range of 545℃ to 600℃, with an annealing time of 30 seconds. Afterwards, the data detection unit uses a four-probe resistivity meter to measure the sheet resistance of the non-metallic doped layer of each test wafer and imports the data into the data judgment unit; and the preset process temperature in step S30 of Embodiment 3 is changed to 580℃.

[0067] The data judgment unit plots a standard curve with annealing temperature on the x-axis and sheet resistance on the y-axis, such as... Figure 6 As shown in the figure, within the temperature range of 545℃ to 600℃, the sheet resistance exhibits a good linear relationship with the annealing temperature, with a linear correlation coefficient R0. 2 =0.9939.

[0068] The calculated annealing temperature is 582℃. Comparing 582℃ with the machine's set temperature of 580℃, the temperature difference is 2℃, which is less than the allowable temperature deviation (±10℃). Therefore, it is determined that the process temperature of the hot annealing machine is normal.

[0069] Performance testing: The sheet resistance values ​​of the test wafers at each annealing temperature in Examples 1-3 were measured after a 6-day interval, and the offset compared to the uninterrupted interval was calculated. The specific measurement results are shown in Table 1.

[0070] Table 1

[0071] Analysis of Table 1 shows that the ion implantation conditions of the present invention exhibit excellent temperature sensitivity and linearity from 450℃ to 600℃, and respond to temperature accurately and sensitively. The sheet resistance after annealing is highly stable over time, and the RS offset is less than 1.5% after a 6-day interval.

[0072] The above description is merely an exemplary embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention specification and drawings under the technical concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.

Claims

1. A method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine, characterized in that, Includes the following steps: S10 provides silicon wafers, as well as standard curves for thermal annealing process temperature and sheet resistance; S20. Perform an ion implantation process on the silicon wafer to form a non-metallic doped layer on the surface of the silicon wafer, thereby obtaining the wafer to be monitored. S30. The wafer to be monitored is sent into a thermal annealing machine and a thermal annealing process with a preset process temperature is performed. S40. Measure the sheet resistance of the non-metallic doped layer and determine whether the measured sheet resistance value conforms to the standard curve. If so, the process temperature of the hot annealing machine is determined to be normal; otherwise, the process temperature of the hot annealing machine is determined to be abnormal. In step S20, the ion implantation depth is 50nm~300nm; In step S30, the preset process temperature is 450℃~600℃.

2. The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine as described in claim 1, characterized in that, The standard curve is specifically a standard curve of the thermal annealing process temperature and sheet resistance of a non-metallic doped layer within a preset process temperature range. The determination method includes the following steps: Multiple silicon wafers from step S10 are provided, and the ion implantation process in step S20 is performed on each of them. The non-metallic doped layer is formed on the surface of each silicon wafer to produce multiple test wafers. Within the preset process temperature range, thermal annealing processes at different temperatures are performed on multiple test wafers, and then the sheet resistance of the non-metallic doped layer of each test wafer is measured. The standard curve was obtained by plotting the corresponding relationship between different thermal annealing process temperatures and the sheet resistance values ​​of non-metallic doped layers.

3. The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine as described in claim 2, characterized in that, The standard curve satisfies the following conditions: Within the preset process temperature range, if the temperature deviation is ±20℃, the sheet resistance of the non-metallic doped layer has a linear relationship, with a linear correlation coefficient greater than or equal to 0.

99.

4. The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine as described in claim 1, characterized in that, When the ion implantation depth is 50nm~300nm, the boron concentration of the non-metallic doped layer of the wafer to be monitored is linearly related to the ion implantation depth.

5. The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine as described in claim 1, characterized in that, The ion implantation dose is 5 × 10⁻⁶. 14 atoms / cm 2 ~5×10 15 atoms / cm 2 ; And / or, the ion implantation energy is 15keV~30keV; And / or, the ions used in the ion implantation include boron ions.

6. The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine as described in claim 1, characterized in that, The volume resistivity of the wafer substrate to be monitored is 3Ω. cm~5Ω cm.

7. The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine as described in claim 1, characterized in that, Step S40 specifically includes the following steps: The sheet resistance measured in step S40 is substituted into the standard curve to calculate the annealing temperature. The annealing temperature is then compared with the preset process temperature of the hot annealing machine in step S30, and the temperature difference is calculated. If the temperature difference is less than or equal to the allowable temperature deviation, the process temperature of the hot annealing machine is normal; if the temperature difference is greater than the allowable temperature deviation, the process temperature of the hot annealing machine is abnormal.

8. The method for monitoring the medium-low temperature thermal annealing temperature of wafers in a thermal annealing machine as described in claim 1, characterized in that, After performing the thermal annealing process at the preset process temperature for 6 days, the sheet resistance value of the non-metallic doped layer measured is less than 1.5% of the value before the interval.

9. A temperature monitoring system for medium-low temperature hot annealing processes, characterized in that, The temperature monitoring system for the medium-low temperature hot annealing process is used to perform the method for monitoring the medium-low temperature hot annealing temperature of the wafer in the hot annealing machine as described in any one of claims 1 to 8; The temperature monitoring system for medium-low temperature thermal annealing processes includes: The process execution unit includes an ion implantation device and a thermal annealing machine. The ion implantation device is used to perform an ion implantation process on a wafer to form a doped layer on the wafer surface. The thermal annealing machine is used to perform a thermal annealing process on the wafer at a preset process temperature. A data detection unit measures the sheet resistance of the doped layer on the wafer surface using a four-probe resistivity meter and / or a sheet resistance meter; and The data judgment unit is used to compare the measured sheet resistance value with the standard curve, calculate the annealing temperature, and further determine whether it is consistent with the machine set temperature.