A method for processing a rework wafer for a pe-poly process that has deposited poly-silicon
The poly silicon layer and silicon dioxide layer of the reworked wafer in the PE-poly process are removed by cleaning with a mixed solution of low-concentration NaOH and additives, while retaining the front structure. This allows for direct feeding into production and solves the problems of cumbersome processing and silicon wafer thickness reduction in existing methods, achieving efficient and low-cost cell fabrication.
Patent Information
- Application Number
- CN202611186738.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-06
- Publication Date
- 2026-11-20
AI Technical Summary
The existing PE-poly process for reworked wafers is cumbersome, consumes a lot of chemicals, and results in significant reduction in silicon wafer thickness, leading to a high breakage rate, slow production pace, and high costs.
The polysilicon layer and silicon dioxide layer on the back side are removed by cleaning with a mixed solution of low-concentration NaOH and additives, while the BSG layer and boron-doped emitter layer on the front side are retained. After cleaning, the cells are directly fed into production, reducing texturing, boron diffusion and alkaline polishing processes. The performance of the cells is improved through multilayer film deposition and annealing.
It simplifies the rework process, reduces chemical consumption, maintains the thickness of the crystalline silicon substrate, improves cell efficiency and yield, and reduces production costs and breakage rate.
Smart Images

Figure CN123146205A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar cell technology, and more particularly to a method for processing rework wafers in which poly silicon has been deposited in the PE-poly process. Background Technology
[0002] Currently, TOPCon cell technology has become the mainstream cell technology in solar cells due to its advantages of high photoelectric conversion efficiency, high reliability, and low cost. The PE-poly route and the LPCVD route are the two main mass production routes for TOPCon cells. The PE-poly route has a slightly lower cost, and the doping concentration of poly silicon can be precisely controlled in layers. The scalability of doping elements is also easy to achieve, making its current production capacity surpass that of the LPCVD route. However, the PE-poly process is implemented using direct PECVD technology, which requires a high-power radio frequency power supply to discharge and ionize the incoming reactive gas into plasma. In this technology, the graphite boat, silicon wafer, and radio frequency power supply are connected to form a discharge electric field. During the production process, due to microcracks in the wafer, damage to the graphite boat, poor contact between the graphite boat and the discharge electrodes in the furnace tube, deformation of the discharge electrodes, and abnormalities in the radio frequency power supply, the process is very prone to termination before completion. Currently, the PE-poly process sequentially deposits the following layers on the polished back surface of TOPCon cells after alkaline polishing: a first ultrathin silicon dioxide tunneling layer, a second low-doped poly silicon layer, a third ultrathin silicon dioxide passivation layer, a fourth highly doped poly silicon layer, and a fifth silicon dioxide mask layer. When the first, second, and third layers are terminated, any incomplete re-plating results in defective finished cells that fail quality verification. Normal process control prevents re-plating and requires rework. Furthermore, process terminations disrupt production schedules. If electrode abnormalities require prolonged processing, the single-crystal silicon substrate on the back of the cell is completely exposed without protection after alkaline polishing. If PE-poly coating is not completed within 30 minutes, rework is necessary. Overall, the PE-poly process results in a high percentage of reworked cells.
[0003] After texturing, boron diffusion, removal of backside BSG, and alkaline polishing, the front side of the rework wafer in the PE-poly process has a BSG layer and a boron-doped emitter layer from the outside to the inside. The current traditional method for processing rework wafers with deposited poly silicon in the PE-poly process is to first clean them with a rework wafer cleaning machine. The specific cleaning steps are as follows: cleaning with a high-concentration HF acid solution to remove the front side BSG layer, cleaning with pure water to remove the acid residue from the acid washing process, cleaning with a high-concentration NaOH solution to remove the boron-doped emitter layer and the back side poly silicon layer, cleaning with pure water to remove the alkali residue from the alkaline washing process, cleaning with a mixed solution of HF and HCl to neutralize the residual alkali and metal ions, cleaning with pure water to remove the acid residue from the previous cleaning process, hot water slow lifting cleaning and dehydration, and hot air drying of the silicon wafer. Then, the wafer is fed back from the texturing process for reprocessing.
[0004] This method is cumbersome, consumes a lot of chemicals, and requires thorough removal of the boron emitter during cleaning, with an etching thickness of 3µm on one side and a total thickness of about 6µm on both sides. After cleaning, the rework wafer undergoes texturing, with an etching thickness of 3µm on one side and a total thickness of about 6µm on both sides. In the alkaline polishing process, the boron doped layer needs to be etched off on the back side, achieving a back-side etching thickness of 3µm. After these processes, the total thickness of the rework wafer in the PE-poly process is reduced by about 15µm. Currently, the mainstream 210*210cm silicon wafer thickness is 130µm. The large wafer size and thin thickness result in a high breakage rate during the original wafer production process. Traditional rework wafer processing methods only achieve a wafer thickness of about 110µm by the PE-poly process. This excessive thinness leads to an even higher breakage rate, further disrupting the production schedule, reducing yield, and making the overall rework wafer processing cost too high. Therefore, a new processing method needs to be developed to overcome these problems. Summary of the Invention
[0005] Purpose of the invention: To address the shortcomings and defects of existing technologies, this invention provides a method for processing rework wafers with deposited poly silicon in the PE-poly process. The method involves fewer cleaning steps for the rework wafers, and the rework wafers do not undergo texturing, boron diffusion, BSG removal, or alkaline polishing before being fed into production. The overall material consumption is low, and the thickness of the silicon substrate in the solar cell remains essentially unchanged. The method involves fewer manufacturing steps, and the finished solar cells have high efficiency and high yield. The overall cost of rework wafer processing is low.
[0006] Technical solution: The present invention provides a method for processing rework wafers with deposited poly silicon in the PE-poly process, characterized by comprising the following steps: 1) Collection and cleaning of reworked pieces: 101) After the reworked sheets are unloaded from the PE-poly process automated machine and loaded into the basket, they are collected and stored separately along with the basket in the reworked sheet cleaning machine area for no more than 24 hours. 102) Place the basket loaded with reworked wafers into the feed channel of the reworked wafer cleaning machine. The machine will run automatically and first run to the tank of low concentration NaOH and additive mixed solution to clean and remove the poly silicon layer and the extremely thin silicon dioxide layer on the back side. 103) Use pure water to rinse and remove residual NaOH; 104) Use a low-concentration mixture of alkali and hydrogen peroxide to clean and remove organic impurities; 105) Use pure water to rinse and remove residual NaOH; 106) The reworked pieces were placed in a low-concentration HCl solution for cleaning to neutralize the residual NaOH and remove metal ions; 107) Use pure water to rinse and remove residual HCl; 108) Use pure hot water for slow lifting and dehydration; 109) Hot air is used to dry the silicon wafers; 2) Rework sheet feeding production: The cleaned rework sheets, along with the basket, are immediately transported to the PE-poly process for feeding and production. The time from the end of the cleaning of the rework sheets to the feeding of the PE-poly process is controlled within 30 minutes.
[0007] Preferably, step 2) of rework sheet feeding production specifically includes the following steps: 201) Using a PE-poly tubular coating equipment, the first ultrathin silicon dioxide tunneling layer, the second low-doped poly silicon layer, the third ultrathin silicon dioxide passivation layer, the fourth high-doped poly silicon layer, and the fifth silicon dioxide mask layer are sequentially deposited on the back of the solar cell. 202) A tubular high-temperature annealing crystallization device is used to convert the phosphorus-doped poly silicon deposited in the PE-poly process into polycrystalline silicon; 203) A chain-type PSG removal device is used to clean and remove the silicon dioxide mask layer coated around the front edge of the PE-poly process cell, and then perform pure water cleaning and drying. 204) Using RCA cleaning equipment, the poly silicon layer deposited around the edge of the front side of the solar cell in the PE-poly process, the BSG layer generated on the front side in the boron diffusion process, and the silicon dioxide mask layer on the back side of the PE-poly process are removed in sequence, and then the cells are cleaned with pure water and dried. 205) A tubular ALD device is used to simultaneously deposit aluminum oxide thin films on the front and back sides of the solar cell; 206) Using a tubular PECVD equipment, a multilayer anti-reflection protective film is deposited on the front side of the solar cell, consisting of a first layer of high refractive index silicon nitride film, a second layer of medium refractive index silicon nitride film, a third layer of low refractive index silicon nitride film, a fourth layer of high refractive index silicon oxynitride film, a fifth layer of low refractive index silicon oxynitride film, and a sixth layer of silicon dioxide film. 207) Using a tubular PECVD equipment, a multilayer antireflective protective film is deposited on the back of the solar cell, consisting of a first layer of high-refractive-index silicon nitride film, a second layer of medium-refractive-index silicon nitride film, and a third layer of low-refractive-index silicon nitride film. 208) Using screen printing sintering equipment, the back main grid, back sub-grid, front main grid, and front sub-grid are printed sequentially, and then sintered uniformly to make the printed silver metal grid lines form ohmic contact with silicon to prepare the front and back metal electrodes. 209) An industrial light injection furnace is used to perform light injection treatment on the solar cells, which activates H atoms from the passivation layer and improves the photoelectric conversion efficiency of the solar cells. 210) Laser-assisted sintering equipment is used to enhance the silver metal electrode on the front side of the solar cell, so that an alloy junction is formed at the silver-silicon contact point, reducing the silver-silicon contact resistance and improving the conversion efficiency of the solar cell. 211) An integrated AOI, EL and IV testing machine is used to test the solar cells and classify them according to the cell efficiency, leakage current, EL image and AOI image, and finally complete the preparation, testing and classification of TOPCon solar cells.
[0008] Preferably, in step 102), the mass fraction of NaOH is 0.2% to 0.8%, the volume fraction of the additive is 0.2% to 0.5%, the cleaning temperature is 60 to 70°C, and the cleaning time is 300 to 500 seconds.
[0009] Preferably, in step 103), the cleaning temperature is 20-30°C and the cleaning time is 80-150 seconds.
[0010] Preferably, in step 104), the mass fraction of NaOH is 0.1% to 0.5%, the mass fraction of H2O2 is 0.5% to 1.5%, the cleaning temperature is 40 to 70°C, and the cleaning time is 80 to 150 seconds.
[0011] Preferably, in step 105), the cleaning temperature is 20-30°C and the cleaning time is 80-150 seconds.
[0012] Preferably, in step 106), the mass fraction of HCl is 0.1% to 0.5%, the cleaning temperature is 20 to 30°C, and the cleaning time is 80 to 150 seconds.
[0013] Preferably, in step 107), the cleaning temperature is 20-30°C and the cleaning time is 80-150 seconds.
[0014] Preferably, in step 108), the slow lifting temperature is 40-80°C and the slow lifting time is 10-40 seconds.
[0015] Preferably, in step 109), the drying temperature is 90-98°C and the drying time is 600-800 seconds.
[0016] The aforementioned rework wafers include the following: First, the process of depositing the second low-doped poly silicon layer in the PE-poly process was abnormally terminated, resulting in numerous defects and uneven thickness in the deposited low-doped poly silicon layer, requiring rework of the entire boat (616 210mm*210mm silicon wafers); Second, the process of depositing the third ultrathin silicon dioxide passivation layer in the PE-poly process was abnormally terminated, resulting in numerous defects and uneven thickness in the deposited ultrathin silicon dioxide passivation layer, requiring rework of the entire boat.
[0017] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: The present invention performs the following steps on the rework wafers in the PE-poly process after poly silicon deposition: cleaning with a low-concentration NaOH and additive mixed solution to remove the poly silicon layer and the extremely thin silicon dioxide layer on the back side; cleaning with pure water to remove the alkali residue from the previous cleaning; cleaning with a low-concentration alkali and hydrogen peroxide mixed solution to remove organic impurities such as additives; cleaning with pure water to remove the alkali residue from the previous cleaning; cleaning with a low-concentration HCl solution to neutralize the residual alkali and remove metal ions; cleaning with pure water to remove the acid residue from the previous cleaning; slow lifting and dehydration with pure hot water; and drying the silicon wafer with hot air. This cleaning method basically retains the BSG layer on the front side and completely retains the boron-doped emitter layer on the front side. After cleaning, the TOPCon solar cell is prepared by feeding it into the PE-poly process.
[0018] This method is used to process rework wafers with polysilicon deposited in the PE-poly process. The rework wafers have fewer cleaning steps, and the production process after cleaning does not involve texturing, boron diffusion, BSG removal, or alkaline polishing. The overall material consumption is low, and the thickness of the silicon substrate in the solar cell remains basically unchanged. The process involves fewer steps, and the finished solar cells have high efficiency and high yield. The overall cost of rework wafer processing is low. Attached Figure Description
[0019] Figure 1 This is a flowchart of the present invention; Figure 2 The above are statistical data charts for embodiments and comparative examples of the present invention. Detailed Implementation
[0020] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0021] The present invention designs a method for processing rework wafers with deposited poly silicon in the PE-poly process, and creatively uses a mixed solution of low-concentration NaOH and additives to clean only the poly silicon layer and ultra-thin silicon dioxide layer on the back side, and a process method for feeding the rework wafers into the PE-poly process after cleaning, and determines the optimal process parameters.
[0022] Example 1: The method for processing rework wafers with deposited poly silicon in the PE-poly process according to this embodiment includes the following steps: 1) Collection and cleaning of reworked pieces: 101) After the reworked sheets are unloaded from the PE-poly process automated machine and loaded into the basket, they are collected and stored separately along with the basket in the reworked sheet cleaning machine area for no more than 24 hours. 102) Place the basket loaded with reworked wafers into the feed channel of the reworked wafer cleaning machine. The machine will start automatically and first run into the tank of low concentration NaOH and additive mixed solution to clean and remove the poly silicon layer and ultra-thin silicon dioxide layer on the back side. The mass fraction of NaOH is 0.5%, the volume fraction of the additive is 0.35%, the temperature is 65℃, and the cleaning time is 400s. 103) Use pure water to rinse away residual NaOH at a temperature of 25℃ for 110 seconds; 104) Organic impurities were removed by cleaning with a low-concentration alkali and hydrogen peroxide mixed solution. The mass fraction of NaOH was 0.25%, the mass fraction of H2O2 was 0.85%, the temperature was 50℃, and the cleaning time was 110s. 105) Use pure water to rinse away residual NaOH at a temperature of 25℃ for 110 seconds; 106) The reworked piece was placed in a low-concentration HCl solution for cleaning to neutralize the residual NaOH and remove metal ions. The mass fraction of HCl was 0.25%, the temperature was 25℃, and the cleaning time was 110s. 107) Use pure water to rinse and remove residual HCl at a temperature of 25°C for 110 seconds; 108) Use pure hot water for slow lifting and dehydration at a temperature of 50℃ for 20 seconds; 109) The silicon wafers are dried using hot air at a temperature of 95°C for 700 seconds. 2) Rework Sheet Feeding Production: The cleaned rework sheets, along with the basket, are immediately transported to the PE-poly process for feeding (the time from the end of cleaning the rework sheets to feeding into the PE-poly process is controlled within 30 minutes). All processes from the feeding process to the completion of the finished battery cell manufacturing are the same as the conventional battery cell manufacturing process. The specific steps are as follows: 201) Using a PE-poly tubular coating equipment, the first ultrathin silicon dioxide tunneling layer, the second low-doped poly silicon layer, the third ultrathin silicon dioxide passivation layer, the fourth high-doped poly silicon layer, and the fifth silicon dioxide mask layer are sequentially deposited on the back of the solar cell. 202) A tubular high-temperature annealing crystallization device is used to convert the phosphorus-doped poly silicon deposited in the PE-poly process into polycrystalline silicon; 203) A chain-type PSG removal device is used to clean and remove the silicon dioxide mask layer coated around the front edge of the PE-poly process cell, and then perform pure water cleaning and drying. 204) Using RCA cleaning equipment, the poly silicon layer deposited around the edge of the front side of the solar cell in the PE-poly process, the BSG layer generated on the front side in the boron diffusion process, and the silicon dioxide mask layer on the back side of the PE-poly process are removed in sequence, and then the cells are cleaned with pure water and dried. 205) A tubular ALD device is used to simultaneously deposit aluminum oxide thin films on the front and back sides of the solar cell; 206) Using a tubular PECVD equipment, a multilayer anti-reflection protective film is deposited on the front side of the solar cell, consisting of a first layer of high refractive index silicon nitride film, a second layer of medium refractive index silicon nitride film, a third layer of low refractive index silicon nitride film, a fourth layer of high refractive index silicon oxynitride film, a fifth layer of low refractive index silicon oxynitride film, and a sixth layer of silicon dioxide film. 207) Using a tubular PECVD equipment, a multilayer antireflective protective film is deposited on the back of the solar cell, consisting of a first layer of high-refractive-index silicon nitride film, a second layer of medium-refractive-index silicon nitride film, and a third layer of low-refractive-index silicon nitride film. 208) Using screen printing sintering equipment, the back main grid, back sub-grid, front main grid, and front sub-grid are printed sequentially, and then sintered uniformly to make the printed silver metal grid lines form ohmic contact with silicon to prepare the front and back metal electrodes. 209) An industrial light injection furnace is used to perform light injection treatment on the solar cells, which activates H atoms from the passivation layer and improves the photoelectric conversion efficiency of the solar cells. 210) Laser-assisted sintering equipment is used to enhance the silver metal electrode on the front side of the solar cell, so that an alloy junction is formed at the silver-silicon contact point, reducing the silver-silicon contact resistance and improving the conversion efficiency of the solar cell. 211) An integrated AOI, EL and IV testing machine is used to test the solar cells and classify them according to the cell efficiency, leakage current, EL image and AOI image, and finally complete the preparation, testing and classification of TOPCon solar cells.
[0023] Example 2: The method for processing rework wafers with deposited poly silicon in the PE-poly process in this embodiment is the same as that in Example 1, except that the mass fraction of NaOH in step 102) is reduced to 0.2% and the volume fraction of additives is reduced to 0.2%. Therefore, it will not be described in detail here.
[0024] Example 3: The method for processing rework wafers with deposited poly silicon in the PE-poly process in this embodiment is the same as that in Example 1, except that the mass fraction of NaOH in step 102) is increased to 0.8% and the volume fraction of additives is increased to 0.5%. Therefore, it will not be described in detail here.
[0025] Example 4: The method for processing rework wafers with deposited poly silicon in the PE-poly process in this embodiment is the same as that in Example 1, except that the cleaning time in step 102) is reduced to 300s. Therefore, it will not be described again here.
[0026] Example 5: The method for processing rework wafers with deposited poly silicon in the PE-poly process in this embodiment is the same as that in Example 1, except that the cleaning time in step 102) is increased to 500s. Therefore, it will not be described again here.
[0027] Example 6: The method for processing rework wafers with deposited poly silicon in the PE-poly process in this embodiment is the same as that in Example 1, except that the cleaning time in step 102) is reduced to 350s. Therefore, it will not be described again here.
[0028] Comparative Example 1: This comparative example illustrates a traditional rework wafer processing method for polysilicon deposited in the PE-poly process. The method includes the following steps: 1) Collection and cleaning of reworked pieces: 101) After the reworked sheets are unloaded from the PE-poly process automated machine and loaded into the basket, they are collected and stored separately along with the basket in the reworked sheet cleaning machine area. There is no requirement for the storage time. 102) Place the basket loaded with rework pieces into the feed channel of the rework piece cleaning machine. The machine will run automatically and first run into the high-concentration HF solution tank to clean and remove the BSG layer on the front side. The mass fraction of HF is 2.5%, the temperature is 25℃, and the cleaning time is 400s. 103) Use pure water to clean and remove residual HF at a temperature of 25°C for 110 seconds; 104) The front boron diffusion layer, the back poly silicon layer and the ultrathin silicon dioxide layer were removed by cleaning with an alkaline solution. The mass fraction of NaOH was 0.75%, the temperature was 65℃ and the cleaning time was 100s. 105) Use pure water to rinse away residual NaOH at a temperature of 25℃ for 110 seconds; 106) Organic impurities were removed by cleaning with a low-concentration alkali and hydrogen peroxide mixed solution. The mass fraction of NaOH was 0.3%, the mass fraction of H2O2 was 0.75%, the temperature was 50℃, and the cleaning time was 110s. 107) Use pure water to rinse away residual NaOH at a temperature of 25℃ for 110 seconds; 108) The reworked piece was placed in a mixed solution of HF and HCl to clean it, neutralize the residual NaOH, and remove metal ions. The mass fraction of HF was 0.85%, the mass fraction of HCl was 0.75%, the temperature was 25℃, and the cleaning time was 110s. 109) Use pure water to clean and remove residual HF and HCl at a temperature of 25°C for 110 seconds. 110) Use pure hot water for slow lifting and dehydration at a temperature of 50℃ for 20 seconds; 111) The silicon wafers are dried using hot air at a temperature of 95°C for 700 seconds. 112) Remove the cleaned rework wafers from the basket to the silicon wafer box, then take them out and package them. When packaging, the direction of the silicon wafer cutting lines must be consistent. 2) Rework Sheet Feeding Production: The packaged rework sheets are transported to the texturing process for feeding and production. All processes from the feeding process to the completion of the finished battery cell are the same as those of conventional battery cell manufacturing processes. The specific steps are as follows: 201) A trough-type alkaline texturing equipment is used to simultaneously perform anisotropic etching on the front and back sides of the silicon wafer to prepare a pyramid-shaped textured surface; 202) A high-temperature tubular boron diffusion apparatus was used to prepare a boron-doped emitter, and a BSG layer was formed on the surface at the same time; 203) Use a chain-type BSG removal device to remove the BSG layer on the back and edges of the silicon wafer; 204) The boron-doped layer on the back side is etched and removed using an alkaline polishing device, and the silicon substrate on the back side is polished. 205) Using a PE-poly tubular coating equipment, the first ultrathin silicon dioxide tunneling layer, the second low-doped poly silicon layer, the third ultrathin silicon dioxide passivation layer, the fourth high-doped poly silicon layer, and the fifth silicon dioxide mask layer are sequentially deposited on the back of the solar cell. 206) A tubular high-temperature annealing crystallization device is used to convert the phosphorus-doped poly silicon deposited in the PE-poly process into polycrystalline silicon; 207) A chain-type PSG removal device is used to clean and remove the silicon dioxide mask layer coated around the front edge of the PE-poly process cell, and then perform pure water cleaning and drying. 208) Using RCA cleaning equipment, the poly silicon layer deposited around the edge of the front side of the solar cell in the PE-poly process, the BSG layer generated on the front side in the boron diffusion process, and the silicon dioxide mask layer on the back side of the PE-poly process are removed in sequence, and then the cells are cleaned with pure water and dried. 209) A tubular ALD device is used to simultaneously deposit aluminum oxide thin films on the front and back sides of the solar cell; 210) Using a tubular PECVD equipment, a multilayer antireflective protective film is deposited on the front side of the solar cell, consisting of a first layer of high refractive index silicon nitride film, a second layer of medium refractive index silicon nitride film, a third layer of low refractive index silicon nitride film, a fourth layer of high refractive index silicon oxynitride film, a fifth layer of low refractive index silicon oxynitride film, and a sixth layer of silicon dioxide film. 211) Using a tubular PECVD equipment, a multilayer antireflective protective film is deposited on the back of the solar cell, consisting of a first layer of high-refractive-index silicon nitride film, a second layer of medium-refractive-index silicon nitride film, and a third layer of low-refractive-index silicon nitride film. 212) Using screen printing sintering equipment, the back main grid, back sub-grid, front main grid, and front sub-grid are printed sequentially, and then sintered uniformly to make the printed silver metal grid lines form ohmic contact with silicon to prepare the front and back metal electrodes. 213) An industrial light injection furnace is used to perform light injection treatment on the solar cells, which activates H atoms from the passivation layer and improves the photoelectric conversion efficiency of the solar cells. 214) Laser-assisted sintering equipment is used to enhance the silver metal electrode on the front side of the solar cell, so that an alloy junction is formed at the silver-silicon contact point, reducing the silver-silicon contact resistance and improving the conversion efficiency of the solar cell. 215) An integrated AOI, EL and IV testing machine is used to test the solar cells and classify them according to the cell efficiency, leakage current, EL image and AOI image, and finally complete the preparation, testing and classification of TOPCon solar cells.
[0029] Specific statistical data of the battery cells prepared in the examples and comparative examples are as follows: Figure 2 As shown, the TOPCon cell prepared in Example 1 has a Voc of 0.738V, an Isc of 18.087A, an FF of 88.55%, and a photoelectric conversion efficiency (Eta) of 26.82%. The average photoelectric conversion efficiency is 0.09% higher than the comparative example, demonstrating a significant advantage. The proportion of defective EL cells, appearance defects, and fragmentation rate are significantly lower than the comparative example, especially the fragmentation rate. This is because the rework wafer processing method of this invention, compared to traditional methods, involves a thicker silicon substrate in the PE-poly process, resulting in higher long-wavelength light absorption, fewer processes, lower contamination levels, and higher overall photoelectric conversion efficiency. Furthermore, the thicker silicon substrate leads to a lower fragmentation rate during production, fewer process anomalies, and a higher product yield, especially given the current trend towards larger, thinner wafers.
[0030] This invention uses a mixed solution of low-concentration NaOH and additives to clean only the poly silicon layer and ultra-thin silicon dioxide layer on the back side. This cleaning method basically preserves the BSG layer on the front side and retains all the boron-doped emitter layer on the front side. After cleaning, the TOPCon solar cell is fabricated by feeding materials into the PE-poly process.
[0031] The present invention has the following beneficial effects: 1) Compared with the traditional PE-poly process for processing rework wafers with deposited poly silicon, the present invention has fewer cleaning steps, lower chemical concentration, and lower overall chemical consumption.
[0032] 2) The rework wafer cleaning method of the present invention uses a mixed solution of low-concentration NaOH and additives for cleaning, and after cleaning, there is no need for texturing and back-side polishing. The thickness reduction of the crystalline silicon substrate is limited. Compared with the traditional processing method to the PE-poly process, the crystalline silicon substrate is thicker, the long-wavelength light absorption rate is high, the process is less and the degree of contamination is low, and the overall photoelectric conversion efficiency of the battery cell is high.
[0033] 3) The processing method of the present invention allows for direct feeding of rework wafers from the PE-poly process after cleaning. This results in fewer production steps, lower overall material consumption, and a thicker silicon substrate. In the current trend of large-size thin wafers, the breakage rate during production is even lower, there are fewer production anomalies, higher product yield, and lower overall cost.
Claims
1. A method for processing rework wafers with deposited poly silicon in the PE-poly process, characterized in that: Includes the following steps: 1) Collection and cleaning of reworked pieces: 101) After the reworked sheets are unloaded from the PE-poly process automated machine and loaded into the basket, they are collected and stored separately along with the basket in the reworked sheet cleaning machine area for no more than 24 hours. 102) Place the basket loaded with reworked wafers into the feed channel of the reworked wafer cleaning machine. The machine will run automatically and first run to the tank of low concentration NaOH and additive mixed solution to clean and remove the poly silicon layer and the extremely thin silicon dioxide layer on the back side. 103) Use pure water to rinse and remove residual NaOH; 104) Use a low-concentration mixture of alkali and hydrogen peroxide to clean and remove organic impurities; 105) Use pure water to rinse and remove residual NaOH; 106) The reworked pieces were placed in a low-concentration HCl solution for cleaning to neutralize the residual NaOH and remove metal ions; 107) Use pure water to rinse and remove residual HCl; 108) Use pure hot water for slow lifting and dehydration; 109) Hot air is used to dry the silicon wafers; 2) Rework sheet feeding production: The cleaned rework sheets, along with the basket, are immediately transported to the PE-poly process for feeding and production. The time from the end of the cleaning of the rework sheets to the feeding of the PE-poly process is controlled within 30 minutes.
2. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: Step 2) of the rework piece production process specifically includes the following steps: 201) Using a PE-poly tubular coating equipment, the first ultrathin silicon dioxide tunneling layer, the second low-doped poly silicon layer, the third ultrathin silicon dioxide passivation layer, the fourth high-doped poly silicon layer, and the fifth silicon dioxide mask layer are sequentially deposited on the back of the solar cell. 202) A tubular high-temperature annealing crystallization device is used to convert the phosphorus-doped poly silicon deposited in the PE-poly process into polycrystalline silicon; 203) A chain-type PSG removal device is used to clean and remove the silicon dioxide mask layer coated around the front edge of the PE-poly process cell, and then perform pure water cleaning and drying. 204) Using RCA cleaning equipment, the poly silicon layer deposited around the edge of the front side of the solar cell in the PE-poly process, the BSG layer generated on the front side in the boron diffusion process, and the silicon dioxide mask layer on the back side of the PE-poly process are removed in sequence, and then the cells are cleaned with pure water and dried. 205) A tubular ALD device is used to simultaneously deposit aluminum oxide thin films on the front and back sides of the solar cell; 206) Using a tubular PECVD equipment, a multilayer anti-reflection protective film is deposited on the front side of the solar cell, consisting of a first layer of high refractive index silicon nitride film, a second layer of medium refractive index silicon nitride film, a third layer of low refractive index silicon nitride film, a fourth layer of high refractive index silicon oxynitride film, a fifth layer of low refractive index silicon oxynitride film, and a sixth layer of silicon dioxide film. 207) Using a tubular PECVD equipment, a multilayer antireflective protective film is deposited on the back of the solar cell, consisting of a first layer of high-refractive-index silicon nitride film, a second layer of medium-refractive-index silicon nitride film, and a third layer of low-refractive-index silicon nitride film. 208) Using screen printing sintering equipment, the back main grid, back sub-grid, front main grid, and front sub-grid are printed sequentially, and then sintered uniformly to make the printed silver metal grid lines form ohmic contact with silicon to prepare the front and back metal electrodes. 209) An industrial light injection furnace is used to perform light injection treatment on the solar cells, which activates H atoms from the passivation layer and improves the photoelectric conversion efficiency of the solar cells. 210) Laser-assisted sintering equipment is used to enhance the silver metal electrode on the front side of the solar cell, so that an alloy junction is formed at the silver-silicon contact point, reducing the silver-silicon contact resistance and improving the conversion efficiency of the solar cell. 211) An integrated AOI, EL and IV testing machine is used to test the solar cells and classify them according to the cell efficiency, leakage current, EL image and AOI image, and finally complete the preparation, testing and classification of TOPCon solar cells.
3. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 102), the mass fraction of NaOH is 0.2% to 0.8%, the volume fraction of the additive is 0.2% to 0.5%, the cleaning temperature is 60 to 70°C, and the cleaning time is 300 to 500 seconds.
4. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 103), the cleaning temperature is 20-30℃ and the cleaning time is 80-150s.
5. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 104), the mass fraction of NaOH is 0.1% to 0.5%, the mass fraction of H2O2 is 0.5% to 1.5%, the cleaning temperature is 40 to 70°C, and the cleaning time is 80 to 150 seconds.
6. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 105), the cleaning temperature is 20-30℃ and the cleaning time is 80-150s.
7. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 106), the mass fraction of HCl is 0.1% to 0.5%, the cleaning temperature is 20 to 30°C, and the cleaning time is 80 to 150 seconds.
8. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 107), the cleaning temperature is 20-30℃ and the cleaning time is 80-150s.
9. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 108), the slow lifting temperature is 40-80℃ and the slow lifting time is 10-40s.
10. The method for processing rework wafers with deposited poly silicon in the PE-poly process according to claim 1, characterized in that: In step 109), the drying temperature is 90-98℃ and the drying time is 600-800s.