A system, method and TGV substrate for TGV substrate metallization

By employing a fully wet process and a continuously charged conductive architecture throughout the entire process, the problems of gapless filling and complex equipment switching in high aspect ratio TGV substrate metallization have been solved, achieving high-quality TGV substrate metallization, reducing costs and improving manufacturing efficiency.

CN123146236APending Publication Date: 2026-11-20TIANJIN XUNLIN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611337114.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing TGV substrate metallization technologies face challenges such as gapless metal filling in high aspect ratio TGV, discontinuous PVD seed layers, copper layer thinning due to acid pickling leading to seed layer breakage, copper surface oxidation and Pd catalyst layer failure due to inter-process transfer, and high investment and complex switching issues caused by discrete equipment.

Method used

The process employs a fully wet process, using a flying target frame and V-shaped conductive blocks to apply bias voltage. Through constant voltage cathode reduction pulses and segmented constant current bias voltage, continuous electrical conduction is achieved throughout the entire process, avoiding scaling on the contact surface of the V-shaped conductive blocks. The same set of equipment can be used to quickly switch between chemical plating and electroplating functions.

Benefits of technology

It achieves 100% conductivity on TGV substrates with a large aspect ratio and near-zero copper layer loss, reducing raw material costs and equipment investment, improving manufacturing efficiency, and solving the problems of decreased conductivity and complex equipment switching in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146236A_ABST
    Figure CN123146236A_ABST
Patent Text Reader

Abstract

The embodiments of the present disclosure provide a system, a method and a TGV substrate for TGV substrate metallization. The method comprises cleaning and in-hole gas replacement treatment of the glass substrate; acid pickling treatment of the glass substrate; sensitization treatment of the glass substrate; immersing the glass substrate in an activation solution containing Pd 2+ to form a continuous catalytic layer; electrochemical copper plating; and electroplating a Cu layer to achieve metallization, wherein the glass substrate is always clamped by the flying target frame and the V-shaped conductive block, the V-shaped conductive block is always located above the surface of each wet tank, and after the glass substrate is transferred into the processing solution of each step, the glass substrate is subjected to constant voltage pulse reduction treatment before the treatment of each step. The method can obtain a high-quality TGV metallized substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of advanced semiconductor packaging technology, and in particular to a method and manufacturing system for metallizing through-glass vias (TGVs), specifically to a system, method, and TGV substrate for metallizing TGV substrates. Background Technology

[0002] As Moore's Law approaches its physical limits, glass substrates, with their excellent high-frequency electrical properties (dielectric constant 3.8-5.0), ultra-low coefficient of thermal expansion (CTE 3-9 ppm / ℃), and high flatness, have become the core material for 2.5D / 3D advanced packaging interconnects. Through-glass via (TGV) technology enables high-density signal transmission in three-dimensional space by forming vertical conductive channels on glass substrates.

[0003] However, achieving void-free metal filling in high aspect ratio TGVs remains a key technical challenge hindering the large-scale application of glass-based packaging. Therefore, current TGV substrate metallization systems, methods, and TGV substrates still require improvement. Summary of the Invention

[0004] This disclosure provides a system, method, and TGV substrate for metallization. The system and method employ a fully wet process, utilizing a flying target frame and V-shaped conductive blocks that do not contact the bath solution to apply a bias voltage. This avoids scaling and chemical contamination at the contact surface of the V-shaped conductive blocks. By controlling the bias voltage, a constant-voltage cathode reduction pulse is applied first to reduce the oxides generated on the copper layer surface during the transfer process to metallic copper, thereby improving the metal filling effect and achieving high-quality metallization of TGV substrates with a large aspect ratio.

[0005] In one aspect of this application, a method for metallizing a TGV substrate is provided, the method comprising: (1) Provide a glass substrate, the glass substrate having a through hole, a conductive bus ring being provided on the edge of the glass substrate, the through hole having a depth-to-width ratio greater than or equal to 6:1, and perform cleaning and gas replacement treatment on the glass substrate. (2) The glass substrate is subjected to acid pickling treatment. During the acid pickling treatment, a constant current bias voltage is applied to the conductive bus ring by a V-shaped conductive block fixed on a movable target frame to remove the oxide on the surface of the seed layer. The thinning amount of the seed layer is less than or equal to 1 nm. (3) Sensitize the glass substrate after step (2), the sensitization process including immersing the glass substrate in a Sn-containing solution. 2+ In the activation solution, a constant current bias voltage is applied to the glass substrate through the V-shaped conductive block, causing Sn to... 2+ They migrate and adsorb to the bottom of the through-hole; (4) The glass substrate treated in step (3) is immersed in a solution containing Pd. 2+ A continuous catalytic layer is formed in the activation solution, and a constant current bias voltage is applied to the glass substrate through the V-shaped conductive block during the formation of the continuous catalytic layer. (5) Immerse the glass substrate treated in step (4) into the electroless copper plating solution, and apply segmented constant current bias voltage through the V-shaped conductive block to perform electrochemical copper plating. (6) The glass substrate processed in step (5) is transferred to an electroplating tank to electroplat a Cu layer to achieve metallization. In steps (2) to (6), the glass substrate is always held by the target frame and the V-shaped conductive block, and the V-shaped conductive block is always positioned above the liquid surface of each wet process tank and does not contact any tank liquid; and After the glass substrate is transferred to the processing liquid for each step (2) to (6), and before each step is performed, the glass substrate is subjected to constant voltage pulse reduction treatment by the V-shaped conductive block.

[0006] This method achieves a continuous charged conductive structure throughout the entire process by using a conductive circuit composed of a V-shaped conductive block outside the liquid surface and an edge busbar ring. Combined with a constant voltage cathode reduction pulse after entering the tank, it solves the problem of the impact of copper layer surface oxidation on electroplating quality during process transfer, thereby obtaining a high-quality TGV metallized substrate.

[0007] According to an embodiment of this application, the pickling solution in step (2) comprises 3-5% by volume H2SO4 and a weak acid, wherein the weak acid is 1-5 g / L ascorbic acid or 5-10 g / L citric acid, the glass substrate comprises a seed layer, the pickling process comprises removing oxides from the surface of the seed layer, the thinning amount of the seed layer is less than or equal to 1 nm, the constant current bias applied in step (2) is 0.02-0.05 A, the processing time is 30-60 s, and the temperature of the bath chamber is 20-25 °C; or the glass substrate surface has no seed layer, and the constant current bias applied in step (2) is 0.01-0.05 A. This can further improve the quality of the pickling process.

[0008] According to embodiments of this application, the method satisfies at least one of the following conditions: the sensitization solution in step (3) comprises 15-25 g / L SnCl2·2H2O and 10-15 mL / L HCl, the constant current bias voltage of the sensitization treatment is 0.015-0.025 A, and the treatment time is 60-120 s; the activation solution in step (4) comprises 0.02-0.15 g / L PdCl2 and 8-12 mL / L HCl, the constant current bias voltage is 0.025-0.035 A, and the treatment time is 60-120 s; the electroless copper plating solution in step (5) comprises 8-12 g / L CuSO4·5H2O, 25-35 g / L EDTA-2Na, 6-10 mL / L HCHO, and 1-2 mg / L α-α' bipyridine, and the pH of the electroless copper plating solution is... 12.0-12.8, processing temperature is 30-32℃; the electroplating solution in step (6) includes 180-220g / L CuSO4·5H2O, 50-70g / L H2SO4, and 40-60ppm Cl. - The additives include at least one of leveling agents, brighteners, and wetting agents, and the temperature of the electroplated Cu layer is 22-26°C.

[0009] According to an embodiment of this application, the electrochemical copper plating in step (5) is achieved by applying segmented constant current bias voltage, which includes: applying a current of 0.05A for 0-2 minutes, a current of 0.3A for 2-5 minutes, and a current of 0.6A for 5-45 minutes; after performing the electrochemical copper plating for 2 minutes, the electrochemical plating tank is subjected to N2 bubbling treatment, with a bubbling pressure of 0.015 bar ± 0.002 bar. This can further improve the quality of electrochemical copper plating.

[0010] According to an embodiment of this application, after step (5) and before step (6), a three-stage cleaning operation is further included on the glass substrate. The three-stage cleaning includes: spraying with 5% volume fraction H2SO4; spraying with deionized water; and immersing with deionized water. During the three-stage cleaning process, a constant current bias voltage of 0.02A is applied to the glass substrate. This can further improve the quality of the treatment in step (6).

[0011] According to an embodiment of this application, the electroplated Cu layer in step (6) is achieved by the following operation: a constant voltage cathode reduction pulse is applied to the glass substrate through the V-shaped conductive block to reduce the oxide on the electrochemically plated copper surface. The voltage of the constant voltage cathode reduction pulse is -0.3V to -0.5V, the duration is 0.3-1.0s, and the current limit value is 0.1-0.3ASD. Subsequently, a bipolar phase-shifting pulse current is applied. The forward current of the bipolar phase-shifting pulse current is 1.0-2.0ASD, the reverse current is 0.1-0.2ASD, the forward-reverse duty cycle is 10:1 to 20:1, the forward pulse width is 200-300ms, and the reverse pulse width is 10-20ms. When the bipolar phase-shifting pulse current is applied, the glass substrate is clamped by the flying target frame and the V-shaped conductive block and oscillated horizontally along the X-axis.

[0012] In another aspect of this application, a system for metallizing a TGV substrate based on the aforementioned method is proposed. This system includes: a conductive moving component comprising a movable target frame and a V-shaped conductive block fixed to the target frame, the target frame having elastic contacts at both ends; and a perforated titanium plate anode assembly comprising multiple wet plating tanks, the multiple wet plating tanks being used for pickling, sensitization, activation, electroless copper plating, and electroplating copper treatments, each of the multiple wet plating tanks having a perforated titanium plate as a counter electrode, and each of the multiple wet plating tanks having a fixed busbar at its opening. The system comprises: a row for establishing an electrical connection via the elastic contact when the target frame is inserted into the slot; an X-axis horizontal swing assembly connected to the target frame for driving the target frame to reciprocate horizontally along a direction parallel to the TGV hole axis; a power supply assembly electrically connected to the electrodes in the multiple wet-processing tanks for independently controlling the electrical signals applied to the counter electrodes in each wet-processing tank; and a control assembly connected to both the X-axis horizontal swing assembly and the power supply assembly for controlling the power supply mode of the power supply assembly and the swing parameters of the X-axis horizontal swing assembly. This system allows for the simple metallization of the TGV substrate using the aforementioned method.

[0013] According to an embodiment of this application, the V-shaped conductive block is made of industrial pure titanium, and the contact surface has a gold-plated layer with a thickness ≥0.5μm. The spring loading pressure of the V-shaped conductive block is ≥8N / block, and the contact resistance is <0.1Ω. The perforated titanium plate is made of industrial pure titanium perforated plate. The perforated titanium plate in the wet process tank corresponding to the chemical copper plating and electroplating copper plating has a Pt / Ti coating or a mixed metal oxide coating. The glass substrate to be processed held by the V-shaped conductive block is the working electrode. The single-sided spacing between the counter electrode and the working electrode in the multiple wet process tanks is 80mm±2mm. The ratio of the counter electrode area to the effective conductive area of ​​the working electrode, Aan / Ac, is ≥5.

[0014] According to an embodiment of this application, the chemical copper plating and electroplating copper treatments are completed in the same wet process tank, which has a drain hole for replacing the treatment solution.

[0015] According to an embodiment of this application, the system further includes: a gas bubbling assembly for bubbling the glass substrate to be processed in the wet process tank; a water spray assembly and an acid spray assembly for spraying the glass substrate to be processed in the wet process tank; and an external circulation heat exchange assembly connected to the plurality of wet process tanks for controlling the temperature in the plurality of wet process tanks.

[0016] In another aspect of this application, a metallized TGV substrate is provided, wherein the TGV substrate is prepared using the method or system described above, wherein the aspect ratio of the through holes of the TGV substrate is 6:1 to 12:1, the inner wall roughness Ra≤1.2μm, the metallization conductivity is 100%, and the thickness of the metal layer at the bottom of the hole is not less than 48% of the thickness of the metal layer at the opening of the hole.

[0017] In summary, the above-described method, system, and TGV substrate prepared therefrom have at least one of the following beneficial effects: 1. High conductivity of through-hole: Piston mass transfer is achieved through bias-driven deep-hole activation and X-axis horizontal oscillation. High conductivity can be achieved even in TGV structures with large depth-to-width ratio and / or without PVD seed layer, with conductivity reaching up to 100%, far exceeding the 47-65% conductivity of traditional colloidal palladium solutions.

[0018] 2. Near-zero copper layer loss: Electrode-based electrochemical reduction and pickling are achieved using electrodes in a wet etching bath. The process primarily employs electrochemical reduction, supplemented by ascorbic acid chemistry. Only oxides are removed without etching the underlying copper layer, resulting in minimal copper layer thinning (≤1 nm, measured by XPS). 0 With a yield of >95%, it solves the problem of seed layer breakage caused by traditional acid washing thinning of 5-15nm.

[0019] 3. Continuous live-line protection throughout the entire process improves coating quality: The V-shaped conductive block outside the liquid surface, combined with the edge busbar structure, ensures continuous charging throughout the entire process. Combined with the constant-voltage cathode reduction pulse after immersion in the tank, it eliminates the impact of oxidation of the electroless copper plating surface during the transfer process on subsequent electroplating. Even with a transfer time extended to 10-15 seconds, the initial plating quality after a 0.5-second reduction pulse treatment shows no significant difference compared to the control group without exposed plating (fill rate deviation <2%), significantly reducing the stringent requirements of the production line on mechanical cycle time.

[0020] 4. Low raw material costs: By utilizing the V-shaped conductive block structure of the flying target frame, the conductive block does not come into contact with the bath liquid, thus avoiding scaling and chemical contamination problems at the contact surface of the V-shaped conductive block. Constant pressure pulse reduction treatment improves the efficiency of the reduction reaction, and the PdCl2 concentration is only 1 / 10 to 1 / 20 of that of the traditional colloidal palladium solution, reducing raw material costs by more than 80%.

[0021] 5. Enables efficient manufacturing: Electrochemical plating and electroplating can share the same tank. The electrochemical plating and electroplating functions can be switched with one click through the control components. The switching time is less than 30 minutes, and the switching process requires no disassembly or assembly, which greatly reduces equipment investment. Attached Figure Description

[0022] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the various drawings denote the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings depict only some embodiments according to this disclosure and should not be construed as limiting the scope of this disclosure.

[0023] Figure 1 This is a schematic flowchart of the preparation method of this application; Figure 2 This is a schematic diagram of the overall structure of the TGV metallization flexible manufacturing system of this application; Figure 3 This is a bar chart showing the comparison of test results from embodiments and comparative examples of this application.

[0024] Among them: 1- target frame, 2- V-shaped conductive block, 3- perforated titanium plate anode plate, 4- slotted fixed busbar, 5- power supply assembly, 6- control assembly. Detailed Implementation

[0025] In the following description, only certain exemplary embodiments are briefly described. As those skilled in the art will recognize, the described embodiments can be modified in various ways without departing from the spirit or scope of this disclosure, and different embodiments can be combined arbitrarily without conflict. Therefore, the drawings and description are considered to be exemplary in nature and not restrictive.

[0026] As one aspect of this disclosure, an embodiment provides a method for metallizing a TGV substrate. As previously mentioned, the prior art has the following main drawbacks when designing metallization for TGV substrates with large aspect ratios: (a) PVD seed layer is discontinuous under high aspect ratio Traditional TGV metallization processes follow a fixed path of "laser modification - etching for hole formation - sputtering seed layer - electroplating for filling". Physical vapor deposition (PVD) coverage drops sharply in micropores with an aspect ratio greater than 6:1. The seed layer thickness in the middle of the hole wall can be as low as 5 nm or even completely broken, leading to subsequent electroplating failure. When the inner hole wall roughness Ra > 0.5 μm, the discontinuity of the PVD seed layer is further aggravated, and a "shadowing effect" occurs at the unevenness of the hole wall, resulting in a seed layer coverage of less than 30% at the bottom of the deep hole. Although some studies have attempted to use electroless copper plating as a seed layer to replace PVD, the uniformity and adhesion of traditional colloidal palladium activation in deep holes still fail to meet mass production requirements.

[0027] (ii) Traditional acid pickling to reduce the thickness of the copper seed layer Current TGV pretreatment processes employ an acid etching step using dilute H₂SO₄ or HF solution immersion to remove the CuO / Cu₂O oxide layer from the copper seed layer surface. However, acid etching inevitably thins the copper layer by 5-15 nm while removing the oxide layer, potentially causing complete breakage of the already thin and discontinuous PVD seed layer. When the copper surface is exposed to air after acid etching, the Cu… 0 It will be rapidly re-oxidized (Cu2O is generated within 30 seconds), forming a cycle of repeated oxidation and removal losses.

[0028] (iii) Inter-process transfer leads to copper surface oxidation and Pd catalyst layer failure. TGV metallization typically requires separate chemical plating and electroplating equipment, and there are two problems during the substrate transfer process between processes: on the one hand, the Pd formed after sensitization / activation... 0 The catalyst layer begins to oxidize upon exposure to air, forming insulating PdO / Pd(OH)2. Meanwhile, during the transfer of the electroless copper plating layer to the electroplating bath, a thin Cu2O / CuO layer forms on its surface, leading to increased interfacial contact resistance and decreased uniformity of plating at the start of the process. Power outages during transfers between processes deprive the catalyst and copper layers of cathodic protection, further exacerbating oxidation. These combined issues result in a 15-20% decrease in conductivity.

[0029] (iv) Separate chemical plating / electroplating equipment, high investment and complex switching Existing solutions require separate equipment for electroless plating and electroplating, resulting in high investment costs and large floor space requirements. Different electrode specifications are used in the electroless plating and electroplating sections, necessitating anode replacement during process switching, thus hindering flexible manufacturing. Furthermore, in acidic electroplating systems, traditional pure titanium anodes are prone to passivation, while soluble phosphorus copper anodes produce anode sludge and Cu. + Byproducts contaminate the plating solution.

[0030] This application aims to address the shortcomings of the prior art by providing a flexible manufacturing method and system for metallizing through-holes in TGV glass, achieving the following objectives: (1) No PVD continuous seed layer is required to achieve 100% conductivity metallization filling in TGV with a depth-to-width ratio ≥ 6:1, which is suitable for harsh conditions with inner hole wall roughness Ra ≤ 1.2 μm. (2) Through the continuous conductive structure of "V-shaped conductive block outside the liquid surface + edge bus ring" throughout the process, combined with constant voltage cathode reduction pulse after entering the tank, the influence of copper layer surface oxidation on electroplating quality during process transfer is completely solved. (3) The same set of hardware equipment can quickly switch between chemical plating and electroplating functions (<30min) without disassembling or assembling any hardware; (4) A perforated titanium plate is used as a unified anode to balance the air permeability of N2 bubbling and the rigidity of pulse current, thus avoiding passivation and anode mud contamination.

[0031] Specifically, refer to Figure 1 The method includes the following steps: (1) Cleaning the glass substrate and gas replacement treatment in the holes. In this step, a glass substrate is first provided. This glass substrate has a through-hole, and a conductive bus ring is provided at the edge of the glass substrate. The aspect ratio of the through-hole is greater than or equal to 6:1. The glass substrate is then cleaned and the gas inside the hole is replaced.

[0032] Specifically, the glass substrate with TGV can first be plasma cleaned using Ar or Ar / H2 mixed gas, with a volume ratio of 95 / 5. At an RF power of 200-500W, both sides are treated for 30-60 seconds each, thereby introducing hydroxyl (-OH) active groups onto the glass surface and hole walls, improving its hydrophilic properties.

[0033] Following vacuum venting and N2 replacement, the substrate is placed in a vacuum chamber and evacuated to a pressure less than -0.095 MPa (absolute pressure ≤ 5 kPa) and held for 30-60 seconds, allowing the air inside the TGV micropores to expand and escape. Then, high-purity N2 (e.g., purity ≥ 99.999%, dew point ≤ -40℃) is slowly reintroduced to atmospheric pressure, allowing nitrogen molecules to fill the pore space in gaseous form. The TGV pore size is in the micrometer range (typically 10-100 μm), much larger than the dynamic diameter of nitrogen molecules (approximately 0.36 nm). Nitrogen gas undergoes only van der Waals adsorption on the glass pore walls, with an adsorption layer thickness < 1 nm, having no noticeable impact on the effective flow cross-section within the pores or on the subsequent wetting and replacement of wet-process pharmaceutical solutions. This step provides a barrier-free channel for subsequent pharmaceutical solutions to enter the micropores.

[0034] In this step, vacuum exhaust and N2 replacement cycles can be performed 2-3 times. When the depth-to-width ratio of the through hole is ≥10:1 or the hole diameter is ≤50μm, this can be increased to 3 times. After exiting the cavity, the next liquid treatment process can be carried out within 30 seconds to prevent the N2 in the hole from being gradually replaced and flowing back by the ambient humid air if more than 30 seconds are exceeded.

[0035] According to an embodiment of this application, a conductive bus ring with a width of 3-5 mm can be prefabricated around the effective metallization area of ​​the glass substrate. For example, a Ti / Cu layer can be prepared by PVD, or a conductive paste or chemical plating can be used to form the conductive bus ring. The bus ring is located at the edge of the substrate and does not overlap with the TGV hole array. The conductive bus ring can serve as a clamping contact of the V-shaped conductive block, withstand the spring loading pressure (≥8N / block), and serve as a transverse current collector conductor for the current to flow from the target bus to the copper layer of each TGV hole on the substrate. In subsequent processing, an initial conductive path can be provided when the substrate has not yet formed a continuous copper layer in the early stage of chemical plating. On the substrate with a seed layer, the bias current flows through the bus ring-hole-hole bottom to maintain cathode polarization. For a substrate without a PVD seed layer, the bus ring also serves as a temporary cathode. In the subsequent step (2), a low current of 0.01A is applied only for wetting and conduction. After the chemically plated copper covers the hole wall, the conductive path changes to bus ring-chemically plated copper layer-hole bottom.

[0036] (2) The glass substrate is subjected to acid pickling treatment. In this step, the glass substrate undergoes acid pickling. The glass substrate is clamped and electrically connected via a target frame and a V-shaped conductive block fixed to the target frame. Specifically, the target frame has elastic contacts at both ends for connecting to the fixed busbar at the opening of the wet pickling tank. The wet tank has a perforated titanium plate as the counter electrode. The V-shaped conductive block contacts the conductive busbar on the glass substrate, and a spring-loaded pressure on the busbar conducts current from the target frame to the conductive busbar on the substrate, achieving electrical connection. This process keeps the V-shaped conductive block above the liquid surface to prevent contamination by the treatment liquid.

[0037] During the pickling process, a constant current bias voltage is applied to the conductive bus ring by a V-shaped conductive block fixed on a movable target frame to remove oxides from the surface of the seed layer. The seed layer is thinned by less than or equal to 1 nm. This improves the quality of subsequent processing, providing a cleaner and more reactive surface.

[0038] Specifically, in this step, the pickling solution includes 3-5% by volume H2SO4 and a weak acid, specifically 1-5 g / L ascorbic acid or 5-10 g / L citric acid. Thus, the reactivity and cleanliness of the substrate surface can be enhanced through a dual mechanism of electrochemical reduction and acid reagent reduction. Driven by a constant current bias voltage at the cathode, electrons are directly injected into the copper surface, electrochemically reducing CuO / Cu2O to Cu. This process involves two steps: 2CuO + 2H + + 2e - → Cu2O + H2O; and Cu2O + 2H + + 2e - → 2Cu + H2O The overall reaction can be simplified to: CuO + 2H + + 2e - → Cu + H2O.

[0039] An acidic environment is conducive to the complete reduction of CuO to metallic Cu, while under alkaline conditions, Cu2O is mainly generated. Therefore, using an acidic treatment solution is beneficial to improving the reduction effect.

[0040] Meanwhile, the presence of ascorbic acid in the treatment solution further promotes a synergistic effect, primarily due to the dissolution of CuO in the acidic solution: CuO + 2H + → Cu 2+ + H2O Subsequently, ascorbic acid will convert Cu 2+ Reduced to Cu + : 2Cu 2+ + C6H8O6→ 2Cu + + C6H6O6+ 2H + Therefore, it can help promote the removal of CuO.

[0041] When the glass substrate includes a seed layer metal, the pickling process can remove oxides from the surface of the seed layer, and the seed layer thinning amount is less than or equal to 1 nm. At this time, the constant current bias voltage is applied at 0.02-0.05 A, the processing time is 30-60 s, and the chamber temperature is 20-25 °C.

[0042] When there is no seed layer on the glass substrate surface, the constant current applied in this step can be 0.01-0.05A. This allows for charged wetting, improving the efficiency and quality of subsequent processing.

[0043] (3) Sensitize the glass substrate. According to an embodiment of this application, in this step, the glass substrate processed in step (2) undergoes a sensitization treatment. The sensitization treatment includes immersing the glass substrate in an immersion solution containing Sn. 2+ In the activation solution, a constant current bias voltage is applied to the glass substrate through a V-shaped conductive block, causing Sn to...2+ It migrates and adsorbs to the bottom of the through hole.

[0044] Specifically, the sensitization treatment solution includes 15-25 g / L SnCl2·2H2O and 10-15 mL / L HCl, the constant current bias voltage for sensitization treatment can be 0.015-0.025 A, and the treatment time is 60-120 s. Under bias drive, Sn... 2+ Ions migrate and adsorb directionally towards the bottom of the pore along the electric field lines, causing Sn at the bottom of the deep pore to be absorbed. 2+ The concentration is significantly higher than that under no bias conditions, thereby improving the quality of metal deposition at the bottom of the well.

[0045] In order to eliminate the surface oxide layer formed during the process of transferring the glass substrate to be treated from step (2) to the wet bath in step (3), the glass substrate can also be subjected to constant voltage pulse reduction treatment using a flying target frame and a V-shaped conductive block before sensitization treatment, and the trace amount of oxides can be removed by electrochemical reduction process.

[0046] (4) Forming the continuous catalyst layer on the glass substrate. According to an embodiment of this application, in this step, the glass substrate treated in step (3) is immersed in a solution containing Pd. 2+ A continuous catalytic layer is formed in the activation solution, and a constant current bias voltage is applied to the glass substrate through a V-shaped conductive block during the formation of the continuous catalytic layer.

[0047] Specifically, the activation solution may include 0.02-0.15 g / L of PdCl2 and 8-12 mL / L of HCl, the constant current bias voltage is 0.025-0.035 A, and the processing time is 60-120 s.

[0048] For example, in this step, the substrate can be immersed in an activation solution, and a constant current bias voltage can be applied. Sn adsorbed on the hole walls under the bias voltage drive... 2+ Pd 2+ The material is co-reduced to Pd, forming a continuous catalytic layer on the pore walls and bottom of the TGV, with a coverage rate as high as 85-92%. Under this condition, the PdCl2 concentration is only 1 / 10 to 1 / 20 of that of the traditional colloidal palladium solution, reducing raw material costs by more than 80%.

[0049] In some embodiments, the PdCl2 concentration can be adjusted according to the depth-to-width ratio of the through-hole. When the depth-to-width ratio is 6:1-8:1, the PdCl2 concentration can be 0.05 g / L; when the depth-to-width ratio is 8:1-10:1, the PdCl2 concentration is preferably 0.08-0.10 g / L; and when the depth-to-width ratio is 10:1-12:1 and the roughness of the hole wall Ra is >1.0 μm, the PdCl2 concentration is preferably 0.12-0.15 g / L.

[0050] Similarly, in order to remove the surface oxide layer formed during the transfer process in different steps, before the treatment in step (4), the glass substrate can be subjected to constant voltage pulse reduction treatment using a flying target frame and a V-shaped conductive block, and the trace amount of oxide can be removed by electrochemical reduction process.

[0051] (5) Electrochemical copper plating is performed on the glass substrate. In this step, the glass substrate treated in step (4) is immersed in a chemical copper plating solution, and electrochemical copper plating is performed by applying a segmented constant current bias voltage through a V-shaped conductive block.

[0052] Specifically, the substrate can be immersed in a chemical copper plating solution, and a segmented constant current bias voltage is applied using a finned frame and a V-shaped conductive block. The chemical copper plating solution in this step can consist of 8-12 g / L CuSO4·5H2O, 25-35 g / L EDTA-2Na, 6-10 mL / L HCHO, and 1-2 mg / L α-α'-bipyridine. The pH of the chemical copper plating solution is 12.0-12.8, and the processing temperature is 30-32℃. The segmented constant current bias voltage includes: applying a 0.05A current for 0-2 min to prevent hydrogen evolution; applying a 0.3A current for 2-5 min to allow the active metal to spread; and applying a 0.6A current for 5-45 min to thicken the metal layer.

[0053] In some embodiments, any fluid disturbance may be prohibited for the first 2 minutes of electroless plating to prevent the washing away of unreduced Pd. 2+ and the newly adsorbed Pd 0 After 2 minutes of electrochemical copper plating, the electrochemical plating bath can be subjected to N2 bubbling treatment. The bubbling pressure can be 0.015 bar ± 0.002 bar. A linear soft start of 2-2.5 minutes is used, while liquid spraying (pressure 0.1-0.3 bar) is activated to enhance liquid film renewal in the orifice area. An external circulation heat exchange system, such as a plate heat exchanger and a circulation pump, can be added to this step to achieve precise control of the plating solution temperature. The flow rate of the heat exchange fluid can be 2-3 L / min, with a filtration accuracy of 5 μm, thereby ensuring temperature uniformity of ±0.5℃. This further improves the quality of electrochemical copper plating.

[0054] To further improve the quality of subsequent processing, after step (5) and before step (6), a three-stage cleaning operation is further included on the glass substrate. The three-stage cleaning specifically includes: spraying with 5% volume fraction H2SO4; spraying with deionized water; and immersion in deionized water. A constant current bias of 0.02A is applied to the glass substrate during the three-stage cleaning process. According to an embodiment of this application, during immersion, the substrate can also be held in place by a target frame and oscillated along the X-axis for a distance of 20mm, repeated 3-5 times. The residual Na at the bottom of the hole before the glass substrate enters the electroplating tank in the next step... + It can reach a level of less than 5 ppm.

[0055] Similarly, in order to eliminate the surface oxide layer formed during the process of transferring the glass substrate to be treated from the previous processing step to the wet bath of the next processing step, a constant voltage pulse reduction treatment can be performed on the glass substrate using a flying target frame and a V-shaped conductive block before the processing in step (5), and a trace amount of oxide can be removed by electrochemical reduction process.

[0056] (6) Electroplating a Cu layer onto the glass substrate to achieve metallization. In this step, the glass substrate processed in step (5) is transferred to an electroplating tank to electroplat a Cu layer for metallization. Before immersing the glass substrate into the electroplating tank using a target frame, the elastic contacts of the target frame can be pre-connected to the busbar at the tank opening to restore the bias voltage instantly upon immersion. After immersion and before the electroplating process begins, a constant voltage cathode reduction pulse can be applied to reduce the Cu2O / CuO generated on the surface of the electroless copper plating layer during the transfer process to metallic copper.

[0057] The electroplating solution in this step may include 180-220 g / L CuSO4·5H2O, 50-70 g / L H2SO4, 40-60 ppm Cl-, and additives. The additives include at least one of a leveling agent, a brightener, and a wetting agent. The temperature for electroplating the Cu layer is 22-26°C. Specifically, the leveling agent may be PEG (polyethylene glycol), the brightener may be SPS (sodium 3-sulfopropyl disulfide), and the wetting agent may be JGB (JanusGreen B).

[0058] The electroplated Cu layer in step (6) can be realized by the following operation: applying a constant-voltage cathodic reduction pulse to the glass substrate through a V-shaped conductive block to reduce oxides on the surface of the electrochemically copper-plated layer. The voltage of the constant-voltage cathodic reduction pulse is -0.3V to -0.5V, which may be a voltage relative to the working electrode. The duration is 0.3-1.0s, and the current limiting value is 0.1-0.3 ASD. The voltage of this pulse is much lower than the deposition potential of copper, Cu 2+ with a reduction potential of about +0.34V vs SHE, so no additional copper layer is deposited, and only the surface oxides are selectively reduced. Immediately after the reduction pulse is completed, switch to a bipolar phase-shifted pulse current for electroplating hole filling: the forward current of the bipolar phase-shifted pulse current is 1.0-2.0 ASD, the reverse current is 0.1-0.2 ASD, the forward-reverse duty ratio is 10:1 to 20:1, the forward pulse width is 200-300ms, and the reverse pulse width is 10-20ms. When performing the bipolar phase-shifted pulse current, the glass substrate is clamped by the flying target frame and the V-shaped conductive block to perform horizontal swinging along the X axis, thereby achieving uniform bottom-up filling.

[0059] To further improve the performance of the metallized substrate obtained by this method, the method may further include a post-treatment operation. Specifically, the post-treatment may include steps such as water washing, passivation, blow-drying and performance testing. Specifically, deionized water can be used for spray rinsing first, followed by BTA passivation. The concentration of BTA (benzotriazole) can be 1-2g / L, pH 7-8, room temperature 20-25°C, and the treatment time is 20-40s. Subsequently, a final water washing operation can be performed, followed by blow-drying with N2.

[0060] Finally, the performance of the substrate can be tested, for example, using a multimeter for resistance testing, and a resistance of <10Ω can be judged as qualified. Sampling inspection of metallographic sections can also be carried out, with 1 substrate sampled respectively from the beginning, middle and end of each batch to detect the copper thickness at the hole bottom and the copper thickness at the hole opening, and a filling is judged as qualified if the thickness at the hole bottom is greater than 48% of the thickness at the hole opening. The conduction rate can also be measured, and the detection method can be to use a multimeter to test the resistance of each hole one by one, and a single hole resistance of <10Ω is judged as conductive. The conduction rate must be 100%.

[0061] According to the embodiments of the present application, each wet processing step can be completed in a wet tank. Fixed busbars are provided at the notches on both sides of the wet tank, and elastic copper brush contacts are installed at both ends of the flying target frame. When the flying target frame is lowered into the tank and reaches the designated position, the copper brush contacts automatically press against the busbars at the tank notches, connecting the independent power supply of the tank. When the flying target frame transfers from one tank to the next, the elastic contacts separate from the busbars of the current tank, the flying target frame translates in the air to above the next tank, and then descends into the tank to make the elastic contacts press against the busbars of the next tank. During this process, the substrate is exposed to the air, and a sub-nanometer Cu2O / CuO oxide film will form on the surface of the electroless copper plating layer.

[0062] To address this issue, this application does not rely on shortening the mechanical transfer time to reduce the requirements for equipment production line cycle time and positioning accuracy. Instead, it adds a constant-voltage cathode reduction pulse step after the target enters the electroplating tank and before the start of the main electroplating pulse. As mentioned earlier, the reduction pulse parameters can be a constant voltage of -0.3V to -0.5V (relative to the working electrode), a duration of 0.3-1.0s, and a current limit of 0.1-0.3ASD. Under the action of this pulse, Cu2O / CuO is electrochemically reduced to Cu: Cu2O + 2H + + 2e - → 2Cu + H2O CuO + 2H + + 2e - → Cu + H2O Once the restoration is complete, the system immediately switches to subsequent processing steps. This restoration pulse step can be configured before and after all transfer steps. The restoration pulse can be managed via PLC recipes and switched with a single button based on the power mode, requiring no additional hardware.

[0063] Furthermore, the V-shaped conductive block of this application does not come into contact with the liquid surface during the process. If the V-shaped conductive block is immersed in the plating solution, copper ions in the chemical plating solution will undergo autocatalytic deposition at the contact surface between the V-shaped conductive block and the substrate. After several batches, the contact resistance will increase from <0.1Ω to >5Ω, leading to bias voltage failure. This application fixes the V-shaped conductive block on the top of the target frame, always positioned above the liquid surface (≥20mm from the liquid surface), extending downwards to below the liquid surface only through the busbar ring at the edge of the substrate, completely avoiding the problem of scaling at the contact surface. This is the hardware basis for achieving "zero disassembly and switching of the same set of V-shaped conductive blocks between chemical plating and electroplating, and 30-minute uninterrupted liquid change".

[0064] In another aspect of this application, a system for metallizing a TGV substrate based on the aforementioned method is proposed. (Reference) Figure 2 The system includes a conductive moving component, which comprises a movable target frame 1 and a V-shaped conductive block 2 fixed on the target frame. The target frame has elastic contacts at both ends. The perforated titanium plate anode assembly includes multiple wet processing tanks, which are used for pickling, sensitization, activation, electroless copper plating, and electroplating copper treatments, respectively. Each wet processing tank has a perforated titanium plate 3 as a counter electrode. Each wet processing tank opening is equipped with a fixed busbar 4 for electrical connection via the elastic contacts when the target frame enters the tank. An X-axis horizontal swing assembly, connected to the target frame, drives the target frame to swing horizontally reciprocatingly along a direction parallel to the TGV hole axis, as shown in the X-axis direction. Figure 2This can be a top-down view of the system. The glass substrate to be processed can be inserted into the wet processing tank perpendicular to the plane of the paper to contact the processing liquid. The top of the busbar conductive ring of the glass substrate is located on the liquid surface and is clamped by the V-shaped conductive block 2. The power supply component 5 is electrically connected to the electrodes in the multiple wet processing tanks and is used to independently control the electrical signals applied to the counter electrodes in each wet processing tank. The control component 6 is connected to both the X-axis horizontal swing component and the power supply component and is used to control the power supply mode of the power supply component and the swing parameters of the X-axis horizontal swing component. This system can easily realize the metallization of the TGV substrate according to the aforementioned method.

[0065] According to embodiments of this application, the target frame 1 can be made of PVDF or titanium alloy, resistant to acid and alkali corrosion, and does not participate in the conductive circuit. The V-shaped conductive block 2 is made of industrial pure titanium, with a gold-plated layer on the contact surface. The thickness of the gold plating layer is ≥0.5μm, the spring loading pressure of the V-shaped conductive block is ≥8N / block, and the contact resistance is <0.1Ω. A micro-ohmmeter can be set at the slot of the target frame 1 to measure the contact resistance between the V-shaped conductive block 2 and the target busbar 4 online. When the contact resistance is >0.3Ω, the control component 6 (e.g., a PLC (Programmable Logic Controller) will automatically prompt "V-shaped conductive block contact surface maintenance", allowing for shutdown, polishing of the gold-plated contact surface, and restoration. The target frame 1 has elastic contacts at both ends, and each wet-process tank opening has a fixed busbar 4, thereby enabling automatic power connection when the target frame drives the glass substrate into the tank, allowing the glass substrate to establish an electrical connection before immersion in the liquid.

[0066] The perforated titanium plate 3 is made of industrial pure titanium perforated plate. The perforated titanium plate in the wet plating tanks corresponding to the chemical copper plating and electroplating copper plating processes has a Pt / Ti coating or a mixed metal oxide coating. Specifically, a pure titanium Gr2 (industrial pure titanium) perforated plate can be used in the chemical plating section, and a Pt / Ti coated or MMO (mixed metal oxide) coated perforated plate can be used in the electroplating section. The glass substrate to be processed, held by a V-shaped conductive block, serves as the working electrode. The single-sided spacing between the counter electrode and the working electrode in multiple wet plating tanks is 80mm ± 2mm, and the ratio of the counter electrode area to the effective conductive area of ​​the working electrode, Aan / Ac, is ≥ 5. Specifically, the single-sided electrode spacing Dca of the anode and cathode throughout the entire process can be uniformly adjusted to 80mm ± 2mm. Large-size substrates (substrate plane edge size > 150mm) can adopt a four-sided anode layout to ensure Aan / Ac ≥ 5 (Aan is the effective conductive area of ​​the perforated titanium plate anode, and Ac is the effective conductive area of ​​the glass substrate to be metallized). The opening ratio and arrangement of the perforated titanium plate can be adjusted according to the actual situation to ensure the air permeability of N2 bubbling and the uniformity of pulse current distribution.

[0067] Therefore, the system may further include an X-axis drive assembly for driving the conductive moving component to achieve horizontal reciprocating oscillation of the target frame 1 along a direction parallel to the TGV hole axis. The X-axis drive assembly may include a servo motor (such as a 750W power electrode), a ball screw, and a linear guide. The X-axis drive assembly can be connected to the aforementioned PLC controller. The X-axis travel is adjustable from 10-50mm via software settings, the speed is adjustable from 10-100mm / s via software settings, and the repeatability is ±0.05mm. The oscillation parameters of each station are managed by the PLC. In some specific embodiments, the following oscillation parameters may be used: chemical plating main tank travel 50mm, peak speed 70mm / s, frequency 0.22Hz, endpoint pause 0.3s; pulse electroplating tank travel 10mm, peak speed 20mm / s, frequency 0.32Hz, endpoint pause 0.5s; other wet plating tanks (sensitization / activation / washing) travel 20-40mm, speed 30-60mm / s. The above parameters can be adjusted using PLC software according to the substrate size and the aspect ratio of the TGV. Since the X-axis swing direction is parallel to the TGV hole axis, a forced piston flow along the hole axis can be generated inside the hole—when the substrate moves horizontally to the right, the liquid inside the hole flows relatively to the left, "drawing" fresh reaction liquid into the bottom of the hole; when the substrate moves in the opposite direction, the reaction products inside the hole are "pushed" out of the hole, achieving complete replacement of the reaction liquid in the deep hole.

[0068] The power supply component 5 and control component 6 enable independent programmable control of the potential of each wet plating tank, ensuring that a failure in one wet plating tank does not affect the production of other tanks. Specifically, wet plating tanks for reduction pickling, sensitization, activation, and transition cleaning can use a 0-5V / 0-0.5A low-power programmable DC power supply with a constant current accuracy of ±0.2%FS. The main electroless plating tank can use a 0-12V / 0-2A programmable DC power supply. The pulse electroplating tank can use a 0-12V / 0-10A bipolar phase-shifting pulse power supply with independent forward and reverse current settings, a programmable phase-shifting dead zone of 0-20ms, and support for inserting a constant-voltage reduction pulse segment before the main pulse.

[0069] According to embodiments of this application, both electroless copper plating and electroplating can be completed using the same wet plating tank, which has a drain hole for replacing the treatment solution. This allows for switching between electroless and electroplating modes using the same hardware system, with a switching time of less than 30 minutes, thereby improving production efficiency and reducing production costs. Specifically, the shared use of electroless and electroplating processes can be achieved through the following operations: (1) Drain the old tank liquid; (2) Clean the tank twice with deionized water; (3) Inject new medication; (4) PLC one-button power mode switching; (5) PLC allows one-button switching of swing parameters; (6) PLC can switch N2 bubbling / stirring / spraying parameters with one key; (7) PLC one-button switching of temperature control settings; (8) pH probe 2-point calibration; (9) Production starts after the operator confirms on the touchscreen.

[0070] Throughout the entire switching process, the anode (perforated titanium plate), target frame, V-shaped conductive block, swing module, and spray pipeline do not require any disassembly or assembly.

[0071] According to an embodiment of this application, the system further includes: a gas bubbling assembly, a water spraying assembly, an acid spraying assembly, and an external circulation heat exchange assembly. The gas bubbling assembly is used to bubble gas onto the glass substrates to be processed in the wet processing tank. The water spraying assembly and the acid spraying assembly are used to spray the glass substrates to be processed in the wet processing tank. The external circulation heat exchange assembly is connected to the plurality of wet processing tanks and is used to control the temperature in the plurality of wet processing tanks. This enables a multi-fluid collaborative system.

[0072] Specifically, the above components can be used to perform the following operations sequentially on the main electroless plating tank: N2 bubbling (adjustable from 0-0.02 bar, linear soft start in 2-2.5 min), liquid spraying (0.1-0.3 bar, orifice enhancement), and external circulation heat exchange. During cleaning, the transition tank can be used for the following treatments: dilute H2SO4 spraying (5% v / v, 5 s), deionized water spraying (10 s), and deionized water immersion (30 s, X-swing 20 mm). The electroplating tank is subjected to weak N2 stirring and external circulation heat exchange (temperature uniformity ±1℃). All wet plating tanks can be pre-installed with N2 bubbling pipes and deionized water spray pipes, activated according to the PLC formula. Control component 6 can have a PLC controller to manage the power mode (including reduction pulse parameters), oscillation parameters, fluid parameters, and temperature control setpoint switching for each station, enabling one-button switching between electroless plating and electroplating functions.

[0073] In another aspect of this application, a metallized TGV substrate is provided, wherein the TGV substrate is prepared using the method or system described above, wherein the aspect ratio of the through holes of the TGV substrate is 6:1 to 12:1, the inner wall roughness Ra≤1.2μm, the metallization conductivity is 100%, and the thickness of the metal layer at the bottom of the hole is not less than 48% of the thickness of the metal layer at the opening of the hole.

[0074] The method proposed in this application will be described in detail below using specific embodiments. Operations not explicitly described in the embodiments are conventional experimental methods, and reagents used, unless otherwise specified, are commercially available conventional reagents.

[0075] Example 1 Based on a TGV glass substrate (borosilicate glass, effective area 50mm × 50mm), a depth-to-width ratio of 6:1 and an inner hole wall roughness Ra≈0.8μm were obtained after laser-induced etching. A discontinuous seed layer of only 5-15nm thickness, Ti / Cu, was obtained by PVD sputtering in the middle of the hole wall. A PVD Ti / Cu bus ring was pre-fabricated at the substrate edge, with a width of 4mm and a thickness of 50nm for Ti and 300nm for Cu. Metallization was then performed sequentially according to the following steps: S1 Plasma Cleaning: Ar / H2 (95 / 5), 300W, 40s each for forward and reverse directions; S2 Vacuum Exhaust and N2 Replacement: Evacuate to ≤-0.095MPa and hold for 45s, then backfill with high-purity N2 (≥99.999%, dew point ≤-40℃) to atmospheric pressure, repeat 2 times, and allow 25s from the time the fluid exits the chamber to the time the fluid enters the liquid. S3 Charged reduction pickling: H2SO4 4% (v / v) + ascorbic acid 3g / L, constant current 0.03A, 45s, room temperature; S4 charged sensitization: SnCl2·2H2O 20g / L + HCl 12mL / L, constant current 0.02A, 90s, X pendulum 40mm / 60mm / s; S5 charged activation: PdCl2 0.05g / L + HCl 10mL / L, constant current 0.03A, 90s, X pendulum 40mm / 60mm / s; S6 Electrochemical Copper Plating: CuSO4 10g / L + EDTA-2Na 30g / L + HCHO 8mL / L + Bipyridine 1mg / L, pH 12.4, 31±0.5℃, segmented constant current 0.05A (0-2min) -0.3A (2-5min) -0.6A (5-30min); 2-2.5min N2 bubbling 0.015bar soft start, liquid spray 0.2bar, X swing 50mm / 70mm / s; S7 Electrical Transition: Before the target enters the electroplating tank, the elastic contact is pre-connected to the busbar, followed by dilute H2SO4 spray for 5s, DI spray for 10s, and DI immersion for 30s, with a constant current of 0.02A. S8 Pulse Electroplating: After the flying target enters the liquid, a constant voltage reduction pulse of -0.4V is applied for 0.5s (current limit 0.2ASD), then switched to a bipolar phase-shifting pulse: CuSO4 200g / L + H2SO4 60g / L + Cl - 50ppm+ additives, bipolar phase-shifting pulse with positive 1.5ASD / negative 0.15ASD, duty cycle 15:1, pulse width 285ms / 19ms / dead zone 10ms, X swing 10mm / 20mm / s, Dca=80mm, processing temperature 24℃; S9 Post-treatment: Deionized water wash - BTA (1.5g / L, pH 7.5, room temperature, 30s) - final wash - N2 drying.

[0076] The obtained TGV substrate was inspected: The conductivity is 100%, the copper thickness at the bottom of the hole is ≥ 65% of the copper thickness at the opening, and no detectable pores are found in the metallographic section.

[0077] Comparative Example 1 Using the substrate from Example 1, metallization was performed based on traditional colloidal palladium activation + chemical copper plating + DC electroplating, with no bias voltage, no X-axis oscillation, and no punched titanium plate anode: (1) Colloidal palladium activation: Immerse the substrate in a commercial colloidal palladium activation solution and treat at room temperature for 5-10 min without bias voltage; (2) Chemical copper plating: Conventional chemical copper plating solution is used, with no bias voltage and no X-axis oscillation, and copper plating is performed for 30 minutes; (3) DC electroplating: DC electroplating is performed using acidic copper sulfate electroplating solution, without bias voltage or X-axis oscillation.

[0078] The obtained TGV substrate was inspected: The conductivity was only 47%, the porosity at the orifice was 35%, and the voltage rose to 8V after 2 hours of anode tank pressure (passivation occurred).

[0079] Example 2 Based on aluminosilicate glass, through-holes with an aspect ratio of 10:1 and a wall roughness Ra≈0.5μm were fabricated via laser etching and HF hole enlargement, without any PVD seed layer. A PVD Ti / Cu bus ring, 4mm wide and 50nm thick Ti / 300nm thick Cu, was pre-fabricated at the substrate edge. Metallization was then performed sequentially according to the following steps: S1-S2 are the same as in Example 1, except as follows: S3 uses ascorbic acid 3g / L and constant current 0.01A for electrowetting only; S4-S5 are the same as in Example 1, but the PdCl2 in S5 is increased to 0.1 g / L; S6 plating time extended to 45 minutes; S7 is the same as in Example 1; S8 is the same as in Example 1 (including reduction pulse); S9 is the same as in Example 1.

[0080] The obtained TGV substrate was inspected: 100% conductivity, copper thickness at the bottom of the hole is ≥ 55% of the copper thickness at the opening.

[0081] Comparative Example 2 The substrate used in Example 2 is different in that it undergoes DC electroplating, and the metallization is performed without bias voltage or oscillation during the electroplating process: The obtained TGV substrate was inspected: The conductivity is only 82%.

[0082] Example 3 Based on alkali-free ultrathin glass, the through-hole has an aspect ratio of 12:1 and an inner wall roughness Ra≈1.2μm. The PVD sputtered Ti / Cu seed layer completely breaks at the center of the hole wall (0nm). A PVD Ti / Cu bus ring is prefabricated at the substrate edge (same as in Example 1). Metallization is performed sequentially according to the following steps: S1 Plasma Cleaning: Ar pure gas, 300W, 50s each for forward and reverse directions; S2 Vacuum Exhaust and N2 Replacement: Evacuate to ≤-0.098MPa and hold for 60s, then backfill with high-purity N2. Repeat 3 times. The time from exiting the chamber to entering the liquid is 22s. S3 Charged wetting: H2SO4 4% (v / v) + ascorbic acid 5g / L, constant current 0.01A, 45s, room temperature (wetting only, no reduction reaction). S4 charged sensitization: SnCl2·2H2O 25g / L + HCl 15mL / L, constant current 0.025A, 120s; S5 charged activation: PdCl2 0.15g / L + HCl 12mL / L, constant current 0.035A, 120s; S6 Electrochemical Copper Plating: CuSO4 12g / L + EDTA-2Na 35g / L + HCHO 10mL / L + Bipyridine 2mg / L, pH 12.4, 31±0.5℃, segmented constant current 0.05A-0.3A-0.6A (5-60min); S7 Charged Transition: Same as Example 1; S8 Pulse Electroplating: Same as Example 1 (including reduction pulse), with the dead zone adjusted to 8ms; S9 Post-processing: Same as Example 1.

[0083] The obtained TGV substrate was inspected: 100% conductivity, copper thickness at the bottom of the hole is ≥ 48% of the copper thickness at the opening of the hole.

[0084] Comparative Example 3 Using the substrate of Example 3, electroplating was performed directly without skipping S3-S6.

[0085] The obtained TGV substrate was inspected: Over 99% of circuits are broken.

[0086] The performance tests of the above embodiments and comparative examples are detailed in Tables 1 and 2 below. Figure 3 : Table 1

[0087] Table 2

[0088] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this disclosure, "multiple" means two or more, unless otherwise explicitly specified.

[0089] In this disclosure, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection, an electrical connection, or a communication connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this disclosure according to the specific circumstances.

[0090] In this disclosure, unless otherwise expressly specified and limited, "above" or "below" a second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of a second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" a second feature includes the first feature being directly above or diagonally above the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature. The foregoing disclosure provides many different embodiments or examples for implementing different structures of this disclosure. To simplify this disclosure, components and arrangements of specific examples are described above. Of course, these are merely examples and are not intended to limit this disclosure. Furthermore, reference numerals and / or reference letters may be repeated in different examples of this disclosure; such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed.

[0091] The above are merely specific embodiments of this disclosure, but the scope of protection of this disclosure is not limited thereto. Any person skilled in the art can easily conceive of various variations or substitutions within the technical scope disclosed in this disclosure, and these should all be included within the scope of protection of this disclosure. Therefore, the scope of protection of this disclosure should be determined by the scope of the claims.

Claims

1. A method for metallizing a TGV substrate, characterized in that, include: (1) Provide a glass substrate, the glass substrate having a through hole, a conductive bus ring being provided on the edge of the glass substrate, the through hole having a depth-to-width ratio greater than or equal to 6:1, and perform cleaning and gas replacement treatment on the glass substrate. (2) The glass substrate is subjected to acid pickling treatment. During the acid pickling treatment, a constant current bias voltage is applied to the conductive bus ring by a V-shaped conductive block fixed on a movable target frame to remove the oxide on the surface of the seed layer. The thinning amount of the seed layer is less than or equal to 1 nm. (3) Sensitize the glass substrate after step (2), the sensitization process including immersing the glass substrate in a Sn-containing solution. 2+ In the activation solution, a constant current bias voltage is applied to the glass substrate through the V-shaped conductive block, causing Sn to... 2+ They migrate and adsorb to the bottom of the through-hole; (4) The glass substrate treated in step (3) is immersed in a solution containing Pd. 2+ A continuous catalytic layer is formed in the activation solution, and a constant current bias voltage is applied to the glass substrate through the V-shaped conductive block during the formation of the continuous catalytic layer. (5) Immerse the glass substrate treated in step (4) into the electroless copper plating solution, and apply segmented constant current bias voltage through the V-shaped conductive block to perform electrochemical copper plating. (6) The glass substrate processed in step (5) is transferred to an electroplating tank to electroplat a Cu layer to achieve metallization. In steps (2) to (6), the glass substrate is always held by the target frame and the V-shaped conductive block, and the V-shaped conductive block is always positioned above the liquid surface of each wet process tank and does not contact any tank liquid; and After the glass substrate is transferred to the processing liquid for each step (2) to (6), and before each step is performed, the glass substrate is subjected to constant voltage pulse reduction treatment by the V-shaped conductive block.

2. The method according to claim 1, characterized in that, The pickling solution in step (2) comprises 3-5% by volume H2SO4 and a weak acid, wherein the weak acid is 1-5 g / L ascorbic acid or 5-10 g / L citric acid. The glass substrate includes a seed layer, the acid pickling process includes removing oxides from the surface of the seed layer, the thinning amount of the seed layer is less than or equal to 1 nm, the constant current bias applied in step (2) is 0.02-0.05 A, the processing time is 30-60 s, and the temperature of the tank room is 20-25 °C. Alternatively, if there is no seed layer on the surface of the glass substrate, the constant current applied in step (2) is 0.01-0.05A.

3. The method according to claim 1, characterized in that, The method satisfies at least one of the following conditions: The sensitization solution in step (3) includes 15-25 g / L SnCl2·2H2O and 10-15 mL / L HCl. The constant current bias voltage of the sensitization treatment is 0.015-0.025 A, and the treatment time is 60-120 s. The activation solution in step (4) includes 0.02-0.15 g / L of PdCl2 and 8-12 mL / L of HCl, the constant current bias voltage is 0.025-0.035 A, and the processing time is 60-120 s; The electroless copper plating solution in step (5) includes 8-12 g / L CuSO4·5H2O, 25-35 g / L EDTA-2Na, 6-10 mL / L HCHO, and 1-2 mg / L α-α' bipyridine. The pH of the electroless copper plating solution is 12.0-12.8, and the processing temperature is 30-32℃. The electroplating solution in step (6) includes 180-220 g / L CuSO4·5H2O, 50-70 g / L H2SO4, and 40-60 ppm Cl. - The additives include at least one of leveling agents, brighteners, and wetting agents, and the temperature of the electroplated Cu layer is 22-26°C. The electrochemical copper plating in step (5) is achieved by applying segmented constant current bias voltage, which includes: applying a current of 0.05A within 0-2min, applying a current of 0.3A within 2-5min, and applying a current of 0.6A within 5-45min; after performing the electrochemical copper plating for 2min, the electrochemical plating tank is subjected to N2 bubbling treatment, and the bubbling pressure is 0.015bar±0.002bar.

4. The method according to claim 1, characterized in that, After step (5) and before step (6), the process further includes a three-stage cleaning operation on the glass substrate. The three-stage cleaning process includes: Spraying treatment was carried out using 5% (v / v) H2SO4. Deionized water was used for spray treatment; and Soaking treatment was performed using deionized water. During the three-stage cleaning process, a constant current bias voltage of 0.02A is applied to the glass substrate.

5. The method according to claim 1, characterized in that, The electroplating of the Cu layer in step (6) is achieved through the following operations: A constant voltage cathode reduction pulse is applied to the glass substrate through the V-shaped conductive block to reduce the oxides on the electrochemically plated copper surface. The voltage of the constant voltage cathode reduction pulse is -0.3V to -0.5V, the duration is 0.3-1.0s, and the current limiting value is 0.1-0.3ASD. Subsequently, a bipolar phase-shifting pulse current is applied. The forward current of the bipolar phase-shifting pulse current is 1.0-2.0 ASD, the reverse current is 0.1-0.2 ASD, the forward-reverse duty cycle is 10:1 to 20:1, the forward pulse width is 200-300 ms, and the reverse pulse width is 10-20 ms. When the bipolar phase-shifting pulse current is applied, the glass substrate is held by the flying target frame and the V-shaped conductive block and oscillated horizontally along the X-axis.

6. A system for metallizing a TGV substrate based on the method described in any one of claims 1-5, characterized in that, include: A conductive moving component, comprising a movable target frame and a V-shaped conductive block fixed on the target frame, wherein the target frame is provided with elastic contacts at both ends; A perforated titanium plate anode assembly includes multiple wet processing tanks, which are used to perform pickling, sensitization, activation, chemical copper plating, and electroplating copper treatments, respectively. Each of the multiple wet processing tanks has a perforated titanium plate as a counter electrode, and each of the openings of the multiple wet processing tanks is provided with a fixed busbar for electrical connection through the elastic contacts when the target frame enters the tank. X-axis horizontal swing assembly, the X-axis horizontal swing assembly is connected to the target frame, and is used to drive the target frame to perform horizontal reciprocating swing along the direction parallel to the TGV hole axis. A power supply assembly, which is electrically connected to electrodes in the plurality of wet processing tanks, is used to independently control the electrical signals applied to the counter electrodes in each of the wet processing tanks. A control component, which is connected to both the X-axis horizontal swing component and the power supply component, is used to control the power mode of the power supply component and the swing parameters of the X-axis horizontal swing component.

7. The system according to claim 6, characterized in that, The V-shaped conductive block is made of industrial pure titanium, and the contact surface has a gold-plated layer with a thickness ≥0.5μm. The spring loading pressure of the V-shaped conductive block is ≥8N / block, and the contact resistance is <0.1Ω. The perforated titanium plate is made of industrial pure titanium perforated plate. The perforated titanium plate in the wet process tank corresponding to the chemical copper plating and electroplating copper plating has a Pt / Ti coating or a mixed metal oxide coating. The glass substrate to be processed, held by the V-shaped conductive block, is the working electrode. The single-sided spacing between the counter electrode and the working electrode in the multiple wet process tanks is 80mm±2mm. The ratio of the counter electrode area to the effective conductive area of ​​the working electrode, Aan / Ac≥5.

8. The system according to claim 6, characterized in that, The chemical copper plating and electroplating copper treatments are completed in the same wet process tank, which has a drain hole for replacing the treatment solution.

9. The system according to claim 6, characterized in that, Further includes: A gas bubbling assembly is used to bubble gas onto the glass substrate to be processed in the wet process tank. A water spray assembly and an acid spray assembly are used to spray the glass substrate to be processed in the wet process tank. An external circulation heat exchange component is connected to the plurality of wet processing tanks and is used to control the temperature inside the plurality of wet processing tanks.

10. A metallized TGV substrate, characterized in that, The TGV substrate is prepared using the method described in any one of claims 1-6 or the system described in any one of claims 7-9. The through-hole of the TGV substrate has a depth-to-width ratio of 6:1 to 12:1, an inner hole wall roughness Ra≤1.2μm, a metallization conductivity of 100%, and a metal layer thickness at the bottom of the hole that is not less than 48% of the metal layer thickness at the opening of the hole.