Infrared radiation sintering method and sintered body of resin-free nano-gold paste
By employing an infrared radiation sintering method using resin-free nano-gold paste and symmetrical dual-source tilted infrared radiation, the electrical insulation and thermal resistance problems caused by the resin matrix are solved, the thermal conductivity and interfacial bonding strength of the sintered body are improved, and the long-term stability of the device is ensured.
Patent Information
- Application Number
- CN202611255996.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-20
AI Technical Summary
In the prior art, the resin matrix in the sintered body between the chip and the substrate results in electrical and thermal insulation, which hinders the transmission of electrons and phonons. The metal particles isolate the thermal conductivity, resulting in weak interfacial bonding. Furthermore, the resin is prone to aging under high temperature and high humidity, leading to device failure.
An infrared radiation sintering method using resin-free nano-gold paste is employed. By using symmetrical dual light sources to irradiate infrared light at an angle, the infrared wavelength and radiation distance are controlled to form a controllable temperature gradient, which promotes solvent escape and improves the thermal conductivity and metallurgical bonding of the sintered body.
This achieves a sintered body with high thermal conductivity and strength, improving the long-term reliability and interfacial bonding strength of the device, and avoiding performance degradation caused by resin aging.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electronic packaging technology, specifically relating to an infrared radiation sintering method and sintered body for resin-free nano-gold paste. Background Technology
[0002] In fields such as wide bandgap power semiconductors and high power density optoelectronic devices, the interconnect layer between the chip and the substrate is the key factor determining the device's performance, power density, and reliability.
[0003] To meet process requirements, current technologies typically fill the space between the chip and the substrate with a metal sintering paste containing polymer resin before sintering. During sintering, the resin partially carbonizes to form a continuous or discontinuous insulating / weakly conductive network, while metal particles (gold, silver) are dispersed and embedded in the resin matrix, forming a resin-metal composite. This composite structure has fundamental defects that affect device performance: the resin matrix (even after carbonization) is an electrical and thermal insulator or a poor conductor, severely hindering the transmission of electrons and phonons; the metal particles are isolated by the resin, preventing the formation of efficient thermal conductivity pathways, resulting in an intrinsic thermal conductivity of the sintered body that is far lower than that of pure metals; the metal particles are often separated from the chip / substrate metallization layer by a very thin resin residue film, making it difficult to form an atomic-level metallurgical bond, resulting in weak interfacial bonding, which becomes the main source of thermal resistance and a weak point for mechanical failure; the aging, decomposition, and moisture absorption expansion of the resin under high temperature, high humidity, and electric field conditions continuously deteriorate the resin-metal and resin-substrate interfaces, causing thermal conductivity and mechanical properties to drift over time or even fail.
[0004] To address these issues, resin-free metal sintering technology has emerged. However, current resin-free technologies primarily focus on formulation, and the resulting sintered body's microstructure can still be considered a simple accumulation of metal particles. In pursuing ultimate performance, improving the interfacial bonding quality between the sintered body and the substrate, as well as its thermal conductivity, remains a challenge. Summary of the Invention
[0005] The purpose of this invention is to provide an infrared radiation sintering method and a sintered body using resin-free nano-gold paste. The sintering method provided by this invention can improve the thermal conductivity of the sintered body, the bonding strength with the substrate, and its long-term reliability.
[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides an infrared radiation sintering method for resin-free nano-gold paste, comprising the following steps: After applying resin-free nano-gold paste to the substrate surface, the chip is attached to obtain a sandwich structure component. The sandwich structure assembly is subjected to infrared radiation sintering to obtain a sintered body; the infrared radiation sintering includes symmetrical dual-source tilted radiation on the outer surfaces of the chip and substrate in the sandwich structure assembly, with the radiation direction forming an angle of 45~75° with the corresponding outer surface; the infrared light wavelength of the infrared radiation sintering is independently 2~5μm; the distance between the light source and the corresponding outer surface during the infrared radiation sintering is 15~30mm.
[0007] Preferably, the peak temperature of the resin-free nano-gold paste during infrared radiation sintering is 250~300℃.
[0008] Preferably, the infrared radiation sintering has a radiation power of 500~3000W and a radiation time of 30~600s.
[0009] Preferably, a pressure not exceeding 5 MPa is applied during the infrared radiation sintering.
[0010] Preferably, the atmosphere for infrared radiation sintering is an inert atmosphere or a reducing atmosphere.
[0011] Preferably, the resin-free nano-gold paste comprises nano-gold particles and a solvent; the mass content of the nano-gold particles is 70-95%.
[0012] Preferably, the average particle size of the gold nanoparticles is 10~1000 nm.
[0013] Preferably, the solvent includes a high-boiling-point solvent and an in-situ reactive sintering co-solvent; the high-boiling-point solvent has a boiling point of 180~350℃; the in-situ reactive sintering co-solvent is a solvent that can decompose upon heating to produce reducing gas, and the decomposition initiation temperature is 180~220℃.
[0014] Preferably, the mass ratio of the high-boiling-point solvent to the in-situ reactive sintering co-solvent is (3~7):(3~7).
[0015] The present invention also provides a sintered body obtained by the infrared radiation sintering method described in the above technical solution.
[0016] This invention provides an infrared radiation sintering method for resin-free nano-gold paste, comprising the following steps: applying resin-free nano-gold paste to the surface of a substrate and then attaching a chip to obtain a sandwich structure assembly; performing infrared radiation sintering on the sandwich structure assembly to obtain a sintered body; the infrared radiation sintering includes symmetrical dual-source tilted radiation on the outer surfaces of the chip and the substrate in the sandwich structure assembly, with the radiation direction forming an angle of 45° to 75° with the corresponding outer surface; the infrared light wavelength of the infrared radiation sintering is independently 2 to 5 μm; the distance between the light source and the corresponding outer surface during the infrared radiation sintering is 15 to 30 mm. This invention employs infrared radiation heating. By limiting the infrared wavelength, heat is primarily absorbed by the nano-gold paste, while the substrate and chip absorb less heat, reducing thermal mismatch stress. Infrared radiation heating provides a rapid heating rate, shortening the sintering cycle, inhibiting abnormal grain growth, and resulting in a fine, dense sintered structure, thus improving the thermal conductivity and reliability of the sintered body. By controlling the infrared wavelength, radiation angle, and radiation distance, a controllable temperature gradient can be formed along the paste thickness, promoting the orderly escape of solvent from the inside out, reducing closed pores, and thereby improving the thermal conductivity of the sintered body. Irradiating the substrate and chip with an infrared light source increases the temperature of the gold paste at the connection end, promoting metallurgical bonding between the sintered body and the substrate and chip, improving bonding strength and thermal conductivity. Results from the embodiments show that the sintered body obtained using the sintering method of this invention achieves a thermal conductivity of 218 W / (m·K), a shear strength of 46.7 MPa, and a strength retention rate of 92.3% after aging at 300℃ for 1000 h. Detailed Implementation
[0017] All raw materials used in this invention are not particularly limited in their source; they can be purchased from the market or prepared using conventional methods known to those skilled in the art.
[0018] There are no particular restrictions on the purity of any of the raw materials used in this invention, but industrially pure raw materials are preferred.
[0019] This invention provides an infrared radiation sintering method for resin-free nano-gold paste, comprising the following steps: After applying resin-free nano-gold paste to the substrate surface, the chip is attached to obtain a sandwich structure component. The sandwich structure assembly is subjected to infrared radiation sintering to obtain a sintered body; the infrared radiation sintering includes symmetrical dual-source tilted radiation on the outer surfaces of the chip and substrate in the sandwich structure assembly, with the radiation direction forming an angle of 45~75° with the corresponding outer surface; the infrared light wavelength of the infrared radiation sintering is independently 2~5μm; the distance between the light source and the corresponding outer surface during the infrared radiation sintering is 15~30mm.
[0020] This invention involves applying resin-free nano-gold paste to the surface of a substrate and then attaching a chip to it to obtain a sandwich structure component.
[0021] In one embodiment of the present invention, the substrate can be a substrate with a metallization layer on its surface, specifically a gold-plated DBC substrate; the chip can be a chip with a metallization layer on its back side, specifically a gold-backed SiC chip; the metallization layer can be one or more of gold, silver, palladium, and platinum. The resin-free nano-gold paste is applied to the metallization layer of the substrate, and the gold-backed side of the chip is adhered to the resin-free nano-gold paste.
[0022] The present invention does not have a particular limitation on the amount of the resin-free nano gold paste used; the substrate and the chip can be bonded according to the amount known to those skilled in the art.
[0023] In this invention, the resin-free nano-gold paste preferably comprises nano-gold particles and a solvent; the mass content of the nano-gold particles is preferably 70-95%, more preferably 80-90%. A mass content of nano-gold particles within the above range facilitates uniform dispersion and maintains a certain degree of adhesion, allowing the chip to adhere to the gold paste.
[0024] In this invention, the average particle size of the gold nanoparticles is preferably 10-1000 nm, more preferably 50-300 nm; as one embodiment of this invention, the average particle size of the gold nanoparticles can be 40 nm, 80 nm, 100 nm, 150 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, or 800 nm. An average particle size within the above range is beneficial for sintering densification and improving thermal conductivity.
[0025] In this invention, the solvent preferably includes a high-boiling-point solvent and an in-situ reactive sintering co-solvent; the boiling point of the high-boiling-point solvent is preferably 180~350℃; the in-situ reactive sintering co-solvent is a solvent that decomposes upon heating to produce reducing gases, and the decomposition initiation temperature is preferably 180~220℃. The high-boiling-point solvent can reduce the evaporation rate in the early stage of sintering and maintain the stability of the gold paste; the in-situ reactive sintering co-solvent can decompose during sintering to produce reducing gases, which react with oxides on the surface of the substrate and the gold nanoparticles, improving the interface cleanliness.
[0026] In this invention, the preferred mass ratio of the high-boiling-point solvent to the in-situ reactive sintering flux is (3~7):(3~7). As one embodiment of this invention, the mass ratio of the high-boiling-point solvent to the in-situ reactive sintering flux can be 3:7, 4:6, 5:5, 6:4, or 7:3. A mass ratio of the high-boiling-point solvent to the in-situ reactive sintering flux within the above range is beneficial for stable solvent evaporation in the early stages of sintering, and the instantaneous local heat and reducing gas concentration provided by the decomposition reaction in the middle stages of sintering can further improve the densification degree.
[0027] In one embodiment of the present invention, the high-boiling-point solvent can be an alcohol solvent, a glycol ether solvent, or an ester solvent, specifically diethylene glycol butyl ether; the in-situ reactive sintering co-solvent can be a nitrogen-containing organic solvent or a sulfoxide solvent, specifically N-methylformamide.
[0028] After obtaining the sandwich structure component, the present invention performs infrared radiation sintering on the sandwich structure component to obtain a sintered body.
[0029] In this invention, the infrared radiation sintering includes symmetrical dual-source tilted radiation on the outer surfaces of the chip and substrate in the sandwich structure assembly. The substrate and chip are primarily made of ceramic-based semiconductors, which absorb relatively little infrared light. Infrared waves can penetrate the substrate and chip to heat the gold paste, thus lowering their temperatures. Furthermore, irradiating the substrate and chip also increases the temperature of the gold paste at the connection points, promoting metallurgical bonding between the gold paste and the substrate and chip. Symmetrical dual-source tilted radiation increases the radiation surface area, ensuring uniform heating of the gold paste and preventing defects caused by uneven temperature distribution.
[0030] In this invention, the angle between the radiation direction of the infrared radiation sintering and the corresponding outer surface is 45° to 75°, preferably 55° to 65°. As one embodiment of this invention, the angle between the radiation direction of the infrared radiation sintering and the corresponding outer surface can be the same, specifically 45°, 50°, 55°, 60°, 65°, or 70°. The larger the angle between the radiation direction and the corresponding outer surface, the smaller the radiation area; at 90°, it is perpendicular irradiation, and the radiation area is equal to the spot diameter. The smaller the angle, the larger the radiation area, but this also increases reflectivity, reduces heating efficiency, and causes thermal field disturbance, making the heating effect uncontrollable. When the angle between the radiation direction and the corresponding outer surface is within the above range, the heating temperature is controllable, while also considering both radiation area and heating efficiency.
[0031] In this invention, the infrared light wavelength for infrared radiation sintering is independently 2~5μm, preferably 3~4μm. Infrared light wavelengths within this range are the main absorption bands of gold nanoparticles, which can directionally heat the gold paste, reducing the temperature of the substrate and chip, thereby reducing thermal mismatch. Furthermore, compared to shorter wavelength infrared light, the penetration ability of infrared light in the above-mentioned band is reduced, which can create a temperature gradient along the thickness direction of the gold paste, promoting the orderly escape of solvents and gases.
[0032] In this invention, the distance between the light source and the corresponding outer surface during infrared radiation sintering is 15-30 mm, preferably 20-25 mm. The distance between the light source and the corresponding outer surface affects the power density; the smaller the distance, the higher the power density, the faster the heating rate of the gold paste, and the greater the temperature gradient. Within the above range, a temperature gradient of 25-40°C can be formed, promoting the orderly escape of the solvent and avoiding excessive temperature gradient that could cause surface overheating, abnormal grain growth, and reduced thermal conductivity and bonding strength.
[0033] In this invention, the peak temperature of the resin-free nano-gold paste during infrared radiation sintering is preferably 250~300℃, more preferably 260~280℃; as one embodiment of this invention, the peak temperature of the resin-free nano-gold paste during infrared radiation sintering can be 250℃, 260℃, 270℃, 280℃, or 290℃. A peak temperature within the above range during infrared radiation sintering of the resin-free nano-gold paste is beneficial for gold atom diffusion and the fusion of nano-gold particles.
[0034] In this invention, the radiation power of the infrared radiation sintering is preferably 500~3000W, more preferably 1000~2000W; as one embodiment of this invention, the radiation power of the infrared radiation sintering can be 600W, 800W, 1000W, 1500W, 2000W, or 2500W. The radiation power of the infrared radiation sintering determines the rate of heat output, affecting the peak temperature and temperature gradient of the resin-free nano-gold paste; when the radiation power of the infrared radiation sintering is within the above range, the resin-free nano-gold paste can reach a suitable temperature, promoting densification and forming a temperature gradient between the surface and the interior, promoting the escape of solvent and gas.
[0035] In this invention, the infrared radiation sintering time is preferably 30-600 s, more preferably 100-300 s; as one embodiment of this invention, the infrared radiation sintering time can be 50 s, 100 s, 200 s, 300 s, 400 s, 500 s, or 600 s. The radiation time affects the sintering progress; radiation times within the above range are beneficial for sintering densification, further improving the thermal conductivity and bonding strength of the sintered body.
[0036] In this invention, during infrared radiation sintering, pressure is preferably applied, preferably not exceeding 5 MPa, and more preferably 0.2~3 MPa. As one embodiment of this invention, the pressure can be 0.3 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 1.5 MPa, 2 MPa, 3 MPa, or 4 MPa. Applying pressure during sintering facilitates the removal of solvent and bubbles, improving density; pressure within the above range can improve density and reduce the risk of damage to the chip.
[0037] In this invention, the atmosphere for infrared radiation sintering is preferably an inert atmosphere or a reducing atmosphere. An inert atmosphere can isolate air and reduce oxidation; a reducing atmosphere can react with the oxide layer on the surface of the gold nanoparticles and the metallization layer, promoting metallurgical bonding between the gold nanoparticles and with the metallization layer.
[0038] In one embodiment of the present invention, the inert atmosphere may be nitrogen; the reducing atmosphere may be a mixture of hydrogen and argon, wherein the volume fraction of hydrogen in the mixture may be 3 to 10%.
[0039] This invention employs infrared radiation heating. By limiting the infrared wavelength, heat is primarily absorbed by the nano-gold paste, while the substrate and chip absorb less heat, reducing thermal mismatch stress. Infrared radiation heating provides a rapid heating rate, shortening the sintering cycle, inhibiting abnormal grain growth, and resulting in a fine, dense sintered structure, thus improving the thermal conductivity and reliability of the sintered body. By controlling the infrared wavelength, radiation angle, and radiation distance, a controllable temperature gradient can be formed along the paste thickness, promoting the orderly escape of solvent from the inside out, reducing closed pores, and thereby improving the thermal conductivity of the sintered body. Irradiating the substrate and chip with an infrared light source can increase the temperature of the gold paste at the connection end, promoting metallurgical bonding between the sintered body and the substrate and chip, and improving bonding strength and thermal conductivity.
[0040] The present invention also provides a sintered body obtained by the infrared radiation sintering method described in the above technical solution.
[0041] The sintered body provided by this invention has a pure metal structure, excellent thermal conductivity, strong bonding with the substrate and chip, good long-term stability, and is suitable for high-performance electronic devices.
[0042] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0043] Example 1 An infrared radiation sintering method for resin-free nano-gold paste, comprising the following steps: After applying resin-free nano-gold paste to the gold-plated surface of the gold-plated DBC substrate, the back-gold SiC chip is attached, with the back-gold surface in contact with the resin-free nano-gold paste. The resin-free nano-gold paste is composed of nano-gold particles with an average particle size of 300nm and a solvent in a mass ratio of 90:10. The solvent is diethylene glycol butyl ether and N-methylformamide in a mass ratio of 1:1. The infrared radiation sintering process involves symmetrical dual-source tilted radiation irradiating the upper surface of the chip and the lower surface of the substrate, with the radiation direction forming an angle of 60° with the substrate or chip. The infrared wavelength of the infrared radiation sintering is 2.5 μm. The distance between the light source and the substrate or chip during the infrared radiation sintering process is 20 mm. The radiation power of the infrared radiation sintering is 600 W, the radiation time is 300 s, the heating rate is 40 °C / s, and the peak temperature is 280 °C. The atmosphere for the infrared radiation sintering process is a nitrogen atmosphere.
[0044] Example 2 An infrared radiation sintering method for resin-free nano-gold paste is the same as in Example 1, except that a pressure of 2 MPa is applied during infrared radiation sintering.
[0045] Comparative Example 1 A sintering method for resin-free nano-gold paste, using the same raw materials as in Example 1, but differing in that a traditional hot plate conduction heating method is used for sintering, with a heating rate of 10℃ / min, a peak temperature of 280℃, and a holding time of 30min.
[0046] Comparative Example 2 An infrared radiation sintering method for resin-free nano-gold paste is the same as in Example 1, except that the infrared wavelength is 1 μm during infrared radiation sintering.
[0047] Comparative Example 3 An infrared radiation sintering method for resin-free nano-gold paste is the same as in Example 1, except that the radiation direction of the infrared radiation sintering is perpendicular irradiation.
[0048] Comparative Example 4 An infrared radiation sintering method for resin-free nano-gold paste is the same as in Example 1, except that the distance between the light source and the substrate and chip is 50 mm during infrared radiation sintering.
[0049] Test Example 1 The shear strength τ, thermal conductivity κ, and strength retention rate η after aging of the sintered bodies obtained in Examples 1-2 and Comparative Examples 1-4 were tested, and the test results are recorded in Table 1.
[0050] Shear strength test: Fix the sintered component on the stage, so that the blade is close to the side root of the chip and the height is parallel to the substrate; set the shearing height, test speed and safe load; the blade moves forward at a constant speed in the horizontal direction, parallel to the substrate and "scoops" towards the chip; record the pushing force when the chip is pushed away.
[0051] Strength retention rate test after aging: The sintered body was placed in an oven at 300℃ for 1000h, and then the shear strength was tested. The shear strength was compared with the initial shear strength to obtain the strength retention rate after aging.
[0052] The thermal conductivity test method is as follows: Sintered silver paste is printed onto a flat polytetrafluoroethylene (PTFE) substrate, sintered according to the actual process, and the sintered silver sheet is polished into a circular disc with a diameter of 12.7 mm and a thickness of 1-3 mm, with a parallelism of <0.01 mm on both sides. A thin graphite layer is sprayed onto the back side to obtain the test sample. The test sample is placed in a sample holder, ensuring that the laser, the test sample, and the infrared detector are coaxial. Under an inert gas environment, a laser pulse irradiates the back side of the test sample, and the infrared detector records the temperature rise curve of the front side. The software calculates the thermal diffusivity based on the temperature rise half-life, and combines it with the specific heat capacity and density to obtain the thermal conductivity. Thermal conductivity = thermal diffusivity * specific heat capacity * density.
[0053] Table 1. Test Records of Sintered Body Properties Obtained by Different Methods
[0054] As can be seen from Table 1, the sintered body obtained in Example 1 has good thermal conductivity and shear strength; Example 2 uses low-pressure assisted sintering, which further improves the thermal conductivity, shear strength and stability of the sintered body.
[0055] Comparative Example 1 uses the traditional sintering method, resulting in a sintered body with poor performance.
[0056] Comparative Example 2 uses short-wave infrared light, which has a large penetration depth and the energy is evenly distributed in the gold paste. The temperature gradient in the thickness direction is close to zero, and the thermal field characteristics are similar to those of traditional heating methods, resulting in poor performance of the sintered body.
[0057] In Comparative Example 3, the vertical incidence caused uneven lateral temperature distribution of the gold paste, insufficient sintering on the side away from the light source, and inconsistent overall performance.
[0058] In Comparative Example 4, the large distance between the light source and the power density decreased significantly, the temperature gradient in the thickness direction weakened, and the solvent evaporation kinetics decreased, resulting in a decline in the performance of the sintered body.
[0059] As can be seen from the above embodiments and comparative examples, the infrared radiation sintering method for resin-free nano-gold paste provided by the present invention can improve the thermal conductivity, shear strength and long-term reliability of the sintered body.
[0060] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. An infrared radiation sintering method for resin-free nano-gold paste, characterized in that, Includes the following steps: After applying resin-free nano-gold paste to the substrate surface, the chip is attached to obtain a sandwich structure component. The sandwich structure assembly is subjected to infrared radiation sintering to obtain a sintered body; the infrared radiation sintering includes symmetrical dual-source tilted radiation on the outer surfaces of the chip and substrate in the sandwich structure assembly, with the radiation direction forming an angle of 45~75° with the corresponding outer surface; the infrared light wavelength of the infrared radiation sintering is independently 2~5μm; the distance between the light source and the corresponding outer surface during the infrared radiation sintering is 15~30mm.
2. The infrared radiation sintering method according to claim 1, characterized in that, The peak temperature of the resin-free nano-gold paste during infrared radiation sintering is 250~300℃.
3. The infrared radiation sintering method according to claim 2, characterized in that, The infrared radiation sintering has a radiation power of 500~3000W and a radiation time of 30~600s.
4. The infrared radiation sintering method according to claim 1, characterized in that, The infrared radiation sintering process applies a pressure not exceeding 5 MPa.
5. The infrared radiation sintering method according to claim 1, characterized in that, The atmosphere for infrared radiation sintering is an inert atmosphere or a reducing atmosphere.
6. The infrared radiation sintering method according to claim 1, characterized in that, The resin-free nano-gold paste comprises nano-gold particles and a solvent; the mass content of the nano-gold particles is 70-95%.
7. The infrared radiation sintering method according to claim 6, characterized in that, The average particle size of the gold nanoparticles is 10~1000 nm.
8. The infrared radiation sintering method according to claim 6, characterized in that, The solvent includes a high-boiling-point solvent and an in-situ reactive sintering co-solvent; the boiling point of the high-boiling-point solvent is 180~350℃; the in-situ reactive sintering co-solvent is a solvent that can decompose upon heating to produce reducing gas, and the decomposition initiation temperature is 180~220℃.
9. The infrared radiation sintering method according to claim 8, characterized in that, The mass ratio of the high-boiling-point solvent to the in-situ reactive sintering flux is (3~7):(3~7).
10. The sintered body obtained by the infrared radiation sintering method according to any one of claims 1 to 9.