Coated granule particles and use thereof for manufacturing tablets by selective laser sintering
By using granules and precursor material particles for coating, combined with selective laser sintering and fluidized bed or jet bed devices, the problem of poor mechanical properties in SLS-printed drug formulations has been solved, enabling the manufacture of high drug loading and multi-layer tablets to meet different drug release requirements.
Patent Information
- Application Number
- CN202580021829.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-18
- Filing Date
- 2025-03-11
- Publication Date
- 2026-11-20
AI Technical Summary
In the prior art, when selective laser sintering (SLS) prints drug formulations, the commonly used pharmaceutical excipients result in poor mechanical properties of the printed tablets, making it difficult to manufacture tablets with high drug loading and multilayers.
Tablets are manufactured using precursor material particles containing pharmaceutical substances and a coating layer formed of thermoplastic material, through selective laser sintering, including coating and additive manufacturing steps, optimizing the size and flowability of the particles, and using fluidized bed or jet bed apparatus for coating.
It enables the manufacture of tablets with high drug loading, with a drug loading of more than 40%, preferably more than 60%, and especially preferably more than 80%, and supports multi-layer tablets and different drug release profiles, thereby improving the mechanical properties and stability of the tablets.
Smart Images

Figure CN123146362A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a precursor material for manufacturing tablets.
[0002] Furthermore, the present invention relates to the use of a precursor material having a plurality of precursor material particles in the manufacture of tablets. Background Technology
[0003] Various technologies and processes are employed to manufacture tablets. In the last decade, additive manufacturing processes have become particularly important for improving the production of tablets with formulations for the release of drug substances.
[0004] In their article titled "Selective Laser Sintering (SLS) 3D Printing of Drugs," published in the *International Journal of Pharmaceutics* (Vol. 529, Issues 1-2, August 30, 2017, pp. 285-293, https: / / doi.org / 10.1016 / j.ijpharm.2018.05.044), Fina et al. noted that there are currently no reports on using SLS to manufacture tablets filled with oral drug formulations; therefore, this study aimed to explore the applicability of SLS printing for drug formulation manufacturing. To this end, two pharmaceutical-grade thermoplastic polymers, Kollicoat IR and Eudragit L100-55, with immediate-release and sustained-release properties respectively, were selected to investigate the versatility of the SLS printer. Each polymer was tested with three different concentrations of acetaminophen. To promote the sintering process, 3% Candurin was added to each powder formulation. ® Goldglanz successfully printed six solid dosage forms; the 3D-printed tablets were robust and durable, with no signs of drug degradation observed.
[0005] In their paper "Development of Composite-Reinforced High-Drug-Loaded Pharmaceutical Printed Tablets by Selective Laser Sintering—Search for Relevant Excipients for Drug 3D Printing" (Materials 2022, 15(6), 2142, https: / / doi.org / 10.3390 / ma15062142), Kulinowski et al. pointed out that while 3D printing high-dose tablets containing pure, fragile, crystalline pharmaceutical active ingredients via selective laser sintering (SLS) is feasible, it is not practical. Currently used pharmaceutical excipients, including polymers, are mainly designed for powder tableting to ensure good mechanical properties. Using these excipients in SLS usually results in poor mechanical properties of the printed tablets. To overcome this problem, a composite printed part consisting of sintered carbon-colored polyamide and metronidazole was manufactured by SLS. The tablets were characterized using dynamic differential calorimetry and infrared spectroscopy, and their mechanical properties were evaluated. This study demonstrates the requirements for excipients used in 3D printing and the necessity of finding suitable materials for this purpose. Summary of the Invention
[0006] Therefore, the object of the present invention is to provide improved precursor materials and their use in the manufacture of tablets.
[0007] This objective is achieved in the type of precursor material for manufacturing tablets mentioned at the beginning by the following manner: the precursor material has a plurality of precursor material particles, wherein each precursor material particle has a granule and a coating layer covering the granule, the granule having a granule diameter, the coating layer having a layer thickness, wherein the granule contains a pharmaceutical substance, and the coating layer is formed by a coating agent containing a thermoplastic material.
[0008] Thermoplastic materials are materials that can undergo thermoplastic deformation within a specific temperature range. This process is reversible, meaning that as long as the material does not thermally decompose due to overheating, the process can be repeated by cooling and reheating to a molten state. Suitably, thermoplastic polymers and / or lipids are referred to herein as thermoplastic materials.
[0009] Granular particles refer to the small, granular or spherical solids that make up the aggregate as a whole.
[0010] Pharmaceutical substances (also known as active substances or pharmaceutical ingredients) are substances used as pharmaceutically active ingredients in the production of pharmaceuticals. Pharmaceutical substances are usually processed into pharmaceuticals together with one or more pharmaceutical excipients, but sometimes excipients may not be used.
[0011] The method for manufacturing tablets includes a coating step and an additive manufacturing step following the coating step, wherein in the coating step, granules containing a drug substance are coated with a coating agent comprising a thermoplastic material to produce precursor material granules, and in the additive manufacturing step, a powdered precursor material containing a large number of precursor material granules is selectively laser sintered to form a tablet.
[0012] This method is preferably performed on equipment for manufacturing tablets, wherein the equipment includes a precursor material manufacturing apparatus and an additive manufacturing apparatus, wherein the precursor material manufacturing apparatus is configured to coat granules containing a pharmaceutical substance with a coating agent comprising a thermoplastic material to produce precursor material particles, and wherein the additive manufacturing apparatus is configured to manufacture tablets from a powdered precursor material having a plurality of precursor material particles by selective laser sintering. Advantageously, the precursor material manufacturing apparatus and the additive manufacturing apparatus are fluidly connected so that precursor material can be transported from the precursor material manufacturing apparatus to the additive manufacturing apparatus.
[0013] For non-spherical granules, the equivalent diameter of the corresponding granules is also considered as the particle size. The equivalent diameter is a measure of the size of irregularly shaped granules. It is calculated by comparing the properties of irregularly shaped granules with those of regularly shaped granules. Advantageously, powdered precursor materials possess both low bulk density and large surface area, allowing for the absorption of more laser energy and the bonding of precursor material particles to form tablets during selective laser sintering. It is also advantageous to produce precursor material particles with improved flowability and distribution (spreadability) from granules through a coating step using thermoplastic materials. Both of these improved properties are important for obtaining thin powder beds for additive manufacturing steps.
[0014] Within the additive manufacturing apparatus, in the additive manufacturing step, in the first step, powdered precursor material is distributed as a powder bed in a thin layer on a platform within the build cavity of the additive manufacturing apparatus. The powder bed, containing a large number of precursor material particles, is then preheated to a temperature slightly below the melting point of the thermoplastic material. This makes it easier for a laser to raise the temperature of certain areas of the powder bed, which the laser solidifies by tracing the shape of the tablet. The laser scans the cross-section of the 3D tablet model and heats the powdered precursor material to a temperature slightly below or just above its melting point, thereby mechanically fusing the precursor material particles together and producing a solid tablet. The fusing of the precursor material particles is particularly advantageous through a coating layer containing thermoplastic material applied to the granular particles, because the precursor material particles are uniformly distributed on the powder bed due to their good distribution and, consequently, due to the uniform coating layer applied to them. Since the unsintered powdered precursor material supports the tablet during printing, no additional support structure is required for tablet production. The platform then descends one layer into the build-up cavity, typically between 50µm and 200µm. The entire process is then repeated for each layer until tablet fabrication is complete.
[0015] The build-up cavity is then preferably cooled in a second step, first inside the additive manufacturing apparatus and then outside the additive manufacturing apparatus, which is designed as a printer, to ensure optimal mechanical properties and prevent tablet deformation.
[0016] In the third step of the additive manufacturing process, the finished tablet is removed from the build-up cavity, and excess powdered precursor material is separated and removed. The excess powdered precursor material can be reused, and the tablet can be post-processed.
[0017] This method can produce tablets with very high drug loading of more than 40%, preferably more than 60%, and particularly preferably more than 80%.
[0018] According to the first process embodiment, the process further includes a granulation step in which granules are produced, comprising a plurality of granular particles, wherein the granulation step occurs prior to the coating step. Suitably, the granulation step is performed as a direct granulation process, a vertical granulation process, or a spray drying process. The granulation device associated with the precursor material manufacturing apparatus is suitably designed as an extruder (particularly a twin-screw extruder), a vertical granulator, or a spray drying device. Preferably, in the first process embodiment, the granulation device is located upstream of the coating apparatus.
[0019] In vertical granulation (also known as high-shear granulation or wet granulation), various powdered initial raw materials are granulated into large, uniformly distributed, and very dense particles through the high mechanical shearing action of a rotating mixing tool and the addition of a liquid granulating agent. In high-shear granulation, the larger particles are preferably further crushed by laterally arranged shredders. The granulating agent is typically a dissolved binder or a water-organic solvent mixture. Commonly used binders include water, polyvinylpyrrolidone, cellulose esters, or gelatin.
[0020] In spray drying, powdered initial raw materials are dissolved, emulsified, or dispersed in a solution of solvent or carrier material. The solution, emulsion, suspension, or dispersion is then atomized and sprayed into a drying chamber through which a hot drying gas stream flows, promoting solvent evaporation. Spray drying produces granules that exhibit significant size variation and poor flowability.
[0021] According to another advantageous design related to the first process scheme, a screening step is performed between the granulation step and the coating step, wherein, for the coating step, granules with a unimodal particle size distribution are produced. To perform the screening step, the precursor material manufacturing apparatus has a screening device in which granules with a unimodal particle size distribution can be produced. Therefore, the screening device of the precursor material manufacturing apparatus is suitably located downstream of the granulation device. Due to the unimodal particle size distribution after the screening step, uniform coating of the granules can be achieved in the coating step.
[0022] In order to coat granules containing a large number of granules, the precursor material manufacturing apparatus has a coating device, wherein the coating device is suitably designed as a fluidized bed device, a spray bed device or a roller coating device.
[0023] In the first process design, the coating step is preferably performed as a roller coating process, in which granular particles are coated with a coating agent in a rotating roller. Roller coating is particularly suitable for coating larger, non-rotating granular particles. In the roller coating process (also known as roller coating or roller coating), the granular particles move gently and controllably within the roller and are coated with a layer containing a thermoplastic material. It is important to distribute the coating agent as uniformly as possible across the granular particles. This is ensured both by appropriate spraying facilities and by uniformly mixing the granules containing a large number of particles within the roller.
[0024] In a second process alternative to the first, the process includes a granulation step, in which granules consisting of a large number of granular particles are produced, wherein the granulation step is performed simultaneously with the coating step. Specifically, the granulation step, performed concurrently with the coating step, is executed as a spray agglomeration process or a spray granulation process. Here, the granulation apparatus associated with the precursor material manufacturing device is suitably designed as a fluidized bed apparatus or a spray bed device. The advantage of employing the second process alternative is that the coating of the precursor material particles and its granulation / agglomeration are carried out simultaneously.
[0025] In spray agglomeration, extremely small powdery initial particles move in a fluidized bed and are sprayed with a binder liquid, thereby forming liquid bridges between the initial particles and producing so-called agglomerated particles. In this case, the binder liquid is also suitably a coating agent. Due to the low kinetic energy during spray agglomeration in a fluidized bed, a porous structure with numerous internal capillaries (cavities) is generated after the residual moisture evaporates. This new structure is further enhanced by the hardened binder liquid. The dust-free, free-flowing agglomerated particles are easy to meter and can be optimally processed. During agglomeration, finely dispersed initial particles are transformed into granular particles in the form of cohesive units by introducing the binder liquid. Therefore, these agglomerated particles are referred to below as granular particles. Correspondingly, agglomerates containing a large number of agglomerated particles generated in spray agglomeration are also called granules. By using a coating agent as a binder liquid, the agglomerated particles in the fluidized bed or spray bed are coated simultaneously.
[0026] In the spray granulation process, parameters such as particle size, residual moisture, and solids content can be selectively influenced, and various product characteristics of the granules can be adjusted. Granules produced by spray granulation have a dense surface structure and high bulk density; due to their small surface area, these granules have very low hygroscopicity and absorb almost no ambient moisture. Furthermore, these granules also possess high flowability, abrasion resistance, drip resistance, easy solubility, and optimal metering. Therefore, these granules are simultaneously coated in fluidized beds or spray beds. Compared to agglomeration methods, spray granules are denser and harder.
[0027] Advantageously, in spray agglomeration or spray granulation processes, the precursor material is manufactured in a fluidized bed or spray bed apparatus, wherein the granules are pre-added and coated with a coating agent. Alternatively, in spray agglomeration or spray granulation processes, the precursor material is manufactured in a fluidized bed or spray bed apparatus, wherein the granules, together with the coating agent, are fed into the fluidized bed or spray bed apparatus as a solution, emulsion, suspension, or melt.
[0028] Coating is a method of selectively influencing the surface structure of granular particles by applying a functional coating. Coating is an effective method for applying coatings in fluidized bed and spray bed systems. It is important to apply the coating agent very uniformly during coating. Coating in fluidized bed and spray bed systems can be carried out using either batch or continuous processes.
[0029] By performing a granulation step before or simultaneously with the coating step, a proper balance can be achieved in the coating step to adjust the particle size, morphology, and size distribution of the precursor material. This balance is always required for selective laser sintering in additive manufacturing steps.
[0030] For precursor material particles, the principle generally applies that larger, rounder, and more unimodal the particle size distribution, the better the flowability. Key factors determining flowability include particle size distribution, particle shape, chemical composition, moisture content, and temperature. The methods listed in the European Pharmacopoeia, namely the angle of repose (also known as the angle of packing or friction angle) and the Hausner factor, are measures of flowability. The angle of repose of granules refers to the maximum angle of inclination relative to the horizontal plane at which the granules can be poured without settling. The Hausner factor, a dimensionless number, is calculated as the ratio of tapped density to bulk density, or the ratio of bulk volume to tapped volume. Powder flowability is considered "excellent" when the Hausner factor is between 1.00 and 1.11. As the Hausner factor increases, flowability deteriorates, with values above 1.60 considered "unacceptable." Therefore, precursor materials with a small angle of repose and a Hausner factor close to 1 are considered preferred. Good flowability also benefits the dispersibility of the precursor material.
[0031] Therefore, for selective laser sintering (SLS), precursor material particles should possess not only good flowability and dispersibility, but also low bulk density and large surface area to absorb more laser energy and fuse together to form a solid tablet during the printing process. Thus, small, spherical precursor material particles with a preferred unimodal particle size distribution are preferred. Accordingly, the precursor material particles preferably have a sphericity greater than or equal to 0.75, suitably greater than or equal to 0.9, and particularly greater than or equal to 0.93. Furthermore, the precursor material particles particularly preferably have a precursor material particle diameter of 20 µm to 200 µm, suitably 50 µm to 150 µm. The coating layer thickness is suitably in the range of 0.1 µm to 50 µm, particularly in the range of 5 µm to 20 µm. Suitably, the ratio of precursor material particle diameter to layer thickness is 2:1 to 15:1, particularly 2:1 to 10:1.
[0032] According to an additional advantageous design of the method, the fluidized bed or spray bed device has a process chamber and a nozzle device. The process chamber has a circular cross-section, and the nozzle device sprays a coating agent into the process chamber along a main spray direction. The main spray direction is designed to be parallel to the tangent of the circular cross-section of the process chamber and is arranged within an arc segment of the circular cross-section, the height of which is 30% of the cross-sectional radius. The coating agent or a suspension containing the coating agent is sprayed or can be sprayed into the fluidized bed or spray bed device through this nozzle device. For this purpose, one directional component of the main spray direction need only be parallel to the tangent. The aforementioned nozzle device is also called a so-called tangential spray nozzle device, which produces a "tangential spray." By tangentially spraying a coating agent containing thermoplastic material, a very uniform coating of the coating agent onto the granular particles is achieved, thereby producing a coating layer with a substantially constant thickness on the granular particles. In addition to tangential spraying, the coating agent can also be sprayed into the process chamber from below (i.e., "bottom spray")—with its main spraying direction in the direction of the flow of process gas in the fluidized bed or jet bed device—and from above (i.e., "top spray")—with its main spraying direction opposite to the flow direction of process gas in the fluidized bed or jet bed device.
[0033] Coatings containing thermoplastic materials may contain other substances besides thermoplastic materials, such as solvents, but may also consist of only at least one thermoplastic material.
[0034] Advantageously, the coating agent used contains a solvent in addition to the thermoplastic material. A solvent is a substance capable of dissolving and diluting gases, liquids, or solids to create a solution. This makes the coating agent easier to atomize, thus easier to coat onto the granular particles. Preferably, water and / or organic solvents are used as solvents. Alcohols and / or ketones and / or alkanes and / or ethers are suitable as organic solvents. Water has the advantage of being less expensive and less environmentally harmful than organic solvents. Since the precursor material particles are surrounded by heated process gases during the coating step, the solvent evaporates or volatilizes during the coating step.
[0035] In another advantageous design of this method, thermoplastic polymers, particularly polyvinylpyrrolidone (PVP), polyvinylpyrrolidone-vinyl acetate copolymer (PVPVA), ethyl cellulose (EC), hydroxypropyl cellulose (HPC), hydroxypropyl methylcellulose (HPMC), or methyl methacrylates (Eudragite), are used as the thermoplastic material. As the name suggests, thermoplastic materials possess thermoplastic properties, meaning they soften upon heating and solidify upon cooling without undergoing chemical changes. Biocompatible materials, especially biocompatible polymers or lipids, are particularly suitable for this method.
[0036] A precursor material comprising a large number of precursor material particles is suitable for manufacturing tablets, wherein, in an additive manufacturing step, the precursor material particles are selectively laser-sintered into tablets. In this process, a high-power laser sintersulates the material (particularly a thermoplastic coating material) into a solid structure based on a three-dimensional model of the tablet.
[0037] In the additive manufacturing step of selectively laser sintering powdered precursor materials into tablets, a powder bed melting system designed as a selective laser sintering printer is used in the additive manufacturing apparatus. This powder bed melting system preferably has at least one laser unit, which is either a CO2 laser or a fiber laser, thus suitably suited for selective laser sintering. The powder bed melting system designed as a selective laser sintering printer has at least one laser unit, each of which has a scanning system formed by at least one mirror controlled by at least one drive unit. Each laser beam from the laser unit heats the precursor material particles to or above their melting point, thereby bonding these precursor material particles together. By using multiple laser units, tablet production can be scaled up, meaning the number of tablets manufactured in the additive manufacturing step can be adjusted. In the additive manufacturing method, selected regions of the precursor material particles constituting the powder bed are fused or welded together by the thermal energy introduced by the laser. Suitable for selective laser sintering, when using a CO2 laser, the optimal wavelength is 10600 nm at a power of 14 W; when using a fiber laser, the optimal wavelength is 1064 nm at a power of 10 W. CO2 lasers are gas lasers based on electrically excited carbon dioxide gas mixtures and exhibit excellent beam quality. In comparison, fiber lasers are approximately 30% more efficient. Fiber lasers also offer higher energy efficiency, longer lifespan, and a more compact design.
[0038] In addition, the additive manufacturing apparatus is suitably designed to manufacture tablets from precursor materials by selective laser sintering in a protective gas atmosphere, wherein nitrogen or argon may be suitably used as the protective gas.
[0039] The tablets produced according to this method for manufacturing tablets thus contain a large number of precursor material particles bonded together by selective laser sintering, wherein the precursor material particles have granular particles and a coating layer covering the granular particles, the granular particles having a granular particle diameter, the coating layer having a layer thickness, wherein the granular particles contain a drug substance, the coating layer being formed by a coating agent containing a thermoplastic material, wherein the coating layer forming a coating layer matrix, and the granular particles being embedded in the coating layer matrix. Tablets with a very high drug loading can thus be obtained, with a drug loading greater than 40%, preferably greater than 60%, and particularly preferably greater than 80%.
[0040] Specifically, the tablets contain different prodrug material particles, each containing particles of a different drug substance. This allows the different drug substances to have different release profiles.
[0041] The tablet comprises multiple layers of precursor material, each consisting of precursor material particles. Advantageously, one of the multiple precursor material layers has precursor material particles that are different from those of the adjacent precursor material layers. Through these multiple precursor material layers, the tablet is formed as a multilayer tablet. Multilayer tablets combine different therapeutic doses in a single dosage form. Furthermore, advantageously, the drug substance contained in each precursor material layer can have different release profiles.
[0042] In addition, the precursor material layers are suitably designed with different packing densities. This results in a higher density of the precursor material layers and a more compact and stable tablet.
[0043] The corresponding tablets are further characterized in that they contain excipient particles, wherein the excipient particles include disintegrating particles and a coating layer covering the disintegrating particles. The disintegrating particles have a disintegrating particle diameter, and the coating layer has a layer thickness. The disintegrating particles contain a disintegrant, and the coating layer is formed by a coating agent containing a thermoplastic material. This allows for the targeted setting of drug release profiles.
[0044] According to another advantageous design of the tablet, the tablet has at least one capillary channel designed to introduce liquids (e.g., gastric juices, in particular) into the tablet interior via capillary action. The release profile can also be adjusted and set via the capillary channel.
[0045] Tablets manufactured according to this method can be coated with a suitable, enteric-coated coating layer during post-processing steps. Attached Figure Description
[0046] The invention will now be described in more detail with reference to the accompanying drawings, in which: Figure 1 A first embodiment of an apparatus for manufacturing tablets is shown; Figure 2 A second embodiment of an apparatus for manufacturing tablets is shown; Figure 3 A third embodiment of an apparatus for manufacturing tablets is shown; Figure 4 A fourth embodiment of an apparatus for manufacturing tablets is shown; Figure 5 A fifth embodiment of an apparatus for manufacturing tablets is shown; Figure 6A sixth embodiment of an apparatus for manufacturing tablets is shown; Figure 7 A schematic structure of a fluidized bed apparatus for manufacturing tablets is shown, wherein the cross-section AA passes through the conical portion of the process chamber; Figure 8 It corresponds to Figure 7 Cross-sectional view of the central section AA passing through the conical part of the process chamber; Figure 9 A schematic structure of an additive manufacturing apparatus in the form of a powder bed melting system is shown, which is designed as a selective laser printer; Figure 10 This illustrates a schematic process for coating granules of a certain diameter using a coating layer with a layer thickness. Figure 11 A multilayer tablet with two precursor material layers and a vertical section AA is shown; Figure 12 It passes through the cutting plane AA Figure 11 The diagram shows a vertical cross-section of a multilayer tablet, in which a coating layer forms a coating matrix and granules are embedded in the coating matrix. Figure 13 Is Figure 11 This diagram illustrates the meandering capillary channels in the lower precursor material layer of a multilayer tablet. Detailed Implementation
[0047] Unless otherwise stated, the following description refers to all embodiments of the apparatus 1 for manufacturing tablets 2 according to the present invention shown in the figures.
[0048] A method for manufacturing tablets 2 is suitably performed on apparatus 1. For this purpose, apparatus 1 has a precursor material manufacturing device 3 for performing at least one coating step and an additive manufacturing device 4 for performing an additive manufacturing step following the coating step. Advantageously, the precursor material manufacturing device 3 is fluidly connected to the additive manufacturing device 4 so that it is possible to transfer a precursor material 10 comprising a plurality of precursor material particles 9 from the precursor material manufacturing device 3 to the additive manufacturing device 4.
[0049] In the coating step, the granular particles 6 containing the drug substance 5 are coated with a coating agent 8 containing thermoplastic material 7 to produce a powdered precursor material 10 containing a plurality of precursor material particles 9. In addition to the thermoplastic material 7, the coating agent 6 may also contain a solvent 57, wherein water and / or organic solvents are particularly suitable as solvents, and alcohols and / or ketones and / or alkanes and / or ethers are suitable as organic solvents. Polyvinylpyrrolidone (PVP), polyvinylpyrrolidone-vinyl acetate copolymer (PVPVA), ethyl cellulose (EC), hydroxypropyl cellulose (HPC), hydroxypropyl methylcellulose (HPMC), or eudrabite are preferably used as the thermoplastic material 7. Thermoplastic material 7, as the name suggests, has thermoplastic properties, i.e., it softens upon heating and solidifies upon cooling without undergoing chemical changes. Biocompatible material 7 is particularly suitable for this process. Suitablely, the precursor material manufacturing apparatus 3 includes a coating device 11, which is specifically designed as a fluidized bed device 12, a spray bed device 13, or a roller coating device 14.
[0050] As in Figures 1 to 4 As shown in the corresponding embodiments, the precursor material manufacturing apparatus 3 further includes a granulation device 28, which produces granules 6 containing the drug substance 5. The granulation device 28 is suitably designed as a vertical granulator 29, a spray dryer 30, a fluidized bed device 12, or a jet bed device 13, and is preferably located upstream of the coating device 11.
[0051] According to device 1 Figure 1 The first embodiment shown in the diagram, performed on the equipment 1, includes a granulation step in which granules 31 consisting of multiple granular particles 6 are produced by vertical granulation. The granulation step is performed prior to the coating step. In vertical granulation (also known as high-shear granulation or wet granulation), various powdered initial raw materials 32 containing pharmaceutical substances 5, with the addition of a liquid granulating agent 33, are formed into large, uniformly distributed, and very dense granular particles 6 by the high mechanical shear action of a rotating mixing tool 34 (particularly an anchor mixer 69, a blade mixer 70, or a paddle mixer). The shape of the mixing tool 34 preferably matches the profile of the mixing container of the vertical granulator 29. In vertical granulation, a dissolved binder or a water-organic solvent mixture is particularly used as the granulating agent 33. Commonly used binders include water, polyvinylpyrrolidone, cellulose esters, or gelatin.
[0052] exist Figure 2In the second embodiment shown, a spray drying apparatus 30 is used to illustrate an alternative design to the granulation apparatus 28, wherein the granulation step also occurs before the coating step. Therefore, the spray drying process is performed using the spray drying apparatus 30. In spray drying, the powdered initial raw material 32 containing the drug substance 5 is dissolved, emulsified, or dispersed in a solvent or carrier material solution. Then, the solution, emulsion, suspension, or dispersion containing the initial raw material 32 is atomized and sprayed into the drying chamber 36, through which a hot drying gas flow 35 promotes solvent evaporation. In spray drying, the resulting granules 6 exhibit significant differences in particle size and poor flowability.
[0053] according to Figure 1 and Figure 2 The apparatus 1 shown performs a sieving step between the granulation and coating steps to produce granules 31 with a unimodal particle size distribution for the coating step. For this purpose, the precursor material manufacturing apparatus 3 has a sieving device 37, which is suitably located downstream of the granulation apparatus 28 and upstream of the coating apparatus 11. In the sieving device 37, the granules 31, consisting of multiple granular particles 6, are conveyed through a sieve 38 with the desired mesh size, thereby producing sieved granules 31 with a unimodal particle size distribution.
[0054] After the screening step, Figure 1 and Figure 2 In both embodiments, in the coating step designed as a roller coating method, the granular particles 6 are coated with a coating agent 8 containing thermoplastic material 7 within a roller coating apparatus 14 having a rotating roller. In the roller coating apparatus 14, the granular particles 6 move gently and controllably within a roller 39 and are coated with a coating layer 27 having a layer thickness 40. It is crucial that the coating agent 8 is distributed as uniformly as possible. This is achieved, on the one hand, by a spraying facility with a corresponding nozzle device 51, and on the other hand, by uniform mixing, ensuring the spraying of the coating agent 8. In the coating step, the roller 39 is also passed through a coating drying gas 41, thereby drying the coating agent 8 containing thermoplastic material 7 into the coating layer 27, which is applied to the granules 31 containing a large number of granular particles 6.
[0055] and Figure 1 and Figure 2 The first two implementation methods shown are different. Figure 3 and Figure 4 The two embodiments shown do not have a sieving step between the granulation and coating steps. The vertical granulation or spray drying process in the granulation step is the same as described in the previous two embodiments. Subsequently, according to... Figure 3 The vertical granulation process shown or according to Figure 4The granules 31 produced during the spray drying process shown are coated in time after the granulation step, in the third embodiment in the fluidized bed apparatus 12 and in the fourth embodiment in the spray bed apparatus 13. In both embodiments, the granules 31 are placed as a substrate in the respective fluidized bed apparatus or spray bed apparatus 12, 13 and sprayed with a coating agent 8 containing thermoplastic material 7.
[0056] Like fluidized beds, jet beds are also based on the principle of fluidization and utilize process gas 45 (especially process air or inert gas such as nitrogen) flowing upward through the fluidized bed device 12 or jet bed device 13 to pneumatically transport granular particles 6. The main difference lies in the design of the process gas inlet. In the jet bed device 13, the process gas inlet is designed as a slit opening 71, combined with a special streamline shape and a rapidly expanding process chamber 42. In the fluidized bed device 13, the process gas inlet is designed as a perforated plate substrate, also known as the inflow substrate 46.
[0057] The following will be exemplified. Figure 7 The working principle and schematic structure of the fluidized bed apparatus 12 for manufacturing tablets 2 are shown, with its cross-section AA passing through the conical portion of the process chamber 42. In the fluidized bed apparatus 12, granular particles 6 are coated to form precursor material particles 9.
[0058] The fluidized bed apparatus 12 comprises, from bottom to top, a distribution chamber 43, a process chamber 42, and an exhaust section 44. Suitably, the process chamber 42 of the fluidized bed apparatus 12 has a circular cross-section 50. Process gas 45, required for coating and drying the precursor material 10 containing a large amount of precursor material particles 9, is fed into the distribution chamber 43, where it is distributed, and then flows into the process chamber 42 via the inflow substrate 46. The lower region of the process chamber 42 is defined by inclined sides 49, making its lower region conical. The process gas 45 flows through the process chamber 42 to the exhaust section 44, preferably exiting the fluidized bed apparatus 12 as exhaust gas 48, which is purified by a dust removal system 47 (particularly a filter element or textile filter element) arranged within the exhaust section 44.
[0059] In process chamber 42, granular particles 6 are pre-added or automatically generated, and are fluidized by being carried upward by process gas 45 toward a dust removal system 47 arranged within exhaust section 44. In the upper region of process chamber 42, the velocity of the process gas decreases, causing the upwardly flowing granular particles 6 to fall back into the lower region of process chamber 42. Through this mechanism, a very uniform fluidized bed of granular particles 6 is formed in process chamber 42.
[0060] For example, in Figure 7Three different nozzle arrangements 51 are shown in the fluidized bed apparatus 12, specifically single-component or multi-component nozzles, which can be installed alternately. The coating agent 8 is sprayed into the process chamber 42 along the main spray direction through the nozzle arrangements 51. If the coating agent 8 containing thermoplastic material 7 is sprayed using the nozzle arrangements 51 located in the lower region of the process chamber 42, where the main spray direction is in the flow direction of the process gas 45 in the fluidized bed apparatus 12, the nozzle arrangements 51 produce a jet stream 56 also known as a "bottom spray". On the other hand, if the nozzle arrangements 51 are located in the upper region of the process chamber 42, and the spraying is performed in the main spray direction opposite to the flow direction of the process gas 45, the nozzle arrangements 51 produce a jet stream 56 also known as a "top spray". According to a third preferred embodiment (the arrangement of which is further specified...), ... Figure 8 As shown in the diagram, the fluidized bed apparatus 12 has a nozzle device 51 arranged beside the process chamber 42, wherein the main spray direction is parallel to the tangent 55 of the circular cross-section 50 of the process chamber 42 and is arranged within an arc segment 52 of the circular cross-section 50, the height 53 of which is 30% of the cross-sectional radius 54, wherein the coating agent 8 or a suspension containing the coating agent 8 is sprayed into the fluidized bed apparatus 12 through the nozzle device 51. For this purpose, only the tangential component of the main spray direction of the jet flow 56 needs to be formed. This nozzle device 51 is also called a so-called tangential spray nozzle device 51, which produces a "tangential spray". By tangentially spraying the coating agent 8 containing thermoplastic material 7, the coating agent 8 is coated very uniformly onto the granular particles 6, thereby producing a coating layer 27 with a substantially constant layer thickness 40 on the granular particles 6, so that the resulting precursor material particles 9 exhibit very good flowability.
[0061] The nozzle device 51 (preferably a two-component nozzle) is configured to spray extremely small droplets 62 with a droplet size of 1µm to 100µm, preferably 1µm to 50µm, and more preferably between 5µm and 10µm. By adjusting the droplet size of the nozzle device 51 and the compressed air applied to it, the shear force occurring during spraying can be precisely controlled, thereby achieving or obtaining a very uniform droplet size of the coating agent 8 to be sprayed. The droplets 62 adhere to the granular particles 6 containing the drug substance 5, and if solvent 57 is used, preferably, film evaporation of the solvent occurs.
[0062] Due to the highly favorable heat and mass transfer and the high-speed circulation of the granules within the spray zone 58 of the process chamber 42 of the fluidized bed apparatus 12, the coating agent 8 is largely deposited on the granules 6, resulting in uniform wetting of the granules on their surfaces 59. This uniform wetting, combined with the high-speed circulation of the granules within the spray zone 58, leads to the formation of a very uniform coating layer 27 on the granules 6. During the drying process, the solvent 57 evaporates and is discharged from the fluidized bed apparatus 12 with the exhaust gas 48. The thermoplastic material 7 contained in the coating agent 8 remains on the granule surface 59 of the granules 6 as a coating layer 27 with a layer thickness 40, thereby ensuring very uniform growth and coating of the resulting precursor material particles 9.
[0063] Figure 10 A schematic process is described in which a precursor material particle 9 is formed by coating a particle 6 having a particle diameter of 60 with a coating layer 27 having a layer thickness of 40.
[0064] The discharge 61 of the coated granular particles 6 (referred to as precursor material particles 9) can be achieved by an overflow section or a volumetric discharge component (especially a rotary valve), or by a gravity screen (preferably a zigzag screen or a riser screen to which screening gas is applied).
[0065] Alternatively, in addition to the coating agent 8, liquid additives or other components may be sprayed into the process chamber 42, thereby uniformly embedding them into the granular structure. The additives may also be included in the coating agent 8.
[0066] exist Figure 5 and Figure 6 In the fifth and sixth embodiments shown, granules 31, composed of a plurality of granular particles 6, are generated in the coating apparatus 11 and simultaneously coated. Therefore, the granulation step and the coating step are performed concurrently. Preferably, the granulation step performed concurrently with the coating step is executed as a spray agglomeration process or a spray granulation process.
[0067] In spray agglomeration, extremely fine powdery initial raw materials 32 (also called initial particles) move in a fluidized bed and are sprayed with a binder liquid, thereby forming liquid bridges between the initial raw materials 32 and producing so-called agglomerated particles. Here, the binder liquid is also suitably a coating agent 8. Due to the low kinetic energy during spray agglomeration in a fluidized bed, residual moisture evaporates, forming a porous structure with many internal capillaries (i.e., cavities). This new structure is further solidified by the hardened binder liquid. The dust-free, free-flowing agglomerated particles are easy to meter and can be further optimized for subsequent processing. In agglomeration, by introducing the binder liquid, the finely dispersed initial raw materials 32 are transformed into granular particles 6 in the form of polymeric units. Therefore, these agglomerated particles are referred to below as granular particles 6. Accordingly, the agglomerates containing a large number of agglomerated particles produced in spray agglomeration are also referred to as granules 31. The agglomerated particles are simultaneously coated in a fluidized bed or spray bed by using the coating agent 8 as a binder liquid.
[0068] During spray granulation, parameters such as particle size, residual moisture, and solids content can be selectively influenced, and various product characteristics of the granules 6 can be adjusted. The granules 6 produced by spray granulation have a dense surface structure and high packing or bulk density; due to their small surface area 59, they have very low hygroscopicity and thus absorb almost no ambient moisture. Furthermore, they possess excellent flowability, abrasion resistance, drip resistance, easy solubility, and optimal metering. Therefore, the granules 6 are simultaneously coated in a fluidized bed or spray bed. Compared to agglomerates, the granules 31 produced by spray granulation are denser and harder.
[0069] exist Figure 5 In the precursor material manufacturing apparatus 3 shown, the precursor material 10 is manufactured by spray granulation in a coating apparatus 11 designed as a fluidized bed apparatus 12, wherein the granules 31 are added in advance and the granules 6 are sprayed with a coating agent 8.
[0070] In a series of experiments, metoprolol succinate was used as the active pharmaceutical ingredient to perform the following procedures: Figure 5 The process involves a β-blocker with extremely poor flowability. The angle of repose is 52°, and the Hausner factor is 1.68. The active pharmaceutical ingredient is pre-placed in a fluidized bed apparatus 12 and coated with a thermoplastic material 7, Kollidon VA 64 (PVPVA), using a tangential spraying method, as this material has good solubility in water and organic solvents. The flowability of the resulting precursor material particles 9 is significantly improved by the simultaneous granulation and coating steps performed in the fluidized bed apparatus 12. At this point, the angle of repose is 31°, and the Hausner factor is 1.21. Another advantage is that the material 7 is uniformly distributed on the surface 59 of the granules, thereby increasing the contact area between the individual precursor material particles 9.
[0071] Instead, precursor material 10 is prepared according to... Figure 6 The precursor material manufacturing apparatus 3 is designed as a spray bed apparatus 13 and is manufactured using a spray agglomeration process in the coating apparatus 11. In this process, the granules 31 are fed into the spray bed apparatus 13 together with the coating agent 8 in the form of a solution, emulsion, suspension or melt.
[0072] Each manufactured precursor material particle 9 includes a granular particle 6 having a particle diameter of 60 and a coating layer 27 covering the granular particle 6, the coating layer having a layer thickness of 40, wherein the granular particle 6 contains a pharmaceutical substance 5, and the coating layer 27 is formed by a coating agent 8 comprising a thermoplastic material 7. The precursor material particle 9 preferably has a sphericity greater than or equal to 0.75, suitably greater than or equal to 0.9, and particularly greater than or equal to 0.93.
[0073] Furthermore, the precursor material particles 9 have a precursor material particle diameter 63 of 20µm to 200µm, preferably 50µm to 150µm. The precursor particle diameter 63 is obtained by adding twice the thickness 40 of the coating layer 27 to the particle diameter 60. Preferably, the coating layer 27 has a thickness 40 in the range of 0.1µm to 50µm, particularly in the range of 5µm to 20µm. By preferably selecting the precursor material particle diameter 63, it is ensured that laser energy can penetrate the precursor material particles 9, and that the coating layers 27 of the precursor material particles 9, made of thermoplastic material 7, can be joined together, particularly fused together. In addition, a smaller precursor material particle diameter 63 has a larger surface area, thereby absorbing more laser energy. It has been shown to be advantageous that the ratio of the particle diameter 60 to the layer thickness 40 of the precursor material particles 9 is 2:1 to 15:1, particularly 2:1 to 10:1.
[0074] Precursor material 10, containing a large number of precursor material particles 9, is specifically used to manufacture tablet 2, wherein, in an additive manufacturing step, the precursor material particles 9 are selectively laser-sintered into tablet 2. Here, a high-power laser sintersulates material 7 (particularly the thermoplastic material 7 of coating agent 8) into a solid coating matrix 64, which is based on a three-dimensional model of tablet 2.
[0075] Within the additive manufacturing apparatus 4, in the additive manufacturing step, a powdered precursor material 10 containing a large number of precursor material particles 9 is selectively laser-sintered into tablets 2. For this purpose, the additive manufacturing apparatus 4 is specifically designed as a powder bed melting system 15, which takes the form of a selective laser sintering printer 16. The powder bed melting system 15, designed as a selective laser sintering printer 16, suitably includes at least one laser unit 17, wherein the laser unit 17 has a CO2 laser 18 or a fiber laser 19. Each laser unit 17 has a scanning system 21 formed by at least one reflector 20, which is controlled by at least one drive unit (not shown) such that each laser beam 22 of the laser unit 17 heats the precursor material particles 9 to or above their melting point, so as to join the precursor material particles 9 together to form tablets 2, particularly by fusing them together. For this purpose, the CO2 laser 18 used suitably has a wavelength in the range of 9600 nm to 10600 nm at a power of 14 W; the fiber laser 19 used has a wavelength of 1064 nm at a power of 10 W. According to a special design of the laser sintering printer 16, which has a structural cavity housing 73, the laser sintering printer 16 is suitable for manufacturing tablets 2 from precursor materials 10 by selective laser sintering under a protective gas atmosphere 23, wherein nitrogen or argon may be suitably used as the protective gas.
[0076] The additive manufacturing process includes three steps: tablet printing, cooling of the printed tablet 2, removal of the cooled tablet 2 from the additive manufacturing apparatus 4, and separation of the tablet 2 from the excess powdered precursor material 10.
[0077] Therefore, within the additive manufacturing apparatus 4, in the first step, powdered precursor material 10 is distributed in thin layer form as a powder bed 24 from the precursor material storage section 71 by a dispensing device 74 onto the platform 25 within the build cavity 26 of the additive manufacturing apparatus 4. The powder bed 24 contains a large number of precursor material particles 9, having the precursor material 10, and is preferably preheated to a temperature slightly below the melting point of the thermoplastic material 7 by a preheating device (not shown). This allows the temperature of certain areas of the powder bed 24 to be slightly increased again by the lasers 18, 19 of the laser unit 17, which solidify these areas by tracing the shape of the tablet 2. The lasers 18, 19 scan the cross-section of the 3D tablet model and accordingly heat the powdered precursor material 10 to a temperature slightly below its melting point or just to its melting point, thereby mechanically fusing the precursor material particles 9 together and producing a solid tablet 2. The precursor material particles 9 are particularly advantageously welded by a coating layer 27 containing thermoplastic material 7 applied to the granules 6, because the good flowability of the precursor material particles 9 and the uniform coating layer 27 ensure their uniform distribution on the powder bed 24 in the platform 25. Since the unsintered powdered precursor material 10 supports the tablet 2 by lasers 18 and 19 during printing, no additional support structure for tablet manufacturing is required in the additive manufacturing apparatus 4. The platform 25 then descends one layer into the build chamber 26 according to the precursor material particle diameter 63 (typically between 50 µm and 200 µm). The entire process is then repeated for each layer until the tablet is manufactured.
[0078] Subsequently, the building cavity 26 is preferably cooled in the second step, first within the additive manufacturing apparatus 4 and then (if necessary) outside the additive manufacturing apparatus 4, which is designed as a laser sintering printer 16, to ensure optimal mechanical properties and to ensure that the tablet 2 does not deform.
[0079] In the third step of the additive manufacturing process, the finished tablet 2 is removed from the construction cavity 26, and excess powdered precursor material 10 is separated and removed. The excess powdered precursor material 10 can be reused, and the tablet 2 can be post-processed if necessary.
[0080] By performing this method on device 1, tablets 2 with a very high drug loading can be produced, with a drug loading of more than 40%, preferably more than 60%, and more preferably more than 80%.
[0081] Therefore, the tablet 2 produced according to method 2 for manufacturing tablets comprises a plurality of precursor material particles 9 interconnected by selective laser sintering, wherein the precursor material particles 9 have granular particles 6 and a coating layer 27 covering the granular particles 6, the granular particles having a granular particle diameter 60 and the coating layer having a layer thickness 40. In this example, the granular particles 6 contain a pharmaceutical substance 5, and the coating layer 27 is formed by a coating agent 8 containing a thermoplastic material 7. The coating layer 27 of each precursor material particle 9 forms a coating layer matrix 64 by laser sintering, wherein the granular particles 6 are embedded in the mutually fused coating layer 27 of each precursor material particle 9.
[0082] Specifically, tablet 2 comprises different precursor material particles 9, wherein the different precursor material particles 9 each contain granular particles 6 of different drug substances 5. This allows the different drug substances 5 to have different release profiles.
[0083] according to Figure 11 The tablet 2 has two precursor material layers 65, which are labeled as the first precursor material layer 65a and the second precursor material layer 65b for easy distinction. The tablet 2 is formed into a multilayer tablet through the two precursor material layers 65a and 65b. Figure 11 A multilayer tablet with two precursor material layers 65a and 65b and a vertical section AA is shown. The precursor material layer 65 of the tablet 2 shown further comprises different precursor material particles 9, which are respectively labeled as first precursor material particle 9a and second precursor material particle 9b for easy distinction. Therefore, the precursor material particles 9a of precursor material layer 65a are different from the precursor material particles 9b of the precursor material layer 65b adjacent to precursor material layer 65a.
[0084] This multilayer tablet integrates different therapeutic drug loads into a single dosage form through different precursor material particles 9a and 9b, because the drug substance 5 contained in the different precursor material particles 9a and 9b in the corresponding precursor material layers 65a and 65b can have different release profiles.
[0085] Figure 12 It shows along Figure 11The diagram shows a vertical cross-sectional view of the cross-section AA of the multilayer tablet. The precursor material layer 65b suitably comprises precursor material particles 9b with different bulk densities, resulting in a higher bulk density of the precursor material layer 65b, thereby improving the overall compactness and stability of the tablet 2. In the illustrated embodiment, the precursor material particles 9a and 9b are coated with the same coating agent 8. This is advantageous because the thermoplastic material 7 forming the coating layer 27 is heated in the same manner during selective laser sintering via the laser sintering printer 16. Different coating agents 8 can be used, but care should be taken when selecting the coating agent 8 to ensure that the melting points of the thermoplastic materials 7 are approximately the same. The coating layer 27 forms a coating matrix 64 in each precursor material layer 65a and 65b, in which granular particles 6 containing the drug substance 5 are embedded. Here, the two coating matrices 64 of the precursor material layers 65a and 65b are also labeled as the first coating matrix 64a and the second coating matrix 64b, respectively. Since the same coating agent 8 was selected for different precursor material particles 9a and 9b, the two coating substrates 64a and 64b can also be optimally fused together.
[0086] Furthermore, the precursor material layer 65b is characterized in that it comprises excipient particles 66, wherein the excipient particles 66 have disintegrating particles 67 and a coating layer 27 covering the disintegrating particles 67, the disintegrating particles having a disintegrating particle diameter, the coating layer having a layer thickness 40, wherein the disintegrating particles 66 contain a disintegrant, and the coating layer 27 is formed of a coating agent 8 comprising thermoplastic material 7, particularly of the same coating agent 8 as the precursor material particles 9. This allows for the targeted determination of the release profile of the drug substance 5 in the tablet 2.
[0087] According to another design of tablet 2 (which serves as...) Figure 13 The schematic diagram is shown as follows Figure 11 The diagram shows a cross-sectional view of the lower precursor material layer 65b of the multilayer tablet (as shown). The precursor material layer 65b of tablet 2 has three meandering capillary channels 68, each designed to introduce liquid (e.g., gastric juice, in particular) into the tablet interior via capillary action. The release profile of tablet 2a can also be adjusted and regulated via the capillary channels 68. Other shapes of the capillary channels are also implemented in embodiments not shown. The shapes of these capillary channels can also vary, for example, in terms of their diameter or depth of penetration into the tablet interior.
[0088] Finally, the manufactured tablets 2 can be refined in a post-processing step. Figure 4In the apparatus 1 shown, the tablets 2 manufactured in the additive manufacturing step within the additive manufacturing apparatus 4 are coated with an enteric coating layer in the post-processing step, here in the roller coating apparatus 14. The coating process performed in the post-processing step operates in the same manner as the coating process described above in the roller coating apparatus 14.
Claims
1. A precursor material (10) for manufacturing tablets (2), characterized in that, The precursor material (10) has a plurality of precursor material particles (9), wherein each precursor material particle (9) has a granular particle (6) and a coating layer (27) covering the granular particle (6), the granular particle having a granular particle diameter (60), the coating layer having a layer thickness (40), wherein the granular particle (6) has a pharmaceutical substance (5), and the coating layer (27) is formed of a coating agent (8) containing a thermoplastic material (7).
2. The precursor material (10) according to claim 1, characterized in that, The precursor material particles (9) have a sphericity greater than or equal to 0.75, suitably greater than or equal to 0.9, and especially greater than or equal to 0.
93.
3. The precursor material (10) according to claim 1 or 2, characterized in that, The precursor material particles (9) have a precursor material particle diameter (63) of 20µm to 200µm, preferably 50µm to 150µm.
4. The precursor material (10) according to any one of claims 1 to 3, characterized in that, The coating layer (27) has a layer thickness (40) in the range of 0.1µm to 50µm, particularly in the range of 5µm to 20µm.
5. The precursor material (10) according to any one of claims 1 to 4, characterized in that, The ratio of the particle diameter (60) to the layer thickness (40) of the precursor material particles (9) is 2:1 to 15:1, especially 2:1 to 10:
1.
6. The precursor material (10) according to any one of claims 4 to 5, wherein, The coating agent (8) used has a solvent (57) in addition to the thermoplastic material (7).
7. The precursor material (10) according to claim 6, characterized in that, As a solvent (57), water and / or organic solvents are used, wherein alcohols and / or ketones and / or alkanes and / or ethers are suitably used as organic solvents.
8. The precursor material (10) according to any one of claims 1 to 7, characterized in that, Polyvinylpyrrolidone (PVP), polyvinylpyrrolidone-vinyl acetate copolymer (PVPVA), ethyl cellulose (EC), hydroxypropyl cellulose (HPC), hydroxypropyl methylcellulose (HPMC) or methacrylates (Eudragite) are used as thermoplastic materials (7).
9. Use of a precursor material (10) having a plurality of precursor material particles (9) in the manufacture of a tablet (2), characterized in that, In the additive manufacturing step, precursor material particles (9) are selectively laser sintered into tablets (2).
10. The use according to claim 9, characterized in that, In the additive manufacturing step, when selectively laser sintering the precursor material particles (9) of the precursor material (10) into tablets (2), a powder bed melting system (15) designed as a selective laser sintering printer (16) is used, wherein the powder bed melting system (15) has at least one laser unit (17), wherein for the selective laser sintering, a CO2 laser (18) or a fiber laser (19) is used, wherein suitably, for the selective laser sintering, when using a CO2 laser (18), a wavelength of 10600 nm at a power of 14 W is used; and when using a fiber laser (19), a wavelength of 1064 nm at a power of 10 W is used.