Composite semipermeable membrane, method for producing the same, separation membrane element, and fluid separation device

By designing specific porous layers with molecular weight cutoff and specific surface area in the composite semipermeable membrane, and forming an uneven shape on the back of the porous layer, combined with a cross-linked polyamide separation functional layer, the problem of reduced water permeability and salt removal under high temperature and high pressure is solved, and performance is maintained under harsh conditions.

CN123146428APending Publication Date: 2026-11-20TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202580029011.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-22
Filing Date
2025-04-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Under high-pressure operating conditions, the water permeability and salt removal capacity of composite semi-permeable membranes are easily reduced, especially during the start-up and shutdown processes under high temperature and high pressure, where existing technologies struggle to effectively maintain their performance.

Method used

By employing a porous layer with a specific range of molecular weight cutoff and specific surface area, and forming an uneven shape on the back side of the porous layer, combined with a cross-linked polyamide separation functional layer, a composite semi-permeable membrane structure is formed. By controlling the structure and material properties of the porous layer, its pressure resistance and salt removal performance can be improved.

Benefits of technology

Maintaining the water permeability and salt removal properties of the composite semi-permeable membrane under high temperature and high pressure, and resisting damage from repeated start-up and shutdown, improves the membrane's durability and salt removal performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146428A_ABST
    Figure CN123146428A_ABST
Patent Text Reader

Abstract

The present invention relates to a composite semipermeable membrane which is a composite semipermeable membrane having a base material, a porous layer provided on the base material, and a separation functional layer provided on the porous layer, the porous layer having a molecular weight cut-off of 10k to 60kDa and a specific surface area of 20 to 50m 2 / g; or to a composite semipermeable membrane which is a composite semipermeable membrane having a base material, a porous layer provided on the base material, and a separation functional layer provided on the porous layer, the porous layer having a molecular weight cut-off of 10k to 60kDa and a tortuosity of 1.5 to 7.0 after the composite semipermeable membrane is supplied with an aqueous solution of NaCl concentration 3.5 mass%, pH 6.5 for 2 hours under conditions of 5.5MPa, 25°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a composite semipermeable membrane useful during high-pressure operation and a method for manufacturing the same. It also relates to a separation membrane element comprising the aforementioned composite semipermeable membrane, and a fluid separation apparatus comprising the aforementioned separation membrane element. Background Technology

[0002] Generally speaking, composite semipermeable membranes, which are obtained by coating a porous layer with a separation functional layer formed by the polycondensation reaction of cross-linked polyamides obtained by polyfunctional amines and polyfunctional acyl halides, are used in reverse osmosis treatments such as seawater desalination to remove solutes from raw water due to their high water permeability and salt removal capacity.

[0003] In reverse osmosis, a pressure greater than the difference between the osmotic pressure on the supply water side and the osmotic pressure on the permeate side is applied to the supply water side of the composite semipermeable membrane. In recent years, reverse osmosis has sometimes been used for ZLD (Zero Liquid Discharge) to achieve zero wastewater discharge and for concentration in valuable substance recovery processes. Depending on the solute concentration, it is also increasingly being operated at higher pressures than before.

[0004] During the high-pressure operation of this reverse osmosis process, the permeability of the composite semipermeable membrane sometimes decreases. Without a pressure path, the permeability of the composite semipermeable membrane is dominated by the separation functional layer, as the permeability of the porous layer is more than 100 times that of the separation functional layer. However, Patent Documents 1-3 indicate that the compaction of the porous layer caused by high-pressure operation reduces its permeability, thus decreasing the permeability of the composite semipermeable membrane.

[0005] Patent document 1 discloses the following reverse osmosis composite membrane: The average membrane thickness t0 [μm] of the support membrane after applying a pressure of 5.5 MPa for 3 hours in the membrane thickness direction and then releasing the pressure is compared with the pure water permeation coefficient p0 [g / (cm²)]. 2 The average membrane thickness t1 [μm] and the pure water permeability p1 [g / (cm)] after the support membrane is released after applying a pressure of 10 MPa in the thickness direction for 3 hours are compared with the pure water permeability p1 [g / (cm)]. 2 By making t1 / t0 and p1 / p0 meet specific numerical ranges, compaction is suppressed.

[0006] Patent Document 2 discloses a composite semi-permeable membrane, wherein a porous support comprises a dense layer in contact with a separation functional layer and a macroporous layer located between the dense layer and a substrate. In particular, it discloses that if the number of macropores per unit length in the membrane direction of the macroporous layer is within a specific range, the thickness of the porous support can be maintained even under high-pressure additional operation.

[0007] Patent document 3 discloses a porous layer structure that is designed to suppress crushing under high temperature and high pressure operation based on the relationship between the porosity and compressive strength of the porous layer, and focuses on the surface elastic modulus and the thickness of the dense layer.

[0008] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2001-252538 Patent Document 2: Japanese Patent Application Publication No. 2018-039003 Patent Document 3: International Publication No. 2023 / 145845 Summary of the Invention

[0009] The problem that the invention aims to solve In high-pressure processes such as ZLD, there are concerns about reduced permeability of composite semipermeable membranes. Furthermore, for example, in seawater desalination systems, temporary system shutdowns sometimes occur, resulting in high-pressure start-ups and shutdowns, subjecting the composite semipermeable membrane to pressure or release from pressure. This leads to repeated damage to the composite semipermeable membrane, reducing its permeability and salt removal capacity.

[0010] Regarding the reduction in water permeability, as disclosed in Patent Documents 1-3, it is clearly stated that it is caused by the compaction of the porous layer, and this can be addressed through porous layer compaction suppression technology. However, the suppression of porous layer compaction under harsh operating conditions such as start-up and shutdown at high temperatures and high pressures is insufficient. Furthermore, conventional porous layer compaction suppression technologies involve changes in the surface structure of the porous layer, which can also cause structural changes at the interface between the crosslinked polyamide and the porous layer, or within the crosslinked polyamide itself. This makes it impossible to obtain a composite semi-permeable membrane that can maintain salt removal performance under harsh operating conditions involving start-up and shutdown.

[0011] The present invention aims to provide a composite semi-permeable membrane that exhibits high retention of water permeability and salt removal performance under high temperature and high pressure conditions with start-up and shutdown cycles, and possesses high salt removal performance. The present invention also aims to provide a method for manufacturing the aforementioned composite semi-permeable membrane. Furthermore, the present invention aims to provide a separation membrane element incorporating the aforementioned composite semi-permeable membrane, and a fluid separation apparatus incorporating the aforementioned separation membrane element.

[0012] Methods for solving problems In order to solve the above-mentioned problems, the composite semipermeable membrane of the present invention comprises the following [1] to

[11] .

[0013] [1] A composite semipermeable membrane having a substrate, a porous layer disposed on the substrate, and a separation functional layer disposed on the porous layer, wherein the porous layer has a molecular weight cutoff of 10k to 60kDa and a specific surface area of ​​20 to 50m². 2 / g.

[0014] [2] A composite semipermeable membrane having a substrate, a porous layer disposed on the substrate, and a separation functional layer disposed on the porous layer, wherein the porous layer has a molecular weight cutoff of 10k to 60kDa, and the tortuosity is 1.5 to 7.0 after supplying the composite semipermeable membrane with an aqueous solution of NaCl concentration of 3.5% by mass and pH 6.5 for 2 hours at 5.5 MPa and 25°C.

[0015] [3] The composite semipermeable membrane as described in [1] or [2] above, wherein the surface of the porous layer opposite to the surface on which the separation functional layer is provided has an uneven shape, and the average equivalent circle diameter of the pores in the recess is 0.30 to 0.60 μm.

[0016] [4] The composite semipermeable membrane as described in any one of [1] to [3] above, wherein the mass per unit area of ​​the porous layer is 10 to 17 g / m². 2 .

[0017] [5] The composite semipermeable membrane as described in any one of [1] to [4] above, wherein the specific surface area of ​​the porous layer is 22 to 40 m². 2 / g.

[0018] [6] The composite semipermeable membrane as described in any one of [1] to [5] above, wherein the molecular weight cutoff of the porous layer is 30k to 45kDa.

[0019] [7] The composite semipermeable membrane as described in any one of [1] to [6] above, wherein the thickness of the porous layer is 10 to 20 μm after the composite semipermeable membrane is supplied with an aqueous solution of NaCl concentration of 3.5% by mass and pH 6.5 for 24 hours under conditions of 7.0 MPa and 45 °C.

[0020] [8] The composite semipermeable membrane as described in any one of [1] to [7] above, wherein the substrate is a long fiber nonwoven fabric with a thickness of 80 to 100 μm and the longitudinal tensile strength of the long fiber nonwoven fabric is 400 to 900 N / 5 cm.

[0021] [9] A separation membrane element having any one of the composite semipermeable membranes described in any one of [1] to [8] above.

[0022]

[10] A fluid separation device having the separation membrane element described above [9].

[0023]

[11] A method for manufacturing a composite semipermeable membrane, comprising the following steps (a) to (c): Process (a): The process of preparing a polymer solution obtained by dissolving a thermoplastic polymer in a good solvent onto a substrate; Step (b): The polymer solution disposed on the substrate is contacted with a first coagulation liquid containing a non-solvent and a good solvent of the thermoplastic polymer to form a porous layer on the substrate, thereby obtaining a porous support formed from the substrate and the porous layer with a good solvent content of 10 to 60 g / m³. 2 The process of constructing porous supports; Step (c): The step of immersing the above porous support in the second solidification liquid.

[0024] Invention Effects According to the present invention, a composite semipermeable membrane with high retention of water permeability and salt removal performance after high temperature and high pressure operation, and with high salt removal performance, can be obtained. Attached Figure Description

[0025] [ Figure 1 ] Figure 1 This is a cross-sectional view of a composite semipermeable membrane according to one embodiment of the present invention.

[0026] [ Figure 2 ] Figure 2 This is an unfolded view of a separation membrane element according to one embodiment of the present invention.

[0027] [ Figure 3 ] Figure 3 This is an image of the substrate side of the porous layer of the composite semi-permeable membrane in Example 1, observed using a scanning electron microscope at 500x magnification. The white areas in the image represent convex regions, and the surrounding gray areas represent concave regions. Detailed Implementation

[0028] The embodiments of the present invention are described in detail below, but the present invention is not limited thereto.

[0029] In this specification, the “~” in numerical range refers to the range including the values ​​before and after it. For example, “0 mass% to 100 mass%” means the range of more than 0 mass% and less than 100 mass%.

[0030] 1. Composite semi-permeable membrane As one embodiment of the present invention, the following is as follows: Figure 1As shown, a composite semi-permeable membrane 1 having a substrate 2, a porous layer 3 disposed on the substrate 2, and a separation functional layer 4 disposed on the porous layer 3 will be described. It should be noted that the composite of the substrate and the porous layer is referred to as a porous support.

[0031] 1.1 Substrate The substrate imparts physical strength to the composite semipermeable membrane. Examples of substrates include fabrics made of polymers such as polyester, polyamide, polyolefin, mixtures thereof, or copolymers thereof.

[0032] From the viewpoints of strength, texture forming ability, and fluid permeability, nonwoven fabrics are preferred as the substrate. Both long-fiber and short-fiber nonwoven fabrics are preferred as nonwoven fabrics.

[0033] Furthermore, long-fiber nonwoven fabrics composed of thermoplastic continuous filaments are less prone to fuzzing. Therefore, by using long-fiber nonwoven fabrics as the substrate, membrane defects can be suppressed. In addition, in the continuous film formation of composite semi-permeable membranes, tension is applied to the substrate in the film formation direction; therefore, long-fiber nonwoven fabrics with excellent dimensional stability are preferred as the substrate.

[0034] 1.1.1 Average single fiber diameter of the substrate When the substrate is a nonwoven fabric, the average single fiber diameter of the fibers constituting the nonwoven fabric is preferably 8 to 14 μm, more preferably 10 to 13 μm, and even more preferably 11 to 12 μm. If the average single fiber diameter is 8 μm or more, internal porosity is maintained throughout the entire substrate. By maintaining porosity in this way, the polymer solution can rapidly penetrate into the interior of the substrate when the porous layer is formed, thus the substrate and the porous layer are firmly bonded, and a composite semi-permeable membrane with excellent peel strength can be obtained. On the other hand, if the average single fiber diameter is 14 μm or less, a substrate and porous layer with excellent uniformity can be obtained.

[0035] The average single fiber diameter is obtained as follows: 10 single fibers are randomly selected from the substrate of the nonwoven fabric, the diameter of the randomly selected position of each single fiber is measured, and the arithmetic mean of the obtained values ​​is calculated as the average single fiber diameter.

[0036] 1.1.2 Weight per unit area of ​​the substrate The substrate used in the composite semi-permeable membrane of this embodiment preferably has a unit area weight of 60-120 g / m². 2 More preferably 60–100 g / m 2 More preferably 70–90 g / m 2By setting the weight per unit area of ​​the substrate within the aforementioned range, high mechanical strength is achieved, enabling it to withstand high-pressure operation, while reducing the thickness of the composite semi-permeable membrane and increasing the membrane area of ​​each separation membrane element.

[0037] 1.1.3 Density of the substrate The density of the substrate used in the composite semi-permeable membrane involved in this embodiment is preferably 0.70 to 0.95 g / cm³. 3 More preferably, it is 0.75–0.95 g / cm³. 3 More preferably, it is 0.80–0.95 g / cm³. 3 By setting the density of the substrate within the aforementioned range, deformation of the porous layer and the separation functional layer caused by infiltration into the substrate due to high-pressure operation can be suppressed. Furthermore, since the polymer solution can rapidly penetrate into the pores inside the substrate during the formation of the porous layer, the substrate and the porous layer are firmly bonded, resulting in a composite semi-permeable membrane with excellent peel strength.

[0038] 1.1.4 Substrate thickness The thickness of the substrate in the composite semi-permeable membrane according to this embodiment is preferably 80 to 100 μm. By setting the thickness of the substrate to the above range, it has high mechanical strength that can withstand high-pressure operation, and the thickness of the composite semi-permeable membrane can be reduced, thereby increasing the membrane area of ​​each separation membrane element.

[0039] The thickness of the substrate can be measured using a pointer-type thickness gauge or a digital thickness gauge. As pointer-type or digital thickness gauges, products from Ozaki Manufacturing Co., Ltd., such as PEACOCK and TECLOCK Corporation, can be used. When using a pointer-type or digital thickness gauge, the thickness is measured at 20 randomly selected locations, and the arithmetic mean is calculated as the thickness of the substrate.

[0040] 1.1.5 Tensile strength of the substrate The composite semi-permeable membrane of this embodiment preferably uses a long-fiber nonwoven fabric composed of thermoplastic continuous filaments as its substrate. Compared to short-fiber nonwoven fabrics, especially papermaking nonwoven fabrics with short fiber lengths, long-fiber nonwoven fabrics have higher mechanical strength, and the composite semi-permeable membrane based on the long-fiber nonwoven fabric substrate exhibits excellent durability even under conditions of high pressure applied during use. Furthermore, when operating as a separation membrane element, the composite semi-permeable membrane based on the long-fiber nonwoven fabric substrate can suppress the reduction in water production caused by the composite semi-permeable membrane sinking into the depressions of the water supply path material, or the resulting membrane damage.

[0041] Furthermore, the tensile strength in the nonwoven longitudinal direction (MD) of the long-fiber nonwoven fabric is preferably 400 to 900 N / 5 cm. By setting the tensile strength within the above range, the composite semi-permeable membrane can exhibit excellent durability even under high pressure conditions during use. Additionally, the tensile strength aspect ratio of the long-fiber nonwoven fabric is preferably 1.0 to 3.0. Here, "tensile strength aspect ratio" refers to the ratio of the tensile strength in the nonwoven longitudinal direction (MD) to the tensile strength in the nonwoven transverse direction (CD) (tensile strength in MD / tensile strength in CD).

[0042] Methods for controlling the tensile strength and tensile strength-to-width ratio of long-fiber nonwoven fabrics include, for example, applying heat and pressure, and stacking multiple layers of long-fiber nonwoven fabrics using calendering rollers to form a laminate. The preferred number of layers in the long-fiber nonwoven fabric is 2 to 5. If the number of layers is 2 or more, the strength is increased compared to a single layer; if it is 5 layers or less, wrinkles and interlayer delamination during lamination can be suppressed.

[0043] 1.2 Porous Layer The porous layer of the composite semi-permeable membrane involved in this embodiment is preferably formed of a thermoplastic polymer. Here, "thermoplastic polymer" refers to a polymer composed of chain-like polymeric substances that exhibits the property of deforming or flowing under external force when heated.

[0044] Examples of thermoplastic polymers include polysulfone (hereinafter "PSf"), polyethersulfone, polyphenylene sulfide sulfone, and polyphenylene sulfone. PSf is typically used due to its high chemical stability, mechanical stability, thermal stability, and ease of molding. The porous layer preferably contains the compounds listed above as its main components. Here, "main component" refers to a component that accounts for 50% or more by mass of the components constituting the porous layer.

[0045] When the thermoplastic polymer described above is PSf, the weight-average molecular weight (hereinafter "Mw") of the PSf, measured by gel permeation chromatography (GPC) using N-methylpyrrolidone as a solvent and polystyrene as a standard, is preferably 10,000 to 200,000, more preferably 15,000 to 100,000. If the Mw of PSf is 10,000 or more, mechanical strength and heat resistance, which are preferred for porous layers, can be obtained. Furthermore, if the Mw is 200,000 or less, the viscosity of the solution is within an appropriate range, and good moldability can be achieved.

[0046] 1.2.1 Specific surface area and molecular weight cutoff of porous layers In a first embodiment of the composite semi-permeable membrane of the present invention, the porous layer has a molecular weight cutoff of 10k to 60kDa and a specific surface area S of 20 to 50m². 2 / g. In this specification, the molecular weight cutoff and specific surface area S of the porous layer can be determined using any composite semipermeable membrane before and after use. For example, the molecular weight cutoff and specific surface area S of the porous layer can be determined after supplying the composite semipermeable membrane with an aqueous solution of 3.5% by mass and pH 6.5 at 7.0 MPa and 45°C for 24 hours, or after supplying the membrane with an aqueous solution of 3.5% by mass and pH 6.5 at 5.5 MPa and 25°C for 2 hours.

[0047] Specific surface area S represents the degree of three-dimensional network structure in a porous layer. A large specific surface area S indicates a dense three-dimensional network structure with numerous small pores. While this three-dimensional network structure hinders water permeability, it also disperses pressure, thus improving the pressure resistance of the porous layer. If the specific surface area S is 20 m², then... 2 If the density is above / g, the porous layer can effectively disperse pressure through its three-dimensional network structure, thus suppressing compaction even under high pressure operation. On the other hand, if it is 50m 2 When the specific surface area S of the porous layer of the composite semi-permeable membrane is below a certain value, the proportion of the three-dimensional network structure that acts as a barrier to the water permeability path can be suppressed, ensuring sufficient permeability. That is, when the specific surface area S of the porous layer of the composite semi-permeable membrane meets the above-mentioned range, the compaction of the porous layer under high pressure is suppressed by the three-dimensional network structure. Therefore, if the specific surface area S of the porous layer of the composite semi-permeable membrane after use meets the above-mentioned range, then the specific surface area S of the composite semi-permeable membrane before use also meets the above-mentioned range.

[0048] From the perspectives of suppressing the compaction of porous layers and ensuring permeability, the specific surface area S is preferably 20–40 m². 2 / g, more preferably 22-40m 2 / g, further preferably 28-35m 2 / g.

[0049] As a method for controlling the specific surface area S to the aforementioned range, for example, a method can be described in which, during the formation of a porous layer, a porous support obtained by immersing it in a first coagulation liquid to form a porous layer is contacted with a second coagulation liquid in a state containing a good solvent of the polymer that forms the porous layer. The specific surface area S can be controlled by the contact time with the first and second coagulation liquids and the temperature of each coagulation liquid.

[0050] Furthermore, maintaining salt removal performance during high-pressure operation with frequent start-ups and shutdowns is also a challenge. Regarding the decrease in salt removal performance, structural changes at the interface between the cross-linked polyamide and the porous layer, or within the cross-linked polyamide itself, are the main causes, making the structure of the porous layer surface forming the cross-linked polyamide crucial. However, a problem exists: if the specific surface area is to be controlled within the aforementioned range, the structure of the porous layer surface also changes, making it difficult to achieve the desired salt removal performance.

[0051] The inventors of this application have conducted repeated and in-depth research on the above-mentioned issues, and have found that the porous layer has a molecular weight cutoff of 10k to 60kDa and a specific surface area of ​​20 to 50m². 2 The composite semi-permeable membrane with a capacity of / g can balance the permeability and salt removal performance under high temperature and high pressure conditions with start-stop operation, as well as high salt removal performance.

[0052] That is, by balancing the aforementioned retention capacity and specific surface area, it is possible to suppress the compaction of the porous layer of the composite semipermeable membrane caused by high-pressure operation, and to suppress the decrease in water permeability and salt removal capacity. Such a composite semipermeable membrane that balances retention capacity and specific surface area has not been achieved in previous technologies.

[0053] "Molecular weight cutoff" refers to the molecular weight of dextran at which 90% of the linear dextran is removed, and can be determined using the method described in "7. Molecular weight cutoff of porous layers" in the examples described later. More preferably, the molecular weight cutoff of porous layers is 30k to 50kDa, and even more preferably 30k to 45kDa.

[0054] By setting the molecular weight cutoff of the porous layer within the aforementioned range, a composite semipermeable membrane capable of maintaining salt removal performance during start-up and shutdown operations can be obtained. When the molecular weight cutoff of the porous layer is greater than 60 kDa, during high-pressure start-up and shutdown operations, the separation functional layer sinks into the surface of the porous layer, causing deformation within the separation functional layer and resulting in a decrease in salt removal performance. Furthermore, when the molecular weight cutoff of the porous layer is less than 10 kDa, during the formation of the polyamide separation functional layer through interfacial polymerization, the amine aqueous solution cannot be adequately supplied from the porous layer to the interface. This not only reduces the permeability of the composite semipermeable membrane but also results in the formation of a low-strength polyamide, which cannot maintain salt removal performance under high-pressure operation. Methods for controlling the molecular weight cutoff of the porous layer within the aforementioned range include adjusting the coagulation temperature during the formation of the porous layer and adjusting the polymer concentration of the polymer solution used to form the porous layer.

[0055] 1.2.2 Tortuosity of porous layers In a second embodiment of the composite semipermeable membrane of the present invention, the porous layer has a molecular weight cutoff of 10k to 60kDa, and the tortuosity is 1.5 to 7.0 after supplying the composite semipermeable membrane with an aqueous solution of NaCl concentration of 3.5% by mass and pH 6.5 for 2 hours at 5.5 MPa and 25°C. Regarding the molecular weight cutoff, as described above.

[0056] "Tortuosity," also known as curvature, refers to the degree of curvature of the flow path through which the permeate passes. That is, the lower the tortuosity, the closer the flow path is to a straight line, resulting in a highly interconnected structure. From a pressure resistance perspective, a three-dimensional network structure formed through non-solvent-induced phase separation is preferred for the porous layer. While the three-dimensional network structure acts as a resistance to the permeation path as described above, it also disperses pressure, thus improving pressure resistance. Specifically, the tortuosity of the porous layer of the composite semi-permeable membrane after operation at 5.5 MPa is 1.5–7.0. This means that even after high-pressure operation, the porous layer retains a highly interconnected three-dimensional network structure. Similar to the specific surface area S mentioned above, the three-dimensional network structure can suppress compaction of the porous layer caused by high-pressure operation. When the tortuosity of the porous layer is greater than 7.0, the high curvature of the flow path within the porous layer makes it prone to flow path blockage accompanied by compaction caused by high-pressure operation, leading to reduced permeability. On the other hand, if the tortuosity is less than 1.5, the pressure cannot be dispersed due to the small proportion of the three-dimensional network structure in the porous layer, so compaction is likely to occur during high-pressure operation exceeding 5.5 MPa.

[0057] The "torsional stiffness" can generally be calculated based on the Kozeny-Carman formula, as described, for example, in the Journal of the Japanese Association for Petroleum Technology (Vol. 75, No. 2 (March, 2010) pp. 164-176). From the viewpoint of suppressing the compaction of porous layers, the tortional stiffness of the porous layer is preferably 1.5 to 5.5, more preferably 1.5 to 4.0. It should be noted that a tortional stiffness of 1.0 refers to fine pores with a straight cylindrical shape. Furthermore, it is more preferable that the tortional stiffness meets the above range after supplying an aqueous solution with a NaCl concentration of 3.5% by mass and a pH of 6.5 for 24 hours at 7.0 MPa and 45°C.

[0058] As a method for controlling the tortuosity of the porous layer to the above-mentioned range, for example, a method can be described in which, during the formation of the porous layer, a porous support obtained by immersing the porous layer in a first coagulating liquid is brought into contact with a second coagulating liquid in a state containing a good solvent of the polymer that forms the porous layer. The contact time with the first and second coagulating liquids and the temperature of each coagulating liquid can be controlled.

[0059] In this specification, the tortuosity is determined using the following formula (1).

[0060] Tortuosity = (ε / 2k) 1 / 2 ·(V / S) ……Equation (1) ε: Porosity of the porous layer after operation at 5.5 MPa [-] k: Permeability coefficient of the porous layer after operation at 5.5 MPa [m] 2 ] V: The pore volume of the porous layer after operation at 5.5 MPa [m] 3 / g] S: Specific surface area of ​​the porous layer after operation at 5.5 MPa [m²] 2 / g] Here, "after operation at 5.5 MPa" refers to the membrane filtration operation of the composite semi-permeable membrane after being supplied with an aqueous solution of NaCl concentration of 3.5% by mass and pH 6.5 for 2 hours at 5.5 MPa and 25°C. Furthermore, the porosity ε of the porous layer after operation at 5.5 MPa can be determined by the density ρ [g / cm³] of the thermoplastic polymer forming the porous layer. 3 The volume of the porous layer, calculated from the mass of the porous layer, is given by the ratio of the volume of the porous layer to the volume of the porous layer calculated from its thickness. Specifically, it is calculated using the methods described in "3. Thickness of the porous layer and the substrate" and "4. Porosity ε of the porous layer" in the embodiments described later.

[0061] The fine pore volume V[m] of the porous layer after operation at 5.5 MPa 3 / g] is the density ρ [g / cm³ of thermoplastic polymers that can form porous layers. 3 The porosity ε of the porous layer after operation at 5.5 MPa was calculated. Specifically, it was calculated using the method described in "5. Pore Volume V of the Porous Layer" in the embodiments described later.

[0062] The permeability k[m] of the porous layer after operation at 5.5 MPa 2 [The thickness L [m] and membrane area A [m²] of the porous layer under the conditions of 25℃ and pressure P [Pa] can be determined. 2 The pure water permeability Q[m] 3 The permeability coefficient k of the porous layer is calculated from the pure water viscosity μ[Pa·s], and specifically, is determined using the method described in “1. Permeability coefficient k of the porous layer” in the examples described later.

[0063] Furthermore, regarding the permeability coefficient k, from the viewpoint of stably obtaining the desirable properties of a porous membrane, a value of 0.35 × 10⁻⁶ is preferred. -17 ~5.0×10 -17 m2 More preferably, it is 0.70×10 -17 ~5.0×10 -17 m 2 Further preferred is 1.0×10 -17 ~5.0×10 -17 m 2 If the permeability coefficient k is within the above range, sufficient water permeability of the porous layer can be obtained, and the compaction of the porous layer can be suppressed even under high temperature and high pressure operation such as 7.0 MPa and 45°C.

[0064] To determine the aforementioned physical properties, as a method for removing the separation functional layer from the composite semipermeable membrane, for example, in the case where the separation functional layer is composed of polyamide, a method can be given by immersing the composite semipermeable membrane in an aqueous sodium hypochlorite solution to decompose and remove it. Specifically, the method described in "1. Permeability coefficient k of the porous layer" in the examples described later is used for removal.

[0065] 1.2.2 Pore diameter on the back side of the porous layer Regarding the composite semi-permeable membrane according to this embodiment, from the viewpoint of improving adhesion to the substrate, it is preferable that the side of the porous layer opposite to the side where the separation functional layer is provided (hereinafter, the "back side") has an uneven shape. The uneven shape of the back side of the porous layer is formed by transferring the uneven shape of the substrate surface, etc. "Uneven shape" refers to a shape with alternating continuous convex and concave portions. The uneven shape can be observed using a scanning electron microscope (hereinafter, "SEM").

[0066] In the composite semi-permeable membrane of this embodiment, the average equivalent circular diameter of the pores in the recesses on the back side of the porous layer is preferably 0.30 to 0.60 μm, more preferably 0.30 to 0.50 μm, and even more preferably 0.30 to 0.40 μm. If the average equivalent circular diameter is within the above range, it is possible to suppress the clogging of the pores on the substrate side of the porous layer caused by high-pressure operation, and water permeability can be easily ensured.

[0067] In the composite semi-permeable membrane described in this embodiment, the number of pores in the recesses on the back side of the porous layer is approximately 25 μm. 2 The preferred number of pores is 15 to 35. The pores in the recesses on the back side of the porous layer serve as flow paths for the filtrate; therefore, the more pores on the back side, the more interconnected and resilient the inner layer structure of the porous layer becomes, allowing it to withstand compaction. The number of pores in the recesses on the back side of the porous layer can be determined by SEM-based surface observation. Specifically, it is determined using the method described in "8. The uneven shape, number of pores, and average equivalent circle diameter of the back side of the porous layer" in the embodiments described later.

[0068] The number of pores in the recesses on the back side of the porous layer and the average equivalent circle diameter of the pores can be controlled, for example, by the coating thickness of the polymer solution onto the substrate and the amount of good solvent in the thermoplastic polymer before step (c) described in “2.1 Formation of Porous Layer”.

[0069] 1.2.3 Mass per unit area of ​​the porous layer The preferred mass per unit area of ​​the porous layer involved in this embodiment is 10–17 g / m². 2 More preferably 10-15 g / m 2 More preferably, it is 11-15 g / m 2 If the mass per unit area of ​​the porous layer is within the aforementioned range, it is easy to balance high mechanical strength capable of withstanding high-pressure operation with good connectivity (low tortuosity). The mass per unit area of ​​the porous layer can be controlled, for example, by the polymer concentration in the polymer solution, the coating thickness of the polymer solution onto the substrate, and the temperature of the coagulation solution.

[0070] 1.2.4 Thickness of the porous layer After supplying the composite semipermeable membrane according to this embodiment with an aqueous solution of NaCl concentration of 3.5% by mass and pH 6.5 for 24 hours at 7.0 MPa and 45°C, the thickness of the porous layer is preferably 10 to 20 μm, more preferably 10 to 18 μm, and even more preferably 10 to 15 μm. If the thickness of the porous layer is within the above range, sufficient strength is maintained to obtain pressure resistance, and it is easy to design a small tortuosity, which can suppress changes in permeability caused by high-pressure operation. Furthermore, the thickness of the porous support after the high-pressure operation is preferably 90 to 120 μm, more preferably 100 to 115 μm. The thickness of the porous layer can be controlled, for example, by the coating thickness of the polymer solution onto the substrate and the temperature of the coagulation solution.

[0071] 1.3 Separate functional layers The separation functional layer of the composite semi-permeable membrane involved in this embodiment preferably contains cross-linked polyamide, and more preferably contains cross-linked polyamide as a main component. Furthermore, the separation functional layer further preferably contains cross-linked aromatic polyamide as the cross-linked polyamide. The main component refers to a component that accounts for 50% or more by mass in the components of the separation functional layer. If the separation functional layer contains 50% or more of cross-linked polyamide, it can exhibit higher removal performance. Furthermore, the content of cross-linked polyamide in the separation functional layer is more preferably 80% or more by mass, and more preferably 90% or more by mass.

[0072] Crosslinked polyamides can be formed by chemically reacting a polyfunctional amine with a polyfunctional acyl halide. Preferably, at least one of the polyfunctional amine and the polyfunctional acyl halide comprises a compound with three or more functions. This yields rigid molecular chains and forms a porous structure suitable for removing fine solutes such as hydrated ions and boron. Preferably, the crosslinked aromatic polyamide is formed as a separation functional layer through a chemical reaction between a polyfunctional aromatic amine and a polyfunctional aromatic acyl halide.

[0073] A "polyfunctional amine" is an amine having at least two primary and / or secondary amino groups in one molecule. Examples of polyfunctional amines include o-phenylenediamine, m-phenylenediamine (hereinafter "m-PDA"), p-phenylenediamine, o-phenylenedimethylamine, m-phenylenedimethylamine, p-phenylenedimethylamine, o-diaminopyridine, m-diaminopyridine, p-diaminopyridine, etc., where two amino groups are bonded to the aromatic ring in any of the ortho, meta, or para positions; 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 3-aminobenzylamine, 4-aminobenzylamine, etc. Polyfunctional aromatic amines such as benzylamine, aliphatic amines such as ethylenediamine and propylenediamine, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, 2,5-dimethylpiperazine, 2-methylpiperazine, 2,6-dimethylpiperazine, 2,3,5-trimethylpiperazine, 2,5-diethylpiperazine, 2,3,5-triethylpiperazine, 2-n-propylpiperazine, 2,5-di-n-butylpiperazine, 1,3-bispiperidinylpropane, 4-aminomethylpiperazine, and other alicyclic polyfunctional amines. These polyfunctional amines can be used alone or in combination.

[0074] In particular, considering the membrane's selectivity, permeability, and heat resistance, m-PDA, p-phenylenediamine, and 1,3,5-triaminobenzene are preferred. Among these, m-PDA is more preferred due to its ease of acquisition and handling. These polyfunctional aromatic amines can be used alone or in combination of two or more.

[0075] "Polyfunctional acyl halides" refer to acyl halides and polyfunctional acid anhydride halides that have at least two halogenated carbonyl groups in one molecule. There are no particular limitations as long as the substance can form a separate functional layer of a cross-linked polyamide through reaction with the aforementioned polyfunctional amines. Examples of trifunctional acyl halides include trimesoyl chloride (hereinafter "TMC"), 1,3,5-cyclohexanetricarboxylate chloride, and 1,2,4-cyclobutanetricarboxylate chloride. Examples of difunctional acyl halides include aromatic difunctional acyl halides such as biphenyl dicarboxylate chloride, biphenylene dicarboxylate chloride, azophthaloyl chloride, terephthaloyl chloride, isophthaloyl chloride, and naphthalene dicarboxylate chloride; aliphatic difunctional acyl halides such as adipyl chloride and sebacyl chloride; and alicyclic difunctional acyl halides such as cyclopentanedicarboxylate chloride, cyclohexanedicarboxylate chloride, and tetrahydrofurandicarboxylate chloride. These polyfunctional acyl halides can be used alone or in combination.

[0076] Considering the selectivity and heat resistance of the membrane, a polyfunctional aromatic acyl chloride having 2 to 4 chlorocarbonyl groups in one molecule is preferred.

[0077] 1.4 Separation Membrane Elements The separation membrane element according to this embodiment includes the composite semi-permeable membrane according to this embodiment. For an example of the configuration of the separation membrane element, see [reference needed]. Figure 2 Please provide an explanation.

[0078] like Figure 2 As shown, the separation membrane element 5 includes a composite semi-permeable membrane 1, a supply-side flow path material 8, a permeation-side flow path material 9, a water collection pipe 10, and end plates 6 and 7.

[0079] The supply-side flow path material 8 is arranged opposite to the supply side of the composite semi-permeable membrane 1 and is wound around the water collection pipe 10 together with the composite semi-permeable membrane 1. As the supply-side flow path material 8, a mesh is preferred, for example.

[0080] The transmissive side flow path material 9 is arranged opposite to the transmissive side of the composite semipermeable membrane 1 and is wound around the water collection pipe 10 together with the composite semipermeable membrane 1. As the transmissive side flow path material 9, for example, tricot knitted fabric or sheet with protrusions can be used.

[0081] The water collection pipe 10 is a hollow cylindrical component with multiple holes on its side.

[0082] End plates 6 and 7 are disc-shaped components with multiple supply ports (or discharge ports).

[0083] The separation of fluid based on the separation membrane element 5 will be described. Supply water 11 is supplied to the separation membrane element 5 from multiple supply ports on the end plate 6. Regarding the supply water 11, it moves within a supply-side flow path formed by the supply-side flow path material 8 on the supply side of the composite semi-permeable membrane 1. The fluid that has permeated through the composite semi-permeable membrane 1 (shown as permeable water 12 in the figure) moves within a permeable-side flow path formed by the permeable-side flow path material 9. The permeable water 12 that reaches the water collection pipe 10 enters the interior of the water collection pipe 10 through its holes. The permeable water 12 flowing within the water collection pipe 10 is discharged to the outside from the end plate 7. On the other hand, the fluid that has not permeated through the composite semi-permeable membrane 1 (shown as concentrated water 13 in the figure) moves within the supply-side flow path and is discharged to the outside from the end plate 7. Thus, the supply water 11 is separated into permeable water 12 and concentrated water 13.

[0084] 2. Manufacturing method of composite semi-permeable membrane 2.1 Formation process of porous layer The porous layer formation process in the manufacturing method of the composite semipermeable membrane of the present invention includes the following steps (a) to (c).

[0085] Process (a): The process of preparing a polymer solution obtained by dissolving a thermoplastic polymer in a good solvent onto a substrate.

[0086] Step (b): The polymer solution disposed on the substrate is contacted with a first coagulating liquid containing a non-solvent and a good solvent of the thermoplastic polymer to form a porous layer on the substrate, thereby obtaining a porous support formed from the substrate and the porous layer with a good solvent content of 10 to 60 g / m³. 2 The process of creating porous supports.

[0087] Step (c): The step of immersing the above porous support in the second solidification liquid.

[0088] In step (a) described above, a polymer solution is coated onto a substrate. Then, in step (b) described above, the polymer solution is brought into contact with a first coagulated liquid containing polymers, a non-solvent and a good solvent, thereby causing phase separation to begin from the surface of the polymer solution and forming a porous layer.

[0089] In conventional methods for forming porous layers, the surface of the polymer solution comes into extensive contact with the coagulated liquid formed from the non-solvent of the polymer, resulting in immediate solidification and the formation of a dense three-dimensional network structure. However, within the polymer solution, the inflow of the coagulated liquid and the outflow of the good solvent from the polymer solution are suppressed due to the dense three-dimensional network structure formed on the surface, thus solidification is relatively slower compared to the surface layer. Therefore, in conventional methods for forming porous layers, phase separation occurs within the polymer solution, resulting in a porous layer with a larger pore size compared to the surface. This large pore size network structure has weak pressure resistance, which is detrimental to high-pressure operation.

[0090] The inventors of this application conducted repeated and in-depth research and found that setting the amount of good solvent in the porous support in step (b) to 10-60 g / m³ is effective. 2 In step (c), the porous support obtained in step (b) is immersed in a second coagulating liquid, causing the interior of the porous layer to completely solidify. This results in a composite semi-permeable membrane with a dense three-dimensional network structure formed inside the porous layer and small pore sizes on the surface of the porous layer. In step (c), the second coagulating liquid is brought into contact with the inner layer while the porous support contains a certain amount of good solvent. The inner layer of the porous layer dissolves, forming a dense three-dimensional network structure with high connectivity, which improves pressure resistance. That is, the molecular weight cutoff and specific surface area S, or the molecular weight cutoff and tortuosity after high-temperature and high-pressure operation, can be controlled within an appropriate range.

[0091] "Polymer" refers to thermoplastic polymers that form the main components of porous layers, as described above.

[0092] "Good solvent" refers to a solvent that dissolves polymers. By selecting a good solvent, the rate at which the good solvent flows out of the polymer solution in step (b) can be adjusted. As a result, the pore size on the back side of the porous layer and the flow path on the back side of the porous layer can be controlled. As a good solvent, at least one solvent selected from the group consisting of amides such as N-methyl-2-pyrrolidone, tetrahydrofuran, dimethyl sulfoxide, tetramethylurea, N,N-dimethylacetamide, N,N-dimethylformamide (hereinafter "DMF"), N,N-dimethylisobutyramide, N,N-diisopropylisobutyramide, N,N-bis(2-ethylhexyl)isobutyramide, acetone, lower alkyl ketones such as methyl ethyl ketone, esters such as trimethyl phosphate, and lactones such as γ-butyrolactone is preferred. Among these, DMF is more preferably used as a good solvent.

[0093] Process (a) can be carried out by coating a substrate with a polymer solution or by immersing the substrate in a polymer solution.

[0094] The coating of a polymer solution onto a substrate can be carried out by various coating methods. Among these, pre-quantity coating methods such as die coating, flow coating, and curtain coating, which can supply a precise amount of polymer solution, are preferred. In the formation of a porous layer, the slit-die method for coating the polymer solution is particularly preferred. The coating thickness of the polymer solution onto the substrate is preferably 50–150 μm, more preferably 80–120 μm. By setting the coating thickness within the above range, the thickness of the porous layer and the pore size on the back side of the porous layer can be controlled within preferred ranges.

[0095] For example, when the polymer solution contains PSf, the PSf concentration (i.e., the concentration of solid components) is preferably 17 to 24 by mass.

[0096] By setting the PSf concentration to the above range, a certain amount of good solvent can be included in step (c), resulting in the ability to control the specific surface area S or the tortuosity after high temperature and high pressure operation to a preferred range.

[0097] Regarding the temperature of the polymer solution during polymer solution coating, when using PSf as the polymer, coating is preferably performed in the range of 10–40°C. Within this range, coating can be carried out without PSf precipitation. It should be noted that the preferred temperature range of the polymer solution can be appropriately adjusted by factors such as the viscosity of the polymer solution used.

[0098] Regarding the thermoplastic polymer contained in the polymer solution, appropriate changes can be made by considering various characteristics such as the strength, permeability, and surface properties of the porous layer.

[0099] It should be noted that the solvent contained in the polymer solution only needs to be a good solvent for the polymer; it can be a single solvent or a mixture of multiple good solvents. The specific solvents can be adjusted appropriately, taking into account the strength characteristics of the porous layer being manufactured and the impregnation of the polymer solution into the substrate.

[0100] In step (b), a polymer solution disposed on a substrate is brought into contact with a first coagulation liquid whose main component is a non-solvent with low solubility of polymer compared to a good solvent in the polymer solution. By coagulating the polymer, a porous layer with a dense three-dimensional network structure can be formed.

[0101] The above contact can be carried out by immersing a substrate containing a polymer solution in a first coagulation solution.

[0102] The first coagulating liquid is a mixed solution of a polymeric non-solvent and a good solvent, with the non-solvent as the main component. Here, "main component" refers to a component that accounts for more than 50% by mass of the components constituting the first coagulating liquid. The concentration of the good solvent in the first coagulating liquid is preferably 10 to 40% by mass.

[0103] Furthermore, the contact time between the polymer solution and the first coagulating liquid is preferably 3 to 60 seconds, more preferably 3 to 30 seconds. If the contact time between the polymer solution and the first coagulating liquid is within the above range, the displacement between the good solvent in the polymer solution and the coagulating liquid can be controlled.

[0104] Furthermore, the temperature of the first coagulation solution is preferably between 10 and 45°C. If the temperature of the first coagulation solution is below 45°C, the vibration of the coagulation surface caused by thermal motion is not intense, and the surface smoothness of the porous layer is increased. In addition, if the temperature of the first coagulation solution is above 10°C, a sufficient coagulation rate can be obtained, resulting in good film formation properties. If the temperature of the coagulation solution is within the above range, the molecular weight cutoff of the porous layer can be controlled within the range of 10k to 60kDa, enabling the formation of a separation functional layer with excellent salt removal properties.

[0105] Examples of non-solvents used for the first coagulation liquid include water, hexane, pentane, benzene, toluene, methanol, ethanol, trichloroethylene, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butane glycol, pentane glycol, hexane glycol, low molecular weight polyethylene glycol, and other aliphatic hydrocarbons, aromatic hydrocarbons, aliphatic alcohols, or mixtures thereof.

[0106] In step (c), the second coagulated liquid is brought into contact with the inner layer of the porous layer while the porous support obtained from step (b) contains a good solvent. By dissolving the inner layer of the porous layer, a dense three-dimensional network structure is formed in the inner layer of the porous layer, which can control the specific surface area S or the tortuosity after specified operation.

[0107] In the manufacturing method of the composite semi-permeable membrane described in this embodiment, an important control factor is the amount of good solvent in the porous support. The amount of good solvent in the porous support during immersion in the second coagulation liquid is 10–60 g / m³. 2 Preferably 20-50 g / m 2 More preferably 30-40 g / m 2 If the amount of good solvent in the porous support is 10 g / m³ 2 The above indicates that the amount of good solvent is sufficient for dissolving polymers. On the other hand, if the amount of good solvent in the porous support is 60 g / m³... 2 The following measures can suppress structural changes in the surface of the porous layer. The amount of good solvent in the porous support when immersed in the second coagulation liquid can be controlled, for example, by the concentration of good solvent, temperature, and contact time between the polymer solution and the first coagulation liquid used in step (b).

[0108] The temperature of the second coagulating liquid used in step (c) is preferably 20 to 90°C, more preferably 50 to 85°C. If the temperature of the coagulating liquid is above 20°C, the inner layer of the porous layer can be fully dissolved, and the tortuosity can be controlled. If the temperature is below 90°C, the changes in the surface structure of the porous layer caused by thermal shrinkage can be suppressed.

[0109] The second coagulation solution used in step (c) only needs to contain a polymeric non-solvent, preferably a mixture of a polymeric non-solvent and a good solvent. The concentration of the good solvent in the second coagulation solution is preferably 0.1% to 10% by mass, more preferably 1% to 10% by mass. If the concentration of the good solvent in the second coagulation solution is 0.1% by mass or more, the inner layer of the porous layer can be sufficiently dissolved; if it is 10% by mass or less, changes in the surface structure of the porous layer can be suppressed.

[0110] Furthermore, since phase separation proceeds continuously, it is preferable to have a short time between step (b) and step (c). The interval from obtaining the porous support in step (b) to performing step (c) is preferably within 10 seconds, more preferably within 7 seconds, and even more preferably within 5 seconds.

[0111] Next, the porous support obtained in step (c) is preferably cleaned with hot water or the like to remove any solvent remaining in the porous support. The temperature of the hot water used for cleaning is preferably 50–100°C, more preferably 60–95°C. If the hot water temperature is below 100°C, the shrinkage of the porous support can be minimized. In addition, if the hot water temperature is above 50°C, a high cleaning effect can be obtained.

[0112] 2.2 Formation process of the separated functional layer Next, the method for forming the separated functional layer will be explained.

[0113] Regarding the separation functional layer, it can be obtained, for example, by chemically reacting a polyfunctional amine with a polyfunctional acyl halide to form a cross-linked polyamide, as described above. From the viewpoint of productivity and performance, interfacial polymerization is the most preferred method for the chemical reaction. That is, the separation functional layer is preferably formed by interfacial polycondensation on the surface of a porous layer using an aqueous solution containing a polyfunctional amine and an organic solvent solution containing a polyfunctional acyl halide. This process forms a cross-linked polyamide. Hereinafter, the process of forming a cross-linked aromatic polyamide by using a polyfunctional aromatic amine as the polyfunctional amine and a polyfunctional acyl chloride as the polyfunctional acyl halide will be specifically described, but the present invention is not limited thereto.

[0114] Interface aggregation includes the following steps (d) and (e).

[0115] Process (d): The process of contacting an aqueous solution containing a polyfunctional aromatic amine with a porous layer.

[0116] Step (e): A step following step (d) that brings the solution of the polyfunctional aromatic acyl chloride into contact with the porous layer.

[0117] In step (d), the concentration of the polyfunctional aromatic amine in the aqueous solution is preferably 0.1 to 20% by mass, and more preferably 0.5 to 15% by mass. If the concentration of the polyfunctional aromatic amine is within the above range, sufficient solute removal performance and water permeability can be obtained.

[0118] The contact between the polyfunctional aromatic amine aqueous solution and the porous layer is preferably carried out uniformly and continuously. Specifically, methods such as coating the porous layer with the polyfunctional aromatic amine aqueous solution or immersing the porous layer in the polyfunctional aromatic amine aqueous solution can be used. The contact time between the porous layer and the polyfunctional aromatic amine aqueous solution is preferably 1 second to 10 minutes, more preferably 10 seconds to 3 minutes.

[0119] After contacting the porous layer with the multifunctional aromatic amine aqueous solution, it is preferable to drain the solution so that no droplets remain on the surface of the porous support. Draining helps suppress the formation of defects in the separation functional layer. Draining methods include, for example, holding the porous support vertically after contacting the multifunctional aromatic amine aqueous solution to allow excess aqueous solution to flow down naturally, or forcibly draining the solution by blowing a stream of air such as nitrogen from an air nozzle. Alternatively, after draining, the membrane surface can be dried to remove some of the water from the aqueous solution.

[0120] The concentration of the polyfunctional aromatic acyl chloride in the above solution is preferably 0.01 to 10% by mass, more preferably 0.02 to 2.0% by mass. If the concentration of the polyfunctional aromatic acyl chloride in the solution is 0.01% by mass or more, a sufficient reaction rate can be obtained. In addition, if the concentration of the polyfunctional aromatic acyl chloride in the solution is 10% by mass or less, the occurrence of side reactions can be suppressed.

[0121] The solvent used in the solution for dissolving polyfunctional aromatic acyl chlorides is preferably an organic solvent that is immiscible with water, dissolves polyfunctional aromatic acyl chlorides, and does not damage the porous support. Any solvent that is inactive to polyfunctional aromatic amines and polyfunctional aromatic acyl chlorides is acceptable. Preferred examples of organic solvents include hydrocarbon compounds such as n-nonane, n-decane, n-undecane, n-dodecane, isooctane, isodecane, and isododecane, or mixtures thereof.

[0122] The method for contacting the organic solvent solution of the multifunctional aromatic acyl chloride with the porous layer that has been in contact with the aqueous solution of the multifunctional aromatic amine can be carried out in the same way as the method for coating the porous layer with the aqueous solution of the multifunctional aromatic amine.

[0123] After the interfacial polymerization reaction, the organic solvent is removed from the membrane surface. The organic solvent can be removed by methods such as: holding the porous support vertically to allow excess organic solvent to flow down naturally; drying the organic solvent by blowing it with a blower; removing excess organic solvent using a mixture of water and air, etc.

[0124] Alternatively, depending on the properties of the target composite semipermeable membrane, aliphatic amines or alicyclic polyfunctional amines can be used instead of polyfunctional aromatic amines, and aliphatic difunctional acyl halides or alicyclic difunctional acyl halides can be used instead of polyfunctional aromatic acyl chlorides, thereby forming cross-linked aliphatic polyamides or cross-linked alicyclic polyamides.

[0125] 3. Utilization methods of composite semi-permeable membranes The composite semi-permeable membrane described in this embodiment, along with a water supply path material such as a plastic mesh, a permeable water flow path material such as a tricot knitted fabric, and a membrane for improving pressure resistance as needed, is wound around a cylindrical water collection pipe with multiple holes, making it suitable as a spiral-type composite semi-permeable membrane element. Furthermore, it is also possible to manufacture a composite semi-permeable membrane assembly by connecting the element in series or in parallel and housing it in a pressure vessel.

[0126] Furthermore, the aforementioned composite semi-permeable membrane, its elements, and components can be combined with a pump that supplies water to them, a device for pre-treating the supplied water, etc., to form a fluid separation device. By using this fluid separation device, the supplied water can be separated into permeable water such as drinking water and concentrated water that has not permeated the membrane, thus obtaining water that meets the desired purpose.

[0127] Examples of liquid mixtures containing 500 mg / L to 100 g / L of TDS (Total Dissolved Solids) can be used as the supply water to be treated by the composite semi-permeable membrane described in this embodiment. These mixtures include seawater, brackish water, and wastewater. Generally, TDS is expressed as "mass / volume" or "mass ratio". By definition, it can be calculated from the mass of the residue after evaporating the solution filtered through a 0.45-micron filter at a temperature of 39.5 to 40.5°C, but it is simpler to calculate it from the practical salinity (S).

[0128] Higher operating pressures result in higher solute removal rates when the supply water passes through the composite semi-permeable membrane. However, considering the increased energy required for operation and the durability of the composite semi-permeable membrane, the preferred operating pressure is 0.5–12 MPa. Higher supply water temperatures decrease the solute removal rate, and lower supply water temperatures reduce membrane permeation flux. Therefore, the preferred supply water temperature is 5–55°C.

[0129] The water production rate change ratio calculated using the method described in "12. High Pressure Test" of the embodiments described later for the composite semi-permeable membrane involved in this embodiment is preferably 0.80 or more, more preferably 0.85 or more, even more preferably 0.90 or more, and particularly preferably 0.94 or more. Furthermore, the removal rate change ratio calculated by the above method is preferably 1.30 or less, more preferably 1.20 or less, and even more preferably 1.10 or less. Further, it is preferable that both the water production rate change ratio and the removal rate change ratio simultaneously satisfy the above ranges.

[0130] In typical composite semipermeable membranes, during operation at temperatures above 35°C with TSDs above 40,000 mg / L accompanied by start-up and shutdown, the water production rate decreases significantly due to the compaction of the porous layer. Therefore, in order to maintain a constant water production rate for the fluid separation device, the operating pressure needs to be increased, and the energy required for operation needs to be increased.

[0131] In the water production method using the composite semi-permeable membrane according to this embodiment, even during operation at temperatures above 35°C and with a TSD of 40,000 mg / L or higher accompanied by start-up and shutdown, compaction of the porous layer does not proceed. Therefore, the decrease in water production capacity of the composite semi-permeable membrane is suppressed, the increase in operating pressure required to maintain a constant water production capacity of the fluid separation device is reduced, and the increase in energy required for operation is reduced.

[0132] Furthermore, if the pH of the supply water becomes high, scale such as magnesium may form in the case of supply water with high solute concentrations, such as seawater. There are also concerns about membrane degradation due to filtering supply water with a high pH. Therefore, the pH of the supply water is preferably neutral.

[0133] Example The present invention will be described in more detail below through examples. However, the present invention is not limited thereto. It should be noted that, unless otherwise specified, the porous support provided for each test was obtained by immersing the composite semi-permeable membrane in a 2% (w / w) sodium hypochlorite aqueous solution for 48 hours and removing the separation functional layer.

[0134] 1. Permeability coefficient k of porous layers The composite semi-permeable membrane was subjected to 5.5 MPa and 25°C with a 3.5% (w / w) NaCl aqueous solution at pH 6.5 for 2 hours. After 5.5 MPa operation, the composite semi-permeable membrane was immersed in a 2% (w / w) sodium hypochlorite aqueous solution for 48 hours to remove the separation functional layer, yielding a porous support. The porous support was cut into 4.3 cm diameter circles and installed in a stirred ultrafiltration cup (Advantec Toyo Kaisha, Ltd. UHP-43K) (effective filtration area: 10.9 cm²). 2 Add 25°C pure water to the sample cell of the ultrafiltration cup and install the lid. Pressurize to 0.2 MPa with nitrogen and measure the pure water permeation rate Q[m] over a certain period of time. 3 / s]. The thickness L [m] and membrane area A [m²] of the porous layer under 25℃ and pressure P [Pa] are determined. 2 The pure water permeability Q[m] 3 The permeability k of the porous layer after operation at 5.5 MPa is calculated using the following formula (2): [ρ[Pa·s], pure water viscosity μ[Pa·s], and pure water viscosity μ[Pa·s]. It should be noted that the significant figures are set to 2 digits.

[0135] k[m 2 =Q×μ×L / (A×P) ……Equation (2) Here, a porous support is used in the measurement, but the water permeability resistance of the substrate in the porous support is so small as to be negligible compared with that of the porous layer. Therefore, the permeability coefficient k obtained from the above equation (2) is regarded as the permeability coefficient of the porous layer.

[0136] 2. Mass per unit area of ​​the porous layer The porous support was cut into rectangles of 0.11m × 0.19m and dried at 120°C for 2 hours. The mass of the porous support was then measured. Additionally, the porous layer was peeled off from the porous support using adhesive tape, and the mass of the substrate was measured. The mass per unit area of ​​the porous layer was calculated using the following formula (3).

[0137] Mass per unit area of ​​porous layer [g / m] 2 = (mass of porous support - mass of substrate) / (0.11 × 0.19) ... Equation (3) 3. Thickness of the porous layer and the substrate The thickness of the porous layer (thickness of the porous layer after high-temperature and high-pressure operation) after supplying a 3.5% by mass NaCl aqueous solution with a pH of 6.5 to the composite semipermeable membrane at 7.0 MPa and 45°C for 24 hours was measured using a pointer-type thickness gauge (TECLOCK Corporation, constant-pressure thickness measuring instrument PG-01A) on the composite semipermeable membrane after operation under these conditions. First, since the separation functional layer is very thin, the combined thickness of the substrate and the porous layer was considered the thickness of the composite semipermeable membrane, and this thickness was measured. Then, the substrate was peeled off from the composite semipermeable membrane with tape, and the thickness of the peeled substrate was measured using the aforementioned pointer-type thickness gauge PG-01A. The difference between the thickness of the composite semipermeable membrane and the thickness of the substrate was taken as the thickness of the porous layer. It should be noted that for each thickness measurement, the arithmetic mean of 20 measurements randomly selected on the same membrane surface was used. Furthermore, the thickness of the substrate of the composite semipermeable membrane was measured using the same method using the composite semipermeable membrane before operation under the aforementioned conditions.

[0138] 4. Porosity ε of porous layers For the porous support obtained using the method described in "1. Permeability coefficient k of the porous layer" after operation at 5.5 MPa, the porosity is calculated using the following equations (4), (5), and (6). It should be noted that the polymer density [g / m³] is... 3 [ ] is the density of the thermoplastic polymer that forms the porous layer. When the porous layer is a mixture of multiple thermoplastic polymers, the mixed density is used.

[0139] Polymer volume [m 3 = Mass per unit area of ​​porous layer × (0.11 × 0.19) / polymer density ... Equation (4) Apparent volume of porous layers [m 3 = Thickness of porous layer × (0.11 × 0.19) …… Equation (5) The porosity ε[-] of the porous layer is equal to 1 - (polymer volume / apparent volume of the porous layer) ... Equation (6) 5. Pore volume V of porous layers The pore volume V of the porous layer after operation at 5.5 MPa is calculated by the following formula (7) based on the relationship between pore volume: (1 / polymer density) = porosity: (1-porosity).

[0140] The pore volume V[cm] of the porous layer 3 / g]=porosity×(1-porosity) / polymer density……Equation (7) 6. Specific surface area S and tortuosity of porous layers The specific surface area S of the porous layer was determined by nitrogen adsorption measurement from the porous support. In addition, the tortuosity after 5.5 MPa operation was calculated using the above formula (1) from the porosity ε, permeability k, pore volume V and specific surface area S of the porous layer after 5.5 MPa operation.

[0141] The porous layer was peeled off from the porous support, and only the peeled porous layer was cut into 5 mm squares using a single-edged cutter to obtain 0.1–0.3 g of test samples. The test samples were dried under vacuum at 45 °C for 4 hours. The specific surface area S of the dried samples was determined by the BET method using a nitrogen adsorption assay apparatus (MicrotracBEL; BELSORP-miniII). A leak check was performed before the measurement, and the measurement was started under the following conditions after confirming that the leakage was less than 5 Pa / min.

[0142] [Adsorbate setting] The adsorbate was set to N2 gas, and the adsorption temperature was set to 77K.

[0143] [Heat Escape Setting] The molecular diameter was set to 0.364 mm, the inner diameter of the sample tube was set to 7.0 mm, and the outer diameter of the glass rod was set to 6.0 mm.

[0144] [Measuring device settings] I chose the "Dewar bottle".

[0145] [Saturated vapor pressure setting] "Actual measurement" was selected.

[0146] [Correction for non-ideal adsorbed gas] The second virial coefficient is set to -4.264 × 10⁻⁶. -7 Pa -1 .

[0147] [Blow-off Settings] Set the sample tube disposal rate to "slow" and the purge gas to Ads (V2).

[0148] [n adsorption cycles setting] The degassing time was set to 120 minutes, and three isotherms were selected.

[0149] [Adsorbate introduction pressure setting] "Display relative pressure" was selected.

[0150] [Measurement Method] The simplified method was selected, and the upper limit of the adsorption relative pressure was set to 0.35, desorption was measured, and the relative pressure of the measured value was specified.

[0151] 7. Molecular weight cutoff of porous layers Aldrich's dextran Mw1500 (product number: 31394), Mw6000 (product number: 31388), Mw15000-20000 (product number: 31387), Mw-40000 (product number: 31389), Mw-60000 (product number: 31397), and Mw-200000 (product number: 31398) were dissolved in distilled water at a concentration of 500 ppm to prepare dextran aqueous solutions, which were used as the raw water.

[0152] The porous support was cut into a circle with a diameter of 4.3 cm, and the cut sample was installed in a stirred ultrafiltration cup (Advantec Toyo Kaisha, Ltd. UHP-43K) (effective filtration area: 10.9 cm²). 2 Add a 25°C dextran solution to the sample cell of the ultrafiltration cup and attach the lid. While stirring at 1000 rpm, increase the pressure until the water production rate reaches 0.2–0.8 [m³]. 3 / m 2 The pressure was set to [per day] to begin filtration. The first 5g of the permeate was discarded as pre-permeate, and the next 5g was collected as the filtration sample. The dextran concentration in the raw water and the filtration sample was determined by GPC.

[0153] The concentration determination using GPC was performed as follows: The sampled solution was filtered through a 0.45-micron pore size filter. The resulting filtrate was analyzed using a GPC column (Tosoh Corporation; TSK-gel-G4000PWXL), at a column temperature of 40°C, with distilled water for liquid chromatography at a flow rate of 1 mL / min as the mobile phase and a sample injection volume of 100 μl. The determination was performed using a differential refractive index system (Tosoh Corporation; RI-8020) with a slice time of 0.02 min and a baseline range of 4.5–11.0 min.

[0154] The calibration curve showing the relationship between retention time and molecular weight of dextran in GPC was calculated as follows. A solution of monodisperse dextran was analyzed using GPC, and the retention times were measured. The retention times at each peak were plotted against the measured molecular weight of the monodisperse dextran, and the calibration curve was derived from the exponential approximation curve. Furthermore, the retention time at which 90% dextran removal was achieved was calculated from the difference in refractive index between the raw water and the filtered sample, and the molecular weight cutoff for 90% dextran removal was determined from the calibration curve.

[0155] 8. The uneven shape of the back surface of the porous layer and the average equivalent circle diameter of the pores. The uneven shape of the back surface of the porous layer and the average equivalent circular diameter of the pores present in the recesses were determined by surface observation based on SEM and image analysis using ImageJ software. First, the composite semi-permeable membrane was air-dried at room temperature, and the substrate was peeled off from the porous layer at a peeling speed of 50 mm / min along a 180-degree direction. A thin layer of platinum was applied to the back surface of the exposed porous layer, and images were observed and captured using a SEM (Hitachi High-Tech S-5500) at an accelerating voltage of 5 kV and magnification of 500x. In the obtained images, as shown... Figure 3 As shown, the image contrast confirmed the presence of a convex portion 14 (white portion) on the back side of the porous layer and a concave portion 15 (gray portion) on the back side of the surrounding porous layer. For the concave portion (gray portion), further observation and image capture were performed at 10,000x magnification. In the obtained images, a 25 μm... 2 The pores within a 5μm × 5μm area were binarized using the mean method in the analysis software (Image-J). After extracting the pore contours using the Find Edge function, the equivalent circle diameter was calculated. The same operation was performed on 5 samples, and the arithmetic mean of the equivalent circle diameters of all pores in the 5 samples was calculated as the average equivalent circle diameter of the pores in the concave area on the back side of the porous layer.

[0156] 9. Tensile strength of the substrate Based on JIS L 1906:2000 5.3.1, a 5cm×30cm substrate obtained by peeling off the composite semipermeable membrane was used as a sample. Under the conditions of clamping interval of 20cm and tensile speed of 10cm / min, five measurements were performed along the longitudinal direction. The value obtained from the obtained strength-elongation curve and rounded to the first decimal place was taken as the longitudinal tensile strength of the substrate.

[0157] 10. Amount of good solvent in porous supports In the fabrication of the composite semi-permeable membrane, a porous support with a porous layer formed on the substrate, obtained by impregnation in the first coagulation solution of step (b), is cut into a rectangle of 0.11m × 0.19m while still wet, along with the substrate. This rectangle is then immersed in a polytetrafluoroethylene container containing 500g of pure water at 90°C for 1 hour. After immersion, 10mL of the extract containing the porous support is collected. The collected extract is analyzed by GC-MS. The concentration of the good solvent in the extract [ppm] is calculated based on a pre-prepared standard curve of peak area versus good solvent concentration of the polymer solution. The amount of good solvent in the porous support is then determined using the following formula (8) from the calculated concentration of the good solvent in the extract.

[0158] Good solvent content in porous supports [g / m] 2= 500 × (concentration of good solvent in solution / 1000) / 1000 / (0.11 × 0.19) …… Equation (8) 11. NaCl removal rate and water production capacity of composite semi-permeable membrane For a composite semi-permeable membrane, raw water (NaCl concentration 3.2% by mass) adjusted to 25°C and pH 6.5 was supplied at an operating pressure of 5.5 MPa and subjected to 24 hours of membrane filtration. Then, the conductivity of the supply water and the permeate water was measured using a multi-parameter water quality meter (MM60R) manufactured by Toa DKK Corporation. Next, the NaCl concentration was calculated by converting the conductivity using a pre-prepared standard curve. From the obtained NaCl concentration, the initial salt removal performance, i.e., the initial NaCl removal rate, was calculated using the following formula (9).

[0159] NaCl removal rate [%] = 100 × {1 - (NaCl concentration in permeate water / NaCl concentration in supply water)} …… Equation (9) In addition, after the above 24-hour membrane filtration treatment, the membrane permeate water volume was measured for 30 minutes, and the initial water production volume was calculated, converted to permeate water volume (cubic meters) per square meter of membrane surface per day. 3 / m 2 / sky].

[0160] 12. High-pressure test For the composite semi-permeable membrane whose performance was evaluated through the above-mentioned "11. NaCl removal rate and water production of composite semi-permeable membrane", raw water (NaCl concentration 3.2% by mass) adjusted to 45℃ and pH 6.5 was supplied at an operating pressure of 7.0 MPa. The membrane filtration process was repeated every hour, with shutdown and operation, for a total of 24 hours. Then, the membrane performance was evaluated using the same method as in "11. NaCl removal rate and water production of composite semi-permeable membrane", and the NaCl removal rate and water production after high temperature and high pressure operation were calculated. In addition, the quality of membrane performance was judged by the water production change ratio and removal rate change ratio calculated by the following formulas (10) and (11).

[0161] Water production change ratio = Water production after high-pressure operation / Initial water production ... Equation (10) Removal rate change ratio = (100 - NaCl removal rate after high-pressure operation) / (100 - initial NaCl removal rate) ... Equation (11) [Example 1] On a long-fiber polyester nonwoven fabric (average thickness 90 μm, longitudinal tensile strength 420 N / 5 cm) as the substrate, the mass per unit area of ​​the porous layer in the composite semi-permeable membrane is 20 g / m² under conditions of 25 °C. 2A DMF solution with a PSf of 20% by mass was coated onto the substrate as a polymer solution. The substrate coated with the polymer solution was then immersed in a first coagulation solution formed from the DMF aqueous solution at 20°C for 15 seconds to create a porous support with a porous layer on the substrate. Next, the porous support was immersed in a second coagulation solution formed from the DMF aqueous solution and left for 5 minutes, followed by washing with hot water at 90°C for 2 minutes. The washed porous support was then immersed in a 3% by mass aqueous solution of m-PDA for 2 minutes. The support was slowly lifted vertically, and excess aqueous solution was removed from the surface of the porous support by blowing nitrogen gas through an air nozzle. Then, a decane solution containing 0.165% by mass of TMC was coated onto the surface to completely wet the membrane, and the membrane was allowed to stand for 1 minute. The membrane was then further vertically drained to remove excess solution, and washed with pure water to obtain a composite semi-permeable membrane with a cross-linked polyamide separation functional layer.

[0162] [Reference Example 1] The composite semipermeable membrane obtained in Example 1 was subjected to an aqueous solution of 7.0 MPa, 45°C, 3.5% NaCl concentration, and pH 6.5 for 24 hours, followed by immersion in a 2% sodium hypochlorite aqueous solution for 48 hours to remove the separation functional layer, thereby obtaining a porous support.

[0163] [Example 2] The substrate coated with the polymer solution was immersed in a first coagulation solution at 40°C for 15 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 1.

[0164] [Example 3] Using a DMF solution with a PSf of 18% by mass as the polymer solution, the substrate coated with the polymer solution was immersed in a first coagulation solution at 20°C for 25 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 1.

[0165] [Example 4] The mass of the porous layer per unit area in the composite semipermeable membrane is defined as 18 g / m³. 2 The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 25°C for 25 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 3.

[0166] [Example 5] A DMF solution with a PSf of 21% by mass was used as the polymer solution, and the mass per unit area of ​​the porous layer in the composite semipermeable membrane was defined as 10 g / m³. 2The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 30°C for 15 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 1.

[0167] [Example 6] The mass of the porous layer per unit area in the composite semipermeable membrane is defined as 12 g / m. 2 The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 30°C for 12 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 1.

[0168] [Example 7] The mass of the porous layer per unit area in the composite semipermeable membrane is defined as 14 g / m. 2 The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 25°C for 15 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 3.

[0169] [Example 8] The mass per unit area of ​​the porous layer in the composite semipermeable membrane is defined as 11 g / m. 2 The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 25°C for 15 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 3.

[0170] [Example 9] Using long-fiber polyester nonwoven fabric (average thickness 95 μm, longitudinal tensile strength 350 N / 5 cm) as the substrate, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained by the same method as in Example 1.

[0171] [Comparative Example 1] A DMF solution with a PSf of 15.7% by mass was used as the polymer solution, and the mass per unit area of ​​the porous layer in the composite semipermeable membrane was calculated to be 25 g / m³. 2 The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 30°C for 5 minutes. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained in the same manner as in Example 1.

[0172] [Comparative Example 2] The mass of the porous layer per unit area in the composite semipermeable membrane is 23 g / m. 2The substrate coated with the polymer solution was immersed in a first coagulated solution formed from the DMF aqueous solution at 25°C for 20 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained in the same manner as in Comparative Example 1.

[0173] [Comparative Example 3] On the same substrate as in Example 1, at 25°C, the mass per unit area of ​​the porous layer in the composite semi-permeable membrane was 20 g / m². 2 A DMF solution with a PSf of 18% by mass was coated onto the substrate as a polymer solution. Then, the substrate coated with the polymer solution was immersed in pure water for less than 1.0 second, followed by pressing pure water at a pressure of 1 kPa for approximately 3 seconds from the substrate side, and then left in pure water for 5 minutes to create a porous support. The obtained porous support was then cross-linked with polyamide using the same method as in Example 1 to obtain a composite semi-permeable membrane with a cross-linked polyamide separation functional layer.

[0174] [Comparative Example 4] A solution with a PSf of 18% by mass was used as the polymer solution, obtained by mixing DMF and DMSO in a 90:10 ratio. The mass of the porous layer per unit area in the composite semipermeable membrane was 25 g / m. 2 The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 25°C for 5 minutes. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained in the same manner as in Example 1.

[0175] [Comparative Example 5] A DMF solution with a PSf of 18.3% by mass was used as the polymer solution, and the mass per unit area of ​​the porous layer in the composite semipermeable membrane was calculated to be 12 g / m³. 2 The substrate coated with the polymer solution was immersed in a first coagulated solution formed from the DMF aqueous solution at 25°C for 2 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained in the same manner as in Example 1.

[0176] [Comparative Example 6] A DMF solution with a PSf of 28% by mass was used as the polymer solution, and the mass per unit area of ​​the porous layer in the composite semipermeable membrane was calculated to be 15 g / m³. 2 The substrate coated with the polymer solution was immersed in a first coagulation solution formed from the DMF aqueous solution at 5°C for 15 seconds. Otherwise, a composite semipermeable membrane with a cross-linked polyamide separation functional layer was obtained in the same manner as in Example 1.

[0177] The structure of the porous layer of the composite semipermeable membrane obtained in the examples and comparative examples, the characteristics of the substrate, and the measurement results of the membrane performance are shown in Tables 1 to 3.

[0178] [Table 1] [Table 2] [Table 3] As can be clearly seen from the results shown in Tables 1, 2 and 3, the composite semi-permeable membranes of Examples 1 to 9 involved in this embodiment have sufficient water production and salt removal properties, and can suppress the reduction of water production even after high-pressure operation.

[0179] Although the invention has been described in detail with reference to specific methods, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention.

[0180] This application is based on Japanese Patent Application No. 2024-068770, filed on April 22, 2024, the entirety of which is incorporated herein by reference.

[0181] Industrial availability The composite semi-permeable membrane of this invention can be used for seawater desalination, brackish water desalination, drinking water production, industrial ultrapure water production, wastewater treatment, and recovery of valuable substances.

[0182] Explanation of reference numerals in the attached figures 1. Composite semi-permeable membrane 2. Substrate 3 Porous layers 4. Separate functional layers 5 Separation Membrane Elements 6 end plates 7 end plates 8. Supply-side flow path materials 9. Through side flow path material 10 water collection pipes 11. Water supply 12 Through water 13 Concentrated Water 14 The convex portion on the back side of the porous layer 15 Recessed portion on the back side of the porous layer

Claims

1. A composite semi-permeable membrane, comprising a substrate, a porous layer disposed on the substrate, and a separation functional layer disposed on the porous layer. The porous layer has a molecular weight cutoff of 10k to 60kDa and a specific surface area of ​​20 to 50m². 2 / g.

2. A composite semi-permeable membrane, comprising a substrate, a porous layer disposed on the substrate, and a separation functional layer disposed on the porous layer. The porous layer has a molecular weight cutoff of 10k to 60kDa, and its tortuosity is 1.5 to 7.0 after being supplied with an aqueous solution of NaCl concentration of 3.5% by mass and pH 6.5 for 2 hours under conditions of 5.5MPa and 25℃.

3. The composite semi-permeable membrane as described in claim 1 or 2, wherein, The surface of the porous layer opposite to the surface where the separation functional layer is located has an uneven shape, and the average equivalent circle diameter of the pores in the concave portion is 0.30 to 0.60 μm.

4. The composite semi-permeable membrane as described in claim 1 or 2, wherein, The mass of the porous layer per unit area is 10–17 g / m³. 2 .

5. The composite semi-permeable membrane as described in claim 1 or 2, wherein, The specific surface area of ​​the porous layer is 22–40 m². 2 / g.

6. The composite semi-permeable membrane as described in claim 1 or 2, wherein, The molecular weight cutoff of the porous layer is 30k to 45kDa.

7. The composite semi-permeable membrane as described in claim 1 or 2, wherein, After supplying the composite semipermeable membrane with an aqueous solution of NaCl concentration of 3.5% by mass and pH 6.5 for 24 hours at 7.0 MPa and 45 °C, the thickness of the porous layer is 10–20 μm.

8. The composite semi-permeable membrane as described in claim 1 or 2, wherein, The substrate is a long-fiber nonwoven fabric with a thickness of 80-100 μm, and the longitudinal tensile strength of the long-fiber nonwoven fabric is 400-900 N / 5 cm.

9. A separation membrane element comprising the composite semipermeable membrane as described in claim 1 or 2.

10. A fluid separation apparatus comprising the separation membrane element as described in claim 9.

11. A method for manufacturing a composite semipermeable membrane, comprising the following steps (a) to (c): Process (a): The process of preparing a polymer solution obtained by dissolving a thermoplastic polymer in a good solvent onto a substrate; Step (b): The polymer solution disposed on the substrate is contacted with a first coagulation liquid containing the thermoplastic polymer and a non-solvent and a good solvent to form a porous layer on the substrate, thereby obtaining a porous support formed from the substrate and the porous layer with a good solvent content of 10 to 60 g / m³. 2 The process of constructing porous supports; Step (c): The step of immersing the porous support in the second solidification liquid.

Citation Information

Patent Citations

  • Reverse osmosis composite membrane

    JP2001252538A

  • Composite semipermeable membrane and production method of the same

    JP2018039003A

  • Paper sheet conveyance device

    JP2024068770A

  • Composite semipermeable membrane and method for producing composite semipermeable membrane