Static mixer, and coating apparatus and coating method using the same
By performing a hydrophilic surface treatment on the housing and components of the static mixer, the problem of gel formation during the mixing process of two-component curable resin compositions was solved, and stable coating of highly reactive resins was achieved.
Patent Information
- Application Number
- CN202580029196.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-09
- Filing Date
- 2025-04-24
- Publication Date
- 2026-11-20
AI Technical Summary
Two-component curable resin compositions are prone to gelation after mixing or contact, which leads to the formation and discharge of gels in the mixing device, affecting coating quality and the maintenance of flange clearance.
A static mixer employing a hydrophilic surface treatment suppresses the discharge of gelled materials by chemically reacting fluorine gas with oxygen on the housing and components.
Even highly reactive two-component curable resin compositions can effectively suppress the generation and expulsion of gels, ensuring coating quality and stability of flange gaps.
Smart Images

Figure CN123146431A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a static mixer, coating apparatus and coating method suitable for coating two-component curable resin compositions. Background Technology
[0002] Previously, inventions such as Patent Document 1, which involve mixing a two-component curable resin composition and then coating its beads onto a flange, were known. However, the two-component curable resin composition begins to react after mixing or contact, thus generating gels within the mixing apparatus, which becomes a problem. Here, gels refer to insoluble cured substances that are locally generated in the composition. Although there is no precise definition, in terms of size, they refer to amorphous lumps with a major axis of about 1 mm to 2 mm. Cured products of the two-component curable resin composition are usually formed after coating from the coating apparatus, but cured products generated in the flow path before coating from the coating apparatus are equivalent to gels. This trend is particularly pronounced in highly reactive two-component curable resin compositions. Furthermore, if the gels generated within the mixing apparatus for mixing the two components are discharged along with the mixture and remain on the flange surface, the gels become contaminants when the flange surfaces are brought together, making it impossible to maintain a constant gap, which becomes a problem.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 3-50287 Summary of the Invention
[0006] The problem that the invention aims to solve
[0007] Previously, if the reactivity of a two-component curable resin composition was reduced, curing would take longer, thus requiring a highly reactive two-component curable resin composition. However, if the reactivity was high, it would be difficult to suppress the discharge of gels generated during mixing.
[0008] Methods for solving problems
[0009] In order to achieve the above-mentioned objectives, the inventors conducted in-depth research and discovered a method for inhibiting the excretion of gelled substances, thereby completing the present invention.
[0010] The main idea of the present invention will now be described. The first embodiment of the present invention is a static mixer, which consists of a housing and components, and has an outlet and an inlet at the end of the housing, wherein the housing and components are subjected to a hydrophilic surface treatment.
[0011] The second embodiment of the present invention is a static mixer according to the first embodiment, wherein the aforementioned elements and housing are formed of polypropylene.
[0012] The third embodiment of the present invention is a static mixer according to the first embodiment, wherein the above-mentioned hydrophilic surface treatment is a surface treatment performed by a chemical reaction between fluorine gas and oxygen.
[0013] The fourth embodiment of the present invention is a static mixer according to the first embodiment, which is installed in a discharge device for a two-component curable resin composition.
[0014] The fifth embodiment of the present invention is a static mixer according to the fourth embodiment, wherein the two-component curable resin composition comprises a silicone resin.
[0015] The sixth embodiment of the present invention is a method for coating a mixture of two-component curable resin compositions, wherein the two-component curable resin composition is supplied from a discharge device to an inlet of a static mixer, and the mixture is coated from an outlet of the static mixer, wherein the static mixer has a hydrophilic surface treatment on its housing and components, and the housing has an outlet and an inlet at its end.
[0016] The seventh embodiment of the present invention is a coating apparatus in which the two-component curable resin composition is supplied from the discharge device to the injection port of a static mixer in a discharge device, and the mixture is coated from the discharge port of the static mixer. The static mixer has a hydrophilic surface treatment on its housing and components, and the housing has an discharge port and an injection port at its end.
[0017] Invention Effects
[0018] If the reactivity of a two-component curable resin composition is reduced, curing will take longer. Therefore, a two-component curable resin composition with high reactivity is required. However, in this invention, even with high reactivity, the discharge of gels generated during mixing can be suppressed. Attached Figure Description
[0019] Figure 1 This is an overall diagram of the static mixer.
[0020] Figure 2 It is the process flow of coating mixtures, and one method of coating. Detailed Implementation
[0021] This invention relates to a coating apparatus in which a two-component curable resin composition is supplied from the discharge device to the inlet of a static mixer, and the mixture is coated from the outlet of the static mixer. The static mixer has a hydrophilic surface treatment on its housing and components, and the housing has an outlet (nozzle) and an inlet at its end. Furthermore, this invention relates to a static mixer used for coating, wherein the static mixer has a hydrophilic surface treatment on its housing and components, and the housing has an outlet and an inlet at its end. Hereinafter, the composition obtained by mixing the two components will be referred to as a mixture.
[0022] Next, the details of the present invention will be described. Any static mixer that can be used in the present invention can be used as long as it has the function of mixing the two components of a two-component curable resin composition. The basic structure is as follows: Figure 1 The device comprises a housing 1 and components 2. The housing 1 has an inlet 4, a length of 70mm to 300mm, and an inner diameter of 4.0mm to 15.0mm. The inner diameter of the outlet (nozzle) 3 is preferably 2.0mm to 5.0mm. The mixing ratio can be changed by altering the segmentation of components 2. Considering mixing efficiency, the number of segments in components 2 is preferably 15 to 20. Considering formability and the hydrophilic surface treatment described later, the materials of the housing and components are preferably PP (polypropylene resin), PE (polyethylene resin), PET (polyethylene terephthalate resin), metal, etc. Specific examples of static mixers include the MA series, MC / MCX series, and SM series manufactured by MIXPAC, but the device is not limited to these.
[0023] The hydrophilic surface treatments that can be used in this invention vary in effect depending on the material of the substrate, but can be used as long as the surface of PP or similar materials can be hydrophilicated. Surface treatments performed by the chemical reaction of fluorine gas with oxygen and / or sulfur dioxide are particularly preferred. More specifically, fluorine hydrophilic treatments are an example. In the presence of oxygen, treatments in which carboxyl groups remain on the substrate surface are preferred, and in the presence of sulfur dioxide, treatments in which sulfone groups remain on the substrate surface are preferred.
[0024] By applying a hydrophilic surface treatment to the housing and components of the aforementioned static mixer, gelation is prevented from being discharged along with the mixture obtained from mixing the two-component curable resin composition, as described later. The hydrophilic surface treatment is mostly performed in batches, allowing for the treatment of the entire housing and components; however, for the housing, treatment of at least the inner wall is sufficient. In the case of highly reactive two-component curable resin compositions, the reaction undoubtedly proceeds rapidly, resulting in gelation. However, it is conceivable that even if gelation occurs, it will adhere to the components, preventing its discharge with the mixture. However, since the two-component curable resin composition is mixed within the static mixer, the formation of gelation cannot be suppressed, necessitating replacement of the static mixer after a specific period.
[0025] The two-component curable resin composition that can be used in this invention refers to the curable resin composition described below, which consists of two formulations, namely Agent A (also called the main agent) and Agent B (also called the curing agent), which initiate polymerization, condensation, and other reactions through mixing or contact. Because the reaction is initiated by mixing or contacting in an atmosphere of 5°C to 35°C, its properties differ from those of single-component curable resin compositions that are cured by heat or light, and ultimately the reaction is completed solely through mixing or contact to form a cured product.
[0026] Examples of two-component curable compositions include compositions in which a compound having hydrolyzable silyl and / or silanol groups is separated from a moisture-curing catalyst in two formulations; compositions in which a compound having (meth)acryloyl groups, an organic peroxide, and a metal catalyst are separated from multiple formulations; compositions in which a compound having cyclic ether groups is separated from a curing agent and / or a curing accelerator in multiple formulations; compositions in which a compound having allyl or vinylsiloxane groups, a crosslinking agent, and a catalyst are separated from multiple formulations; and combinations thereof, but are not limited to these. As the main skeleton of each compound, various skeletons can be used, such as polyurethane skeletons; polyether skeletons; polyester skeletons; polycarbonate skeletons; polyurethane-modified skeletons; polyepoxy-modified skeletons; polyurea skeletons; polyorganosiloxane skeletons; polybutadiene skeletons, polyisoprene skeletons, polyisobutylene skeletons, and other polyolefin skeletons; poly(meth)acrylate skeletons and their hydrogenated skeletons, but are not limited to these. The present invention preferably comprises a two-component curable resin composition with a polyorganosiloxane backbone as the main skeleton, which is a composition in which a compound having hydrolyzable silyl groups and / or silanols is separated from a moisture-curing catalyst in two formulations. A further preferred main skeleton is a polydimethylsiloxane backbone (silicone).
[0027] As the aforementioned moisture-curing catalysts, metal catalysts exhibiting moisture-curing properties, such as tin, titanium, zirconium, zinc, and aluminum, can be used. Specifically, examples include triphenylaluminum, trioctylaluminum, tetrabutyl titanate, tetraisopropyl titanate, dibutyltin dilaurate, zinc naphthenate, zinc octanoate, zinc octenate, and zirconium naphthenate.
[0028] The reaction forms of the aforementioned hydrolyzable silyl groups include deacetic acid type, deoxime type, dealcohol type, and deacetone type, but are not limited to these.
[0029] Fillers may be added to the above-mentioned two-component curable resin composition. Specifically, examples include glass powder, silica powder, alumina powder, talc powder, mica powder, silicone rubber powder, calcium carbonate powder, aluminum nitride powder, etc., but are not limited to these.
[0030] The aforementioned two-component curable resin composition may contain compounds with hydrolyzable silane groups. Specifically, examples include silicate compounds such as methyl silicate, ethyl silicate, propyl silicate, and butyl silicate; alkyl silane coupling agents such as dimethyldimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, and hexyltrimethoxysilane; vinyl silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane; phenyl silane coupling agents such as phenyltrimethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane. Silane coupling agents containing amino groups, such as N-2-(aminoethyl)-3-aminopropylmethyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; silane coupling agents containing glycidyl groups, such as 3-epoxypropoxypropylmethyldimethoxysilane, 3-epoxypropoxypropyltrimethoxysilane, and 3-epoxypropoxysilyltriethoxysilane; and silane coupling agents containing (meth)acryloyl groups, such as 3-(meth)acryloyloxypropylmethyldimethoxysilane, 3-(meth)acryloyloxypropylmethyldiethoxysilane, and 3-(meth)acryloyloxypropyltriethoxysilane, but not limited to these.
[0031] Examples of agent A in the above-mentioned two-component curable resin composition include compositions comprising a compound having a hydrolyzable silane, a moisture-curing catalyst, and a filler. Examples of agent B in the above-mentioned two-component curable resin composition include compositions comprising a compound having a silanol, a coupling agent, and a filler, but are not limited to these. Furthermore, agent A and agent B are preferably mixed in a ratio of 1:2 to 2:1.
[0032] The discharge device usable in this invention refers to a discharge device having a supply port directly connected to a static mixer. More specifically, the discharge device includes containers for agent A and agent B of a two-component curable resin composition, each container being equipped with a valve and designed to pressurize the contents of each container. The curable resin composition can be fed into the injection port of the static mixer while adjusting the internal pressure of each container, and applied from the discharge port (nozzle) of the static mixer.
[0033] In addition, the aforementioned discharge device is fixed to the robotic arm. The discharge device itself moves or the object being coated moves while the discharge device is fixed, thereby enabling the bead coating of a specific coating pattern.
[0034] Examples of containers include pressure cans, cylinders, syringes, and dispensers. By attaching a pressure gauge to the container, the pressure can be monitored. Furthermore, methods of pressurization include adjusting the internal pressure by introducing a gas such as compressed air into the container, or adjusting the pressure using the movement distance of a piston based on a ball screw. Methods of directly pressurizing the composition or pressurizing via a plunger can be used, but these are not limited to these. To quantitatively discharge a specific volume, methods utilizing the movement distance of a piston based on a ball screw are preferred.
[0035] Examples of valves mentioned above include needle valves, diaphragm valves, and spool valves, but they are not limited to these. Discharge of agent A, agent B, and mixtures can be achieved simply by opening the valve (discharge begins) and closing the valve (discharge stops).
[0036] As a discharge device, a two-component discharge type discharge device, such as MH-2B-ST-KM manufactured by ThreeBond Co., Ltd. can be used, but it is not limited to these.
[0037] The coating method of this invention is a method for coating a mixture of two-component curable resin compositions. It involves supplying the two-component curable resin composition from a discharge device to the inlet of a static mixer and coating the mixture from the outlet of the static mixer. The static mixer has a hydrophilic surface treatment on its housing and components, and the housing has an outlet and an inlet at its end. The steps are performed through steps 1 to 5 described below, and other steps may be added between steps. More specifically, according to... Figure 2 The coating process is carried out.
[0038] [Pressure Measurement Process]
[0039] The internal pressure is read after a specific time elapsed since step 3 (described later). This specific time is defined as 1 to 10 seconds, shorter than the settling time in step 5 (described later). The initial pressures of agent A and agent B can be the same or different. Hereinafter, the pressure measurement process will be referred to as the "pressure measurement process," and the measured pressure will be referred to as the "measured pressure." The specific time elapsed since step 3 will be referred to as the "elapsed time."
[0040] [Process 1]
[0041] As step 1, the pressure inside the container is set by multiplying the measured pressure by a coefficient. The coefficient is 1.0 to 3.0, and the pressure is reset to the value obtained by multiplying by this coefficient. The reset pressure is equivalent to the pre-pressurization. The pressures for agent A and agent B can be the same or different.
[0042] [Process 2]
[0043] As step 2, the valve is opened to supply agent A and agent B to the static mixer respectively, where the components are used to mix agent A and agent B.
[0044] [Process 3]
[0045] As step 3, the time for discharging the mixture from the outlet of the static mixer is set. The discharge time is affected by the internal pressure and can be set from 1 second to 5 minutes. Here, discharge can be carried out at a specific discharge rate, determined by the internal pressure of the container and the discharge time. In particular, from the viewpoint of quantitative control, it is preferable that the container is a dispenser and that the composition is pressurized and discharged by a ball screw.
[0046] [Process 4]
[0047] As part of step 4, the valve is closed to stop the discharge of the mixture from the outlet of the static mixer.
[0048] [Step 5]
[0049] As step 5, a settling period is performed. This refers to a state where the discharge device is not operating, excluding any movement of the discharge device itself. This is to allow the pressure inside the container to stabilize for a specific period of time. Hereinafter, this time will be referred to as the "settling time". The settling time is preferably 30 seconds to 5 minutes. If the settling time is longer than 5 minutes, there is a risk of gel formation due to the curing properties of the two-component curable resin composition.
[0050] When the container is a dispenser, the capacity of the two-component curable resin composition that can be held in the dispenser is limited. Therefore, it is necessary to supply the composition to the dispenser separately from the tank, pressure pump, etc. The composition can be replenished to the dispenser between any of the steps 1 to 5 described above.
[0051] Example
[0052] The present invention will now be described in more detail by way of examples, but the present invention is not limited to these examples.
[0053] Static mixer
[0054] • Shell inner diameter: 8mm, outlet inner diameter: 2.4mm, volume: 6.7cc, overall length: 177mm, material: PP
[0055] • Number of component segments: 18; Material: PP
[0056] Two-component curable resin composition
[0057] • A two-component silicone sealant (ThreeBond 1292E / ThreeBond 1293E, manufactured by ThreeBond Co., Ltd) that separates a compound having hydrolyzable silyl and / or silanol with a moisture-curing catalyst in two formulations. (Hereinafter, ThreeBond will also be referred to as TB, TB 1292E as Agent A, and TB 1293E as Agent B).
[0058] Discharge device
[0059] • Two-component discharge type discharge device (MH-2B-ST-KM, manufactured by ThreeBond Co., Ltd.)
[0060] The static mixer was set to MH-2B-ST-KM, and Agent A and Agent B were filled into the container (a dispenser pressurized by a ball screw) respectively. The de-adhesion time was measured and the gelation confirmation test was carried out.
[0061] [De-adhesion time measurement]
[0062] The detack time of TB 1292E / TB 1293E was determined. Curing was performed on the coating surface using atmospheric moisture by coating a composition in which hydrolyzable silyl and / or silanol compounds and a moisture-curing catalyst were separately contained in two formulations and left in an open environment. Agent A and Agent B were mixed in a 1:1 weight ratio and coated, then placed in several environments as described in Table 1. The resin was touched with a toothpick every 1 minute, and the time it took for the stringiness to disappear was defined as the "detack time (minutes)". The results are shown in Table 1. The test method was performed according to the method specified in JIS A 5758.
[0063]
[0064] It can be seen that TB 1292E / TB 1293E has high reactivity and can exhibit de-sticking properties in as little as 1 minute, depending on the external environment.
[0065] [Gel Confirmation Test]
[0066] The TB 1292E / TB 1293E were placed in a two-component discharge device, and the mixture was discharged via a static mixer consisting of a housing and components to confirm the gelation. As a more specific procedure, this was repeated... Figure 2 The cycle of steps 1 to 5 as described in the document is as follows. Here, the settings are: "Elapsed time" in the pressure measurement step = 3 seconds, "coefficient" in step 1 = 1.8, "resting time" in step 5 = 3 minutes, and in step 3, the mixture is beaded while moving along a rectangular path with a revolution of 1400 mm every 6 seconds. The weight of the mixture per revolution is 10 g. Other conditions are as described in the evaluation conditions below, and the above cycle is performed 80 times for each condition. The height of the beads is set to 2.5 mm and the width is set to 3 mm. In each cycle, while visually observing the height and width of the beads, the mixture is spread with a spatula at positions where the height and width of the beads differ from the set portions to confirm the presence of gelation. Each time gelation is confirmed at one point on a bead, it is counted as one "gelation confirmation number". The results are shown in Table 2.
[0067] Evaluation criteria
[0068] Surface treatment
[0069] Includes: Components and housings whose surfaces have been treated using a hydrophilic treatment (fluorination hydrophilic treatment) based on the technology of Takamatsu Tei Sang Co., Ltd.
[0070] None: Untreated components and housings
[0071] Operating environment
[0072] 5℃×35%RH, 23℃×50%RH, 35℃×95%RH.
[0073]
[0074] Comparing Examples 1-3, which involved hydrophilicating the static mixer, with Comparative Examples 1-3, which were untreated, the number of times gels were observed under any operating environment varied significantly. If gels were applied as in Comparative Examples 1-3, there was a risk of deviation occurring in the gaps between the flanges when the mixture was sandwiched between flanges. Furthermore, as mentioned above, for two-component curable resin compositions with short detack times, the humidity of the operating environment had an impact. Although the exact reason is unclear, in Comparative Examples 1-3, gels increased with increasing humidity, whereas as described in Examples 1-3, no gels were observed under varying humidity levels, and even with increased humidity, the amount of gels did not increase.
[0075] Industrial applicability
[0076] This invention relates in particular to the coating of mixtures of two-component curable resin compositions suitable for sealing surfaces of automotive parts, electrical / electronic components, etc., enabling the coating of highly reactive mixtures of two-component curable resin compositions without the discharge of gels, and the mixture forming a uniform cured product.
[0077] This application is based on Japanese Patent Application No. 2024-076636, filed on May 9, 2024, the disclosure of which is referenced and incorporated herein by reference in its entirety.
[0078] Explanation of reference numerals in the attached figures
[0079] 1: Shell,
[0080] 2: Components
[0081] 3: Discharge port (nozzle)
[0082] 4: Injection port.
Claims
1. A static mixer comprising a housing and components, wherein the housing has an outlet and an inlet at one end, wherein, The housing and components underwent a hydrophilic surface treatment.
2. The static mixer according to claim 1, wherein, The components and housing are molded from polypropylene.
3. The static mixer according to claim 1, wherein, The hydrophilic surface treatment is a surface treatment performed through the chemical reaction of fluorine gas and oxygen.
4. The static mixer according to claim 1, which is installed in a discharge device for a two-component curable resin composition.
5. The static mixer according to claim 4, wherein, The two-component curable resin composition comprises a silicone resin.
6. A method for coating a mixture of two-component curable resin compositions, wherein, The two-component curable resin composition is supplied from the discharge device to the injection port of the static mixer, and the mixture is coated from the discharge port of the static mixer, on which the housing and components have undergone hydrophilic surface treatment, the housing having the discharge port and the injection port at its end.
7. A coating apparatus, wherein, In a discharge device for a two-component curable resin composition, the two-component curable resin composition is supplied from the discharge device to the inlet of a static mixer, and the mixture is coated from the outlet of the static mixer, on which the housing and components have undergone hydrophilic surface treatment, the housing having the outlet and the inlet at its end.
Citation Information
Patent Citations
Technique for forming sealing material composed mainly of organopolysiloxane
JP1991050287A
Information processing method, information processing device and program
JP2024076636A