Supported oxide catalysts including tantalum with high yield in 1,3-butadiene production

By preparing supported oxide catalysts with specific pore sizes and compositions, the problems of low activity and insufficient yield of existing catalysts were solved, achieving efficient production of 1,3-butadiene and extending the catalyst's lifespan.

CN123146435APending Publication Date: 2026-11-20SYNTHOS SA +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202580014124.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-02-07
Filing Date
2025-02-07
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing supported oxide catalysts suffer from low activity and insufficient yield in the production of 1,3-butadiene, especially the tantalum oxide catalyst used in fluidized beds, which has a small average pore size and poor wear resistance.

Method used

The catalyst is prepared by using a supported oxide catalyst with a specific average pore size range, containing 0.1 to 10% by weight of Ta₂O₅, with an average pore size of 180 to 245 Å, preferably 180 to 240 Å, more preferably 190 to 230 Å, and most preferably 200 to 210 Å, in combination with appropriate amounts of aluminum and sodium. The preparation method of the catalyst includes impregnation, drying and calcination steps, using ordered or disordered porous silica support.

Benefits of technology

The yield of 1,3-butadiene was increased, the online operating time of the catalyst was extended, the average coke deposition was reduced, and the activity and stability of the catalyst were significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The present invention relates to a supported oxide catalyst comprising: tantalum, calculated as Ta2O5, in an amount of 0.1 to 10 weight percent (wt.%) based on the total weight of the supported oxide catalyst, the supported oxide catalyst having an average pore diameter of 180 to 245 A. Furthermore, the present invention relates to: a catalyst reaction tube for the production of 1,3-butadiene comprising at least one packing of a supported oxide catalyst as defined herein; a fixed bed reactor for the production of 1,3-butadiene comprising one or more catalyst reaction tubes as defined herein; and a plant for the production of 1,3-butadiene comprising one or more fixed bed reactors as defined herein. The present invention also relates to a process for the production of 1,3-butadiene as defined herein and to a process for the production of a supported oxide catalyst as defined herein.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a supported oxide catalyst comprising tantalum and having a specific average pore size. Furthermore, this invention relates to: a catalyst reaction tube for the production of 1,3-butadiene comprising at least one packing of a supported oxide catalyst as defined herein; a fixed-bed reactor for the production of 1,3-butadiene comprising one or more catalyst reaction tubes as defined herein; and an apparatus for the production of 1,3-butadiene comprising one or more fixed-bed reactors as defined herein. The invention also relates to a method for producing 1,3-butadiene as defined herein. Background Technology

[0002] 1,3-Butadiene is one of the most important raw materials in the synthetic rubber industry. As a monomer, it is used in the production of various synthetic polymers such as polybutadiene rubber, acrylonitrile-butadiene-styrene polymers, styrene-butadiene rubber, nitrile-butadiene rubber, and styrene-butadiene latex. For example, 1,3-butadiene is a byproduct of ethylene production from naphtha steam cracking and can be separated by extractive distillation (Chem. Soc. Rev., 2014, 43, 7917; ChemSusChem, 2013, 6, 1595; Chem. Central J., 2014, 8, 53).

[0003] The depletion of non-renewable fossil fuel resources and environmental factors have recently become a strong driving force for exploring renewable resources of 1,3-butadiene and its precursors. Among the many available renewable energy sources, biomass appears to have the greatest potential for producing 1,3-butadiene. This strategy has two main advantages: reducing dependence on fossil fuels and decreasing carbon dioxide emissions (ChemSusChem, 2013, 6, 1595).

[0004] The conversion of ethanol, for example, to obtain 1,3-butadiene from biomass, can be carried out using two methods reported in the literature: a one-step process (Lebedev process) and a two-step process (Ostromislensky process).

[0005] In the early 20th century, Lebedev published a one-step process that uses a multifunctional catalyst with acid-base properties to directly convert ethanol into 1,3-butadiene (J. Gen. Chem., 1933, 3, 698; Chem. Ztg., 1936, 60, 313).

[0006] On the other hand, the so-called two-step method can be carried out by converting ethanol to acetaldehyde in the first step. The purpose of the first step is to feed the mixture of ethanol and acetaldehyde into the second step or a fixed-bed reactor. In the second step, the mixture of ethanol and acetaldehyde is converted to 1,3-butadiene in the presence of, for example, a silica-supported tantalum catalyst (Catal. Today, 2016, 259, 446).

[0007] WO2022165190A1 relates to a method for preparing a supported tantalum oxide catalyst precursor or catalyst having a controlled Ta distribution, and the resulting supported Ta catalyst. In one embodiment, the method includes selecting a Ta precursor that has appropriate reactivity with the surface hydroxyl groups of a solid oxide support material to produce a desired Ta distribution in the catalyst precursor or catalyst. In another embodiment, the method includes controlling the number of available surface hydroxyl groups on the support material to react with the Ta precursor by a thermal method such as calcination, thereby achieving the desired Ta distribution.

[0008] US2018 / 0208522 A1 relates to a catalyst for converting a feed comprising ethanol and acetaldehyde into 1,3-butadiene. The catalyst comprises at least elemental tantalum and at least one acid-washed mesoporous oxide matrix comprising at least 90% by weight silica prior to washing, wherein the elemental tantalum comprises 0.1% to 30% by mass of the mesoporous oxide matrix. The teaching of US2018 / 0208522 A1 relies on acid washing of the mesoporous oxide support to increase the selectivity of the catalyst for 1,3-butadiene and / or the productivity of the catalyst for 1,3-butadiene. At the end of the washing step and before impregnation with the active component, the catalyst contains 0 to 500 ppm of sodium. The aluminum concentration in the catalyst and the yield of 1,3-butadiene are not disclosed in US2018 / 0208522 A1.

[0009] Kim et al. (Chemical Engineering Journal 278 (2015) 217–223) demonstrated the production of butadiene from ethanol and acetaldehyde using a tantalum oxide-supported spherical silica catalyst in a circulating fluidized bed. They found that the average pore size of the Q10 supported catalyst was approximately 150 Å. The literature further indicates that larger pore sizes result in weaker catalysts and lower abrasion resistance.

[0010] There has been a persistent need for supported oxide catalysts for the production of 1,3-butadiene that are highly active and, in particular, capable of providing high yields of 1,3-butadiene. Summary of the Invention

[0011] In a first aspect, the present invention relates to a supported oxide catalyst comprising tantalum, calculated as Ta2O5 and in an amount of 0.1 to 10% by weight based on the total weight of the supported oxide catalyst, wherein the average pore size of the supported oxide catalyst is 180 to 245 Å.

[0012] The average aperture is calculated using the following formula, assuming a cylindrical aperture: Å)= , The surface area (SA) and pore volume (PV) were measured using an Autosorb-6 Testing Unit from Anton Paar GmbH via nitrogen porosimetry. Supported oxide catalysts were pulverized into powder, and approximately 0.2 g samples were taken for analysis. The samples were first degassed in an Autosorb-6 Degassing Unit at 350°C for at least 4 hours. The surface area at multiple points was calculated using BET theory, and data points within the P / P0 range of 0.05 to 0.30 were used. Pore volume measurements were recorded at a P / P0 of 0.984 in the desorption leg.

[0013] In the study of this invention, it was found that the tantalum-supported oxide catalyst of the present invention, having a defined average pore size, provides a higher yield of 1,3-butadiene and allows for a longer time-on-stream.

[0014] In a preferred embodiment, the supported oxide catalyst includes: (i) aluminum in an amount of 5 to 350 ppm and (ii) sodium in an amount of 35 to 500 ppm, each based on the total weight of the supported oxide catalyst.

[0015] The sodium and aluminum content expressed in parts per million (ppm) in this article is relative to the total weight of the supported oxide catalyst.

[0016] In another preferred embodiment, the supported oxide catalyst comprises: (i) aluminum in an amount of 5 to 60 ppm and (ii) sodium in an amount of 35 to 70 ppm, each based on the total weight of the supported oxide catalyst; or (i) aluminum in an amount of 50 to 350 ppm and (ii) sodium in an amount of 300 to 500 ppm, each based on the total weight of the supported oxide catalyst.

[0017] Preferably, the average pore size of the supported oxide catalyst according to the present invention is 180 to 240 Å, more preferably 190 to 230 Å, more preferably 195 to 220 Å, and most preferably 200 to 210 Å.

[0018] Preferably, the supported oxide catalyst according to the present invention comprises: tantalum, which is calculated as Ta2O5 and is present in an amount of 0.5 to 5% by weight based on the total weight of the supported oxide catalyst, more preferably 2 to 3% by weight based on the total weight of the supported oxide catalyst.

[0019] Supported oxide catalysts have advantages because they allow for control over the concentration and dispersion of active sites, are easy to prepare by impregnating supports of any form and shape, and allow the reacting molecules to easily access all active sites of the catalyst.

[0020] In a preferred embodiment, the supported oxide catalyst includes one or more of the following: ordered porous silica support and non-ordered porous silica support, other porous oxide supports and mixtures thereof, preferably derived from ZrO2, TiO2, MgO, ZnO, NiO and CeO2.

[0021] Preferably, the supported oxide catalyst includes one or more of an ordered porous silica support or a disordered porous silica support.

[0022] Most preferably, the supported oxide catalyst comprises disordered porous silica.

[0023] Preferably, the BET specific surface area of ​​the supported oxide catalyst according to the present invention is 130 to 550 m². 2 / g, preferably 180 to 280 m 2 / g.

[0024] In a preferred embodiment, the supported oxide catalyst includes: (iv) calcium, which is 1 to 100 ppm based on the total weight of the supported oxide catalyst.

[0025] In a preferred embodiment, the supported oxide catalyst includes: (v) iron, each in an amount of 1 to 50 ppm based on the total weight of the supported oxide catalyst.

[0026] In a preferred embodiment, the supported oxide catalyst includes: (vi) titanium, which is 1 to 150 ppm based on the total weight of the supported oxide catalyst.

[0027] In a second aspect, the present invention relates to a catalyst reaction tube for the production of 1,3-butadiene, comprising at least one packing material of a supported oxide catalyst according to the present invention, and one or more packing materials of inert material.

[0028] In one embodiment, the inert material is selected from the group consisting of silicon carbide, inert ceramic bed, ceramic beads, extruder, rings with a diameter of 2 to 7 mm, stainless steel mesh, foam, and mixtures thereof.

[0029] According to a preferred embodiment, the inert material packing material contacts the packing material of the supported oxide catalyst according to the invention, i.e., the reaction zone, and separates the packing materials of the supported oxide catalyst according to the invention from each other (if there are more than one packing material of the supported oxide catalyst in the catalyst reaction tube). They are preferably located at the reactant inlet and outlet of the reaction tube.

[0030] According to one embodiment, a layer of supported oxide catalyst according to the present invention is packed inside the catalyst reaction tube, preferably located at the center of the catalyst reaction tube. The supported oxide catalyst according to the present invention is in contact with inert material packing on both sides, that is, the inert material packing is preferably located at the feed inlet and outlet of the catalyst reaction tube. According to this embodiment, the catalyst reaction tube includes a reaction zone.

[0031] According to another embodiment, the catalyst reaction tube is alternately loaded with packing material of the supported oxide catalyst according to the present invention and packing material of inert material. The inert material packing material is preferably located at the feed inlet and outlet of the catalyst reaction tube and is in contact with the packing material of the supported oxide catalyst according to the present invention. According to this embodiment, the catalyst reaction tube includes multiple reaction zones.

[0032] In a third aspect, the present invention relates to a fixed-bed reactor for the production of 1,3-butadiene, comprising one or more catalyst reaction tubes according to the invention.

[0033] In a fourth aspect, the present invention relates to an apparatus for the production of 1,3-butadiene, comprising one or more fixed-bed reactors as defined herein, and means for regenerating a supported oxide catalyst in one or more fixed-bed reactors.

[0034] According to one embodiment, the apparatus further includes a pre-reactor for producing acetaldehyde, having one or more reaction tubes comprising a supported or unsupported (bulk) catalyst, the supported or unsupported (bulk) catalyst comprising one or more of zinc, copper, silver, chromium and nickel, preferably comprising one or more of zinc and copper.

[0035] The tantalum oxide contained in the supported oxide catalyst according to the first aspect of the invention itself does not function in the oxidation of ethanol to acetaldehyde. Therefore, in order to produce 1,3-butadiene using the supported oxide catalyst according to the invention, the feed stream must contain ethanol and acetaldehyde. This mixture of ethanol and acetaldehyde can be produced, for example, from ethanol in a pre-reactor for the production of acetaldehyde, which includes a supported or unsupported (bulk) catalyst as defined above, and then fed into a fixed-bed reactor for the production of 1,3-butadiene, which includes one or more catalyst reaction tubes according to the invention. Alternatively, ethanol and acetaldehyde can be obtained from commercial sources and fed directly into a fixed-bed reactor for the production of 1,3-butadiene, which includes one or more catalyst reaction tubes according to the invention.

[0036] In a fifth aspect, the present invention relates to a method for producing 1,3-butadiene, the method comprising: (1) A feed comprising ethanol and acetaldehyde is contacted with a supported oxide catalyst according to the present invention to obtain a crude product comprising 1,3-butadiene.

[0037] Preferably, in the method according to the invention, the contact (1) is carried out at a temperature of 200 to 500°C, preferably 250 to 450°C, and more preferably 300 to 400°C.

[0038] In a preferred embodiment of the method according to the present invention, the contact of (1) is 0.2 to 10 h. -1 Preferably 0.3 to 5 hours -1 More preferably 0.5 to 3 h -1 The weight hourly space velocity is measured.

[0039] The contact (1) is preferably carried out at a pressure of 0 to 10 barg, more preferably 1 to 3 barg, and most preferably 1 to 2 barg.

[0040] Preferably, the method according to the sixth aspect of the invention further includes the following steps: (2) The crude product is separated into at least a first fraction comprising 1,3-butadiene, a second fraction comprising acetaldehyde, and a third fraction comprising ethanol. Preferably, at least a portion of the second part, at least a portion of the third part, or at least a portion of both the second and third parts are recycled back into the feed.

[0041] According to a preferred embodiment of the method of the sixth aspect of the present invention, the contact (1) is carried out in a continuous flow of feed in a fixed-bed reactor as described in the third aspect.

[0042] In another preferred embodiment of the method according to the invention, the feed comprises at least 50% by weight of ethanol based on its total weight, preferably 60 to 75% by weight of ethanol.

[0043] In another preferred embodiment of the method according to the invention, the feed comprises at least 15% by weight of acetaldehyde based on its total weight, preferably 20 to 35% by weight of acetaldehyde.

[0044] In another preferred embodiment of the method according to the present invention, the molar ratio of ethanol to acetaldehyde in the feed is 1 to 7, preferably 1.5 to 5, more preferably 1.7 to 4, and most preferably 2.0 to 3.0.

[0045] A method for producing the supported oxide catalyst according to the present invention is further disclosed, comprising or consisting of the following steps: (i) Impregnating a support with a solution of tantalum precursor, wherein the contents of aluminum and sodium are defined by the following formula based on the weight of the catalyst support, to form a supported tantalum catalyst precursor. The lower limit (LL) is defined as: carrier [M] LL =Catalyst [M] LL / (1 - catalyst [Ta2O5] wt%), where M = Na or Al; and The upper limit (UL) is defined as: the carrier [M] UL =Catalyst [M] UL / (1 - catalyst [Ta2O5] wt%), where M = Na or Al; (ii) Drying the supported tantalum catalyst precursor; and (iii) Calcining the dried supported tantalum catalyst precursor to form a supported tantalum catalyst.

[0046] In the above formula, the carrier [M] LL This indicates the lower limit of the concentration (by weight) of metal M (M being sodium or aluminum, respectively) in the carrier to be used and impregnated in step (i), which depends on... a. Catalyst [M] LL That is, the lower limit of the concentration (wt / wt) of metal M (M is sodium or aluminum) in the supported oxide catalyst according to the present invention finally obtained in step (iii), and b. Catalyst [Ta2O5] wt%, i.e., the concentration of Ta2O5 in the supported oxide catalyst according to the present invention finally obtained in step (iii) (wt / wt).

[0047] Similarly, in the above formula, the carrier [M] ULThis indicates the upper limit of the concentration (by weight) of metal M (M being sodium or aluminum, respectively) in the carrier to be used and impregnated in step (i), which depends on... a. Catalyst [M] UL That is, the upper limit of the concentration (by weight) of metal M (M being sodium or aluminum, respectively) in the supported oxide catalyst according to the present invention finally obtained in step (iii), and b. Catalyst [Ta2O5] wt%, i.e., the concentration of Ta2O5 in the supported oxide catalyst according to the present invention finally obtained in step (iii) (wt / wt).

[0048] Regarding the sodium and aluminum content of the supported oxide catalyst according to the first aspect of the invention, it preferably corresponds to catalyst [M]. LL and catalyst [M] UL The preferred implementation method.

[0049] In a preferred embodiment, the carrier impregnated in step (i) of the method according to the invention comprises one or more ordered porous silica and disordered porous silica, other porous oxides and mixtures thereof, preferably derived from ZrO2, TiO2, MgO, ZnO, NiO and CeO2.

[0050] Preferably, the carrier impregnated in step (i) of the method according to the present invention is a silica carrier, preferably an ordered porous silica carrier or a disordered porous silica carrier.

[0051] According to a preferred embodiment of the method for producing a supported oxide catalyst, the supported oxide catalyst is a silica-supported oxide catalyst, and the method includes or comprises the following steps: (i) Reacting an aqueous silicate, preferably a sodium silicate solution, with an acid to form a hydrosol; (ii) Dispersion, preferably by spraying, more preferably by spraying into the air and breaking into droplets; and gelation of the hydrosol to form hydrogel beads; (iii) One or more optional additional steps, including (pre)aging, acidification, washing, and pH adjustment. a. Aging hydrogel beads at temperature T1 b. Acidification of aged hydrogel beads, c. Wash the acidified and aged hydrogel beads, preferably with deionized water acidified to pH 3 to 4. d. Adjust the pH value of the washed hydrogel beads obtained in step (c), preferably to a pH value of about 8 to 10; (iv) Aging the hydrogel beads at temperature T2, where T2 > T1 (if applicable, e.g., if one of the optional steps in (iii) is used). (v) Acidification of the aged hydrogel beads obtained in step (iv), (vi) Wash the acidified and aged hydrogel beads (obtained in step (v)) preferably with deionized and acidified water to pH 3 or 4; (vii) Optionally adjust the pH value of the washed hydrogel beads obtained in step (vi), preferably to a pH value of about 3 to 10, and most preferably to a pH value of about 9; (viii) Dry the washed hydrogel beads obtained in step (vi) or (vii) to obtain a silica carrier, preferably using an oven; (ix) Optionally, the silica support obtained in step (viii) may be sieved (to collect the desired particle size fraction). (x) Impregnate the silica support obtained in step (viii) or (ix) with a solution of tantalum precursor to form a supported tantalum catalyst precursor, preferably wherein the tantalum precursor is tantalum ethoxide, most preferably wherein the tantalum ethoxide precursor is stabilized with 2,4-pentanedione and / or the tantalum ethoxide precursor is dissolved in a suitable organic solvent such as isopropanol; (xi) Drying the supported tantalum catalyst precursor, preferably by heating under atmospheric pressure or vacuum; and (xii) Calcination of the dried supported tantalum catalyst precursor, preferably at a temperature of about 400 to 600°C for about 2 to 5 hours, to form a supported tantalum catalyst.

[0052] The term "supported tantalum catalyst precursor" as used in this article refers to, for example, an intermediate product before calcination. In contrast, "tantalum-containing supported oxide catalyst" refers to a product after calcination.

[0053] Preferably, the temperature T1 in the method according to the present invention is 20 to 50°C.

[0054] Preferably, the temperature T2 in the method according to the present invention is 40 to 130°C.

[0055] In a sixth aspect, the present invention relates to the use of a supported oxide catalyst according to the first aspect of the invention for the production of 1,3-butadiene from a feed comprising ethanol and acetaldehyde, preferably for increasing the yield of 1,3-butadiene.

[0056] Provided that it is technically reasonable, a preferred embodiment of any aspect of the present invention (see the first to sixth aspects above) may correspond to a preferred embodiment of another aspect of the present invention (as defined above) or may be derived from a preferred embodiment of another aspect of the present invention (as defined above). Detailed Implementation Example 1. Preparation of silica support

[0057] The following is a description of the general steps used to manufacture a silica carrier according to embodiments of this disclosure. Figure 1 A flowchart illustrating the general steps used to manufacture a silica support according to embodiments of this disclosure is provided. A general but more detailed description of silica supports and methods for their preparation is provided in US20210269562A1, which is incorporated herein by reference.

[0058] In one embodiment, a dilute sodium silicate solution with a SiO2:Na2O weight ratio of 3.3 is reacted with dilute sulfuric acid to form a hydrosol having the following composition: 12 wt% SiO2 and a molar ratio of H2SO4:Na2O of 0.8. The resulting hydrosol is alkaline.

[0059] The hydrosol was then sprayed into the air, where it broke down into droplets and solidified into beads several millimeters in diameter before being captured by the sulfuric acid solution, resulting in a bead / solution system with a pH less than 2. The beads were then washed with acidified deionized water at a pH of approximately 3, followed by another wash with deionized water. The pH of the bead / solution system was then raised to 8 to 9 by adding an ammonia solution. The beads used in the comparative example were then aged at 70 °C. For the example of the present invention, the beads were aged at 125 °C using a Parr bomb. The aging time for both samples was approximately 16 hours.

[0060] The washed and aged hydrogel beads contain approximately 15 to 18% SiO2 and have a pH of 8 to 9. After washing, the pH of the beads is raised to approximately 9 using an ammonium hydroxide solution. The beads are then dried in an oven. Finally, the beads are sieved to obtain the desired particle size fraction. Note that pH adjustment before drying is optional, and the beads are typically dried to a pH of 3 to 9. 2. Catalyst Preparation

[0061] Before use, silica beads with a size of 2 to 5 mm should be pre-dried so that the loss of drying (LOD) is <0.5% by weight when measured at 120°C. The following is a general description of the preparation of supported oxide catalysts based on 100 g of silica support on a dry basis. In a broader sense, the tantalum precursor is added to silica via the incipient wetness impregnation method.

[0062] For every 100 g (dry basis) of silica support, a stabilized tantalum precursor solution is prepared by mixing approximately 5 to 6 g of a tantalum precursor, such as 5.7 g of tantalum ethoxide, with 2 to 3 g, such as 2.8 g of 2,4-pentanedione (acetone acetyl). Typically, 8.5 g of the stabilized tantalum precursor solution is dissolved in 65 to 76 g of isopropanol and then added to pre-dried silica beads. The amount of isopropanol is adjusted based on the pore volume of the support so that the solution is contained only within the silica pores, with no free solution outside the pores. Impregnation takes approximately 15 to 40 minutes. The impregnated silica is placed in a sealed container for at least 1 hour before evaporating the solvent by heating under atmospheric pressure or vacuum. The dried material is then calcined in air to 550°C for 4 hours to obtain a finished supported oxide catalyst containing approximately 3.0 wt% Ta₂O₅.

[0063] Since the tantalum ethoxide, acetone acetyl or isopropanol used do not contain large amounts of Na or Al, it can be assumed that Na and Al are present in the support. 3. Methods for Sodium and Aluminum Analysis

[0064] The sodium and aluminum contents in the supported oxide catalyst were determined by atomic absorption spectrometry (AA) and inductively coupled plasma (ICP) spectrometry, respectively. A Perkin-Elmer PinAAcle™ 900F spectrometer was used for atomic absorption spectrometry, and a Perkin-Elmer Optima 8300 ICP-OES spectrometer was used for ICP. The supported oxide catalyst sample was digested with hydrofluoric acid (HF). The generated silicon tetrafluoride (SiF4) was dispersed as smoke, and the residue was analyzed for sodium and aluminum. The sodium and aluminum contents were reported as parts per million (ppm) in the supported oxide catalyst after drying at 120°C. If necessary, the sodium and aluminum contents in the support and tantalum starting material could be determined separately. 4. Tantalum Analysis Methods

[0065] The tantalum content in the supported oxide catalyst was measured using inductively coupled plasma (ICP) spectrometry on a Perkin-Elmer Optima 8300 ICP-OES spectrometer. The supported oxide catalyst sample was digested with hydrofluoric acid (HF). The resulting silicon tetrafluoride (SiF4) was dispersed as smoke, and the residue was analyzed for tantalum content. The results are reported based on the dry weight of the supported oxide catalyst after calcination at 500–550 °C. Table 1: Physicochemical properties of the supported oxide catalysts synthesized by the above method. 1 The commercial support material CARiACT Q10 (from Fuji Silysia Chemical, Ltd., not prepared according to the above support preparation method) was used to measure the elemental composition of the tantalum catalyst before it was ready for use. Two samples were measured. 2 On a dry basis.

[0066] Table 1 lists the average pore size values ​​of the Q10-based catalyst (refer to Kim et al.), but the catalytic properties of the catalyst were not tested. 5. Catalyst testing

[0067] Twenty grams of the supported oxide catalysts A (in this invention) and B (comparative catalyst) synthesized according to the above method were placed in a continuously operating stainless steel fixed-bed reactor. The fixed-bed reactor was initially heated to 325°C, and the nitrogen flow rate was 200 ml / min. Then, a mixture of 94 wt% aqueous ethanol and acetaldehyde at a mass ratio of 2.5:1 was used as feed (the mass fraction of 94 wt% aqueous ethanol, 2.5, is related to the total weight of aqueous ethanol), and the mixture was subjected to a nitrogen flow (200 ml / min) at a weight hourly space velocity (WHSV) of 1.0 h⁻¹. -1 The reaction was carried out at a pressure of 1.5 barg. The composition of the effluent was monitored periodically using an online gas chromatography system equipped with a flame-ionization detector coupled to a mass spectrometer (GC / MS).

[0068] The results are calculated as follows and listed in Tables 2 and 3 below (EtOH represents ethanol; AcH represents acetaldehyde): *100 *100 Table 2: Process conditions: Temperature = 325 (±2)℃, Pressure = 1.5 barg, WHSV = 1.0 h -1 94% by weight of EtOH:AcH = 2.5:1 by weight, TOS = 220 hours: 1 Comparative catalyst B began to deteriorate after approximately 120 hours. Table 3: Process conditions: Temperature = 325 (±2)℃, Pressure = 1.5 barg, WHSV = 1.0 h -1 94% by weight of EtOH:AcH = 2.5:1 by weight / weight. 1 The comparative catalyst remained stable in the flow for only about 120 hours. 2 125-hour average.

[0069] As can be clearly seen from the results in Tables 2 and 3 above, compared with catalysts having lower average pore size, the catalyst according to the present invention not only exhibits lower average coke deposition but also shows a higher overall conversion over time. Since the selectivity for butadiene does not change over time, the yield of butadiene by the catalyst according to the present invention is more stable over time.

Claims

1. A supported oxide catalyst, characterized in that... include: Tantalum, calculated as Ta2O5 and in an amount of 0.1 to 10% by weight based on the total weight of the supported oxide catalyst, has an average pore size of 180 to 245 Å.

2. The supported oxide catalyst as described in claim 1, comprising: (i) Aluminum, in amounts of 5 to 350 ppm; (ii) Sodium, in amounts of 35 to 500 ppm, each based on the total weight of the supported oxide catalyst.

3. The supported oxide catalyst as described in claim 2, comprising: (i) aluminum, in an amount of 5 to 60 ppm; and (ii) sodium, in an amount of 35 to 70 ppm, each based on the total weight of the supported oxide catalyst, or (i) aluminum, in an amount of 50 to 350 ppm; and (ii) sodium, in an amount of 300 to 500 ppm, each based on the total weight of the supported oxide catalyst.

4. The supported oxide catalyst as described in any one of claims 1 to 3, wherein the average pore size is 180 to 240 Å, preferably 190 to 230 Å, more preferably 195 to 220 Å, and most preferably 200 to 210 Å.

5. The supported oxide catalyst according to any one of claims 1 to 4, comprising: Tantalum, Its amount, calculated as Ta2O5 and based on the total weight of the supported oxide catalyst, is 0.5% to 5% by weight. Preferably, the amount of it, calculated as Ta2O5 and based on the total weight of the supported oxide catalyst, is 2 to 3 by weight.

6. The supported oxide catalyst according to any one of claims 1 to 5, wherein the supported oxide catalyst comprises one or more of ordered porous silica supports, disordered porous silica supports, other porous oxide supports, and mixtures thereof, wherein the other porous oxide supports are preferably derived from ZrO2, TiO2, MgO, ZnO, NiO, and CeO2. Preferably, the supported oxide catalyst comprises one or more of ordered porous silica supports and disordered porous silica supports. Specifically, the supported oxide catalyst mentioned herein includes disordered porous silica.

7. The supported oxide catalyst according to any one of claims 1 to 6, wherein the BET specific surface area of ​​the supported oxide catalyst is 130 m². 2 / g to 550 m 2 / g, preferably 180 m 2 / g to 280 m 2 / g.

8. The supported oxide catalyst according to any one of claims 1 to 7, comprising: (iv) Calcium, in amounts of 1 to 100 ppm; (v) Iron, in amounts ranging from 1 to 50 ppm; and / or (vi) Titanium, in amounts ranging from 1 to 150 ppm, Each is based on the total weight of the supported oxide catalyst.

9. A catalyst reaction tube for the production of 1,3-butadiene, characterized in that... It includes at least one packing layer of a supported oxide catalyst as described in any one of claims 1 to 8, and one or more packing layers of inert material.

10. A fixed-bed reactor for the production of 1,3-butadiene, characterized in that... Includes one or more catalyst reaction tubes as described in claim 9.

11. A production facility for the production of 1,3-butadiene, characterized in that... include: (x) one or more fixed-bed reactors as described in claim 10; and (y) means for regenerating the supported oxide catalyst in the one or more fixed-bed reactors. Preferably, the apparatus further includes (z) a pre-reactor for producing acetaldehyde, having one or more reaction tubes comprising a supported or unsupported (bulk) catalyst comprising one or more of zinc, copper, silver, chromium, magnesium and nickel.

12. A method for producing 1,3-butadiene, the method comprising: (1) Contacting a feed comprising ethanol and acetaldehyde with a supported oxide catalyst as described in any one of claims 1 to 8 to obtain a crude product comprising 1,3-butadiene.

13. The method as described in claim 12, wherein: The contact described in (1) is carried out at a temperature of 200 to 500 °C, preferably 250 to 450 °C, and more preferably 300 to 400 °C; and / or The contact in (1) is for 0.2 to 10 hours. -1 Preferably 0.3 to 5 h -1 The optimal time is 0.5 to 3 hours. -1 The heavy space speed proceeds.

14. The method as described in claim 12 or 13, wherein the contact in (1) is performed at a pressure of 0 to 10 barg, preferably 1 to 3 barg, and most preferably 1 to 2 barg.

15. The method as described in any one of claims 12 to 14, further comprising the step of: (2) The crude product is separated into at least a first fraction comprising 1,3-butadiene, a second fraction comprising acetaldehyde, and a third fraction comprising ethanol. Preferred among them At least a portion of the second part or at least a portion of the third part is recycled back into the feed; or At least a portion of both the second and the third portions is recycled back into the feed.

16. The method of any one of claims 12 to 15, wherein the contact of (1) is carried out in a continuous flow of the feed in a fixed-bed reactor as described in claim 10.

17. Use of a supported oxide catalyst as described in any one of claims 1 to 8 for the production of 1,3-butadiene from a feed comprising ethanol and acetaldehyde, preferably for increasing the yield of 1,3-butadiene.

Citation Information

Patent Citations

  • Tantalum-based catalyst deposited on silica for the transformation of ethanol into butadiene

    US20180208522A1

  • Chromium-on-silica catalysts and methods of making the same

    US20210269562A1

  • Method for manufacturing a supported tantalum catalyst

    WO2022165190A1