Highly active catalytic material for nh3 conversion and its preparation by one-step impregnation

By developing a method for preparing Ru- and alkali metal-loaded catalytic materials on acid-treated support materials, the problem of insufficient catalytic material activity in high-pressure NH₃ reforming reactions was solved, achieving low-temperature and high-efficiency H₂ conversion and improving the hydrothermal resistance of the catalytic materials.

CN123146436APending Publication Date: 2026-11-20BASF SE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202580029477.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-22
Filing Date
2025-04-17
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies struggle to efficiently convert NH₃ to H₂ in high-pressure reforming reactions, and the catalytic materials lack sufficient activity and hydrothermal resistance, failing to meet the demands of industrial applications.

Method used

A novel catalytic material was prepared by loading Ru and alkali metals onto an acid-treated support material using a one-step impregnation method, including calcination, acid treatment, and impregnation processes, thereby optimizing the composition and structure of the support material.

Benefits of technology

The method achieves efficient conversion of NH₃ to H₂ at low temperatures, exhibits high hydrothermal resistance, is suitable for high-pressure conditions, and improves the activity and stability of the catalytic material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146436A_ABST
    Figure CN123146436A_ABST
Patent Text Reader

Abstract

The present invention relates to a process for preparing a catalytic material, the process comprising (i) molding a mixture comprising one or more sources of a support material; (ii) calcining the moldings obtained from (i) in a gaseous atmosphere, obtaining moldings comprising a support material; (iii) impregnating the moldings with an aqueous solution comprising both a source of Ru and a source of an alkali metal, such as potassium acetate. Furthermore, the present invention relates to a catalytic material obtained or obtainable by said process and to the use thereof. Still further, the present invention relates to a process for converting NH3 into H2 and N2 using said catalytic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing catalytic materials, particularly catalytic materials comprising Ru and alkali metals supported on a carrier material, the catalytic materials obtained and / or obtained by said method, and their uses. Furthermore, this invention relates to a method for using said catalytic material to convert NH3 to H2 and N2. Background Technology

[0002] NH3 is considered a future energy carrier, capable of chemically storing large amounts of H2. Therefore, sustainable NH3 could potentially be generated on a large scale from renewable energy sources. On-site reforming of NH3 where H2 is needed (see Equation 1 below) may be the final step in completing the H2 value chain based on renewable electricity.

[0003] (1) 2 NH3 N2 + 3 H2

[0004] To enhance the decomposition of ammonia into nitrogen and hydrogen, the use of supported Ru catalysts has been discussed. For example, K. Lamb et al. investigated the ammonia decomposition kinetics on LiOH-promoted Ru / Al₂O₃ in the *Int. J. of Hydrogen Energy*, 2019, 44, 3726-3736. On the other hand, A. Di Carlo et al. investigated ammonia decomposition on a commercial Ru / Al₂O₃ catalyst at different operating pressures and temperatures in the *Int. J. of Hydrogen Energy*, 2014, 39, 808-814, noting that a larger dissociation rate was achieved at lower pressures.

[0005] TA Le et al. discussed the method for generating CO-free products via ammonia decomposition in Korean J. Chem. Eng. 2021, 38(6), 1087-1103. x The development of ruthenium and nickel catalysts for H2. However, the literature indicates that alkaline earth metal oxide supports, and in particular basic supports such as MgO or neutral supports such as carbon nanotubes, will provide better results than amphoteric supports such as Cr2O3 and TiO2 or acidic supports such as Al2O3, ZrO2 or SiO2.

[0006] M. Miyamoto et al., in *Int. J. of Hydrogen Energy*, 2018, 43, 730-738, discussed the use of La-doped ZrO2 supports to improve their basicity and their applications in reactions for hydrogen production. Similarly, B. Lorenzut et al., in *ChemCatChem*, 2010, 2, 1096-1106, disclosed the use of lanthanum-stabilized zirconium oxide and indicated that basic oxides would be more efficient as supports for Ru catalysts compared to acidic oxides. Z. Wang et al., in *Int. J. of Hydrogen Energy*, 2019, 44, 7300-7307, specifically discussed Ba-modified ZrO2 supports for Ru and their applications in ammonia decomposition.

[0007] Ru supported on ZrO2 can also be used as a catalyst in other reactions. Therefore, WO 2015 / 086639 A2 relates to Ru / ZrO2 catalysts used in the hydrogenation of aromatic compounds, while WO 2018 / 046393 A1 relates to Ru / ZrO2 catalysts used in the hydrogenation of nitriles.

[0008] On the other hand, S.-F. Yin et al., in Applied Catalysis B Environmental, 2004, 48, 237-241, discussed the use of carbon nanotubes (CNTs) as supports for Ru nanoparticles in the production of hydrogen through ammonia decomposition. The activity order of different supports was indicated as follows: Ru / CNT > Ru / MgO > Ru / activated carbon > Ru / ZrO2 Ru / Al2O3.

[0009] However, in order to obtain H2 directly under high pressure (10-50 bar), NH3 reforming itself must also be carried out at these pressures. Therefore, there is still a need for improved and cost-effective methods for NH3 reforming that allow for the direct supply of H2 under the conditions required for its further reactions.

[0010] In this regard, S. Sayas et al. investigated high-pressure ammonia decomposition on a Ru-K / CaO catalyst at pressures up to 40 bar in Catal. Sci. Technol. [Catalysis Science and Technology] 2020, 10, 5027–5035. As described by TA Le et al. in Korean J. Chem. Eng. [Korean Journal of Chemical Engineering] 2021, 38(6), 1087-1103, S. Sayas et al. taught that the properties of the support have shown a strong influence on the catalytic performance of Ru-based catalysts, with the use of basic and neutral supports generally yielding better catalytic properties in the use of basic supports such as MgO and La2O3, neutral supports such as carbon nanotubes, and acidic supports such as Al2O3. GB 1377191 A relates to the cracking of ammonia into nitrogen and hydrogen and discloses a catalyst comprising metallic cobalt or cobalt oxide or both supported on a mixed oxide having a predominantly spinel structure.

[0011] However, a novel catalytic material is still needed, particularly regarding its activity in the conversion of NH3 to N2 and H2. Furthermore, a method for preparing such a catalytic material, which is particularly efficient, is needed. In addition, a method for using said catalytic material to perform NH3 conversion is still needed. Detailed Implementation

[0012] Therefore, the subject of this invention is to provide a method for preparing novel catalytic materials that exhibit improved activity, particularly in NH3 reforming reactions for the production of H2.

[0013] Surprisingly, it has been found that novel catalytic materials can be prepared, wherein the catalytic materials particularly comprise Ru and alkali metals supported on a support material, and more particularly comprise a support material that has undergone acid treatment. It has also been surprisingly found that the novel catalytic materials according to the invention allow for NH3 conversion at low temperatures, particularly when used in applications involving high pressures. Furthermore, the novel catalytic materials prepared according to the invention have been found to exhibit high hydrothermal resistance, particularly when used under high pressure conditions (considering the water that may be present during the reaction, and especially considering the small amount of water present in industrial-grade ammonia for its stability).

[0014] Therefore, the present invention relates to a catalytic material, including a method for preparing the catalytic material, the method comprising:

[0015] (i) Molding a mixture containing one or more carrier material sources;

[0016] (ii) Calcine the molded article obtained by (i) in a gaseous atmosphere to obtain a molded article containing a carrier material;

[0017] (iii) Impregnate the molded article with an aqueous solution containing both a Ru source and an alkali metal source.

[0018] Preferably, the source of the one or more carrier materials is selected from the group consisting of: M 1 O source, M 2 2O3 source, M 3 O2 source, M 4 O2O5 source and mixtures of two or more of them,

[0019] The source of one or more carrier materials is more preferably selected from the group consisting of: M 1 O source, M 2 2O3 source, M 3 O2 sources and mixtures of two or more of them,

[0020] The source of one or more carrier materials is more preferably selected from the group consisting of: M 1 O source, M 2 O2 source and mixtures of two or more of them,

[0021] More preferably, the one or more carrier materials source is M. 1 O source and M 2 The source is composed of 2O3, wherein the one or more carrier materials source are more preferably composed of M 1 O and M 2 2O3 source composition,

[0022] Where M 1 M represents one or more divalent elements. 2 M represents one or more trivalent elements. 3 M represents one or more tetravalent elements. 4 It represents one or more pentavalent elements.

[0023] Preferably, the one or more carrier material sources comprise one or more compounds selected from the group consisting of, and preferably consisting of: oxides, hydroxides, carbonates, nitrates, bicarbonates, hydroxycarbonates, M 1 and M 2 Mixed metal oxides, M 1 and M 3 Mixed metal oxides, M 1 and M 4 Mixed metal oxides, M 2 and M 3 Mixed metal oxides, M 2 and M 4 Mixed metal oxides, M 3 and M 4Mixed metal oxides, M 1 and M 2 Mixed metal hydroxy carbonates, M 1 and M 3 Mixed metal hydroxy carbonates, M 1 and M 4 Mixed metal hydroxy carbonates, M 2 and M 3 Mixed metal hydroxy carbonates, M 2 and M 4 Mixed metal hydroxy carbonates, M 3 and M 4 Mixed metal hydroxy carbonates and mixtures of two or more of them.

[0024] Preferably, the one or more carrier material sources contain M 1 O source and M 2 O2 source.

[0025] The one or more carrier material sources contain M 1 O source and M 2 In the case of a 2O3 source, it is preferable that the M 1 O source and the M 2 The 2O3 source comprises one or more compounds selected from the group consisting of, preferably, M 1 and M 2 Mixed metal oxides, M 1 and M 2 Mixed metal hydroxy carbonates and their mixtures.

[0026] Furthermore, the one or more carrier material sources contain M 1 O source and M 2 In the case of a 2O3 source, it is preferable that the M 1 O source and the M 2 The 2O3 source has an M content in the range of 1:10 to 10:1.0, more preferably in the range of 1:2.5 to 2.5:1, more preferably in the range of 1:2 to 2:1, and more preferably in the range of 1:2.1 to 1:1.9. 1 With M 2 The molar ratio.

[0027] Furthermore, the one or more carrier material sources contain M 1 O source and M 2 In the case of a 2O3 source, it is preferable that the M 1 O source and the M 2 2O3 source contains based on contained in M 1 O source and the M 2M in 2O3 source 1 O calculation of M 1 and with M 2 M calculated from 2O3 2 The total weight, 10 to 34% by weight, more preferably 25 to 31% by weight, more preferably 27 to 29% by weight, in M 1 O calculation of M 1 .

[0028] Furthermore, the one or more carrier material sources contain M 1 O source and M 2 In the case of a 2O3 source, it is preferable that the M 1 O source and the M 2 2O3 source contains based on contained in M 1 O source and the M 2 M in 2O3 source 1 O calculation of M 1 and with M 2 M calculated from 2O3 2 The total weight, 66 to 90% by weight, more preferably 69 to 75% by weight, more preferably 71 to 73% by weight, in M 2 M calculated from 2O3 2 .

[0029] Preferably, the carrier material is selected from M. 1 O, M 2 2O3, M 3 O2, M 4 2O5, M 1 M 2 The group consisting of 2O4 and mixtures of two or more thereof, more preferably selected from M 1 O, M 2 2O3 and M 1 M 2 The group consisting of 2O4, wherein the carrier material is more preferably M. 1 M 2 2O4, where M 1 M represents one or more divalent elements. 2 M represents one or more trivalent elements. 3 M represents one or more tetravalent elements. 4 It represents one or more pentavalent elements.

[0030] Preferably, M 1 Elements selected from Groups 2, 10, 11, and 12 of the periodic table, where M... 1More preferably, it is selected from the group consisting of Mg, Ca, Ni, Cu, Zn, Mn, Co, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Mg, Ni, Cu, Zn, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Mg, Zn, Cu, and mixtures thereof; more preferably, it is selected from the group consisting of Mg, Zn, and mixtures thereof, wherein M 1 More preferably, it is Mg.

[0031] Preferably, M 2 Elements selected from Groups 5, 6, 7, 8, and 13 of the periodic table, where M... 2 More preferably, it is selected from the group consisting of Al, Ga, In, Cr, Fe, V, Mn, Co, La, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, Cr, Fe, V, Mn, La, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, La, V, Mn, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, La, and mixtures of two or more thereof, wherein M... 2 More preferably, it is Al.

[0032] Preferably, M 3 Elements selected from Groups 4 and 14 of the periodic table, where M... 3 More preferably, it is selected from the group consisting of Si, Ge, Sn, Ti, Zr, Hf, Ce, and mixtures of two or more of them, wherein M 3 More preferably, it is selected from the group consisting of Si, Ti, Zr, Hf, Ce, and mixtures of two or more of them.

[0033] In M 3 When elements are selected from Group 14 of the periodic table, M is preferred. 3 It does not contain carbon.

[0034] Preferably, M 4 Selected from Group 5 of the periodic table, where M 4 More preferably, it is selected from the group consisting of V, Nb, Ta, and mixtures of two or more of them.

[0035] Preferably, the X-ray diffraction pattern of the molded article obtained by (ii) includes at least the following reflections:

[0036]

[0037] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0038] More preferably, it includes at least the following reflections:

[0039]

[0040] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0041] More preferably, it includes at least the following reflections:

[0042]

[0043] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0044] Where M 1 More preferably Mg and wherein M 2 More preferably, it is Al.

[0045] Preferably, the molded article obtained by (ii) has a water adsorption amount in the range of 25 to 70 wt%, more preferably in the range of 37 to 47 wt%, and even more preferably in the range of 40 to 44 wt%, wherein the water adsorption amount is preferably determined according to Reference Example 1.1.

[0046] Preferably, the molded article obtained by (ii) has a thickness of 35.0 to 100.0 m. 2 Within the range of / g, more preferably from 40.0 to 60.0 m 2 Within the range of / g, more preferably from 45.0 to 55.0 m 2 The BET specific surface area within the range of / g, wherein the BET specific surface area is preferably determined according to Reference Example 1.3.

[0047] Preferably, the molded article obtained by (ii) has a total pore volume in the range of 0.20 to 0.7 ml / g, more preferably in the range of 0.30 to 0.42 ml / g, and even more preferably in the range of 0.33 to 0.39 ml / g, wherein the total pore volume is preferably determined according to Reference Example 1.4.

[0048] Preferably, molding the mixture according to (i) includes tableting or extrusion.

[0049] Preferably, the calcination according to (ii) is carried out at a temperature in the range of 300°C to 1400°C, more preferably in the range of 700°C to 1100°C, and even more preferably in the range of 900°C to 1000°C.

[0050] Preferably, the calcination according to (ii) is carried out for a period of time ranging from 0.1 to 48 h, more preferably from 0.5 to 24 h, and even more preferably from 1 to 12 h.

[0051] Preferably, the gas atmosphere according to (ii) comprises, preferably, one or more of oxygen and nitrogen, more preferably air.

[0052] Preferably, the method further includes, preferably after (ii) and before (iii),

[0053] (ii') Treat the molded article obtained by (ii) with acid.

[0054] Where the method further includes (ii'), it is preferred that the treatment according to (ii') includes immersing the molded article in acid.

[0055] Furthermore, where the method further includes (ii'), it is preferred that the treatment according to (ii') lasts for a period of time ranging from 10 to 400 minutes, more preferably from 45 to 75 minutes, and even more preferably from 55 to 65 minutes.

[0056] Furthermore, where the method further includes (ii'), it is preferred that the treatment according to (ii') is carried out at a temperature in the range of 0°C to 75°C, more preferably in the range of 10°C to 40°C, and even more preferably in the range of 15°C to 35°C.

[0057] Furthermore, where the method further includes (ii'), it is preferred that the acid according to (ii') is an aqueous acid solution.

[0058] When the acid according to (ii') is an aqueous acid solution, it is preferable that the aqueous acid solution has an acid-to-water weight ratio in the range of 1:1 to 1:10, more preferably in the range of 1:3 to 1:5, and even more preferably in the range of 1:3.9 to 1:4.1.

[0059] Furthermore, when the acid according to (ii') is an aqueous acid solution, it is preferable that the aqueous acid solution has an acid concentration in water in the range of 2.5 to 4.5 mol / L, more preferably in the range of 3.2 to 3.7 mol / L, and even more preferably in the range of 3.3 to 3.6 mol / L.

[0060] Furthermore, where the method further includes (ii'), it is preferred that the acid according to (ii') comprises, preferably consists of, one or more of the following: inorganic acid and organic acid, more preferably one or more of HNO3, HCl, H2SO4, H3PO4, formic acid, oxalic acid, and acetic acid, more preferably HNO3.

[0061] Furthermore, where the method further includes (ii'), preferably, the method is further included after (ii') and before (iii), preferably after (ii') and before (ii'') as defined below.

[0062] (ii'.1) Wash the molded product obtained from (ii') with deionized water.

[0063] Furthermore, where the method further includes (ii'), it is preferred that the method further includes (ii') after and before (iii), preferably after (ii'.1) and before (iii), preferably after (ii'.1) and before (ii'').

[0064] (ii'.2) Dry the molded article obtained by (ii') or (ii'.1) in a gaseous atmosphere.

[0065] When the method further includes (ii'.2), it is preferred that the drying according to (ii'.2) is carried out at a temperature in the range of 80°C to 160°C, more preferably in the range of 100°C to 140°C, and even more preferably in the range of 110°C to 130°C.

[0066] Furthermore, where the method further includes (ii'.2), it is preferred that the drying according to (ii'.2) is carried out for a period of time ranging from 0.5 to 20 hours, more preferably from 2 to 16 hours, and even more preferably from 3 to 12 hours.

[0067] Furthermore, where the method further includes (ii'.2), it is preferred that the gas atmosphere according to (ii'.2) comprises, preferably, one or more of oxygen and nitrogen, more preferably air.

[0068] Furthermore, where the method further includes (ii'), it is preferred that the method further includes

[0069] (ii'') Calcination of the molded article obtained by (ii'), (ii'.1) or (ii'.2) in a gaseous atmosphere.

[0070] When the method further includes (ii''), it is preferred that the calcination according to (ii'') is carried out at a temperature in the range of 400°C to 1200°C, more preferably in the range of 600°C to 950°C, and even more preferably in the range of 825°C to 875°C.

[0071] Furthermore, when the method further includes (ii''), it is preferred that the calcination according to (ii'') lasts for a period of time ranging from 0.1 to 1.5 h, more preferably from 0.3 to 0.7 h, and even more preferably from 0.4 to 0.6 h.

[0072] Furthermore, where the method further includes (ii''), it is preferred that the gas atmosphere according to (ii'') comprises, preferably, one or more of oxygen and nitrogen, more preferably air.

[0073] Preferably, the treatment according to (iii) is achieved by impregnation, more preferably by initial wet impregnation.

[0074] Preferably, the treatment according to (iii) is carried out for a period of time ranging from 0.1 to 12 hours, more preferably from 0.15 to 9 hours, and even more preferably from 0.2 to 6 hours.

[0075] Preferably, the treatment according to (iii) is carried out at a temperature in the range of 0°C to 50°C, more preferably in the range of 10°C to 40°C, and even more preferably in the range of 15°C to 35°C.

[0076] Preferably, the Ru source comprises, and preferably consists of, one or more of the following: Ru nitrosyl salt (more preferably Ru(NO)NO3), Ru halide (preferably RuCl3 hydrate) and Ru acetate.

[0077] Preferably, the alkali metal is selected from the group consisting of Li, Na, K, Rb, Cs and mixtures of two or more thereof, more preferably from the group consisting of K, Cs and mixtures of two or more thereof, wherein the alkali metal is more preferably K or Cs, and wherein the alkali metal is more preferably K.

[0078] Preferably, the alkali metal source comprises, and preferably consists of, one or more of the organic or inorganic salts of the alkali metal, more preferably one or more of the acetate, nitrate, and halide of the alkali metal, preferably an acetate or nitrate.

[0079] Preferably, in the aqueous solution according to (iii), the molar ratio of Ru, calculated as an element, to the alkali metal, calculated as the sum of one or more alkali metals as elements, is in the range of 0.10:1 to 1.00:1, more preferably in the range of 0.20:1 to 0.50:1, and even more preferably in the range of 0.25:1 to 0.45:1.

[0080] Preferably, in (iii), the aqueous solution further comprises an acid, wherein the acid comprises, preferably consists of, one or more of the following: inorganic acid and organic acid, more preferably one or more of HNO3, HCl, H2SO4, H3PO4, formic acid, oxalic acid, and acetic acid, more preferably HNO3.

[0081] In (iii), the aqueous solution further comprises an acid, wherein the acid comprises one or more of an inorganic acid and an organic acid, preferably composed of one or more of an inorganic acid and an organic acid, and preferably, the aqueous solution has an acid-to-water weight ratio in the range of 1:1 to 1:10, more preferably in the range of 1:3 to 1:5, and even more preferably in the range of 1:3.9 to 1:4.1.

[0082] Preferably, the method further includes

[0083] (iv) Drying the molded article obtained by (iii) in a gaseous atmosphere, wherein the drying is more preferably carried out at a temperature in the range of 80°C to 220°C, more preferably 90°C to 200°C, more preferably 100°C to 180°C, wherein the gaseous atmosphere more preferably contains one or more of nitrogen and oxygen, more preferably air.

[0084] Preferably, the method further includes

[0085] (v) Activating the molded article obtained by (iii) or (iv) in a gaseous atmosphere containing hydrogen, wherein the activation is carried out at a temperature in the range of 200°C to 400°C, more preferably 240°C to 360°C, wherein the activation is carried out for a period of time in the range of 0.1 to 48 h, more preferably 0.5 to 36 h, wherein the gaseous atmosphere preferably contains an inert gas, wherein the inert gas is more preferably one or more of Ar and N2, more preferably N2, wherein the gaseous atmosphere more preferably contains 0.01 to 10 vol% H2 in the inert gas, more preferably 0.5 to 6 vol% H2.

[0086] Furthermore, the present invention relates to a catalytic material that is obtained or obtainable by any of the embodiments disclosed herein.

[0087] Preferably, the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material.

[0088] When the catalyst material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, preferably, the support material is selected from M. 1 O, M 2 2O3, M 3 O2, M 4 2O5, M 1 M 2 The group consisting of 2O4 and mixtures of two or more thereof, more preferably selected from M 1 O, M 2 2O3 and M 1 M 2 The group consisting of 2O4, wherein the carrier material is more preferably M. 1 M 2 2O4,

[0089] Where M 1 M represents one or more divalent elements. 2 M represents one or more trivalent elements. 3 M represents one or more tetravalent elements. 4 It represents one or more pentavalent elements.

[0090] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that the support material comprises a crystalline phase having a spinel structure, wherein the crystalline phase having a spinel structure is preferably determined according to Reference Example 1.2.

[0091] Furthermore, when the catalyst material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that M... 1 Elements selected from Groups 2, 10, 11, and 12 of the periodic table, where M... 1 More preferably, it is selected from the group consisting of Mg, Ca, Ni, Cu, Zn, Mn, Co, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Mg, Ni, Cu, Zn, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Mg, Zn, Cu, and mixtures thereof; more preferably, it is selected from the group consisting of Mg, Zn, and mixtures thereof, wherein M 1 More preferably, it is Mg.

[0092] Furthermore, when the catalyst material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that M... 2 Elements selected from Groups 5, 6, 7, 8, and 13 of the periodic table, where M... 2 More preferably, it is selected from the group consisting of Al, Ga, In, Cr, Fe, V, Mn, Co, La, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, Cr, Fe, V, Mn, La, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, La, V, Mn, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, La, and mixtures of two or more thereof, wherein M... 2 More preferably, it is Al.

[0093] Furthermore, when the catalyst material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that M... 3 Elements selected from Groups 4 and 14 of the periodic table, where M... 3 More preferably, it is selected from the group consisting of Si, Ge, Sn, Ti, Zr, Hf, Ce, and mixtures of two or more of them, wherein M 3 More preferably, it is selected from the group consisting of Si, Ti, Zr, Hf, Ce, and mixtures of two or more of them.

[0094] Furthermore, when the catalyst material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that M... 4 Selected from Group 5 of the periodic table, where M 4 More preferably, it is selected from the group consisting of V, Nb, Ta, and mixtures of two or more of them.

[0095] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, preferably, the alkali metal is selected from the group consisting of Li, Na, K, Rb, Cs, and mixtures of two or more thereof, more preferably from the group consisting of K, Cs, and mixtures of two or more thereof, wherein the alkali metal is more preferably K or Cs, and wherein the alkali metal is more preferably K.

[0096] Furthermore, in the case where the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that the catalytic material further comprises: based on M 1 O calculates one or more divalent elements M 1 M 2 One or more trivalent elements M calculated by 2O3 2 M 3 One or more tetravalent elements M calculated by O2 3 M 4 One or more pentavalent elements M calculated using 2O5 4 The total weight of the alkali metal, in elemental form, is 0.5 to 5.0 wt%, more preferably 2.0 to 4.0 wt%, more preferably 2.4 to 3.6 wt%, more preferably 2.6 to 3.4 wt%, and more preferably 3.0 to 3.4 wt%.

[0097] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that the catalytic material comprises: based on M 1 O calculates one or more divalent elements M 1 M 2 One or more trivalent elements M calculated by 2O3 2 M 3 One or more tetravalent elements M calculated by O2 3 M 4 One or more pentavalent elements M calculated using 2O5 4 The total weight of Ru, in elemental form, is 0.5 to 5 wt%, more preferably 1.0 to 3.0 wt%, more preferably 1.4 to 2.6 wt%, more preferably 1.6 to 2.4 wt%, and more preferably 1.8 to 2.2 wt%.

[0098] Furthermore, when the catalyst material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are loaded on the support material, it is preferable that the support material has a total pore volume in the range of 0.10 to 0.90 ml / g, more preferably in the range of 0.18 to 0.75 ml / g, more preferably in the range of 0.25 to 0.60 ml / g, more preferably in the range of 0.33 to 0.53 ml / g, more preferably in the range of 0.37 to 0.49 ml / g, and more preferably in the range of 0.40 to 0.46 ml / g, wherein the total pore volume is preferably determined according to Reference Example 1.4.

[0099] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are loaded on the support material, it is preferable that the support material has a crystallinity in the range of 50% to 100%, more preferably 60% to 100%, more preferably 70% to 95%, and more preferably 80% to 90%, wherein the crystallinity is preferably determined according to Reference Example 1.2.

[0100] When the carrier material has a crystallinity in the range of 50% to 100%, it is preferred that 50% to 100%, more preferably 70% to 100%, and even more preferably 95% to 100% of the crystalline phase has a spinel structure as determined by XRD, preferably as determined according to Reference Example 1.2.

[0101] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are loaded on the support material, it is preferable that the X-ray diffraction pattern exhibited by the catalytic material includes at least the following reflections:

[0102]

[0103] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0104] More preferably, it includes at least the following reflections:

[0105]

[0106] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0107] More preferably, it includes at least the following reflections:

[0108]

[0109] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0110] Where M 1 More preferably Mg and wherein M 2 More preferably, it is Al.

[0111] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are loaded on the support material, it is preferable that the support material has a median pore size in the range of 0.001 to 0.1 µm, more preferably in the range of 0.005 to 0.05 µm, more preferably in the range of 0.02 to 0.04 µm, more preferably in the range of 0.027 to 0.035 µm, and more preferably in the range of 0.028 to 0.034 µm, wherein the pore size distribution is preferably determined according to Reference Example 1.5.

[0112] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are loaded on the support material, it is preferable that the support material has a water adsorption capacity in the range of 10 to 80 wt%, more preferably in the range of 30 to 60 wt%, more preferably in the range of 40 to 50 wt%, and even more preferably in the range of 43 to 47 wt%, wherein the water adsorption capacity is preferably determined according to Reference Example 1.1.

[0113] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that the support material has a thickness of 20.0 to 150.0 m. 2 Within the range of / g, more preferably from 30.0 to 90.0 m 2 Within the range of / g, more preferably from 40.0 to 65.0 m 2 Within the range of / g, more preferably from 45.0 to 55.0 m 2 The BET specific surface area within the range of / g, wherein the BET specific surface area is preferably determined according to Reference Example 1.3.

[0114] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are loaded on the support material, it is preferable that Ru is uniformly dispersed throughout the catalytic material.

[0115] Furthermore, when the catalyst material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are supported on the support material, it is preferable that the alkali metal M... 3 It is uniformly dispersed throughout the catalytic material.

[0116] Furthermore, when the catalytic material comprises Ru, an alkali metal, and a support material, wherein Ru and the alkali metal are loaded on the support material, preferably, 85 to 100 wt%, preferably 90 to 100 wt%, more preferably 95 to 100 wt%, more preferably 98 to 100 wt%, more preferably 99 to 100 wt%, and more preferably 99.9 to 100 wt%, of the catalytic material is composed of the support material, Ru, and the alkali metal.

[0117] Preferably, the catalytic material is in the form of an extrusion, tablet, or granules.

[0118] When the catalytic material is in the form of an extrusion, tablet, or granules, it is preferred that the extrusion or tablet has a cross-section, wherein the cross-section is circular, hexagonal, rectangular, square, triangular, elliptical, star-shaped polygon, or clover-shaped, preferably circular, hexagonal, rectangular, square, triangular, elliptical, star-shaped polygon with 3, 4, 5, 6, 7, or 8 apexes, clover-shaped, four-leaf-shaped, or hexalobed, more preferably circular, hexagonal, rectangular, square, triangular, elliptical, star-shaped polygon with 3 or 4 apexes, clover-shaped, four-leaf-shaped, or hexalobed.

[0119] Preferably, the catalytic material is in the form of a tablet with a cross section, wherein the cross section is tetralobed.

[0120] When the catalytic material is in the form of a tablet with a cross-section, wherein the cross-section is tetralobed, it is preferable that the tablet has a thickness, wherein the thickness is in the range of 2.0 to 13.0 mm, more preferably in the range of 5.0 to 10.0 mm, and even more preferably in the range of 6.5 to 9.0 mm.

[0121] When the catalytic material is in the form of a tablet with a cross-section, wherein the cross-section is tetralobed, it is preferable that the tablet has a diameter D in the range of 5 to 20 mm, more preferably in the range of 7 to 17 mm, and even more preferably in the range of 9 to 15 mm.

[0122] Preferably, the catalytic material is in the form of a tablet with a cross-section, wherein the cross-section is hexagonal.

[0123] When the catalytic material is in the form of a tablet with a cross-section, wherein the cross-section is hexagonal, it is preferable that the tablet has a thickness, wherein the thickness is in the range of 2.0 to 15.0 mm, more preferably in the range of 5.0 to 12.0 mm, and even more preferably in the range of 8.0 to 9.0 mm.

[0124] When the catalytic material is in the form of a tablet with a cross-section, wherein the cross-section is hexagonal, it is preferable that the tablet has a diameter D in the range of 5 to 25 mm, more preferably in the range of 12 to 19 mm, and even more preferably in the range of 14 to 17 mm.

[0125] Furthermore, when the catalytic material is in the form of an extrusion, tablet, or granules, it is preferable that the catalytic material is in the form of an extrusion with a cross section, wherein the cross section is circular, star-shaped polygonal, or trilobal.

[0126] When the catalytic material is in the form of an extrusion with a cross section, wherein the cross section is circular, star-shaped, polygonal, or trilobal, it is preferable that the extrusion has a thickness, wherein the thickness is in the range of 1.0 to 12.0 mm, more preferably in the range of 1.5 to 10.0 mm, and even more preferably in the range of 2.0 to 8.0 mm.

[0127] Furthermore, when the catalytic material is in the form of an extrusion with a cross section, wherein the cross section is circular, star-shaped, polygonal, or trilobal, it is preferable that the extrusion has a diameter, wherein the diameter is in the range of 1 to 20 mm, more preferably in the range of 2 to 18 mm, and even more preferably in the range of 3 to 16 mm.

[0128] Furthermore, the present invention relates to a method for converting NH3 into H2 and N2, the method comprising:

[0129] (A) Providing a reactor containing a catalytic material according to any one of the embodiments disclosed herein;

[0130] (B) Prepare a feed gas stream containing NH3;

[0131] (C) The feed gas stream prepared in (B) is fed into the reactor provided in (A) and the feed gas stream is brought into contact with the catalyst material, wherein the contact is carried out at a pressure greater than 10 absolute bar and at a temperature in the range of 200°C to 650°C;

[0132] (D) Remove the effluent gas stream from the reactor, which contains H2 and N2.

[0133] Preferably, the contact is carried out at a pressure in the range of 11 to 50 bar, more preferably 15 to 40 bar, and even more preferably 19 to 31 bar.

[0134] Preferably, the contact is carried out at a temperature in the range of 250°C to 650°C, more preferably 275°C to 625°C, and even more preferably 300°C to 600°C.

[0135] Preferably, the feed gas stream prepared in (B) contains 1 to 100 vol.-%, more preferably 3 to 99.99 vol.-%, more preferably 5 to 99.95 vol.-%, more preferably 10 to 99.9 vol.-%, more preferably 20 to 99.8 vol.-%, more preferably 30 to 99.7 vol.-%, more preferably 40 to 99.6 vol.-%, and more preferably 50 to 99.5 vol.-%.

[0136] Preferably, the feed gas stream prepared in (B) contains 0 to 50 vol.-%, more preferably 0.01 to 30 vol.-%, more preferably 0.03 to 15 vol.-%, more preferably 0.05 to 5 vol.-%, more preferably 0.1 to 1 vol.-%, more preferably 0.12 to 0.5 vol.-%, and more preferably 0.14 to 0.16 vol.-%. of N2.

[0137] Preferably, the feed gas stream prepared in (B) contains 0 to 75 vol.-%, more preferably 0 to 60 vol.-%, more preferably 0 to 50 vol.-%, more preferably 0 to 40 vol.-%, more preferably 0 to 35 vol.-%, and more preferably 0 to 30 vol.-%. of H2.

[0138] Preferably, the feed gas stream prepared in (B) contains 100 to 50,000 ppmv, preferably 200 to 30,000 ppmv, more preferably 500 to 25,000 ppmv, more preferably 500 to 20,000 ppmv, more preferably 500 to 15,000 ppmv, more preferably 750 to 15,000 ppmv, more preferably 1,000 to 11,000 ppmv, more preferably 1,000 to 10,000 ppmv, more preferably 2,000 to 8,000 ppmv, more preferably 3,000 to 7,500 ppmv, more preferably 4,500 to 7,000 ppmv, more preferably 5,000 to 6,500 ppmv of H2O.

[0139] Preferably, the total amount of NH3, N2 and H2 contained in the feed gas stream prepared in (B) is in the range of 90 to 100 wt.-%, more preferably 95 to 99.95 vol.-%, more preferably 98 to 99.9 vol.-%, more preferably 99 to 99.85 vol.-%, and more preferably 99.7 to 99.8 vol.-%.

[0140] Preferably, the feed stream is supplied at a rate of 500 to 20,000 h.-1 More preferably 500 to 16,000 h -1 More preferably 700 to 14,000 h -1 More preferably 800 to 12,000 h -1 More preferably 900 to 10,000 h -1 More preferably 1,000 to 8,000 h -1 And more preferably 3,000 to 5,000 h -1 The gas hourly space velocity within the range is fed into the reactor.

[0141] Furthermore, the present invention relates to the use of the catalytic material according to any one of the embodiments disclosed herein for the conversion of NH3 into H2 and N2.

[0142] Furthermore, the present invention relates to a method, preferably according to any one of the embodiments disclosed herein, the method comprising the step of converting H2 that is available or obtained according to (D) of any one of the embodiments disclosed herein to obtain product Ω.

[0143] Preferably, the product Ω is selected from:

[0144] -Building unit or monolith; or

[0145] -A polymer (preferably polymer A), a polymer composition (preferably polymer composition A), or a polymer product (preferably polymer product A); or

[0146] - Cleaning polymers, cleaning surfactants, descaling compounds, cleaning biocides, or combinations thereof or formulations thereof; or

[0147] -Agricultural chemical compositions, agricultural chemical formulations, adjuvants, or agricultural chemical active ingredients; or

[0148] - Active pharmaceutical ingredient or its intermediate, pharmaceutical excipient, animal feed additive, human food additive, dietary supplement, aromatic chemical or aromatic composition; or

[0149] - Aqueous polymer dispersions, preferably polyurethane or polyurethane-poly(meth)acrylate hybrid polymer dispersions, emulsions, binders for paper and fiber coatings, UV-curable acrylic polymers for hot melts and coatings, polyisocyanates, hyperbranched polyester polyols, polymer dispersants for inorganic binder compositions, unsaturated polyester polyols, or 100% curable compositions; or

[0150] - Cosmetic surfactants, emollients, waxes, cosmetic polymers, UV filters, other cosmetic ingredients, or combinations thereof or formulations thereof; or

[0151] - Polymer B, polymer composition B, coating composition, other functional composition, foil, molded body, coating or coated substrate.

[0152] Preferably, the product Ω contains 1 wt% or more, more preferably 2 wt% or more, more preferably 5 wt% or more, more preferably 15 wt% or more, more preferably 30 wt% or more, more preferably 40 wt% or more, more preferably 60 wt% or more, more preferably 80 wt% or more, more preferably 90 wt% or more, more preferably 95 wt% or more; and / or

[0153] The product Ω contains H2 that is obtainable or acquireable according to (D) of any one of the embodiments disclosed herein, in an amount of 100 wt% or less, more preferably 95 wt% or less, more preferably 90 wt% or less, more preferably 50 wt% or less, more preferably 25 wt% or less, more preferably 10 wt% or less; and

[0154] More preferably, the content is determined based on identity preservation and / or segregation and / or mass balance and / or book and embodiment chain of custody models, preferably based on mass balance, and preferably according to the International Sustainability and Carbon Certification (ISCC) standard.

[0155] The publicly disclosed prior art content; No. 684; paragraphs

[1000] to

[8005] ; ISSN: 2198-4786; publication date: February 12, 2024, shall be regarded as reference RF1, which is incorporated herein by reference in its entirety. Preferably, the product Ω is the product as described in reference RF1; paragraphs

[1000] to

[8005] . Preferably, the method described herein is further a method for producing the product.

[0156] The conversion step for obtaining product Ω preferably includes one or more steps as described below, and can be performed by conventional methods well known to those skilled in the art. The conversion step preferably includes one or more steps selected from the following:

[0157] Recycling, preferably through depolymerization, gasification, pyrolysis and / or steam cracking; and / or

[0158] Purification, preferably crystallization, (solvent) extraction, distillation, evaporation, hydrogenation, absorption, adsorption, and / or ion exchange; and / or

[0159] Assembling, preferably foaming, synthesis, chemical transformation, chemical conversion, polymerization and / or blending; and / or

[0160] Molding, preferably foaming, extrusion and / or molding; and / or

[0161] Finishing, preferably coating and / or smoothing.

[0162] Additionally, one or more of these steps are described in detail in reference RF1; paragraphs

[1000] through

[8005] .

[0163] As used in the context of product Ω herein, the term "building unit" includes compounds in a gaseous or liquid state under standard conditions of 0°C and 0.1 MPa. Building units are typically used in the chemical industry to form secondary products that offer greater structural complexity and / or higher molecular weight than the building unit upon which the secondary product is based. Building units are preferably selected from the group consisting of free hydrogen, carbon monoxide, carbon dioxide, ethylene oxide, ethylene glycol, syngas containing mixtures of hydrogen and carbon monoxide, alkanes, alkenes, alkynes, and aromatic compounds. Alkanes, alkenes, alkynes, and aromatic compounds particularly contain 1 to 12 carbon atoms, respectively.

[0164] As used in the context of the product Ω herein, the term "monomer" includes molecules that can react with each other to form polymer chains by polymerization. Monomers are preferably selected from the group consisting of: (meth)acrylic acid, salts of (meth)acrylic acid; particularly sodium, potassium, and zinc salts; (meth)acrylaldehyde and (meth)acrylates. (Meth)acrylates containing 1 to 22 carbon atoms, particularly 1 to 8 carbon atoms, are preferred. The terms (meth)acrylic acid, (meth)acrylaldehyde, or (meth)acrylate refer to acrylic acid, acrolein, or acrylates, and where applicable, also refer to methacrylic acid, methacrolein, or methacrylates. Further, monomers may be selected from hexamethylenediamine (HMD) and adipic acid.

[0165] The building blocks may further be intermediate compounds. As used in the context of the product Ω herein, the term "intermediate compound" includes organic reagents that are used to form compounds with higher molecular complexity. Intermediate compounds may, for example, be selected from the group consisting of phosgene, polyisocyanates, and propylene oxide. Polyisocyanates are particularly aromatic diisocyanates and polyisocyanates, preferably toluene diisocyanate (TDI) and / or diphenylmethane diisocyanate (MDI).

[0166] The building blocks and monomers, as well as one or more typical transformation steps used to obtain the building blocks or monomers, are described in more detail in paragraphs

[1000] through

[1012] of reference RF1.

[0167] As used in the context of product Ω herein, the term “polymer A” includes thermoplastics (e.g., polyamides or thermoplastic polyurethanes), thermosettings (e.g., polyurethanes), elastomers (e.g., polybutadiene) or copolymers or mixtures thereof, and is defined in more detail in paragraphs

[2001] through

[2007] of reference RF1.

[0168] As used in the context of product Ω herein, the term “polymer composition A” includes all compositions comprising the polymer as described above and one or more additives (e.g., reinforcing agents, colorants, modifiers and / or flame retardants), and is defined in more detail in paragraph

[2008] of reference RF1.

[0169] As used in the context of product Ω herein, the term “polymer product A” includes any product comprising polymer A and / or polymer composition A as described above, and is defined in more detail in paragraphs

[2009] and

[2010] of reference RF1.

[0170] One or more steps for obtaining a polymer (preferably polymer A), a polymer composition (preferably polymer composition A), or a polymer product (preferably polymer product A) are described in more detail in paragraph

[2011] of reference RF1.

[0171] As used in the context of this product Ω, the term "industrial polymer" includes rheological polymers based on polycarboxylate, alkoxylated polyalkyleneamine, alkoxylated polyalkyleneimide, polyether, dye-inhibiting and dirt-releasing cleaning polymers, as defined in more detail in paragraphs

[3035] through

[3044] of reference RF1. As used in the context of this product Ω, the term "industrial surfactant" includes nonionic, anionic, and amphoteric industrial surfactants, as defined in more detail in paragraphs

[3008] through

[3034] of reference RF1. As used in the context of this product Ω, the term "industrial descaling compound" includes nonphosphate-based detergent builders (NPB) and phosphonates (CoP), as described in more detail in paragraphs

[3001] through

[3005] of reference RF1. As used in the context of this product Ω, the term "industrial biocide" refers to compounds that kill or inhibit the growth or reproduction of microorganisms, as defined in more detail in paragraphs

[3006] through

[3007] of reference RF1. As used in the context of product Ω herein, the term “industrial solvent” includes alkylamides, alkyl lactamides, alkyl esters, lactates, alkyl diesters, cyclic alkyl diesters, cyclic carbonates, aromatic aldehydes, and aromatic esters, as defined in more detail in paragraphs

[3045] through

[3055] of reference RF1. As used in the context of product Ω herein, the term “industrial dispersant” includes anionic and nonionic industrial dispersants, as defined in more detail in paragraphs

[3056] through

[3058] of reference RF1. The term “compositions and / or formulations thereof” with respect to industrial polymers, industrial surfactants, scale-removing compounds, and / or industrial biocides refers to industrial compositions and / or institutional products and / or textile and household care products and / or personal care products, as defined in more detail in paragraph

[3059] of reference RF1. One or more conversion steps for obtaining industrial polymers, industrial surfactants, scale-removing compounds, and / or industrial biocides are defined in more detail in paragraph

[3060] of reference RF1. The conversion steps for obtaining industrial compositions or formulations of industrial polymers, industrial surfactants, scale-removing compounds and / or industrial biocides are defined in more detail in paragraph

[3061] of reference RF1.

[0172] As used in the context of the product Ω herein, the term "agrochemical composition" typically refers to a composition comprising an agrochemical active ingredient and at least one agrochemical formulation adjuvant. Examples of agrochemical compositions, active ingredients, and adjuvants are described in more detail in paragraph

[4001] of reference RF1.

[0173] Agricultural chemical compositions can be in any conventional formulation form. These agricultural chemical compositions are prepared in known ways, for example, as described in: Mollet and Grubemann, Formulation technology, Wiley VCH, Weinheim, 2001; or Knowles, New developments in crop protection product formulation, Agrow Reports DS243, T&F Informa, London, 2005. One or more conversion steps to obtain agricultural chemical active ingredients and adjuvants can be similar to one or more production steps of their analogues based on petrochemicals or other precursors not obtained through recycling processes. Additionally, the conversion of compounds mentioned in the sections “Polymers” and “Cosmetic Surfactants, Emollients, Waxes, Cosmetic Polymers, UV Filters, Other Cosmetic Ingredients or Combinations or Formulations thereof” can be carried out as described in those sections and the corresponding paragraphs in reference RF1.

[0174] As used in the context of product Ω herein, the terms active pharmaceutical ingredient and / or intermediate thereof include substances that provide pharmacological activity or other direct action in the diagnosis, cure, relief, treatment, or prevention of a disease, or that affect the structure or any function of the body. Intermediates are isolated products generated during a multi-step synthetic route of the active pharmaceutical ingredient. As used in the context of product Ω herein, the term pharmaceutical excipient includes compounds or mixtures of compounds used in compositions for various pharmaceutical applications that are substantially non-pharmaceutical in themselves. Active pharmaceutical ingredients and / or intermediates thereof, as well as pharmaceutical excipients, are defined in more detail in paragraph

[5001] of reference RF1.

[0175] One or more conversion steps for obtaining an active pharmaceutical ingredient and / or its intermediates and pharmaceutical excipients may include one or more synthetic steps and may be carried out by conventional synthesis and techniques well known to those skilled in the art.

[0176] As used in the context of the product Ω herein, the terms animal feed additive, human food additive, and dietary supplement include vitamins, provitamins, and their active metabolites, including intermediates and precursors, especially vitamins A, B, E, D, K and their esters (like acetate, propionate, palmitate) or their alcohols (like retinol) or their salts or any combination thereof; tetraterpenes, especially isoprene-like compounds, like carotenoids and lutein, including their intermediates and precursors and mixtures and derivatives thereof, especially β-carotene, canthaxanthin, hesperidin, astaxanthin, zeaxanthin, lutein, lycopene, apocarotenoids, and any combination thereof; Organic acids, especially formic acid, propionic acid and their salts (such as sodium, calcium or ammonium salts) and any combination thereof, such as, but not limited to, formic acid and sodium formate, propionic acid and ammonium propionic acid, formic acid and propionic acid, formic acid and sodium formate, and mixtures of propionic acid, propionic acid and sodium propionic acid and formic acid and sodium formate; glycerides of carboxylic acids and short and medium chain fatty acids, conjugated linoleic acid (such as omega-6 fatty acid (C18:2) methyl esters) and 1,2-propanediol; and beverage stabilizers such as polyvinylpyrrolidone polymers or polyvinylimazole / polyvinylpyrrolidone copolymers. Animal feed additives, human food additives and dietary supplements are defined in more detail in paragraph

[5002] of reference RF1.

[0177] One or more conversion steps used to obtain animal feed additives, human food additives, or dietary supplements may include one or more synthetic steps and may be carried out by conventional synthesis and techniques well known to those skilled in the art.

[0178] As used in the context of the product Ω herein, the terms aromatic chemicals and aromatic compositions include volatile organic compounds with a molecular weight between 70 and 250 g / mol, including those with a carbon skeleton of C5-C6. 16 Functional groups of carbon atoms, the carbon skeleton including straight chains, branches, and rings (e.g., rings with a size of C5-C). 18 The aromatic chemicals are bicyclic or tricyclic aliphatic chains, but do not necessarily contain one or more unsaturated structural elements such as double bonds, triple bonds, aromatic or heteroaromatic groups, and preferably, one or more additional functional groups are selected from alcohols, ethers, esters, ketones, aldehydes, acetals, carboxylic acids, nitriles, thiols, and amines. In one aspect, aromatic chemicals are terpenoid-based aromatic chemicals, such as those selected from monoterpenes and monoterpenoids, sesquiterpenes and sesquiterpenoids, diterpenes, triterpenes, or tetraterpenes. Aromatic chemicals can be combined with other aromatic chemicals to obtain aromatic compositions. Aromatic chemicals and aromatic compositions are defined in more detail in paragraph

[5003] of reference RF1.

[0179] One or more conversion steps for obtaining aromatic chemicals and aromatic compositions may include one or more synthetic steps and may be carried out by conventional synthesis and techniques well known to those skilled in the art.

[0180] As used in the context of product Ω herein, the term "aqueous polymer dispersion" includes one or more aqueous compositions comprising one or more dispersed polymers, and is defined in more detail in the section entitled "Aqueous Polymer Dispersions" of reference RF1

[6001] . One or more dispersed polymers may be selected from one or more acrylic emulsion polymers, one or more styrene acrylic emulsion polymers, one or more styrene butadiene dispersions, one or more aqueous dispersions comprising composite particles, one or more acrylate alkyd hybrid dispersions, one or more polyurethanes (including UV-curable polyurethanes), and one or more polyurethane-poly(meth)acrylate hybrid polymers. As used in the context of product Ω herein, the term "emulsion polymer" includes one or more polymers prepared by free radical emulsion polymerization. One or more aqueous polyurethane dispersions are defined in more detail in the section entitled "Polyurethane Dispersions" of reference RF1

[6002] . One or more UV-curable polyurethanes are defined in more detail in the section of reference RF1

[6017] . One or more polyurethane-poly(meth)acrylate hybrid polymers are defined in more detail in section

[6016] of reference RF1.

[0181] As used in the context of product Ω herein, the term “polymer dispersant” preferably includes one or more polymers comprising polyether side chains, particularly one or more polycarboxylate ether polymers and one or more condensation products as defined in more detail in the paragraph entitled “Polymer Dispersants” in reference RF1

[6020] .

[0182] One or more conversion (polymerization) steps for obtaining one or more aqueous polymer dispersions comprising one or more emulsion polymers are defined in more detail in the section entitled “Emulsion Polymerization” in reference RF1

[6003] .

[0183] One or more conversion (polymerization) steps for obtaining one or more waterborne polyurethane dispersions are defined in more detail in the section entitled “Methods for preparing waterborne polyurethane dispersions”

[6014] and the section entitled “UV-curable waterborne polyurethane dispersions, their preparation and use and compositions containing them”

[6017] of reference RF1.

[0184] Compositions and uses of one or more aqueous polymer dispersions and one or more polymer dispersants are defined in more detail in the following sections of reference RF1:

[0185] The section titled "Applications of Aqueous Polymer Dispersions"

[6004] ,

[0186] The section titled "Adhesives for Building and Construction Coatings"

[6005]

[0187] The section titled "Adhesives for Paper Coatings"

[6006]

[0188] The section titled "Adhesives for Fiber Bonding"

[6007]

[0189] The section titled "Adhesive Polymers and Adhesive Compositions"

[6008]

[0190] The section titled "Aqueous Polyurethane Dispersions Suitable for Coating Compositions"

[6015]

[0191] The section titled "Waterborne polyurethane-poly(meth)acrylate hybrid polymer dispersions suitable for coating compositions"

[6016]

[0192] The section titled "Waterborne UV-curable polyurethane dispersions, their preparation and uses, and compositions containing them"

[6017]

[0193] Section entitled “Inorganic binder compositions containing polymer dispersants and their uses”

[6018]

[6019] 100% curable coating compositions.

[0194] One or more UV-crosslinkable poly(meth)acrylates and their uses are defined in more detail in the section entitled “UV-crosslinkable poly(meth)acrylates for UV-curable solvent-free hot melt adhesives and their use in the preparation of pressure-sensitive self-adhesive articles” in reference RF1

[6009] .

[0195] One or more polyisocyanates, one or more compositions comprising them, and their uses are defined in more detail in the section entitled “Polyisocyanates” in reference RF1

[6010] .

[0196] One or more hyperbranched polyester polyols and their uses are defined in more detail in the section entitled "Organic solvent-based hyperbranched polyester polyols suitable for coating compositions" in reference RF1

[6011] . One or more conversion steps for obtaining hyperbranched polyester polyols are defined in more detail in the section entitled "Preparation of organic solvent-based hyperbranched polyester polyols" in reference RF1

[6012] . One or more coating compositions comprising one or more hyperbranched polyester polyols, one or more polyisocyanates and one or more additives, and the substrates coated thereon are defined in more detail in the section entitled "Organic solvent-based two-component coating compositions comprising hyperbranched polyester polyols and polyisocyanates" in reference RF1

[6013] .

[0197] One or more unsaturated polyester polyols, one or more solvent-based coating compositions comprising said one or more unsaturated polyester polyols, and one or more substrates for coating with said one or more coating compositions are defined in more detail in the section entitled “Organic solvent-based coating compositions comprising unsaturated polyester polyols” in reference RF1

[6018] .

[0198] One or more 100% curable coating compositions are defined in more detail in section

[6019] of reference RF1.

[0199] One or more polymeric dispersants for use in inorganic binder compositions are defined in more detail in section

[6020] of reference RF1. One or more inorganic binder compositions containing polymeric dispersants and their uses are defined in more detail in section

[6021] of reference RF1. One or more conversion steps for obtaining one or more polymeric dispersants are defined in more detail in section

[6020] of reference RF1. The term “inorganic binder composition” containing one or more polymeric dispersants, as used in the context of the product Ω herein, preferably includes, in particular, hydraulic coagulation compositions and compositions containing calcium sulfate, and is defined in more detail in section

[6021] of reference RF1 entitled “Inorganic Binder Compositions Containing Polymer Dispersants and Their Uses Therein.” Specific one or more building material formulations containing one or more polymeric dispersants, or one or more building products produced from building material formulations containing polymeric dispersants, are disclosed in more detail in section

[6021] of reference RF1.

[0200] As used in the context of this product Ω, the term "cosmetic surfactant" includes nonionic, anionic, cationic, and amphoteric surfactants, and is defined in more detail in paragraph

[7002] of reference RF1. As used in the context of this product Ω, the term "emollient" refers to a compound used to protect, moisturize, and / or lubricate the skin, and is defined in more detail in paragraph

[7003] of reference RF1. As used in the context of this product Ω, the term "wax" includes pearlescent agents and opacifiers, and is defined in more detail in paragraph

[7004] of reference RF1. As used in the context of this product Ω, the term "cosmetic polymer" includes any polymer that can be used as an ingredient in cosmetic formulations, and is defined in more detail in paragraph

[7005] of reference RF1. As used in the context of this product Ω, the term "UV filter" refers to a compound that blocks or absorbs ultraviolet light, and is defined in more detail in paragraph

[7006] of reference RF1.

[0201] As used in the context of product Ω herein, the term “additional cosmetic ingredient” includes any ingredient suitable for the preparation of cosmetic formulations. Several sources disclose ingredients acceptable for cosmetics. For example, the database Cosing on the European Commission’s internet page discloses cosmetic ingredients, and the International Dictionary and Handbook of Cosmetic Ingredients edited by the Personal Care Products Association (PCPC) discloses cosmetic ingredients. The term “compositions and / or formulations thereof” with respect to cosmetic surfactants, emollients, waxes, cosmetic polymers, UV filters and / or other cosmetic ingredients refers to personal care and / or cosmetic compositions or formulations as defined in more detail in paragraph

[7007] of reference RF1. One or more conversion steps used to obtain cosmetic surfactants, emollients, waxes, cosmetic polymers, UV filters or other cosmetic ingredients are defined in more detail in paragraph

[7008] of reference RF1.

[0202] The terms “polymer B”, “polymer composition B”, “coating composition”, “other functional composition”, “foil”, “molded body”, “coating” and “coated substrate” are well known to those skilled in the art and are defined in more detail from paragraphs

[8000] to

[8005] of reference RF1.

[0203] The unit absolute pressure bar refers to absolute pressure, where 1 bar equals 10 5 Pa.

[0204] The invention is further illustrated by the following set of embodiments and combinations of embodiments derived from the dependent relationships and reverse references shown. In particular, it should be noted that in each instance of reference to a series of embodiments, such as in the context of the term "method as described in any one of Embodiments 1 to 4," each embodiment in this series is intended to clearly disclose to those skilled in the art that the wording of this term should be understood by those skilled in the art to be synonymous with "method as described in any one of Embodiments 1, 2, 3, and 4." Furthermore, it should be clearly noted that the following set of embodiments represents appropriate structural portions of the general description of preferred aspects of the invention and therefore appropriately supports, but does not represent, the claims of the invention.

[0205] 1. A method for preparing a catalytic material, the method comprising:

[0206] (i) Molding a mixture containing one or more carrier material sources;

[0207] (ii) Calcine the molded article obtained by (i) in a gaseous atmosphere to obtain a molded article containing a carrier material;

[0208] (iii) Impregnate the molded article with an aqueous solution containing both a Ru source and an alkali metal source.

[0209] 2. The method as described in Example 1, wherein the one or more carrier material sources are selected from the group consisting of: M 1 O source, M 2 2O3 source, M 3 O2 source, M 4 O2O5 source and mixtures of two or more of them,

[0210] The one or more carrier material sources are preferably selected from the group consisting of: M 1 O source, M 2 2O3 source, M 3 O2 sources and mixtures of two or more of them,

[0211] The source of one or more carrier materials is more preferably selected from the group consisting of: M 1 O source, M 2 O2 source and mixtures of two or more of them,

[0212] More preferably, the one or more carrier materials source is M. 1 O source and M 2 The source is composed of 2O3, wherein the one or more carrier materials source are more preferably composed of M 1 O and M 2 2O3 source composition,

[0213] Where M 1 M represents one or more divalent elements. 2 M represents one or more trivalent elements. 3 M represents one or more tetravalent elements. 4 It represents one or more pentavalent elements.

[0214] 3. The method as described in Example 1 or 2, wherein the one or more carrier material sources comprise one or more compounds selected from the group consisting of, preferably, oxides, hydroxides, carbonates, nitrates, bicarbonates, hydroxycarbonates, M 1 and M 2 Mixed metal oxides, M 1 and M 3 Mixed metal oxides, M 1 and M 4 Mixed metal oxides, M 2 and M 3 Mixed metal oxides, M 2 and M 4 Mixed metal oxides, M 3 and M 4 Mixed metal oxides, M 1 and M 2 Mixed metal hydroxy carbonates, M1 and M 3 Mixed metal hydroxy carbonates, M 1 and M 4 Mixed metal hydroxy carbonates, M 2 and M 3 Mixed metal hydroxy carbonates, M 2 and M 4 Mixed metal hydroxy carbonates, M 3 and M 4 Mixed metal hydroxy carbonates and mixtures of two or more of them.

[0215] 4. The method as described in any one of Examples 1 to 3, wherein the one or more carrier material sources comprise M 1 O source and M 2 O2 source.

[0216] 5. The method as described in Example 4, wherein the M 1 O source and the M 2 The 2O3 source comprises one or more compounds selected from the group consisting of, preferably, M 1 and M 2 Mixed metal oxides, M 1 and M 2 Mixed metal hydroxy carbonates and their mixtures.

[0217] 6. The method as described in Example 4 or 5, wherein the M 1 O source and the M 2 The 2O3 source has an M content in the range of 1:10 to 10:1.0, preferably in the range of 1:2.5 to 2.5:1, more preferably in the range of 1:2 to 2:1, and even more preferably in the range of 1:2.1 to 1:1.9. 1 With M 2 The molar ratio.

[0218] 7. The method as described in any one of Examples 4 to 6, wherein the M 1 O source and the M 2 2O3 source contains based on contained in M 1 O source and the M 2 M in 2O3 source 1 O calculation of M 1 and with M 2 M calculated from 2O3 2 The total weight, 10 to 34 wt%, preferably 25 to 31 wt%, more preferably 27 to 29 wt%, in M 1 O calculation of M 1 .

[0219] 8. The method as described in any one of Examples 4 to 7, wherein the M 1 O source and the M 2 2O3 source contains based on contained in M 1 O source and the M 2 M in 2O3 source 1 O calculation of M 1 and with M 2 M calculated from 2O3 2 The total weight, 66 to 90% by weight, preferably 69 to 75% by weight, more preferably 71 to 73% by weight, in M 2 M calculated from 2O3 2 .

[0220] 9. The method as described in any one of Examples 1 to 8, wherein the carrier material is selected from M. 1 O, M 2 2O3, M 3 O2, M 4 2O5, M 1 M 2 The group consisting of 2O4 and mixtures of two or more thereof, preferably selected from M 1 O, M 2 2O3 and M 1 M 2 The group consisting of 2O4, wherein the carrier material is more preferably M. 1 M 2 2O4,

[0221] Where M 1 M represents one or more divalent elements. 2 M represents one or more trivalent elements. 3 M represents one or more tetravalent elements. 4 It represents one or more pentavalent elements.

[0222] 10. The method as described in any one of Examples 2 to 9, wherein M 1 Elements selected from Groups 2, 10, 11, and 12 of the periodic table, where M... 1 Preferably, it is selected from the group consisting of Mg, Ca, Ni, Cu, Zn, Mn, Co, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Mg, Ni, Cu, Zn, and mixtures of two or more thereof; even more preferably, it is selected from the group consisting of Mg, Zn, Cu, and mixtures thereof; even more preferably, it is selected from the group consisting of Mg, Zn, and mixtures thereof, wherein M 1 More preferably, it is Mg.

[0223] 11. The method as described in any one of Examples 2 to 10, wherein M 2 Elements selected from Groups 5, 6, 7, 8, and 13 of the periodic table, where M... 2 Preferably, it is selected from the group consisting of Al, Ga, In, Cr, Fe, V, Mn, Co, La, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, Cr, Fe, V, Mn, La, and mixtures of two or more thereof; even more preferably, it is selected from the group consisting of Al, La, V, Mn, and mixtures of two or more thereof; even more preferably, it is selected from the group consisting of Al, La, and mixtures of two or more thereof, wherein M... 2 More preferably, it is Al.

[0224] 12. The method as described in any one of Examples 2 to 11, wherein M 3 Elements selected from Groups 4 and 14 of the periodic table, where M... 3 Preferably, it is selected from the group consisting of Si, Ge, Sn, Ti, Zr, Hf, Ce, and mixtures of two or more of them, wherein M 3 More preferably, it is selected from the group consisting of Si, Ti, Zr, Hf, Ce, and mixtures of two or more of them.

[0225] 13. The method as described in Example 12, wherein M 3 It does not contain carbon.

[0226] 14. The method as described in any one of Examples 2 to 13, wherein M 4 Selected from Group 5 of the periodic table, where M 4 Preferably, it is selected from the group consisting of V, Nb, Ta, and mixtures of two or more of them.

[0227] 15. The method as described in any one of Examples 1 to 14, wherein the X-ray diffraction pattern exhibited by the molded article obtained by (ii) includes at least the following reflections:

[0228]

[0229] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0230] Preferably, it includes at least the following reflections:

[0231]

[0232] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0233] More preferably, it includes at least the following reflections:

[0234]

[0235] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0236] Where M 1 More preferably Mg and wherein M 2 More preferably, it is Al.

[0237] 16. The method as described in any one of Examples 1 to 15, wherein the molded article obtained by (ii) has a water adsorption amount in the range of 25 to 70 wt%, preferably in the range of 37 to 47 wt%, more preferably in the range of 40 to 44 wt%, wherein the water adsorption amount is preferably determined according to Reference Example 1.1.

[0238] 17. The method as described in any one of Examples 1 to 16, wherein the molded article obtained by (ii) has a thickness of 35.0 to 100.0 m. 2 Within the range of / g, preferably between 40.0 and 60.0 m 2 Within the range of / g, more preferably from 45.0 to 55.0 m 2 The BET specific surface area within the range of / g, wherein the BET specific surface area is preferably determined according to Reference Example 1.3.

[0239] 18. The method of any one of Examples 1 to 17, wherein the molded article obtained by (ii) has a total pore volume in the range of 0.20 to 0.7 ml / g, preferably in the range of 0.30 to 0.42 ml / g, more preferably in the range of 0.33 to 0.39 ml / g, wherein the total pore volume is preferably determined according to Reference Example 1.4.

[0240] 19. The method of any one of Examples 1 to 18, wherein molding the mixture according to (i) includes tableting or extrusion.

[0241] 20. The method as described in any one of Examples 1 to 19, wherein the calcination according to (ii) is carried out at a temperature in the range of 300°C to 1400°C, preferably in the range of 700°C to 1100°C, and more preferably in the range of 900°C to 1000°C.

[0242] 21. The method as described in any one of Examples 1 to 20, wherein the calcination according to (ii) is carried out for a period of time ranging from 0.1 to 48 h, preferably from 0.5 to 24 h, and more preferably from 1 to 12 h.

[0243] 22. The method of any one of Examples 1 to 21, wherein the gas atmosphere according to (ii) comprises, preferably, one or more of oxygen and nitrogen, preferably air.

[0244] 23. The method as described in any one of Examples 1 to 22, further comprising:

[0245] (ii') Treat the molded article obtained by (ii) with acid.

[0246] 24. The method as described in Example 23, wherein the treatment according to (ii') includes immersing the molded article in the acid.

[0247] 25. The method as described in Example 23 or 24, wherein the processing according to (ii') lasts for a period of time ranging from 10 to 400 minutes, preferably from 45 to 75 minutes, and more preferably from 55 to 65 minutes.

[0248] 26. The method as described in any one of Examples 23 to 25, wherein the treatment according to (ii') is carried out at a temperature in the range of 0°C to 75°C, preferably in the range of 10°C to 40°C, and more preferably in the range of 15°C to 35°C.

[0249] 27. The method as described in any one of Examples 23 to 26, wherein the acid according to (ii') is an aqueous acid solution.

[0250] 28. The method as described in Example 27, wherein the acid-water solution has an acid-to-water weight ratio in the range of 1:1 to 1:10, preferably in the range of 1:3 to 1:5, and more preferably in the range of 1:3.9 to 1:4.1.

[0251] 29. The method as described in Examples 27 or 28, wherein the aqueous acid solution has an acid concentration in water in the range of 2.5 to 4.5 mol / L, preferably in the range of 3.2 to 3.7 mol / L, and more preferably in the range of 3.3 to 3.6 mol / L.

[0252] 30. The method as described in any one of Examples 23 to 29, wherein the acid according to (ii') comprises, preferably, one or more of an inorganic acid and an organic acid, preferably one or more of HNO3, HCl, H2SO4, H3PO4, formic acid, oxalic acid, and acetic acid, more preferably HNO3.

[0253] 31. The method as described in any one of Examples 23 to 30, further comprising, preferably, after (ii') and before (iii), and after (ii') and before (ii'').

[0254] (ii'.1) Wash the molded product obtained from (ii') with deionized water.

[0255] 32. The method as described in any one of Examples 23 to 31, further comprising, after (ii') and before (iii), preferably after (ii'.1) and before (iii), preferably after (ii'.1) and before (ii''),

[0256] (ii'.2) Dry the molded article obtained by (ii') or (ii'.1) in a gaseous atmosphere.

[0257] 33. The method as described in Example 32, wherein the drying according to (ii'.2) is carried out at a temperature in the range of 80°C to 160°C, preferably in the range of 100°C to 140°C, and more preferably in the range of 110°C to 130°C.

[0258] 34. The method as described in Example 32 or 33, wherein the drying according to (ii'.2) is carried out for a period of time ranging from 0.5 to 20 hours, preferably from 2 to 16 hours, and more preferably from 3 to 12 hours.

[0259] 35. The method as described in any one of Examples 32 to 34, wherein the gas atmosphere according to (ii'.2) comprises, preferably, one or more of oxygen and nitrogen, preferably air.

[0260] 36. The method as described in any one of Examples 23 to 35, further comprising:

[0261] (ii'') Calcination of the molded article obtained by (ii'), (ii'.1) or (ii'.2) in a gaseous atmosphere.

[0262] 37. The method as described in Example 36, wherein the calcination according to (ii'') is carried out at a temperature in the range of 400°C to 1200°C, preferably in the range of 600°C to 950°C, and more preferably in the range of 825°C to 875°C.

[0263] 38. The method as described in Example 36 or 37, wherein the calcination according to (ii'') is carried out for a period of time ranging from 0.1 to 1.5 h, preferably from 0.3 to 0.7 h, and more preferably from 0.4 to 0.6 h.

[0264] 39. The method as described in any one of Examples 36 to 38, wherein the gas atmosphere according to (ii'') comprises, preferably, one or more of oxygen and nitrogen, preferably air.

[0265] 40. The method as described in any one of Examples 1 to 39, wherein the treatment according to (iii) is achieved by impregnation, more preferably by initial wet impregnation.

[0266] 41. The method as described in any one of Examples 1 to 40, wherein the treatment according to (iii) is carried out for a period of time ranging from 0.1 to 12 h, preferably from 0.15 to 9 h, and more preferably from 0.2 to 6 h.

[0267] 42. The method as described in any one of Examples 1 to 41, wherein the treatment according to (iii) is carried out at a temperature in the range of 0°C to 50°C, preferably in the range of 10°C to 40°C, and more preferably in the range of 15°C to 35°C.

[0268] 43. The method as described in any one of Examples 1 to 42, wherein the Ru source comprises, preferably consists of, one or more of the following: Ru nitrosyl salt (preferably Ru(NO)NO3), Ru halide (preferably RuCl3 hydrate) and Ru acetate.

[0269] 44. The method of any one of Examples 1 to 43, wherein the alkali metal is selected from the group consisting of Li, Na, K, Rb, Cs and mixtures of two or more thereof, preferably from the group consisting of K, Cs and mixtures of two or more thereof, wherein the alkali metal is more preferably K or Cs, and wherein the alkali metal is more preferably K.

[0270] 45. The method of any one of Examples 1 to 44, wherein the alkali metal source comprises, preferably, one or more of the organic or inorganic salts of the alkali metal, preferably one or more of the acetate, nitrate, and halide of the alkali metal, preferably an acetate or nitrate.

[0271] 46. ​​The method as described in any one of Examples 1 to 45, wherein, in the aqueous solution according to (iii), the molar ratio of Ru, calculated as an element, to the alkali metal, calculated as the sum of one or more alkali metals as elements, is in the range of 0.10:1 to 1.00:1, preferably in the range of 0.20:1 to 0.50:1, and more preferably in the range of 0.25:1 to 0.45:1.

[0272] 47. The method of any one of Examples 1 to 46, wherein in (iii) the aqueous solution further comprises an acid, wherein the acid comprises, preferably comprises, one or more of the following: inorganic acid and organic acid, preferably one or more of HNO3, HCl, H2SO4, H3PO4, formic acid, oxalic acid, and acetic acid, more preferably HNO3.

[0273] 48. The method as described in Example 47, wherein the aqueous solution has an acid to water weight ratio in the range of 1:1 to 1:10, preferably in the range of 1:3 to 1:5, and more preferably in the range of 1:3.9 to 1:4.1.

[0274] 49. The method as described in any one of Examples 1 to 48, further comprising:

[0275] (iv) Drying the molded article obtained by (iii) in a gaseous atmosphere, wherein the drying is preferably carried out at a temperature in the range of 80°C to 220°C, preferably 90°C to 200°C, more preferably 100°C to 180°C, wherein the gaseous atmosphere preferably contains one or more of nitrogen and oxygen, more preferably air.

[0276] 50. The method as described in any one of Examples 1 to 49, further comprising:

[0277] (v) Activating the molded article obtained by (iii) or (iv) in a gaseous atmosphere containing hydrogen, wherein the activation is carried out at a temperature in the range of 200°C to 400°C, preferably 240°C to 360°C, wherein the activation is carried out for a period of time in the range of 0.1 to 48 h, preferably 0.5 to 36 h, wherein the gaseous atmosphere preferably contains an inert gas, wherein the inert gas is preferably one or more of Ar and N2, more preferably N2, wherein the gaseous atmosphere more preferably contains 0.01 to 10 vol-%, more preferably 0.5 to 6 vol-%, of H2, preferably in the inert gas.

[0278] 51. A catalytic material, which is obtained or can be obtained by any one of Examples 1 to 50.

[0279] 52. The catalytic material as described in Example 51, comprising Ru, an alkali metal and a support material, wherein Ru and the alkali metal are supported on the support material.

[0280] 53. The catalytic material as described in Example 52, wherein the support material is selected from M. 1 O, M 2 2O3, M 3 O2, M 4 2O5, M 1 M 2 The group consisting of 2O4 and mixtures of two or more thereof, preferably selected from M 1 O, M 2 2O3 and M 1 M 2 The group consisting of 2O4, wherein the carrier material is more preferably M. 1 M 2 2O4,

[0281] Where M 1 M represents one or more divalent elements. 2 M represents one or more trivalent elements. 3 M represents one or more tetravalent elements. 4 It represents one or more pentavalent elements.

[0282] 54. The catalytic material as described in Example 52 or 53, wherein the support material comprises a crystalline phase having a spinel structure, wherein the crystalline phase having a spinel structure is preferably determined according to Reference Example 1.2.

[0283] 55. The catalytic material as described in Examples 54 or 55, wherein M 1 Elements selected from Groups 2, 10, 11, and 12 of the periodic table, where M... 1Preferably, it is selected from the group consisting of Mg, Ca, Ni, Cu, Zn, Mn, Co, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Mg, Ni, Cu, Zn, and mixtures of two or more thereof; even more preferably, it is selected from the group consisting of Mg, Zn, Cu, and mixtures thereof; even more preferably, it is selected from the group consisting of Mg, Zn, and mixtures thereof, wherein M 1 More preferably, it is Mg.

[0284] 56. The catalytic material as described in any one of Examples 53 to 55, wherein M 2 Elements selected from Groups 5, 6, 7, 8, and 13 of the periodic table, where M... 2 Preferably, it is selected from the group consisting of Al, Ga, In, Cr, Fe, V, Mn, Co, La, and mixtures of two or more thereof; more preferably, it is selected from the group consisting of Al, Cr, Fe, V, Mn, La, and mixtures of two or more thereof; even more preferably, it is selected from the group consisting of Al, La, V, Mn, and mixtures of two or more thereof; even more preferably, it is selected from the group consisting of Al, La, and mixtures of two or more thereof, wherein M... 2 More preferably, it is Al.

[0285] 57. The catalytic material as described in any one of Examples 53 to 56, wherein M 3 Elements selected from Groups 4 and 14 of the periodic table, where M... 3 Preferably, it is selected from the group consisting of Si, Ge, Sn, Ti, Zr, Hf, Ce, and mixtures of two or more of them, wherein M 3 More preferably, it is selected from the group consisting of Si, Ti, Zr, Hf, Ce, and mixtures of two or more of them.

[0286] 58. The catalytic material as described in any one of Examples 53 to 57, wherein M 4 Selected from Group 5 of the periodic table, where M 4 Preferably, it is selected from the group consisting of V, Nb, Ta, and mixtures of two or more of them.

[0287] 59. The catalytic material as described in any one of Examples 53 to 58, comprising a composition based on M 1 O calculates one or more divalent elements M 1 M 2 One or more trivalent elements M calculated by 2O3 2 M 3 One or more tetravalent elements M calculated by O2 3 M 4 One or more pentavalent elements M calculated using 2O54 The total weight of the alkali metal, 0.5 to 5.0 wt%, preferably 2.0 to 4.0 wt%, more preferably 2.4 to 3.6 wt%, more preferably 2.6 to 3.4 wt%, more preferably 3.0 to 3.4 wt%, in elemental terms.

[0288] 60. The catalytic material as described in any one of Examples 53 to 59, comprising a composition based on M 1 O calculates one or more divalent elements M 1 M 2 One or more trivalent elements M calculated by 2O3 2 M 3 One or more tetravalent elements M calculated by O2 3 M 4 One or more pentavalent elements M calculated using 2O5 4 The total weight of Ru, in elemental form, is 0.5 to 5 wt%, preferably 1.0 to 3.0 wt%, more preferably 1.4 to 2.6 wt%, more preferably 1.6 to 2.4 wt%, and more preferably 1.8 to 2.2 wt%.

[0289] 61. The catalytic material as described in any one of Examples 52 to 60, wherein the alkali metal is selected from the group consisting of Li, Na, K, Rb, Cs and mixtures of two or more thereof, preferably selected from the group consisting of K, Cs and mixtures of two or more thereof, wherein the alkali metal is more preferably K or Cs, and wherein the alkali metal is more preferably K.

[0290] 62. The catalytic material as described in any one of Examples 52 to 61, wherein the support material has a total pore volume in the range of 0.10 to 0.90 ml / g, preferably in the range of 0.18 to 0.75 ml / g, more preferably in the range of 0.25 to 0.60 ml / g, more preferably in the range of 0.33 to 0.53 ml / g, more preferably in the range of 0.37 to 0.49 ml / g, and more preferably in the range of 0.40 to 0.46 ml / g, wherein the total pore volume is preferably determined according to Reference Example 1.4.

[0291] 63. The catalytic material as described in any one of Examples 52 to 62, wherein the support material has a crystallinity in the range of 50% to 100%, preferably 60% to 100%, more preferably 70% to 95%, and even more preferably 80% to 90%, wherein the crystallinity is preferably determined according to Reference Example 1.2.

[0292] 64. The catalytic material as described in Example 63, wherein 50% to 100%, preferably 70% to 100%, more preferably 95% to 100% of the crystalline phase has a spinel structure as determined by XRD, preferably as determined according to Reference Example 1.2.

[0293] 65. The catalytic material as described in any one of Examples 52 to 64, wherein the X-ray diffraction pattern exhibited by the catalytic material includes at least the following reflections:

[0294]

[0295] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0296] Preferably, it includes at least the following reflections:

[0297]

[0298] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0299] More preferably, it includes at least the following reflections:

[0300]

[0301] This involves 100% the intensity of the maximum peak in the X-ray powder diffraction pattern, which is preferably determined according to reference example 1.2.

[0302] Where M 1 More preferably Mg and wherein M 2 More preferably, it is Al.

[0303] 66. The catalytic material as described in any one of Examples 52 to 65, wherein the support material has a median pore size in the range of 0.001 to 0.1 µm, preferably in the range of 0.005 to 0.05 µm, more preferably in the range of 0.02 to 0.04 µm, more preferably in the range of 0.027 to 0.035 µm, and more preferably in the range of 0.028 to 0.034 µm, wherein the pore size distribution is preferably determined according to Reference Example 1.5.

[0304] 67. The catalytic material as described in any one of Examples 52 to 66, wherein the support material has a water adsorption capacity in the range of 10 to 80 wt%, preferably in the range of 30 to 60 wt%, more preferably in the range of 40 to 50 wt%, and even more preferably in the range of 43 to 47 wt%, wherein the water adsorption capacity is preferably determined according to Reference Example 1.1.

[0305] 68. The catalytic material as described in any one of Examples 52 to 67, wherein the support material has a thickness of 20.0 to 150.0 m. 2 Within the range of / g, more preferably from 30.0 to 90.0 m 2 Within the range of / g, more preferably from 40.0 to 65.0 m 2 Within the range of / g, more preferably from 45.0 to 55.0 m 2 The BET specific surface area within the range of / g, wherein the BET specific surface area is preferably determined according to Reference Example 1.3.

[0306] 69. The catalytic material as described in any one of Examples 52 to 68, wherein the Ru is uniformly dispersed throughout the catalytic material.

[0307] 70. The catalytic material as described in any one of Examples 52 to 69, wherein the alkali metal M 3 It is uniformly dispersed throughout the catalytic material.

[0308] 71. The catalytic material as described in any one of Examples 52 to 70, wherein 85 to 100 wt%, preferably 90 to 100 wt%, more preferably 95 to 100 wt%, more preferably 98 to 100 wt%, more preferably 99 to 100 wt%, and more preferably 99.9 to 100 wt%, of the catalytic material is composed of the support material, Ru, and the alkali metal.

[0309] 72. The catalytic material as described in any one of Examples 51 to 71, which is in the form of an extrusion, tablet or granules.

[0310] 73. The catalytic material as described in Example 72, wherein the extrudate or the tablet has a cross section, wherein the cross section is circular, hexagonal, rectangular, square, triangular, elliptical, star-shaped polygon or clover-shaped, preferably circular, hexagonal, rectangular, square, triangular, elliptical, star-shaped polygon with 3, 4, 5, 6, 7 or 8 apexes, clover-shaped, tetralobed or hexalobed, more preferably circular, hexagonal, rectangular, square, triangular, elliptical, star-shaped polygon with 3 or 4 apexes, clover-shaped, tetralobed or hexalobed.

[0311] 74. The catalytic material as described in any one of Examples 51 to 73, wherein the catalytic material is in the form of a tablet having a cross section, wherein the cross section is tetralobed.

[0312] 75. The catalytic material as described in Example 74, wherein the tablet has a thickness, wherein the thickness is in the range of 2.0 to 13.0 mm, preferably in the range of 5.0 to 10.0 mm, and more preferably in the range of 6.5 to 9.0 mm.

[0313] 76. The catalytic material as described in Examples 74 or 75, wherein the tablet has a diameter D in the range of 5 to 20 mm, preferably in the range of 7 to 17 mm, and more preferably in the range of 9 to 15 mm.

[0314] 77. The catalytic material as described in any one of Examples 51 to 76, wherein the catalytic material is in the form of a tablet having a cross-section, wherein the cross-section is hexagonal.

[0315] 78. The catalytic material as described in Example 77, wherein the tablet has a thickness, wherein the thickness is in the range of 2.0 to 15.0 mm, preferably in the range of 5.0 to 12.0 mm, and more preferably in the range of 8.0 to 9.0 mm.

[0316] 79. The catalytic material as described in Example 77 or 78, wherein the tablet has a diameter D in the range of 5 to 25 mm, preferably in the range of 12 to 19 mm, and more preferably in the range of 14 to 17 mm.

[0317] 80. The catalytic material as described in Example 72, wherein the catalytic material is in the form of an extrusion having a cross section, wherein the cross section is circular, star-shaped polygonal, or trilobal.

[0318] 81. The catalytic material as described in Example 80, wherein the extrudate has a thickness, wherein the thickness is in the range of 1.0 to 12.0 mm, preferably in the range of 1.5 to 10.0 mm, and more preferably in the range of 2.0 to 8.0 mm.

[0319] 82. The catalytic material as described in Example 80 or 81, wherein the extrudate has a diameter, wherein the diameter is in the range of 1 to 20 mm, preferably in the range of 2 to 18 mm, and more preferably in the range of 3 to 16 mm.

[0320] 83. A method for converting NH3 into H2 and N2, the method comprising:

[0321] (A) A reactor containing a catalytic material according to any one of Examples 51 to 82;

[0322] (B) Prepare a feed gas stream containing NH3;

[0323] (C) The feed gas stream prepared in (B) is fed into the reactor provided in (A) and the feed gas stream is brought into contact with the catalyst material, wherein the contact is carried out at a pressure greater than 10 absolute bar and at a temperature in the range of 200°C to 650°C;

[0324] (D) Remove the effluent gas stream from the reactor, which contains H2 and N2.

[0325] 84. The method as described in Example 83, wherein the contact is performed at a pressure in the range of 11 to 50 bar, preferably 15 to 40 bar, and more preferably 19 to 31 bar.

[0326] 85. The method as described in Example 83 or 84, wherein the contact is carried out at a temperature in the range of 250°C to 650°C, preferably 275°C to 625°C, and more preferably 300°C to 600°C.

[0327] 86. The method of any one of Examples 83 to 85, wherein the feed gas stream prepared in (B) comprises 1 to 100 vol.-%, preferably 3 to 99.99 vol.-%, more preferably 5 to 99.95 vol.-%, more preferably 10 to 99.9 vol.-%, more preferably 20 to 99.8 vol.-%, more preferably 30 to 99.7 vol.-%, more preferably 40 to 99.6 vol.-%, and more preferably 50 to 99.5 vol.-%.

[0328] 87. The method of any one of Examples 83 to 86, wherein the feed gas stream prepared in (B) comprises 0 to 50 vol.-%, preferably 0.01 to 30 vol.-%, more preferably 0.03 to 15 vol.-%, more preferably 0.05 to 5 vol.-%, more preferably 0.1 to 1 vol.-%, more preferably 0.12 to 0.5 vol.-%, and more preferably 0.14 to 0.16 vol.-%.

[0329] 88. The method of any one of Examples 83 to 87, wherein the feed gas stream prepared in (B) comprises 0 to 75 vol.-%, preferably 0 to 60 vol.-%, more preferably 0 to 50 vol.-%, more preferably 0 to 40 vol.-%, more preferably 0 to 35 vol.-%, and more preferably 0 to 30 vol.-%. of H2.

[0330] 89. The method of any one of Examples 83 to 88, wherein the feed gas stream prepared in (B) comprises 100 to 50,000 ppmv, preferably 200 to 30,000 ppmv, more preferably 500 to 25,000 ppmv, more preferably 500 to 20,000 ppmv, more preferably 500 to 15,000 ppmv, more preferably 750 to 15,000 ppmv, more preferably 1,000 to 11,000 ppmv, more preferably 1,000 to 10,000 ppmv, more preferably 2,000 to 8,000 ppmv, more preferably 3,000 to 7,500 ppmv, more preferably 4,500 to 7,000 ppmv, more preferably 5,000 to 6,500 ppmv of H2O.

[0331] 90. The method as described in any one of Examples 83 to 89, wherein the total amount of NH3, N2 and H2 contained in the feed gas stream prepared in (B) is in the range of 90 to 100 wt.-%, preferably 95 to 99.95 vol.-%, more preferably 98 to 99.9 vol.-%, more preferably 99 to 99.85 vol.-%, and more preferably 99.7 to 99.8 vol.-%.

[0332] 91. The method as described in any one of Examples 83 to 90, wherein the feed stream is subjected to a flow rate of 500 to 20,000 h. -1 Preferably 500 to 16,000 h -1 More preferably 700 to 14,000 h -1 More preferably 800 to 12,000 h -1 More preferably 900 to 10,000 h -1 More preferably 1,000 to 8,000 h -1 And more preferably 3,000 to 5,000 h -1 The gas hourly space velocity within the range is fed into the reactor.

[0333] 92. Use of the catalytic material according to any one of Examples 51 to 82 for converting NH3 into H2 and N2.

[0334] 93. A method, preferably according to any one of Examples 83 to 91, comprising the step of converting H2 that is available or obtainable according to (D) as described in any one of Examples 83 to 91 to obtain product Ω.

[0335] 94. The method as described in Example 93, wherein the product Ω is selected from:

[0336] -Building unit or monolith; or

[0337] -A polymer (preferably polymer A), a polymer composition (preferably polymer composition A), or a polymer product (preferably polymer product A); or

[0338] - Cleaning polymers, cleaning surfactants, descaling compounds, cleaning biocides, or combinations thereof or formulations thereof; or

[0339] -Agricultural chemical compositions, agricultural chemical formulations, adjuvants, or agricultural chemical active ingredients; or

[0340] - Active pharmaceutical ingredient or its intermediate, pharmaceutical excipient, animal feed additive, human food additive, dietary supplement, aromatic chemical or aromatic composition; or

[0341] - Aqueous polymer dispersions, preferably polyurethane or polyurethane-poly(meth)acrylate hybrid polymer dispersions, emulsions, binders for paper and fiber coatings, UV-curable acrylic polymers for hot melts and coatings, polyisocyanates, hyperbranched polyester polyols, polymer dispersants for inorganic binder compositions, unsaturated polyester polyols, or 100% curable compositions; or

[0342] - Cosmetic surfactants, emollients, waxes, cosmetic polymers, UV filters, other cosmetic ingredients, or combinations thereof or formulations thereof; or

[0343] - Polymer B, polymer composition B, coating composition, other functional composition, foil, molded body, coating or coated substrate.

[0344] 95. The method as described in Examples 93 or 94,

[0345] The product Ω contains H2 that is obtainable or acquireable according to (D) as described in any one of Examples 83 to 91, at a content of 1 wt% or more, preferably 2 wt% or more, more preferably 5 wt% or more, more preferably 15 wt% or more, more preferably 30 wt% or more, more preferably 40 wt% or more, more preferably 60 wt% or more, more preferably 80 wt% or more, more preferably 90 wt% or more, more preferably 95 wt% or more; and / or

[0346] The product Ω contains H2 that is obtainable or acquireable according to (D) as described in any one of Examples 83 to 91, in an amount of 100 wt% or less, preferably 95 wt% or less, more preferably 90 wt% or less, more preferably 50 wt% or less, more preferably 25 wt% or less, more preferably 10 wt% or less; and

[0347] Preferably, the content is determined based on identity preservation and / or segregation and / or mass balance and / or book and embodiment chain of custody models, preferably based on mass balance, and preferably according to the International Sustainability and Carbon Certification (ISCC) standard.

[0348] The invention is further illustrated by the following examples, comparative examples, and reference examples.

[0349] Experimental Section

[0350] Reference Example 1: Determining the Method

[0351] Reference Example 1.1: Determination of Water Adsorption Capacity

[0352] Place the dried molded product in water until it is completely submerged. Leave the product in the water for 60 minutes. Afterward, allow the outer surface of the product to dry and determine its weight. Calculate the water absorption rate (also known as water adsorption capacity) as a percentage by weight using Formula I:

[0353] Water absorption rate = (Weight of wet molded product - Weight of dry molded product) / Weight of dry molded product (I).

[0354] Reference Example 1.2: Determination of X-ray Powder Diffraction and Crystallinity

[0355] Powder X-ray diffraction (PXRD) data were collected using a diffractometer (D8 Advance II series, Bruker AXS GmbH) equipped with a LYNXEYE detector that operates with a copper anode X-ray tube at 40 kV and 40 mA. The geometry was Bragg-Brentano, and an air scattering shield was used to reduce air scattering.

[0356] Crystallinity calculation: The crystallinity of the sample was determined using the software DIFFRAC.EVA provided by Bruker AXS in Karlsruhe, according to the method described on page 121 of the user manual. Default parameters were used for the calculation.

[0357] Phase composition was calculated using the modeling software DIFFRAC.TOPAS (DIFFRAC.TOPAS version 6, 2017 user manual, BRUSH AXS, Karlsruhe) provided by BRUSH AXS. The diffraction pattern was simulated using the crystal structure of the determined phases, instrument parameters, and grain size of individual phases. In addition to a function modeling the background intensity, it was fitted to the data.

[0358] Data Collection: Samples were homogenized in a mortar and then pressed into a standard flat sample holder provided by Bruker AXS for geometric data collection in the Bragg-Brentano region. A flat surface was achieved by compressing and flattening the sample powder using a glass plate. Data were collected in 0.02° 2θ steps from an angle range of 2° to 70° 2θ, with the variable divergence slit set at an angle of 0.1°. Crystal content describes the ratio of the intensity of the crystal signal to the total scattered intensity.

[0359] Refer to Example 1.3: Determination of BET specific surface area

[0360] The BET specific surface area was determined by nitrogen physisorption at 77 K according to the method disclosed in DIN 66131.

[0361] Refer to Example 1.4: Determination of Total Orifice Volume

[0362] The total pore volume was determined according to DIN 66133 by mercury porosimetry. For this purpose, the MicroActiveAutoPore V 9600 was used.

[0363] Refer to Example 1.5: Determination of Aperture Distribution

[0364] The pore size distribution was determined according to DIN 66133 by mercury porosimetry. For this purpose, the MicroActiveAutoPore V 9600 was used.

[0365] Reference Example 2.1: Preparation of Carrier Materials

[0366] Pural Mg 30 (containing Mg calculated as MgO and Al calculated as Al2O3 in a weight ratio of 30:70) quadrilobe was calcined in air at 950°C for 3 h.

[0367] Reference Example 2.2: Acid Treatment of Carrier Materials

[0368] The calcined four-leaf molded parts obtained in Reference Example 2.1 were treated with nitric acid as follows. The calcined four-leaf molded parts were placed in a glass beaker, which was then filled with an aqueous solution containing HNO3 (20 wt% concentration, corresponding to 3.3 mol / L). All molded parts were completely covered by the acidic solution. After 60 minutes, the acidic solution was removed, and the obtained four-leaf molded parts were washed with demineralized water. The four-leaf molded parts were dried at 120°C for 4 h (heating rate 5°C / min). Following the drying step, a calcination step was performed at 850°C for 0.5 h (heating rate 5°C / min) to remove residual nitrates. The characteristics of the molded parts before and after acid treatment are recorded in Table 1 below.

[0369] The water absorption rate was determined according to Reference Example 1.1, the total pore volume was determined according to Reference Example 1.4, the median pore size was determined according to Reference Example 1.5, and the BET specific surface area was determined according to Reference Example 1.3.

[0370] Table 1

[0371] Characteristics of Pural Mg 30 four-leaf shaped parts before and after treatment with an aqueous solution containing HNO3.

[0372]

[0373] Comparative Example 3: Preparation of Catalytic Materials Containing Ru and K

[0374] 20 g of the acid-treated carrier material, prepared according to Reference Example 2.2, as a molding article, was impregnated with an aqueous solution containing 2.173 g of Ru(NO)(NO3)3 (corresponding to 19.5 wt% Ru in the aqueous solution). The impregnation target was to achieve 95% pore volume based on the water absorption rate (determined according to Reference Example 1), and therefore the Ru(NO)(NO3)3 aqueous solution was further diluted with an aqueous NO3 solution (20% HNO3 in water). After drying at 180°C for 4 h, the Ru-containing molding article was impregnated with 1.859 g of potassium acetate (K(CH3COO)) dissolved in demineralized water to fill 90% of the pore volume based on the water absorption rate (determined according to Reference Example 1). The resulting material was then dried at 120°C for 2 h.

[0375] Example 4: Preparation of catalytic materials containing Ru and K

[0376] Ten g of the acid-treated support material, prepared according to Reference Example 2.2, as a molding article, was impregnated with an aqueous solution containing Ru and K. This Ru- and K-containing aqueous solution was prepared by dissolving 0.930 g of potassium acetate (K(CH3COO)) in an aqueous solution containing 1.086 g of Ru(NO)(NO3)3 (corresponding to 19.5 wt% Ru in the aqueous solution). The resulting Ru- and K-containing aqueous solution was further diluted with an aqueous HNO3 solution (20% HNO3 in water) to impregnate 95% of the pore volume based on the water absorption rate (determined according to Reference Example 1). After drying at 120°C for 2 h, the resulting catalyst material was further heat-treated at 180°C for 4 h.

[0377] Example 5: Preparation of catalytic materials containing Ru and K

[0378] 10 g of untreated support material was prepared according to Reference Example 2.1. Then, a catalyst was prepared by impregnating the untreated support material with an aqueous solution containing Ru and K according to the procedure of Example 4.

[0379] Example 6: Catalytic testing in NH3 reforming under high pressure

[0380] Prior to testing, the catalysts according to Comparative Examples 3, 4, and 5 were activated at 300°C in a reducing atmosphere of 5% H2 in Ar (residence time 1 h, heating rate 2°C / min). After catalyst activation, a feed stream was applied (see table below, NH3 + H2O + 5 vol% Ar). In the corresponding tests, the pressure of NH3 (p(NH3)) was set to 30 absolute bar. The gas hourly space velocity (GHSV) relative to the NH3 content was set to 4.000 h. -1 The temperature varies between 300°C and 650°C.

[0381] Table 1 shows the catalysts from Comparative Example 3 and Example 4 at 4,000 h⁻¹. -1 Experimental results were obtained at a gas hourly space velocity (GHSV) of 30 absolute bar and a pressure p(NH3), with the feed further comprising 5,000 ppmv of H2O and 5 vol-% Ar. The catalyst was tested between 300°C and 650°C. The temperature was increased in 50°C steps. NH3 conversion is given as a percentage. Results from Examples 3 and 4 are compared. Figure 1 As shown in the image. (See image below.) Figure 1 The test results shown indicate that the catalyst approaches equilibrium conversion at 550°C, while the relatively active catalyst in Example 4 approaches equilibrium conversion at 500°C.

[0382] Table 1:

[0383] Results of ammonia conversion on Ru-based catalysts in Comparative Examples 3, 4, and 5.

[0384]

[0385] Therefore, as can be seen from the catalytic test results of the corresponding catalytic materials in Comparative Examples 3 and 4 and 5, the catalytic material according to the invention provides highly efficient ammonia decomposition under high pressure. Thus, an improved method for converting NH3 to H2 and N2 can be provided, which, in particular, allows highly efficient ammonia decomposition under high pressure when using the catalytic material according to the invention.

[0386] Furthermore, it has been unexpectedly found that, for Examples 4 and 5, highly efficient decomposition can be provided even at low temperatures, particularly even under high pressure conditions. Furthermore, it has been unexpectedly found that, compared to the catalyst of Example 5 without acid treatment of the support material, the catalyst of Example 4, containing the acid-treated support material, exhibits even better high-efficiency decomposition at low temperatures. In addition, it has been quite unexpectedly found that, even when using industrial-grade ammonia containing a small amount of water for stabilization purposes, under harsh hydrothermal conditions at high pressure due to the presence of water in the ammonia decomposition reaction, the catalyst according to the invention can provide a highly efficient method. Attached Figure Description

[0387] Figure 1 The graph shows the results of NH3 reforming determined according to Example 6 for the catalysts used in Comparative Examples 3 and 4, where the NH3 conversion is given as % on the vertical axis and the temperature is given as °C on the horizontal axis.

[0388] References cited:

[0389] -K. Lamb et. al. in Int. J. of Hydrogen Energy 2019, 44, 3726-3736

[0390] -A. Di Carlo et al. in Int. J. of Hydrogen Energy 2014, 39, 808-814

[0391] -TA Le et al. in Korean J. Chem. Eng. 2021, 38(6), 1087-1103

[0392] -M. Miyamoto et al. in Int. J. of Hydrogen Energy 2018, 43, 730-738

[0393] -B. Lorenzut et al. in ChemCatChem 2010, 2, 1096 – 1106

[0394] -Z. Wang et al. in Int. J. of Hydrogen Energy 2019, 44, 7300-7307

[0395] -WO 2015 / 086639 A2

[0396] -WO 2018 / 046393 A1

[0397] -S.-F. Yin et al. in Applied Catalysis B Environmental 2004, 48, 237–241

[0398] -S. Sayas et al. in Catal.Sci. Technol.2020, 10, 5027–5035

[0399] -GB 1377191 A。

Claims

1. A method for preparing a catalytic material, the method comprising: (i) Molding a mixture containing one or more carrier material sources; (ii) Calcine the molded article obtained by (i) in a gaseous atmosphere to obtain a molded article containing a carrier material; (iii) Impregnate the molded article with an aqueous solution containing both a Ru source and an alkali metal source.

2. The method of claim 1, further comprising, after (ii) and before (iii) (ii') Treat the molded article obtained by (ii) with acid.

3. The method as described in claim 2, wherein, The treatment according to (ii') includes immersing the molded article in the acid.

4. The method as described in claim 2 or 3, wherein, The treatment according to (ii') lasts for a period of time ranging from 10 to 400 minutes.

5. The method according to any one of claims 2 to 4, wherein, According to (ii'), the acid is an aqueous solution of acid.

6. The method of claim 5, wherein, The aqueous solution of this acid has an acid concentration in water ranging from 2.5 to 4.5 mol / L.

7. The method as claimed in any one of claims 2 to 6, further comprising (ii') after and before (iii). (ii'.1) Wash the molded article obtained from (ii') with deionized water.

8. The method as claimed in any one of claims 2 to 7, further comprising following (ii') and preceding (iii). (ii'.2) Dry the molded article obtained by (ii') or (ii'.1) in a gaseous atmosphere.

9. The method according to any one of claims 1 to 8, wherein, The Ru source contains one or more of Ru nitrosyl salts, Ru halides, and Ru acetates.

10. The method according to any one of claims 1 to 9, wherein, The alkali metal is selected from the group consisting of Li, Na, K, Rb, Cs, and mixtures of two or more of them.

11. The method according to any one of claims 1 to 10, wherein, In the aqueous solution according to (iii), the molar ratio of Ru, calculated as an element, to the alkali metal, calculated as the sum of one or more alkali metals as elements, is in the range of 0.10:1 to 1.00:

1.

12. A catalytic material, which is obtained or can be obtained by the method according to any one of claims 1 to 11.

13. A method for converting NH3 into H2 and N2, the method comprising: (A) A reactor containing the catalytic material as described in claim 11; (B) Prepare a feed gas stream containing NH3; (C) The feed gas stream prepared in (B) is fed into the reactor provided in (A) and the feed gas stream is brought into contact with the catalyst material, wherein the contact is carried out at a pressure greater than 10 absolute bar and at a temperature in the range of 200°C to 650°C; (D) Remove the effluent gas stream from the reactor, which contains H2 and N2.

14. Use of the catalytic material as described in any one of claims 11 for converting NH3 into H2 and N2.

15. A method comprising the step of converting H2 that is available or obtainable according to claim 13(D) to obtain product Ω.

Citation Information

Patent Citations

  • Catalyst and oxidation process

    GB1377191A

  • Method for hydrogenating aromatic compounds

    WO2015086639A2

  • Method for hydrating nitriles in the presence of a ruthenium catalyst carried on zro2

    WO2018046393A1