ceramic sheet

By controlling parameters such as the surface roughness and grain size of the ceramic sheets, the problem of picking up two ceramic sheets during handling was solved, ensuring the strength and stability of the ceramic sheets and achieving the effect of preventing two sheets from being picked up.

CN123146471APending Publication Date: 2026-11-20NIPPON SHOKUBAI CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580027426.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-15
Filing Date
2025-04-10
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

During the handling of ceramic sheets, when multiple ceramic sheets are stacked, it is easy to pick up two sheets at once, and surface roughening treatment can lead to a decrease in strength.

Method used

By controlling parameters such as the arithmetic mean roughness of the main surface of the ceramic sheet, the difference between the highest and lowest points, the slope of the approximate straight line, and the grain size, the ceramic sheet is ensured to maintain its strength while preventing two sheets from picking up. The ceramic sheet is manufactured using laser microscopy and a specific heat treatment process.

Benefits of technology

This technology effectively prevents the picking up of two ceramic sheets while maintaining their strength, thus improving the handling stability and reliability of the ceramic sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146471A_ABST
    Figure CN123146471A_ABST
Patent Text Reader

Abstract

The ceramic sheet has a first main surface and a second main surface, each of which has an arithmetic average roughness of 0.01 μm or more and 1.0 μm or less, and when the first main surface and the second main surface are each measured by a laser microscope, in at least one of the first main surface and the second main surface, an average of a difference between the highest points and the lowest points in 10 intervals is 1.0 μm or more and 4.0 μm or less, a coefficient of variation of the difference is 0.05 or more and 0.3 or less, a cumulative relative frequency of a slope of an approximate straight line calculated every 1.314 μm is 20% or more and 70% or less, the slope of the approximate straight line is -0.3 or more and 0.3 or less, a cumulative relative frequency of the slope of the approximate straight line is 85% or more and 100% or less, and a cumulative relative frequency of the slope of the approximate straight line is 99.9% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to ceramic sheets. Background Technology

[0002] Ceramics are materials with excellent electrical, magnetic, and biocompatibility properties in addition to mechanical properties such as heat resistance and wear resistance, and are therefore widely used in many fields. Among them, zirconium oxide-based ceramics have excellent oxygen ion conductivity. Therefore, sheet-shaped ceramic bodies (ceramic sheets) are sometimes used as solid electrolytes in solid oxide fuel cells (SOFCs). For example, Patent Document 1 discloses a method for manufacturing electrolyte sheets for solid oxide fuel cells.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-79506 Summary of the Invention

[0006] The problem that the invention aims to solve

[0007] Furthermore, from the perspective of maximizing handling efficiency, multiple ceramic sheets are sometimes left to stand in a state of direct overlap. When only the top ceramic sheet in such a stack is subjected to adsorption and handling, ceramic sheets that are tightly packed together with it may also be handled simultaneously. That is, during the adsorption and handling of ceramic sheets, two sheets may sometimes be unintentionally picked up.

[0008] To prevent the two pieces from picking up as described above, roughening the surface of the ceramic sheet could be considered. However, simply roughening the surface of the ceramic sheet would reduce its strength.

[0009] One aspect of this disclosure is to provide a ceramic sheet that can prevent two pieces from picking up while maintaining the strength of the ceramic sheet.

[0010] Methods for solving problems

[0011] One aspect of this disclosure provides ceramic sheets as described in [1] to [9].

[0012] [1] A ceramic sheet having a first main surface and a second main surface, wherein, The arithmetic mean roughness of the first principal surface and the second principal surface mentioned above is 0.01 μm or more and 1.0 μm or less. When measuring the first principal surface and the second principal surface using a laser microscope, in at least one of the first principal surface and the second principal surface... The average difference between the highest and lowest points in any 10 randomly selected intervals (each interval being 150 μm) is greater than 1.0 μm and less than 4.0 μm. The coefficient of variation of the difference between the highest and lowest points in the above 10 randomly selected intervals is greater than 0.05 and less than 0.3. For every 1.314 μm, the cumulative relative frequency of the approximate straight line with a slope greater than -0.1 and less than 0.1 is greater than 20% and less than 70%. The cumulative relative frequencies of the aforementioned approximate straight lines with a slope of -0.3 or higher but less than 0.3 are between 85% and 100%. The cumulative relative frequency of the above approximate straight line with a slope of -1.5 or higher and less than 1.5 is 99.9% or higher and less than 100%.

[0013] [2] According to the ceramic sheet described in [1], the cumulative relative frequency of the slope of the above approximate straight line being greater than -1.0 and less than 1.0 is greater than 99.0% and less than 100%.

[0014] [3] According to the ceramic sheet described in [1] or [2], wherein the cumulative relative frequency of the slope of the above approximate straight line is 99.0% or more and 100% or less.

[0015] [4] The ceramic sheet according to any one of [1] to [3], wherein, in both the first main surface and the second main surface, the cumulative relative frequency of the slope of the approximate straight line being more than -0.3 and less than 0.3 is more than 85% and less than 100%, and the cumulative relative frequency of the slope of the approximate straight line being more than -1.5 and less than 1.5 is more than 99.9% and less than 100%.

[0016] [5] The ceramic sheet according to any one of [1] to [4] further comprises a side surface connecting the first main surface and the second main surface. The grain size of at least one of the first main surface and the second main surface is more than 90% and less than 130% of the grain size of the side surface.

[0017] [6] The ceramic sheet according to any one of [1] to [5] has a thickness of 30 μm or more and 200 μm or less, and the area of ​​each of the first main surface and the second main surface is 100 cm². 2 Above and 400cm 2 The following values ​​are 0.015 g / cm³. 2 Above and 0.15g / cm 2 the following.

[0018] [7] The ceramic sheet according to any one of [1] to [6], wherein the average value of the kurtosis (Rku) of at least one of the first main surface and the second main surface is less than 3.

[0019] [8] The ceramic sheet according to any one of [1] to [7] is a zirconium oxide sheet containing at least one rare earth element selected from the group consisting of scandium, yttrium and cerium in a total amount of 3 mol% or more and 15 mol% or less based on oxide conversion.

[0020] [9] The ceramic sheet according to any one of [1] to [8] is an electrolyte sheet for a solid oxide fuel cell.

[0021] Another aspect of this disclosure provides a method for manufacturing ceramic sheets as described below in

[10] to

[15] .

[0022]

[10] A method for manufacturing a ceramic sheet, which is the method for manufacturing a ceramic sheet as described in any one of [1] to [9], comprising: The first step involves preparing a slurry by mixing ceramic powder, binder, and solvent; In the second process, a green sheet is formed by applying the above-mentioned slurry to the coated surface of the substrate film. The third step involves degreasing the raw sheets to form a degreased form of the raw sheets; and The fourth step involves firing the aforementioned degreased body to form the ceramic sheet. In the third process described above, the raw slices are heat-treated at a temperature between 100°C and 450°C. In the fourth step described above, the degreased body is fired at a firing temperature of 1200°C or higher and 1600°C or lower.

[0023]

[11] According to the method for manufacturing ceramic sheets described in

[10] , wherein, The coated surface was treated with an alkaline reagent. The heat treatment temperature mentioned above is above 370℃ and below 450℃. The firing temperature is above 1350℃ and below 1450℃.

[0024]

[12] The method for manufacturing ceramic sheets according to

[10] or

[11] , wherein the arithmetic mean roughness of the coated surface is 0.2 μm or more and 0.7 μm or less.

[0025]

[13] The method for manufacturing ceramic sheet according to

[10] or

[11] , wherein the arithmetic mean roughness of the coated surface is 0.3 μm or more and 0.6 μm or less.

[0026]

[14] The method for manufacturing ceramic sheet according to any one of

[10] to

[13] , wherein the ceramic powder is a zirconium oxide powder.

[0027]

[15] The method for manufacturing ceramic sheets according to any one of

[10] to

[14] , wherein the second step is a step of forming a green sheet by applying the slurry in sheet form to the coated surface of a substrate film using a doctor blade method.

[0028] Invention Effects

[0029] According to one aspect of this disclosure, it is possible to provide a ceramic sheet that can prevent the occurrence of two pieces picking up while maintaining the strength of the ceramic sheet. Attached Figure Description

[0030] Figure 1 This is a schematic cross-sectional view of a ceramic sheet in one embodiment.

[0031] Figure 2 It is a graph showing the shape analysis results of a selected interval of the surface profile based on the first principal plane of the laser microscope.

[0032] Figure 3 It is Figure 2 A portion of the enlarged curve graph.

[0033] Figure 4 (a) is a sheet surface image of the PET side of Example 1. Figure 4 (b) is the result of the measurement of the surface shape profile of the PET surface in Example 1.

[0034] Figure 5 (a) is a sheet surface image of the PET side of Example 2. Figure 5 (b) is the result of the measurement of the surface shape profile of the PET surface in Example 2.

[0035] Figure 6 (a) is a sheet surface image of the PET side of Comparative Example 1. Figure 6 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 1.

[0036] Figure 7 (a) is a sheet surface image of the air surface in Comparative Example 1. Figure 7 (b) is the result of the measurement of the surface shape profile of the air surface in Comparative Example 1.

[0037] Figure 8 (a) is a sheet surface image of the PET side of Comparative Example 2. Figure 8 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 2.

[0038] Figure 9 (a) is a sheet surface image of the PET side of Comparative Example 4. Figure 9 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 4.

[0039] Figure 10 (a) is a sheet surface image of the PET side of Comparative Example 5. Figure 10 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 5.

[0040] Figure 11 (a) is a sheet surface image of the PET side of Comparative Example 6. Figure 11 (b) shows the measurement results of the surface shape profile of the PET surface of Comparative Example 6. Detailed Implementation

[0041] The following describes one embodiment of the present disclosure in detail, but the present disclosure is not limited thereto.

[0042] The following is for reference Figure 1 A detailed description of one embodiment of the ceramic sheet is provided. Figure 1 This is a schematic cross-sectional view of a ceramic sheet according to one embodiment. It should be noted that the ceramic sheet of one embodiment is a solid electrolyte (electrolyte sheet for solid oxide fuel cells) used in solid oxide fuel cells (hereinafter referred to as "SOFC"), but the ceramic sheet disclosed herein is not limited to solid electrolytes for SOFCs. In one example, the ceramic sheet is a zirconia sheet with stabilized zirconia powder as the main material. From the viewpoint of conductivity (ionic conductivity) as an electrolyte sheet, the content of zirconia-based oxides in the zirconia sheet is, for example, 80% by mass or more relative to 100% by mass of the zirconia sheet. This content can be 90% by mass or more, 95% by mass or more, 97% by mass or more, or 99% by mass or more. The stabilized zirconia powder can be cubic zirconia powder or tetragonal zirconia powder. In this case, the ratio (%) of cubic crystals obtained by X-ray diffraction measurement of the ceramic sheet can be 50% or more, and the ratio (%) of tetragonal crystals can also be 50% or more. It should be noted that in this disclosure, the above-mentioned stabilization includes partial stabilization. Therefore, stabilized zirconia can also be interpreted as partially stabilized zirconia.

[0043] As a raw material for the ceramic sheet disclosed herein, a known stabilized zirconium oxide powder can be used, for example. This powder may contain at least one of the following: selected from CaO, SrO, BaO, Y2O3, La2O3, Ce2O3, Pr2O3, Nd2O3, Sm2O3, Eu2O3, Gd2O3, Tb2O3, Dy2O3, Ho2O3, Er2O3, Yb2O3, PbO, WO3, MoO3, V2O5, Ta2O5, and Nb2O5. Furthermore, the powder may further contain gallate oxides such as LaGaO3.

[0044] In one embodiment, the ceramic powder comprises powdered zirconia-based ceramic (zirconia powder). The zirconia-based ceramic is, for example, zirconia containing a stabilizer. The stabilizer comprises at least one of the following: alkaline earth metal oxides selected from MgO, CaO, SrO, and BaO; rare earth element oxides selected from Sc2O3, Y2O3, La2O3, CeO2, Pr2O3, Nd2O3, Sm2O3, Eu2O3, Gd2O3, Tb2O3, Dy2O3, Ho2O3, Er2O3, and Yb2O3; and oxides selected from Bi2O3 and In2O3. The zirconia-based ceramic may also contain oxides such as Al2O3, SiO2, Ge2O3, B2O3, SnO2, Ta2O5, and Nb2O5 as additives.

[0045] From the viewpoint of oxygen ion conductivity, strength, and toughness, zirconia-based ceramics can be zirconia powder containing at least one rare earth element selected from the group consisting of scandium, yttrium, cerium, gadolinium, and ytterbium, in a total amount calculated based on oxides, at a proportion of 0.5 mol% to 20 mol% or more, or 3 mol% to 15 mol% or more. In this case, the ceramic sheet disclosed herein can be a zirconia sheet containing at least one rare earth element selected from the group consisting of scandium, yttrium, cerium, gadolinium, and ytterbium, in a total amount calculated based on oxides, at a proportion of 0.5 mol% to 20 mol% or more, or 3 mol% to 15 mol% or more. Zirconia-based ceramics can be zirconia powder containing at least one rare earth element selected from the group consisting of scandium, yttrium, and cerium, in a total amount calculated based on oxides, at a proportion of 0.5 mol% to 20 mol%, 0.5 mol% to 15 mol%, 3 mol% to 20 mol%, or 3 mol% to 15 mol%. In this case, for the ceramic sheet of this disclosure, the zirconia-based ceramic can be a zirconia sheet containing at least one rare earth element selected from the group consisting of scandium, yttrium, and cerium, in a total amount calculated based on oxides, at a proportion of 0.5 mol% to 20 mol%, 0.5 mol% to 15 mol%, 3 mol% to 20 mol%, or 3 mol% to 15 mol%.

[0046] When scandium is included as a rare earth element, stabilized zirconia ceramics are sometimes called scandium oxide stabilized zirconia (ScSZ). When yttrium is included as a rare earth element, stabilized zirconia ceramics can be called yttrium oxide stabilized zirconia (YSZ). When both scandium and cerium are included as rare earth elements, stabilized zirconia ceramics can be called scandium oxide and cerium oxide stabilized zirconia (ScCeSZ). Stabilized zirconia ceramics can be obtained, for example, by heat-treating a mixture of commercially available zirconia powder and powdered rare earth elements, followed by pulverizing the mixture. The heat-treated mixture can also be a product obtained by pre-firing or sintering a molded body of commercially available zirconia powder and powdered rare earth elements.

[0047] Stabilized zirconia powder can be either cubic or tetragonal. Cubic zirconia powder refers to a zirconia-based oxide containing cubic zirconia as its main component (main crystalline phase). Cubic zirconia is a substance whose diffraction peaks can be observed using X-ray diffraction. Tetragonal zirconia powder, on the other hand, is a zirconia-based oxide containing tetragonal zirconia as its main component (main crystalline phase). Tetragonal zirconia is also a substance whose diffraction peaks can be observed using X-ray diffraction.

[0048] In one embodiment, cubic or tetragonal zirconia powder with a specific particle size distribution can be used as the raw material zirconia powder. When using cubic zirconia powder as the raw material, the cubic crystal ratio (%) of the powder is, for example, 50% or more. The cubic crystal ratio can be 60% or more, 80% or more, 90% or more, or 95% or more. When using tetragonal zirconia powder as the raw material, the tetragonal crystal ratio (%) of the powder is, for example, 50% or more. The tetragonal crystal ratio can be 60% or more, 80% or more, 90% or more, or 95% or more. Furthermore, the average primary particle size of the cubic or tetragonal zirconia powder is, for example, 0.003 μm or more and 0.2 μm or less, or 0.005 μm or more and 0.15 μm or less. This average primary particle size is calculated, for example, by measurement results using a transmission electron microscope. It should be noted that when the raw material zirconia powder is cubic or tetragonal, stabilizers or other additives may be included as needed.

[0049] The ceramic powder may contain, in addition to zirconium oxide powder, powders of alumina, cerium oxide, titanium oxide, silicon oxide, niobium oxide, thallium oxide, mullite, cordierite, spinel, forsterite, anorthite, barium feldspar, enstatite, aluminum nitride, and silicon nitride, etc., without compromising the desired effect. The content of this powder relative to the total amount of raw material powders may be, for example, 0.01% by mass or more and 5% by mass or 0.05% by mass or more and 3% by mass.

[0050] The 50% volume diameter (D50) of the ceramic powder is, for example, 0.05 μm or more and 0.8 μm or less, and the 90% volume diameter (D90) is, for example, 0.3 μm or more and 1.5 μm or less. With D90 below 1.5 μm, the aggregates of the ceramic powder are less likely to become excessively large. Therefore, the resulting ceramic sheets are well densified. On the other hand, with D90 above 0.3 μm, the dispersibility of the ceramic powder during slurry preparation becomes good. D90 can be above 0.5 μm, above 0.6 μm, below 1.0 μm, or below 0.8 μm. The 10% volume diameter (D10) of the ceramic powder is, for example, 0.03 μm or more and 0.6 μm or less. In this case, there are fewer particles in the ceramic powder, thus reducing the occurrence of localized sintering, uneven sintering, etc. D10 can be above 0.06μm, above 0.1μm, below 0.6μm, below 0.5μm, or below 0.4μm.

[0051] The 50% volume diameter (D50) is measured using a laser diffraction / scattering particle size distribution measuring device (manufactured by Horiba Manufacturing Co., Ltd., trade name "LA-920"). It represents the particle size at which the total volume of each particle is accumulated, starting from the smallest particle size, relative to 50% of the total particle volume. Similarly, the 90% and 10% volume diameters are the particle sizes at which the total volume of each particle is accumulated, starting from the smallest particle size, relative to 90% and 10% of the total particle volume, respectively. It should be noted that the particle size distribution of ceramic powder can be adjusted by a combination of grinding methods such as ball mills, bead mills, planetary mills, and spray mills, and classification methods such as cyclone classifiers. Alternatively, commercially available products with the desired particle size distribution can be used.

[0052] like Figure 1 As shown, the ceramic sheet 1 has a first main surface 1a, a second main surface 1b, and a side surface 1c. The first main surface 1a and the second main surface 1b are each surfaces intersecting the thickness direction of the ceramic sheet 1, and can form a thin film such as a conductive layer for electrodes. In one embodiment, the first main surface 1a and the second main surface 1b are each square, but this is not a limitation. The first main surface 1a and the second main surface 1b can also be circular, elliptical, triangular, quadrilateral, or other polygonal shapes. The side surface 1c is the surface connecting the first main surface 1a and the second main surface 1b. In one embodiment, the ceramic sheet 1 has four side surfaces 1c with quadrilateral shapes, but this is not a limitation. For example, when the first main surface 1a and the second main surface 1b are each circular, the ceramic sheet 1 may have one side surface 1c with an annular shape.

[0053] In one embodiment, the area of ​​the first main surface 1a and the second main surface 1b is 100 cm². 2 Above and 400cm 2 The thickness of ceramic sheet 1 is 30μm or more and 200μm or less, and the weight per unit area of ​​the main surface of ceramic sheet 1 is 0.015g / cm². 2 Above and 0.15g / cm 2 In this case, it can be said that ceramic plate 1 is relatively large and its weight is relatively small.

[0054] In one embodiment, at least one of the first main surface 1a and the second main surface 1b is a rough surface. In other words, at least one of the first main surface 1a and the second main surface 1b is roughened. The roughening treatment of the ceramic sheet 1 is performed, for example, in the manufacture of the green sheet, which is the raw material for the ceramic sheet 1. In one example, the roughening treatment is performed by forming a green sheet by coating a slurry onto a film with a predetermined unevenness beforehand and drying it. In this case, unevenness reflecting the predetermined unevenness is formed on the surface of the green sheet that is in contact with the film. Alternatively, the roughening treatment can be performed by pressing a material with a predetermined unevenness into contact with the surface of the green sheet. Alternatively, the roughening treatment can be performed by chemical etching or the like on the green sheet. In this case, the conditions of the roughening treatment are appropriately adjusted. The film with the predetermined unevenness is, for example, a film that has been chemically etched beforehand, but is not limited thereto. However, when a film or paper with a coating containing fillers is used as the film with the predetermined unevenness, the ceramic sheet 1 tends not to satisfy one of the parameters described below. It should be noted that the above-mentioned film is, for example, a resin film such as a polyethylene terephthalate (PET) film having a specified thickness and exhibiting flexibility.

[0055] In one embodiment, the arithmetic mean roughness (Ra) of the first principal surface 1a and the second principal surface 1b is 0.01 μm or more and 1.0 μm or less. The arithmetic mean roughness can be ≥0.01μm and ≤0.7μm, ≥0.01μm and ≤0.5μm, ≥0.01μm and ≤0.4μm, ≥0.1μm and ≤1.0μm, ≥0.1μm and ≤0.7μm, ≥0.1μm and ≤0.5μm, ≥0.1μm and ≤0.4μm, ≥0.15μm and ≤1.0μm, ≥0.15μm and ≤0.7μm, ≥0.15μm and ≤0.5μm, ≥0.15μm and ≤0.4μm, ≥0.2μm and ≤1.0μm, ≥0.2μm and ≤0.7μm, ≥0.2μm and ≤0.5μm, or ≥0.2μm and ≤0.4μm. The surface roughness (arithmetic mean roughness) of the first principal surface 1a and the second principal surface 1b is measured, for example, using a known surface roughness measuring device.

[0056] In one example, the kurtosis (Rku) of at least one of the first principal surface 1a and the second principal surface 1b is, for example, less than 3. Kurtosis refers to the sharpness of a surface as a measure of its sharpness. Surfaces with a kurtosis greater than 3 tend to have sharp concave and convex portions. Surfaces with a kurtosis less than 3 tend to have a flattened shape due to the unevenness distribution. Therefore, it can be said that at least one of the first principal surface 1a and the second principal surface 1b is unlikely to have sharp concave and convex portions. As a result, it is unlikely that there will be areas of localized stress concentration in the ceramic sheet 1, that is, it is unlikely that there will be areas in the ceramic sheet 1 that become crack initiation points. The kurtosis of each of the first principal surface 1a and the second principal surface 1b is measured, for example, using a known contact surface roughness measuring device such as a stylus type, or a non-contact surface roughness measuring device such as a laser microscope. The aforementioned kurtosis can be less than 3.46 or less, or less than 2.39.

[0057] In one example, the grain size of at least one of the first main surface 1a and the second main surface 1b is more than 90% and less than 130% of the grain size of the side surface 1c. In this case, the inter-grain deviation within the ceramic sheet 1 is small, and the ceramic sheet 1 can be evaluated as high quality. The grain size of at least one of the first main surface 1a and the second main surface 1b can be more than 90% and less than 115.1%, more than 107.1% and less than 115.1%, or more than 107.1% and less than 130% of the grain size of the side surface 1c. Each grain size is, for example, equivalent to the average grain size obtained by image analysis of a photograph taken using a scanning electron microscope at 3000x magnification. In one example, firstly, the area of ​​each grain in the photograph is calculated using image analysis software, and then the average area of ​​the grain is calculated. Next, assuming the shape of the grain is a circle, the diameter calculated from the average area is used as the grain size using the formula for the area of ​​a circle. The grain size of at least one of the first main surface 1a and the second main surface 1b, and the grain size of the side surface 1c, are, for example, 0.3 μm or more and 5.0 μm or less, but are not limited thereto. It should be noted that, generally, when the surface of a ceramic sheet has depressions smaller than the grain size, particle growth on that surface is hindered, and there is a tendency for the grain size of the surface to become smaller. Therefore, the grain size of the surface with the aforementioned smaller depressions tends to be significantly different from the grain size of other surfaces.

[0058] In one embodiment, when measuring the first main surface 1a and the second main surface 1b using a laser microscope, the average difference between the highest and lowest points of any 10 selected intervals in at least one of the first main surface 1a and the second main surface 1b is 1.0 μm or more and 4.0 μm or less. A surface whose average value meets the above-mentioned range can be evaluated as a surface where concave portions are formed at an appropriate depth and / or convex portions are formed at an appropriate height. In other words, a surface with an average value of 1.0 μm or more and 4.0 μm or less can be evaluated as not being a smooth surface, and can be evaluated as not having excessively large concave or convex shapes formed on that surface. The aforementioned average values ​​can be 1.0 μm or more and 3.0 μm or less, 1.0 μm or more and 2.5 μm or less, 1.0 μm or more and 2.0 μm or less, 1.2 μm or more and 4.0 μm or less, 1.2 μm or more and 3.0 μm or less, 1.2 μm or more and 2.5 μm or less, 1.2 μm or more and 2.0 μm or less, 1.5 μm or more and 4.0 μm or less, 1.5 μm or more and 3.0 μm or less, 1.5 μm or more and 2.5 μm or less, or 1.5 μm or more and 2.0 μm or less. These average values ​​can be obtained, for example, by performing shape analysis of the surface profile using a laser microscope. It should be noted that when calculating the average difference between the highest and lowest points of any of the 10 selected intervals on the first principal surface 1a and the second principal surface 1b, the standard deviation of the difference between the highest and lowest points of any of the 10 selected intervals can also be calculated. The standard deviation of the difference between the highest and lowest points of any 10 intervals of at least one of the first principal plane 1a and the second principal plane 1b is, for example, greater than 0.10 and less than 1.0, but not limited thereto. The standard deviation of the difference between the highest and lowest points of any 10 intervals of at least one of the first principal plane 1a and the second principal plane 1b can be calculated by known methods.

[0059] Here, refer to Figure 2 An example of a method for calculating the difference between the highest and lowest points of a randomly selected interval of the first principal surface 1a will be explained. Here, the aforementioned randomly selected interval corresponds to an interval of 150 μm in length randomly extracted from a region obtained by photographing a portion of the first principal surface 1a with a 100x objective lens. Figure 2 This is a graph showing the shape analysis results of a selected section of the surface profile based on the first principal plane 1a of a laser microscope. Figure 2 In the diagram, the vertical axis represents height, and the horizontal axis represents the measured distance. Figure 2 The curve shown Figure 10In the diagram, line 11 represents the highest point of a randomly selected interval, line 12 represents the lowest point of a randomly selected interval, and arrow 13 represents the difference between the highest and lowest points of a randomly selected interval. Thus, by performing shape analysis on the surface profile of a randomly selected interval of the first main surface 1a, the difference between the highest and lowest points of that randomly selected interval can be calculated. By using the same method to calculate the differences between the highest and lowest points of nine randomly selected intervals of the first main surface 1a that are different from the aforementioned randomly selected interval, the average value of the differences between the highest and lowest points of ten randomly selected intervals can be calculated. In one example, the ten randomly selected intervals are intervals extracted from the same first main surface 1a. In this case, at least one of the aforementioned nine randomly selected intervals can be an interval extracted from an area obtained by photographing a portion of the first main surface 1a, but is not limited to this. Each of the ten randomly selected intervals of the first main surface 1a can also be an interval extracted from a different photographing area. In another example, the ten randomly selected intervals are intervals extracted from different first main surfaces 1a. That is, the 10 randomly selected intervals are extracted from 10 ceramic pieces 1. It should be noted that the average difference between the highest and lowest points of the 10 randomly selected intervals of the second main surface 1b is also calculated using the above method. The 10 randomly selected intervals of the second main surface 1b can be extracted from one ceramic piece 1 or from multiple ceramic pieces 1.

[0060] The coefficient of variation (Cv value) of the difference between the highest and lowest points of the 10 selected intervals mentioned above is, for example, 0.05 or higher and 0.3 or lower. Surfaces with a coefficient of variation satisfying the above value range can be evaluated as surfaces with a tendency to uniformly form unevenness. The aforementioned coefficient of variation can be 0.05 or higher and 0.20 or lower, 0.05 or higher and 0.15 or lower, 0.05 or higher and 0.13 or lower, 0.09 or higher and 0.3 or lower, 0.09 or higher and 0.2 or lower, 0.09 or higher and 0.15 or lower, 0.09 or higher and 0.13 or lower, 0.10 or higher and 0.3 or lower, 0.10 or higher and 0.20 or lower, 0.10 or higher and 0.15 or lower, or 0.10 or higher and 0.13 or lower. The coefficient of variation of the difference between the highest and lowest points of any 10 intervals of the first principal plane 1a is equivalent to the value obtained by dividing the standard deviation of the difference by the average value mentioned above (standard deviation of the difference / average value mentioned above).

[0061] For example, the average difference between the highest and lowest points of any 10 intervals of the first main surface 1a is set as the first average value, the average difference between the highest and lowest points of any 10 intervals of the second main surface 1b is set as the second average value, the coefficient of variation of the difference between the highest and lowest points of any 10 intervals of the first main surface 1a is set as the first coefficient of variation, and the coefficient of variation of the difference between the highest and lowest points of any 10 intervals of the second main surface 1b is set as the second coefficient of variation. In this case, in one embodiment, the difference between the first average value and the second average value may be 0.1 μm or more and less than 0.8 μm, and the difference between the first coefficient of variation and the second coefficient of variation may be 0 or more and less than 0.1. In this case, it is less likely that the strength of the ceramic sheet 1 will decrease due to at least one of the surface shapes of the first main surface 1a and the second main surface 1b. Furthermore, it is less likely that the first main surface 1a or the second main surface 1b of one ceramic sheet 1 will be tightly fitted to the first main surface 1a or the second main surface 1b of another ceramic sheet 1. Therefore, when stacking ceramic sheets 1, it is less likely that two adjacent ceramic sheets 1 will stick together and be difficult to separate, or that the two ceramic sheets 1 will be picked up.

[0062] In one embodiment, when measuring the first principal surface 1a and the second principal surface 1b using a laser microscope, in at least one of the first principal surface 1a and the second principal surface 1b, the cumulative relative frequency of the approximate straight line with a slope of -0.1 or higher and less than 0.1 per 1.314 μm is 20% or higher and less than 70%, the cumulative relative frequency of the approximate straight line with a slope of -0.3 or higher and less than 0.3 is 85% or higher and less than 100%, and the cumulative relative frequency of the approximate straight line with a slope of -1.5 or higher and less than 1.5 is 99.9% or higher and less than 100%. A surface whose approximate straight line satisfies all of the above numerical ranges can be evaluated as a surface with relatively few smooth portions, a majority of smooth concave and convex portions, and almost no large concave or convex portions. The cumulative relative frequency of the approximate curve with a slope of -0.1 or higher and less than 0.1 can be 20% or higher and less than 60.3%, or 20% or higher and less than 48.9%. The cumulative relative frequencies of the aforementioned approximate curves with a slope of -0.3 or less than 0.3 can be either 94.2% or less than 100%, or 97.2% or less than 100%. The cumulative relative frequencies of the aforementioned approximate curves with a slope of -1.5 or less than 1.5 can be 100%. The cumulative relative frequencies of the aforementioned approximate straight lines with a slope of -1.0 or less than 1.0 can be either 99.0% or less than 100%, or 99.9% or less than 100%. The cumulative relative frequencies of the aforementioned approximate straight lines with a slope of -0.5 or less than 0.5 can be either 99.0% or less than 100%, 99.1% or less than 100%, or 99.8% or less than 100%. In both the first principal plane 1a and the second principal plane 1b, the cumulative relative frequency of the aforementioned approximate line with a slope of -0.3 or higher and less than 0.3 is 85% or higher and less than 100%, and the cumulative relative frequency of the aforementioned approximate line with a slope of -1.5 or higher and less than 1.5 is 99.9% or higher and less than 100%; the cumulative relative frequency of the aforementioned approximate line with a slope of -0.3 or higher and less than 0.3 is 94.2% or higher and less than 100%, and the cumulative relative frequency of the aforementioned approximate line with a slope of -1.5 or higher and less than 1.5 is 99.9% or higher and less than 100%; or the cumulative relative frequency of the aforementioned approximate line with a slope of -0.3 or higher and less than 0.3 is 97.2% or higher and less than 100%, and the cumulative relative frequency of the aforementioned approximate line with a slope of -1.5 or higher and less than 1.5 is 99.9% or higher and less than 100%.

[0063] The slope of the aforementioned approximate straight line of the first principal surface 1a can be calculated from the shape analysis results of the surface profile of an arbitrary interval of the first principal surface 1a obtained based on a laser microscope. Similarly, the slope of the aforementioned approximate straight line of the second principal surface 1b can be calculated from the shape analysis results of the surface profile of an arbitrary interval of the second principal surface 1b obtained based on a laser microscope. Here, refer to... Figure 3 An example of a method for calculating the slope of an approximate straight line calculated for every 1.314 μm of any one interval of the first principal plane 1a is given. Figure 3 It is Figure 2 A magnified portion of the curve graph. Figure 3 In the diagram, the vertical axis represents height, and the horizontal axis represents the measured distance. Figure 3 The curve 20 shown is formed by multiple points (plot). These points show the surface shape profile obtained at 0.146 μm intervals. Therefore, the slope of the approximate straight line can be calculated by constructing an approximate straight line using 10 consecutive points that include the starting point of one of the aforementioned optional intervals.

[0064] In one implementation, the slope of the approximate straight line is calculated once every 1 point offset from the starting point. Thus, the slope is calculated. Figure 3 The slopes of approximate lines 21 to 24, etc., are shown. The calculation of the slopes of such approximate lines continues until the slope of the approximate line formed using 10 points including the endpoint of the aforementioned chosen interval is calculated. Through this process, the slopes of multiple approximate lines are calculated for the aforementioned chosen interval of the first principal surface 1a. Furthermore, using the same method, the slopes of multiple approximate lines are also calculated for each of the nine chosen intervals of the first principal surface 1a that are different from the aforementioned chosen interval. Then, the slopes of all approximate lines obtained from the aforementioned ten chosen intervals are classified according to their respective levels. Through this process, the cumulative relative frequency of the slope of the approximate line calculated per 1.314 μm of the first principal surface 1a is obtained when the slope is at a specified level (e.g., a slope of -0.1 or higher and 0.1 or lower). It should be noted that the cumulative relative frequency of the slope of the approximate line calculated per 1.314 μm of the second principal surface 1b is also calculated using the same method as for the first principal surface 1a.

[0065] In one embodiment, the three-point bending strength of ceramic sheet 1 is, for example, 400 MPa or more, and the Weibull coefficient of ceramic sheet 1 is, for example, 9.0 or more. In this case, the strength of ceramic sheet 1 tends to be comparable to that of ceramic sheets without roughening treatment. The aforementioned three-point bending strength can be 410 MPa or more, or 430 MPa or more. It should be noted that the three-point bending strength of ceramic sheet 1 is measured, for example, according to the method of JIS R 1601:2008. In addition, the Weibull coefficient is obtained from the measurement results of the three-point bending strength of multiple ceramic sheets 1.

[0066] The following describes an example of a method for manufacturing ceramic sheet 1 according to one embodiment. First, a slurry is prepared by mixing the aforementioned ceramic powder, solvent, and binder (first step). In the first step, for example, the ceramic powder, solvent, and binder are mixed using a pulverizing device such as a ball mill, bead mill, planetary mill, or spray mill to prepare the slurry. For example, the ceramic powder, solvent, and binder are mixed using a pulverizing device for 10 minutes or more and 5000 minutes or less. In the preparation of the slurry, the pulverizing time of the ceramic powder can be, for example, 30 minutes or less, 25 minutes or less, or 20 minutes or less. Furthermore, in the first step, the slurry can be degassed using a known method. Agglomerated particles of the aforementioned stabilized zirconia powder or other ceramic powder may be present in the slurry. In other words, the slurry can be prepared with these agglomerated particles present.

[0067] There are no restrictions on the types of solvents included in the slurry as solvents, and appropriate solvents can be selected from those used in the manufacture of ceramic sheets in the past. Examples of solvents include water; alcohols such as ethanol, 2-propanol, 1-butanol, and 1-hexanol; ketones such as acetone and 2-butanone; aliphatic hydrocarbons such as pentane, hexane, and heptane; aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; and acetates such as methyl acetate, ethyl acetate, and butyl acetate. The above solvents can be single solvents or mixtures of two or more. The proportion of solvent relative to the total mass of the slurry is, for example, 20% by mass or more and 90% by mass or less.

[0068] There are no restrictions on the type of binder used in the slurry; it can be appropriately selected from organic and inorganic binders used in the manufacture of ceramic sheets in the past. Examples of organic binders include ethylene copolymers, styrene copolymers, acrylate and methacrylate copolymers, vinyl acetate copolymers, maleic acid copolymers, vinyl acetal resins, vinyl formaldehyde resins, polyvinyl butyral resins, vinyl alcohol resins, cellulose resins such as ethyl cellulose, and waxes. Examples of inorganic binders include at least one selected from zirconium oxide sol, silica sol, alumina sol, and titanium dioxide sol.

[0069] The mass ratio of ceramic powder to binder in the slurry is not particularly limited. For example, the binder can be 5 to 30 parts by mass or 10 to 20 parts by mass relative to 100 parts by mass of ceramic powder. The binder content in the slurry is appropriately selected considering the particle size of the ceramic powder, the required strength and flexibility of the ceramic sheet to be manufactured, etc. It should be noted that known dispersants, plasticizers, lubricants, surfactants, and / or defoamers can be further added to the slurry as needed.

[0070] Next, the slurry is coated in sheet form and then dried to form a green sheet (second step). In the second step, firstly, the slurry is coated onto the substrate film (the coated surface of the substrate film). Then, the coated slurry is dried to form a green sheet on the substrate film. Methods for coating the slurry into sheet form onto the substrate film include, for example, casting and doctor blade coating. It should be noted that screen printing can be performed in the second step, using a slot die coater, lip coater, gravure coater, etc.

[0071] In one embodiment, a surface treatment based on an alkaline reagent is performed on the coated surface of the substrate film. Examples of methods for alkaline reagent-based surface treatment include etching of the substrate film surface using alkaline reagents such as aqueous sodium hydroxide solution, aqueous potassium hydroxide solution, or aqueous ammonia solution. The concentration of the alkaline reagent can be, for example, 0.5% by mass or more and 50% by mass or less. In another embodiment, a surface treatment using plasma or an ion beam can be performed on the coated surface of the substrate film. Examples of methods for surface treatment using plasma or an ion beam include dry etching using plasma or an ion beam. A single surface treatment or multiple surface treatments can be applied to the coated surface of the substrate film. The arithmetic mean roughness of the coated surface of the substrate film is 0.2 μm or more and 0.7 μm or less. The arithmetic mean roughness can be 0.2 μm or more and 0.6 μm or less, 0.3 μm or more and 0.7 μm or less, or 0.3 μm or more and 0.6 μm or less. The aforementioned arithmetic mean roughness is measured, for example, using a known surface roughness measuring device. By applying a slurry to the substrate film (the coated surface of the substrate film), the contact surface in the green sheet that contacts the substrate film (corresponding to the first main surface 1a of the subsequent ceramic sheet 1) has an arithmetic mean roughness that reflects the aforementioned specified arithmetic mean roughness.

[0072] In one embodiment, a resin film with a defined irregularity is used as the substrate film, for example. By applying a slurry onto the resin film, irregularities reflecting the defined irregularities are formed on the contact surface (corresponding to the first main surface 1a of the subsequent ceramic sheet 1) in the green sheet that contacts the resin film.

[0073] Next, a degreased body of the green sheet is formed by degreasing the green sheet (third step). In the third step, the green sheet is first peeled off from the substrate film. Then, the green sheet is heat-treated to form a degreased body from which organic components (binders and other organic additives) have been removed from the green sheet. The heat treatment is not particularly limited and can be performed using conventionally known methods. The conditions for the heat treatment in the third step are not particularly limited and can be set to known conditions, for example. For example, the degreased body is formed by heating the green sheet at a heat treatment temperature of 100°C or higher and 450°C or lower, and at a heat treatment time of approximately 2 hours or higher and approximately 50 hours. The degreased body formed in the third step is an intermediate ceramic sheet, equivalent to a sheet-like component after the organic components have been removed from the green sheet. The heat treatment temperature in the third step can be 370°C or higher and 450°C or lower, 400°C or higher and 450°C or lower, or 400°C. Here, the heat treatment temperature refers to the highest temperature in the heat treatment, and the heat treatment time refers to the time held at the aforementioned heat treatment temperature.

[0074] In the third step, heat treatment can be performed with multiple green sheets overlapping each other. In this case, spacers such as alumina sheets can be placed between adjacent green sheets, or no spacers can be placed. If the contact surfaces of the green sheets are unevenly formed in the second step, the third step can be used to heat treat a laminate consisting only of multiple green sheets. In this case, the aforementioned unevenness is formed on the contact surfaces of each green sheet, thus reducing the contact area between adjacent green sheets. Therefore, in the third step, adhesion between green sheets and between degreased products can be prevented. Here, an organic powder for effectively preventing adhesion between green sheets can be dispersed between adjacent green sheets. The organic powder can be, for example, natural organic powder such as edible corn starch, or synthetic organic resin powder such as sublimable resin powder such as melamine cyanurate. The amount of organic powder used is, for example, about 0.005 mg / cm² relative to the area of ​​the green sheets. 2 Above and approximately 2 mg / cm 2 The number of overlapping green slices depends on the area of ​​the green slices, for example, more than 2 slices and less than 40 slices.

[0075] Next, the degreased body is fired to form a ceramic sheet (fourth step). In the fourth step, the degreased body is fired at a high temperature to form a ceramic sheet as a sintered body. The firing conditions in the fourth step are not particularly limited, and are set to known conditions for example. The sintering temperature (firing temperature) in the fourth step is, for example, 1200°C or higher and 1600°C or lower, 1200°C or higher and 1500°C or lower, 1200°C or higher and 1450°C or lower, 1300°C or higher and 1600°C or lower, 1300°C or higher and 1500°C or lower, 1300°C or higher and 1450°C or lower, 1350°C or higher and 1600°C or lower, 1350°C or higher and 1500°C or lower, or 1350°C or higher and 1450°C or lower. The heating time from the above heat treatment temperature (e.g., 400°C, 450°C, etc.) to the above sintering temperature is, for example, 8 hours or higher and 30 hours or lower. The fourth step is carried out, for example, in an air atmosphere or a low-oxygen atmosphere. In the fourth step, similar to the third step, multiple degreased bodies can be fired in an overlapping state. In this case, the resting state of the multiple degreased bodies is the same as, but not limited to, the resting state of the multiple green sheets in the third step.

[0076] For the ceramic sheet 1 of one embodiment described above, the arithmetic mean roughness of each of the first main surface 1a and the second main surface 1b is 0.1 μm or more and 1.0 μm. Furthermore, when the first main surface 1a and the second main surface 1b are measured using a laser microscope, the average difference between the highest and lowest points of at least one of the first main surface 1a and the second main surface 1b in any of the selected 10 intervals is 1.0 μm or more and 4.0 μm or less; the coefficient of variation of the difference between the highest and lowest points in the selected 10 intervals is 0.05 or more and 0.3 or less; the cumulative relative frequency of the slope of the approximate straight line calculated per 1.314 μm being -0.1 or more and 0.1 or less is 20% or more and 70% or less; the cumulative relative frequency of the slope of the approximate straight line being -0.3 or more and 0.3 or less is 85% or more and 100% or less; and the cumulative relative frequency of the slope of the approximate straight line being -1.5 or more and 1.5 or less is 99.9% or more and 100% or less. Therefore, at least one of the first main surface 1a and the second main surface 1b of the ceramic sheet 1 is not a smooth surface, but a surface with few large-sized concave and convex parts, and with smooth concave and convex parts making up the majority of the surface. In other words, at least one of the first main surface 1a and the second main surface 1b of the ceramic sheet 1 can be said to be a surface with smooth undulations throughout and almost no large concave and convex parts. Therefore, it is not easy for the strength of the ceramic sheet 1 to be reduced due to the surface shape of at least one of the first main surface 1a and the surface shape of the second main surface 1b. In addition, at least one of the first main surface 1a and the second main surface 1b of the ceramic sheet 1 is not easy to fit closely with the first main surface 1a and the second main surface 1b of another ceramic sheet 1. Therefore, according to one embodiment, a ceramic sheet 1 can be provided that can prevent the occurrence of two pieces picking up while maintaining the strength of the ceramic sheet 1.

[0077] In one embodiment, the cumulative relative frequency of an approximate straight line with a slope of -1.0 or higher and 1.0 or lower can be 99.0% or higher and 100% or lower, and the cumulative relative frequency of an approximate straight line with a slope of -0.5 or higher and 0.5 or lower can be 99.0% or higher and 100% or lower. In this case, it can be said that at least one of the first main surface 1a and the second main surface 1b is a surface with almost no large concave or convex portions. Therefore, it is less likely that the strength of the ceramic sheet 1 will decrease due to the surface shape of at least one of the first main surface 1a and the surface shape of the second main surface 1b.

[0078] In one embodiment, the cumulative relative frequency of approximate straight lines with a slope of -0.3 or higher and less than 0.3 in both the first main surface 1a and the second main surface 1b is 85% or higher and less than 100%, and the cumulative relative frequency of approximate straight lines with a slope of -1.5 or higher and less than 1.5 is 99.9% or higher and less than 100%. In this case, it can be said that most of the concave and convex portions formed on both the first main surface 1a and the second main surface 1b are smooth concave and convex portions. Therefore, it is less likely that the strength of the ceramic sheet 1 will decrease due to the surface shape of the first main surface 1a and the surface shape of the second main surface 1b.

[0079] In one embodiment, the ceramic sheet 1 has a side surface 1c connecting a first main surface 1a and a second main surface 1b, wherein the grain size of at least one of the first main surface 1a and the second main surface 1b can be more than 90% and less than 130% of the grain size of the side surface 1c. In this case, it can be said that at least one of the first main surface 1a and the second main surface 1b is a surface free from particle growth inhibition caused by the formation of depressions, i.e., free from residual stress caused by the inhibition of particle growth on the roughened surface after sintering. Therefore, it is preferable that the strength reduction of the ceramic sheet 1 is less likely to occur due to at least one of the surface shapes of the first main surface 1a and the second main surface 1b.

[0080] Regarding the two-piece picking of the aforementioned ceramic sheet, the larger the area of ​​the main surface of the ceramic sheet, the easier it is to occur; the lighter the ceramic sheet, the easier it is to occur. Therefore, in one embodiment, the thickness of the ceramic sheet 1 can be 30 μm or more and 200 μm or less, and the area of ​​each of the first main surface 1a and the second main surface 1b is 100 cm². 2 Above and 400cm 2 Below, the weight of ceramic piece 1 is 0.015 g / cm³. 2 Above and 0.15g / cm 2 In this case, the ceramic sheet 1 is relatively large, and the weight per unit area of ​​the main surface of the ceramic sheet 1 is relatively small. Here, the surface shape of the present disclosure is applied to the ceramic sheet 1. Therefore, when adsorption and transport are performed only on the uppermost ceramic sheet 1 in a stack formed by multiple ceramic sheets 1 directly overlapping each other, it is possible to suppress the picking up of two ceramic sheets 1.

[0081] In one embodiment, when the average difference between the highest and lowest points of any 10 intervals of the first main surface 1a is set as the first average value, and the average difference between the highest and lowest points of any 10 intervals of the second main surface 1b is set as the second average value, and the coefficient of variation of the difference between the highest and lowest points of any 10 intervals of the first main surface 1a is set as the first coefficient of variation, and the coefficient of variation of the difference between the highest and lowest points of any 10 intervals of the second main surface 1b is set as the second coefficient of variation, the difference between the first average value and the second average value can be 0.1 μm or more and less than 0.8 μm, and the difference between the first coefficient of variation and the second coefficient of variation can be 0.04 or more and less than 0.15. In this case, it is preferable that the strength reduction of the ceramic sheet 1 caused by at least one of the surface shapes of the first main surface 1a and the second main surface 1b is less likely to occur. Furthermore, in two adjacent ceramic sheets 1, it is preferable that the first main surface 1a or the second main surface 1b of one ceramic sheet 1 is not tightly fitted to the first main surface 1a or the second main surface 1b of the other ceramic sheet 1.

[0082] In one embodiment, the average kurtosis (Rku) of at least one of the first principal surface 1a and the second principal surface 1b is less than 3. In this case, it is not easy to create localized stress concentration sites in the ceramic sheet 1, i.e., sites that become crack initiation points in the ceramic sheet 1.

[0083] In one embodiment, the ceramic sheet 1 may be a zirconium oxide sheet containing at least one rare earth element selected from the group consisting of scandium, yttrium, and cerium in a total amount calculated based on oxides. In this case, the ceramic sheet 1 can function well as a solid electrolyte for SOFC.

[0084] The method for manufacturing a ceramic sheet 1 according to one embodiment described above includes: a first step in which a slurry is prepared by mixing ceramic powder, a binder, and a solvent; a second step in which a green sheet is formed by applying the slurry to a coated surface of a substrate film; a third step in which a degreased body of the green sheet is formed by degreasing the green sheet; and a fourth step in which the ceramic sheet is formed by firing the degreased body. In the third step, the green sheet is heat-treated at a heat treatment temperature of 100°C or higher and 450°C or lower, and in the fourth step, the degreased body is fired at a firing temperature of 1200°C or higher and 1600°C or lower. This provides a method for manufacturing a ceramic sheet 1 that can maintain the strength of the ceramic sheet 1 while preventing the picking up of two sheets.

[0085] In one embodiment, the coated surface may be surface-treated with an alkaline reagent, the heat treatment temperature may be 370°C or higher and 450°C or lower, and the firing temperature may be 1350°C or higher and 1450°C or lower. In this case, the ceramic sheet 1 can be manufactured more appropriately. Here, the arithmetic mean roughness of the coated surface of the substrate film may be 0.2 μm or higher and 0.7 μm or lower, or 0.3 μm or higher and 0.6 μm or lower. In this case, by transferring a suitable surface roughness to the surface of the green sheet in contact with the coated surface, a ceramic sheet 1 with a suitable surface roughness is formed. Therefore, it is possible to manufacture a ceramic sheet 1 that can maintain the strength of the ceramic sheet 1 while preventing the occurrence of two-piece pick-up.

[0086] In one embodiment, the ceramic powder may be a zirconia-based powder. In this case, a ceramic sheet 1 that can function well as a solid electrolyte for SOFCs can be manufactured.

[0087] In one embodiment, the second step can also be a step of forming a green sheet by applying a slurry in sheet form to the coated surface of a substrate film using a doctor blade. In this case, it is easy to manufacture ceramic sheets 1 with an arithmetic mean roughness of 0.01 μm or more and 1.0 μm or less for both the first and second main surfaces.

[0088] The above embodiments have described one aspect of this disclosure. Therefore, this disclosure is not limited to the above embodiments and variations are possible.

[0089] Example

[0090] The following examples illustrate the present disclosure in more detail, but the present disclosure is not limited to these examples.

[0091] <Example 1>

[0092] As the raw material powder, stabilized zirconia powder (manufactured by Daiichi Rare Element Chemical Industry Co., Ltd., trade name "10Sc1CeSZ", D50: approx. 0.5 μm) containing 10 mol% scandium oxide and 1 mol% cerium oxide in a solid solution was prepared. Next, 100 parts by weight of the raw material powder, 3.5 parts by weight of the dispersant (commercially available polycarboxylate type polymeric dispersant), and 50 parts by weight of the mixed solvent of toluene / ethyl acetate (mass ratio = 1:1) were contained in a nylon mill loaded with zirconia balls. Then, the raw material powder, dispersant, and mixed solvent were ground for 1 hour to prepare slurry I. Next, 18.5 parts by weight of the binder composed of methacrylic acid copolymer (number average molecular weight: 100,000, glass transition temperature: 0°C) and 1.5 parts by weight of dibutyl phthalate as a plasticizer were added to the above-mentioned nylon mill containing slurry I, and ground again for 20 hours to prepare slurry II. The obtained slurry II was transferred to a jacketed cylindrical degassing container equipped with an anchor mixer. While the mixer was rotating at 30 rpm, the mixture was concentrated and degassed under reduced pressure at a jacket temperature of 40°C. The viscosity at 25°C was adjusted to 3 Pa·s to prepare a raw material slurry for coating.

[0093] Next, in a coating apparatus, the aforementioned raw material slurry is coated onto a substrate film to form a coating. Here, the raw material slurry is continuously coated using a doctor blade method. Furthermore, as the substrate film, a PET film (film thickness: 100 μm, arithmetic mean roughness (Ra): 0.45 μm) that has undergone surface processing with an alkaline reagent is used, and the raw material slurry is coated onto the surface-processed surface (coated surface) of the PET film. Next, in the coating apparatus, the coating on the substrate film is dried at 100°C for approximately 1 hour to obtain a strip of green sheet for solid electrolyte with a thickness of approximately 0.12 mm. Then, the strip of green sheet is punched and peeled from the PET film using a Thomson cutter with one side approximately 200 mm thick to obtain an approximately square green sheet. Hereinafter, the surface of the green sheet that contacts the PET film, which serves as the substrate film (i.e., the contact surface of the green sheet) will sometimes be referred to as the "PET surface", and the surface located on the opposite side of the PET surface and that does not contact the substrate film (i.e., the exposed surface of the green sheet) will be referred to as the "air surface".

[0094] Next, two 200mm square porous alumina sheets (porosity: 20%, thickness: 0.2mm) are overlapped on a firing rack. Then, the green sheet is placed on top of the two overlapping porous alumina sheets. At this point, the green sheet is positioned on the porous alumina sheets with the air surface facing it. Then, using porous alumina sheets of the aforementioned size as spacers, the green sheet and the porous alumina sheets are alternately overlapped. Finally, another porous alumina sheet of the aforementioned size is placed on top of the uppermost porous alumina sheet to form a laminate. Then, 20 sets of the same laminates are prepared. Here, each laminate contains 5 green sheets.

[0095] Next, using an intermittent hot air circulating electric furnace, the temperature was raised from room temperature to 400°C over 30 hours to produce degreased sheets from each green sheet within the laminate. Then, 20 sets of laminates containing the degreased sheets were transferred to an intermittent firing furnace, where the temperature was raised from room temperature to 400°C over 3 hours, and then from 400°C to 1430°C over 24 hours. The temperature was then held at 1430°C for 3 hours, followed by cooling to 900°C over 6 hours. Finally, the sheets were cooled to room temperature within the firing furnace, thus producing 100 ceramic sheets with sides approximately 150 mm thick and a thickness of 90 μm. It should be noted that... Figure 4 (a) is a sheet surface image of the PET side of Example 1.

[0096] <Example 2>

[0097] A PET film (film thickness: 100 μm, arithmetic mean roughness (Ra): 0.35 μm) that has undergone surface processing with an alkaline reagent was used as the substrate film to make the thickness of the green sheet 160 μm. Otherwise, a green sheet with a side diameter of about 140 mm was produced by the same method as in Example 1.

[0098] Next, two 200mm square porous alumina sheets (porosity: 20%, thickness: 0.2mm) are overlapped on a firing rack. The green sheets are then placed on the two overlapping porous alumina sheets. The green sheets are then positioned on the porous alumina sheets with the air surface facing each other. Next, commercially available food-grade cornstarch is sprinkled onto the PET surface of the green sheets placed on the porous alumina sheets, and spread evenly using a brush. Commercially available food-grade cornstarch is also sprinkled onto the PET surface of another nine green sheets, and spread evenly using a brush. Next, nine green sheets placed on the porous alumina sheets are continuously overlapped with the PET surface of the food-grade cornstarch-sprinkled sheets facing upwards. Finally, an porous alumina sheet of the aforementioned dimensions is placed on top of the ten overlapping green sheets to form a laminate. Ten laminates are then prepared.

[0099] Next, using an intermittent hot air circulating electric furnace, the temperature was raised from room temperature to 400°C over 30 hours to produce degreased bodies from each green sheet within the laminate. Then, 10 sets of laminates containing the degreased bodies were transferred to an intermittent firing furnace, where the temperature was raised from room temperature to 400°C over 3 hours, and then from 400°C to 1390°C over 24 hours. The temperature was then held at 1390°C for 3 hours, and cooled to 900°C over 6 hours. Finally, the temperature was cooled to room temperature within the firing furnace, thus producing 100 ceramic sheets with sides approximately 105 mm thick and a thickness of 120 μm. It should be noted that... Figure 5 (a) is a sheet surface image of the PET side of Example 2.

[0100] <Example 3>

[0101] A long strip of green sheet was obtained using the same method as in Example 1. Next, the long strip of green sheet located on the substrate film was cut into approximately squares with sides of approximately 220 mm using a rotary cutter. This yielded a green sheet located on the substrate film with sides of approximately 220 mm (green sheet with substrate film). Next, a PET film (film thickness: 100 μm, arithmetic mean roughness (Ra): 0.45 μm, the same as the substrate film) that had undergone surface processing with an alkaline reagent was overlapped onto the exposed surface of the green sheet with substrate film. At this time, the surface-processed surface of the PET film was in contact with the exposed surface of the green sheet with substrate film. This formed a green sheet sandwiched between a pair of films. Next, the green sheet sandwiched between a pair of PET films was placed in the pressing section of a compression molding machine (manufactured by Shinto Metal Industries, Ltd., model "S-37.5"), and pressed at a pressing temperature of 25°C and a pressing pressure of 25.0 MPa (256 kgf / cm²). 2 Pressurization is applied for 20 seconds. After pressurization, the PET film in contact with the exposed surface is peeled off from the green sheet, and the green sheet with the substrate film is punched using a Thomson cutter with one side approximately 200 mm. Then, the substrate film is peeled off from the green sheet, thereby obtaining an approximately square green sheet. Through the same operation, 100 approximately square green sheets with one side approximately 200 mm are obtained.

[0102] Next, the above-mentioned raw sheets were degreased and fired using the same method as in Example 1 to produce 100 ceramic sheets with one side of about 150 mm and a thickness of 90 μm.

[0103] <Example 4>

[0104] A long strip of green sheet was obtained using the same method as in Example 2. Next, the long strip of green sheet located on the substrate film was cut into approximately squares with sides of approximately 220 mm using a rotary cutter. This yielded a green sheet located on the substrate film with sides of approximately 220 mm (green sheet with substrate film). Then, a PET film (film thickness: 100 μm, arithmetic mean roughness (Ra): 0.35 μm, the same as the substrate film) that had undergone surface processing with an alkaline reagent was overlapped onto the exposed surface of the green sheet with substrate film. At this time, the surface-processed surface of the PET film was in contact with the exposed surface of the green sheet with substrate film. This formed a green sheet sandwiched between a pair of films. Next, the green sheet sandwiched between a pair of PET films was placed in the pressing section of a compression molding machine (manufactured by Shinto Metal Industries, Ltd., model "S-37.5"), and pressed at a pressing temperature of 25°C and a pressing pressure of 25.0 MPa (256 kgf / cm²). 2 Pressurization is applied for 20 seconds. After pressurization, the PET film in contact with the exposed surface is peeled off from the green sheet, and the green sheet with the substrate film is punched using a Thomson cutter with one side approximately 140 mm. Then, the substrate film is peeled off from the green sheet, thereby obtaining an approximately square green sheet. Through the same operation, 100 approximately square green sheets with one side approximately 140 mm are obtained.

[0105] Next, the above-mentioned raw sheets were degreased and fired using the same method as in Example 2 to produce 100 ceramic sheets with one side of about 105 mm and a thickness of 120 μm.

[0106] <Comparative Example 1>

[0107] One hundred ceramic sheets were fabricated using a commercially available, untreated PET film (film thickness: 125 μm, arithmetic mean roughness (Ra): 0.07 μm) as the substrate film, otherwise fabricated using the same method as in Example 1. It should be noted that... Figure 6 (a) is a sheet surface image of the PET side of Comparative Example 1. Figure 7 (a) is a sheet surface image of the air surface of Comparative Example 1.

[0108] <Comparative Example 2>

[0109] A commercially available PET film coated with a filler-containing resin (film thickness: 100 μm, arithmetic mean roughness (Ra): 0.39 μm) was used as the substrate film, and 100 ceramic sheets were fabricated using the same method as in Example 1. It should be noted that... Figure 8 (a) is a sheet surface image of the PET side of Comparative Example 2.

[0110] <Comparative Example 3>

[0111] Using a commercially available PET film coated with a filler-containing resin (film thickness: 100 μm, arithmetic mean roughness (Ra): 0.89 μm) as the substrate film, 100 ceramic sheets were otherwise produced by the same method as in Example 2.

[0112] <Comparative Example 4>

[0113] A long strip of green sheet was obtained using the same method as in Example 1. The long strip of green sheet was punched and peeled from the PET film using a Thomson cutter with one side approximately 180 mm, thereby obtaining an approximately square green sheet.

[0114] (Paste Preparation & Printing)

[0115] 8.2 g of 10 g of ethyl cellulose (approximately 49% ethoxylated) (manufactured by Wako Pure Chemical Industries, Ltd.) was dissolved in 73.8 g of α-terpineol (manufactured by Kanto Chemical Co., Ltd.) to prepare a paste binder solution. 40 g of EPOSTAR MA1002 (manufactured by Nippon Shokubai Co., Ltd., average particle size: 2 μm) as organic particles was added to 82 g of the obtained binder solution, and the mixture was prepared by scraping with a spatula to obtain an organic particle paste. Next, the organic particle paste was printed onto the PET surface of a raw sheet using a screen printing machine (manufactured by NEWLONG Precision Industries, Ltd.: LS-150 type) and a printing plate (screen: Tetron, #500) with a pattern having approximately 155 mm on each side. The organic particle paste was then air-dried to form a raw sheet with a printed layer. Finally, using a Thomson cutter, approximately square raw sheets with printed layers, each with a side of approximately 150 mm, were cut. Through the same operation, 100 approximately square raw films with a printed layer, each with a side of about 150 mm, were obtained.

[0116] (Defatting and firing)

[0117] Commercially available food-grade cornstarch is sprinkled onto the printed layers (PET side) of 10 approximately square raw sheets with printed layers, and the cornstarch is spread evenly using a brush. Next, 10 raw sheets with the cornstarch sprinkled on them, PET side up, are stacked consecutively. Each raw sheet is then positioned on two overlapping porous alumina sheets (approximately 200 mm on one side, porosity approximately 20%, thickness 0.2 mm). Then, a porous alumina sheet (approximately 160 mm on one side, porosity approximately 20%, thickness 0.2 mm) is placed on top of the 10 overlapping raw sheets, forming a laminate. Ten sets of laminates are then prepared.

[0118] Next, using an intermittent hot air circulating electric furnace, the temperature was raised from room temperature to 400°C over 30 hours to produce degreased bodies from each green sheet within the laminate. Then, 10 sets of laminates containing the degreased bodies were transferred to an intermittent firing furnace, where the temperature was raised from room temperature to 400°C over 3 hours, and then from 400°C to 1390°C over 24 hours. They were then held at 1350°C for 3 hours and cooled to 900°C over 6 hours. Finally, they were cooled to room temperature within the firing furnace, thus producing 100 ceramic sheets with sides approximately 115 mm thick and a thickness of 90 μm. It should be noted that... Figure 9 (a) is a sheet surface image of the PET side of Comparative Example 4.

[0119] <Comparative Example 5>

[0120] A long strip of green sheet was obtained using the same method as in Example 1. The strip of green sheet was punched and peeled from the PET film using a Thomson cutter with one side approximately 160 mm in diameter, resulting in an approximately square green sheet. The green sheet was then placed on a heating table, with the air surface of the green sheet facing the heating table. A die was then pressed onto the PET surface of the green sheet. This formed a laminate consisting of the heating table, the green sheet, and the die stacked sequentially. Here, the pressing portion and the substrate portion of the die are made of resin. The protrusions included in the pressing portion are hemispherical, with a height of 25 μm, a diameter of 50 μm, and a spacing of 100 μm between adjacent protrusion vertices. Furthermore, the pressing portion is coated with fluororesin.

[0121] Next, the aforementioned laminate is placed in the pressing section of a compression molding machine (manufactured by Shinto Metal Industries, Ltd., model "S-37.5"), and pressed at a temperature of 25°C and a pressure of 22.5 MPa (230 kgf / cm²). 2 Pressurize the green sheet under a pressing time of 2 seconds. After pressing, peel the mold off the green sheet to obtain a green sheet with multiple indentations. Through the same operation, obtain 100 green sheets with approximately 160 mm sides that are approximately square.

[0122] Two 200mm square porous alumina sheets (porosity: 20%, thickness: 0.2mm) are overlapped on a firing rack. Next, the green sheet is placed on top of the two overlapping porous alumina sheets. The green sheet is then positioned on the porous alumina sheets with the air surface facing it. Alumina porous sheets of the aforementioned size are then used as spacers, and the green sheet and the porous alumina sheets are alternately overlapped. Finally, another porous alumina sheet of the aforementioned size is placed on top of the uppermost porous alumina sheet to form a laminate. Twenty sets of the same laminate are then prepared. Each laminate contains five green sheets.

[0123] Next, using an intermittent hot air circulating electric furnace, the temperature was raised from room temperature to 400°C over 30 hours to produce degreased bodies from each green sheet within the laminate. Then, 10 sets of laminates containing the degreased bodies were transferred to an intermittent firing furnace, where the temperature was raised from room temperature to 400°C over 3 hours, and then from 400°C to 1430°C over 24 hours. They were then held at 1410°C for 3 hours and cooled to 900°C over 6 hours. Finally, they were cooled to room temperature within the firing furnace, thus producing 100 ceramic sheets with sides approximately 120 mm thick and a thickness of 90 μm. It should be noted that... Figure 10 (a) is a sheet surface image of the PET side of Comparative Example 5.

[0124] <Comparative Example 6>

[0125] A long strip of green sheet was obtained using the same method as in Example 1. The strip of green sheet was punched and peeled from the PET film using a Thomson cutter with one side approximately 160 mm in diameter, resulting in an approximately square green sheet. Next, the obtained green sheet was clamped between two roughening papers (arithmetic mean roughness (Ra): 3.1 μm, thickness: 0.335 mm) and subjected to pressure treatment using a compression forming machine (manufactured by Shinto Metal Industries, Ltd., model "S-37.5"). The pressure treatment conditions were set as follows: pressure temperature 25°C, pressure 273 kN, and holding time 15 seconds. The green sheet was rotated 90° after each pressure treatment, for a total of four pressure treatments. After the pressure treatment, the two roughening papers were peeled off the green sheet to form a roughened green sheet. Then, 100 roughened green sheets were obtained using the same method.

[0126] Two 200mm square porous alumina sheets (porosity: 20%, thickness: 0.2mm) are overlapped on a firing rack. Next, a roughened green sheet is placed on top of the two overlapping porous alumina sheets. The roughened green sheet is then placed on the porous alumina sheets with the air surface facing it. Alumina porous sheets of the aforementioned size are then used as spacers, and the green sheet and the porous alumina sheets are alternately overlapped. Finally, another porous alumina sheet of the aforementioned size is placed on the topmost porous alumina sheet to form a laminate. Twenty such laminates are then prepared. Each laminate contains five green sheets.

[0127] Next, using an intermittent hot air circulating electric furnace, the temperature was raised from room temperature to 400°C over 30 hours to produce degreased bodies from each green sheet within the laminate. Then, 10 sets of laminates containing the degreased bodies were transferred to an intermittent firing furnace, where the temperature was raised from room temperature to 400°C over 3 hours, and then from 400°C to 1430°C over 24 hours. They were then held at 1410°C for 3 hours and cooled to 900°C over 6 hours. Finally, they were cooled to room temperature within the firing furnace, thus producing 100 ceramic sheets with sides approximately 120 mm thick and a thickness of 90 μm. It should be noted that... Figure 11 (a) is a sheet surface image of the PET side of Comparative Example 6.

[0128] (Surface roughness)

[0129] The arithmetic mean roughness (Ra) of the ceramic sheets of Examples 1-4 and Comparative Examples 1-6 was measured using a stylus-type surface roughness tester (Surftest SJ-201 manufactured by Mitutoyo Co., Ltd., standard: JISB0601:2001). The surface roughness of Examples 1-4 and Comparative Examples 1-6 is shown in Table 1 below.

[0130] (Surface shape height difference)

[0131] First, 10 ceramic sheets were randomly selected from each of the 100 ceramic sheets prepared in Examples 1-4 and Comparative Examples 1-6. Next, using a laser microscope (Lasertec Corporation, OPTELICS HYBRID+), a randomly selected interval was extracted from each surface of each ceramic sheet, and the surface shape profile of that interval was analyzed. Specifically, a surface shape profile of 150 μm in length was measured in a randomly selected interval of an image of the sheet surface taken with a 100x objective lens. The highest and lowest points were determined from this surface shape profile, and the difference between the highest and lowest points was taken as the height difference. Thus, a total of 10 intervals (each interval being 150 μm) were calculated from the 10 ceramic sheets selected from each of Examples 1-4 and Comparative Examples 1-6. Then, the mean, standard deviation, and coefficient of variation of the height difference were calculated. The mean and coefficient of variation of the height differences for Examples 1-4 and Comparative Examples 1-6 are shown in Table 1 below.

[0132] Figure 4 (b) shows the measurement results of the surface shape profile of the PET surface in Example 1. Figure 5 (b) shows the measurement results of the surface shape profile of the PET surface in Example 2. Figure 6 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 1. Figure 7 (b) shows the measurement results of the surface shape profile of the air surface in Comparative Example 1. Figure 8(b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 2. Figure 9 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 4. Figure 10 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 5. Figure 11 (b) shows the measurement results of the surface shape profile of the PET surface in Comparative Example 6. Figure 4 (b) Figure 11 In figures (b), the horizontal axis represents the measured distance, and the vertical axis represents the height. Figure 4 (b) Figure 11 Figures (b) show the surface shape profiles of five optional sections. For improved readability, in... Figure 4 (b) Figure 11 In Figure (b), the initial heights of the surface shape profiles are staggered.

[0133] (Surface shape slope)

[0134] The slope of the surface shape was calculated from the surface shape profile described above. Specifically, the surface shape profile was composed of points obtained at 0.146 μm intervals, and the slope of an approximate straight line drawn from 10 adjacent points (length: 1.314 μm) was calculated. This approximate straight line slope calculation was performed until the slope of an approximate straight line formed by 10 points including the endpoint of one of the selected intervals was calculated. The slope calculation of the approximate straight line was performed on each of the 10 selected ceramic sheets. Then, for the slope data of all 10 intervals obtained, the frequency of each level was calculated, thereby calculating the cumulative relative frequency. The cumulative relative frequencies of the slopes of the approximate straight lines of Examples 1-4 and Comparative Examples 1-6 are shown in Table 2 below.

[0135] (Three-point bending strength)

[0136] For the ceramic sheets of Examples 1-6 and Comparative Examples 1-4, three-point bending strength tests were performed according to JIS R 1601:2008. In the three-point bending strength test of Example 1, 20 test pieces (length: 60 mm, width: 4 mm, thickness: 100 μm) prepared by the method described in Example 1 were prepared. Then, with the PET side of all test pieces facing down, the three-point bending strength was measured at room temperature. The average value of the measured three-point bending strength of the 20 test pieces was taken as the three-point bending strength of the ceramic sheet of Example 1. Furthermore, the Weibull coefficient was calculated from the measured three-point bending strength. In Examples 2-4 and Comparative Examples 1-6, the three-point bending strength was measured and the Weibull coefficient was calculated using the same method as in Example 1. The three-point bending strength and Weibull coefficient of Examples 1-4 and Comparative Examples 1-6 are shown in Table 3 below.

[0137] (Frequency of two-piece pickup)

[0138] In each of Examples 1-6 and Comparative Examples 1-4, 100 ceramic sheets were stacked. The ceramic sheets were stacked with their air surfaces facing upwards. This formed a stack consisting only of 100 overlapping ceramic sheets. Next, using four adsorption pads as adsorption transporters, the sheet transport tests described in (1) to (4) below were performed. Here, the four adsorption pads were positioned at the vertices of a 5cm square.

[0139] (1) Use four adsorption pads to vacuum adsorb the air surface of the uppermost ceramic sheet in the laminate, and lift the ceramic sheet vertically by 10cm.

[0140] (2) After (1) above, move the ceramic piece 50cm in the horizontal direction.

[0141] (3) After (2) above, let the ceramic sheet descend and release the adsorption, and let the sheet stand still.

[0142] (4) Repeat the above (1) to (3) 100 times consecutively.

[0143] In (1) above, sometimes the topmost piece is lifted up together with the piece below it (two-piece pickup occurs). During visual observation, the number of times two-piece pickup occurs is counted as the two-piece pickup frequency. The two-piece pickup frequencies of Examples 1-4 and Comparative Examples 1-6 are shown in Table 3 below.

[0144] (Grain size)

[0145] For the PET surface and side surface of the ceramic sheets prepared in Examples 1-4 and Comparative Examples 1-6 respectively, 3000x photographs were taken using a scanning electron microscope. Then, each photograph was analyzed using image analysis software to calculate the area of ​​all grains within the photograph. Next, assuming the grain shape to be circular, the diameter calculated from the average area using the formula for the area of ​​a circle was taken as the grain size. Based on the above, the ratio obtained by dividing the grain size of the PET surface of Examples 1-6 and Comparative Examples 1-4 by the grain size of the side surface was calculated. The ratio obtained by dividing the grain size of the PET surface of Examples 1-4 and Comparative Examples 1-6 by the grain size of the side surface is shown in Table 3 below.

[0146] (Kushin)

[0147] In the ceramic sheets prepared in Examples 1, 2, and Comparative Examples 1-6, the kurtosis of the PET surface of five randomly selected sheets was measured using a laser microscope (Lasertec Co., Ltd., OPTELICS (registered trademark) HYBRID+). The kurtosis of the air surface of five randomly selected sheets from Comparative Example 1 was also measured using the same method. The kurtosis, mean kurtosis, standard deviation, and coefficient of variation of the five sheets measured in Examples 1, 2, and Comparative Examples 1-6 are shown in Table 4 below.

[0148]

[0149] Symbol Explanation

[0150] 1… Ceramic tile, 1a… First main surface, 1b… Second main surface, 1c… Side surface.

Claims

1. A ceramic sheet having a first main surface and a second main surface, wherein, The arithmetic mean roughness of the first principal surface and the second principal surface is respectively greater than 0.01 μm and less than 1.0 μm. When measuring the first principal surface and the second principal surface using a laser microscope, in at least one of the first principal surface and the second principal surface... The average difference between the highest and lowest points in any 10 randomly selected intervals (each interval being 150 μm) is greater than 1.0 μm and less than 4.0 μm. The coefficient of variation of the difference between the highest and lowest points of the selected 10 intervals is greater than 0.05 and less than 0.

3. For every 1.314 μm, the cumulative relative frequency of the approximate straight line with a slope greater than -0.1 and less than 0.1 is greater than 20% and less than 70%. The cumulative relative frequency of the approximate straight line with a slope of -0.3 or higher and less than 0.3 is 85% or higher and less than 100%. The cumulative relative frequency of the approximate straight line with a slope of -1.5 or higher and below 1.5 is 99.9% or higher.

2. The ceramic sheet according to claim 1, wherein, The cumulative relative frequency of the approximate straight line with a slope of -1.0 or higher and less than 1.0 is 99.0% or higher and less than 100%.

3. The ceramic sheet according to claim 2, wherein, The cumulative relative frequency of the approximate straight line with a slope of -0.5 or higher and less than 0.5 is 99.0% or higher and less than 100%.

4. The ceramic sheet according to any one of claims 1 to 3, wherein, In both the first principal plane and the second principal plane, the cumulative relative frequency of the approximate straight line with a slope of -0.3 or higher and less than 0.3 is 85% or higher and less than 100%, and the cumulative relative frequency of the approximate straight line with a slope of -1.5 or higher and less than 1.5 is 99.9% or higher and less than 100%.

5. The ceramic sheet according to any one of claims 1 to 3, wherein, It also has a side surface that connects the first main surface and the second main surface. The grain size of at least one of the first main surface and the second main surface is more than 90% and less than 130% of the grain size of the side surface.

6. The ceramic sheet according to any one of claims 1 to 3, wherein the thickness is 30 μm or more and 200 μm or less, and the area of ​​each of the first main surface and the second main surface is 100 cm². 2 Above and 400cm 2 The following values ​​are 0.015 g / cm³. 2 Above and 0.15g / cm 2 the following.

7. The ceramic sheet according to any one of claims 1 to 3, wherein, The average kurtosis (Rku) of at least one of the first principal plane and the second principal plane is less than 3.

8. The ceramic sheet according to any one of claims 1 to 3, wherein the ceramic sheet contains at least one rare earth element selected from the group consisting of scandium, yttrium and cerium in a proportion of at least 3 mol% and less than 15 mol% based on the total amount of oxides.

9. The ceramic sheet according to any one of claims 1 to 3, wherein it is an electrolyte sheet for a solid oxide fuel cell.

10. A method for manufacturing a ceramic sheet, which is the method for manufacturing a ceramic sheet according to any one of claims 1 to 3, comprising: The first process, in which... A slurry is prepared by mixing ceramic powder, binder, and solvent. In the second process, a green sheet is formed by applying the slurry to the coated surface of the substrate film. The third step involves degreasing the raw sheet to form a degreased body of the raw sheet; and The fourth step involves firing the degreased body to form the ceramic sheet. In the third step, the green slices are heat-treated at a temperature above 100°C and below 450°C. In the fourth step, the degreased body is fired at a firing temperature of 1200°C or higher and 1600°C or lower.

11. The method for manufacturing ceramic sheets according to claim 10, wherein, The coated surface was treated with an alkaline reagent. The heat treatment temperature is above 370°C and below 450°C. The firing temperature is above 1350°C and below 1450°C.

12. The method for manufacturing ceramic sheets according to claim 10, wherein, The arithmetic mean roughness of the coated surface is greater than 0.2 μm and less than 0.7 μm.

13. The method for manufacturing ceramic sheets according to claim 11, wherein, The arithmetic mean roughness of the coated surface is greater than 0.3 μm and less than 0.6 μm.

14. The method for manufacturing ceramic sheets according to claim 10, wherein, The ceramic powder is a zirconia-based powder.

15. The method for manufacturing ceramic sheets according to claim 10, wherein, The second step is to form a green sheet by applying the slurry in sheet form to the coated surface of the substrate film using a doctor blade method.

Citation Information

Patent Citations

  • Solid oxide fuel cell electrolyte sheet manufacturing method

    JP2012079506A