Resin composition for forming processing machine washing
By using a specific ratio of acrylonitrile-styrene copolymer (AS) resin, rubber components, and surfactants in the detergent for molding machines, the problem of resin powder generation has been solved, achieving efficient cleaning and excellent workability.
Patent Information
- Application Number
- CN202580026741.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-10
- Filing Date
- 2025-04-01
- Publication Date
- 2026-11-20
AI Technical Summary
In existing molding and processing machines, detergents produce resin powder during granulation and transportation due to contact between granules, resulting in reduced workability. Therefore, it is necessary to improve both detergency and workability.
A resin composition containing acrylonitrile-styrene copolymer (AS) resin, rubber components, and aliphatic or aromatic surfactants is used. The rubber component content is controlled between 3 and 15 parts by weight, and the surfactant content is reasonably proportioned to reduce the generation of resin powder.
While maintaining the same washability, the operability of the molding machine has been significantly improved, the amount of resin powder has been reduced to less than 1g, and the washing efficiency has been improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This disclosure relates to a resin composition for washing a molding machine. This application claims priority to Japanese Patent Application No. 2024-063514, filed on April 10, 2024, the contents of which are incorporated herein by reference. Background Technology
[0002] In the molding process of thermoplastic resins, injection molding machines and extrusion molding machines are mainly used. After use, these molding machines leave behind the aforementioned resin, additives, and resin deterioration products generated during molding. If the next molding process is carried out with these residues still present, the residues will mix into the molded article, thereby deteriorating the appearance of the molded article or reducing the expected resin properties. Therefore, granular detergents are usually used before the next molding process (e.g., Patent Document 1).
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2008-201975 Summary of the Invention
[0006] The problem that the invention aims to solve
[0007] However, conventional detergents, such as those in Patent Document 1, suffer from the problem that resin powder is generated during granule manufacturing and transportation due to contact between granules. Since the generated resin powder reduces workability, there is a need to reduce resin powder and improve workability. It should be noted that the term "resin powder" in this disclosure refers to powdery resin generated during transportation and other processes caused by collisions between granules.
[0008] This disclosure is an invention that solves the above-mentioned problems, and its object is to provide a resin composition for washing molding machines that provides the same or better washing properties as the conventional one, while having excellent workability.
[0009] Methods for solving problems
[0010] The inventors of this disclosure have discovered that a resin composition for washing molding machines can achieve the same or better washing performance as conventional resin compositions while also exhibiting excellent workability. This resin composition for washing molding machines comprises an acrylonitrile-styrene copolymer (AS) resin, a rubber component, and an aliphatic surfactant and / or an aromatic surfactant. The content of the rubber component is within a specific range, and the amount of resin powder generated during manufacturing or transportation is less than a certain amount.
[0011] That is, this disclosure provides a resin composition for washing a molding and processing machine, which includes an acrylonitrile-styrene copolymer (AS) resin, a rubber component, and an aliphatic surfactant and / or an aromatic surfactant, wherein the content of the rubber component is 3 to 15 parts by weight relative to 100 parts by weight of the AS resin.
[0012] Preferably, the content of the structural unit derived from the cyanide vinyl compound in the above-mentioned AS-based resin is 34% by mass or less. By being within the above range, it is easy to suppress discoloration while maintaining an appropriate viscosity of the above-mentioned resin composition for washing molding machines.
[0013] Relative to 100 parts by weight of the aforementioned AS-based resin, the content of the aforementioned aliphatic surfactant and the aforementioned aromatic surfactant is preferably 0.5 to 10 parts by weight. By being within the above range, it is possible to easily exert the detergent and self-draining properties of the resin while easily preventing metering abnormalities during injection molding.
[0014] Invention Effects
[0015] The resin composition for washing molding machines disclosed herein exhibits excellent workability while maintaining the same or better washing properties as previous methods. Detailed Implementation
[0016] [Resin composition for washing molding machines]
[0017] The resin composition for washing molding machines disclosed herein (hereinafter sometimes referred to as "the resin composition of the present disclosure") comprises an acrylonitrile-styrene copolymer (AS) resin, a rubber component, and an aliphatic surfactant and / or an aromatic surfactant. The content of the rubber component is 3 to 15 parts by mass relative to 100 parts by mass of the aforementioned AS resin, thereby sufficiently reducing the amount of resin powder and thus providing excellent workability.
[0018] Regarding the resin composition disclosed herein, when 1000g of it is placed in an antistatic polyethylene bag and manually shaken up and down and left and right a total of 100 times in a state including air, the amount of resin powder produced is 1g or less, more preferably 0.7g or less, and even more preferably 0.5g or less. By keeping the amount of resin powder to 1g or less, a resin composition with excellent workability can be prepared.
[0019] When the measurements were performed under the conditions of the following embodiments, the amount of resin composition necessary for washing PC / ABS resin was preferably 700g or less, more preferably 600g or less. By keeping the amount of resin composition necessary for washing PC / ABS resin at 700g or less, resin can be efficiently discharged from the molding machine, and sufficient washing properties can be achieved.
[0020] Similarly, when the test is conducted under the conditions of the following embodiments, the amount of ABS resin necessary for washing is preferably 700g or less, more preferably 600g or less, and even more preferably 500g or less. By keeping the amount of resin composition necessary for washing the ABS resin at 700g or less, the resin in the molding machine can be discharged efficiently, and sufficient washing properties can be achieved.
[0021] Furthermore, when evaluating self-excretion performance under the conditions of the following embodiments, it is preferable that the excretion is within 400g, more preferably within 350g, and even more preferably within 300g.
[0022] The melt flow rate (MFR) of the resin composition disclosed herein, measured at a temperature of 240°C and a nominal load of 5 kg, is preferably 3 to 40 g / 10 min, more preferably 5 to 35 g / 10 min, and even more preferably 8 to 25 g / 10 min. If the MFR is 3 g / 10 min or higher, it is easier to achieve good flowability. Furthermore, if the MFR is 40 g / 10 min or lower, it is easier to achieve good heat resistance and mechanical strength.
[0023] (Acrylonitrile-styrene copolymer (AS) resin)
[0024] The resin composition disclosed herein comprises an acrylonitrile-styrene copolymer (AS) resin, and is particularly preferably included as a main component. The aforementioned AS resin is a thermoplastic copolymer resin obtained by copolymerizing a cyanide vinyl compound with an aromatic vinyl compound. Only one type of AS resin may be used, or two or more types may be used.
[0025] Examples of the aforementioned vinyl cyanide compounds include acrylonitrile and methacrylonitrile, with acrylonitrile being particularly preferred.
[0026] Examples of the aforementioned aromatic vinyl compounds include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, p-tert-butylstyrene, vinylnaphthalene, methoxystyrene, monobromostyrene, dibromostyrene, fluorostyrene, tribromostyrene, etc., with styrene and α-methylstyrene being particularly preferred.
[0027] Furthermore, the aforementioned AS-based resins may also include other vinyl compounds besides the aforementioned cyanide vinyl compounds and aromatic vinyl compounds as constituent monomers. Examples of such other vinyl compounds include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate; α,β-unsaturated carboxylic acids such as acrylic acid and methacrylic acid, and maleic anhydride; maleimides such as N-phenylmaleimide, N-methylmaleimide, and N-cyclohexylmaleimide; and monomers containing glycidyl groups such as glycidyl methacrylate.
[0028] Specifically, the aforementioned AS-based resin is preferably a copolymer resin comprising structural units derived from acrylonitrile and structural units derived from styrene, and more preferably a copolymer resin composed of structural units derived from acrylonitrile and structural units derived from styrene. That is, AS resin is preferred as the aforementioned AS-based resin.
[0029] There is no particular limitation on the intrinsic viscosity when the above-mentioned AS-based resin is melted in CHCl3, but it is preferably 0.61 to 1.21, more preferably 0.82 to 1.07. By making the intrinsic viscosity 0.61 or higher, the washing properties can be improved, and by making it 1.21 or lower, the self-draining properties can be improved.
[0030] The content of the structural unit from which the cyanide vinyl compound is derived in the aforementioned AS-based resin is preferably 34% by mass or less, more preferably 31% by mass or less, and even more preferably 29% by mass or less, relative to the total amount of the AS-based resin (100% by mass). By keeping the content of the structural unit from which the cyanide vinyl compound is derived at 34% by mass or less, it is easy to suppress discoloration while maintaining an appropriate viscosity for the AS-based resin. Furthermore, there is no particular limitation on the lower limit, but it is preferably 22% by mass or more, more preferably 23% by mass or more.
[0031] The melt flow rate (MFR) of the aforementioned AS-based resin, measured at a temperature of 220°C and a nominal load of 10 kg, is preferably 9 to 70 g / 10 min, more preferably 15 to 40 g / 10 min. If the MFR is 9 g / 10 min or higher, it facilitates fluidity. Furthermore, if the MFR is 70 g / 10 min or lower, it facilitates the development of heat resistance and mechanical strength.
[0032] The content of the structural unit that is the source of the aromatic vinyl compound in the above-mentioned AS-based resin is preferably 66 to 78% by mass, more preferably 69 to 77% by mass, relative to the total amount of the AS-based resin (100% by mass). By keeping the content of the structural unit that is the source of the aromatic vinyl compound within the above range, it is easy to suppress discoloration while maintaining an appropriate viscosity of the AS-based resin.
[0033] When the aforementioned AS-based resin contains structural units derived from other vinyl compounds, their content relative to the total amount of the AS-based resin (100% by mass) is preferably 10% by mass or less, more preferably 1% by mass or less. By keeping the content of structural units derived from other vinyl compounds at 10% by mass or less, it is easier to achieve the function of an AS-based resin.
[0034] Regarding the content of the aforementioned AS-based resin, in the total amount (100% by mass) of the resin composition disclosed herein, it is preferably greater than 50% by mass, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. By ensuring that the content of the AS-based resin is greater than 50% by mass, it can function as the main component of the resin composition disclosed herein. Furthermore, there is no particular upper limit, but it is preferably 97% by mass or less, more preferably 95% by mass or less.
[0035] The aforementioned AS-based resins can be produced by known or conventional methods, such as bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, and other known polymerization methods.
[0036] (Rubber composition)
[0037] The resin composition disclosed herein contains a rubber component. By including the aforementioned rubber component in the resin composition of this disclosure, when the resin composition of this disclosure is formed into granules, the cross-section of the granules can be made smooth, and the amount of resin powder during contact between granules can be reduced. As the aforementioned rubber component, only one type can be used, or two or more types can be used.
[0038] As the aforementioned rubber component, the rubber component can be used alone, or a rubber-containing resin can be used. From the viewpoint of maximizing compatibility with the aforementioned AS-based resins, a rubber-containing resin is preferred; and as such, a styrene-based resin containing a rubber component is more preferred. It should be noted that in this disclosure, even a resin that contains only a portion of a rubber component, such as the aforementioned rubber-containing resin, can be treated as a rubber component as a whole.
[0039] Examples of rubber components include diene rubbers, urethane rubbers, silicone rubbers, and polysulfide rubbers. Among these, diene rubbers are preferred. Examples of diene rubbers include natural rubber, polyisoprene rubber, polybutadiene rubber, butyl rubber, chloroprene rubber, and modified rubbers (epoxidized natural rubber, hydrogenated natural rubber, hydrogenated butadiene-acrylonitrile copolymer rubber, etc.).
[0040] In addition, examples of rubber components contained in the aforementioned rubber-containing resins include polybutadiene, polyisoprene, random copolymers and block copolymers of styrene and butadiene, acrylonitrile-butadiene copolymers, and copolymers of (meth)acrylate and butadiene, ethylene-propylene random copolymers and block copolymers, ethylene-butene random copolymers and block copolymers, ethylene-α-olefin copolymers, ethylene-methacrylate copolymers and ethylene-butyl acrylate copolymers, and ethylene-unsaturated carboxylic acid ester copolymers, as well as ethylene-vinyl acetate copolymers. This includes copolymers of vinyl groups, copolymers of ethylene, propylene, and hexadiene, and other polymers of ethylene and propylene with non-conjugated dienes; acrylic rubbers such as polybutyl acrylate, poly(2-ethylhexyl acrylate), and copolymers of butyl acrylate and 2-ethylhexyl acrylate; polysiloxane rubbers; IPN-type rubbers formed from polysiloxane rubber components and poly(meth)acrylate alkyl ester rubber components: that is, rubbers having a structure in which the two rubber components are intertwined in an inseparable manner; and silicone rubbers such as IPN-type rubbers formed from polysiloxane rubber components and polyisobutylene rubber components. Among these, polybutadiene, polyisoprene, and diene copolymers are preferred, with polybutadiene being particularly preferred.
[0041] Examples of styrene-based resins containing the aforementioned rubber components include HIPS resin, MS resin, ABS resin, AES resin, ASA resin, MBS resin, MABS resin, MAS resin, SMA resin, and styrene-based thermoplastic elastomers (e.g., (hydrogenated) styrene-butadiene-styrene copolymer, (hydrogenated) styrene-isoprene-styrene copolymer, etc.). From the viewpoint of compatibility with the aforementioned styrene-based resins, ABS resin is preferred.
[0042] When the rubber component comprises a rubber-containing resin, the content of the rubber component in the total amount (100% by mass) of the rubber-containing resin is preferably 18-80% by mass, more preferably 35-70% by mass, and even more preferably 40-60% by mass. By making the content of the rubber component 18% by mass or more, it is easy to reduce the amount of resin powder. In addition, by making it 80% by mass or less, it is easy to be compatible with other resin components contained in the resin composition of this disclosure.
[0043] Furthermore, when ABS resin is included as the aforementioned rubber component, the content of acrylonitrile-derived structural units in the total amount of ABS resin (100% by mass) is preferably 28% by mass or less, more preferably 27% by mass or less, and even more preferably 26% by mass or less. By keeping the content of acrylonitrile-derived structural units at 28% by mass or less, it is easy to suppress discoloration while maintaining a suitable viscosity of the ABS resin. While there is no particular limitation on the lower limit, it is preferably 18% by mass or more, more preferably 23% by mass or more.
[0044] The content of the aforementioned rubber component is 3 to 15 parts by weight relative to 100 parts by weight of the aforementioned AS-based resin, preferably 4 to 14 parts by weight, and more preferably 5 to 10 parts by weight. By including 3 or more parts by weight of rubber component, the amount of resin powder can be reduced. In addition, by including 15 or less parts by weight, washability can be maintained.
[0045] Furthermore, the content of the aforementioned rubber component in the total amount (100% by mass) of the resin composition disclosed herein is preferably 2 to 13% by mass, more preferably 3 to 12% by mass. By including 2% or more of the rubber component, the amount of resin powder can be reduced. In addition, by including 13% or less by mass, washability can be maintained.
[0046] Furthermore, when the rubber component contains ABS resin, the specific viscosity of the ABS resin is preferably 0.2 to 0.8%, more preferably 0.3 to 0.7%, and even more preferably 0.4 to 0.6%.
[0047] It should be noted that the above specific viscosity was obtained as follows: ABS resin was dissolved in acetone, separated into an acetone-soluble portion and an acetone-insoluble portion, and after the acetone in the acetone-soluble portion was volatilized, it was dissolved in dimethylformamide to prepare a 0.4 g / 100 ml solution, which was then measured at 30 °C.
[0048] (Aliphatic surfactants and / or aromatic surfactants)
[0049] The resin composition disclosed herein contains an aliphatic surfactant and / or an aromatic surfactant. The surfactants are added to the resin composition of this disclosure to enhance detergency while also providing self-discharging properties. As the aliphatic surfactant and / or the aromatic surfactant, only one or more of them may be used. Furthermore, one or more of the aliphatic surfactant and the aromatic surfactant may be used.
[0050] Examples of aliphatic surfactants include nonionic aliphatic surfactants and anionic aliphatic surfactants.
[0051] Examples of nonionic aliphatic surfactants mentioned above include sorbitan fatty acid esters, glycerol fatty acid esters, polyoxyalkylene ethers, and polyoxyalkylene fatty acid esters.
[0052] Examples of the aforementioned sorbitan fatty acid esters include sorbitan monooleate, sorbitan monostearate, sorbitan monoisostearate, sorbitan monopalmitate, sorbitan monolaurate, sorbitan trioleate, sorbitan tristearate, sorbitan sesquistearate, sorbitan sesquioleate, sorbitan sesquiisostearate, and sorbitan coconut oil fatty acid ester. In addition, examples of epoxy alkane adducts of sorbitan fatty acid esters include polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan monoisostearate, polyoxyethylene sorbitan monococoate, polyoxyethylene sorbitan monococoate, polyoxyethylene sorbitan tristearate, and polyoxyethylene sorbitan trioleate.
[0053] The aforementioned glycerol fatty acid esters include either monoglyceride or polyglycerol fatty acid esters. Examples of monoglyceride fatty acid esters include glyceryl monocaprylate, glyceryl monodecanoate, glyceryl monolaurate, glyceryl monomyristate, glyceryl monopalmitate, glyceryl monostearate, glyceryl monoisostearate, glyceryl monobehenate, glyceryl monooleate, glyceryl monosinic acid, glyceryl sesquioleate, glyceryl distearate, glyceryl diisostearate, and glyceryl arachidonic acid. Examples of polyglycerol fatty acid esters with a degree of polymerization of 2 to 10 include monocaprylic acid diglyceride, monocaprylic acid decaglyceride, monocapric acid hexaglyceride, monolauric acid tetraglyceride, monolauric acid hexaglyceride, monolauric acid decaglyceride, monolauric acid poly(4-10) glyceride, monomyristate decaglyceride, monostearate decaglyceride, monoisostearate decaglyceride, monostearate poly(2-10) glyceride, monooleic acid diglyceride, monooleic acid hexaglyceride, sesquioleic acid diglyceride, diisostearate poly(2-10) glyceride, distearate poly(6-10) glyceride, triisostearate diglyceride, and tristearate poly(10) glyceride. Additionally, examples of epoxide adducts of glycerol fatty acid esters include monostearate polyoxyethylene glyceride and monooleic acid polyoxyethylene glyceride.
[0054] As the aforementioned polyoxyalkylene oxide ethers, both monooxyalkylene oxide ethers and polyoxyalkylene oxide ethers are included. Examples of the aforementioned polyoxyalkylene oxide ethers include polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene oil-based ether, polyoxyethylene polyoxypropylene lauryl ether, polyoxypropylene cetyl ether, polyoxypropylene isocetyl ether, polyoxypropylene stearyl ether, and polyoxypropylene oil-based ether.
[0055] The aforementioned polyoxyethylene fatty acid esters include both monooxyethylene fatty acid esters and polyoxyethylene fatty acid esters. Specifically, examples of the aforementioned polyoxyethylene fatty acid esters include ethylene glycol mono- and di-fatty acid esters, diethylene glycol mono- and di-fatty acid esters, polyethylene glycol mono- and di-fatty acid esters, propylene glycol mono- and di-fatty acid esters, and polypropylene glycol mono- and di-fatty acid esters.
[0056] Specifically, examples of the aforementioned ethylene glycol mono- and di-fatty acid esters include ethylene glycol monolaurate, ethylene glycol monopalmitate, ethylene glycol monostearate, ethylene glycol dilaurate, ethylene glycol dipalmitate, and ethylene glycol distearate. Among these, ethylene glycol distearate is more preferred.
[0057] Examples of aliphatic surfactants with anionic structures include alkyl or alkenyl ether sulfates, alkyl or alkenyl sulfates, α-olefin sulfonates with 8 to 20 carbon atoms, alkane sulfonates, alkyl or alkenyl ether carboxylates, and alkali metal salts of saturated or unsaturated fatty acids with 12 to 20 carbon atoms. Alkane sulfonates are preferred.
[0058] Examples of the aforementioned alkane sulfonates include sodium octyl sulfonate, sodium ethylhexyl sulfonate, sodium undecyl sulfonate, sodium dodecyl sulfonate, sodium dodecyl sulfonate, sodium hexadecyl sulfonate, and sodium octadecyl sulfonate. The salt can be a sodium salt, or a potassium salt, ammonium salt, etc. Among these, sodium alkane sulfonates are preferred, and mixtures of sodium alkane sulfonates having 10 to 18 carbon atoms are more preferred.
[0059] The content of the aforementioned aliphatic surfactant relative to the total amount of surfactant used (100% by mass) is preferably 50-90% by mass, more preferably 55-85% by mass, and even more preferably 60-70% by mass. By ensuring that the content of the aliphatic surfactant relative to the total amount of surfactant is within the above range, it is easy to achieve detergency with various resins.
[0060] The content of the above-mentioned aliphatic surfactant relative to the total amount (100% by mass) of the resin composition disclosed herein is preferably 0.5 to 10% by mass, more preferably 2 to 8% by mass.
[0061] Examples of aromatic surfactants include nonionic aromatic surfactants and anionic aromatic surfactants.
[0062] Examples of nonionic aromatic surfactants include polyoxyethylene bisphenol A ether, polyoxyethylene bisphenol F ether, polyoxyethylene polycyclic phenyl ether, polyoxyethylene phenyl ether, polyoxyethylene styrene phenyl ether, polyoxyethylene styrene phenyl ether, polyoxyethylene stilbene phenyl ether, polyoxyethylene cumyl phenyl ether, polyoxyethylene tribenzyl phenyl ether, and polyoxyethylene benzyl ether.
[0063] Examples of aromatic surfactants that are anionic in nature include alkylbenzene sulfonates and aromatic condensed phosphates, with aromatic condensed phosphates being particularly preferred.
[0064] As the aforementioned alkylbenzene sulfonates, linear alkylbenzene sulfonates with 8 to 20 or fewer carbon atoms in the alkyl group can be used, specifically, sodium decylbenzene sulfonate, sodium undecylbenzene sulfonate, sodium dodecylbenzene sulfonate, sodium tridecylbenzene sulfonate, sodium tetradecylbenzene sulfonate, sodium pentadecylbenzene sulfonate, sodium hexadecylbenzene sulfonate, etc. Besides sodium salts, the salts can also be potassium salts, ammonium salts, etc.
[0065] Examples of the aforementioned aromatic condensed phosphates include resorcinol bis(diphenyl) phosphate, bisphenol A bis(diphenyl) phosphate, and resorcinol bis(dimethyl) phosphate, with resorcinol bis(dimethyl) phosphate being the most preferred.
[0066] The content of the aromatic surfactant relative to the total amount of surfactant used (100% by mass) is preferably 10 to 50% by mass, more preferably 15 to 45% by mass, and even more preferably 20 to 40% by mass. By keeping the content of the aromatic surfactant relative to the total amount of surfactant within the above range, it is easy to achieve detergency with various resins.
[0067] The content of the above-mentioned aromatic surfactant relative to the total amount (100% by mass) of the resin composition disclosed herein is preferably 0.5 to 5% by mass, more preferably 1 to 4% by mass.
[0068] The total content of the aforementioned aliphatic surfactant and aromatic surfactant relative to the total amount (100% by mass) of the resin composition of this disclosure is preferably 0.5 to 10% by mass, more preferably 1 to 9% by mass, and even more preferably 3 to 8% by mass. By making the content of the aliphatic surfactant and aromatic surfactant 0.5% by mass or more, it is easy to exert the detergent and self-draining properties of the resin. In addition, by making it 10% by mass or less, it is easy to prevent metering abnormalities during injection molding. It should be noted that when the resin composition of this disclosure contains only one of the aforementioned aliphatic surfactant and aromatic surfactant, it is preferable that their content meets the above range.
[0069] Furthermore, the resin composition of this disclosure preferably contains an inorganic filler. By containing an inorganic filler, the detergent properties can be achieved by utilizing the abrasive effect of the inorganic filler while adjusting the viscosity of the resin composition of this disclosure. Only one type of inorganic filler may be used, or two or more types may be used.
[0070] Both natural and synthetic materials can be used as the aforementioned inorganic fillers. Examples of such inorganic fillers include talc, mica, wollastonite, calcium silicate, kaolin, montmorillonite, bentonite, sepiolite, sericite, sparganite, calcium carbonate, magnesium carbonate, titanium dioxide, aluminum hydroxide, magnesium hydroxide, zeolite, diatomaceous earth, glass powder, glass beads, and white sand microspheres.
[0071] The shape of the aforementioned inorganic filler is not particularly limited and can be any shape (plate-like, needle-like, granular, fibrous, etc.). Furthermore, these inorganic fillers can be fillers obtained through calcination or fillers obtained by surface hydrophobic treatment using silane coupling agents, titanate coupling agents, etc. In addition, the volume average particle diameter is preferably 0.1–50 μm, more preferably 1–30 μm. The aforementioned volume average particle size can be determined by laser diffraction scattering.
[0072] The content of the aforementioned inorganic filler relative to the total amount (100% by mass) of the resin composition disclosed herein is preferably 0.1 to 10% by mass, more preferably 0.5 to 5% by mass. By making the content of the inorganic filler 0.1% by mass or more, it is easy to improve the washability. In addition, by making it 10% by mass or less, it is easy to make the viscosity of the resin composition disclosed herein moderate.
[0073] Furthermore, the resin composition disclosed herein preferably further contains phosphates and / or condensed phosphates. The presence of phosphates and / or condensed phosphates enhances detergency and displacement properties. As the aforementioned phosphates and / or condensed phosphates, only one or more of them may be used. Additionally, one or more of the aforementioned phosphates and condensed phosphates may be used.
[0074] Examples of the aforementioned phosphates include sodium phosphate and disodium hydrogen phosphate.
[0075] Examples of the aforementioned condensed phosphates include sodium dihydrogen pyrophosphate, sodium pyrophosphate, sodium tripolyphosphate, sodium tetrapolyphosphate, sodium pentapolyphosphate, and sodium metaphosphate.
[0076] The content of the above-mentioned phosphate and the above-mentioned condensed phosphate relative to the total amount (100% by mass) of the resin composition disclosed herein is preferably 0.1 to 10% by mass, more preferably 0.5 to 5% by mass. By keeping the content of the above-mentioned phosphate and the above-mentioned condensed phosphate within the above range, it is easy to achieve detergency and displacement properties.
[0077] The resin composition disclosed herein may also contain other components besides those described above. Examples of such other components include flame retardants, anti-drip agents, dyes and pigments, heat stabilizers, ultraviolet absorbers, fluorescent whitening agents, lubricants, processing aids, dispersants, release agents, thickeners, antioxidants, antistatic agents, and foaming agents. Only one of these other components may be used, or two or more may be used.
[0078] The content of the other components mentioned above relative to the total amount (100% by mass) of the resin composition disclosed herein is preferably 10% by mass or less, more preferably 5% by mass or less, and may also be 0% by mass.
[0079] The method for manufacturing the resin composition disclosed herein is not particularly limited. A preferred manufacturing method includes the following steps: the AS-based resin, the rubber component, the surfactant, and, as needed, the phosphate, condensed phosphate, inorganic filler, and other components are melt-blended using a melt-blending apparatus such as a kneader, extruder, or Banbury mixer; the resulting melt-blended mixture is then extruded in a linear fashion to form granules. From the viewpoint of being able to adequately blend raw materials such as thermoplastic resins, an extruder is preferred as the melt-blending apparatus.
[0080] When blending and melting the various components, commonly used equipment can be used, such as premixing devices like drum mixers, screw mixers, and high-speed mixers, as well as melt blending equipment like gravimetric feeders, single-screw extruders, twin-screw extruders, and continuous kneaders. Furthermore, during melt blending, open devolatilization, where devolatilized components are removed from the open port (exhaust port) under normal pressure, is preferred; and depressurized devolatilization, where devolatilized components are removed from the open port (exhaust port) by reducing pressure, can be performed as needed.
[0081] Furthermore, the temperature for the process of forming granules from wire into particles is preferably 40 to 150°C, more preferably 50 to 120°C. The resin composition disclosed herein can form a smooth cross-section even under rapid cooling, thus reducing resin powder generated due to friction between particles.
[0082] As a washing method for a molding machine using the resin composition of this disclosure, one example is to feed the resin composition of this disclosure into the barrel of a resin molding machine, heat the resin composition of this disclosure to maintain plasticization (melting), and then discharge the plasticized resin composition of this disclosure from the barrel of the resin molding machine. In particular, since the amount of resin powder in the resin composition of this disclosure is reduced, the workability when feeding it into the barrel is excellent.
[0083] Examples of suitable resin molding machines include injection molding machines and extrusion molding machines; however, they are not particularly limited to any type that has a barrel for heating and melting the resin for mixing. That is, the resin composition of this disclosure can be widely used in known resin molding machines. The barrel temperature of the resin molding machine when heating the resin composition of this disclosure is preferably set to 180°C or higher, more preferably 200°C or higher. There is no particular upper limit to the heating temperature, but it is typically around 400°C.
[0084] When the resin composition disclosed herein completes a given operation in an extruder or injection molding machine, it can efficiently wash away residual resin materials contained in the molding material, such as the resin itself and dyes and pigments, that remain in the molding machine. Therefore, it can be suitably used as a washing resin composition for washing molding machines used for thermoplastic resins. That is, the resin composition disclosed herein is preferably a detergent for extruders or injection molding machines.
[0085] In addition, the resin composition disclosed herein can be suitably used as a resin such as PA, PMMA, PLA, ABS, AS, PVC, PVDF, TPU, PC, PET, PBT, POM, etc., which are intended to be washed, as well as resin compositions containing the above-mentioned resins as main components (preferably 50% by mass or more).
[0086] The various methods disclosed in this specification can be combined with any other features disclosed in this specification. Each embodiment and its combination is an example, and appropriate additions, omissions, substitutions, and other modifications can be made to the configuration without departing from the spirit of this disclosure. Furthermore, the inventions disclosed herein are not limited to the embodiments or the following examples, but only to the scope of the claimed technical solutions.
[0087] Example
[0088] The following describes one embodiment of the present disclosure in more detail based on an example.
[0089] Examples 1-3, Comparative Examples 1-2
[0090] The components shown in Table 1 were mixed using a drum mixer (trade name "SFC-50", manufactured by KAWATA Corporation) (mixing time: 120 seconds, mixing speed: 120 rpm), and then extruded into granules using an extruder (trade name "TEX-30", manufactured by Nippon Steel Co., Ltd.) under the following conditions: nozzle diameter 32 mm, barrel temperature C1 210°C, C2 to C8 230°C (C1 is the upstream side, C8 is the downstream side), die temperature 240°C, screw speed 200 rpm, and discharge rate 20 kg / h. This produced the molding and processing machine washing resin compositions of Examples 1 to 3 and Comparative Examples 1 to 2. It should be noted that, under the conditions of a measurement temperature of 240°C and a nominal load of 5 kg, the MFR of the resin composition for washing the molding machine in Example 1 was 13 g / 10 min, the MFR of the resin composition for washing the molding machine in Example 2 was 15 g / 10 min, the MFR of the resin composition for washing the molding machine in Example 3 was 18 g / 10 min, the MFR of the resin composition for washing the molding machine in Comparative Example 1 was 25 g / 10 min, and the MFR of the resin composition for washing the molding machine in Comparative Example 2 was 8.0 g / 10 min.
[0091] The components used in Table 1 are described in detail below.
[0092] • Styrene-acrylonitrile copolymer: 28% by mass of structural units derived from vinyl cyanide compounds; MFR (measured at 220°C, nominal load 10 kg): 9.7 g / 10 min; intrinsic viscosity: 1.07.
[0093] • Styrene-acrylonitrile-butadiene copolymer: 45% by mass of structural units derived from aromatic vinyl compounds, 15% by mass of structural units derived from cyanide vinyl compounds, 40% by mass of structural units derived from rubber components, acetone-soluble specific viscosity 0.5%, intrinsic viscosity: 0.45
[0094] • Sodium alkane sulfonate: (trade name "WeyClean SAS93", manufactured by Clariant Japan)
[0095] • Sodium dodecylbenzenesulfonate: (trade name "Newrex Soft 60-N", manufactured by Nippon Oil Company)
[0096] • Ethylene glycol distearate: (trade name "Emanon 3201M-V", manufactured by Kao Corporation)
[0097] • Aromatic condensed phosphate esters: (trade name "PX-200", manufactured by Daihachi Chemical Industry Co., Ltd.)
[0098] • Sodium phosphate: (trade name "disodium phosphate (anhydrous)", manufactured by Taiping Chemical Industry Co., Ltd.)
[0099] Talc: (Trade name "Talc FU-51", manufactured by Lin Huacheng Company)
[0100] [evaluate]
[0101] The resin compositions for washing molding machines prepared in the Examples and Comparative Examples were evaluated as follows, and the results are recorded in Table 1.
[0102] (1) Amount of resin powder produced
[0103] 1000g each of the resin compositions for washing molding machines from Examples 1-3 and Comparative Examples 1-2 were placed in an antistatic polyethylene bag and stirred manually by shaking the bag up, down, left, and right a total of 100 times while containing air. Then, the entire contents of the antistatic polyethylene bag were passed through a 4.0mm sieve, and the amount (g) of resin powder that passed through the sieve was measured.
[0104] (2) -1. Washability of PC / ABS
[0105] 500g of PC / ABS resin (trade name "Novalloy S1100", manufactured by Daicel Mewa Co., Ltd.) is pre-filled into an injection molding machine (trade name "2000i-100B", manufactured by FANUC Corporation, injection speed 100mm / sec, rotation speed 100rpm, nozzle temperature 260℃ - front of barrel 270℃ - middle of barrel 260℃ - rear of barrel 250℃, back pressure 0.3MPa, stroke 50mm) and then discharged.
[0106] Then, the stroke was adjusted to 40 mm, and the molding machine washing resin compositions of Examples 1-3 and Comparative Examples 1-2 were added to the injection molding machine at 100 g per batch, up to a maximum of 1000 g, to replace the PC / ABS resin. The moment when the coloring of the PC / ABS resin could no longer be observed under visual conditions was defined as the washing completion point, and the mass (g) of the washing resin composition necessary for the washing completion point was measured.
[0107] (2) -2. Washability of ABS
[0108] Except for replacing PC / ABS resin (trade name "Novalloy S1100", manufactured by Caillou Mewa Co., Ltd.) with black ABS resin granules (trade name "Sebian V 500", manufactured by Caillou Mewa Co., Ltd.) and setting the nozzle temperature of the injection molding machine to 220°C - 230°C at the front of the barrel - 220°C at the middle of the barrel - 210°C at the rear of the barrel, the washability of the ABS resin was determined by the same method as in (2)-1.
[0109] (3) Self-excretion
[0110] After the molding machine washing resin compositions of Examples 1-3 and Comparative Examples 1-2 were discharged under the same conditions as those used to evaluate the washability of ABS, the barrel temperature was set to 230°C, and injection molding was performed using transparent AS resin (trade name "Sebian 050SF", manufactured by Daicel Meihua Co., Ltd.). Cases where no residue was found within 400g were evaluated as ○, and cases where residue of the molding machine washing resin composition remained even when more than 400g was used were evaluated as ×.
[0111] [Table 1]
[0112]
[0113] The resin compositions for washing molding machines in Examples 1-3 were confirmed to have washability equal to or better than conventional products, while reducing the amount of resin powder and resulting in excellent workability. On the other hand, it was confirmed that in the absence of rubber components, a large amount of resin powder was generated, resulting in poor workability (Comparative Example 1). Furthermore, it was confirmed that when the rubber components were present in excessive amounts compared to AS-based resins, the washability was poor (Comparative Example 2).
Claims
1. A resin composition for washing a molding machine, comprising: Acrylonitrile-styrene copolymer resins, i.e., AS-based resins Rubber components, and Aliphatic surfactants and / or aromatic surfactants, In the resin composition for washing the molding and processing machine, the content of the rubber component is 3 to 15 parts by mass relative to 100 parts by mass of the AS-based resin.
2. The resin composition for washing in a molding and processing machine according to claim 1, wherein, The content of structural units derived from cyanide vinyl compounds in the AS-based resin is less than 34% by mass.
3. The resin composition for washing in a molding and processing machine according to claim 1 or 2, wherein, The content of the aliphatic surfactant and the aromatic surfactant is 0.5 to 10 parts by weight relative to 100 parts by weight of the AS-based resin.
Citation Information
Patent Citations
Resin composition for cleaning
JP2008201975A
Panel formwork
JP2024063514A