Container and method of manufacturing the same
Containers manufactured using a multi-layer co-extrusion blow molding process employ a three- or more-layer structure, with the outer layer in contact with the outside, the inner layer in contact with the inside, and the middle layer being an active structure. This solves the problems of insufficient moisture-proof performance and material waste in containers, achieving efficient and environmentally friendly protection for moisture-sensitive products.
Patent Information
- Application Number
- CN202580029986.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-18
- Filing Date
- 2025-03-18
- Publication Date
- 2026-11-20
AI Technical Summary
Existing containers are insufficient in protecting moisture-sensitive products, resulting in significant material waste during manufacturing. Furthermore, direct contact between the desiccant layer and the contents may lead to the failure of the contact layer.
The container is manufactured using a multi-layer co-extrusion blow molding process, employing a three- or more-layer structure. The outer layer is in contact with the external atmosphere, the inner layer is in contact with the interior, and the middle layer is an active structure, including active materials such as desiccants. A second active layer is formed by recycling waste materials to reduce material waste, and a concentration gradient is set between the layers to improve gas barrier performance.
It improves the container's moisture-proof performance, reduces material waste during the manufacturing process, avoids direct contact between active materials and contents, enhances gas diffusion barrier, and maintains the container's environmental friendliness.
Smart Images

Figure CN123146484A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a container for receiving and protecting sensitive products such as pharmaceuticals or medical articles, drugs, pills, tablets, test strips, granules, powders, or food.
[0002] This disclosure also relates to a method for manufacturing containers using a multilayer co-extrusion blow molding apparatus, and to a method for preparing active formulations suitable for extrusion blow molding. Background Technology
[0003] Containers used to protect sensitive products, such as moisture-sensitive products (e.g., pharmaceuticals or medical items), are important for preserving such products and ensuring their quality. Such containers may specifically include a desiccant layer and / or one or more other active layers. The container may need to be airtight to prevent the stored product from deteriorating, even after the container has been opened and closed several times.
[0004] Containers used to protect sensitive products can be manufactured using multilayer extrusion blow molding of desiccant polymer blends. Such blends contain a desiccant embedded within a polymer resin matrix, forming a desiccant layer within the container.
[0005] There is a continued need to improve the moisture-proof properties of such containers and to accelerate their manufacturing. It is also desirable to avoid direct contact between the desiccant layer of the container and the contents received inside. In other words, it is desirable for such containers to include a contact layer adapted to contact the interior space of the items received within the container. Furthermore, it is desirable to improve the environmental friendliness of the manufacturing methods used to produce these containers.
[0006] Therefore, improvements are needed to the containers and their manufacturing methods to address at least one of the aforementioned drawbacks. Summary of the Invention
[0007] One aspect of this disclosure relates to a container comprising an internal chamber for receiving sensitive products. The term sensitive products may specifically cover moisture-sensitive products (such as food, pharmaceuticals, or medical articles). The internal chamber is defined by walls, which consist of three or more layers. The term "defined" does not mean that the walls must completely enclose the internal chamber. The walls may include one or more openings that provide passage to the internal chamber. Typically, the internal chamber may have a bottom surface, side surfaces, and an opening at the top, which can be closed by a lid member. An example of a container is a bottle-shaped container.
[0008] The three or more layers may include an outer layer configured to contact the external atmosphere surrounding the container. The outer layer contacts the external atmosphere when the container is placed in it (e.g., when the container is placed in a location used for storing items).
[0009] The outer layer may include at least 95 wt% (weight percentage) of the base polymer. Throughout this document, the wt% amount of a component in the layer is a percentage of the weight of the component relative to the total weight of the composition of the layer.
[0010] When referring to a base polymer in this document, a base polymer may include any one or more of the following base polymers (or constitute a combination thereof): polyolefins, polyisoprene, thermoplastic cellulose, ethylene-vinyl acetate copolymer, ethylene-methacrylate copolymer, ethylene-butyl acrylate copolymer, acrylonitrile-butadiene-styrene, polystyrene, styrene-ethylene-butene-styrene copolymer, styrene-butene-styrene copolymer, styrene-butadiene copolymer, polyester, polyanhydride, polysulfone, polyacrylate, thermoplastic polyurethane (TPU), polyacetal (POM), polylactic acid (PLA), and mixtures thereof.
[0011] The base polymer may specifically include or be composed of polyolefins. Typical polyolefin base polymers include polyolefins, such as homopolymers and copolymers of monoolefins and dienes, such as polypropylene (PP) and polyethylene (PE), which may optionally be crosslinked, such as high-density polyethylene (HDPE) and low-density polyethylene (LDPE).
[0012] The three or more layers may include active structures arranged from the outermost layer inwards. Positioning from the outermost layer inwards means that the outermost layer faces outwards (and, therefore, towards the external atmosphere), while the inner surface of the outermost layer faces the active structures.
[0013] In the sense that the outer layer can contact the active structure, the inner side of the outer layer can directly face the active structure. In this case, the active structure includes a layer that contacts the inner side of the outer layer. Alternatively, the inner side of the outer layer can indirectly face the active structure. In this case, one or more layers can exist between the outer layer and the active structure. In other words, when considering all three or more layers facing the external atmosphere from the inner chamber, the order is as follows: (optional one or more additional layers), active structure, (optional one or more additional layers), and outer layer.
[0014] Therefore, the container can, for example, consist of the following layers from the inside out: an active structure and an outer layer.
[0015] The active structure may include a first active layer. The first active layer may comprise a base polymer and one or more active materials. The first active layer may comprise a first wt% amount of the one or more active materials of C1.
[0016] Whenever active materials are mentioned in this article, they may belong to the group including: hygroscopic agents (or desiccants); oxygen absorbers (or oxygen scavengers); odor absorbers; moisture release sources; release sources of volatile organic compounds such as fragrances, aromas, and nutrients; and mixtures thereof.
[0017] It should be understood that, within the meaning of this disclosure, when referring to a given active material, the term "absorption" is used to encompass all chemical and physical phenomena in which gases can be retained by said active material. In particular, this includes bulk phenomena, commonly referred to as "absorption," in which gas molecules enter the active material; or surface phenomena, commonly referred to as "adsorption," in which gas molecules attach to the surface of the active material.
[0018] The active material may contain or be composed of an inorganic desiccant material, which may be selected from the group consisting of: molecular sieves, zeolites, silica gel, clay, hydrated salts, metal oxides and mixtures thereof.
[0019] The active structure may include a second active layer. The second active layer may include at least 95 wt% of all materials present in the other layers of the container wall belonging to the three or more layers. The second active layer may contain a second wt% amount C2 of the one or more active materials, wherein the second wt% amount C2 is less than the first wt% amount C1. The term "other layers of the container wall" refers to all layers other than the second active layer itself.
[0020] Providing a second active layer allows for a reduction in manufacturing waste and thus improves environmental friendliness. In particular, material waste from the blow molding process can be reused during manufacturing.
[0021] The container can be manufactured using a multi-layer extrusion blow molding (EBM) process (among other processes).
[0022] Multi-layer extrusion blow molding (EBM) process may involve the following steps: co-extruding different materials into a preform and closing two half-die around the preform.
[0023] At the bottom of the preform, where the two mold halves meet, the preform can be compressed into a flat shape by the clamping opening of the blow molding die. Then, air can be used to stretch the preform to press it against the mold wall.
[0024] After the container cools and solidifies in the mold cavity, excess material at the neck and bottom sections can be removed. This excess material discarded at the bottom is called "pinch-off" because the bottom end of the material is clamped and sealed in the mold to form the base of the container. The material that can be discarded at the top is called "neck flash" and can be removed by a cutting device corresponding to a cutting area on the mold.
[0025] Instead of discarding the blank scrap, it can be partially or completely reused. After re-grinding, the material waste can be co-extruded to form a second active layer, in which the concentration of one or more active materials is lower than that in the first active layer. The lower concentration may be due to "dilution" by the material in the outer and / or other layers.
[0026] Therefore, containers can be manufactured in a more efficient and environmentally friendly way, producing less waste and being highly recyclable.
[0027] Similar to blanking waste, instead of discarding the neck flash, the neck flash can be partially or completely reused. After re-grinding, material waste containing only blanking waste, only neck flash, or a combination of neck flash and blanking waste can be co-extruded to form a second active layer, in which the concentration of one or more active materials is lower than that in the first active layer. The lower concentration may be due to "diluting" by one or more materials in the outer and / or other layers.
[0028] The ratio of the second wt% amount C2 of the one or more active materials in the second active layer to the first wt% amount C1 of the one or more active materials in the first active layer can be less than 0.75, preferably less than 0.6, and preferably less than 0.5. This concentration gradient between the first and second active layers with respect to one or more active materials can correspond to the material of the first active layer being “diluted” by one or more materials of the outer and / or other layers. This “dilution” can be achieved by regrinding waste from the blow molding process to form the second active layer. This reduces manufacturing waste and improves recyclability.
[0029] Compared to the first active layer, a second active layer with a lower filling rate of one or more active materials and a higher amount of base polymer can provide higher gas diffusion resistance. Therefore, gases (e.g., moisture and / or oxygen) can travel through the first active layer more easily than through the second active layer. Consequently, the concentration gradient of one or more active materials between the first and second active layers can allow gases traveling from the outside or inside of the container to be blocked between the second active layer and another "barrier" layer (e.g., an outer or inner layer), allowing them to remain within and diffuse in the more permeable first active layer, thereby increasing the likelihood of their absorption by one or more active materials.
[0030] In the first active layer, the first wt% amount C1 of one or more active materials can be equal to or greater than 50 wt%. The first wt% amount C1 can be equal to or greater than 60 wt%. These ranges with at least a minimum wt% value ensure sufficient functionality, such as the absorption capacity of a container. Furthermore, these ranges with at least a minimum wt% value can provide a suitable desiccant filling rate suitable for forming the second active layer by regrinding material waste from the blow molding process.
[0031] The second active layer can be arranged from the first active layer inwards. This means that from the inside to the outside of the container wall, the order of the layers can be (optional one or more layers) - second active layer - (optional one or more layers) - first active layer - (optional one or more layers) - outer layer. This arrangement can cause gas arriving at the container from the outside to reach the "more active" first active layer before reaching the more inner layers.
[0032] The second active layer may be adjacent to the first active layer. As mentioned above, the second active layer, having a lower filling rate of one or more active materials and a higher amount of base polymer compared to the first active layer, can provide higher gas diffusion resistance. Therefore, gases (e.g., moisture and / or oxygen) can travel through the first active layer more easily than through the second active layer. Gases traveling from the outside of the container and through the "barrier" outer layer may then tend to be blocked by the second active layer located inside the first active layer, allowing the gas to diffuse within the more permeable first active layer, where it can be trapped by one or more active materials before reaching the internal chamber of the container.
[0033] The container may include an inner layer configured to contact the container's internal atmosphere. When in use, the inner layer may contact the container's internal atmosphere (just as the inner surface of a bottle contacts the internal space inside the bottle).
[0034] The inner layer may include at least 95 wt% of the base polymer.
[0035] The active structure can be arranged between the outer and inner layers. This provides the benefit of preventing direct contact between one or more active materials and the contents of the container. This protects sensitive products. The container may be suitable, for example, for containing food and / or pharmaceuticals and / or medical products.
[0036] Advantageously, when the active structure is arranged between the outer and inner layers as described above, gas traveling from the outside of the container and passing through the “barrier” outer layer may tend to be blocked by the inner layer, allowing the gas to remain within and diffuse in the active layer of the active structure, thereby increasing the likelihood that the gas will be absorbed by one or more active materials.
[0037] The inner layer can have a thickness of 0.5 mm or less. The inner layer can have a thickness of 0.3 mm or less. The thickness of the inner layer can be small enough to ensure effective absorption of gases from the internal chamber of the container.
[0038] The base polymer of the outer layer can be polyethylene (PE). Alternatively, the base polymer of the outer layer can be high-density polyethylene (HDPE) with a melt flow index (MFI) of less than 1 g / 10 min as measured according to ASTM D1238 (190°C, 2.16 kg). In this case, the outer layer can have high gas barrier properties and is well-suited for multilayer extrusion blow molding (e.g., HDPE grades designed for extrusion blow molding).
[0039] Throughout this article, the melt flow index (MFI) values were measured according to standard test method ASTM D1238 Procedure A with a load of 2.16 kg and at a temperature of 190°C.
[0040] The outer layer can have a thickness equal to or greater than 0.3 mm. The outer layer can have a thickness equal to or greater than 0.4 mm. In this way, the thickness of the outer layer can be large enough to block gases from the outside.
[0041] The first active layer can contain the same base polymer as the outer layer. This improves chemical compatibility. It also enhances cohesion during the extrusion blow molding process, as these materials may be less prone to breakage or separation when blow-stretched during the manufacturing process.
[0042] The first active layer may contain one or more active materials, and optionally one or more desiccants.
[0043] The base polymer and one or more active materials together can constitute at least 95 wt% of the first active layer. This can improve chemical compatibility. It can also improve cohesion during the extrusion blow molding process, because these materials may be less prone to cracking or separation when blow-stretched.
[0044] The first active layer may comprise a base polymer and a molecular sieve. The base polymer and the molecular sieve together may constitute at least 95 wt% of the first active layer. The molecular sieve can maintain very low humidity levels and is therefore well-suited for packaging moisture-sensitive products such as probiotics or diagnostic test strips.
[0045] The active structure may include an intermediate layer disposed between the first active layer and the second active layer. The intermediate layer may include at least 95 wt% of the base polymer.
[0046] Therefore, the first and second active layers can be separated, for example, by a “barrier” intermediate layer. This can, for example, create a “5-layer” container wall structure comprising the following layers in sequence from the inside to the outside of the container: an inner layer (e.g., HDPE containing a white colorant), a second active layer (e.g., a desiccant compound layer), an intermediate layer, a first active layer (e.g., another desiccant compound layer) (the latter three layers constitute the active structure), and an outer layer (e.g., HDPE containing a white colorant). Due to the presence of the intermediate layer with undamaged gas barrier properties, gas traveling from the outside of the container is trapped in the first active layer, while gas from the inside of the container is trapped in the second active layer.
[0047] The active structure may include one or more additional layers. For example, the active structure may include one or more EVOH layers that enhance oxygen barrier properties.
[0048] The container wall may comprise polyethylene (PE), optionally high-density polyethylene (HDPE), and one or more active materials, optionally one or more desiccants. Polyethylene (PE) and one or more active materials together may constitute at least 95 wt% of the container wall. This simplifies the structure and therefore simplifies manufacturing because only one type of base polymer is used for the container composition. Furthermore, this choice of material can improve the uniformity of the composition of material waste from the blow molding process.
[0049] The container wall may comprise polyethylene (PE), optionally high-density polyethylene (HDPE), and molecular sieves. The polyethylene (PE) and molecular sieves together may constitute at least 95 wt% of the container wall. This allows for further simplification of the container's material formulation (using only one type of desiccant), and the material properties can reduce the variability in the properties of material waste from the blow molding process.
[0050] The container wall may comprise high-density polyethylene (HDPE) and molecular sieves, and the HDPE and molecular sieves together may constitute at least 95 wt% of any layer of the container wall. This allows material waste from the blow molding process to also consist of at least 95 wt% HDPE and molecular sieves, thereby increasing the compatibility between the recycled material layer obtained by recycling material waste from the blow molding process and one or more adjacent layers.
[0051] The container walls can contain between 60 wt% and 90 wt% high-density polyethylene (HDPE); between 10 wt% and 40 wt% molecular sieves; and between 0 wt% and 10 wt%, optionally between 0 wt% and 5 wt% additives. This provides a suitable desiccant fill rate for "recycling" into the blow-molded layer. Therefore, the container manufacturing process can be highly efficient and continuous.
[0052] Additives may include colorant masterbatches and / or processing aids.
[0053] The container can be an extruded blow-molded container with a draw ratio equal to or greater than 25%. Despite the presence of an active layer containing one or more active materials, stretchability is maintained, and with these active layers, the melt readily separates at the interface between the base polymer and one or more active materials.
[0054] The draw ratio should be understood as the ratio between the maximum and minimum external dimensions of the container. Dimensions are measured in a plane perpendicular to the main axis corresponding to the extrusion direction. In the case of containers with a circular cross-section (a circular shape in a cross-sectional plane perpendicular to the main axis), the draw ratio is the ratio of the container's outer diameter, measured on the sidewall, to the outer diameter of the container's neck (excluding threads).
[0055] The container can be an extruded blow-molded container with a draw ratio equal to or greater than 30%. Despite the presence of an active layer containing one or more active materials, stretchability can be maintained with particularly high reliability, with which the melt readily separates at the interface between the base polymer and one or more active materials.
[0056] The container walls can be regrindable, resulting in a regrindable compound containing at least one base polymer and at least one active material, with a melt flow index (MFI) between 0.1 and 2.0 g / 10 min, optionally between 0.1 and 1.0 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg). The MFI of the regrindable compound can thus be maintained within a processable MFI window obtained by regrinding backfill and / or neck flash and forming a second active layer. To achieve this desired MFI range, input parameters can include the selection of raw materials and processing parameters during compounding (screw design, operating parameters). For polymer resins processable in multilayer extrusion blow molding machines, careful adjustment of the material's MFI may be necessary. Too high an MFI (low viscosity) can cause parison sag, meaning the extruded parison may experience sagging under its own weight. In contrast, too low an MFI (high viscosity) may affect productivity or make resin extrusion impossible. Therefore, the MFI of the reclaimed material compound may need to be within a window that allows for processing via extrusion blow molding. The scope of protection required can be appropriate.
[0057] This disclosure also relates to a container including an internal chamber for receiving sensitive products, the internal chamber being defined by a wall. The term "defined" does not mean that the wall must completely enclose the internal chamber. The wall may include one or more openings providing passage to the internal chamber. Typically, the internal chamber may have a bottom surface and side surfaces, as well as an opening at the top, which can be closed by a cover member.
[0058] The wall may include an outer layer configured to contact the external atmosphere surrounding the container. When the container is placed in the external atmosphere (e.g., when the container is placed indoors), the outer layer contacts the external atmosphere (just as the outer surface of the bottle contacts the external atmosphere).
[0059] The outer layer may include at least 95 wt% of the base polymer.
[0060] The wall may include active structures arranged from the outermost layer inwards. Positioning from the outermost layer inwards means that the outermost layer faces outwards (and, therefore, towards the external atmosphere), while the inner surface of the outermost layer faces the active structures. In the sense that the outermost layer can contact the active structures, the inner surface of the outermost layer can directly face the active structures. The active structures then include layers that contact the inner surface of the outermost layer. Alternatively, one or more layers may exist between the outermost layer and the active structures.
[0061] In other words, when considering all the layers from the inner chamber toward the outer atmosphere, the order can be as follows: (optional one or more additional layers), active structure, (optional one or more additional layers), and outer layer. Therefore, the container can, for example, consist of the following layers from the inside out: active structure and outer layer.
[0062] The active structure may contain a base polymer and at least one active material.
[0063] The container walls may be regrindable, thereby producing a regrindable material compound comprising at least one base polymer and at least one active material, wherein the melt flow index (MFI) of the regrindable material compound is between 0.1 and 2.0 g / 10 min, optionally between 0.1 and 1.0 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg).
[0064] This disclosure also relates to a method of manufacturing a container including an internal chamber for receiving sensitive products. The term sensitive products may specifically cover moisture-sensitive products (such as food, pharmaceuticals, or medical articles).
[0065] This method may include co-extruding different materials into a preform using a multi-layer extrusion blow molding machine comprising multiple hoppers. The preform may be tubular.
[0066] The method may include closing the two halves of a blow molding die around the preform to enclose the preform in the cavity of the blow molding die.
[0067] At the bottom part of the preform, where the two half molds are joined, the preform can be compressed into a flat shape by the clamping opening of the blow molding die, for example.
[0068] The method may include inflating the preform with air and pressing the preform against the wall of the mold.
[0069] This method may include cooling and solidifying the preform in the mold cavity.
[0070] Excess material at the bottom portion of the blank can be removed, and after removal, the bottom portion of the blank can be clamped to form a clamped portion, thereby forming a container having an internal cavity defined by a wall having a clamped portion at the bottom.
[0071] At least a portion of the excess material can be recycled. Recycling produces recycled material. The recycled material can consist only of clamping scrap, only of neck flash, or a combination of both clamping scrap and neck flash. The recycled material can be fed into at least one of the hoppers of a multi-stage extrusion blow molding machine.
[0072] In other words, instead of discarding all the excess material, at least a portion (optionally, all) of the excess material can be reused. After re-grinding, the waste material can be co-extruded to form an additional (second) active layer, in which the concentration of active material is lower than that in the first active layer. The lower concentration may be due to "dilution" by the material in the outer and / or other layers.
[0073] Therefore, containers can be manufactured in a more efficient and environmentally friendly way.
[0074] Excess material at the neck of the parison at the top can be removed. An opening can be formed at the top of the parison.
[0075] This disclosure also relates to a container manufactured by the described method.
[0076] This disclosure also relates to a method for preparing active formulations suitable for extrusion blow molding (EBM). The method may include the following steps: (a) Mixing a base polymer with at least one active material such that the at least one active material is distributed within the base polymer to obtain the resulting active compound; (b) Forming a container including an internal cavity by extrusion blow molding (EBM) through co-extrusion of the following: An outer layer configured to contact the external atmosphere surrounding the container, wherein the outer layer comprises at least 95 wt% of a base polymer, and An active structure, arranged from the outermost layer inwards, wherein the active structure comprises the obtained active compound, such that the amount of the obtained active compound in the container is at least 20 wt%. (c) Optionally, adjust the melt flow index (MFI) of the base polymer used to obtain the resulting active compound and repeat steps (a) and (b) until the melt flow index (MFI) of the regrind material compound obtained through the wall of the regrinding vessel, as measured according to ASTM D1238 (190°C, 2.16 kg), is between 0.1 and 2.0 g / 10 min, or optionally between 0.1 and 1.0 g / 10 min.
[0077] The resulting active blend can be a homogeneous active blend, wherein the wt% amount of the at least one active material in the active blend remains constant within a tolerance of ± 5%.
[0078] The mixing apparatus for performing mixing step (a) can be a co-rotating twin-screw extruder.
[0079] The wt% amount of the at least one active material in the active compound may be equal to or greater than 50 wt%, and optionally equal to or greater than 60 wt%.
[0080] The at least one active material can be at least one desiccant, optionally a molecular sieve. A molecular sieve desiccant (e.g., 4A molecular sieve in powder form with an average particle size of 8 µm) can be added to the molten base polymer and blended in a two-component apparatus. The wt% amount of the molecular sieve desiccant in the active blend can be 65 wt% ± 5 wt%.
[0081] Additional advantages and features of this disclosure (which may be implemented individually or in combination with one or more features discussed above, provided that these features do not contradict each other) will become apparent from the following description of specific embodiments. Attached Figure Description
[0082] To better understand this disclosure and to show how it can be implemented, reference will now be made to the accompanying drawings by way of example only.
[0083] The description is given with reference to the attached figures, in which: Figure 1 This is a front view of an embodiment of a container for atmosphere control according to the present disclosure; Figure 2 This is a cross-sectional view and an enlarged view of a portion of the four walls of the container according to an embodiment of the container for atmosphere control according to the present disclosure. Figure 3 This is a cross-sectional view of an extruder with four hoppers used during the manufacture of an embodiment of a container for atmosphere control according to the present disclosure; Figure 4 These are schematic diagrams illustrating different stages of an embodiment of a manufacturing method according to the present disclosure involving extrusion blow molding; Figure 5 It is a graph illustrating experimental results of short-term absorption of an exemplary container for atmosphere control according to the present disclosure; Figure 6 It is a graph illustrating experimental results of long-term absorption of an exemplary container for atmosphere control according to the present disclosure; Figure 7 This is a cross-sectional view of an embodiment of a container for atmosphere control according to the present disclosure, and an enlarged view of a portion of the three-layered walls of the container; and Figure 8 This is a cross-sectional view of an embodiment of a container for atmosphere control according to the present disclosure, and an enlarged view of a portion of the five-layered wall of the container.
[0084] Figure 1This is a front view of an embodiment of a container 1 for atmosphere control according to the present disclosure.
[0085] Container 1 includes an internal chamber for receiving sensitive products. The internal chamber 2 is defined by a wall 3.
[0086] The container 1 is provided with an opening 4 and a neck 5, the neck being provided with threads 6, and a cap (not shown) can be screwed onto the threads to close the container 1.
[0087] Figure 2 Depicting Figure 1 Container 1 along Figure 1 The cross-sectional view of line II-II depicted in the figure. Figure 2 As shown on the right, this embodiment of container 1 includes a wall 3, which is further composed of four layers.
[0088] The four layers of wall 3 include an outer layer 30, which is in contact with the external atmosphere surrounding container 1.
[0089] The outer layer 30 comprises at least 95 wt% of a base polymer. In this embodiment, the base polymer of the outer layer 30 is high-density polyethylene (HDPE) having a melt flow index (MFI) of less than 1 g / 10 min when measured according to ASTM D1238 (190°C, 2.16 kg). However, other embodiments may contain other base polymers, such as another type of polyethylene (PE). The outer layer in this embodiment has a thickness greater than 0.4 mm. However, for other embodiments, this thickness may be smaller.
[0090] The four layers of wall 3 also include multilayer active structures 40 arranged from the outer layer 30 inward.
[0091] Figure 1 The embodiment also includes an inner layer 35 positioned inward relative to the multilayer active structure 40. In other words, the multilayer active structure 40 is arranged between the outer layer 30 and the inner layer 35.
[0092] The inner layer 35 is in contact with the internal atmosphere of the container present in the internal space 2. The inner layer 35 comprises at least 95 wt% of a base polymer. In this embodiment, the base polymer of the inner layer 35 is high-density polyethylene (HDPE). However, other embodiments may contain other base polymers, such as another type of polyethylene (PE). The inner layer in this embodiment has a thickness of less than 0.3 mm. However, the inner layer in other embodiments may be thicker.
[0093] The multilayer active structure 40 includes a first active layer 41, which comprises a base polymer and an active material. The first active layer 41 comprises the active material in a first wt% amount of C1.
[0094] In this embodiment, the first wt% amount C1 of the active material in the first active layer 41 is greater than 60 wt%. However, other embodiments may have a lower wt% amount.
[0095] The first active layer comprises at least 95 wt% of the same base polymer as the outer layer, as well as a desiccant. Other embodiments may additionally or alternatively include one or more other active materials.
[0096] The base polymer and one or more active materials together constitute at least 95 wt% of the first active layer 41.
[0097] The first active layer 41 comprises a base polymer and a molecular sieve. The base polymer and the molecular sieve together constitute at least 95 wt% of the first active layer 41.
[0098] The multilayer active structure 40 also includes a second active layer 42. The second active layer 42 contains all the materials present in any other layer, namely, all the materials present in the first active layer 41, the outer layer 30, and the inner layer 35.
[0099] In fact, at least 95% by weight of the second active layer 42 is composed of materials present in the first active layer 41, the outer layer 30 and the inner layer 35.
[0100] The second active layer 40 contains the active material in a second wt% amount C2, wherein the second wt% amount C2 is less than the first wt% amount C1.
[0101] The second active layer 42 is adjacent to the first active layer 41 and is positioned inward relative to the first active layer 41.
[0102] The container wall is generally composed of high-density polyethylene (HDPE) between 60 wt% and 90 wt%, molecular sieves between 10 wt% and 40 wt%, and additives between 0 wt% and 10 wt%. Additives may include known colorant masterbatches and / or known processing aids.
[0103] Figure 1 and Figure 2 Container 1 is an extruded blow-molded container with a draw ratio greater than 30%. However, other containers may have lower draw ratios.
[0104] The wall of container 1 is regrindable, thereby producing a regrindable material compound comprising at least one base polymer and at least one active material, wherein the melt flow index (MFI) of the regrindable material compound is between 0.1 and 2.0 g / 10 min, optionally between 0.1 and 1.0 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg).
[0105] Figure 3 An embodiment of a multi-layer extrusion blow molding machine 50 comprising multiple hoppers 51, 52, 53, 54 is depicted for implementing a method of manufacturing a container, the container including an internal chamber for receiving sensitive products.
[0106] Figure 4 The illustration depicts a method of manufacturing a container that includes an internal chamber for receiving sensitive products.
[0107] Step S1 is illustrated in Figure 4 The left side. This step involves using... Figure 3 The multi-layer extrusion blow molding machine 50 co-extrudes different materials to form a preform 55. In the illustrated embodiment of the method, the preform is tubular.
[0108] The two half molds 60 and 61 of the blow molding die close around the parison 55 to enclose the parison 55 in the mold cavity of the blow molding die.
[0109] At the bottom portion 56 of the preform 55 (see...) Figure 4 The second figure from the left in step S2 (shown in the middle diagram), that is, where the two half molds 60 and 61 are joined, in step S2, the preform 55 is flattened into a flat shape by the clamping opening of the blow molding die.
[0110] In step S3, the blank 55 is inflated with air and pressed against the walls of the two half molds 60 and 61.
[0111] Then the preform 55 is cooled and solidified in the mold cavity.
[0112] In step S4 (illustrated in...) Figure 4 On the right side, open the two half molds 60 and 61. Excess material portion 57 remains attached to the bottom portion 56 of the preform 55. This excess material portion 57 is cut off and then discarded according to known methods.
[0113] According to an embodiment, excess material portion 57 is removed to form a blank portion at the bottom of the container (e.g., for example). Figure 1 and Figure 2 As shown), this forms a container 1 having an internal chamber defined by a wall having a blank clamping portion at the bottom.
[0114] The excess material portion 57 is recycled into regrind material and fed into… Figure 3 At least one of the hoppers 51, 52, 53, and 54 of the multi-layer extrusion blow molding machine 50 shown.
[0115] The illustrated embodiment of the method further includes the step of removing excess material 58 of the neck flash at the top portion of the preform 55 and thereby forming an opening at the top of the preform 55.
[0116] In use Figure 3 The illustrated extrusion blow molding machine 50 is before and during the execution Figure 4 Prior to the steps illustrated, an active compound suitable for extrusion blow molding (EBM) is prepared. For this purpose, the base polymer and active material are mixed to obtain a homogeneous active compound.
[0117] A bottle is manufactured as an example of a container according to this disclosure. The moisture-proof efficiency of the manufactured bottle is then experimentally evaluated.
[0118] Specifically, a 60 cm one was manufactured. 3 Bottle (this is described in more detail in the section on "Examples").
[0119] The data logger is placed inside the manufactured bottle, and the bottle is sealed with an induction foil seal. The bottle with the built-in data logger is then kept in a climate chamber set at 40°C and 75%RH.
[0120] The humidity inside the bottle is recorded every 30 minutes by a data logger.
[0121] After 26 days, the bottle was removed from the climate chamber and opened to remove the data logger, and the %RH recorded by the data logger over time was collected.
[0122] Figure 5 The obtained measurement results are depicted. For example, the measurement at 60 cm is shown. 3 The trend of relative humidity (%) in the bottle over time. Figure 5 As can be seen, the moisture content inside the bottle dropped to 0%RH within the first 10 days and remained at 0%RH until the end of the test on day 26. The humidity inside the bottle decreased from an initial 50%RH to below 10%RH in less than 24 hours.
[0123] The multi-layered bottles manufactured to act as active moisture barriers are effective in both removing moisture contained inside the bottle and preventing moisture from entering from the external environment.
[0124] Measurements were also taken over a longer period of time. Figure 6 The results obtained from the experiment are illustrated.
[0125] Next, place the data logger inside the manufactured bottle and seal the bottle with an induction foil seal. Keep the bottle with the built-in data logger in a climate chamber set at 40°C and 75% RH.
[0126] The humidity inside the bottle is recorded every 30 minutes by a data logger.
[0127] After 130 days, the bottle was removed from the climate chamber and opened to remove the data logger, and the %RH recorded by the data logger over time was collected.
[0128] As shown in the figure at 60 cm 3 The trend of relative humidity (%) in the bottle over time. Figure 6 As can be seen from the curve, the moisture inside the bottle remains at 0% RH for at least 100 days.
[0129] Multi-layered bottles, which act as active moisture barriers, are effective in both removing moisture contained inside the bottle and preventing moisture from entering from the external environment.
[0130] Figure 7 This is a cross-sectional view of an embodiment of a container 1 for atmosphere control according to the present disclosure, and an enlarged view of a portion of the three-layered walls of the container 1.
[0131] The parts of this description will be similar to those for... Figure 1 and Figure 2 The embodiments provided are described below. Repeated content will be omitted, but the same reference numerals will be used to denote similar parts.
[0132] Figure 7 Implementation examples and Figure 1 and Figure 2 The differences between the embodiments are: Figure 7 The wall 3 in the embodiment includes three (instead of four) layers.
[0133] Figure 7 The three layers of the wall 3 of the container 1 include an outer layer 30, which is in contact with the external atmosphere surrounding the container 1.
[0134] The outer layer 30 comprises at least 95 wt% of a base polymer. In this embodiment, the base polymer of the outer layer 30 is high-density polyethylene (HDPE) having a melt flow index (MFI) of less than 1 g / 10 min as measured according to ASTM D1238 (190°C, 2.16 kg). However, other embodiments may contain other base polymers, such as another type of polyethylene (PE). The outer layer in this embodiment has a thickness greater than 0.4 mm. However, for other embodiments, this thickness may be smaller.
[0135] The three layers of wall 3 also include multilayer active structures 40 arranged from the outer layer 30 inward.
[0136] The multilayer active structure 40 includes a first active layer 41, which comprises a base polymer and an active material. The first active layer 41 comprises the active material in a first wt% amount of C1.
[0137] In this embodiment, the first wt% amount C1 of the active material in the first active layer 41 is greater than 60 wt%. However, other embodiments may have a lower wt% amount.
[0138] The first active layer comprises at least 95 wt% of the same base polymer as the outer layer, as well as a desiccant. Other embodiments may additionally or alternatively include one or more other active materials.
[0139] The base polymer and one or more active materials together constitute at least 95 wt% of the first active layer 41.
[0140] The first active layer 41 comprises a base polymer and a molecular sieve. The base polymer and the molecular sieve together constitute at least 95 wt% of the first active layer 41.
[0141] The multilayer active structure 40 also includes a second active layer 42. The second active layer 42 contains all the materials present in any other layer, namely, those present in the first active layer 41 and the outer layer 30, respectively.
[0142] In fact, at least 95% by weight of the second active layer 42 is composed of the material present in the first active layer 41 and the outer layer 30.
[0143] The second active layer 40 contains the active material in a second wt% amount C2, wherein the second wt% amount C2 is less than the first wt% amount C1.
[0144] The second active layer 42 is adjacent to the first active layer 41 and is positioned inward relative to the first active layer 41.
[0145] Figure 7 Container 1 is an extruded blow-molded container with a draw ratio greater than 30%. However, other containers may have lower draw ratios.
[0146] The wall of container 1 is regrindable, thereby producing a regrindable material compound comprising at least one base polymer and at least one active material, wherein the melt flow index (MFI) of the regrindable material compound is between 0.1 and 2.0 g / 10 min, optionally between 0.1 and 1.0 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg).
[0147] Figure 8This is a cross-sectional view of an embodiment of a container 1 for atmosphere control according to the present disclosure, and an enlarged view of a portion of the five-layered wall of the container 1.
[0148] The parts of this description will be similar to those for... Figure 1 and Figure 2 Implementation examples and for Figure 7 The embodiments provided are described below. Repeated content will be omitted, but the same reference numerals will be used to denote similar parts.
[0149] Figure 7 Implementation examples and Figure 8 The differences between the embodiments are: Figure 8 The wall 3 in the embodiment includes five (instead of three) layers.
[0150] The five layers of wall 3 include an outer layer 30, which is in contact with the external atmosphere surrounding container 1.
[0151] The outer layer 30 comprises at least 95 wt% of a base polymer. In this embodiment, the base polymer of the outer layer 30 is high-density polyethylene (HDPE) having a melt flow index (MFI) of less than 1 g / 10 min when measured according to ASTM D1238 (190°C, 2.16 kg). However, other embodiments may contain other base polymers, such as another type of polyethylene (PE). The outer layer in this embodiment has a thickness greater than 0.4 mm. However, for other embodiments, this thickness may be smaller.
[0152] The five layers of wall 3 also include multilayer active structures 40 arranged from the outer layer 30 inward.
[0153] Figure 8 The embodiment also includes an inner layer 35 positioned inward relative to the multilayer active structure 40. In other words, the multilayer active structure 40 is arranged between the outer layer 30 and the inner layer 35.
[0154] The inner layer 35 is in contact with the internal atmosphere of the container present in the internal space 2. The inner layer 35 comprises at least 95 wt% of a base polymer. In this embodiment, the base polymer of the inner layer 35 is high-density polyethylene (HDPE). However, other embodiments may contain other base polymers, such as another type of polyethylene (PE). The inner layer in this embodiment has a thickness of less than 0.3 mm. However, the inner layer in other embodiments may be thicker.
[0155] The multilayer active structure 40 includes a first active layer 41, which comprises a base polymer and an active material. The first active layer 41 comprises the active material in a first wt% amount of C1.
[0156] In this embodiment, the first wt% amount C1 of the active material in the first active layer 41 is greater than 60 wt%. However, other embodiments may have a lower wt% amount.
[0157] The first active layer comprises at least 95 wt% of the same base polymer as the outer layer, as well as a desiccant. Other embodiments may additionally or alternatively include one or more other active materials.
[0158] The base polymer and one or more active materials together constitute at least 95 wt% of the first active layer 41.
[0159] The first active layer 41 comprises a base polymer and a molecular sieve. The base polymer and the molecular sieve together constitute at least 95 wt% of the first active layer 41.
[0160] The multilayer active structure 40 also includes a second active layer 42. The second active layer 42 contains all the materials present in any other layer, namely, all the materials present in the first active layer 41, the outer layer 30, and the inner layer 35.
[0161] In fact, at least 95% by weight of the second active layer 42 is composed of materials present in the first active layer 41, the outer layer 30 and the inner layer 35.
[0162] The second active layer 40 contains the active material in a second wt% amount C2, wherein the second wt% amount C2 is less than the first wt% amount C1.
[0163] The multilayer active structure 40 includes an intermediate layer 43 located between the first active layer 41 and the second active layer 42. In other words, the multilayer active structure 40 of this embodiment is a three-layer active structure. The intermediate layer 43 comprises at least 95 wt% of a base polymer. In this embodiment, the base polymer of the intermediate layer 43 is high-density polyethylene (HDPE). However, other embodiments may contain other base polymers, such as another type of polyethylene (PE).
[0164] Figure 8 Container 1 is an extruded blow-molded container with a draw ratio greater than 30%. However, other containers may have lower draw ratios.
[0165] The wall of container 1 is regrindable, thereby producing a regrindable material compound comprising at least one base polymer and at least one active material, wherein the melt flow index (MFI) of the regrindable material compound is between 0.1 and 2.0 g / 10 min, optionally between 0.1 and 1.0 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg).
[0166] Example Examples of containers 1 according to the present disclosure have been manufactured to implement the methods according to the present disclosure, and measurements have been performed on these containers 1 to investigate various properties of them.
[0167] Specifically, an example of a container produced using multilayer extrusion blow molding has a diameter of 60 cm. 3 100 cm 3 and 150cm 3 The internal capacity of the four-layer bottle.
[0168] The manufactured four-layer bottle comprises four layers: an inner layer, an active structure including a second active layer (adjacent to the inner layer) and a first active layer (adjacent to the outer layer), and an outer layer facing outwards.
[0169] The material composition of the manufactured bottles is summarized in Table 1:
[0170] Table 1 The melt flow index (MFI) of the constituent materials of each of the outer and inner layers is 0.22 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg).
[0171] The melt flow index (MFI) of reclaimed material from blow molding process waste from containers can be determined by cutting a portion of the container's sidewall and reclaiming it, then measuring the MFI of the resulting reclaimed material according to ASTM D1238 (190°C, 2.16 kg). Using this procedure, the melt flow index (MFI) of the reclaimed material from blow molding process waste from containers used for the second active layer, as measured according to ASTM D1238 (190°C, 2.16 kg), is 0.18 g / 10 min.
[0172] The stretch ratio for each of the three bottle sizes is given in Table 2 below:
[0173] Table 2 The bottle is manufactured according to an example of the disclosed method.
[0174] The preparation of the active mixture for the first active layer (layer 2 in Table 1) includes the following steps: - Mix 35 wt% of molten HDPE base polymer and 65 wt% of molecular sieve desiccant in a twin-screw extruder heated to about 200°C; - Extruding the blend of HDPE base polymer and molecular sieve desiccant into strips; - Cool the strip material and granulate it; - Samples of the obtained active compound granules were taken at an output of 15 kg / h at the beginning, middle, and end of the 7-hour production test, and the wt% amount C1 of the molecular sieve desiccant in the active compound was measured. The data obtained for the wt% amount C1 in the active compound are listed in Table 3 below:
[0175] Table 3 The blending process is considered complete when the resulting active compound is homogeneous and the wt% amount C1 of the active material in the active compound is constant within a tolerance of ± 5%.
[0176] The selection of the HDPE base polymer used to obtain the active blend includes the following steps: - Use active compound to form layer 2 of a multilayer extrusion blow molding test container with internal chambers and the layer structure described in Table 1 above; - Measure the melt flow index (MFI) of the re-grind material compound obtained by passing it through the wall of the re-grind test vessel, and adjust the melt flow index (MFI) of the HDPE base polymer used to obtain the active compound until the melt flow index (MFI) of the re-grind material compound is between 0.1 and 1.0 g / 10 min when measured according to ASTM D1238 (190°C, 2.16 kg).
[0177] During each molding cycle, excess material is generated as waste at the neck and bottom portions of the bottle. Instead of discarding the waste material from each bottle (“preform scrap” and “neck flash”), the extrusion blow molding (EBM) process waste is re-milled to form a second active layer (layer 3 in Table 1). The waste material from both the top and bottom is kept clean and re-milled back into the production process. 100% of the re-milled material can be reused if needed.
[0178] Using a bottle mold, such as Figure 3 The four-layer extrusion blow molding (EBM) machine shown is used to produce an exemplary four-layer bottle.
[0179] The hopper of the extrusion blow molding (EBM) machine is filled as follows: - The outer hopper (1) and the inner hopper (4) are filled with 97 wt% HDPE and 3 wt% white colorant masterbatch. - The hopper (2) corresponding to the first active layer is filled with a moisture-absorbing compound prepared from HDPE base polymer and desiccant molecular sieve, and - The hopper (3) corresponding to the second active layer is filled with a moisture-absorbing compound obtained from waste material from the recycled extrusion blow molding (EBM) process.
[0180] Begin extruding the parison and check for consistency and straightness. If the parison is not extruded properly, adjust the machine temperature and pressure until they are consistent.
[0181] Once the consistency and straightness of the preform are confirmed, the extrusion blow molding (EBM) machine is operated according to normal operating standards, and bottle samples are collected.
[0182] The bottle sample is cut and each layer is examined using a microscope or another optical measuring device. Then, based on these measurements, the extruder is adjusted to achieve the desired thickness for each layer.
[0183] Once the thickness of each layer is confirmed, the extrusion blow molding (EBM) operation is resumed, and the finished bottles are collected into aluminum bags and sealed to preserve the bottle's absorbency properties.
[0184] As a next step, the layer thickness is measured. To do this, the bottle is cut vertically in half next to the seam line.
[0185] Next, cut a section of the bottle from the straight part of the side wall. The cut should be as close to the center of the bottle as possible (vertical).
[0186] The cut section is then placed in an ultramicrotome and several thin slices (typically 2-3 slices) are cut off and discarded until the cut surface is fresh and free of scratches or deformation.
[0187] Next, cut the slice to be measured. The thickness of the slice must be less than 0.75 mm.
[0188] The sheet to be measured is placed in the fixture in such a way that the sheet lies flat and parallel to the surface.
[0189] The fixture is moved to an optical measurement device, such as the SmartScope from OGP, to measure the layer thickness. The thickness is measured perpendicular to the side wall of the bottle at the midpoint of the sheet length.
[0190] The layer thicknesses measured for each bottle size are given in Table 4 below.
[0191]
[0192] Table 4 The advantage of sandwiching at least one active layer (e.g., a desiccant layer) between two "primary layers" of the polymer resin is that one or more thin active layers (e.g., one or more desiccant layers) can be incorporated. Within the meaning of this invention, it should be understood that a "primary layer" of the polymer resin is a polymer resin layer that does not contain active material. This is the case in the example above, where the outer and inner layers (and possibly intermediate layers) are.
[0193] In the case of material blends containing a base polymer and mineral fillers such as desiccants, the melt is prone to cracking at the interface between the polymer and the mineral filler (desiccant).
[0194] In the molten form of an active polymer compound (e.g., a desiccant polymer compound), the active material particles (e.g., desiccant particles) form regions of increased brittleness, and the preform is prone to tearing, with the fracture point originating from the active material particles (e.g., desiccant particles).
[0195] By sandwiching one or more active polymer layers (e.g., one or more desiccant polymer layers) between two adjacent layers containing “native polymer” resins belonging to the same chemical family as the resins used in the active polymer blend (e.g., desiccant polymer blend), the thinness of the one or more active polymer layers is not limited to the needs of producing unsupported preforms, and the ability to stretch one or more active polymer layers (e.g., one or more desiccant polymer layers) during subsequent blow molding sequences without causing tearing can be significantly improved.
[0196] This might be considered particularly important because: - Active polymers (e.g., desiccant polymers) are more expensive than barrier polymers typically used in the production of moisture-barrier containers; the amount of active polymer (e.g., desiccant polymer) used only needs to be sufficient to provide the desired performance, and In layers formed of active polymers (e.g., desiccant polymers), contaminants (e.g., water molecules) require a longer time to reach particles located far from the surface; to maintain proper reactivity of the active material (e.g., desiccant), it may be preferable to reduce the thickness of the active layer (e.g., desiccant layer). This may be particularly important because the preferred polymer for forming the active polymer blend (e.g., desiccant blend) is HDPE, which is known to be a moisture-barrier material.
[0197] As a next step, the moisture-proof efficiency of the manufactured bottles will be evaluated. (The above is combined with...) Figure 5 and Figure 6 The results of the measurement are described.
[0198] It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed apparatus and systems without departing from the scope of this disclosure. Other aspects of this disclosure will be apparent to those skilled in the art in light of the practice of this specification and the features disclosed herein. This specification and examples are intended to be illustrative only. Many additional changes and modifications are possible and are to be understood to fall within the framework of this disclosure.
Claims
1. A container comprising an internal chamber for receiving a sensitive product, the internal chamber being defined by a wall comprising three or more layers, the three or more layers comprising: An outer layer configured to contact an external atmosphere surrounding the container, wherein the outer layer comprises at least 95 wt% of a base polymer; An active structure, wherein the active structure is arranged from the outer layer inward, and wherein the active structure comprises: - A first active layer, comprising a base polymer and one or more active materials, wherein the first active layer comprises one or more active materials in a first wt% amount of C1. - A second active layer comprising all the materials present in the other layers of the container wall in an amount of at least 95 wt%, the second active layer comprising the one or more active materials in a second wt% amount C2, wherein the second wt% amount C2 is less than the first wt% amount C1.
2. The container as claimed in claim 1, wherein, The ratio of the second wt% amount C2 of the one or more active materials in the second active layer to the first wt% amount C1 of the one or more active materials in the first active layer is less than 0.75, preferably less than 0.6, and preferably less than 0.
5.
3. The container as claimed in claim 1 or 2, wherein, The first wt% amount C1 of the one or more active materials in the first active layer is equal to or greater than 50 wt%, and optionally equal to or greater than 60 wt%.
4. The container as claimed in any of the preceding claims, wherein, The second active layer is arranged inward from the first active layer.
5. The container as claimed in any of the preceding claims, wherein, The second active layer is adjacent to the first active layer.
6. The container as claimed in any of the preceding claims, the container comprising an inner layer configured to contact the internal atmosphere of the container, wherein the inner layer comprises at least 95 wt% of a base polymer, and the active structure is disposed between the outer layer and the inner layer.
7. The container of claim 6, wherein, The inner layer has a thickness of less than or equal to 0.5 mm, and optionally less than or equal to 0.3 mm.
8. The container as claimed in any of the preceding claims, wherein, The base polymer of the outer layer is polyethylene (PE), and optionally high-density polyethylene (HDPE) with a melt flow index (MFI) of less than 1 g / 10 min as measured according to ASTM D1238 (190°C, 2.16 kg).
9. The container as claimed in any of the preceding claims, wherein, The outer layer has a thickness of 0.3 mm or greater, and optionally 0.4 mm or greater.
10. The container as claimed in any of the preceding claims, wherein, The first active layer comprises the same base polymer as the outer layer and one or more active materials, optionally one or more desiccants, wherein the base polymer and the one or more active materials together constitute at least 95 wt% of the first active layer.
11. The container as claimed in any of the preceding claims, wherein, The first active layer comprises a base polymer and a molecular sieve, wherein the base polymer and the molecular sieve together constitute at least 95 wt% of the first active layer.
12. The container as claimed in any of the preceding claims, wherein, The active structure includes an intermediate layer disposed between the first active layer and the second active layer, the intermediate layer comprising at least 95 wt% of a base polymer.
13. The container as claimed in any of the preceding claims, wherein, The container wall comprises polyethylene (PE), optionally high-density polyethylene (HDPE), and one or more active materials and optionally one or more desiccants, wherein the polyethylene (PE) and the one or more active materials together constitute at least 95 wt% of the container wall.
14. The container as claimed in any of the preceding claims, wherein, The container wall comprises polyethylene (PE), optionally high-density polyethylene (HDPE), and a molecular sieve, wherein the polyethylene (PE) and the molecular sieve together constitute at least 95 wt% of the container wall.
15. The container as claimed in any of the preceding claims, wherein, The container wall includes: - High-density polyethylene (HDPE) between 60 wt% and 90 wt%. - Molecular sieves between 10 wt% and 40 wt%, - Additives between 0 wt% and 10 wt%, optionally between 0 wt% and 5 wt%.
16. The container as claimed in any of the preceding claims, wherein, The container is an extruded blow-molded container having a draw ratio of 25% or higher, optionally 30% or higher.
17. The container as claimed in any of the preceding claims, wherein, The container wall is rewritable, thereby producing a rewritable material compound comprising at least one base polymer and at least one active material, wherein the melt flow index (MFI) of the rewritable material compound is between 0.1 g / 10 min and 2.0 g / 10 min, optionally between 0.1 g / 10 min and 1.0 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg).
18. A container comprising an internal chamber for receiving a sensitive product, the internal chamber being defined by a wall comprising: An outer layer configured to contact an external atmosphere surrounding the container, wherein the outer layer comprises at least 95 wt% of a base polymer; An active structure, arranged from the outer layer inwards, wherein the active structure comprises a base polymer and at least one active material. The walls of the container are regrindable, thereby producing a regrindable material compound comprising at least one base polymer and at least one active material, wherein the melt flow index (MFI) of the regrindable material compound is between 0.1 g / 10 min and 2.0 g / 10 min, optionally between 0.1 g / 10 min and 1.0 g / 10 min, as measured according to ASTM D1238 (190°C, 2.16 kg).
19. A method of manufacturing a container, the container including an internal chamber for receiving sensitive products, the method comprising the steps of: Different materials are co-extruded into preforms using a multi-layer extrusion blow molding machine with multiple hoppers; The two halves of the blow molding die are closed around the parison to enclose the parison in the mold cavity of the blow molding die, wherein at the bottom portion of the parison, i.e., where the two halves are closed, the parison is compressed by the clamping opening of the blow molding die. The preform is inflated and pressed against the wall of the mold; The preform is cooled and solidified in the mold cavity; In this process, excess material is removed from the bottom portion of the preform, and after the removal, the bottom portion of the preform is clamped to form a clamped portion, thereby forming the container having the internal chamber defined by a wall having the clamped portion at the bottom. In this process, at least a portion of the excess material is re-grinded into re-grind material, and the re-grind material is fed into at least one of the hoppers of the multilayer extrusion blow molding machine.
20. A container manufactured by the method of claim 19.
21. A method for preparing an active compound suitable for extrusion blow molding (EBM), the method comprising the following steps: (a) Mixing a base polymer with at least one active material such that the at least one active material is distributed within the base polymer to obtain the resulting active compound; (b) Forming a container including an internal cavity by extrusion blow molding (EBM) through co-extrusion of the following: An outer layer, configured to contact the external atmosphere surrounding the container, wherein the outer layer comprises at least 95 wt% of a base polymer, and An active structure, the active structure being arranged from the outer layer inwards, wherein the active structure comprises the obtained active compound, such that the amount of the obtained active compound in the container is at least 20 wt%; (c) Optionally, the melt flow index (MFI) of the base polymer used to obtain the resulting active compound is adjusted and steps (a) and (b) are repeated until the melt flow index (MFI) of the re-grind material compound obtained by re-grinding the wall of the container, as measured according to ASTM D1238 (190°C, 2.16 kg), is between 0.1 g / 10 min and 2.0 g / 10 min, and optionally between 0.1 g / 10 min and 1.0 g / 10 min.
22. An active compound obtainable by the method of claim 21, wherein, The amount of at least one active material in the active compound is equal to or greater than 50 wt%, and optionally equal to or greater than 60 wt%.
23. The active compound of claim 22, wherein, The at least one active material is at least one desiccant, optionally a molecular sieve.