Polyolefin composition comprising a recycled plastic material, an elastomer and a polypropylene homopolymer

By adding high-flowability polypropylene homopolymer and elastomer to recycled polypropylene and polyethylene, the toughness and stiffness issues of recycled materials in engineering applications are solved, achieving excellent mechanical properties of polyolefin compositions suitable for applications such as suitcases.

CN123146641APending Publication Date: 2026-11-20BOREALIS AG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202580029686.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-24
Filing Date
2025-04-23
Publication Date
2026-11-20

Smart Images

  • Figure SMS_16
    Figure SMS_16
  • Figure SMS_17
    Figure SMS_17
  • Figure SMS_18
    Figure SMS_18
Patent Text Reader

Abstract

The present invention relates to a polyolefin composition comprising: a) 60 to 85 wt% (based on the total weight of the polyolefin composition) of a plastic material blend comprising polypropylene and polyethylene in a ratio of 14:6 to 49:1, b) 10 to 30 wt% (based on the total weight of the polyolefin composition) of at least one C2 / C4 and / or C2 / C8 elastomer as compatibilizer having an MFR2 (ISO 1133 at 190 °C under a 2.16 kg load) equal to or below 30 g / min, c) 3 to 10 wt% (based on the total weight of the polyolefin composition) of a polypropylene homopolymer having an MFR2 (ISO 1133 at 230 °C under a 2.16 kg load) of at least 800 g / 10 min, and d) optionally further additives, wherein the sum of all ingredients always adds up to 100 wt%, wherein the polyolefin composition has an impact strength (ISO 179-1, Charpy 1 eA + 23 °C) of at least 30 kJ / m 2 2, a melt flow rate MFR2 (230 °C, 2.16 kg, measured according to ISO 1133) of at least 15 g / 10 min and a tensile strain at break (Iso 527-2) of at least 80 %.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention relates to polyolefin compositions comprising recycled plastic material, at least one elastomer, and at least one polypropylene homopolymer. The invention also relates to articles comprising said polyolefin composition.

[0002] describe

[0003] Polyolefins, particularly polyethylene and polypropylene, are increasingly being consumed in large quantities across a wide range of applications, including packaging for food and other items, fibers, automotive components, and a wide variety of manufactured goods. Polyethylene-based materials are particularly problematic due to their extensive use in packaging. Given the enormous volume of waste collected compared to the amount recycled back into the stream, intelligent reuse of plastic waste streams and mechanical recycling of plastic waste still hold great potential.

[0004] A major trend in the polyolefin sector is the use of recycled materials from a wide variety of sources. Durable goods streams, such as those from yellow bags, yellow bins, community collections, waste electrical equipment (WEE), or end-of-life vehicles (ELVs), contain a wide variety of plastics. These materials can be processed to recycle acrylonitrile-butadiene-styrene (ABS), high-impact polystyrene (HIPS), polypropylene (PP), and polyethylene (PE) plastics. Separation can be achieved using density separation in water followed by further separation based on fluorescence, near-infrared absorption, or Raman fluorescence. However, obtaining pure recycled polypropylene or pure recycled polyethylene is often difficult.

[0005] Typically, a large volume of recycled polypropylene on the market is a mixture of polypropylene (PP) and polyethylene (PE), especially for post-consumer waste streams. Furthermore, commercially recycled materials from post-consumer waste sources are routinely cross-contaminated with non-polyolefin materials (such as polyethylene terephthalate, polyamide, and polystyrene) or non-polymer materials (such as wood, paper, glass, or aluminum). This cross-contamination severely limits the end-use of the recycled stream, leaving no profitable end-use. Polyolefin recycled materials, especially those from post-consumer waste streams, are mixtures of PE and PP. The better the quality of the recycled material, the less available it is, and the more expensive it is.

[0006] It is known in the art that higher impact strength can be achieved by adding elastomers such as ethylene-propylene rubber, which act as compatibilizers; however, this limits the stiffness of the resulting composition. Furthermore, many of these elastomers are only available as higher molecular weight forms or in non-granulated form, the latter requiring specific mixing equipment.

[0007] EP 0 575 465 B1 covers a polymer blend composition comprising: (a) 30% to 70% by weight of a low-melt polymer comprising an ethylene / α-olefin copolymer, said low-melt polymer having a content of 0.88 g / cm³. 3 Up to 0.915 g / cm 3 (a) density, MFR of 1.5 dg / min to 7.5 dg / min, molecular weight distribution not greater than 3.5, compositional distribution width index greater than 70%, and substantially single melting point in the range of 60°C to 115°C as measured as DSC peak Tm; and (b) 70 wt% to 30 wt% of a propylene-based polymer having 88 mol% to 100 mol% propylene and 12 mol% to 0 mol% α-olefins other than propylene.

[0008] US 5,266,392 A claims protection for a polyethylene / polypropylene blend comprising: ≥50% by weight crystalline polypropylene; at least about 10% by weight linear low-density polyethylene with a density of about 0.915 to about 0.94 dispersed in a matrix of said polypropylene; and a certain amount of an ethylene / α-olefin plastomer compatibilizer having an α-olefin content of about 5 mol% to about 25 mol%, a melt index greater than about 50 dg / min, a weight-average molecular weight of about 5000 to about 50,000, and about 0.88 g / cm³. 3 Approximately 0.90 g / cm 3 The density and at least 10% X-ray crystallinity. This covers the use of plastomers as compatibilizers in a very common manner, including recycled plastomers. Only plastomers with relatively low and relatively high densities are excluded, but pure HDPE is also excluded.

[0009] WO 2015 / 169690 A1 relates to polypropylene-polyethylene blends comprising: (A) 75 wt% to 90 wt% of a blend of (A-1) and (A-2): (A-1) 30 wt% to 70 wt% polypropylene, (A-2) 70 wt% to 30 wt% polyethylene; and (B) 10 wt% to 25 wt% of a compatibilizer for a multiphase polyolefin composition comprising (B-1) 55 wt% to 90 wt% of polypropylene with an MFR2 of 1.0 g / 10 min to 300 g / 10 min (at 230°C and 2.16 kg load according to ISO 1133) and (B-2) 45 wt% to 10 wt% of a copolymer of ethylene and propylene or C4 to C10 α-olefins, said copolymer having a glass transition temperature Tg (measured by DMTA) below -25°C and at least 3.0. The intrinsic viscosity (measured in decahydronaphthalene at 135°C) is dl / g, wherein the blend has (i) a Charpy notched impact strength (measured at 23°C according to ISO 179-1eA) that is at least 2% higher than that of the same blend without compatibilizer (B), and simultaneously (ii) a flexural modulus (according to ISO 178) that is at least 3% higher than that of the same blend without compatibilizer (B), and additionally (iii) a heat deformation resistance (determined by DMTA) expressed as the temperature at which the storage modulus G' reaches 40 MPa (T(G'=40 MPa)) is at least 4° higher than that of the same blend without compatibilizer (B).

[0010] WO2020 / 089196 A1 discloses a polyethylene-polypropylene composition which can be obtained by blending the following a) and b): a) 80% to 97% by weight of a recycled blend (A) comprising A-1) polypropylene and A-2) polyethylene, wherein the weight ratio of polypropylene to polyethylene is 3:7 to 7:3; b) 3% to 20% by weight of a compatibilizer (B), said compatibilizer (B) being a C2C8 plasmid.

[0011] WO2020 / 201084 A1 relates to a polyethylene-polypropylene composition which can be obtained by blending the following a) and b): a) a recycled blend (A) comprising polypropylene and polyethylene, comprising 75.0% to 94.0% by weight of the total weight of the polyethylene-polypropylene composition, wherein the weight ratio of polypropylene to polyethylene is in the range of 3:7 to 7:3; b) a compatibilizer (B) comprising 6.0% to 25.0% by weight of the total weight of the polyethylene-polypropylene composition, wherein the compatibilizer (B) is a copolymer of 1-butene and ethylene.

[0012] For many engineering applications, the limiting factor for the wider use of recycled materials is their poor impact performance. As described in the prior art, the use of specific elastomers or plasmids can help improve the toughness of recycled material-based composites.

[0013] On the other hand, using plastics can reduce stiffness and viscosity (two important properties for consumers). In addition, other properties may also be affected.

[0014] Therefore, one object of the present invention is to provide a polyolefin composition comprising polyolefin materials recycled from household waste plastic materials that does not have the disadvantages of polymer compositions according to the prior art. In particular, there is an urgent need for composite solutions that combine virgin materials with recycled materials to balance the aforementioned problems and provide the market with advanced material products.

[0015] This objective is achieved by providing a polyolefin composition comprising the following:

[0016] a) A blend of recycled plastic materials of polypropylene and polyethylene in a ratio of 14:6 to 49.5:1, comprising 60% to 85% by weight (based on the total weight of the polyolefin composition).

[0017] b) 10% to 30% by weight (based on the total weight of the polyolefin composition) of at least one C2 / C4 and / or C2 / C8 elastomer as a compatibilizer with an MFR2 (ISO 1133, 2.16 kg load at 190°C) equal to or less than 30 g / min.

[0018] c) 3% to 10% by weight (based on the total weight of the polyolefin composition) of a polypropylene homopolymer with an MFR2 (ISO 1133, 2.16 kg load at 230°C) of at least 800 g / 10 min, and

[0019] d) Optional additional additives, wherein the total of all ingredients always amounts to 100% by weight.

[0020] The polyolefin composition has

[0021] - At least 30 kJ / m 2 Impact strength (ISO179-1, Charité 1eA+23℃).

[0022] - A melt flow rate MFR2 of at least 15 g / 10 min (230°C, 2.16 kg, measured according to ISO 1133), and

[0023] - At least 80% of the tensile strain at break (Iso 527-2).

[0024] Therefore, blends of polypropylene and polyethylene are mixed with elastomers and virgin polypropylene homopolymers with high melt flow rates to obtain polyolefin compositions with excellent mechanical properties. In particular, the polyolefin compositions of the present invention, which combine blends of polypropylene and polyethylene with elastomers and high-flow-rate polypropylene homopolymers, achieve balanced composite behavior for suitcase applications.

[0025] The polyolefin compositions of the present invention are characterized by a balanced property profile based solely on blends of polypropylene and polyethylene, elastomers, and virgin copolymers. The use of elastomers and high-flow-rate virgin polypropylene homopolymers improves the toughness and impact properties of the polypropylene and polyethylene blends. Simultaneously, the stiffness and viscosity (two important properties for consumers) of compositions containing polypropylene and polyethylene blends are not compromised. This balanced composite property makes the polyolefin compositions of the present invention attractive for many engineering applications. Particularly noteworthy is that polyolefin compositions containing a large amount of polypropylene and polyethylene blends exceeding 55% by weight and up to 85% by weight can provide both good toughness and favorable property characteristics.

[0026] The amount of a blend of polypropylene and polyethylene (e.g., a blend of recycled plastic materials containing polypropylene and polyethylene recovered from waste plastic materials derived from post-consumer waste and / or post-industrial waste) used in the polyolefin composition of the present invention in a content ratio of 14:6 to 49.5:1, preferably 15:5 to 49.5:1, more preferably 16:4 to 49.5:1, and even more preferably 17:3 to 49.5:1) is, according to the present invention, in the range of 55% to 85% by weight, preferably 60% to 80% by weight, more preferably 65% ​​to 75% by weight (based on the total weight of the polyolefin composition).

[0027] For the purposes of this specification and the appended claims, the term "recycled" is used to indicate that the material is recovered from post-consumer waste and / or industrial waste. That is, post-consumer waste refers to an object that has completed at least one first use cycle (or life cycle), i.e., has served its first purpose and has passed through the hands of a consumer; while industrial waste refers to manufacturing waste that typically does not reach consumers. In the spirit of this invention, the "recycled polymer" may also comprise up to 17% by weight, preferably up to 3% by weight, more preferably up to 1% by weight, and even more preferably up to 0.1% by weight of other components derived from the first use, based on the total weight of the recycled polymer. The type and amount of these components affect the physical properties of the recycled polymer. The physical properties given below relate to the main components of the recycled polymer.

[0028] As further described below, other components typically derived from the first use include thermoplastic polymers (such as polystyrene and PA 6), talc, chalk, ink, wood, paper, limonene, and fatty acids. The content of polystyrene (PS) and polyamide 6 (PA 6) in the recycled polymer can be determined by Fourier transform infrared spectroscopy (FTIR), while the content of talc, chalk, wood, and paper can be measured by thermogravimetric analysis (TGA).

[0029] According to the present invention, the total amount of at least one C2 / C4 or C2 / C8 elastomer used in the polyolefin composition of the present invention is 10% to 30% by weight, preferably 15% to 25% by weight, and more preferably 18% to 23% by weight (based on the total weight of the polyolefin composition).

[0030] The term "virgin" refers to newly produced materials and / or objects that are not recycled before their first use. Unless otherwise specified, a polymer is referred to as a "virgin" polymer.

[0031] According to the present invention, the total amount of any virgin polypropylene homopolymer used in the polyolefin composition of the present invention may be from 3% to 10% by weight, preferably from 4% to 8% by weight, and more preferably from 5% to 6% by weight (based on the total weight of the polyolefin composition).

[0032] It should be understood that the polyolefin composition may also contain additional additives, and in each of the embodiments described herein, the total of all components always amounts to 100 by weight.

[0033] It should also be understood that polyolefin compositions may be (substantially) free of any (native) polypropylene block copolymers. Such block copolymers comprise two or more homopolymer subunits linked by covalent bonds.

[0034] Furthermore, the polyolefin composition may be (substantially) free of any multiphase propylene copolymers. Such multiphase propylene copolymers may contain randomly inserted ethylene or butene as comonomers. This applies to any added virgin multiphase polypropylene polymer, but not to any possible trace amounts of any multiphase polypropylene polymer that may still be present in recycled materials.

[0035] It should be understood that the polyolefin compositions of the present invention do not contain talc (except in amounts present in recycled materials), glass fiber, or any other solid material.

[0036] According to one embodiment, the polyolefin composition of the present invention comprises:

[0037] a) A blend of recycled plastic materials of polypropylene and polyethylene in a ratio of 14:6 to 49.5:1, comprising 63% to 80% by weight, preferably 65% ​​to 75% by weight (based on the total weight of the polyolefin composition).

[0038] b) 15% to 25% by weight, preferably 18% to 23% by weight (based on the total weight of the polyolefin composition), of at least one C2 / C4 and / or C2 / C8 elastomer as a compatibilizer with an MFR2 (ISO 1133, 2.16 kg load at 190°C) equal to or less than 30 g / min.

[0039] c) 4% to 9% by weight, more preferably 5% to 7% by weight (based on the total weight of the polyolefin composition), of a polypropylene homopolymer with an MFR2 (ISO 1133, 2.16 kg load at 230°C) of at least 800 g / 10 min, and

[0040] d) Optional additional additives, wherein the total of all ingredients always amounts to 100 by weight.

[0041] Polyolefin compositions

[0042] The compositions according to the invention preferably exhibit an excellent balance of properties in terms of fluidity (as can be seen from melt flow rate), impact characteristics, and especially mechanical properties (e.g., tensile properties).

[0043] The polyolefin compositions of the present invention may have one or more of the properties described below, preferably all of them.

[0044] In one embodiment, the impact strength (ISO 179-1, Charpy 1eA + 23°C) of the polyolefin composition of the present invention is at least 35.0 kJ / m. 2 Preferably at least 40.0 kJ / m 2 Especially at 30.0 kJ / m 2 Up to 60.0 kJ / m 2 Within that range, and more specifically at 35.0 kJ / m 2 Up to 55.0 kJ / m 2 Within that range, and even more specifically at 40.0 kJ / m 2 Up to 55.0 kJ / m 2 Within the range.

[0045] In another embodiment, the melt flow rate MFR2 (ISO 1133, 2.16 kg, 230°C) of the polyolefin composition is at least 16.0 g / 10 min, preferably at least 17.5 g / 10 min, more preferably at least 17.5 g / 10 min, particularly in the range of 15.0 g / 10 min to 30.0 g / 10 min, preferably 16.0 g / 10 min to 25.0 g / 10 min, more preferably 17.0 g / 10 min to 20.0 g / 10 min.

[0046] In another embodiment, the tensile strain at break (ISO 527-2) of the polyolefin composition of the present invention is at least 90%, more preferably at least 100%, even more preferably at least 150%, and still more preferably at least 200%, particularly in the range of 80% to 400%, preferably 90% to 300%, and more preferably 100% to 250%.

[0047] In yet another embodiment, the tensile modulus (ISO 527-2) of the polyolefin composition of the present invention is at least 800 MPa, preferably at least 850 MPa, more preferably at least 870 MPa, particularly in the range of 800 MPa to 1500 MPa, and even more particularly in the range of 850 MPa to 1000 MPa.

[0048] Furthermore, the tensile strength of the composition is preferably at least 10 MPa, more preferably at least 15 MPa, more preferably at least 16 MPa, even more preferably at least 17 MPa, particularly in the range of 10 MPa to 25 MPa, and even more particularly in the range of 15 MPa to 20 MPa.

[0049] In another embodiment, the puncture energy (ISO 6603-2, 23°C) of the polyolefin composition of the present invention is at least 25.0 J, preferably at least 30.0 J, more preferably at least 32.0 J, particularly in the range of 25.0 J to 50.0 J, more particularly in the range of 30.0 J to 40.0 J, and even more particularly in the range of 32.0 J to 37.0 J.

[0050] In a preferred embodiment, the polyolefin composition of the present invention may have one or more of the following properties, preferably all of them:

[0051] - Impact strength (ISO 179, Charpy 1eA + 23℃) at 30.0 kJ / m 2 Up to 60.0 kJ / m 2 Within that range, and more specifically at 35.0 kJ / m 2 Up to 55.0 kJ / m 2Within that range, and even more specifically at 40.0 kJ / m 2 Up to 55.0 kJ / m 2 Within the range;

[0052] - The melt flow rate MFR2 (230°C, 2.16 kg, measured according to ISO 1133-1) is in the range of 15.0 g / 10 min to 30.0 g / 10 min, preferably 16.0 g / 10 min to 25.0 g / 10 min, more preferably 17.0 g / 10 min to 20.0 g / 10 min;

[0053] - Puncture energy (ISO 6603-2, 23°C) is in the range of 25.0 J to 50.0 J, more particularly in the range of 30.0 J to 40.0 J, and even more particularly in the range of 32.0 J to 37.0 J;

[0054] - The tensile strain at break (ISO 527-2, 23°C) is in the range of 80% to 400%, preferably 90% to 300%, and more preferably 100% to 250%;

[0055] - Tensile modulus (ISO 527-2, 23°C) is in the range of 800 MPa to 1500 MPa, and more particularly in the range of 850 MPa to 1000 MPa.

[0056] Blends of recycled plastic materials

[0057] The case used Recycle Plastic material blends are obtained from recycled waste streams. The blends can be recycled post-consumer or post-industrial waste, such as from the automotive industry, or alternatively a combination of both. Particularly preferred is that the blends consist of recycled post-consumer and / or post-industrial waste.

[0058] In one aspect, the blend can be a polypropylene (PP) enriched material from recycled plastics, containing significantly more polypropylene than polyethylene. Polypropylene-rich recycled waste streams can be obtained, for example, from the automotive industry, particularly since some automotive parts, such as bumpers, are sources of fairly pure polypropylene material in the recycled stream, or through enhanced sorting. Rich PP recyclables can also be obtained from yellow bag feedstock when sorted accordingly. Rich PP material can be obtained through selective treatment, degassing, and filtration, and / or through separation based on type and color (e.g., NIR or Raman sorting and VIS sorting). It can also be obtained from household waste streams (i.e., products of household recycling), for example, from the "yellow bag" recycling systems operated by the "Green Dot" organization in some areas of Germany.

[0059] Preferably, the polypropylene-rich recyclable material is obtained from recycled waste using plastic recycling processes known in the art. Such PP-rich recyclables are commercially available from sources such as Corepla (the Italian Consortium for the collection, recovery, recycling of packaging plastic wastes), Resource Plastics Corp. (Brampton, Ontario), Kruschitz GmbH, Plastics and Recycling (Austria), Vogt Plastik GmbH (Germany), mtmPlastics GmbH (Germany), etc. Non-exhaustive examples of polypropylene-enriched recycled materials include: Dipolen® PP, Purpolen® PP (Mtm Plastics GmbH), MOPRYLENE PC B-420 White, MOPRYLENE PC B 440 (MorssinkhofPlastics, Netherlands), SYSTALEN PP-C24000; Systalen PP-C44000; Systalen PP-C14901, Systalen PP-C17900, Systalen PP-C2400, Systalen 13704 GR 015, Systalen 13404 GR014, Systalen PP-C14900 GR000 (Der Grüne Punkt, Germany), Vision (Veolia) PPC BC 2006HS, or PP MONO.

[0060] This invention is considered applicable to a wide range of recycled polypropylene materials or materials or compositions with a high content of recycled polypropylene. The polypropylene-rich recycled material can be in granular form.

[0061] As previously stated, the polyolefin composition according to the invention comprises a polymer blend as a blending compound, the polymer blend comprising polypropylene and polyethylene; wherein the weight ratio of polypropylene to polyethylene is from 14:6 to 49:1, and wherein the polymer blend is a recycled material.

[0062] In another preferred embodiment of the invention, the ratio of polypropylene to polyethylene is specified as 15:5 to 49:1, and more preferably 16:4 to 49:1. The weight ratio of polypropylene to polyethylene is preferably 17:3 to 49:1.

[0063] According to one embodiment, relative to the total weight of the composition of the blend, the recycled plastic material blend contains the following relative amounts of propylene-derived units: greater than 50% by weight, preferably greater than 53% by weight, more preferably greater than 60% by weight, more preferably greater than 70% by weight, more preferably greater than 75% by weight, more preferably greater than 80% by weight, even more preferably greater than 90% by weight, and even more preferably greater than 95% by weight.

[0064] In another preferred embodiment of the invention, the polypropylene content in the recycled material blend is in the range of 75% to 99% by weight, and preferably in the range of 83% to 95% by weight, based on the total weight of the recycled material blend. The polypropylene content in the blend can be determined by FTIR spectroscopy as described in the experimental section. More preferably, the polypropylene component of the recycled material blend contains more than 95% by weight, preferably 96% to 99.9% by weight, of isotactic polypropylene, and most preferably consists of isotactic polypropylene.

[0065] Furthermore, the blend may contain ethylene-derived units in the following relative amounts: less than 47% by weight, more preferably less than 40% by weight, more preferably less than 30% by weight, more preferably less than 20% by weight, and most preferably less than 10% by weight. The recycled blend preferably contains ethylene-derived units in the following amounts: 5.0% by weight to 17.5% by weight, more preferably 6.0% by weight to 15.0% by weight, and even more preferably 7.5% by weight to 13.0% by weight. Typically, the relative amount of ethylene-derived units is greater than 5% by weight relative to the total weight of the blend. It should be understood that the ethylene present is preferably ethylene derived from polyethylene and copolymers containing ethylene.

[0066] In another preferred embodiment of the invention, based on the total weight of the recycled blend, the polyethylene content in the blend ranges from 1% to 25% by weight, preferably from 5% to 20% by weight, and more preferably from 7% to 17% by weight. The polyethylene content in the recycled blend can be determined by CRYSTEX as described in the experimental section. More preferably, the component consists of polyethylene and a copolymer containing ethylene.

[0067] The recycled plastic blends were appropriately characterized using CRYSTEX QC analysis. In CRYSTEX QC analysis, crystalline fractions (CF) and soluble fractions (SF) were obtained, and the crystalline fractions (CF) and soluble fractions (SF) could be quantified and analyzed regarding monomer and comonomer content and intrinsic viscosity (iV).

[0068] In one embodiment, the ethylene C2 content (as determined by CRYSTEX analysis) of the recycled material in the mixed plastic polypropylene blend is in the range of 5% to 20% by weight, more preferably 5% to 15% by weight, and even more preferably 11% to 13% by weight. Recycled propylene with a C2 content of less than 13% by weight is preferred.

[0069] In CRYSTEX analysis, blends of recycled plastic materials exhibited the following characteristics:

[0070] - The content of the crystal fraction (CF), as determined by CRYSTEX analysis, is in the range of 80.0 wt% to 96.0 wt%, preferably in the range of 82.5 wt% to 95.5 wt%, and more preferably in the range of 85.0 wt% to 95.0 wt%.

[0071] - The soluble fraction (SF) content, as determined by CRYSTEX QC analysis, is in the range of 4.0 wt% to 20.0 wt%, preferably in the range of 4.5 wt% to 17.5 wt%, and more preferably in the range of 5.0 wt% to 15.0 wt%.

[0072] The crystal fraction (CF) has one or more of the following characteristics, preferably all of them:

[0073] - such as by quantitative 13 The ethylene content (C2(CF)) determined by C-NMR-calibrated FT-IR spectra is in the range of 2.5 wt% to 20.0 wt%, preferably in the range of 3.5 wt% to 18.0 wt%, more preferably in the range of 5.0 wt% to 15.0 wt%; and / or

[0074] - The intrinsic viscosity (iV(CF)) in decahydronaphthalene, measured at 135°C according to DIN ISO 1628 / 1, is less than 2.5 dl / g, preferably in the range of 1.1 dl / g to 2.5 dl / g, more preferably in the range of 1.2 dl / g to 2.5 dl / g, and even more preferably in the range of 1.4 dl / g to 2.0 dl / g.

[0075] The soluble fraction (SF) has one or more of the following properties, preferably all of them:

[0076] - such as by quantitative 13 The ethylene content (C2(SF)) determined by FT-IR spectra calibrated by C-NMR spectroscopy is preferably in the range of 20.0 wt% to 55.0 wt%, more preferably in the range of 22.0 wt% to 50.0 wt%, and even more preferably in the range of 24.0 wt% to 45.0 wt%; and / or

[0077] - The intrinsic viscosity (iV(SF)) in decahydronaphthalene, measured at 135°C according to DIN ISO 1628 / 1, is in the range of 0.9 dl / g to 2.3 dl / g, preferably in the range of 1.0 dl / g to 2.2 dl / g, more preferably in the range of 1.1 dl / g to 2.1 dl / g, for example in the range of 1.8 dl / g to 2.1 dl / g.

[0078] The polyethylene fraction of the recycled material may include recycled high-density polyethylene (rHDPE), recycled medium-density polyethylene (rMDPE), recycled low-density polyethylene (rLDPE), linear low-density polyethylene (LLDPE), and mixtures thereof. In one particular embodiment, the recycled material has an average density greater than 0.8 g / cm³. 3 Preferably greater than 0.9 g / cm 3 The optimal value is greater than 0.91 g / cm³. 3 High-density PE.

[0079] Another preferred embodiment of the invention specifies that, based on the total weight of the recycled blend, the recycled blend contains less than 5% by weight, preferably less than 3% by weight, and more preferably 0.01% by weight to 2% by weight of a thermoplastic polymer different from polypropylene and polyethylene, more preferably less than 4.0% by weight of PA 6 and less than 5% by weight of polystyrene, and even more preferably, the blend contains 0.5% by weight to 3% by weight of polystyrene.

[0080] According to another preferred embodiment of the invention, the recycled material blend contains less than 5% by weight, preferably less than 4% by weight, and more preferably 0.01% by weight to 4% by weight of talc, based on the total weight of the recycled material blend.

[0081] In another preferred embodiment of the invention, the recycled blend contains less than 4% by weight, preferably less than 3% by weight, and more preferably 0.01% to 2% by weight of chalk, based on the total weight of the recycled blend.

[0082] According to another preferred embodiment of the invention, the recycled material blend contains less than 1% by weight, preferably less than 0.5% by weight, and more preferably 0.01% by weight to 1% by weight of paper, based on the total weight of the recycled material blend.

[0083] Another preferred embodiment of the invention specifies that, based on the total weight of the recycled material blend, the recycled material blend contains less than 1% by weight, preferably less than 0.5% by weight, and more preferably 0.01% by weight to 1% by weight of wood.

[0084] In another preferred embodiment of the invention, the recycled blend contains less than 1% by weight, preferably less than 0.5% by weight, and more preferably 0.01% by weight to 1% by weight of metal, based on the total weight of the recycled blend.

[0085] According to the present invention, the limonene content of the recycled blend, as determined by solid-phase microextraction (HS-SPME-GC-MS), is from 0.1 ppm to 100 ppm, more preferably from 1 ppm to 50 ppm, and most preferably from 2 ppm to 35 ppm. Limonene is conventionally found in recycled polyolefin materials and originates from packaging applications in the fields of cosmetics, detergents, shampoos, and similar products. Therefore, when the recycled blend contains materials derived from such a stream of household waste, the recycled blend contains limonene.

[0086] Fatty acid content is another indicator of the recovery source of the recycled material blend. However, in some cases, due to special treatments during the recovery process, the fatty acid content may be below the detection limit. According to the present invention, the fatty acid content of the recycled material blend, as determined by solid-phase microextraction (HS-SPME-GC-MS), is preferably 1 ppm to 200 ppm, more preferably 1 ppm to 150 ppm, more preferably 2 ppm to 100 ppm, and most preferably 3 ppm to 80 ppm.

[0087] In a preferred aspect, the recycled blend (i) contains less than 5% by weight, preferably less than 1.5% by weight, of polystyrene; and / or (ii) contains less than 3.5% by weight, preferably less than 1% by weight, of talc; and / or (iii) contains less than 1.0% by weight, preferably less than 0.5% by weight, of polyamide.

[0088] Due to the recycled source, the blend may also contain organic fillers, and / or inorganic fillers, and / or additives in an amount of up to 10% by weight, preferably 3% by weight, relative to the weight of the blend.

[0089] Therefore, in one embodiment of the polyolefin composition of the present invention, the recycled plastic material blend comprises:

[0090] A-1) Polypropylene content of 50% to 99% by weight,

[0091] A-2) Polyethylene content of 1% to 40% by weight,

[0092] A-3) 0% to 5.0% by weight of polystyrene and / or copolymers such as ABS,

[0093] A-4) 0% to 3.0% by weight of stabilizer.

[0094] A-5) 0% to 4.0% by weight of polyamide-6,

[0095] A-6) 0% to 3.0% by weight of talc,

[0096] A-7) 0% to 3.0% by weight chalk,

[0097] A-8) Paper from 0% to 1.0% by weight,

[0098] A-9) 0% to 1.0% by weight of timber,

[0099] A-10) 0% to 0.5% by weight of metals,

[0100] A-11) such as limonene at concentrations of 0.1 ppm to 100 ppm as determined by solid-phase microextraction (HS-SPME-GC-MS), and

[0101] A-12) Total fatty acid content from 0 ppm to 200 ppm, as determined by solid-phase microextraction (HS-SPME-GC-MS).

[0102] All quantities are given relative to the total weight of the recycled blend.

[0103] As stated above, based on the total weight of the recycled material blend, the recycled material blend may contain one or more additional components selected from the following:

[0104] A-4) Up to 3.0% by weight of stabilizer, preferably up to 2.0% by weight of stabilizer.

[0105] A-5) up to 4.0% by weight of polyamide-6, preferably up to 2.0% by weight of polyamide-6.

[0106] A-6) Up to 3.0% by weight of talc, preferably up to 1.0% by weight of talc.

[0107] A-7) up to 3.0% by weight of chalk, preferably up to 1.0% by weight of chalk.

[0108] A-8) Up to 1.0% by weight of paper, preferably up to 0.5% by weight of paper.

[0109] A-9) up to 1.0% by weight of timber, preferably up to 0.5% by weight of timber, and

[0110] A-10) up to 0.5% by weight of metal, preferably up to 0.1% by weight of metal.

[0111] In one embodiment, the recycled plastic material blend comprises polypropylene and polyethylene, and its melt flow rate MFR2 (230°C, 2.16 kg, measured according to ISO 1133) is at least 5.0 g / 10 min, preferably at least 10.0 g / 10 min, more preferably at least 15.0 g / 10 min, particularly in the range of 5.0 g / 10 min to 70.0 g / 10 min, preferably 8.0 g / 10 min to 60.0 g / 10 min, more preferably 10.0 g / 10 min to 50.0 g / 10 min.

[0112] According to one embodiment, the melt flow rate MFR2 (ISO 1133, 230°C, 2.16 kg) of the recycled plastic material can be in the range of 15 g / 10 min to 50 g / 10 min, and preferably in the range of 18 g / 10 min to 36 g / 10 min.

[0113] According to another embodiment, the melt flow rate MFR2 (ISO 1133, 230°C, 2.16 kg) of the recycled plastic material can be in the range of 5 g / 10 min to 20 g / 10 min, and preferably in the range of 10 g / 10 min to 15 g / 10 min.

[0114] In another preferred embodiment of the invention, the Charpy notched impact strength of the recycled blend, measured at 23°C according to ISO 179-1eA, is greater than 3.0 kJ / m. 2 Preferably at 4.0 kJ / m 2 Up to 8.0 kJ / m 2 Within the range, and more preferably within 5.0 kJ / m 2 Up to 6.5 kJ / m 2 Within the range.

[0115] Another preferred embodiment of the invention specifies that the tensile modulus of the recycled blend, measured according to ISO 527-2, is in the range of 800 MPa to 1500 MPa, preferably in the range of 1100 MPa to 1400 MPa, and more preferably in the range of 1200 MPa to 1300 MPa.

[0116] In one embodiment, the recycled blend preferably has one or more of the following characteristics, preferably all of them:

[0117] - The melt flow rate MFR2 (230°C, 2.16 kg, ISO 1133) is 6.0 g / 10 min to 40 g / 10 min, preferably 8.0 g / 10 min to 40 g / 10 min, more preferably 9.0 g / 10 min to 36 g / 10 min; and / or

[0118] - The polydispersity index (PI) is 2.0 Pa. -1 Up to 5.0 Pa -1 2.2 Pa is preferred. -1 Up to 4.5 Pa -1 More preferably 2.5Pa -1 Up to 4.0 Pa -1 ; and / or

[0119] - Complex viscosity η at 0.05 radians / second 0.05 For 1000 Up to 5000 1200 is preferred Up to 4500 , more preferably 1400 Up to 4000 ; and / or

[0120] - Complex viscosity η at 300 radians / second 300 100 Up to 500 150 is preferred Up to 400 , more preferably 175 Up to 300 , and / or

[0121] - Density is 905 kg / m³ 3 Up to 930 kg / m 3 910 kg / m 3 Up to 925 kg / m 3 More preferably 913 kg / m 3 Up to 922 kg / m 3 ; and / or

[0122] - Limonene content, as determined by solid-phase microextraction (HS-SPME-GC-MS): 0.1 ppm to 50 ppm; and / or

[0123] - Tensile modulus of 1000 MPa to 1500 MPa, preferably 1100 MPa to 1400 MPa; and / or

[0124] The Charpy notched impact strength (CNIS at 23℃) is 3.0 kJ / m. 2 Up to 7.5 kJ / m 2 4.0 kJ / m 2 Up to 7.0 kJ / m 2 .

[0125] Preferred recycled blends used in the polyolefin compositions of the present invention will now be described in more detail.

[0126] Blend A1

[0127] The preferred recycled blend A1 is available from mtm Plastics GmbH.

[0128] Blend A1 is a material based on post-consumer recycled polypropylene with the following properties: 915 kg / m³ 3 Density (determined according to DIN EN ISO 1183), melt flow rate of 20 g / 10 min to 22 g / 10 min (determined according to DIN EN ISO 1133, at 230 °C / 2.16 kg), %, tensile modulus greater than 1100 MPa (determined according to DIN EN ISO 527, at 1 mm / min), yield stress greater than 25 MPa (determined according to DIN EN ISO 527, at 50 mm / min), and tensile strain at break greater than 13% (determined according to DIN EN ISO 527, at 50 mm / min).

[0129] The recycled blend A1, as if through... 13 The C2(SF) content of the soluble fraction determined by quantitative FT-IR spectroscopy calibrated by C-NMR spectroscopy is in the range of 20 wt% to 40 wt%, preferably 25 wt% to 38 wt%, more preferably 26 wt% to 35 wt%, for example, 30 wt% to 33 wt%.

[0130] The recycled blend A1, as if through... 13 The C2(CF) content of the crystal fraction determined by quantitative FT-IR spectroscopy calibrated by C-NMR spectroscopy is in the range of 3 wt% to 20 wt%, preferably 5 wt% to 15 wt%, more preferably 6 wt% to 12 wt%, for example 8 wt% to 11 wt%.

[0131] Specifically, blend A1 has a concentration of less than 1 mg / m³. 3 The following parameters were considered: limonene content, PP / PE ratio of 91 / 6, total C2 content of 8% to 13% by weight, C2 (CF) content of 7% to 12% by weight, C2 (SF) content of 27% to 33% by weight, IV (CF) content of 1.52 dl / g, IV (SF) content of 1.94 dl / g, iV (iV) content of 1.58 dl / g (overall blend), MFR2 of 21 g / 10 min to 22 g / 10 min, tensile modulus of 1200 MPa to 1300 MPa, and 5 KJ / m². 2 Up to 6 KJ / m 2Notched impact strength (Charles test 23℃);

[0132] Blend A2

[0133] The preferred recycled blend A2 is also available from mtm Plastics GmbH.

[0134] Blend A2 is a material based on post-consumer recycled polypropylene with the following properties: 915 kg / m³ 3 The density (determined according to DIN EN ISO 1183), melt flow rate of 11 g / 10 min to 13 g / 10 min (determined according to DIN EN ISO 1133, at 230 °C / 2.16 kg), tensile modulus greater than 1100 MPa (determined according to DIN EN ISO 527, at 1 mm / min), yield stress greater than 28 MPa (determined according to DIN EN ISO 527, at 50 mm / min), and tensile strain at break greater than 47% (determined according to DIN EN ISO 527, at 50 mm / min).

[0135] The recycled blend A2, as if through... 13 The C2(SF) content of the soluble fraction determined by quantitative FT-IR spectroscopy calibrated by C-NMR spectroscopy is in the range of 25 wt% to 45 wt%, preferably 27 wt% to 40 wt%, and more preferably 28 wt% to 36 wt%.

[0136] The recycled blend A2, as if through... 13 The C2(CF) content of the crystal fraction determined by quantitative FT-IR spectroscopy calibrated by C-NMR spectroscopy is in the range of 4 wt% to 20 wt%, preferably 5 wt% to 16 wt%, and more preferably 8 wt% to 14 wt%.

[0137] Specifically, blend A2 has a concentration of less than 1 mg / m³. 3 The following parameters were measured: limonene content, PP / PE ratio of 92 / 8, total C2 content of 8% to 15% by weight, C2 (CF) content of 8% to 14% by weight, C2 (SF) content of 28% to 36% by weight, IV (CF) content of 1.71 dl / g, IV (SF) content of 1.26 dl / g, iV (total blend) content of 1.71 dl / g, MFR2 of 11 g / 10 min to 13 g / 10 min, tensile modulus of 1200 MPa to 1300 MPa, and 5 KJ / m². 2 Up to 6 KJ / m 2 Notched impact strength (Charles test 23℃);

[0138] elastomer

[0139] As described above, the polyolefin composition according to the present invention comprises at least one C2 / C4 and / or C2 / C8 elastomer as a compatibilizer.

[0140] C2 / C4 plastomers are plastomer copolymers containing ethylene monomers and butene comonomers, exhibiting both elastomer and plastic properties. C2C8 plastomers are plastomer copolymers containing ethylene monomers and 1-octene comonomers, also exhibiting both elastomer and plastic properties.

[0141] Therefore, it is preferred that butene comonomer or 1-octene comonomer be incorporated into the C2 / C4 or C2C8 plastic body in a random form, so that the C2 / C4 or C2C8 plastic body is a random copolymer of ethylene and butene or ethylene and 1-octene.

[0142] Random copolymers are different from block copolymers that have ethylene-rich blocks and comonomer-rich blocks (butene-rich or 1-octene-rich blocks) in the polymer chain.

[0143] The elastomer is preferably a native polymer that is incorporated into the other components of the polypropylene-polyethylene composition of the present invention. Residual C2 / C4 or C2C8 plasmons that may be present in the blended plastics (A) are not classified under compatibilizer (B).

[0144] In one embodiment, the MFR2 (ISO 1133, 2.16 kg load at 190°C) of at least one C2 / C4 and / or C2 / C8 elastomer is equal to or less than 20 g / 10 min; preferably equal to or less than 10 g / 10 min; more preferably equal to or less than 5 g / 10 min, for example in the range of 0.1 g / 10 min to 30.0 g / 10 min, preferably 0.2 g / 10 min to 20.0 g / 10 min, more preferably 0.3 g / 10 min to 10.0 g / 10 min.

[0145] In another embodiment, the density (ISO 1183) of at least one C2 / C4 and / or C2 / C8 elastomer is equal to or less than 900 kg / m³. 3 Preferably equal to or lower than 890 kg / m 3 More preferably equal to or less than 880 kg / m 3 Even more preferred is 870 kg / m 3 More preferably equal to or lower than 860 kg / m 3 For example, at 500 kg / m 3 Up to 900 kg / m 3 Within this range, especially at 660 kg / m 3Up to 890 kg / m 3 Within that range, and more specifically at 700 kg / m 3 Up to 880 kg / m 3 Within the range.

[0146] More specifically, the melt flow rate (MFR2) of the C2 / C4 plasmid, as determined according to ISO 1133 at 190°C and 2.16 kg, is in the range of 0.1 g / 10 min to 10.0 g / 10 min, preferably 0.2 g / 10 min to 8.0 g / 10 min, and more preferably 0.3 g / 10 min to 5.0 g / 10 min.

[0147] Furthermore, the density of C2 / C4 plasmon, as determined according to ISO 1183, is 800 kg / m³. 3 Up to 900 kg / m 3 850kg / m 3 Up to 890 kg / m 3 More preferably 860 kg / m 3 Up to 880 kg / m 3 .

[0148] Furthermore, the glass transition temperature Tg of the C2 / C4 plasmon, determined by DSC according to ISO 11357, is preferably -30°C to -70°C, more preferably -40°C to -60°C, and even more preferably -50°C to -60°C.

[0149] The melt flow rate (MFR2) of the C2 / C8 plasmid, as determined according to ISO 1133 at 190°C and 2.16 kg, is in the range of 0.1 g / 10 min to 15.0 g / 10 min, preferably 0.2 g / 10 min to 12.0 g / 10 min, and more preferably 0.3 g / 10 min to 10.0 g / 10 min.

[0150] Furthermore, the density of C2 / C8 plasmon, as determined according to ISO 1183, is 860 kg / m³. 3 Up to 885 kg / m 3 Optimal weight is 862 kg / m³ 3 Up to 884 kg / m 3 More preferably 865 kg / m 3 Up to 883 kg / m 3 .

[0151] Furthermore, the melting temperature Tm of the C2 / C8 plasmon, as determined by DSC according to ISO 11357, is below 85°C, preferably 40°C to 74°C, and more preferably 45°C to 73°C.

[0152] Furthermore, the glass transition temperature Tg of the C2 / C8 plasmon, determined by DSC according to ISO 11357, is preferably -40°C to -75°C, more preferably -45°C to -70°C, and even more preferably -50°C to -65°C.

[0153] C2 / C4 and C2C8 plastomers are typically polymerized in solution in the presence of metallocene catalysts. Suitable metallocene catalysts and polymerization conditions for the production of C2C8 plastomers have been well established in the art.

[0154] Suitable C2 / C4 or C2C8 plastomers as compatibilizers (B) are also available, for example, from Borealis AG under the trade name Queo®, from DOW Chemical Corp (USA) under the trade name Engage®, or from Exxon Mobil (USA) under the trade name Exact®.

[0155] virgin polypropylene homopolymer

[0156] As previously stated, the polyolefin composition of the present invention comprises 4% to 8% by weight, more preferably 5% to 6% by weight (based on the total weight of the polyolefin composition) of a polypropylene homopolymer with an MFR2 (ISO 1133, 2.16 kg load at 230°C) of at least 800 g / 10 min.

[0157] In one embodiment, the MFR2 (ISO 1133, 2.16 kg load at 230°C) of at least one polypropylene homopolymer is at least 1000 g / 10 min, preferably at least 1200 g / 10 min.

[0158] The polypropylene homopolymer used as the primary polymer in the polyolefin composition of the present invention can be at least one polypropylene homopolymer (PPH-1) with a melt flow rate MFR2 (230°C, 2.16 kg, measured according to ISO 1133) in the range of 1000 g / 10 min to 1500 g / 10 min, preferably 1100 g / 10 min to 1300 g / 10 min, more preferably 1200 g / 10 min to 1250 g / 10 min.

[0159] The polypropylene homopolymer (PPH-1) has a melt temperature of at least 140°C, preferably at least 150°C, and more preferably in the range of 150°C to 160°C, for example, 158°C (according to ISO 11357-3); and a melt density of at least 700 kg / m³. 3 Preferably at least 800 kg / m 3 Preferably at 700 kg / m 3 Up to 1200 kg / m 3Within the range, more preferably within 800 kg / m 3 Up to 1000 kg / m 3 For example, 850 kg / m 3 Up to 950 kg / m 3 Density within the range (according to ISO 1183-1).

[0160] It should be understood that the polyolefin compositions of the present invention may contain not only one, but two or more, polypropylene virgin homopolymers with different melt flow rates. This allows for adjustment of the melt flow rate of the final polyolefin composition.

[0161] additive

[0162] As previously stated, the polyolefin compositions of the present invention may contain additives.

[0163] Typically, based on the weight of the total composition, the amount of these additives ranges from 0% to 5.0% by weight, preferably from 0.01% to 3.0% by weight, and more preferably from 0.01% to 2.0% by weight.

[0164] Examples of additives used in compositions include pigments or dyes (e.g., carbon black), stabilizers (antioxidants), acid stabilizers and / or UV stabilizers, antistatic agents, nucleating agents, and utilization agents (e.g., processing aids). Preferred additives are carbon black, at least one antioxidant, and / or at least one UV stabilizer.

[0165] Examples of commonly used antioxidants in this field are sterically hindered phenols (e.g., CAS No. 6683-19-8, also known as Irganox 1010 FF). TM Sold by BASF), phosphorus-based antioxidants (e.g., CAS No. 31570-04-4, also known as Hostanox PAR 24 (FF)). TM Sold by Clariant or by BASF as Irgafos 168 (FF)™, sulfur-based antioxidants (e.g., CAS No. 693-36-7, as Irganox PS-802 FL) TM These antioxidants may be sold by BASF, nitrogen-based antioxidants (e.g., 4,4'-bis(1,1'-dimethylbenzyl)diphenylamine), or antioxidant blends. Preferred antioxidants may be tris(2,4-di-tert-butylphenyl) phosphite and / or octadecyl 3-(3',5'-di-tert-butyl-4-hydroxyphenyl) propionate.

[0166] Antiacids are also well known in the art. Examples include calcium stearate, sodium stearate, zinc stearate, magnesium and zinc oxides, synthetic hydrotalcites (e.g., SHT, CAS No. 11097-59-9), lactates and lactyl salts, as well as calcium stearate (CAS No. 1592-23-0) and zinc stearate (CAS No. 557-05-1).

[0167] Common anti-blocking agents are natural silica, such as diatomaceous earth (e.g., CAS No. 60676-86-0 (SuperfFloss)). TM ), CAS number 60676-86-0 (SuperFloss E TM ), or CAS number 60676-86-0 (Celite499) TM Synthetic silica (e.g., CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 7631-86-9, CAS No. 112926-00-8, CAS No. 7631-86-9, or CAS No. 7631-86-9), silicates (e.g., aluminum silicate (kaolin) CAS No. 1318-74-7, Sodium aluminum silicate CAS No. 1344-00-9, Calcined kaolin CAS No. 92704-41-1, Aluminum silicate CAS No. 1327-36-2, or Calcium silicate CAS No. 1344-95-2, Synthetic zeolites (e.g., Sodium aluminosilicate calcium hydrate CAS No. 1344-01-0, CAS No. 1344-01-0, or Sodium aluminosilicate calcium hydrate CAS No. 1344-01-0).

[0168] UV stabilizers are, for example, bis-(2,2,6,6-tetramethyl-4-piperidinyl)-sebate (CAS No. 52829-07-9, Tinuvin 770); 2-hydroxy-4-n-octyloxybenzophenone (CAS No. 1843-05-6, Chimassorb 81). Preferred UV stabilizers can be low molecular weight UV stabilizers and / or high molecular weight UV stabilizers, such as hexadecyl-3,5-di-tert-butyl-4-hydroxybenzoate; mixtures of esters of 2,2,6,6-tetramethyl-4-piperidinol and higher fatty acids (mainly stearic acid); and / or poly((6-morpholino-s-triazine-2,4-diyl)(1,2,2,6,6-pentamethyl-4-piperidinyl)imino)hexamethylene(1,2,2,6,6-pentamethyl-4-piperidinyl)imino).

[0169] α-nucleating agents such as sodium benzoate (CAS No. 532-32-1); 1,3:2,4-bis(3,4-dimethylbenzyl)sorbitol (CAS 135861-56-2, Millad 3988).

[0170] Suitable antistatic agents are, for example, glycerides (CAS No. 97593-29-8), ethoxylated amines (CAS No. 71786-60-2 or 61791-31-9), or ethoxylated amides (CAS No. 204-393-1).

[0171] These additives are typically added to each individual component of the polymer in amounts ranging from 100 ppm to 2,000 ppm.

[0172] It should be understood that the polyolefin composition as defined herein can be obtained by a method comprising the following steps:

[0173] - The following mixture is provided: a) a blend of polypropylene and polyethylene in a ratio of 14:6 to 49:1, comprising 60% to 85% (based on the total weight of the polyolefin composition); b) at least one C2 / C4 and / or C2 / C8 elastomer as a compatibilizer, comprising 10% to 30% (based on the total weight of the polyolefin composition) of MFR2 (ISO 1133, 2.16 kg load at 190°C) equal to or less than 30 g / min; c) a polypropylene homopolymer comprising 3% to 10% (based on the total weight of the polyolefin composition) of MFR2 (ISO 1133, 2.16 kg load at 230°C) at least 1000 g / 10 min; and d) optional additional additives, wherein the sum of all components always totals 100% by weight.

[0174] - To melt the mixture in the extruder, and

[0175] - Optionally, the obtained polyolefin composition may be granulated.

[0176] The present invention also relates to articles comprising the polyolefin composition according to the present invention.

[0177] The polyolefin compositions according to the invention can be used in a wide range of applications, such as for the manufacture of structural products, pumps, fans, appliances, automotive parts, pipes and fittings, packaging, covers and closures, especially household appliances.

[0178] Experimental Section

[0179] The following examples illustrate certain aspects and embodiments of the invention as described in the claims. However, those skilled in the art will understand that the following description is merely illustrative and should not be construed as limiting the invention in any way.

[0180] Test methods

[0181] Unless otherwise specified, the following terms and determination methods apply to the above general description of the invention and the following embodiments.

[0182] The crystalline and soluble fractions and their respective characteristics (IV and ethylene content) were determined using Crystex.

[0183] The crystalline fraction (CF) and soluble fraction (SF) of polypropylene (PP) compositions, as well as the comonomer content and intrinsic viscosity of each fraction, were analyzed using the Crystex (crystallization extraction) method. Potential instruments that can be used are the Crystex QC or Crystex 42 (Polymer Char; Valencia, Spain). Detailed information on this technique and method can be found in the literature (Ljiljana Jeremic, Andreas Albrecht, Martina Sandholzer & Markus Gahleitner (2020): Rapid characterization of high-impact ethylene-propylene copolymer composition by crystallization extraction separation: comparability to standard separation methods, International Journal of Polymer Analysis and Characterization, 25:8, 581-596).

[0184] The crystalline and amorphous fractions were separated by temperature cycling: dissolution at 160 °C, crystallization at 40 °C, and redissolution in 1,2,4-trichlorobenzene at 160 °C. SF and CF were quantified, and the ethylene content (C2) was determined using an integrated infrared detector (IR4). The intrinsic viscosity (IV) was determined using an online 2-capillary viscometer.

[0185] The IR4 detector measures two different wavelengths (CH3 stretching vibrations at approximately 2960 cm⁻¹). -1 (centered) and CH stretching vibration (2700 cm) -1 Up to 3000 cm -1A multi-wavelength detector at the IR absorbance at () was used to determine the concentration and ethylene content in the ethylene-propylene copolymer. The IR4 detector was calibrated with a series of eight EP copolymers with known ethylene contents ranging from 2 wt% to 69 wt% (determined by 13C-NMR) and individual concentrations ranging from 2 mg / ml to 13 mg / ml. The following calibration equation was applied to simultaneously obtain both concentration and ethylene content characteristics for the various polymer concentrations expected during Crystex analysis:

[0186]

[0187]

[0188] The constants a to f in equation 1 and the constants a to e in equation 2 are determined using least squares regression analysis.

[0189] Use the following relationship to convert CH3 / 1000C to ethylene content in weight percent:

[0190]

[0191] XS calibration correlates the amounts of soluble fraction (SF) and crystalline fraction (CF) with the amounts of "xylene cold soluble" (XCS) and xylene cold insoluble (XCI) fractions, respectively, as determined by the standard gravimetric method according to ISO 16152. XS calibration is performed by testing various EP copolymers with XS contents ranging from 2% to 31% wt%. Linear calibration curves are used.

[0192] The intrinsic viscosity (IV) of the parent EP copolymer and its soluble and crystalline fractions was determined using an online 2-capillary viscometer and correlated with the corresponding IV determined by a standard method in decahydronaphthalene according to ISO 1628-3. Calibration was performed using various EP copolymers and PP polymers with IVs ranging from 2 dL / g to 4 dL / g. The determined calibration curves were linear.

[0193] Weigh the sample to be analyzed at a concentration of 10 mg / ml to 20 mg / ml.

[0194] After filling vials with 1,2,4-TCB containing 250 mg / L 2,6-tert-butyl-4-cresol (BHT) as an antioxidant, the sample was dissolved at 170°C until complete dissolution was achieved under constant stirring or gentle shaking. To prevent sample degradation, the polymer solution was covered with a nitrogen atmosphere during dissolution.

[0195] For PP compositions containing inorganic fillers, pigments, or any other non-TCB-soluble polymeric substances, these need to be removed. This can be accomplished by thermal filtration prior to injection.

[0196] A defined volume of polymer solution is injected into a column packed with an inert support, where crystallization of the sample and separation of the soluble and crystalline fractions occur. This process is repeated twice. During the first injection, the entire sample is measured at high temperature to determine the IV [dl / g] and C2 [wt%] of the PP composition. During the second injection, the soluble fraction (at low temperature) and the crystalline fraction (at high temperature) are measured under crystallization cycles (wt% SF, wt% C2, IV).

[0197] Determine the content of isotactic polypropylene (iPP), polystyrene (PS), ethylene, and polyamide-6 in blend A).

[0198] Calibration standards were prepared by blending iPP and HDPE to form calibration curves. The thickness of the calibration standard film was 300 μm. To quantify the contents of iPP, PS, and PA6 in the samples, quantitative IR spectra were recorded in solid state using a Bruker Vertex 70 FTIR spectrometer. Spectra were recorded for 25 mm × 25 mm square films with a thickness of 50 μm to 100 μm prepared by compression molding at 190 °C and 4 mPa to 6 mPa. Standard transmission FTIR spectroscopy was used at 4000 cm⁻¹. -1 Up to 400 cm -1 Spectral range, 6 mm aperture, 2 cm -1 Spectral resolution, 16 background scans, 16 spectral scans, 32 interferogram zero fill factor and Norton Beer strong apodization.

[0199] iPP measured at 1167 cm -1 The absorption of the band at the location was measured, and the iPP content was quantified according to the calibration curve (absorption / thickness (in cm) relative to iPP content (in weight %)).

[0200] Measured 1601 cm -1 (PS) and 3300 cm -1 The absorption at (PA6) was measured, and the PS and PA6 contents were quantified according to the calibration curve (absorption / thickness (in cm) relative to PS and PA contents (in wt%)). The ethylene content was obtained by subtracting the contents of iPP, PS, and PA6 from 100. The analysis was performed using a dual determination method.

[0201] Intrinsic viscosity

[0202] Intrinsic viscosity (iV) was measured in decahydronaphthalene at 135°C according to DIN ISO 1628 / 1 (October 1999).

[0203] melt flow rate

[0204] Melt flow rate (MFR) is determined according to ISO 1133 and expressed in g / 10 min. MFR is an indicator of the polymer's flowability and therefore its processability. A higher melt flow rate generally corresponds to a lower polymer viscosity. The MFR2 for polypropylene was determined at a temperature of 230 °C and a load of 2.16 kg.

[0205] density:

[0206] Density was measured according to ISO 1183-187. Sample preparation was performed by compression molding according to ISO 1872-2:2007.

[0207] Xylene soluble fraction at room temperature (XCS, wt%): The amount of polymer soluble in xylene is determined at 25°C according to ISO 16152; 5th edition; 2005-07-01.

[0208] DSC analysis, melting temperature (T) m ) and heat of fusion (H f ), crystallization temperature (T) c ) and heat of crystallization (H c ): Samples ranging from 5 mg to 7 mg were measured using a TAInstrument Q200 differential scanning calorimeter (DSC). The DSC was operated according to ISO 11357 / Part 3 / Method C2 at a scan rate of 10 °C / min with heating / cooling / heating cycles over a temperature range of -30 °C to +225 °C. Crystallization temperature (T c ) and enthalpy of crystallization (H c The melting temperature (T) is determined by the cooling step, while the melting temperature (T) is determined by the cooling step. m ) and enthalpy of fusion (H m The value is determined by the second heating step.

[0209] The flexural modulus was determined according to ISO 178 Method A (three-point bending test) on an 80 mm × 10 mm × 4 mm specimen. A test speed of 2 mm / min and a span length 16 times the thickness were used, as per the standard. The test temperature was 23 ± 2 °C. All materials were injection molded according to ISO 19069-2 using a melt temperature of 230 °C, regardless of the material melt flow rate.

[0210] Notched impact strength (NIS)

[0211] Charpy notched impact strength (NIS) was measured according to ISO 179 1eA at +23°C or -20°C using an 80×10×4 mm gauge prepared according to ISO 19069-2. 3 For the injection molded rod test specimens, all materials were tested at a melting temperature of 230°C, and the melt flow rate of the materials was not considered.

[0212] Inorganic residues

[0213] Inorganic residues were quantified using a Perkin Elmer TGA 8000 according to DIN ISO 1172:1996. Approximately 10 to 20 mg of material was placed in a platinum dish. The temperature was equilibrated at 50°C for 10 minutes, then increased to 950°C under nitrogen at a heating rate of 20°C / min. Ash content was assessed as % by weight at 850°C.

[0214] Limonene detection

[0215] Limonene was determined based on a static headspace (HS) method. The analysis used an HS injector in combination with gas chromatography (GC) and mass spectrometry (MS) for screening purposes.

[0216] Samples were transported to the laboratory in sealed aluminum-coated polyethylene (PE) bags. Prior to analysis, the samples were cold-ground, and a fraction of 2,000 ± 0.100 g was weighed into 20 ml HS vials and tightly sealed. Each sample was determined twice.

[0217] HS / GC / MS parameters

[0218] • HS parameters (Agilent G1888 headspace sampler)

[0219] Vial equilibration time: 120 minutes (samples), 5 minutes (standards)

[0220] Oven temperature: 100℃ (samples), 200℃ (standards)

[0221] Ambient temperature: 110℃ (sample), 205℃ (standard)

[0222] Transmission line temperature: 120℃ (sample), 210℃ (standard)

[0223] low rock

[0224] • GC parameters (Agilent 7890A GC system)

[0225] Column: ZB-WAX 7HG-G007-22 (30 m × 250 µm × 1 µm)

[0226] Carrier gas: Helium 5.0

[0227] Flow rate: 2 ml / min

[0228] Flow split ratio: 5:1

[0229] GC oven program: 35℃ for 0.1 minutes

[0230] 10℃ / minute up to 250℃

[0231] 250℃ for 1 minute

[0232] • MS Specifications (Agilent 5975C Inert XL MSD)

[0233] Acquisition mode: Scan

[0234] Scan parameters:

[0235] Low quality: 20

[0236] High quality: 200

[0237] Threshold: 10

[0238] Software / Data Evaluation

[0239] MSD ChemStation E.02.02.1431

[0240] MassHunter GC / MS data acquisition B.07.05.2479

[0241] AMDIS GC / MS Analysis Version 2.71

[0242] NIST / EPA / NIH Mass Spectrometry Library (2011 Edition)

[0243] NIST Mass Spectrometry Search Program Version 2.0 g

[0244] AMDIS deconvolution parameters

[0245] Minimum matching factor: 80

[0246] Threshold: Low

[0247] Scanning direction: High to low

[0248] Data file format: Agilent file

[0249] Instrument type: Quadrupole

[0250] Component width: 20

[0251] Adjacent peak subtraction: two

[0252] Resolution: High

[0253] Sensitivity: Very high

[0254] Shape requirements: Medium

[0255] Solvent tailing: 91 m / z

[0256] Column bleed: 207 m / z

[0257] Minimum model peaks: 2

[0258] Minimum S / N: 10

[0259] Minimum confirmed peaks: 0.5

[0260] · MSD ChemStation integration parameters

[0261] Integrator: ChemStation

[0262] Initial area reject: 0

[0263] Initial peak width: 0.005

[0264] Shoulder detection: Off

[0265] Initial threshold: 10.5

[0266] In this study, the expression "below the limit of detection (<LOD)" describes a situation where the match factor is below 80 (AMDIS) or the signal-to-noise ratio of the peak in the sample run (Pk-pk S / N = corrected signal / Pk-pk noise, MSD ChemStation signal-to-noise ratio report) is below 3. The results only relate to the measured samples, the measurement time and the applied parameters.

[0267] standard solutions

[0268] For positive identification and comparison with the (minimum) odor detection threshold (ODT), a limonene standard was used.

[0269] For HS / GC / MS analysis, 5 µl of the corresponding standard was injected into a 20 ml HS vial, tightly sealed and measured.

[0270] Assuming complete evaporation of the reference material, the concentration c of limonene in the HS G was estimated as listed in Table 1 below.

[0271]

[0272] Data evaluation

[0273] The concentration c of the analyte in the HS GBy considering the mass m G and available HS volume V G To calculate (Equation 1).

[0274]

[0275] To estimate the concentration of the analyte in the HS above the polymer sample, a single-point calibration response factor Rf (Equation 2) is required. The peak area of ​​the analyte is obtained by integrating the extracted ion chromatogram (EIC). The corresponding target ions are listed in Table 1.

[0276]

[0277] Concentration of analyte in HS above polymer sample It is calculated by multiplying the response factor by the area of ​​the EIC peak of the sample (Equation 3).

[0278]

[0279] Furthermore, the odor relevance of the analytes in the HS above the polymer sample was estimated using the odor activity value (OAV). Therefore, the concentration of the analytes in the HS above the polymer sample was... Compare with the (lowest) odor detection threshold (ODT) found in the literature (Equation 4) [Van Gemert LJ, Odour Thresholds: Compilations of odor threshold values ​​in air, water and other media, Utrecht, Oliemans Punter & Partners BV, 2011]. Values ​​higher than 1 indicate that the analyte is odor-related at a given HS temperature.

[0280]

[0281] Considerations and limitations

[0282] It must be taken into account that some substances have an ODT below the detection limit (LOD) of this method. Therefore, components below the LOD may be missed, even though they are still relevant to the overall odor.

[0283] OAV is based on the assumption that the HS parameters are related to the measurement conditions determined by ODT to some extent. Of course, this is not entirely applicable, as a temperature setting of 100°C may not be chosen for such experiments and therefore has limited practical value. Nevertheless, this method can at least indicate the odor relevance of the defined labeled substance.

[0284] Tensile properties (uniaxial tensile test) according to ISO 527-2

[0285] Tensile properties (tensile modulus, tensile strength, tensile strain at strength, tensile stress at break, tensile strain at break) are determined according to ISO 527-2 Method B on a dog-bone mold according to ISO 1A ISO 527-2 or ISO 527-2 Method B. A test speed of 1 mm / min is used for tensile modulus, and 50 mm / min is used for all other properties, as per the standard. The test temperature is 23 ± 2 °C. Injection molding or compression molding is performed according to ISO 19069-2 (for PP).

[0286] Instrumental puncture of rigid plastics (ISO 6603- Part 2)

[0287] Maximum force, deflection at maximum force, energy required to reach maximum force, puncture deflection, and puncture energy were determined according to ISO 6603-2 in the instrument puncture impact behavior test. The specimens were injection-molded sheets according to ISO 19069-2 (for PP) and cut to dimensions of 60 mm × 60 mm × 2 mm. The test conditions used were: impact velocity of 4.4 m / s, 20 mm diameter lubricated impact head, at 23 ± 2 °C. The specimens were clamped with a 40 mm diameter support ring.

[0288] Different blends of recycled materials can be used. The blends used in the examples are characterized by the following properties:

[0289] Blend A1

[0290] A blend of recycled plastic materials, A1, was used, which has a density of 915 kg / m³. 3 Density (determined according to DIN EN ISO 1183), melt flow rate of 21 g / 10 min to 22 g / 10 min (determined according to DIN EN ISO 1133, 230℃ / 2.16kg), tensile modulus of 1200 MPa to 1300 MPa (determined according to DIN EN ISO 527, 1 mm / min), 5 kJ / m 2 Up to 6 KJ / m 2 Impact strength (Charles test 23°C), yield stress greater than 25 MPa (determined according to DIN EN ISO 527, 50 mm / min), and tensile strain at break greater than 13% (determined according to DIN EN ISO 527, 50 mm / min).

[0291] Specifically, blend A1 has a concentration of less than 1 mg / m³. 3The following parameters were considered: limonene content, PP / PE ratio of 91 / 6, total C2 content of 8% to 13% by weight, C2 (CF) content of 7% to 12% by weight, C2 (SF) content of 27% to 33% by weight, IV (CF) content of 1.52 dl / g, IV (SF) content of 0.94 dl / g, iV (overall blend) content of 1.58 dl / g, MFR2 of 21 g / 10 min to 22 g / 10 min, tensile modulus of 1200 MPa to 1300 MPa, and 5 kJ / m². 2 Up to 6 KJ / m 2 Notched impact strength (Charles test 23℃).

[0292] As the compatibilizer, the following commercially available ethylene-copoly-1-octene polymer (C2C8 polymer) or ethylene-copoly-1-butene (C2C4) is used as the plastic body P:

[0293] P-1 commercially available has 860 kg / m 3 The density and melt flow rate of MFR2 (190°C, ISO 1133) ethylene-co-butene polymer

[0294] P-2 commercially available has 860 kg / m 3 The density and melt flow rate of MFR2 (190°C, ISO 1133) of the ethylene-copolymer-1-octene have the following properties: MFR2 (190°C, ISO 1133).

[0295] P-3 commercially available has 868 kg / m 3 The ethylene-copolymer-1-octene has a density of 0.5 g / 10 min, a melt flow rate MFR2 (190 °C, ISO 1133), and a melt temperature Tm of 47 °C.

[0296] P-4 commercially available has 883 kg / m 3 The density and melt flow rate of MFR2 (190°C, ISO 1133) of the ethylene-copolymer-1-octene are as follows: MFR2 (190°C, ISO 1133).

[0297] The polypropylene homopolymer (PPH-1) used as the primary polymer in the polyolefin compositions of the present invention has a melt flow rate MFR2 of 1050 g / 10 min to 1350 g / 10 min (230 °C, 2.16 kg, measured according to ISO 1133), a melt temperature of 155 °C to 160 °C (according to ISO 11357-3), and 850 kg / m³. 3 Up to 950 kg / m 3 Density (according to ISO 1183-1).

[0298] The following additives are used: Antioxidants: AO1 (AO200GRA), AO2 (AO102GRA); Formulation agent: HC001A-B1 (polypropylene homopolymer).

[0299] Table 2 covers polyolefin compositions including the following:

[0300] - Comparative Example (CE1): Blend of recycled materials (Blend A1) and 20% by weight of plasmid P-4;

[0301] - Comparative Example (CE2): Blend of recycled materials (blend A1) and 20% by weight of plasmon P-1;

[0302] - Comparative Example (CE3): Blend of recycled materials (blend A1) and 20% by weight of plastisol P-3;

[0303] - Example of invention (IE1): a blend of recycled materials (blend A1), 22% by weight of plasmon P-2 and 5% by weight of polypropylene homopolymer PPH-1;

[0304] - Example of invention (IE2): a blend of recycled materials (blend A1), 22% by weight of plasmon P-1 and 5% by weight of polypropylene homopolymer PPH-1;

[0305] - Example of invention (IE3): Blend of recycled materials (blend A1), 22% by weight of plasmon P-1 and 5% by weight of polypropylene homopolymer PPH-1.

[0306]

[0307] As can be seen in Table 2, the compositions of the present invention exhibit an excellent combination of properties, wherein MFR > 15 g / 10 min, tensile strength > 10 MPa, tensile strain at break > 200%, and final Charpy notched impact strength at +23°C > 40 kJ / m. 2 .

[0308] In particular, for all IE1 to IE3, the balance between impact stiffness and impact strength (the ratio between Charpy / modulus, Charpy / strength, puncture / modulus, and puncture / strength) is excellent.

[0309] Specifically, the puncture energy measured at -20°C for any of IE1 to IE3 is higher than that for CE1. The Charpy NIS measured at +23°C for any of IE1 and IE2 is higher than that for any of CE1 to CE3.

Claims

1. A polyolefin composition comprising: a) A blend of recycled plastic materials of polypropylene and polyethylene in a ratio of 14:6 to 49.5:1, comprising 60% to 85% by weight (based on the total weight of the polyolefin composition). b) 10% to 30% by weight (based on the total weight of the polyolefin composition) of at least one C2 / C4 and / or C2 / C8 elastomer as a compatibilizer with an MFR2 (ISO 1133, 2.16 kg load at 190°C) equal to or less than 30 g / min. c) 3% to 10% by weight (based on the total weight of the polyolefin composition) of a polypropylene homopolymer with an MFR2 (ISO 1133, 2.16 kg load at 230°C) of at least 800 g / 10 min, and d) Optional additional additives, wherein the total of all ingredients always amounts to 100% by weight. The polyolefin composition is characterized by: - At least 30 kJ / m 2 Impact strength (ISO179-1, Charité 1eA+23℃). - A melt flow rate MFR2 of at least 15 g / 10 min (230°C, 2.16 kg, measured according to ISO 1133), and - At least 80% of the tensile strain at break (ISO 527-2).

2. The polyolefin composition according to claim 1, characterized in that, The polyolefin composition comprises: a) A blend of recycled plastic materials of polypropylene and polyethylene in a ratio of 14:6 to 49.5:1, comprising 63% to 80% by weight, preferably 65% ​​to 75% by weight (based on the total weight of the polyolefin composition). b) 15% to 25% by weight, preferably 18% to 23% by weight (based on the total weight of the polyolefin composition), of at least one C2 / C4 and / or C2 / C8 elastomer as a compatibilizer with an MFR2 (ISO 1133, 2.16 kg load at 190°C) equal to or less than 30 g / min. c) 4% to 9% by weight, more preferably 5% to 7% by weight (based on the total weight of the polyolefin composition), of a polypropylene homopolymer with an MFR2 (ISO 1133, 2.16 kg load at 230°C) of at least 800 g / 10 min, and d) Optional additional additives, wherein the total of all ingredients always amounts to 100 by weight.

3. The polyolefin composition according to any one of the preceding claims, characterized in that, Impact strength (ISO 179-1, Charpy 1eA + 23℃) is at least 35.0 kJ / m 2 Preferably at least 40.0 kJ / m 2 Especially at 30.0 kJ / m 2 Up to 60.0 kJ / m 2 Within that range, and more specifically at 35.0 kJ / m 2 Up to 55.0 kJ / m 2 Within that range, and even more specifically at 40.0 kJ / m 2 Up to 55.0 kJ / m 2 Within the range.

4. The polyolefin composition according to any one of the preceding claims, characterized in that, The melt flow rate MFR2 (ISO 1133, 2.16 kg, 230°C) is at least 16.0 g / 10 min, preferably at least 17.5 g / 10 min, more preferably at least 17.5 g / 10 min, particularly in the range of 15.0 g / 10 min to 30.0 g / 10 min, preferably 16.0 g / 10 min to 25.0 g / 10 min, more preferably 17.0 g / 10 min to 20.0 g / 10 min.

5. The polyolefin composition according to any one of the preceding claims, characterized in that, The tensile strain at break (ISO527-2) is at least 90%, more preferably at least 100%, even more preferably at least 150%, and even more preferably at least 200%, particularly in the range of 80% to 400%, preferably 90% to 300%, and more preferably 100% to 250%.

6. The polyolefin composition according to any one of the preceding claims, characterized in that, The tensile modulus (ISO 527-2) is at least 800 MPa, preferably at least 850 MPa, more preferably at least 870 MPa, particularly in the range of 800 MPa to 1500 MPa, and even more particularly in the range of 850 MPa to 1000 MPa.

7. The polyolefin composition according to any one of the preceding claims, characterized in that, The plastic material blend containing polypropylene and polyethylene is a recycled plastic material blend containing polypropylene and polyethylene in a ratio of 14:6 to 49.5:1, recovered from waste plastic materials derived from post-consumer waste and / or post-industrial waste.

8. The polyolefin composition according to any one of the preceding claims, characterized in that, The melt flow rate (MFR2, 230°C, 2.16 kg, measured according to ISO 1133) of the blend of the recycled plastic materials comprising polypropylene and polyethylene is at least 5.0 g / 10 min, preferably at least 10.0 g / 10 min, more preferably at least 15.0 g / 10 min, particularly in the range of 5.0 g / 10 min to 70.0 g / 10 min, preferably 8.0 g / 10 min to 60.0 g / 10 min, more preferably 10.0 g / 10 min to 50.0 g / 10 min.

9. The polyolefin composition according to any one of the preceding claims, characterized in that, The recycled plastic blends exhibited the following characteristics in CRYSTEX analysis (as described in the experimental section): The content of the crystallization fraction (CF), as determined by CRYSTEX analysis, is in the range of 80.0 wt% to 96.0 wt%, preferably in the range of 82.5 wt% to 95.5 wt%, and more preferably in the range of 85.0 wt% to 95.0 wt%. The soluble fraction (SF) content, as determined by CRYSTEX analysis, is in the range of 4.0 wt% to 20.0 wt%, preferably in the range of 4.5 wt% to 17.5 wt%, and more preferably in the range of 5.0 wt% to 15.0 wt%.

10. The polyolefin composition according to claim 9, characterized in that, The crystal fraction (CF) has one or more of the following characteristics, preferably all of them: ο By quantitative 13 The ethylene content (C2(CF)) determined by C-NMR-calibrated FT-IR spectra is in the range of 2.5 wt% to 20.0 wt%, preferably in the range of 3.5 wt% to 18.0 wt%, more preferably in the range of 5.0 wt% to 15.0 wt%; and / or The intrinsic viscosity (iV(CF)) in decahydronaphthalene, measured at 135°C according to DIN ISO 1628 / 1, is less than 2.5 dl / g, preferably in the range of 1.1 dl / g to 2.5 dl / g, more preferably in the range of 1.2 dl / g to 2.5 dl / g, and even more preferably in the range of 1.4 dl / g to 2.0 dl / g. The soluble fraction (SF) has one or more of the following properties, preferably all of them: -Through quantitative 13 The ethylene content (C2(SF)) determined by FT-IR spectra calibrated by C-NMR spectroscopy is preferably in the range of 20.0 wt% to 55.0 wt%, more preferably in the range of 22.0 wt% to 50.0 wt%, and even more preferably in the range of 24.0 wt% to 45.0 wt%; and / or The intrinsic viscosity (iV(SF)) in decahydronaphthalene, measured at 135°C according to DIN ISO 1628 / 1, is in the range of 0.9 dl / g to 2.3 dl / g, preferably in the range of 1.0 dl / g to 2.2 dl / g, and more preferably in the range of 1.1 dl / g to 2.1 dl / g.

11. The polyolefin composition according to any one of the preceding claims, characterized in that, The MFR2 (ISO 1133, 2.16 kg load at 190°C) of the at least one C2 / C4 and / or C2 / C8 elastomer is equal to or less than 20 g / 10 min; preferably equal to or less than 10 g / 10 min; more preferably equal to or less than 5 g / 10 min.

12. The polyolefin composition according to any one of the preceding claims, characterized in that, The density (ISO 1183) of the at least one C2 / C4 and / or C2 / C8 elastomer is equal to or less than 900 kg / m³. 3 Preferably equal to or lower than 890 kg / m 3 More preferably equal to or less than 880 kg / m 3 Even more preferred is 870 kg / m 3 More preferably equal to or lower than 860 kg / m 3 .

13. The polyolefin composition according to any one of the preceding claims, characterized in that, The MFR2 (ISO 1133, 2.16 kg load at 230°C) of the at least one polypropylene homopolymer is at least 1000 g / 10 min, preferably at least 1200 g / 10 min.

14. Use of the polyolefin composition according to any one of the preceding claims in the manufacture of appliances, particularly household appliances.

15. An article comprising a polyolefin composition according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Derivatized alkylpolysilane preceramic polymers

    CA1318747C

  • Substituted phenols as stabilizers for chlorinated polymers

    CA2043931A1

  • Heat sealable blend of very low density polyethylene or plastomer with polypropylene based polymers and heat sealable film and articles made thereof

    EP0575465B1

  • Plastomer compatibilized polyethylene / polypropylene blends

    US5266392A

  • Polypropylene - polyethylene blends with improved properties

    WO2015169690A1