Powder composition, film, laminate, coated article, and forming method
By using a powder composition of molten fluororesin powder and binder resin powder with an average particle size of 100μm to 1000μm, the problems of foaming and poor adhesion in rotational molding are solved, achieving efficient primer and topcoat processing and forming a smooth film, which is suitable for multi-layer coating of metal substrates.
Patent Information
- Application Number
- CN202580030411.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-01
- Filing Date
- 2025-04-21
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies for processing fluoropolymer coatings via rotational molding suffer from problems such as foaming, poor adhesion, and reduced coating life. In particular, without the use of heat stabilizers, the processing efficiency for transparent coatings is low and the yield is poor.
A powder composition comprising molten fluororesin powder with an average particle size of 100μm to 1000μm and binder resin powder is used to process primer and topcoat by rotational molding, avoiding the use of heat stabilizers, and utilizing the fluidity of molten fluororesin and the adhesiveness of binder resin to form a smooth film.
It achieves foam suppression during rotational molding, improves bond strength and yield, avoids the problem of reduced coating life, and maintains the performance of transparent powder coatings, making it suitable for processing multi-layer films.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] This disclosure relates to powder compositions, films, laminates, coated articles, and molding methods. Background Technology
[0002] Methods for processing powder compositions containing fluorinated resins by rotational molding are known (Patent Documents 1-4). In such methods, a primer is required to improve the adhesion between the substrate and the coating. Liquid primer compositions are commonly used for this primer processing (Patent Documents 1-3). Furthermore, the use of powder primers is also known, and the processing of such powder primers is typically performed by electrostatic coating (Patent Document 4).
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-43283
[0006] Patent Document 2: Japanese Patent Application Publication No. 2005-335185
[0007] Patent Document 3: Japanese Patent Application Publication No. 2008-45140
[0008] Patent Document 4: Japanese Patent Application Publication No. 2022-137848 Summary of the Invention
[0009] The problem that the invention aims to solve
[0010] The purpose of this disclosure is to provide a primer for use in the processing of fluoropolymer coatings by rotational molding, which enables the coating process by rotational molding.
[0011] Methods for solving problems
[0012] This disclosure relates to a powder composition characterized by comprising molten fluororesin powder and binder resin powder with an average particle size of 100 μm to 1000 μm.
[0013] This disclosure also pertains to a powder composition comprising molten fluororesin powder and binder resin powder, characterized in that the overall average particle size of the powder composition is 100 μm to 1000 μm.
[0014] The aforementioned molten fluoropolymer can be a perfluoropolymer.
[0015] The aforementioned molten fluoropolymer can be a tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer.
[0016] The aforementioned molten fluoropolymer can be a non-perfluorinated polymer.
[0017] The aforementioned molten fluoropolymer can be an ethylene / tetrafluoroethylene copolymer.
[0018] The aforementioned adhesive resin preferably comprises at least one selected from the group consisting of polyamide-imide, polyphenylene sulfide, polyethersulfone, aromatic polyether ketones, and polyether-imide.
[0019] The average particle size of the above-mentioned binder resin powder is preferably 100 to 3000 μm.
[0020] The preferred mass ratio of the above-mentioned molten fluororesin powder to the above-mentioned binder resin powder is 50:50 to 95:5.
[0021] Preferably, the average particle size of the molten fluororesin powder is 200 μm to 600 μm, the melt flow rate of the molten fluororesin is 10 g / 10 min to 30 g / 10 min, the molten fluororesin is a tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer or an ethylene / tetrafluoroethylene copolymer, the average particle size of the binder resin powder is 100 μm to 3000 μm, the binder resin comprises at least one selected from the group consisting of polyamide imide, polyphenylene sulfide, polyethersulfone, aromatic polyetherketone resin and polyetherimide, the content of the molten fluororesin powder relative to the total amount of the molten fluororesin powder and the binder resin powder is 50% to 90% by mass, and the total content of the molten fluororesin powder and the binder resin powder relative to the total amount of the powder composition is 98% to 100% by mass.
[0022] The powder composition described above is preferably a primer composition.
[0023] This disclosure also describes a film formed from the above-mentioned powder composition.
[0024] This disclosure also describes a laminate containing a molten fluoropolymer on the aforementioned film.
[0025] This disclosure also pertains to coated articles having the aforementioned laminated body disposed on a metal substrate.
[0026] This disclosure is also a molding method, characterized by having the following steps: step (1), processing the above-mentioned powder composition by rotational molding; and step (2), processing the powder composition containing molten fluororesin, i.e., topcoat, on the film formed by step (1) by rotational molding.
[0027] Invention Effects
[0028] The composition disclosed herein is a powder composition that can be processed by rotational molding, thereby enabling it to be used as a primer for fluoropolymer powder coatings, exhibiting superior adhesion. Detailed Implementation
[0029] The following is a detailed description of this disclosure.
[0030] The powder compositions disclosed herein relate to powder compositions suitable for use as primers when processing powder compositions containing fluorinated resins by rotational molding.
[0031] When processing the primer using the conventional method described above, problems such as foaming and poor adhesion arise when processing the topcoat layer by rotational molding. In particular, processing transparent primers without heat stabilizers or shrinkage-inhibiting fillers is very time-consuming, requiring repair of foamed areas, resulting in a very poor yield. As mentioned above, adding heat stabilizers to the topcoat can solve this problem, but this introduces practical problems such as reduced film life due to mechanical strength issues and dissolution problems.
[0032] On the other hand, if the primer can also be processed by rotational molding, then the same apparatus can be used for both primer processing and topcoat molding. Furthermore, if sufficient performance can be obtained without mixing heat stabilizers into the topcoat, then the aforementioned practical challenges can be overcome by using transparent powder coatings.
[0033] The powder composition disclosed herein is based on the viewpoint described above and is suitable for use as a primer that can be processed by rotational molding. By using such a powder composition, the aforementioned issues of balancing foam suppression and adhesive strength can be resolved. Furthermore, the powder composition disclosed herein also has the advantage of being able to form a sufficiently smooth film.
[0034] (The first method of this disclosure)
[0035] The first aspect of this disclosure is a powder composition comprising a molten fluoropolymer powder with an average particle size of 100 to 1000 μm and a binder resin powder. That is, a molten fluoropolymer powder with a relatively large average particle size is used in combination with the binder resin powder. This achieves the aforementioned objective. When the average particle size of the molten fluoropolymer powder is 100 μm or more, foaming can be sufficiently suppressed. When the average particle size of the molten fluoropolymer powder is 100 μm or more, the flowability of the powder composition tends to improve. On the other hand, when the average particle size of the molten fluoropolymer powder is 1000 μm or less, a sufficiently smooth film can be formed.
[0036] The lower limit of the aforementioned average particle size is more preferably 150 μm, and even more preferably 200 μm. The upper limit of the aforementioned average particle size is more preferably 800 μm, and even more preferably 600 μm.
[0037] It should be noted that the average particle size of the molten fluoropolymer powder is a value determined from an image of the powder composition observed under an electron microscope using particle analysis software. Examples of particle analysis software include SIF's MultiImageTool. In such a method, by utilizing the element identification function of the device, the average particle size of only the molten fluoropolymer powder can be determined from a powder composition containing both molten fluoropolymer powder and binder resin powder.
[0038] (Second method of this disclosure)
[0039] The second aspect of this disclosure is a powder composition comprising molten fluoropolymer powder and binder resin powder, wherein the average particle size of the powder composition as a whole is 100 to 1000 μm. That is, it is a powder composition with a relatively large average particle size, where the average particle size refers to the average particle size of the molten fluoropolymer powder and the binder resin powder as a whole. If the average particle size of the powder composition as a whole is 100 μm or more, foaming can be sufficiently suppressed. In addition, if the average particle size of the powder composition as a whole is 100 μm or more, the flowability of the powder composition tends to increase. On the other hand, if the average particle size of the powder composition as a whole is 1000 μm or less, a sufficiently smooth film can be formed.
[0040] The lower limit of the above-mentioned average particle size is more preferably 150 μm, and even more preferably 200 μm. The upper limit of the above-mentioned average particle size is more preferably 900 μm, and even more preferably 800 μm.
[0041] The average particle size of the powder composition in the second aspect of this disclosure is determined by image analysis-based particle size determination.
[0042] The powder compositions disclosed herein are two such powder compositions, but in either case, their effects are the same when used as a primer. Regarding factors other than the average particle size, they are substantially the same and will not be distinguished hereafter.
[0043] (Meltable fluoropolymer powder)
[0044] Examples of molten fluoropolymers used in this disclosure include polymers obtained by polymerizing one or more monomers, such as chlorofluoroethylene (CFC) monomers, vinylidene fluoride (VDF) monomers, trifluoroethylene monomers, and perfluoropolymers, such as tetrafluoroethylene, hexafluoropropylene, and perfluoro(alkyl vinyl ether) monomers. These monomers may further include one or more vinyl monomers, such as ethylene and propylene. The main chain of the perfluoropolymer consists of carbon atoms, fluorine atoms, and, depending on the case, oxygen atoms, and does not have CH or CH2 atoms, and includes perfluorovinyl monomers and perfluoro(alkyl vinyl ether) monomers. The oxygen atom is typically an ether oxygen atom.
[0045] For the aforementioned molten fluoropolymer, as a comonomer that is copolymerized in small quantities with the aforementioned monomer components, monomers having functional groups such as hydroxyl and carbonyl groups can be used, as well as monomers having cyclic structures. Examples of the aforementioned cyclic structures include structures with cyclic ether structures such as cyclic acetal structures, and preferably structures in which at least two carbon atoms constituting the aforementioned cyclic ether structure are part of the main chain of the aforementioned molten fluoropolymer.
[0046] Examples of the aforementioned molten fluoropolymers include olefin / fluoroolefin copolymers such as ethylene / tetrafluoroethylene copolymer [ETFE], ethylene / chlorotrifluoroethylene copolymer [ECTFE], and propylene / tetrafluoroethylene copolymer; and perfluoropolymers such as tetrafluoroethylene / hexafluoropropylene copolymer [FEP] and tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer [PFA]. These perfluoropolymers use the aforementioned perfluorinated monomers as monomer components.
[0047] Depending on the application, when the aforementioned molten fluoropolymer is a perfluoropolymer, a material copolymerized with tetrafluoroethylene is more preferred, and the aforementioned perfluoromonomers can be used as other comonomers. Among these copolymers, FEP or PFA are particularly preferred from the viewpoint of superior heat resistance and chemical resistance, and from the viewpoint of substrate protection.
[0048] The aforementioned molten fluoropolymer can be a non-perfluoropolymer. In the case of a non-perfluoropolymer, ETFE is particularly preferred.
[0049] The aforementioned molten fluoropolymer needs to be molten. If it is molten, it can be melt-processed through the firing process described later.
[0050] The melt flowability of molten fluoropolymers is typically expressed by melt flow rate (MFR), which is an indicator of flowability. MFR, according to ASTM D3159, is expressed as the weight extruded from a 2 mm diameter nozzle over 10 minutes with a 5 kg load. In the case of perfluoropolymers such as PFA and FEP, MFR is measured at 372 °C; in the case of ETFE, it is measured at 297 °C.
[0051] The preferred melt flow rate (MFR) of the aforementioned molten fluoropolymer is 0.1 to 50 g / 10 min. When within the above melt flow rate range, the adhesion between the resulting primer film and the molten perfluoropolymer film is further improved due to the flow characteristics of the molten fluoropolymer.
[0052] Specifically, the MFR of the aforementioned perfluoropolymer is preferably 1 to 40 g / 10 min. A more preferred lower limit is 5 g / 10 min, and a further preferred lower limit is 10 g / 10 min. A more preferred upper limit is 30 g / 10 min. When within the above-mentioned melt flow rate range, both interlayer adhesion and corrosion resistance can be achieved.
[0053] The above-mentioned molten fluoropolymer can have a melt flow rate within the above-mentioned range by adjusting the above-mentioned molecular weight.
[0054] In the first aspect of this disclosure, the average particle size of the molten fluoropolymer powder is 100 to 1000 μm. It is preferable to have good processability during rotational molding by keeping the average particle size within this range. The preferred lower limit of the average particle size is 100 μm, more preferably 150 μm, and even more preferably 200 μm. The preferred upper limit is 600 μm. In the second aspect of this disclosure, the average particle size of the molten fluoropolymer powder is preferably within the above range.
[0055] The manufacturing method of the aforementioned molten fluoropolymer powder is not particularly limited; for example, it can be obtained by copolymerization using conventionally known polymerization methods such as emulsion polymerization. As needed, the molten fluoropolymer obtained by copolymerization is pulverized into molten fluoropolymer powder having an average particle size within the aforementioned range. The pulverization method is not particularly limited; for example, conventionally known methods can be used. For example, the following method can be used: the dried molten fluoropolymer powder obtained by the aforementioned emulsion polymerization method is compressed into flakes using rollers, pulverized using a pulverizer, and then classified.
[0056] Adhesive resin powder can be made from a resin that is meltable, has a high affinity for metal substrates compared to fluororesins, facilitates adhesion to metal substrates, and has heat resistance that also withstands the processing temperature of fluororesins.
[0057] The resin that can be used as such a binder resin powder is preferably at least one (e.g., 1 to 5) selected from the group consisting of polyamide-imide, polyphenylene sulfide, polyethersulfone, aromatic polyetherketones (aromatic polyetherketones), and polyetherimide. These resins are preferred in terms of high heat resistance and excellent physical properties. The molten fluoropolymer resin that can be used in molten fluoropolymer resin powder is a fluoropolymer resin, while the binder resin that can be used in binder resin powder can be, for example, a non-fluoropolymer resin.
[0058] The average particle size of the binder resin powder is preferably 20 to 3000 μm. This type of binder resin powder allows for both good film formation and adhesion to the metal substrate during rotational molding, which is preferable. The preferred lower limit for the above-mentioned average particle size is 100 μm, more preferably 150 μm, and even more preferably 200 μm. The preferred upper limit is 2000 μm.
[0059] The aforementioned polyamide-imide (PAI) is a resin composed of polymers having amide and imide bonds in their molecular structure. There are no particular limitations on the PAI; examples include resins formed from high molecular weight polymers obtained through the following reactions: reactions of aromatic diamines having intramolecular amide bonds with aromatic tetracarboxylic acids such as pyromellitic acid; reactions of aromatic tricarboxylic acids such as trimellitic anhydride with diamines such as 4,4-diaminophenyl ether and diisocyanates such as diphenylmethane diisocyanate; reactions of diacids having intramolecular aromatic imide rings with diamines; and so on. From the perspective of excellent heat resistance, the aforementioned PAI is preferably composed of polymers having aromatic rings in their main chain.
[0060] Examples of polyphenylene sulfide resins include those having repeating units represented by the following formula.
[0061] -(Ar-S)-
[0062] (In the formula, Ar represents arylene and S represents sulfur).
[0063] Examples of arylene groups include p-phenylene, m-phenylene, o-phenylene, alkyl-substituted phenylene, phenyl-substituted phenylene, halogen-substituted phenylene, amino-substituted phenylene, amide-substituted phenylene, p,p'-diphenylene sulfone, p,p'-biphenylene, and p,p'-biphenylene ether.
[0064] In the aforementioned polyphenylene sulfide resin, the arylene group, which is the repeating unit in the resin, preferably contains 70 mol% or more of phenylene. Furthermore, polyphenylene sulfide resins can be broadly classified into resins with cross-linked or branched structures (cross-linked type) and resins that do not substantially have cross-linked or branched structures (linear type). This disclosure pertains to either the cross-linked type or the linear type.
[0065] The melt flow rate (MFR) of the aforementioned polyphenylene sulfide resin is preferably 10–2500 g / 10 min, more preferably 400–1800 g / 10 min. By using polyphenylene sulfide resin within this range, resin flowability can be achieved while maintaining the resin's physical properties. The aforementioned MFR refers to the amount of resin extruded from the bottom opening of a cylindrical extrusion plasticizer within a certain time after heating and pressurizing the resin at a specific temperature and pressure; it is a well-known parameter indicating the resin's flowability. Specifically, the aforementioned MFR is the value measured according to the test method described in ISO 1133 (ASTM D1238-86) (316°C, 5 kg load).
[0066] If the molecular weight flow rate (MFR) is less than 10 g / 10 min, the fluidity during processing will be insufficient, and the constraints of processing conditions will increase. If the MFR exceeds 2500 g / 10 min, the molecular weight of the resin will be relatively low, which may lead to a decrease in the quality of the molded product, such as a reduction in mechanical properties.
[0067] Polyphenylene sulfide resins with the desired MFR can usually be obtained by adjusting the molecular weight to the high molecular weight range.
[0068] Commercially available products can be used as polyphenylene sulfide resins possessing the aforementioned properties. Examples include those manufactured by DIC (trade name DIC·PPS), manufactured by Toray Industries (trade name TORELIA), manufactured by Solvay (trade name Ryton), manufactured by TOSOH (trade name SUSTEEL), manufactured by Celanese (trade name Celanese(R)PPS), manufactured by NHU (trade name NHU-PPS), etc.
[0069] The polyethersulfone resin (PES) described above is a resin composed of polymers having repeating units represented by the following general formula.
[0070] [Chemistry 1]
[0071] There are no particular limitations on PES, for example, resins made of polymers obtained by the condensation polymerization of dichlorodiphenyl sulfone and bisphenol.
[0072] Aromatic polyetherketone resins are not particularly limited as long as they contain repeating units composed of arylene, ether [-O-] and carbonyl [-C(=O)-], for example, repeating units represented by any of the following formulas (a1) to (a5).
[0073] [-Ar-O-Ar-C(=O)-] (a1)
[0074] [-Ar-O-Ar-C(=O)-Ar-C(=O)-] (a2)
[0075] [-Ar-O-Ar-O-Ar-C(=O)-] (a3)
[0076] [-Ar-O-Ar-C(=O)-Ar-O-Ar-C(=O)-Ar-C(=O)-] (a4)
[0077] [-Ar-O-Ar-O-Ar-C(=O)-Ar-C(=O)-] (a5)
[0078] (In the formula, Ar represents a divalent aromatic hydrocarbon cyclogroup that may have substituents)
[0079] Examples of divalent aromatic hydrocarbon cyclic groups represented by Ar include aryl groups with 6 to 10 carbon atoms, such as phenylene (o-phenylene, m-phenylene, or p-phenylene), naphthylene, biphenylene (2,2'-biphenylene, 3,3'-biphenylene, 4,4'-biphenylene), and triaryl groups (o-, m-, or p-triphenylene). These aromatic hydrocarbon cyclic groups may have substituents, such as halogen atoms, alkyl groups (such as methyl, which are straight-chain or branched alkyl groups with 1 to 4 carbon atoms), haloalkyl groups, hydroxyl groups, alkoxy groups (such as methoxy, which are straight-chain or branched alkoxy groups with 1 to 4 carbon atoms), mercapto groups, alkylthio groups, carboxyl groups, sulfonyl groups, amino groups, N-substituted amino groups, and cyano groups. It should be noted that in the repeating units (a1) to (a5), the types of Ar can be the same or different. Preferred Ar types are phenylene (e.g., p-phenylene) and biphenylene (e.g., 4,4'-biphenylene).
[0080] Examples of resins having repeating units (a1) include polyetherketones (e.g., "PEEK-HT" manufactured by Victrex). Examples of resins having repeating units (a2) include polyetherketoneketones (e.g., "PEKK" manufactured by Arkema+OxfordPerformance Material). Examples of resins having repeating units (a3) include polyetheretherketones (e.g., "VICTREX PEEK" manufactured by Victrex, "Vestakeep (registered trademark)" manufactured by Evonik, "Vestakeep-J" manufactured by Daicel Evonik, and "KetaSpire (registered trademark)" manufactured by Solvay Speciality Polymers), and polydiphenyl ether-phenyl ether-phenyl ketones (e.g., "Kadel (registered trademark)" manufactured by Solvay Speciality Polymers). Examples of resins having repeating units (a4) include polyetherketoneketones (e.g., "VICTREX ST" manufactured by Victrex). Examples of resins having repeating units (a5) include polyether ether ketone ketones. In the repeating unit composed of aryl, ether, and carbonyl groups, the ratio of ether segments (E) to ketone segments (K) is, for example, E / K = 0.5 to 3, preferably around 0.5 to 2.0. The ether segments impart flexibility to the molecular chain, while the ketone segments impart rigidity. Therefore, the more ether segments there are, the faster the crystallization rate and the higher the final crystallinity can be achieved; conversely, the more ketone segments there are, the higher the glass transition temperature and melting point tend to be. These aromatic polyether ketone resins can be used alone or in combination of two or more.
[0081] Among these aromatic polyetherketone resins, those having any one of the repeating units (a1) to (a4) are preferred. For example, as the above-mentioned aromatic polyetherketone resin, at least one (e.g., 1 to 4) resin selected from the group consisting of polyetherketone, polyetheretherketone, polyetherketoneketone, and polyetherketoneetherketoneketone is preferred. Furthermore, at least one (e.g., 1 to 3) resin selected from the group consisting of polyetherketone, polyetheretherketone, and polyetherketoneketone is more preferred. In particular, polyetherketoneketone is preferred from the perspective of improved thin-wall processability and increased tensile elongation.
[0082] The melting point of the aforementioned aromatic polyetherketone resin is preferably 300°C or higher, more preferably 320°C or higher. A melting point within this range improves the heat resistance of the resulting molded article. Furthermore, a melting point of 380°C or lower is preferred. When aromatic polyetherketone resins with melting points above this level are compounded, the thermal degradation of the fluorinated copolymer during compounding is severe, potentially making it impossible to maintain physical properties. The aforementioned melting point corresponds to the maximum value in the heat of melting curve obtained by heating at a rate of 10°C / min using a differential scanning calorimeter (DSC).
[0083] The melt flow rate (MFR) of the above-mentioned aromatic polyetherketone resin, measured under conditions of 380°C and 5000g load, is preferably 1 to 150 g / 10 min, more preferably 5 to 130 g / 10 min, and even more preferably 10 to 100 g / 10 min. With an MFR within the above range, thin-wall processability is improved, and an insulating layer (B) with high tensile elongation can be obtained. The MFR of the above-mentioned aromatic polyetherketone resin was measured using a melt flow index tester according to ASTM D1238.
[0084] The glass transition temperature of the aforementioned aromatic polyetherketone resin is preferably 130°C or higher. More preferably, it is 135°C or higher, and even more preferably, it is 140°C or higher. Insulated wires with excellent heat resistance can be obtained by using glass transition temperatures within the above range. There is no particular limitation on the upper limit of the glass transition temperature, but from a moldability viewpoint, it is preferably 220°C or lower, and more preferably 180°C or lower. The aforementioned glass transition temperature is measured according to JIS K7121 using a differential scanning calorimetry (DSC) apparatus under measurement conditions consisting of a heating rate of 20°C / min.
[0085] (Polyetherimide resin)
[0086] Polyether ether imide resin is a resin composed of polymers having repeating units represented by the following general formula.
[0087] [Chemistry 2]
[0088] Commercially available resins can be used as such resins.
[0089] In the powder composition disclosed herein, the aforementioned binder resin may be only one type, or two or more types may be used in combination. There is no particular limit to the upper limit of the number of types of binder resins; for example, it may be 10 types.
[0090] The aforementioned adhesive resin is used in powder form. There is no particular limitation on the method for manufacturing the powder form of the aforementioned adhesive resin; it can be obtained using known methods.
[0091] The average particle size of the aforementioned binder resin powder is preferably 100 to 3000 μm. Being within this range is preferred in terms of suitability for rotational molding. The lower limit of the aforementioned average particle size is more preferably 150 μm, and even more preferably 200 μm. The upper limit of the aforementioned average particle size is more preferably 2500 μm, and even more preferably 2000 μm.
[0092] In the powder composition disclosed herein, the mass ratio of molten fluoropolymer powder to binder resin powder is preferably 50:50 to 95:5. That is, the powder composition of this disclosure preferably contains 50 to 95% by mass of molten fluoropolymer powder relative to the total amount of molten fluoropolymer powder and binder resin powder. Within the above range, it is preferable to achieve both adhesion between the substrate and the primer layer and adhesion between the topcoat layer and the primer layer. The lower limit of the above-mentioned molten fluoropolymer powder content is more preferably 60% by mass, and even more preferably 70% by mass. The upper limit of the above-mentioned molten fluoropolymer powder content is more preferably 90% by mass, and even more preferably 80% by mass.
[0093] The powder composition disclosed herein may contain components other than molten fluoropolymer powder and binder resin powder, as needed, without impairing the effects of the present disclosure. Examples of such other components include coloring pigments, anti-aging agents, heat stabilizers, fillers, leveling agents, etc. These other components may be included in the molten fluoropolymer powder or binder resin powder.
[0094] It should be noted that when using components other than molten fluoropolymers and binder resins, their content relative to the total amount of the powder composition is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less.
[0095] The total content of the molten fluoropolymer powder and the binder resin powder, relative to the total amount of the powder composition, is preferably 95% by mass or more and 100% by mass or less. More preferably, the total content is 97% by mass or more, and even more preferably 98% by mass or more. The total content may be less than 100% by mass or less, or 99.9% by mass or less.
[0096] (Primer composition)
[0097] The powder composition disclosed herein is preferably used as a primer composition. That is, it is preferable to process the powder composition of this disclosure on a substrate and then further process a topcoat layer (topcoat film forming composition).
[0098] When using the powder composition disclosed herein as a binder composition, there are no particular limitations on the substrate, and examples include elemental metals such as iron, aluminum, copper, and nickel, as well as their alloys. Examples of such alloys include metals such as stainless steel (SUS), and non-metallic inorganic materials such as enamel, glass, and ceramics.
[0099] When using the powder composition disclosed herein as a primer composition, the topcoat is not particularly limited, but is preferably a powder coating containing fluororesin.
[0100] In the above-mentioned topcoat, the fluororesin contained is not particularly limited, and molten fluororesin, exemplified as a fluororesin in the powder composition of this disclosure, can be used.
[0101] In the above-mentioned topcoat, the average particle size of the fluororesin contained therein is preferably 100 to 1000 μm, with the lower limit of the above average particle size more preferably 100 μm, further preferably 150 μm, and even more preferably 200 μm. The upper limit of the above average particle size is more preferably 800 μm, and even more preferably 600 μm.
[0102] In the above-mentioned topcoat, the MFR of the fluoropolymer is preferably 1 to 40 g / 10 minutes. A more preferred lower limit is 5 g / 10 minutes, and a further preferred lower limit is 10 g / 10 minutes. An even more preferred upper limit is 30 g / 10 minutes.
[0103] When processing a multilayer film using the above-described primer composition and topcoat, it is preferable that the fluoropolymer contained in both compositions is the same. That is, when used as a primer for a topcoat containing ETFE, the powder composition of this disclosure preferably contains ETFE. When used as a primer for a topcoat containing PFA, the powder composition of this disclosure preferably contains PFA.
[0104] The aforementioned topcoat preferably does not contain heat stabilizers. Conventionally, topcoats used in rotational molding processes employ methods to suppress foaming by containing heat stabilizers. When the powder composition of this disclosure is used as a primer, foaming and other problems are less likely to occur; therefore, even if the topcoat does not contain heat stabilizers, the conventional problems will not arise, which is preferable.
[0105] If the topcoat contains heat stabilizers, coloring of the film and leaching of heat stabilizer components can sometimes occur. Therefore, using a topcoat that does not substantially contain heat stabilizers has the advantage of preventing such problems.
[0106] It should be noted that the heat stabilizer referred to here is the heat stabilizer commonly used in the coatings industry, specifically, such as amine antioxidants, organic sulfur compounds, and metal powders. In this disclosure, "substantially" not containing heat stabilizers means less than 0.001% by mass relative to the total amount of the topcoat.
[0107] The aforementioned topcoat preferably does not contain pigments. Conventionally, topcoats used in rotational molding processes employ methods that adjust the film hue derived from heat stabilizers by including pigments. When the powder composition of this disclosure is used as a primer, problems such as foaming are less likely to occur; therefore, the topcoat does not need to contain pigments and heat stabilizers, which is preferable.
[0108] If the topcoat contains pigments, the pigment components may sometimes leach out. Therefore, using a topcoat that is substantially free of pigments has the advantage of preventing such problems.
[0109] It should be noted that the pigments referred to here are those commonly used in the coatings industry, specifically, such as carbon black and titanium dioxide. In this disclosure, "substantially" not containing pigments means less than 0.001% by mass relative to the total amount of the topcoat.
[0110] In the above-mentioned topcoat, the content of components other than the fluororesin is preferably 0.1% by mass or less. When the topcoat contains fluororesin, the content of fluororesin relative to the total amount of the topcoat is preferably 99.9% by mass or more and 100.0% by mass or less. The lower limit is more preferably 99.99% by mass, and even more preferably 99.999% by mass.
[0111] (Molding method)
[0112] The molding method disclosed herein is characterized by having: step (1), processing the above-mentioned powder composition by rotational molding; and step (2), processing a topcoat, which is a powder composition containing molten fluororesin, on the film processed by step (1) by rotational molding.
[0113] That is, after processing using the powder composition disclosed herein and rotational molding as step (1), the topcoat containing molten fluororesin, i.e., the powder composition, is rotationally molded in step (2). As a result, problems such as foaming are not generated, and a topcoat film can be formed with sufficient adhesive strength.
[0114] In the molding method disclosed herein, there are no particular limitations on the substrate being processed, although it needs to have a tubular shape. This is because rotational molding is a processing method in which a resin film is formed inside the tubular substrate while it is being rotated.
[0115] There are no particular limitations on the aforementioned base materials; for example, tanks, pipes, joints, valves, etc., can be cited.
[0116] In step (1) above, the powder composition of this disclosure is processed by rotational molding, thereby forming a primer film on a substrate. Specifically, step (1) is a step in which the powder composition is placed in a tube and heated while the tube is rotated to form a film. In this step, the processing temperature is preferably 250 to 400°C. Good processing can be achieved within this temperature range.
[0117] The thickness of the film formed in step (1) above is preferably 100 to 10000 μm. Good physical properties can be obtained within this range. It should be noted that the thickness is measured using a magnetic / eddy current film thickness gauge. The lower limit of the above thickness is more preferably 300 μm, and even more preferably 500 μm. The upper limit of the above thickness is more preferably 8000 μm, and even more preferably 6000 μm.
[0118] In step (2) above, the topcoat is rotated to form a topcoat film on the primer film. Specifically, step (2) involves placing the topcoat, which is a powder composition, in a tube on a substrate on which a film has been formed in step (1), and heating it while rotating the tube to form a film. This process allows the formation of a topcoat film. In step (2), the processing temperature is preferably 250–400°C. Within this temperature range, good processing is possible.
[0119] The thickness of the film formed in step (2) above is preferably 100 to 10000 μm. Good physical properties can be obtained within this range. It should be noted that the thickness is measured using an electromagnetic / eddy current film thickness gauge. The lower limit of the above thickness is more preferably 300 μm, and even more preferably 500 μm. The upper limit of the above thickness is more preferably 8000 μm, and even more preferably 6000 μm.
[0120] The molding method disclosed herein is applicable to fields such as chemicals, pharmaceuticals, food, and semiconductors.
[0121] (film)
[0122] This disclosure also relates to a film. The film of this disclosure is formed from the powder composition described above. The film of this disclosure can be manufactured, for example, by performing the above-described process (1).
[0123] (Layered structure)
[0124] This disclosure also relates to a laminate. The laminate of this disclosure is a laminate in which a film containing a molten fluororesin is disposed on the film of the above-described disclosure. The film containing the molten fluororesin can be manufactured, for example, by using a powder coating containing a molten fluororesin as a topcoat and performing the above-described step (2).
[0125] (Painted items)
[0126] This disclosure also relates to coated articles. The coated articles of this disclosure are coated articles on a metal substrate having the aforementioned laminate of this disclosure disposed thereon. The metal substrate is not particularly limited; examples include metal cans, metal pipes, metal fittings, and metal valves. The applications of the coated articles of this disclosure are not particularly limited; for example, they can be used in the fields of chemicals, pharmaceuticals, food, and semiconductors.
[0127] Example
[0128] The present disclosure will now be described in detail based on embodiments. In the following embodiments, unless otherwise stated, “parts” and “%” represent “parts by mass” and “% by mass”, respectively.
[0129] The ingredients used in the following examples are as follows.
[0130] Fluorinated copolymer A: PFA: PFA manufactured by Daikin Industries, Ltd. (MFR 15g / 10min)
[0131] Fluorinated copolymer B: ETFE: ETFE manufactured by Daikin Industries, Ltd. (MFR 28g / 10min)
[0132] Adhesive Resin A: PAI: Torlon PAI manufactured by Solvay
[0133] Adhesive Resin B: PPS: Ryton PPS manufactured by Solvay
[0134] Adhesive resin C: PES: Sumitomo Chemical Co., Ltd., Sumikaexcel PES
[0135] Adhesive resin D: PEEK: KetaSpire PEEK manufactured by Solvay
[0136] Adhesive resin E: PEI: ULTEM PEI manufactured by Sabic
[0137] Heat stabilizer A: Nocrac White manufactured by Ouchi Shinshin Chemical Industry Co., Ltd.
[0138] Heat stabilizer B: Nocceler MZ manufactured by Ouchi Shinshin Chemical Industry Co., Ltd.
[0139] Heat stabilizer C: Copper(II) oxide powder manufactured by Kanto Chemical Co., Ltd.
[0140] (Preparation of powder compositions containing molten fluoropolymer resin)
[0141] The molten fluoropolymer raw material powder was compacted and shaped using a roller press manufactured by Freund Turbo, and then pulverized using an ACM pulverizer manufactured by Hosokawa Micron to obtain molten fluoropolymer powder.
[0142] (Preparation of powdered compositions containing binder resins)
[0143] The binder resin raw material (granules or flakes) is pulverized using an atomizer-type pulverizer to obtain powder.
[0144] (Preparation of powder compositions)
[0145] The pulverized particles were mixed using an FM Mixer manufactured by NIPPON COKE & ENGINEERING to obtain a powder composition.
[0146] (Molding method)
[0147] The obtained powder composition is processed by the following method.
[0148] On a stainless steel plate (SUS403, surface roughness Ra: 2-3 μm) that had been sandblasted with alumina powder (TosaEmery#40, manufactured by Uji Denka Kogyo Co., Ltd.), the powder composition was processed to achieve a 1000 μm film thickness after firing. The PFA system was fired at 350°C for 60 minutes, and the ETFE system was fired at 300°C for 60 minutes. Then, PFA powder (MFR: 17 g / 10 min, average particle size: 210 μm) or ETFE powder (MFR: 28 g / 10 min, average particle size: 198 μm) was processed onto the obtained film to achieve a total film thickness of 3000 μm after firing. The film was then fired at 350°C for 60 minutes or at 300°C for 60 minutes to obtain a laminate.
[0149] (Evaluation Method)
[0150] (Average particle size)
[0151] Regarding the determination of average particle size, the average particle size was determined from an arbitrary 500 particles using particle analysis software (SIF MultiImageTool) based on images of the powder composition observed with an electron microscope.
[0152] (Angle of Repose)
[0153] The angle of repose was measured as an indicator of the flowability of the mixed powder. This was done using a conical fixture (exit diameter...). Fill a 20mm thick container with approximately 5g of powder and drop it from a height of 40mm. Measure the angle between the slope of the hill formed by the powder and the horizontal plane, and use this angle as the angle of repose.
[0154] (Smoothness)
[0155] The appearance was evaluated using the processed plate used in the peel strength test. Regarding the smoothness of the processed surface, the surface roughness Ra (arithmetic mean roughness) was calculated by averaging the measured values of 5 points using a surface roughness shape measuring machine (Mitutoyo SJ-210, Mitutoyo Co., Ltd.) according to JIS B 0601-1994.
[0156] (Foaming state)
[0157] For the foaming after processing, the coating was visually inspected and judged according to the foaming condition, ranging from 1 to 5.
[0158] 5: No foaming; 4: Foaming at 1 location; 3: Foaming at 2-4 locations; 2: Foaming at 5-9 locations; 1: Foaming at 10 or more locations.
[0159] (Peel strength)
[0160] On a stainless steel plate (SUS403, surface roughness Ra: 2-3 μm) that had been sandblasted with alumina powder (TosaEmery#40, manufactured by Uji Denka Kogyo Co., Ltd.), the powder composition was processed to achieve a 1000 μm film thickness after firing. The PFA system was fired at 350°C for 60 minutes, and the ETFE system was fired at 300°C for 60 minutes. Then, PFA powder (MFR: 17 g / 10 min, average particle size: 210 μm) or ETFE powder (MFR: 28 g / 10 min, average particle size: 198 μm) was processed onto the obtained film to achieve a total film thickness of 3000 μm after firing. The film was then fired at 350°C for 60 minutes or at 300°C for 60 minutes to obtain a laminate. After a 10 mm wide slit was formed on the laminate, the peel strength of the test piece was measured using a Tensilon universal testing machine along a 90° direction at a tensile speed of 50 mm / min, according to JIS K 6854-1. The test results are shown in Tables 1-3.
[0161] [Table 1]
[0162] [Table 2]
[0163] [Table 3]
[0164] Based on the results of the above embodiments, by using the powder composition of this disclosure as a primer, it is possible to achieve a suitable coating film formation.
[0165] Industrial applicability
[0166] The powder composition disclosed herein is suitable for use as a primer when applying fluoropolymers by rotational molding.
Claims
1. A powder composition, characterized in that, It contains molten fluoropolymer powder and binder resin powder with an average particle size of 100μm to 1000μm.
2. A powder composition comprising molten fluoropolymer powder and binder resin powder, characterized in that, The average particle size of the powder composition is 100 μm to 1000 μm.
3. The powder composition according to claim 1 or 2, wherein, Molten fluoropolymers are perfluoropolymers.
4. The powder composition according to any one of claims 1 to 3, wherein, The molten fluoropolymer is a copolymer of tetrafluoroethylene and perfluoro(alkyl vinyl ether).
5. The powder composition according to claim 1 or 2, wherein, Molten fluoropolymers are non-perfluorinated polymers.
6. The powder composition according to claim 1, 2 or 5, wherein, The molten fluoropolymer is an ethylene / tetrafluoroethylene copolymer.
7. The powder composition according to any one of claims 1 to 6, wherein, The adhesive resin comprises at least one selected from the group consisting of polyamide-imide, polyphenylene sulfide, polyethersulfone, aromatic polyether ketones, and polyether-imide.
8. The powder composition according to any one of claims 1 to 7, wherein, The average particle size of the binder resin powder is 100μm to 3000μm.
9. The powder composition according to any one of claims 1 to 8, wherein, The mass ratio of molten fluoropolymer powder to binder resin powder is 50:50 to 95:
5.
10. The powder composition according to any one of claims 1 to 9, wherein, The average particle size of the molten fluoropolymer powder is 200 μm to 600 μm. The melt flow rate of the molten fluoropolymer is 10 g / 10 min to 30 g / 10 min. The molten fluoropolymer is a tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer or an ethylene / tetrafluoroethylene copolymer. The average particle size of the binder resin powder is 100 μm to 3000 μm. The adhesive resin comprises at least one selected from the group consisting of polyamide imide, polyphenylene sulfide, polyethersulfone, aromatic polyetherketone, and polyetherimide. The content of molten fluoropolymer powder relative to the total amount of molten fluoropolymer powder and binder resin powder is 50% to 90% by mass. The total content of molten fluoropolymer powder and binder resin powder is 98% to 100% by mass relative to the total amount of the powder composition.
11. The powder composition according to any one of claims 1 to 10, wherein it is a primer composition.
12. A film formed from the powder composition according to any one of claims 1 to 11.
13. A laminate having a film comprising a molten fluoropolymer on the film of claim 12.
14. A coated article having the laminate of claim 13 disposed on a metal substrate.
15. A molding method, characterized in that, It has the following processes: Step (1) involves processing the powder composition according to any one of claims 1 to 11 using rotational molding; and Step (2) involves processing a powder composition containing molten fluororesin, i.e., a topcoat, on the film formed in step (1) using rotational molding.