Polyimide precursor composition and polyimide film

By using a composition of a specific aromatic polyimide precursor and a solvent to form a polyimide film, the problems of insufficient coloring and light transmittance of aromatic polyimide films are solved, and a flexible display substrate material with high heat resistance and high light transmittance is realized.

CN123146646APending Publication Date: 2026-11-20UBE CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580029401.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-26
Filing Date
2025-04-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing aromatic polyimide films have coloring problems in display applications, still require high-temperature processing in some processes, and have insufficient light transmittance, which cannot meet the requirements of flexible displays.

Method used

A polyimide film is formed by heat treatment using a composition containing a specific aromatic polyimide precursor and a solvent, which improves light transmittance and heat resistance, and is suitable for substrates of flexible displays.

Benefits of technology

While maintaining the heat resistance and linear coefficient of thermal expansion of aromatic polyimide films, it significantly improves light transmittance and heat resistance, making it suitable as a substrate material for flexible displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123146646A_ABST
    Figure CN123146646A_ABST
Patent Text Reader

Abstract

Provided is a polyimide precursor composition for producing an aromatic polyimide film having at least one of light transmittance and heat resistance improved. The polyimide precursor composition includes: a polyimide precursor having a repeating unit represented by the following general formula (I); a solvent A selected from the group consisting of 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropanamide, 1-butyl-2-pyrrolidinone, N,N-diphenylformamide, N,N-diethylbenzamide, benzamide aniline, and 1-phenyl-2-pyrrolidinone; and a solvent B selected from the group consisting of N,N-dimethylpropanamide, N,N-diethylformamide, N,N-diethylacetamide, N,N-dimethylisobutyramide, N,N-diethylpropanamide, and tetramethylurea. (In the formula, R1 and R2 are each a hydrogen atom or the like, and 50 mol% or more of X1 is an aromatic group and / or 50 mol% or more of Y1 is an aromatic group.)
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyimide precursor composition and a polyimide film with excellent heat resistance, which are suitable for use in electronic devices such as flexible device substrates. Background Technology

[0002] Polyimide films are widely used in electrical / electronic devices, semiconductors, and other fields due to their excellent heat resistance, chemical resistance, mechanical strength, electrical properties, and dimensional stability. On the other hand, with the advent of a highly information-based society, significant progress has been made in recent years in the development of optical materials such as optical fibers and waveguides in the field of optical communication, and in the development of liquid crystal alignment films and color filter protective films in the field of display devices. Particularly in the display device field, research is actively underway on lightweight and highly flexible plastic substrates as a replacement for glass substrates, as well as the development of bendable and rollable displays.

[0003] In displays such as liquid crystal displays (LCDs) and organic EL displays, semiconductor elements such as TFTs are formed to drive each pixel. Therefore, the substrate is required to have heat resistance and dimensional stability. Due to its excellent heat resistance, chemical resistance, mechanical strength, electrical properties, and dimensional stability, polyimide film is expected to become a substrate material for display applications.

[0004] Since polyimide is typically yellowish-brown, its use in transmissive devices such as backlit liquid crystal displays is limited. However, in recent years, polyimide films with excellent light transmittance in addition to mechanical and thermal properties have been developed, and there is growing expectation for them as substrates for display applications (see Patent Documents 1 to 4).

[0005] In the manufacture of polyimide, N-methyl-2-pyrrolidone (NMP) and N,N-dimethylacetamide (DMAc) are commonly used as solvents. On the other hand, Patent Document 5 discloses that certain organic solvents are superior to NMP.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: WO 2012 / 011590

[0009] Patent Document 2: WO 2013 / 179727

[0010] Patent Document 3: WO 2014 / 038715

[0011] Patent Document 4: WO 2022 / 176956

[0012] Patent Document 5: WO 2015 / 186782 Summary of the Invention

[0013] The problem the invention aims to solve

[0014] Compared to (semi)alicyclic polyimides such as those in Patent Documents 1 to 4, aromatic polyimides, while having coloring issues, generally exhibit excellent heat resistance. Therefore, if coloring can be minimized, they have the potential to be used as substrates for displays. In recent years, although film deposition methods for thin-film transistors (TFTs) have improved and deposition temperatures have decreased compared to conventional methods, high-temperature processing is still required in some processes. Furthermore, a larger process margin results in higher yields. Therefore, even for aromatic polyimides, which generally exhibit excellent heat resistance, further improvements in heat resistance offer the advantage of adaptability to various processes.

[0015] Especially in smartphones and other devices equipped with under-display cameras, light travels from the display to the camera; therefore, the polyimide film used for the display needs to have high light transmittance, especially in the sensitive areas of the sensor.

[0016] Therefore, an object of the present invention is to provide a polyimide precursor composition for manufacturing polyimide films, wherein at least one, preferably both, of light transmittance and heat resistance is improved while utilizing the advantages of aromatic polyimide films (such as heat resistance and linear coefficient of thermal expansion). Furthermore, another object of the present invention is to provide polyimide films and polyimide film / substrate laminates obtained from the polyimide precursor for use in flexible electronic devices, particularly as substrates for flexible displays.

[0017] Technical means to solve the problem

[0018] The main disclosures of this application are summarized as follows.

[0019] 1. A polyimide precursor composition comprising: A polyimide precursor having repeating units represented by the following general formula (I); Solvent A is selected from at least one solvent A chosen from the group consisting of 1,3-dimethyl-2-imidazolidineone (DMI), 3-methoxy-N,N-dimethylpropionamide (MPA), 1-butyl-2-pyrrolidone (NBP), N,N-diphenylformamide, N,N-diethylbenzamide, benzoylaniline, and 1-phenyl-2-pyrrolidone; and Solvent B is selected from the group consisting of N,N-dimethylpropionamide (DMPA), N,N-diethylformamide (DEF), N,N-diethylacetamide (DEAc), N,N-dimethylisobutyramide (DMIB), N,N-diethylpropionamide (DEPA) and tetramethylurea (TMU).

[0020] [Chemistry 1]

[0021] (Wherein, in general formula I, X1 is a tetravalent aliphatic or aromatic group, Y1 is a divalent aliphatic or aromatic group, and R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms, and...)

[0022] Where X1 comprises more than 50 mol% aromatic groups and / or Y1 comprises more than 50 mol% aromatic groups.

[0023] 2. The polyimide precursor composition as described in item 1 above, wherein, X1 comprises 50 mol% or more of the structure represented by formula (II-1) and / or formula (II-2), and Y1 with a molar percentage of 50% or more is the structure represented by formula (III). [Chemistry 2]

[0024] [Chemistry 3] .

[0025] 3. The polyimide precursor composition as described in item 1 or 2 above, wherein the total amount of solvent A and solvent B is more than 80% by mass of the total mass of the solvents.

[0026] 4. The polyimide precursor composition as described in any of the preceding items, wherein, based on the total mass of solvent A and solvent B, the mass of solvent A is greater than 1% by mass and less than 90% by mass.

[0027] 5. The polyimide precursor composition as described in any of the preceding items, wherein the solvent A and the solvent B are selected from the following combinations (a) to (g): (a) Solvent A comprises 1,3-dimethyl-2-imidazolidineone, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (b) Solvent A comprises 1-butyl-2-pyrrolidone, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (c) Solvent A comprises 3-methoxy-N,N-dimethylpropionamide, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (d) Solvent A comprises 1-phenyl-2-pyrrolidone, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (e) Solvent A comprises N,N-diphenylformamide, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (f) Solvent A comprises N,N-diethylbenzamide, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; and (g) Solvent A contains benzoylaniline, and solvent B contains N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide.

[0028] 6. The polyimide precursor composition as described in any of the preceding items, wherein the polyimide obtained from the polyimide precursor composition has a 0.5% weight loss temperature higher than (i) and (ii) below, or higher than (ii) when solvent A is solid at 25°C: (i) The 0.5% weight loss temperature of the polyimide obtained from the polyimide precursor composition using a solvent containing only solvent A; (ii) The 0.5% weight loss temperature of the polyimide obtained from the polyimide precursor composition using a solvent containing only solvent B.

[0029] 7. The polyimide precursor composition as described in any of the preceding items, wherein a polyimide film with a thickness of 10 µm obtained from the polyimide precursor composition has a light transmittance at a wavelength of 450 nm that is higher than (i) and (ii) below, or higher than (ii) when the solvent A is solid at 25°C: (i) The light transmittance at 450 nm of the polyimide film obtained by using the polyimide precursor composition containing only solvent A; (ii) The light transmittance at 450 nm of the polyimide film obtained by using the polyimide precursor composition with a solvent containing only solvent B.

[0030] 8. A polyimide film obtained from the polyimide precursor composition described in any one of the preceding items.

[0031] 9. A polyimide film / substrate laminate, comprising: Polyimide films obtained from the polyimide precursor compositions described in any one of the foregoing items; and Support substrate.

[0032] 10. The laminate as described in Item 9, wherein the supporting substrate is a glass substrate.

[0033] 11. A method for manufacturing a polyimide film / substrate laminate, comprising the following steps: (a) applying the polyimide precursor composition of any one of the preceding items onto a support substrate; and (b) The polyimide precursor on the support substrate is heat-treated to form a laminate containing a polyimide film on the support substrate.

[0034] 12. The method as described in Project 11, wherein the supporting substrate is a glass substrate.

[0035] 13. A flexible electronic device comprising the polyimide film of item 10 or the polyimide film / substrate laminate of item 11 or 12.

[0036] 14. A method for manufacturing a flexible electronic device, comprising the following steps: (a) applying the polyimide precursor composition of any one of the preceding items onto a support substrate; and (b) The polyimide precursor on the support substrate is heat-treated to obtain a polyimide film / substrate laminate, wherein the polyimide film is laminated on the support substrate; (c) Forming at least one layer selected from conductor layers and semiconductor layers on the polyimide film of the laminate; and (d) Separate the supporting substrate from the polyimide film.

[0037] 15. The method as described in Item 14, wherein the supporting substrate is a glass substrate.

[0038] The effects of the invention

[0039] According to the present invention, a polyimide precursor composition for manufacturing polyimide films is provided, wherein at least one, preferably both, of light transmittance and heat resistance is improved while utilizing the advantages of aromatic polyimide films (such as heat resistance and linear coefficient of thermal expansion). Furthermore, according to the present invention, polyimide films and polyimide film / substrate laminates obtained from the polyimide precursor can be provided.

[0040] Furthermore, according to one aspect of the invention, a polyimide film and a polyimide film / substrate laminate obtained using the above-described polyimide precursor composition can be provided. Furthermore, according to another aspect of the invention, a method for manufacturing a flexible electronic device using the said polyimide precursor composition and a flexible electronic device can be provided. Detailed Implementation

[0041] The term "flexible (electronic) device" in this application refers to a device that is flexible in itself, typically with a semiconductor layer (such as transistors or diodes) formed on a substrate to complete the device. This "flexible (electronic) device" differs from devices such as chip-on-film (COF) devices, which mount "rigid" semiconductor components such as IC chips on a conventional flexible printed circuit board (FPC). However, for the operation or control of the "flexible (electronic) device" of this application, "rigid" semiconductor components such as IC chips can also be mounted on a flexible substrate or electrically connected to it for combined use. Suitable flexible (electronic) devices include display devices such as liquid crystal displays, organic EL displays, and electronic paper, as well as light-receiving devices such as solar cells and CMOS sensors.

[0042] The polyimide precursor composition of the present invention will be described below, followed by a method for manufacturing a flexible electronic device.

[0043] <<Polyimide Precursor Compositions>>

[0044] The polyimide precursor composition for forming a polyimide film comprises a polyimide precursor and at least two solvents. The polyimide precursor is dissolved in the solvents.

[0045] The polyimide precursor has repeating units represented by the following general formula (I): [Chemistry 4]

[0046] (In general formula I, X1 is a tetravalent aliphatic or aromatic group, Y1 is a divalent aliphatic or aromatic group, and R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms.)

[0047] Polyamic acids with hydrogen atoms in R1 and R2 are particularly preferred.

[0048] Of all repeating units in the polyimide precursor, for X1, preferably 50 mol% or more (preferably exceeding 50 mol%), more preferably 70 mol% or more, are aromatic groups; furthermore, 80 mol% or more, 90 mol% or more, and 95 mol% or more are sequentially more preferred. In similar descriptions below, "sequentially more preferred" is omitted. For Y1, preferably 50 mol% or more (preferably exceeding 50 mol%), more preferably 70 mol% or more, are aromatic groups; furthermore, 80 mol% or more, 90 mol% or more, and 95 mol% or more are sequentially more preferred.

[0049] X1 is preferably the structure represented by formula (II-1) and / or formula (II-2) below, and Y1 is preferably the structure represented by formula (III) below. In particular, for X1, it is preferred that it has a structure represented by formula (II-1) and / or formula (II-2) of 50 mol% or more (preferably more than 50 mol%), more preferably 70 mol% or more; furthermore, 80 mol% or more, 90 mol% or more, and 95 mol% or more are preferred in that order. X1 other than the structure represented by formula (II) is also preferably an aromatic group.

[0050] Regarding Y1, it is preferable to have a structure represented by formula (III) of 50 mol% or more (preferably more than 50 mol%), more preferably 70 mol% or more; furthermore, 80 mol% or more, 90 mol% or more, and 95 mol% or more are preferred in that order. Y1 other than the structure represented by formula (III) is also preferably an aromatic group.

[0051] [Chemistry 5]

[0052] [Chemistry 6]

[0053] The polyimide precursor composition of the present invention contains at least two solvents, wherein at least one solvent A is selected from the group consisting of 1,3-dimethyl-2-imidazolium ketone (DMI), 3-methoxy-N,N-dimethylpropionamide (MPA), 1-butyl-2-pyrrolidone (NBP), N,N-diphenylformamide, N,N-diethylbenzamide, benzoylaniline and 1-phenyl-2-pyrrolidone, and at least one solvent B is selected from the group consisting of N,N-dimethylpropionamide (DMPA), N,N-diethylformamide (DEF), N,N-diethylacetamide (DEAc), N,N-dimethylisobutyramide (DMIB), N,N-diethylpropionamide (DEPA) and tetramethylurea (TMU).

[0054] The polyimide precursor will now be described by providing monomers (tetracarboxylic acid component, diamine component, and other components) of general formula (I) for X1 and Y1, followed by a method for manufacturing the precursor.

[0055] In this specification, the term "tetracarboxylic acid component" refers to tetracarboxylic acid derivatives used as raw materials in the manufacture of polyimide, including tetracarboxylic acid, tetracarboxylic dianhydride, and other tetracarboxylic acid silyl esters, tetracarboxylic acid esters, and tetracarboxylic acid chlorides. While there are no particular limitations, tetracarboxylic dianhydride is more convenient from a manufacturing perspective; therefore, examples of using tetracarboxylic dianhydride as the tetracarboxylic acid component will be described below. The diamine component is a diamine compound having two amino groups (-NH2), which is used as a raw material in the manufacture of polyimide.

[0056] In the present specification, the polyimide film refers to both a film formed on a supporting (carrier) substrate and present in a laminate, and a film obtained by separating the substrate. In addition, the material constituting the polyimide film, that is, the material obtained by subjecting a polyimide precursor composition to heat treatment (imidization), may also be referred to as "polyimide material".

[0057] <X1 and tetracarboxylic acid component>

[0058] As described above, among all repeating units in the polyimide precursor, X1 preferably contains an aromatic group, and more preferably 50 mol% or more of X1 is an aromatic group. X1 is preferably an aromatic group in which four bonds are directly bonded to an aromatic ring. As the raw material thereof, a tetracarboxylic dianhydride in which four -COOH groups are directly bonded to an aromatic ring is preferable.

[0059] When X1 is a tetravalent aromatic group, it is preferably a tetravalent group of an aromatic ring having 6 to 40 carbon atoms.

[0060] Examples of the tetravalent group having an aromatic ring include the following groups.

[0061] [Chemical Formula 7]

[0062] (wherein Z1 is a direct bond, or any one of the following divalent groups: [Chemical Formula 8]

[0063] wherein Z2 in the formula is a divalent organic group, Z3 and Z4 are each independently an amide bond, an ester bond or a carbonyl bond, and Z5 is an organic group containing an aromatic ring.)

[0064] Specific examples of Z2 include aliphatic hydrocarbon groups having 2 to 24 carbon atoms and aromatic hydrocarbon groups having 6 to 24 carbon atoms.

[0065] Specific examples of Z5 include aromatic hydrocarbon groups having 6 to 24 carbon atoms.

[0066] Since the resulting polyimide film can have high heat resistance and high light transmittance, the following groups are particularly preferable as the tetravalent group having an aromatic ring.

[0067] [Chemical Formula 9]

[0068] (wherein Z1 is a direct bond or a hexafluoroisopropylidene bond)

[0069] Since the resulting polyimide film can have high heat resistance, high light transmittance and low linear thermal expansion coefficient, Z1 is more preferably a direct bond.

[0070] Furthermore, preferred groups include those in formula (9) above where Z1 is a group containing a fluorene group represented by formula (3A) below: [Chemistry 10]

[0071] Z 11 and Z 12 Each is independently a (preferably identical) single bond or divalent organic group. Z 11 and Z 12 Preferably, it contains an organic group with an aromatic ring, and more preferably has a structure represented, for example, by formula (3A1): [Chemistry 11]

[0072] (Z 13 and Z 14 Each can be independently a single bond, -COO-, -OCO-, or -O-, where, when Z 14 When connected to a fluorene group, Z is preferred. 13 It is -COO-, -OCO-, or -O- and Z 14 It has a single bond structure; R 91 It is an alkyl or phenyl group having 1 to 4 carbon atoms, preferably methyl, and n is an integer from 0 to 4, preferably 1).

[0073] Examples of particularly preferred aromatic tetracarboxylic acid components include 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, pyromellitic acid, 3,3',4,4'-benzophenone tetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 4,4'-oxydiphthalic acid, bis(3,4-dicarboxyphenyl) sulfone, m-terphenyl-3,4,3',4'-tetracarboxylic acid, p-terphenyl-3,4,3',4'-tetracarboxylic acid, dicarboxyphenyl dimethylsilane, dicarboxyphenoxybiphenyl sulfide, and sulfonyldiphthalic acid, and their derivatives, including tetracarboxylic dianhydride, tetracarboxylic silyl ester, tetracarboxylic ester, and tetracarboxylic chloride. Examples of tetracarboxylic acid components providing X1 as a repeating unit of general formula (I) having a tetravalent group containing a fluorine atom include 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane and its derivatives, including tetracarboxylic dianhydride, tetracarboxylic silyl ester, tetracarboxylic ester, and tetracarboxylic chloride. Furthermore, preferred examples of compounds include (9H-fluorene-9,9-diyl)bis(2-methyl-4,1-phenylene)bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid ester). The tetracarboxylic acid components can be used alone or in combination of several.

[0074] Of these tetracarboxylic acid components, particularly preferred compounds are 3,3',4,4'-biphenyltetracarboxylic acid (and its derivatives, especially dianhydride s-BPDA) and oxydiphthalic acid (and its derivatives, especially dianhydride ODPA), which provide the structures represented by formulas (II-1) and (II-2). In a preferred embodiment, it is preferable to use a tetracarboxylic acid component containing s-BPDA and / or ODPA in the proportions described in formulas (II-1) and / or (II-2). In this case, other tetracarboxylic acid components can be selected from the above-mentioned compounds.

[0075] [Chemistry 12]

[0076] In another preferred embodiment, the tetracarboxylic acid component may be selected from the above-mentioned tetracarboxylic acid components without selecting 3,3',4,4'-biphenyltetracarboxylic acid (and its derivatives, especially dianhydride s-BPDA).

[0077] When an aliphatic group is selected as X1, either an alicyclic group or a chain aliphatic group can be used, but a group with an alicyclic structure is preferred.

[0078] As a tetravalent group having an alicyclic structure, it is preferable to have an alicyclic structure having 4 to 40 carbon atoms; more preferably, the group has at least one aliphatic 4 to 12-membered ring; even more preferably, it is an aliphatic 4-membered ring or an aliphatic 6-membered ring. Preferred examples of tetravalent groups having an aliphatic 4-membered ring or an aliphatic 6-membered ring include the following groups.

[0079] [Chemistry 13]

[0080] (where R) 31 To R 38 Each is an independent directly bonded or divalent organic group; R 41 To R 47 and R 71 To R 73 Each independently represents one of the groups selected from those represented by the following formulas: -CH2-, -CH=CH-, -CH2CH2-, -O-, and -S-; and R 48 (These are organic groups with aromatic or alicyclic structures.)

[0081] R 31 R 32 R 33 R 34 R 35 R 36 R 37 and R38 Specific examples include direct bonding, organic groups containing aromatic or alicyclic structures, aliphatic hydrocarbon groups having 1 to 6 carbon atoms, or oxygen atoms (-O-), sulfur atoms (-S-), carbonyl bonds, ester bonds, and amide bonds. Direct bonding is particularly preferred.

[0082] Having an aromatic ring as R 31 To R 38 and R 48 Examples of organic groups include the following groups.

[0083] [Chemistry 14]

[0084] (W1 is a directly bonded or divalent organic group; n) 11 up to n 13 Each can independently represent an integer from 0 to 4; R 51 R 52 and R 53 Each group can be an alkyl, halogenated, hydroxyl, carboxyl, or trifluoromethyl group having 1 to 6 carbon atoms.

[0085] Specific examples of W1 include direct bonding, divalent groups represented by the following formula (5), and divalent groups represented by the following formula (6).

[0086] [Chemistry 15]

[0087] (where R in equation (6) 61 To R 68 Each can independently represent either a directly bonded or divalent group represented by formula (5).

[0088] As a tetravalent group having an alicyclic structure, a group having a bridged alicyclic structure is preferred, and the following groups are particularly preferred.

[0089] [Chemistry 16]

[0090] Examples of alicyclic tetracarboxylic dianhydrides having an alicyclic structure-containing group include norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic dianhydride (abbreviation: CpODA), 2,2'-binorbornane-5,5',6,6'-tetracarboxylic dianhydride (abbreviation: BNBDA); monocyclic alicyclic tetracarboxylic dianhydrides such as 1,2,3,4-cyclobutanetetracarboxylic dianhydride and cyclohexane-1,2,4,5-tetracarboxylic dianhydride; and alicyclic tetracarboxylic dianhydrides having two or more rings, such as [1,1'-bis(cyclohexane)]-3,3',4,4'-tetracarboxylic dianhydride, [1,1'-bis(cyclohexane)]-2,3,3',4'-tetracarboxylic dianhydride, [1,1'-bis(cyclohexane)]-2,2',3,3'-tetracarboxylic dianhydride, 4,4'-methylenebis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-(propane-2,2-diyl)bis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-oxybis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-thiobis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-sulfonylbis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-(dimethylsilanediyl)bis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-(tetrafluoropropane-2,2-diyl)bis(cyclohexane-1,2-dicarboxylic anhydride), octahydropentalene-1,3,4,6-tetracarboxylic dianhydride, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride, 6-(carboxymethyl)bicyclo[2.2.1]heptane-2,3,5-tricarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.2]oct-5-ene-2,3,7,8-tetracarboxylic dianhydride, tricyclo[4.2.2.02,5]decane-3,4,7,8-tetracarboxylic dianhydride, tricyclo[4.2.2.02,5]dec-7-ene-3,4,9,10-tetracarboxylic dianhydride, 9-oxatricyclo[4.2.1.02,5]nonane-3,4,7,8-tetracarboxylic dianhydride, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethanonaphthalene-2c,3c,6c,7c-tetracarboxylic dianhydride, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethanonaphthalene-2t,3t,6c,7c-tetracarboxylic dianhydride, decahydro-1,4-ethano-5,8-methanonaphthalene-2,3,6,7-tetracarboxylic dianhydride and tetradecahydro-1,4:5,8:9,10-trimethanoanthracene-2,3,6,7-tetracarboxylic dianhydride. These may be used alone or in combination of two or more.

[0091] <Y1 and diamine component>

[0092] As described above, in all repeating units of the polyimide precursor, Y1 preferably contains aromatic groups, and more preferably, more than 50 mol% (preferably more than 50 mol%) of Y1 is an aromatic group.

[0093] When Y1 is a divalent group having an aromatic ring, it is preferably a divalent group having an aromatic ring having 6 to 40 carbon atoms, more preferably 6 to 20 carbon atoms.

[0094] Examples of divalent groups having an aromatic ring include the following groups.

[0095] [Chemistry 17]

[0096] (W1 is a directly bonded or divalent organic group; n) 11 up to n 13 Each represents an integer from 0 to 4 independently; and R 51 R 52 and R 53 Each of these can be an alkyl, halogenated, hydroxyl, carboxyl, or trifluoromethyl group having 1 to 6 carbon atoms.

[0097] Specific examples of W1 include direct bonding, divalent groups represented by formula (5) as described below, and divalent groups represented by formula (6) as described below.

[0098] [Chemistry 18]

[0099] [Chemistry 19]

[0100] (where R in equation (6) 61 To R 68 Each can independently represent either a direct bond or any of the divalent groups represented by formula (5).

[0101] Since the resulting polyimide can possess high heat resistance, high light transmittance, and low linear coefficient of thermal expansion, W1 here is particularly preferably directly bonded, or selected from the group consisting of groups represented by the following formulas: -NHCO-, -CONH-, -COO-, and -OCO-. Furthermore, W1 is particularly preferably any of the divalent groups represented by formula (6), wherein R... 61 To R 68 For direct bonding, or choose one of the groups represented by the following formula: -NHCO-, -CONH-, -COO- and -OCO-.

[0102] Furthermore, preferred groups include those in formula (4) above where W1 is a group containing a fluorene group represented by formula (3B) below: [Chemistry 20]

[0103] Z 11 and Z 12 Each is independently a (preferably identical) single bond or divalent organic group. Z 11 and Z 12 Preferably, it contains an organic group with an aromatic ring, and more preferably has a structure represented, for example, by formula (3B1): [Chemistry 21]

[0104] (Z 13 and Z 14 Each can be independently a single bond, -COO-, -OCO-, or -O-, where, when Z 14 When connected to a fluorene group, Z is preferred. 13 It is -COO-, -OCO-, or -O- and Z 14 It has a single bond structure; R 91 It is an alkyl or phenyl group having 1 to 4 carbon atoms, preferably phenyl, and n is an integer from 0 to 4, preferably 1).

[0105] Another preferred group includes compounds in formula (4) above where W1 is a phenylene group, i.e., triphenyl diamine compounds, and particularly preferred are compounds in which all bonds are in the para position.

[0106] Another preferred group includes W1 in formula (4) above, which represents the first structure in formula (6) containing a single benzene ring, and wherein R 61 and R 62 It is a compound with a 2,2-propylidene group.

[0107] Another preferred group includes W1 in the above formula (4) which is a compound represented by formula (3B2).

[0108] [Chemistry 22]

[0109] Examples of particularly preferred aromatic diamine components include p-phenylenediamine, m-phenylenediamine, benzidine, 3,3'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, m-toluidine, 4,4'-diaminobenzoylaniline, 3,4'-diaminobenzoylaniline, N,N'-bis(4-aminophenyl)terephthalamide, N,N'-p-phenylenebis(p-aminobenzoamide), 4-aminophenoxy-4-diaminobenzoate, bis(4-aminophenyl)terephthalate, Biphenyl-4,4'-dicarboxylic acid bis(4-aminophenyl) ester, p-phenylene bis(p-aminobenzoate), bis(4-aminophenyl)-[1,1'-biphenyl]-4,4'-dicarboxylic acid ester, [1,1'-biphenyl]-4,4'-dimethylbis(4-aminobenzoate), 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, p-methylenebis(phenylenediamine), 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene Benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, bis(4-aminophenyl)sulfone, 3,3'-bis(trifluoromethyl)benzidine, 3,3'-bis((aminophenoxy)phenyl)propane, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(4-(4-aminophenoxy)diphenyl)sulfone, bis(4-(3-aminophenoxy)diphenyl) Sulfone, octafluorobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 2,4-bis(4-aminoanilino)-6-amino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-methylamino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-ethylamino-1,3,5-triazine and 2,4-bis(4-aminoanilino)-6-anilino-1,3,5-triazine. Examples of diamine components providing Y1 as a repeating unit of general formula (I) having a divalent group containing a fluorine atom include 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, and 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.In addition, preferred diamine compounds include 9,9-bis(4-aminophenyl)fluorene, 4,4'-(((9H-fluorene-9,9-diyl)bis([1,1'-biphenyl]-5,2-diyl))bis(oxy))diamine, [1,1':4',1''-terphenyl]-4,4''-diamine, and 4,4'-([1,1'-binaphthyl]-2,2'-diylbis(oxy))diamine. The diamine components can be used alone or in combination.

[0110] Of these diamine components, a particularly preferred compound is p-phenylenediamine (PPD), which provides the structure represented by formula (III). In a preferred embodiment, a diamine component containing p-phenylenediamine in the proportion described in formula (III) is preferably used. In this case, other diamine components can be selected from the above-mentioned compounds.

[0111] [Chemistry 23]

[0112] In another preferred embodiment, the diamine component may be selected from the above-mentioned diamine components without selecting p-phenylenediamine.

[0113] When choosing an aliphatic group as Y1, either an alicyclic group or a chain aliphatic group can be used, but a group with an alicyclic structure is preferred.

[0114] As a divalent group having an alicyclic structure, it is preferred to have an alicyclic structure having 4 to 40 carbon atoms, more preferably the group has at least one aliphatic 4 to 12-membered ring, and even more preferably an aliphatic 6-membered ring.

[0115] Examples of divalent groups with alicyclic structures include the following groups: [Chemistry 24]

[0116] (where V1 and V2 are each independently a directly bonded or divalent organic group; n) 21 up to n 26 Each can independently represent an integer from 0 to 4; R 81 To R 86 Each is independently an alkyl, halogenated, hydroxyl, carboxyl, or trifluoromethyl group having 1 to 6 carbon atoms; and R 91 R 92 and R 93 Each is independently selected from one of the groups represented by the following formulas: -CH2-, -CH=CH-, -CH2CH2-, -O-, and -S-).

[0117] Specific examples of V1 and V2 include direct bonding and divalent organic groups represented by formula (5) as described above.

[0118] Since the resulting polyimide can have high heat resistance and low linear coefficient of thermal expansion, the following groups are particularly preferred as divalent groups with alicyclic structures.

[0119] [Chemistry 25]

[0120] Among them, the following groups are preferred as divalent groups with alicyclic structures.

[0121] [Chemistry 26]

[0122] Examples of diamine components in which Y1 is a repeating unit of general formula (I) having an alicyclic structure include 1,4-diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-2-ethylcyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,2-diaminocyclohexane, and 1,3-diaminocyclohexane. Cyclobutane, 1,4-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, diaminodicycloheptane, diaminomethyldicycloheptane, diaminooxydicycloheptane, diaminomethoxydicycloheptane, isophorone diamine, diaminotricyclodecane, diaminomethyltricyclodecane, bis(aminocyclohexyl)methane, bis(aminocyclohexyl)isopropylidene, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirodiindane, and 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirodiindane. The diamine components can be used alone or in combination.

[0123] As the repeating unit represented by general formula (I), any aliphatic tetracarboxylic acid (especially dianhydride) and / or aliphatic diamine other than alicyclic compounds can be used. Based on a total of 100 mol% of the tetracarboxylic acid and diamine components, their contents are preferably less than 30 mol%, more preferably less than 20 mol%, less than 10 mol%, less than 5 mol%, and less than 2 mol% (inclusive).

[0124] Polyimides derived from monomers primarily containing s-BPDA and PPD are widely known to possess excellent heat resistance, mechanical strength, and thermal properties, and are highly reliable among users. Therefore, if the polyimide precursor compositions of the present invention can slightly improve these properties, or even slightly alleviate the weaknesses related to coloring, they will have significant practical benefits for applications in flexible devices.

[0125] Solvent

[0126] The polyimide precursor composition of the present invention contains solvents including solvent A and solvent B as described above. At least one solvent A is selected from the group consisting of 1,3-dimethyl-2-imidazolium ketone (DMI), 3-methoxy-N,N-dimethylpropionamide (MPA), 1-butyl-2-pyrrolidone (NBP), N,N-diphenylformamide, N,N-diethylbenzamide, benzoylaniline, and 1-phenyl-2-pyrrolidone. At least one solvent B is selected from the group consisting of N,N-dimethylpropionamide (DMPA), N,N-diethylformamide (DEF), N,N-diethylacetamide (DEAc), N,N-dimethylisobutyramide (DMIB), N,N-diethylpropionamide (DEPA), and tetramethylurea (TMU). Solvent A has a higher boiling point than solvent B. Furthermore, even compounds that are solid at room temperature (e.g., 25°C), such as 1-phenyl-2-pyrrolidone, can be used when mixed with other solvents. For example, when solvent A is a solid compound and solvent B is a liquid, there are no particular restrictions on the method of mixing the solvents; solvent A can be added to solvent B in solid form to dissolve it, or solvent A can be heated above its melting point to become a liquid and then mixed with solvent B.

[0127] These solvents are also preferred because they are not designated as substances of very high concern under the EU's REACH regulation.

[0128] There is no limitation on the mass ratio of solvent A to solvent B, as long as both solvents are included. Relative to the total mass of solvent A and solvent B, the mass of solvent A is greater than 0%, preferably greater than 1%, more preferably 1.5% or more, more preferably 2% or more, and subsequently more preferably 3% or more, 5% or more; it can also be 8% or more, 10% or more, 20% or more, 25% or more, or 30% or more. Relative to the total mass of solvent A and solvent B, the upper limit of the mass of solvent A is less than 100%, preferably less than 90%, and can also be less than 80%, less than 75%, or less than 70%.

[0129] In one embodiment, from a processability point of view, it is preferable that the amount of solvent A is small and the amount of solvent B is large; relative to the total mass of solvent A and solvent B, the mass of solvent A may preferably be 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 8% or less.

[0130] In one embodiment, for example, the ratio is preferably 10 / 90 to 90 / 10, more preferably 20 / 80 to 80 / 20, even more preferably 25 / 75 to 75 / 25, and even more preferably 30 / 70 to 70 / 30.

[0131] Furthermore, from another perspective, solvent A can be added in such a manner that the number of moles of solvent A is 0.5 moles or more, preferably 1 mole or more, relative to 1 mole of repeating unit of polyimide precursor. The upper limit can be determined based on the concentration of polyimide precursor and the mass ratio of solvent A to solvent B.

[0132] In the polyimide precursor composition, the total amount of solvent A and solvent B relative to the total amount of solvent is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and most preferably 95% by mass or more; 100% by mass is also preferred.

[0133] While there are no particular restrictions on the combination of solvent A and solvent B, examples of such combinations include: (a) Solvent A contains DMI, and solvent B contains DMPA, TMU, or DMIB; (b) Solvent A contains NBP, and solvent B contains DMPA, TMU, or DMIB; (c) Solvent A contains MPA, and solvent B contains DMPA, TMU, or DMIB; (d) Solvent A comprises 1-phenyl-2-pyrrolidone, and solvent B comprises DMPA, TMU, or DMIB; (e) Solvent A comprises N,N-diphenylformamide, and solvent B comprises DMPA, TMU, or DMIB; (f) Solvent A comprises N,N-diethylbenzamide, and solvent B comprises DMPA, TMU, or DMIB; and (g) Solvent A contains benzoyl aniline, and solvent B contains DMPA, TMU, or DMIB.

[0134] In particular, the combination of solvent A and solvent B is preferably any of the following combinations: (a') Solvent A contains DMI, and solvent B contains DMPA; (b') Solvent A contains NBP, and solvent B contains DMPA, TMU, or DMIB; (c') Solvent A contains MPA, and solvent B contains DMPA; (d') Solvent A comprises 1-phenyl-2-pyrrolidone, and solvent B comprises DMPA, TMU, or DMIB; (e') Solvent A contains N,N-diphenylformamide, and solvent B contains DMPA; (f') Solvent A comprises N,N-diethylbenzamide, and solvent B comprises DMPA; and (g') Solvent A contains benzoyl aniline, and solvent B contains DMPA, TMU, or DMIB.

[0135] In each of the combinations (a) to (g) and (a') to (g') above, other solvents A may be used with the specified solvent A. Typically, based on the total mass of solvent A, the mass of the specified solvent A is, for example, 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 100%. Similarly, other solvents B may be used with the specified solvent B. Typically, based on the total mass of solvent B, the mass of the specified solvent B is, for example, 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, or 100%.

[0136] In one specific embodiment of the present invention, solvent A contains 1,3-dimethyl-2-imidazolium ketone (DMI), preferably in an amount of 50% by mass or more (preferably more than 50% by mass), and its content may also be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. Solvent A may consist solely of DMI. In the same or different embodiments, solvent B may contain N,N-dimethylpropionamide (DMPA), preferably in an amount of 50% by mass or more (preferably more than 50% by mass), and its content may also be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. Solvent B may consist solely of DMPA.

[0137] In one specific embodiment of the invention, solvent A comprises 1,3-dimethyl-2-imidazolium ketone, and solvent B comprises N,N-dimethylpropionamide. Based on the total mass of the solvents, the total content of 1,3-dimethyl-2-imidazolium ketone and N,N-dimethylpropionamide is preferably 80% by mass or more, more preferably 90% by mass or more, and may also be 100% by mass. The mass ratio of 1,3-dimethyl-2-imidazolium ketone to N,N-dimethylpropionamide may be within the range of solvent A and solvent B described above, but for example, it may be in the range of 20 / 80 to 80 / 20.

[0138] As a balance, the solvent may be included in addition to solvent A and solvent B (hereinafter referred to as "other solvents"), but the boiling point of the other solvents is preferably lower than that of solvent A. The boiling point of the other solvents may also be lower than that of solvent B.

[0139] Examples of other solvents include water, or amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and N-ethyl-2-pyrrolidone; cyclic ester solvents such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, and α-methyl-γ-butyrolactone; carbonate solvents such as ethylene carbonate and propylene carbonate; diol solvents such as triethylene glycol; phenolic solvents such as m-cresol, p-cresol, 3-chlorophenol, and 4-chlorophenol; acetophenone, sulfolane, and dimethyl sulfoxide. In addition, other commonly used organic solvents are included, namely phenol, o-cresol, butyl acetate, ethyl acetate, isobutyl acetate, propylene glycol methyl acetate, ethyl cellosolve, butyl cellosolve, 2-methyl acetic acid cellosolve, ethyl acetic acid cellosolve, butyl acetic acid cellosolve, tetrahydrofuran, dimethoxyethane, diethoxyethane, dibutyl ether, diethylene glycol dimethyl ether, methyl isobutyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, acetone, butanol, ethanol, xylene, toluene, chlorobenzene, turpentine, mineral oil, and naphtha solvents. Two or more of these solvents may be used in combination as other solvents.

[0140] Even if other solvents are used, these solvents are preferably not designated as substances of very high concern under the EU REACH regulation. In this regard, N,N-dimethylacetamide, N-methylpyrrolidone, N-methylacetamide and N,N-dimethylformamide are preferably not used, or if used, their amounts are preferably minimized.

[0141] The polyimide precursor composition of the present invention can be manufactured by reacting a tetracarboxylic acid component with a diamine component in a solvent, particularly in a solvent containing at least one selected from solvent A of the present application and at least one selected from solvent B. Based on the chemical structures of R1 and R2, the polyimide precursors used in the present invention (polyimide precursors comprising at least one repeating unit represented by formula (I)) can be classified as follows: 1) Polyamic acid (R1 and R2 are hydrogen atoms), 2) Polyamate (at least a portion of R1 and R2 is alkyl), and 3) 4) Polyamic acid silyl ester (at least a portion of R1 and R2 is alkylsilyl).

[0142] Various polyimide precursors can be readily manufactured using the methods described below. However, the methods for manufacturing the polyimide precursors used in this invention are not limited to those described below.

[0143] 1) Polyamic acid

[0144] The polyimide precursor can be suitably obtained in the form of a polyimide precursor solution by reacting a tetracarboxylic acid dianhydride, which is a tetracarboxylic acid component, with a diamine component in a substantially equimolar ratio in a solvent at a lower temperature below 120°C, for example, while suppressing imidization. Preferably, the molar ratio of the diamine component to the tetracarboxylic acid component [moles of the diamine component / moles of the tetracarboxylic acid component] is 0.90 to 1.10, more preferably 0.95 to 1.05.

[0145] More specifically, the polyimide precursor can be obtained by dissolving a diamine in a solvent, gradually adding a tetracarboxylic dianhydride to the solution while stirring, and then stirring at 0°C-120°C, preferably 5°C-80°C, for 1 hour to 72 hours, although the manufacturing method is not limited to this. When the reaction is carried out above 80°C, the molecular weight changes according to the temperature profile of the polymerization and imidization occurs due to heat, thus sometimes making it impossible to stably produce the polyimide precursor. The order of addition of the diamine and tetracarboxylic dianhydride in the above manufacturing method is preferred because it facilitates an increase in the molecular weight of the polyimide precursor. On the other hand, the order of addition of the diamine and tetracarboxylic dianhydride in the above manufacturing method can also be reversed, which is preferred because it reduces the amount of precipitate.

[0146] 2) Polyamide ester

[0147] Tetracarboxylic acid dianhydride can be reacted with any alcohol to obtain diester dicarboxylic acid, which is then reacted with a chlorinating agent (thionyl chloride, oxalyl chloride, etc.) to obtain diester dicarboxylic acid chloride. Polyimide precursors can be obtained by stirring the diester dicarboxylic acid chloride with a diamine in a solvent at -20°C to 120°C, preferably -5°C to 80°C, for 1 to 72 hours. When the reaction is carried out above 80°C, the molecular weight varies according to the temperature profile of the polymerization, and imidization occurs due to heat, thus sometimes making it difficult to stably produce polyimide precursors. Polyimide precursors can also be easily obtained by dehydrating and condensing the diester dicarboxylic acid with a diamine using phosphorus-based condensing agents, carbodiimide condensing agents, etc.

[0148] 3) Polyamyl silyl ester (indirect method)

[0149] Silylated diamines can be obtained by reacting diamines with a silylating agent beforehand. If necessary, the silyllated diamines can be purified by distillation or other methods. Then, the silyllated diamines are dissolved in a dehydrating solvent, and tetracarboxylic dianhydride is gradually added to the solution while stirring. The mixture is then stirred at 0°C-120°C, preferably 5°C-80°C, for 1 hour to 72 hours to obtain a polyimide precursor. When the reaction is carried out above 80°C, the molecular weight changes according to the temperature profile of the polymerization, and imidization occurs due to heat; therefore, it is sometimes impossible to stably produce polyimide precursors.

[0150] 4) Polyamyl silyl ester (direct method)

[0151] Polyimide precursors can be obtained by mixing a polyamic acid solution obtained using method 1) with a silylating agent, and then stirring at 0°C-120°C, preferably 5°C-80°C, for 1 hour to 72 hours. When the reaction is carried out above 80°C, the molecular weight will vary according to the temperature history of the polymerization, and imidization will occur due to heat, so it is sometimes impossible to stably produce polyimide precursors.

[0152] For the silylating agents used in methods 3) and 4), chlorine-free silylating agents are preferred because purification of the silylated polyamic acid or the resulting polyimide is unnecessary. Examples of chlorine-free silylating agents include N,O-bis(trimethylsilyl)trifluoroacetamide, N,O-bis(trimethylsilyl)acetamide, and hexamethyldisilazane. N,O-bis(trimethylsilyl)acetamide and hexamethyldisilazane are particularly preferred because they are fluorine-free and inexpensive.

[0153] Meanwhile, in the silylation reaction of diamines in method 3), amine catalysts such as pyridine, piperidine, and triethylamine can be used to promote the reaction. These catalysts can be used as is for the polymerization of polyimide precursors.

[0154] There are no particular restrictions on the manufacture of polyimide precursors, but the monomers and solvents are added to a concentration such that the solid component concentration of the polyimide precursor (mass concentration converted to polyimide) is, for example, 5-45% by mass.

[0155] While there are no particular limitations on the logarithmic viscosity of the polyimide precursor, the logarithmic viscosity of the polyimide precursor in a 0.5 g / dL N-methyl-2-pyrrolidone solution at 30°C is preferably 0.2 dL / g or higher, more preferably 0.3 dL / g or higher, and particularly preferably 0.4 dL / g or higher. When the logarithmic viscosity is 0.2 dL / g or higher, the molecular weight of the polyimide precursor is high, resulting in polyimides with excellent mechanical strength and heat resistance.

[0156] <Imidazole compounds>

[0157] The polyimide precursor composition preferably also contains at least one imidazole compound. The imidazole compound is not particularly limited, as long as it has an imidazole skeleton; examples include 1,2-dimethylimidazole, 1-methylimidazole, 2-methylimidazole, 2-phenylimidazole, imidazole, and benzimidazole. From the viewpoint of storage stability of the polyimide precursor composition, 2-phenylimidazole and benzimidazole are preferred. Two or more imidazole compounds may be used in combination.

[0158] The content of the imidazole compound in the polyimide precursor composition can be appropriately selected based on the balance between the additive effect and the stability of the polyimide precursor composition. The amount of the imidazole compound relative to 1 mole of a repeating unit of the polyimide precursor is preferably greater than 0.0001 mol to less than 2 mol. The addition of the imidazole compound is effective in improving light transmittance, linear coefficient of thermal expansion, and / or mechanical properties, and within this content range, it also has a positive effect on the storage stability of the polyimide precursor composition.

[0159] The content of each imidazole compound relative to 1 mole of repeating unit of polyimide precursor is more preferably 0.0005 moles or more, more preferably 0.0008 moles or more, more preferably 0.001 moles or more, more preferably 1.0 mole or less, more preferably 0.5 moles or less, more preferably 0.1 moles or less, more preferably 0.05 moles or less, and most preferably 0.01 moles or less.

[0160] The addition of imidazole compounds can improve the storage stability of polyimide precursor compositions, which is particularly advantageous from the viewpoints of transportation, distribution, and storage. Storage stability may be especially improved when the polyimide-converted mass concentration (solids concentration) is high, particularly when applied to solutions in which the solids concentration in the composition is 10% by mass or more, preferably 15% by mass or more.

[0161] Properties of Polyimide Precursor Compositions

[0162] There is no particular limitation on the concentration of the polyimide precursor in the polyimide precursor composition, but it is typically 5% to 45% by mass, preferably 8% to 25% by mass, and more preferably 10% to 20% by mass, based on the mass concentration converted from polyimide (hereinafter also referred to as the solids concentration). Here, the mass converted from polyimide refers to the mass when all repeating units are completely imidized. Generally, since the polyimide precursor composition is obtained by reacting the tetracarboxylic acid component and the diamine component in a solvent in a specified amount and using them as is, the solids concentration of the polyimide precursor composition is approximately equal to the amount of tetracarboxylic acid component and the diamine component added. The concentration can also be adjusted by diluting or concentrating the solution as needed.

[0163] While there are no particular limitations on the viscosity (rotational viscosity) of the polyimide precursor composition of the present invention, an E-type rotational viscometer was used at a temperature of 25°C and a shear rate of 50 sec. -1 The rotational viscosity measured is preferably from 0.01 to 1000 Pa·sec, more preferably from 0.1 to 100 Pa·sec, even more preferably from 0.5 to 20 Pa·sec, and even more preferably from 1 to 10 Pa·sec. Furthermore, thixotropy may be imparted as needed. When the viscosity is within the above range, the composition is easy to handle during coating or film formation, the varnish exhibits less rejection and excellent leveling properties, thus a good film can be obtained.

[0164] The fabrication of the membrane will be described in detail later. The polyimide precursor composition is cast onto a support substrate, and imidization and desolventization are performed by heat treatment to form a polyimide film, thereby obtaining a laminate of the support substrate and the polyimide film (polyimide film / substrate laminate).

[0165] In the process of forming films during device manufacturing, coating machines such as slit coaters with slits as discharge outlets are used. Generally, if the viscosity is too high, discharge becomes difficult, or the coating speed decreases, leading to a reduction in production throughput; conversely, if the viscosity is too low, stable casting may become difficult. Therefore, the polyimide precursor composition used in the industrial device manufacturing process needs to have an appropriate viscosity that matches the slit spacing, and the thickness of the cast film is affected by the viscosity. On the other hand, since the thickness of the polyimide film depends on the product of the solids concentration of the polyimide precursor composition and the thickness of the cast film, if the concentration is made too low in order to adjust to a suitable coating viscosity, it becomes impossible to manufacture a polyimide film with the specified thickness. In this invention, by using a mixed solvent selected from "solvent A and solvent B of this application," an appropriate solids concentration can be achieved at an appropriate viscosity.

[0166] The polyimide precursor composition using this mixed solvent also exhibits excellent viscosity stability. Variations in viscosity can cause changes in the thickness of the cast film, which in turn affects the thickness of the polyimide film, or necessitates significant adjustments to the coating machine settings, thus causing practical problems. The polyimide precursor composition using this mixed solvent is more stable than compositions using only solvent A or only solvent B, and preferably more stable than both compositions using only solvent A and compositions using only solvent B. For example, if a composition containing only solvent A is more stable than a composition containing only solvent B, then a composition using a mixed solvent containing both solvent A and solvent B exhibits equal or higher stability than a composition containing only solvent A.

[0167] Viscosity stability can be evaluated, for example, based on the viscosity of the polyimide precursor composition 30 days after preparation, relative to its viscosity immediately after preparation.

[0168] The polyimide precursor composition of the present invention may contain, as needed, chemical imidizing agents (acetic anhydrides such as acetic anhydride, and amine compounds such as pyridine and isoquinoline), antioxidants, ultraviolet absorbers, fillers (including inorganic particles such as silica), dyes, pigments, coupling agents such as silane coupling agents, primers, flame retardants, defoamers, leveling agents, rheology control agents (flow promoters), etc.

[0169] In the presence of an imidazole compound, the composition can be prepared by adding and mixing an imidazole compound or a solution of an imidazole compound into the polyimide precursor composition obtained after the reaction, and then mixing them. Alternatively, the tetracarboxylic acid component can be reacted with the diamine component in the presence of the imidazole compound.

[0170] <<Applications of Polyimide Precursor Compositions and Physical Properties of Membranes>>

[0171] Polyimides and polyimide films can be manufactured using the polyimide precursor compositions of the present invention. There are no particular limitations on the manufacturing method; any known imidization method can be appropriately applied. The resulting polyimides can be in the form of films, laminates of polyimide films with other substrates, coatings, powders, beads, molded bodies, foams, etc.

[0172] Depending on the application, the thickness of the polyimide film is preferably 1 µm or more, more preferably 2 µm or more, even more preferably 5 µm or more, and for example, 250 µm or less, preferably 150 µm or less, more preferably 100 µm or less, even more preferably 50 µm or less.

[0173] The polyimide film of the present invention exhibits excellent light transmittance, mechanical properties, thermal properties, and heat resistance (glass transition temperature, thermal decomposition resistance); in particular, at least one of light transmittance and thermal decomposition resistance is improved, and in the preferred embodiment, both are improved. Here, "heat resistance" is related to phase transition (expressed by glass transition temperature, melting temperature, etc.) and thermal decomposition (expressed by weight loss). Since these are different phenomena, they are not directly related. The polyimide and polyimide film of the present invention are excellent in both glass transition temperature (Tg) and thermal decomposition resistance.

[0174] TFTs used in displays such as liquid crystal displays (LCDs) and organic EL displays include amorphous silicon TFTs (a-Si TFTs), low-temperature polycrystalline silicon TFTs (LTPS TFTs), high-temperature polycrystalline silicon TFTs, and oxide TFTs. In particular, high-temperature film deposition is advantageous for forming semiconductor layers with high charge mobility. Amorphous silicon TFTs, which can be deposited at relatively low temperatures, require a film deposition temperature of 300°C to 400°C, while low-temperature polycrystalline silicon TFTs require a film deposition temperature below 600°C (e.g., around 500°C).

[0175] If the polyimide film lacks sufficient resistance to thermal decomposition, for example, during TFT formation, degassing caused by polyimide decomposition may lead to bulging between the polyimide film and the barrier film, or contaminate the manufacturing equipment. As a substrate for flexible electronic devices, a film that is stable at high temperatures, i.e., exhibits excellent resistance to thermal decomposition and minimal degassing at the process temperature, is preferred. From a process margin perspective, a film with a higher thermal decomposition (initiation) temperature is preferred, even if the difference is very small (e.g., around 2°C).

[0176] The thermal decomposition resistance of polyimide films (or the polyimides constituting them) can be evaluated, for example, based on the 0.5% weight loss temperature, 1% weight loss temperature, 5% weight loss temperature, etc., of the polyimide film. When slight degassing is a concern, it is generally preferred to use indicators of minute weight loss, such as 0.5% or 1% weight loss temperature, for evaluation.

[0177] In one embodiment of this application, compared to examples using only solvent A and / or (preferably "and") only solvent B, the 0.5% weight loss temperature of examples using a mixed solvent of solvent A and solvent B of the present invention is preferably 1°C or higher, more preferably 2°C or higher, and even more preferably 3°C or higher. However, if other evaluation indicators such as light transmittance at 450 nm are excellent, the 0.5% weight loss temperature of examples using a mixed solvent can be comparable to that of examples using only solvent A or solvent B, and in some cases, even a difference of about 2°C is acceptable.

[0178] The 1% temperature of weight loss can be evaluated in the same way.

[0179] If solvent A is a solid at room temperature (e.g., 25°C), the above-mentioned improvement is preferably achieved relative to instances where only solvent B is used.

[0180] Furthermore, compared to examples using only NMP as a solvent, the 0.5% weight loss temperature of examples using a mixed solvent of solvent A and solvent B is preferably improved with the same temperature difference as described above. However, since the absence of NMP is also a significant advantage, the 0.5% weight loss temperature of examples using this mixed solvent is acceptable compared to examples using only NMP. For example, the reduction is preferably controlled within about 5°C, more preferably within 3°C, and more preferably within 2°C.

[0181] The 1% temperature of weight loss can be evaluated in the same way.

[0182] In one embodiment of the invention, for example in a system using DMI and DMPA in combination, the 0.5% weight loss temperature is preferably above 553°C, more preferably above 554°C, and even more preferably above 555°C. The 1% weight loss temperature is preferably above 575°C, more preferably above 576°C, and even more preferably above 577°C.

[0183] The polyimide film of the present invention has an extremely low coefficient of linear thermal expansion. In one embodiment of the present invention, when measured using a film with a thickness of 10 µm, the coefficient of linear thermal expansion (CTE) of the polyimide film at 150°C to 250°C is preferably less than 20 ppm / K, more preferably less than 20 ppm, further preferably less than 15 ppm / K, and even more preferably less than 11 ppm / K.

[0184] In one embodiment of the present invention, the glass transition temperature (Tg) of the polyimide film (or the polyimide constituting it) is preferably 300°C or higher, more preferably 310°C or higher, and even more preferably 320°C or higher.

[0185] In one embodiment of this application, in an example using a mixed solvent of solvent A and solvent B of the present invention, the light transmittance of the polyimide film at 450 nm, measured using a film with a thickness of 10 µm, is preferably improved by 1% or more, more preferably by 2% or more, compared to an example using only solvent A and / or (preferably "and") only solvent B. However, if other evaluation indicators such as thermal decomposition resistance (0.5% weight loss temperature) are excellent, the light transmittance at 450 nm of the example using the mixed solvent can be comparable to that of the example using only solvent A or only solvent B, and in some cases, even about 2% lower is acceptable.

[0186] If solvent A is a solid at room temperature (e.g., 25°C), the above-mentioned improvement is preferably achieved relative to instances where only solvent B is used.

[0187] Furthermore, compared to the example using only NMP as a solvent, the light transmittance at 450 nm in the example using a mixed solvent of solvent A and solvent B is preferably improved with the same temperature difference as described above. However, since the absence of NMP is also a significant advantage, the light transmittance at 450 nm in the example using this mixed solvent can be comparable to that in the example using only NMP, and a reduction of up to 3%, preferably up to 2%, and more preferably up to 1% is acceptable.

[0188] In one embodiment of the invention, for example in a system using a combination of DMI and DMPA, the light transmittance of a 10 µm thick film at 450 nm is preferably 68% or more, more preferably 69% or more, and even more preferably 70% or more. Furthermore, when measured using a 10 µm thick film, the yellowness index (YI) of the polyimide film is preferably 40 or less, more preferably 35 or less, even more preferably 33 or less, and even more preferably 32 or less. Typically, it is preferably 0 or more.

[0189] In one embodiment of the invention, when measuring using a film with a thickness of 10 µm, the haze value of the polyimide film is preferably less than 1.0%, more preferably less than 0.8%, and even more preferably less than 0.7%. For example, if the haze value exceeds 1%, it is unsuitable for optical applications because the white turbidity is visually identifiable.

[0190] Furthermore, in one embodiment of the present invention, when a film with a thickness of 10 µm is used for measurement, the elongation at break of the polyimide film is preferably greater than 10%, more preferably 15% or more, and even more preferably 20%, 25% or more, and 30% or more in sequence.

[0191] In another preferred embodiment of the invention, the tensile strength of the polyimide film is preferably 150 MPa or more, more preferably 200 MPa or more, even more preferably 220 MPa or more, even more preferably 250 MPa or more, and even more preferably 280 MPa or more. For example, a value obtained from a film with a thickness of about 5 to 100 µm can be used as the tensile strength.

[0192] It is particularly preferred that the desired properties of the polyimide film described above are simultaneously satisfied.

[0193] Polyimide films can be manufactured using known methods. A typical method involves casting a polyimide precursor composition onto a support substrate and then heating and imidizing the support substrate to obtain a polyimide film. This method, combined with the manufacture of a polyimide film / substrate laminate, is described below. Alternatively, a polyimide film can also be obtained by casting a polyimide precursor composition onto a support substrate and heating and drying it to form a self-supporting film, peeling the self-supporting film off the substrate, for example, by holding both sides of the film in a degassed state using a tenter frame and performing thermal imidization.

[0194] <<Fabrication of Polyimide Film / Substrate Laminates and Flexible Electronic Devices>>

[0195] Polyimide film / substrate laminates can be manufactured using the polyimide precursor composition of the present invention. The polyimide film / substrate laminate is manufactured by: (a) coating the polyimide precursor composition onto a support substrate; and (b) heat-treating the polyimide precursor on the support substrate to form a laminate, wherein a polyimide film is laminated on the support substrate (polyimide film / substrate laminate). The method for manufacturing a flexible electronic device of the present invention includes using the polyimide film / substrate laminate manufactured by steps (a) and (b) above, and further includes the steps of: (c) forming at least one layer selected from conductor layers and semiconductor layers on the polyimide film of the laminate; and (d) separating the substrate from the polyimide film.

[0196] First, in step (a), the polyimide precursor composition is cast onto a substrate, and imidized and desolventized by heat treatment to form a polyimide film, thereby obtaining a laminate supporting the substrate and the polyimide film (polyimide film / substrate laminate).

[0197] As the supporting substrate, heat-resistant materials are used, such as plate-shaped or sheet-shaped substrates made of ceramic materials (glass, alumina, etc.), metallic materials (iron, stainless steel, copper, aluminum, etc.), or semiconductor materials (silicon, compound semiconductors, etc.), or film-shaped or sheet-shaped substrates made of heat-resistant plastic materials (polyimide, etc.). Generally, flat and smooth plate-shaped substrates are preferred, typically using: glass substrates such as soda-lime glass, borosilicate glass, alkali-free glass, and sapphire glass; semiconductor (including compound semiconductor) substrates such as silicon, GaAs, InP, and GaN; and metallic substrates such as iron, stainless steel, copper, and aluminum.

[0198] Glass substrates are particularly preferred as supporting materials. Flat, smooth, and large-area glass substrates have been developed and are readily available. The thickness of the plate-like substrate, such as the glass substrate, is not limited, but from the viewpoint of ease of handling, it is, for example, 20 µm to 4 mm, preferably 100 µm to 2 mm. The size of the plate-like substrate is not particularly limited, but one side (the long side in the case of a rectangle) is, for example, about 100 mm to 4000 mm, preferably about 200 mm to 3000 mm, and more preferably about 300 mm to 2500 mm.

[0199] These substrates, such as glass substrates, can have inorganic thin films (e.g., silicon oxide films) or resin films formed on their surfaces.

[0200] There are no particular limitations on the method of casting the polyimide precursor composition onto the substrate, and examples include slot coating, die coating, doctor blade coating, spray coating, inkjet coating, nozzle coating, spin coating, screen printing, bar coating, electrodeposition and other conventionally known methods.

[0201] In step (b), the polyimide precursor composition is heat-treated on a supporting substrate to convert it into a polyimide film, thereby obtaining a polyimide film / substrate laminate. The heat treatment conditions are not particularly limited, but for example, it is preferable to dry the material in a temperature range of 50°C to 150°C, followed by treatment at a maximum heating temperature of, for example, 150°C to 600°C, preferably 200°C to 550°C, and more preferably 250°C to 500°C.

[0202] The thickness of the polyimide film is preferably 1 µm or more, more preferably 2 µm or more, and even more preferably 5 µm or more. If the thickness is less than 1 µm, the polyimide film cannot maintain sufficient mechanical strength, and for example, when used as a substrate for flexible electronic devices, it may not be able to withstand stress and may crack. Furthermore, the thickness of the polyimide film is preferably 100 µm or less, more preferably 50 µm or less, and even more preferably 20 µm or less. As the thickness of the polyimide film increases, it may become difficult to reduce the thickness of the flexible device. In order to make it thinner while maintaining sufficient durability as a flexible device, the thickness of the polyimide film is preferably 2 to 50 µm.

[0203] In this invention, the warpage of the polyimide film / substrate laminate is preferably small. Details of the measurement are described in Japanese Patent No. 6798633. In one embodiment, when evaluating the properties of the polyimide film in the polyimide film / silicon substrate (wafer) laminate by the residual stress between the polyimide film and the silicon substrate, the residual stress is preferably less than 27 MPa. Here, it is assumed that the polyimide film is placed in a dry state at 23°C.

[0204] The polyimide film in the polyimide film / substrate laminate may have a second layer, such as a resin film or an inorganic film, on its surface. That is, after forming a polyimide film on a substrate, a second layer can be laminated to form a flexible electronic device substrate. It preferably has at least an inorganic film, and particularly preferably a film that functions as a barrier layer against water vapor, oxygen (air), etc. Examples of water vapor barrier layers include those containing silicon nitride (SiN). x ), silicon dioxide (SiO) x ), silicon oxynitride (SiO) x N y Inorganic films are composed of inorganic materials from the group consisting of metal oxides, metal nitrides, and metal nitrides, such as alumina (Al₂O₃), titanium dioxide (TiO₂), and zirconium oxide (ZrO₂). Commonly known methods for forming these films include physical vapor deposition (PVD) methods such as vacuum evaporation, sputtering, and ion plating, as well as chemical vapor deposition (CVD) methods such as plasma CVD and catalytic chemical vapor deposition (Cat-CVD). This second layer can also be multilayered.

[0205] When the second layer has multiple layers, resin films and inorganic films can be combined, examples of which include laminates obtained by forming a barrier layer / polyimide layer / barrier layer three-layer structure on a polyimide film in a polyimide film / substrate laminate.

[0206] In step (c), using the polyimide / substrate laminate obtained in step (b), at least one layer selected from conductor layers and semiconductor layers is formed on the polyimide film (including a second layer such as an inorganic film deposited on the surface of the polyimide film). These layers may be formed directly on the polyimide film (including the second layer), or they may be formed on the surface of other deposited (laminated) layers required for the device, i.e., indirectly on the polyimide film.

[0207] For the conductor layer and / or semiconductor layer, the appropriate conductor layer and (inorganic or organic) semiconductor layer are selected according to the components and circuits required by the target electronic device. When forming at least one of the conductor layer and semiconductor layer in step (c) of the present invention, it is also preferable to form at least one of the conductor layer and semiconductor layer on the polyimide film on which the inorganic film has been formed.

[0208] The conductor layer and semiconductor layer include layers formed on the entire surface of the polyimide film and layers formed on a portion of the polyimide film. In this invention, step (d) can be performed immediately after step (c), or step (d) can be performed after forming at least one layer selected from the conductor layer and semiconductor layer in step (c) and forming other device structures after step (c).

[0209] When manufacturing a TFT liquid crystal display device as a flexible device, metal wiring, TFTs made of amorphous silicon or polycrystalline silicon, and transparent pixel electrodes are formed, for example, on a polyimide film on which an inorganic film is formed over the entire surface, as needed. The TFT includes, for example, a gate metal layer, a semiconductor layer (e.g., an amorphous silicon film), a gate insulating layer, and wiring connected to the pixel electrodes. The required structure for a liquid crystal display can then be formed on top of this using known methods. Furthermore, transparent electrodes and color filters can also be formed on the polyimide film.

[0210] In the manufacture of organic EL displays, transparent electrodes, light-emitting layers, hole transport layers, electron transport layers, etc., are formed on polyimide films on which inorganic films are formed throughout the entire surface, as required, and TFTs are formed as required.

[0211] Since the polyimide film preferred by the present invention has excellent properties such as heat resistance and toughness, there are no particular limitations on the methods for forming the circuits, components and other structures required for the device.

[0212] Next, in step (d), the supporting substrate is separated from the polyimide film. The separation method can be a mechanical separation method, which physically separates the substrate by applying external force, or a so-called laser separation method, which separates the substrate by applying a laser beam from the substrate surface.

[0213] After separating the support substrate, the device is completed by forming or assembling the required structure or components on a (semi) article having a polyimide film as a substrate.

[0214] As another method for manufacturing flexible electronic devices, after manufacturing a polyimide film / substrate laminate and separating the polyimide film by step (b) above, at least one layer selected from conductor layers and semiconductor layers and the necessary structure are formed on the polyimide film as described in step (c) above, thereby enabling the manufacture of (semi) products using the polyimide film as a substrate.

[0215] Example

[0216] The present invention will be further described below with reference to embodiments and comparative examples. However, the present invention is not limited to the embodiments described below.

[0217] In the following embodiments, the evaluation was performed using the following methods.

[0218] Evaluation of Polyimide Films

[0219] [Light transmittance at 450 nm]

[0220] The light transmittance of a 10 µm thick polyimide film at 450 nm was determined using a UV-Vis spectrophotometer V-650DS (manufactured by JASCO Corporation).

[0221] [0.5%, 1%, 5% temperature of weight loss]

[0222] A polyimide film with a thickness of approximately 10 µm was used as the specimen. A thermogravimetric analyzer (Q5000IR) manufactured by TA Instruments Inc. was used to heat the film from 25 °C to 600 °C in a nitrogen atmosphere at a heating rate of 10 °C / min. Using the weight at 150 °C as 100%, the 0.5%, 1%, and 5% weight loss temperatures were determined from the resulting weight curves.

[0223] Evaluation of Polyimide Precursor Compositions (Varnish)

[0224] Viscosity determination of polyimide precursor compositions

[0225] Using a TV-22E rotational viscometer manufactured by Toki Sangyo Co., Ltd., at a temperature of 25°C and a 50-second interval... -1The rotational viscosity of the polyimide precursor composition (varnish) was determined at a shear rate of 0.

[0226] The "viscosity retention rate (%)" was calculated by dividing the viscosity after 30 days of storage at 23°C by the viscosity of the freshly prepared varnish, and was used to evaluate "viscosity stability". For samples where a significant decrease in viscosity was observed before the 30-day period, viscosity stability was evaluated based on the viscosity retention rate at that time point (and rated as "poor viscosity stability").

[0227] <Ingredients>

[0228] The abbreviations of the raw materials used in the following embodiments are as follows.

[0229] [Diamine component]

[0230] PPD: p-phenylenediamine

[0231] [Tetracarboxylic acid component]

[0232] s-BPDA: 3,3',4,4'-Biphenyltetracarboxylic acid dianhydride

[0233] [solvent]

[0234] DMI: 1,3-Dimethyl-2-imidazolidineone

[0235] NBP: 1-Butyl-2-pyrrolidone

[0236] MPA: 3-Methoxy-N,N-Dimethylpropionamide

[0237] DMPA: N,N-Dimethylpropionamide

[0238] NMP: N-methyl-2-pyrrolidone

[0239] <Example 1>

[0240] [Preparation of polyimide precursor compositions]

[0241] 10.8 g (0.1 mol) of PPD was added to a reaction vessel purged with nitrogen, and solvents A and B were added to form a mixed solvent containing 75% by mass of 1,3-dimethyl-2-imidazolium ketone (DMI) as solvent A and 25% by mass of N,N-dimethylpropionamide (DMPA) as solvent B. The total mass of solvents A and B was 292.9 g, which resulted in a total mass of 12% by mass of the monomers added (the sum of the diamine and carboxylic acid components). The mixture was then stirred at room temperature for 3 hours. 29.1 g (0.1 mol) of s-BPDA was then gradually added to the solution. After stirring at room temperature for 12 hours, a homogeneous and viscous polyimide precursor composition was obtained.

[0242] The initial viscosity (viscosity immediately after preparation) of the obtained polyimide precursor composition was measured, and then stored in a sealed container filled with nitrogen at 23°C. The "viscosity retention rate (%)" was calculated by dividing the viscosity measured 30 days after the start of storage by the initial viscosity, and was used as an indicator of viscosity stability. The results are shown in Table 1.

[0243] [Manufacturing of polyimide films]

[0244] A 6-inch Eagle-XG (registered trademark) glass substrate (500 µm thick) manufactured by Corning was used as the glass substrate. A polyimide precursor composition was coated onto the glass substrate, and the substrate was thermally imidized by heating from room temperature to 430°C under a nitrogen atmosphere (oxygen concentration below 200 ppm) to obtain a polyimide film / substrate laminate. The laminate was then immersed in water at 40°C (e.g., a temperature range of 20°C to 100°C) to separate the polyimide film from the glass substrate. After drying, the properties of the polyimide film were evaluated. The film thickness of the polyimide film was approximately 10 µm. The evaluation results are shown in Table 1.

[0245] <Examples 2 to 38, Comparative Examples 1 to 12 and Reference Example 1>

[0246] The polyimide precursor composition was obtained in the same manner as in Example 1, except that the solvent composition was changed to those described in Tables 1 to 7 while maintaining the same varnish concentration (monomer concentration). Subsequently, polyimide films were prepared in the same manner as in Example 1, and the film properties were evaluated in the same manner. The results are shown in Tables 1 to 7. The values ​​listed for the dianhydride items in the tables represent the content of each component relative to 100 mol% of the total dianhydride. The values ​​listed for the diamine items in the tables represent the content of each component relative to 100 mol% of the total diamine. The values ​​listed for the solvent items in the tables represent the content of each solvent relative to 100 wt% of the total solvent. For the examples listed in Table 1, the viscosity stability of the obtained polyimide precursor compositions was evaluated in the same manner as in Example 1.

[0247] <Examples 39 to 58, Comparative Examples 13 to 17 and Reference Example 2>

[0248] The polyimide precursor composition was obtained in the same manner as in Example 1, except that the monomer composition and solvent of Example 1 were changed to those described in Tables 8 to 10. Subsequently, polyimide films were prepared in the same manner as in Example 1, and the film properties were evaluated in the same manner. The results are shown in Tables 8 to 10. The values ​​in the tables represent the content of each component in the same way as in Tables 1 to 7.

[0249] <Evaluation Results>

[0250] In the embodiments using the mixed solvent specified in this application, at least one of the following was improved compared to the comparative examples using a single solvent: 0.5% weight loss temperature (thermal decomposition resistance) and light transmittance at 450 nm. In systems using s-BPDA and PPD as monomers, the embodiments using DMI as solvent A (Examples 1 to 3) exhibited superior properties even compared to Reference Example 1 using NMP as solvent. Viscosity stability was also not an issue. Furthermore, the system using ODPA and PPD as monomers exhibited superior properties even compared to Reference Example 2 using NMP as solvent.

[0251] [Table 1]

[0252] Note: The viscosity stability of Comparative Example 2 indicates the viscosity retention rate after day 16.

[0253] [Table 2]

[0254] [Table 3]

[0255] [Table 4]

[0256] [Table 5]

[0257] [Table 6]

[0258] [Table 7]

[0259] [Table 8]

[0260] [Table 9]

[0261] [Table 10]

[0262] Industrial availability

[0263] This invention is applicable to the manufacture of flexible electronic devices, such as display devices like liquid crystal displays, organic EL displays, and electronic paper, as well as light-receiving devices like solar cells and CMOS sensors.

Claims

1. A polyimide precursor composition comprising: A polyimide precursor having repeating units represented by the following general formula (I); Solvent A is selected from at least one solvent A chosen from the group consisting of 1,3-dimethyl-2-imidazolidineone, 3-methoxy-N,N-dimethylpropionamide, 1-butyl-2-pyrrolidone, N,N-diphenylformamide, N,N-diethylbenzamide, benzoylaniline, and 1-phenyl-2-pyrrolidone; and Solvent B is selected from at least one solvent chosen from the group consisting of N,N-dimethylpropionamide, N,N-diethylformamide, N,N-diethylacetamide, N,N-dimethylisobutyramide, N,N-diethylpropionamide, and tetramethylurea. [Chemistry 1] in, In general formula I, X1 is a tetravalent aliphatic or aromatic group, Y1 is a divalent aliphatic or aromatic group, and R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms. Where X1 comprises more than 50 mol% aromatic groups and / or Y1 comprises more than 50 mol% aromatic groups.

2. The polyimide precursor composition of claim 1, wherein, X1 comprises 50 mol% or more of the structure represented by formula (II-1) and / or formula (II-2), and Y1 with a molar percentage of 50% or more is the structure represented by formula (III). [Chemistry 2] [Chemistry 3] 。 3. The polyimide precursor composition according to claim 1, wherein the total amount of solvent A and solvent B is 80% or more of the total mass of the solvents.

4. The polyimide precursor composition of claim 1, wherein, Based on the total mass of solvent A and solvent B, the mass of solvent A is greater than 1% by mass and less than 90% by mass.

5. The polyimide precursor composition of claim 1, wherein, Solvent A and solvent B are selected from the following combinations (a) to (g): (a) Solvent A comprises 1,3-dimethyl-2-imidazolidineone, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (b) Solvent A comprises 1-butyl-2-pyrrolidone, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (c) Solvent A comprises 3-methoxy-N,N-dimethylpropionamide, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (d) Solvent A comprises 1-phenyl-2-pyrrolidone, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (e) Solvent A comprises N,N-diphenylformamide, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; (f) Solvent A comprises N,N-diethylbenzamide, and solvent B comprises N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide; and (g) Solvent A contains benzoylaniline, and solvent B contains N,N-dimethylpropionamide, tetramethylurea, or N,N-dimethylisobutyramide.

6. The polyimide precursor composition of claim 1, wherein, The polyimide obtained from the polyimide precursor composition has a 0.5% weight loss temperature higher than (i) and (ii) below, or higher than (ii) when solvent A is solid at 25°C: (i) The 0.5% weight loss temperature of the polyimide obtained from the polyimide precursor composition using a solvent containing only solvent A; (ii) The 0.5% weight loss temperature of the polyimide obtained from the polyimide precursor composition using a solvent containing only solvent B.

7. The polyimide precursor composition of claim 1, wherein, The polyimide film with a thickness of 10 µm obtained from the polyimide precursor composition has a light transmittance at a wavelength of 450 nm that is higher than that described in (i) and (ii), or higher than that described in (ii) when the solvent A is solid at 25°C: (i) The light transmittance at 450 nm of the polyimide film obtained by using the polyimide precursor composition containing only solvent A; (ii) The light transmittance at 450 nm of the polyimide film obtained by using the polyimide precursor composition with a solvent containing only solvent B.

8. A polyimide film obtained from the polyimide precursor composition according to any one of claims 1 to 7.

9. A polyimide film / substrate laminate, comprising: Polyimide films obtained from the polyimide precursor compositions of any one of claims 1 to 7; and Support substrate.

10. The laminate as claimed in claim 9, wherein, The supporting substrate is a glass substrate.

11. A method for manufacturing a polyimide film / substrate laminate, comprising the following steps: (a) Applying the polyimide precursor composition of any one of claims 1 to 7 onto a support substrate; as well as (b) The polyimide precursor on the support substrate is heat-treated to form a laminate containing a polyimide film on the support substrate.

12. The method of claim 11, wherein, The supporting substrate is a glass substrate.

13. A flexible electronic device comprising the polyimide film of claim 8.

14. A method for manufacturing a flexible electronic device, comprising the following steps: (a) Applying the polyimide precursor composition of any one of claims 1 to 7 onto a support substrate; (b) The polyimide precursor on the support substrate is heat-treated to obtain a polyimide film / substrate laminate, wherein the polyimide film is laminated on the support substrate; (c) Forming at least one layer selected from conductor layers and semiconductor layers on the polyimide film of the laminate; and (d) Separate the supporting substrate from the polyimide film.

15. The method of claim 14, wherein, The supporting substrate is a glass substrate.

Citation Information

Patent Citations

  • Polyimide precursor, polyimide, varnish, polyimide film, and substrate

    WO2014038715A1

  • Method for producing polyimide film

    WO2015186782A1