Cu-based alloy having electromagnetic wave shielding function and electromagnetic wave shielding member using the same
By adding ferromagnetic elements such as Fe, Co, and Ni to the Cu matrix and forming spherical or fragmented precipitates with Si, the problems of magnetic noise shielding effect and machinability of Cu-based alloys in electromagnetic wave shielding are solved, achieving efficient electromagnetic wave shielding and excellent mechanical properties.
Patent Information
- Application Number
- CN202580003945.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-03-20
- Filing Date
- 2025-12-10
- Publication Date
- 2026-11-20
AI Technical Summary
Existing Cu-based alloys have problems such as weak magnetic noise shielding effect, heat generation and corrosion in electromagnetic wave shielding, and it is difficult to achieve a fine and uniform particle distribution, which leads to limitations in machinability and mechanical properties.
By adding ferromagnetic elements Fe, Co, and Ni to a Cu matrix and utilizing the negative mixing enthalpy relationship of Si to form spherical or fragmented dendritic precipitates, combined with casting and thermomechanical processing, an alloy with excellent electromagnetic wave shielding function was prepared.
It achieves efficient electromagnetic wave shielding capability, while improving the workability and mechanical properties of the alloy, reducing heat generation and corrosion risks, and possessing economic competitiveness.
Smart Images

Figure CN123146702A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a Cu-based alloy with electromagnetic wave shielding function, its preparation method, and electromagnetic wave shielding components using the Cu-based alloy. This invention claims priority to Korean Patent Application No. 10-2025-0036016, filed with the Korean Patent Office on March 20, 2025, the entire contents of which are incorporated herein by reference. Background Technology
[0002] Electromagnetic shielding aims to protect the internal components of equipment and block external interference, typically achieved using materials that prevent electromagnetic interference. As mentioned above, electromagnetic shielding often utilizes a metal mesh placed around the interior of equipment potentially susceptible to electromagnetic interference to absorb interference propagating through the air. Historically, metal meshes like copper (Cu), aluminum (Al), or iron (Fe) have been used.
[0003] Among such metallic materials, non-ferrous metals, represented by Cu, are effective at shielding electrical noise, but are known to be relatively weak at shielding magnetic noise. On the other hand, while Fe is effective at shielding magnetic noise, it generates heat when interacting with electromagnetic waves and is prone to corrosion.
[0004] To overcome this problem, the method of using alternating stacked Cu foil and Fe foil has been analyzed, but this method is very cumbersome and results in high costs, thus limiting its commercialization.
[0005] As an effective way to achieve the above-mentioned electromagnetic wave shielding, research has been conducted in recent years to approach the electromagnetic wave shielding described above by developing the composition of alloys.
[0006] In particular, in recent years, alloying Cu with Fe has resulted in the fine and uniform distribution of Fe-rich particles within the Cu matrix, thus actively developing alloys for effective electromagnetic wave shielding. However, to date, when particles precipitate in cast microstructures, they grow in a columnar dendritic morphology, limiting isotropic properties and restricting the achievement of fine and uniform particle distribution. Therefore, there is a need to develop an alloy composition and preparation method that can achieve a fine and uniform distribution of spherical precipitates within a Cu matrix. Summary of the Invention
[0007] (a) Technical problems to be solved The purpose of this invention is to add a ferromagnetic element to Cu that is ferromagnetic at room temperature and has a positive enthalpy of mixing with Cu, and can form a second precipitate phase through phase separation. By utilizing the negative enthalpy of mixing relationship and solid solubility between the ferromagnetic element and Si, a composition is proposed that allows the second precipitate phase rich in ferromagnetic elements to precipitate in the form of spherical or fragmented dendritic particles.
[0008] The present invention also aims to identify the optimal combination of composition and process conditions for alloys that can be used as electromagnetic wave shielding components by confirming that solid solutions containing the ferromagnetic elements on a Cu matrix can form fine precipitate phase regions when using different processes.
[0009] Another object of the present invention is to provide a composition that, by further including elements that influence the spheroidization of precipitates, forms spherical precipitate particles in the casting structure.
[0010] Furthermore, the purpose of this invention is to solve the above-mentioned problems and provide a novel alloy composition with excellent electromagnetic wave shielding function, as well as excellent processability, mechanical properties and price competitiveness, and an electromagnetic wave shielding component made of composite material using the alloy.
[0011] However, the technical problems to be solved by the present invention are not limited to the above-mentioned contents, and other technical problems not mentioned can be clearly understood by those skilled in the art through the following description.
[0012] (II) Technical Solution To address the aforementioned technical problems, one aspect of the present invention provides an electromagnetic wave shielding alloy comprising: a first phase, the first phase being composed of a Cu matrix; and a second precipitated phase, the second precipitated phase being rich in one or more ferromagnetic elements selected from Fe, Co, and Ni, wherein the second precipitated phase comprises spherical or fragmented dendritic precipitates.
[0013] According to one embodiment, the second precipitated phase may further contain Si.
[0014] According to one embodiment, the alloy may have a composition represented by Formula 1.
[0015] [Formula 1] Cu x TM 100-x-y Si y In Formula 1, TM must contain one or more selected from Fe, Co and Ni, and selectively contain one or more selected from Cr, Mn, V, Mg, Zn, Ta and Bi, where x is 51-94% by weight and y is 0.1-5% by weight.
[0016] According to one embodiment, in Formula 1, TM may contain Fe, Ni and Co in a total content of 50 atomic% (at.%) or more.
[0017] According to one embodiment, the alloy can be obtained solely through a casting process, without requiring a thermomechanical processing (TMT) process.
[0018] According to one embodiment, the alloy can be obtained by simultaneously performing a casting process and a thermomechanical processing (TMT) process.
[0019] According to one embodiment, the alloy may comprise an FCC structure of a Cu matrix first phase.
[0020] According to one embodiment, in a second precipitated phase rich in one or more ferromagnetic elements selected from Fe, Co and Ni, the total content of Fe, Co and Ni in the second precipitated phase can be 50 atomic% or more.
[0021] According to one embodiment, the second precipitated phase may not contain columnar dendrite (CD) precipitates with an equivalent circular diameter greater than 10 μm.
[0022] According to one embodiment, the equivalent circular diameter of the precipitated particles of the second precipitated phase can be less than 10 μm.
[0023] According to one embodiment, the TM can be Fe. That is, the alloy can have a composition of Cu. x Fe 100-x-y Si y The composition can be represented as x, which can be 51-94% by weight, and y, which can be 0.1-5% by weight.
[0024] According to one embodiment, when the TM is Fe, the second precipitated phase may comprise one or more of the following phases: Fe solid solution, FeSi, Fe2Si, Fe3Si, and Fe5Si3.
[0025] According to one embodiment, when the TM is Fe, the x can be 70-92% by weight and the y can be 0.2-3.4% by weight.
[0026] According to one embodiment, when TM is Fe, the ΔT (liquid phase temperature (T) of the electromagnetic wave shielding alloy L Fe precipitation phase formation temperature (T) Fe It can be below 150K.
[0027] According to one embodiment, the TM may consist of three or more elements, and the three or more elements may constitute a complex concentrated alloy (CCA).
[0028] According to one embodiment, when the TM is composed of three or more elements, the second precipitated phase may include one or more of the following phases: FCC CCA solid solution, (CCA)Si, (CCA)2Si, (CCA)3Si, and (CCA)5Si3.
[0029] According to one embodiment, when the TM contains one or more of Mg, Zn, Ta and Bi, the total content of Mg, Zn, Ta and Bi relative to the total weight of the TM can be less than 5% by weight.
[0030] Another aspect of the present invention provides a method for preparing an electromagnetic wave shielding alloy, comprising the following steps: melting Cu metal; adding a metallic element comprising one or more ferromagnetic elements selected from Fe, Co and Ni and Si to the molten Cu metal; and casting the molten alloy and then cooling it.
[0031] According to one embodiment, the metallic element may further include one or more elements selected from Cr, Mn, V, Mg, Zn, Ta, and Bi.
[0032] According to one embodiment, the prepared alloy can be an electromagnetic wave shielding alloy according to one embodiment of the present invention described above.
[0033] According to one embodiment, the step of cooling the molten alloy after casting can be a step of cooling after casting in a single liquid phase region above the solubility gap. More specifically, the cooling can be carried out through the solubility gap. In detail, an alloy that has been melted and formed into a sufficiently uniformly distributed composition in a single liquid phase region will separate into two liquid phases, one rich in Cu and the other in Fe, after a cooling process through the solubility gap. The Cu-rich liquid phase can then form the matrix phase, and the Fe-rich liquid phase can form the precipitated phase.
[0034] According to one embodiment, cooling of the solubility gap can reduce ΔT (= liquid phase-liquid phase separation temperature (T)). L Fe precipitation phase formation temperature (T) Fe It meets the requirement of being below 150K.
[0035] According to one embodiment, after the step of cooling the molten alloy after casting, a post-processing step of performing thermomechanical machining (TMT) may be further included.
[0036] Another aspect of the present invention provides an electromagnetic wave shielding component comprising an alloy and a polymer resin according to an embodiment of the present invention.
[0037] (III) Beneficial Effects This invention proposes a novel alloy composition that has not been previously proposed, which enables spherical or fragmented dendritic precipitates to be finely and uniformly distributed in a Cu matrix. Furthermore, through a second precipitate phase with excellent magnetic shielding capabilities, it provides an alloy that improves electromagnetic wave shielding capabilities while exhibiting excellent processability and mechanical properties.
[0038] Specifically, the Cu matrix has high electrical conductivity, which can effectively reflect electromagnetic waves, thereby contributing to the electromagnetic wave shielding capability of the alloy. The second precipitated phase, which is rich in ferromagnetic elements, can absorb magnetic waves that are not reflected on the surface of the Cu matrix, thereby helping to improve the electromagnetic wave shielding capability of the alloy.
[0039] In this invention, a suitable compositional region for forming spherical or fragmented dendritic precipitates in Cu-Fe-Si based alloys was identified. By appropriately controlling the particle distribution and morphology of a second precipitate containing one or more ferromagnetic elements selected from Fe, Co, and Ni, and possessing excellent magnetic shielding capabilities, superior electromagnetic wave shielding effects can be achieved. Furthermore, because the spherical or fragmented dendritic precipitates are finely and uniformly distributed in the matrix, not only is the isotropic electromagnetic wave shielding capability excellent, but the limitations in processability and mechanical properties caused by stress concentration due to columnar dendritic particle morphology can also be overcome.
[0040] Furthermore, the alloy composition proposed in this invention can be used to provide a variety of electromagnetic wave shielding components with high conductivity and excellent electromagnetic wave shielding capabilities.
[0041] However, the effects of the present invention are not limited to those described above, but also include all the effects naturally achieved by the various configurations proposed by the present invention. Attached Figure Description
[0042] Figure 1 Based on one embodiment of the present invention, the three elements Cu, Fe, and Si are used to illustrate the binary phase diagrams of Cu-Fe, Fe-Si, and Si-Cu on the Gibbs Triangle of the Cu-Fe-Si ternary system.
[0043] Figure 2 Cu x Fe 100-x-y Si y Pseudo binary phase diagrams for ternary alloy systems at x = 94 wt%, 90 wt%, 80 wt%, 60 wt%, and 50 wt%.
[0044] Figure 3 To illustrate the phase transformation behavior in alloy systems with additional metallic elements (Co, Ni, Cr, Mn, and Si) in the Cu-Fe base composition, the following are pseudo-binary phase diagrams of the Cu-(FeCoNi), (b) Cu-(FeCoNiCr), (c) Cu-(FeCoNiMn), (d) Cu-(FeCoNiCrMn), (e) Cu-(FeCoNiCrSi), and (f) Cu-(FeCoNiMnSi) multi-element alloy systems.
[0045] Figure 4 The results of analysis using a backscattered electron (BSE) detector in a scanning electron microscope (SEM) are shown for the fine structures of (a) Comparative Example 1, which consists of dendrites and (b) Example 1, which consists of spherical shapes, in the second precipitated phase in the Cu matrix.
[0046] Figure 5 The fine microstructures after casting of (a) Example 4, (b) Example 5, (c) Example 6, (d) Example 8, (e) Example 11 and (f) Example 14 are SEM images showing the morphology of the second precipitated phase formed in the Cu matrix.
[0047] Figure 6 Cu 90 Fe 10-y Si y Pseudo-binary phase diagram of ternary alloy systems.
[0048] Figure 7 SEM images showing the morphology of the second precipitated phase formed in the Cu matrix in experimental examples (Comparative Examples 5 to 8, Examples 19 to 21) of complex enriched alloys (CCA) containing equiatomic ratios in a Cu matrix.
[0049] Figure 8 The XRD analysis results of (a) Example 5, (b) Example 8 and (c) Comparative Example 2 are shown.
[0050] Figure 9 Cu x Fe 99-x Si 1.0 With Cu x Fe 98.6-x Si 1.4 The composition of the ternary alloy system on the pseudo-binary phase diagram, namely (a) the solidification behavior, microstructure differences and final microstructure of Example 4 and (b) Example 5 when cooled in the liquid phase.
[0051] Figure 10 The following figures illustrate ΔT (liquid phase temperature) for Examples 4, 5, 6, 8, 11, 12, 14, and 15. L Fe precipitation phase formation temperature (T) Fe )).
[0052] Figure 11 To illustrate the baseline for further addition of a third element in Cu-Fe-Si or Cu-CCA-Si alloys to control the nucleation and growth rate of the second precipitate phase, i.e., added to the Cu matrix, the following graphs are provided: (a) the effect of each element on nucleation behavior affecting grain size, and (b) the factor (relative columnar growth restriction factor, G) representing the ability of each element to inhibit the growth of columnar fine structures.
[0053] Figure 12 A low-magnification SEM image of the fine structure of Example 30 is shown.
[0054] Figure 13 The images shown are high-magnification SEM images of Example 30 and SEM-EDS elemental mapping images that can confirm the constituent elements of the precipitates formed on the Cu matrix in the microstructure.
[0055] Figure 14 SEM-EDS elemental line scan images are used to confirm the concentration distribution of the second phase precipitated on the Cu matrix in Example 30. Best practice
[0056] The embodiments of the present invention are illustrated for the purpose of explaining the technical concept of the invention. The scope of the invention is not limited to the embodiments presented below or the specific description of these embodiments.
[0057] Unless otherwise defined, all technical and scientific terms used in this invention have the meanings commonly understood by one of ordinary skill in the art to which this invention pertains. All terms used in this invention are chosen for the purpose of clearly illustrating the invention and are not intended to limit the scope of the invention.
[0058] The terms “comprising,” “including,” “possessing,” “having,” etc., used in this invention, unless otherwise stated in the statement or sentence containing such terms, should be understood as open-ended terms that include the possibility of other embodiments.
[0059] Unless otherwise stated, the singular expressions described in this invention may also include the meaning of the plural expressions, and this also applies to the singular expressions recorded in the claims.
[0060] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. Furthermore, in the following description of embodiments, repeated descriptions of the same or corresponding constituent elements may be omitted. However, even if such descriptions are omitted, it does not mean that the constituent element is not included in a particular embodiment.
[0061] Among the various methods of electromagnetic wave shielding through alloys, the importance of research on alloys that simultaneously utilize the advantages of Cu and Fe has become increasingly prominent in recent years.
[0062] Through numerous experiments and studies, the inventors discovered that when casting Cu-10Fe alloys using Cu and Fe, a material is formed in the Cu matrix as a second Fe precipitate through solubility gaps, and this material is effective for electromagnetic wave shielding. This alloy composition not only possesses excellent electromagnetic wave shielding performance but also offers economic advantages. However, in this alloy composition, the formation of columnar dendrites of phase-separated Fe second precipitate in the Cu matrix can lead to reduced machinability due to localized stress concentration during deformation. This results in the problem of severe plastic deformation, which is inherent in the application of electromagnetic wave shielding materials.
[0063] To address this problem, the inventors devised a composition control scheme to ensure workability in Cu-Fe alloys, resulting in a dendritic structure formed by uniform, near-spherical particles precipitating during casting instead of a Fe-rich second precipitate. This led to the completion of this invention.
[0064] Furthermore, embodiments of the present invention aim to depart from the existing Cu-10Fe alloy composition, proposing a combination composition that can achieve optimal electromagnetic wave shielding performance by adjusting the Cu to Fe ratio or by mixing other metallic elements. This allows for the achievement of excellent shielding performance while minimizing heat generation and corrosion issues generated by Fe-based alloys during electromagnetic wave shielding. In particular, electromagnetic wave shielding performance can be maximized by controlling the fine structure of Cu and Fe and ensuring their uniform distribution within the matrix.
[0065] This combination of metal components used for specialized alloy design can be derived from the enthalpy relationship between metals.
[0066] The table above shows the enthalpy of mixing relationships between various dissimilar elements (unit: kJ / mol). This confirms that Cu and Fe have a positive enthalpy of mixing (+13 kJ / mol), and also confirms the enthalpy of mixing relationships for many other metals, such as Cu and Fe with V, Cr, Mb, Mo, Ta, and Mn. Furthermore, it confirms that Fe and Si have a particularly high negative enthalpy of mixing (-35 kJ / mol, approximately twice the enthalpy of mixing between Cu and Si).
[0067] Considering these factors, when alloying with relatively inexpensive Si, the enthalpy difference in mixing between elements separated from the Cu phase and Si is significantly greater than the difference in mixing enthalpy between Cu and Si. Therefore, Si tends to combine with phase-separated elements (e.g., Fe) rather than the Cu matrix. Thus, by adding Si, it is expected to control other alloying components, including Fe (which forms a precipitate phase in the alloys of this invention), to ensure stable alloying.
[0068] By focusing on the mixing enthalpy relationships of these elements, alloy compositions that can achieve the aforementioned objectives can be designed. As an example, among the element groups that have a binary positive mixing enthalpy with Cu, the group of Fe, Co, and Ni, which are ferromagnetic elements, can be initially defined.
[0069] Furthermore, in some embodiments, a large negative enthalpy of mixing relationship between Fe and Si is considered, which can be addressed by adding Si and inducing Fe to form a precipitate together with Si through casting. That is, in some embodiments, the second precipitate may further contain Si.
[0070] In the alloy design described above, the addition of Si, which has a large negative enthalpy of mixing with phase-separating elements (especially Fe), has the effect of suppressing the growth of precipitates formed by phase-separating elements. This can induce the formation of small-sized dendrites, or even completely fragmented dendrites. Alternatively, it can induce preferential bonding between phase-separating elements and Si, causing Fe-rich precipitates to precipitate directly as spherical particles. The growth rate of these spherical, Fe-rich precipitates may be relatively slower.
[0071] Next, in order to achieve a sufficient level of electromagnetic wave shielding in the precipitated phase, the transition metal (TM) can be limited to 50% or more of ferromagnetic elements such as Fe, Ni, and Co.
[0072] The inventors have confirmed that, based on compositional differences, various morphologies of precipitated particles can be obtained during casting in Cu-Fe-Si based alloys. Furthermore, they have classified the regions in the Cu-Fe-Si based alloys that form Fe-rich second precipitates according to the morphology of these precipitates, and this is illustrated in the figures. Figure 1 In order to ensure magnetic shielding capability, the Fe content in the Fe-rich second precipitate is preferably above 50 atomic%, and Fe can be replaced by Co or Ni as ferromagnetic elements.
[0073] The following is for reference Figures 1 to 3 The images shown illustrate in detail the composition proposed in this invention and experimental examples for deriving this composition.
[0074] Figure 1 Based on an embodiment of the present invention, binary phase diagrams of Cu-Fe, Fe-Si, and Si-Cu are shown on a Gibbs triangle of a Cu-Fe-Si ternary system. The inventors have indicated regions where a second precipitate containing Fe-rich and fully fragmented dendritic precipitates forms during casting on a Cu matrix by using diagonal lines, and regions where a second precipitate containing Fe-rich and spherical precipitates forms during casting by using black lines.
[0075] More specifically, Figure 1 The areas filled with diagonal lines within the Gibbs triangle of the Cu-Fe-Si ternary system represent regions where mainly Fe-rich solid solution alloys precipitate without other Fe-Si intermetallic compounds, including the various regions described below according to one embodiment of the invention. The composition indicated by diagonal lines, i.e., 51% to 94% Cu and 0.1% to 5% Si, represents regions where spherical or fragmented dendritic precipitates with an equivalent diameter of 10 μm or less are formed. The areas filled with black, i.e., the composition range of 70% to 92% Cu and 0.2% to 3.4% Si, represents regions where a second precipitate mainly forms spherical precipitates.
[0076] Figure 2 Cu x Fe 100-x-y Si yIn a ternary alloy system, pseudo-binary phase diagrams are shown for x = 94 wt%, 90 wt%, 80 wt%, 60 wt%, and 50 wt%. The calculated phase diagrams indicate the regions expected to form Fe-rich solid solution second precipitates, the regions expected to form M(Fe,Cu)-Si intermetallic compounds, and the regions expected to undergo liquid-liquid phase separation. Specifically, square dashed lines indicate the regions expected to form Fe-rich solid solution second precipitates, dashed lines indicate the regions expected to form M(Fe,Cu)-Si intermetallic compounds, and diagonal lines indicate the regions expected to undergo liquid-liquid phase separation. The compositions within the square dashed lines are most likely to form Fe-rich solid solution second precipitates first upon solidification, and the compositions within the diagonal line regions are highly likely to form spherical Fe-rich solid solution second precipitates. The compositions within the dashed line regions are most likely to form M(Fe,Cu)-Si intermetallic compounds first upon solidification.
[0077] The inventor based on Figure 2 The pseudo-binary phase diagram shown illustrates the alloy composition of this invention.
[0078] Reference Figure 2 Cu x Fe 100-x-y Si y The pseudo-binary phase diagram of the ternary alloy system can define the appropriate Si content that is soluble in Fe, and can predict the characteristics of precipitated phases in each composition region based on the Si content.
[0079] First, in the region where the Cu content (x) is 51-94 wt%, and the Si content (y) is 0.1 wt% or more but less than 5 wt%, a Fe-rich second solid solution precipitate suitable for electromagnetic wave shielding may form. However, when the Cu content (x) is below 51 wt%, an inversion between the first and second phases occurs, potentially changing the precipitate composition from Fe-rich to Cu-rich, which is undesirable. Furthermore, when the Cu content (x) is above 94 wt%, the insufficient fraction of Fe precipitates may reduce the electromagnetic wave shielding capability. Finally, when the Si content (y) is greater than 5 wt%, a Fe-Si based compound phase is mainly formed, potentially leading to a sharp decrease in magnetic shielding capability.
[0080] Additionally, the region with Cu content (x) ranging from 70 wt% to 92 wt% and Si content (y) ranging from 0.2 wt% to 3.4 wt%, i.e. Figure 1In the region filled with black, Fe-rich spherical precipitates can precipitate as a second precipitate phase. During cooling, the Fe-rich second precipitate phase, due to the addition of Si, is easily controlled to have a spherical morphology within the limited solidification range near the solubility gap in the alloy composition of this invention. Furthermore, compared to precipitates with FCC / BCC structures precipitated in Si-free alloys, the growth rate of precipitates with high Si content is significantly reduced. Therefore, within this composition range, a spherical second phase can be precipitated using only a single casting process, thereby achieving superior processing performance and electromagnetic wave shielding capabilities. The second precipitate phase can include spherical particles with a diameter of less than 5 μm or a completely fragmented dendritic morphology with a length of less than 5 μm. Therefore, this composition is likely the most preferred region in Cu-Fe-Si ternary alloys. When the Cu content (x) is less than 70 wt%, excessive Fe content may lead to the formation of coarse precipitates with an equivalent circular diameter greater than 10 μm. Furthermore, when the Cu content (x) is 92 wt% or more, such as… Figure 2 As shown, there is no liquid-liquid phase separation region, making it difficult to form a precipitated phase with an equivalent circular diameter of less than 10 μm.
[0081] According to one embodiment, when the spherical precipitates are not perfectly spherical or have a fragmented dendritic morphology, the size of the precipitates can be evaluated by the equivalent circle diameter (ECD). The equivalent circle diameter and the diameter can be measured by microscopic observation. In this specification, the equivalent circle diameter of a particle refers to the diameter converted to the diameter of a circle with the same area as the actual area of the particle, regardless of its morphology.
[0082] According to one embodiment, the equivalent circular diameter of the precipitated particles of the second precipitated phase can be less than 10 μm. More specifically, the equivalent circular diameter of the second precipitated phase can be 0.1 μm, 0.5 μm or more, or 1 μm or more, and independently, can be less than 10 μm, less than 9 μm, less than 8 μm, less than 7 μm, less than 6 μm, or less than 5 μm.
[0083] As described above, embodiments of the present invention can provide a composition of a Cu-based alloy with excellent electromagnetic wave shielding capabilities, and can prepare an alloy with multiple morphologies of second precipitates in various regions.
[0084] Figure 3To illustrate the phase transformation behavior in alloy systems with additional metallic elements (Co, Ni, Cr, Mn, and Si) in the Cu-Fe base composition, the following are pseudo-binary phase diagrams of the Cu-(FeCoNi), (b) Cu-(FeCoNiCr), (c) Cu-(FeCoNiMn), (d) Cu-(FeCoNiCrMn), (e) Cu-(FeCoNiCrSi), and (f) Cu-(FeCoNiMnSi) multi-element alloy systems.
[0085] Through the above Figure 3 The phase diagrams of the alloy compositions in (a) to (f) confirm that even when at least a portion of Fe is replaced with one or more of Co, Ni, Cr, and Mn to form a complex concentrated alloy (CCA), and when Si is further added, the morphology of the phase diagram remains the same as... Figure 3 The phase diagram is similar to that of the Cu-Fe binary system. This result suggests that, in the corresponding composition, similar to the Cu-Fe binary alloy system, precipitated phases based on phase separation can be controlled. Even when Fe is replaced by the aforementioned elements, Fe, Ni, and Co, as ferromagnetic elements, preferably account for more than 50 atomic percent of the elements other than Cu and Si.
[0086] The embodiment of the Cu-based alloy in which spherical precipitates are formed as the second precipitate phase, as proposed in this invention, is not limited to Cu-Fe-Si ternary alloys. According to one embodiment, in addition to Cu-Fe-Si ternary alloys, the alloy can be constructed by replacing the Fe with a complex enriched alloy (CCA) containing three or more elements selected from the alloying element group consisting of Fe, Co, Ni, V, Cr, and Mn, wherein Fe, Co, Ni, V, Cr, and Mn are third-period transition metals (TM) with atomic radii similar to Fe. In this case, to prevent a decrease in magnetic shielding capability, the content of Fe, Co, and Ni, as ferromagnetic elements, is preferably 50 atomic percent or more. As described above, when a CCA containing three or more elements selected from the alloying element group consisting of Fe, Co, Ni, V, Cr, and Mn is added to replace Fe, the stability of the second precipitate phase is improved due to the increase in configuration entropy, and the precipitation of intermetallic compounds such as silicides can be suppressed, which is therefore preferable. In this case, the further included composition can also form particles of a second precipitate that precipitates together with Fe and Si, and similar results as those in Cu-Fe-Si ternary alloys can be obtained within a similar compositional range.
[0087] To address the aforementioned technical problems, one aspect of the present invention provides an electromagnetic wave shielding alloy comprising: a first phase, the first phase being composed of a Cu matrix; and a second precipitated phase, the second precipitated phase being rich in one or more ferromagnetic elements selected from Fe, Co, and Ni, wherein the second precipitated phase comprises spherical or fragmented dendritic precipitates.
[0088] In one embodiment, the second precipitated phase may further contain Si.
[0089] In this specification, the second precipitated phase rich in ferromagnetic elements can be understood as containing metal elements in which the total content of Fe, Co, and Ni is greater than 50 atomic%.
[0090] Specifically, the alloy may have a composition represented by Formula 1.
[0091] [Formula 1] Cu x TM 100-x-y Si y In Formula 1, TM must contain one or more selected from Fe, Co and Ni, and selectively contain one or more selected from Cr, Mn, V, Mg, Zn, Ta and Bi, where x is 51-94% by weight and y is 0.1-5% by weight.
[0092] 101 In one embodiment, the TM may contain Fe, Ni, and Co with a total content of 50 atomic% or more. By ensuring that the total content of the ferromagnetic elements in the TM is 50 atomic% or more, the second precipitate can be enriched with the ferromagnetic elements. Since the second precipitate remains rich in ferromagnetic (Fe, Co, Ni) elements, the alloy with a uniformly distributed second precipitate can have high magnetic properties. In this invention, by controlling the second precipitate into spherical precipitate particles and uniformly dispersing them throughout the entire alloy region, an alloy with high electromagnetic wave shielding effect can be prepared.
[0093] The composition consists of one or more ferromagnetic elements selected from Fe, Co, and Ni combined with Si in a Cu matrix at room temperature to form spherical or fragmented dendritic precipitates in Cu. In the above composition, fragmented dendritic (FD) morphology or spherical (S) precipitates with an equivalent circular diameter of less than 10 μm can precipitate as a second precipitate phase, thus enabling the formation of alloys with high electromagnetic wave shielding capabilities.
[0094] In the described embodiment, if Si is not added to the alloy composition, columnar dendritic second precipitates with an equivalent circular diameter greater than 10 μm may precipitate simultaneously. In this case, as described above, due to localized stress concentration during alloy processing, it becomes difficult to perform the severe plastic deformation primarily used as an electromagnetic wave shielding component.
[0095] In some experimental examples with specific compositions described below, it was confirmed that the spherical precipitates failed to form uniformly, instead concentrating in certain areas. In such cases, the Fe-rich precipitates, which possess electromagnetic wave shielding capabilities, cannot form uniformly, potentially leading to deterioration of the alloy properties. Furthermore, in some experimental examples with specific compositions, the precipitates may form columnar dendrites (CD) instead of being spherically dispersed. In such cases, it may be difficult to process and shape the specimens, thus reducing the performance and application potential as an electromagnetic wave shielding material.
[0096] Figure 1 In the case of a composition where the black-filled region has x of 70% to 92% by weight and y of 0.2% to 3.4% by weight, a fine microstructure with uniformly dispersed spherical (S) precipitates can be formed, which is therefore more preferable. Thus, in this composition region, an alloy with superior workability and electromagnetic wave shielding capability can be achieved. The second precipitate in this composition may include spherical particles with a diameter of 5 μm or less, or fragmented dendrites (FD) with an equivalent circular diameter of 5 μm or less. In this composition region, the second precipitate can precipitate directly during the casting process. Therefore, in this composition region, no additional subsequent processes are required after the formation of the second precipitate.
[0097] According to one embodiment, the alloy may contain spherical precipitates that have separated into a second precipitate phase. SEM images described later confirm that when the second precipitate phase separates within the solubility gap, a portion of it forms dendrites, and a portion forms spherical precipitates. In another embodiment, irregularly shaped particles may also form. When the second precipitate phase precipitates as columnar dendrites (CD) with an equivalent circular diameter greater than 10 μm, it may present difficulties in molding and processing it as an electromagnetic wave shielding component.
[0098] According to one embodiment, in Formula 1, TM can be Fe. That is, the alloy has a composition of Cu. x Fe 100-x-y Si y The composition is indicated by x, which can be 51-94% by weight, and y, which can be 0.1-5% by weight. When the alloy has a composition of Cu... x Fe 100-x-y Si yWhen the composition is indicated, an alloy with excellent electromagnetic wave shielding performance and competitive price can be provided.
[0099] When TM is Fe, the second precipitated phase may contain one or more of the following phases: Fe solid solution, FeSi, Fe2Si, Fe3Si, and Fe5Si3.
[0100] In some embodiments of the invention, a portion of the total content of Fe, Co, and Ni in the alloy composition can be replaced by Co, Ni, V, Cr, and Mn elements that readily form complex condensed alloys (CCAs). Even in this embodiment, within a similar compositional range, the morphology control of the precipitated phases in the Cu matrix can be achieved to the desired level. Specifically, the number of elements constituting the TM can be three or more, and these three or more elements can constitute a complex condensed alloy (CCA).
[0101] When preparing Cu-TM-Si multi-element alloys, the three or more TM elements can form a second precipitate with Si, and can precipitate as the second precipitate while maintaining the CCA state, without forming individual compounds such as silicides.
[0102] When the number of elements constituting the TM is three or more, and the three or more elements constitute a complex concentrated alloy, the second precipitated phase may include one or more of the following: a CCA solid solution with an FCC structure, (CCA)Si, (CCA)2Si, (CCA)3Si, and (CCA)5Si3.
[0103] The composition of the complex concentrated alloy can have an equiatomic ratio or a non-equiatomic ratio.
[0104] According to one embodiment, the diameter of the spherical precipitates can be less than 5 μm. When the diameter is greater than 5 μm, it may be difficult to uniformly disperse them in the first phase. The diameter of the spherical precipitates can be greater than 0.1 μm.
[0105] According to one embodiment, when the TM contains one or more of Mg, Zn, Ta, and Bi, the total content of Mg, Zn, Ta, and Bi relative to the total weight of the TM can be less than 5% by weight. When these elements form a second precipitate in the Cu matrix, they are expected to simultaneously promote nucleation and inhibit precipitate growth.
[0106] In the described embodiment, metals other than Fe and Si in the Cu matrix can act as dopants or seeders added for a specific purpose.
[0107] Another aspect of the present invention provides a method for preparing an electromagnetic wave shielding alloy, comprising the following steps: melting Cu metal; adding a metallic element comprising one or more ferromagnetic elements selected from Fe, Co and Ni and Si to the molten Cu metal; and casting the molten alloy and then cooling it.
[0108] The step of cooling the alloy after casting can be as follows: arc heating is performed in the single-phase region above the solubility gap of the alloy, and then solidification is carried out by cooling through a copper mold using a drop casting method, thereby precipitating a second precipitated phase.
[0109] At this point, the metallic element may further include one or more elements selected from Cr, Mn, V, Mg, Zn, Ta, and Bi.
[0110] The amounts of ferromagnetic elements, Si, and additional metallic elements added to the molten Cu metal can satisfy the above-described composition of the electromagnetic wave shielding alloy.
[0111] According to one embodiment, the alloy may be an alloy according to one embodiment of the present invention described above.
[0112] According to one embodiment, after the step of casting the alloy, a post-processing step of performing thermomechanical machining may be further included.
[0113] However, the alloy casting method proposed in this invention is not limited to the above-mentioned drop casting method after arc melting. As mentioned above, any conventional alloy casting method that can form spherical precipitates containing Fe on a Cu matrix is within the technical concept of this invention.
[0114] Another aspect of the present invention provides an electromagnetic wave shielding component that may comprise an alloy according to an embodiment of the present invention; and a polymer resin.
[0115] In one embodiment of the present invention, the polymer resin may include one or more of photocurable resins, thermocurable resins, and thermoplastic resins. The polymer resin introduced in this invention can be any material that can be mixed with the alloy to form a component, and its composition is not particularly limited. The electromagnetic wave shielding component, as an example, can be fabricated in the form of a film or cable, but the shape of the component is not particularly limited in this invention.
[0116] The contents mentioned in the electromagnetic wave shielding alloy, the method for preparing the electromagnetic wave shielding alloy, and the electromagnetic wave shielding component of the present invention are equally applicable, provided they do not contradict each other.
[0117] All alloys described below are prepared using parent elements with a purity of 99.9% or higher and are fabricated using an arc melting apparatus, which features rapid cooling and high vacuum to minimize the effects of defects such as oxidation and porosity. Corresponding commercial casting methods can be applied to the preparation of the Cu-TM-Si based casting alloys to be developed in this invention.
[0118] For example, the above alloys can be prepared using a variety of commercial casting processes, such as high-frequency induction melting, which is easy to prepare alloys with uniform microstructures; resistance heating, which allows for precise temperature control; rapid solidification, which is beneficial for forming continuous solid solutions; spark plasma sintering, which allows for precise control of microstructures and preparation of parts with the desired shape; and hot isostatic pressing, which are also easy to prepare.
[0119] All the embodiments described below were prepared using only a simple casting process. However, commercially available thermomechanical processing (TMT) methods for optimizing the mechanical and electromagnetic properties of alloys can be applied to the Cu-TM-Si based cast alloys proposed in this invention.
[0120] For example, rolling, forging, or extrusion can be performed at temperatures above 900°C to facilitate recrystallization, and hot working can be applied to minimize internal defects and stress. To increase strength through work hardening, processes such as room-temperature rolling or wire drawing can be used. Furthermore, various commercial thermomechanical processing methods can be applied as needed, such as cold working, which optimizes microstructure and mechanical properties by combining staged strain control with subsequent heat treatment; annealing and aging processes, which improve mechanical properties by removing internal stress and inducing a uniform distribution of fine precipitates within a temperature range of 300°C to 900°C; multi-stage thermomechanical processing, which forms a uniform microstructure through repeated heat treatment and deformation processes; and severe plastic deformation (SPD) processes, which form ultrafine grains. Detailed Implementation
[0121] The following describes in detail experimental examples of various compositions conducted by the inventors of this invention, along with images of the phase precipitation results observed on the surface and graphs showing the crystal structure test results. The experimental examples described later are the results of observing the crystal structure and the morphology of the second precipitated phase in each composition of various alloys prepared by the inventors, ranging from binary to multi-component alloys, using X-ray diffraction analysis and scanning electron microscopy.
[0122] All alloy samples in the following examples and comparative examples were prepared by weighing appropriate amounts of each metallic element according to the compositions described in Tables 1 to 3 and then melting them together. The molten multi-element alloy was then drop-cast and cooled to room temperature to precipitate a second precipitate. The dispersion and morphology of the second precipitate in the prepared alloy samples were observed.
[0123] The experimental samples presented in Table 1 below can be samples within the composition range proposed in the embodiments of the present invention, or comparative samples of the control group not included in the range. Specifically, the following sample compositions were prepared by changing the contents of other elements while keeping the Cu content fixed at 90% by weight, and observing the crystal structure and particle morphology of the second precipitated phase based on the composition. Based on the particle morphology of the second precipitated phase, columnar dendrites were labeled CD, fragmented dendrites were labeled FD (fragmented dendrite), and spherical particles were labeled S (spherical).
[0124] [Table 1] Comparative Example 1 is [Equation 1]Cu x TM 100-x-y Si y (When TM=Fe) Alloys with x values of 10 wt% and y values of 0 wt% are described in Examples 1 to 15 and Comparative Examples 2 to 4, which are alloy compositions formed according to an experimental example with y values ranging from 0.1 wt% to 7 wt%. Examples 1 to 15, being alloy compositions with y values ranging from 0.1 wt% to 5 wt%, are preferred embodiments where silicide precipitation is suppressed and a fine microstructure consisting of an FCC Cu matrix phase and a Fe-rich BCC precipitate phase. Furthermore, Examples 1 and 5 to 14, being alloy compositions with y values ranging from 0.2 wt% to 3.4 wt%, forming a fine microstructure with a uniformly dispersed spherical (S)BCC Fe precipitate phase, are more preferred embodiments.
[0125] The examples and comparative examples presented in [Table 2] below are experimental results of adding one or more of Co, Ni, V, Cr and Mn to the Cu-Fe-Si ternary alloys in [Table 1] above. The examples and comparative examples presented in [Table 2] are also composed of 90% by weight Cu matrix and 10% by weight of the remaining elements.
[0126] [Table 2] The experimental results of Comparative Examples 5 to 8 confirmed that when Si is not present, columnar dendrites (CD) with an equivalent circular diameter greater than 10 μm or irregularly shaped particles will simultaneously precipitate as a second precipitate in Cu-CCA.
[0127] In the case of Cu-CCA-Si in Examples 16 to 18, Fe-rich second precipitates in the form of spherical particles (S) or fragmented dendritic (FD) were precipitated, thus forming a fine structure similar in composition range to the Cu-Fe-Si ternary alloys proposed in the examples in [Table 1].
[0128] in addition, Figures 4 to 9 SEM images of the fine structure of experimental sample specimens prepared according to the present invention, with each composition present. Among these samples, some are example samples corresponding to the compositional regions of the alloy proposed in this invention, while others are comparative example samples prepared for reference but not corresponding to the compositional regions of the alloy proposed in this invention. Spherical or dendritic precipitation can be confirmed in the surface images of each sample.
[0129] Figure 4 The fine structures of (a) Comparative Example 1 composition formed as columnar dendrites (CD) and (b) Example 1 composition formed as spherical particles in the second precipitate in the Cu matrix are shown, with results analyzed using a backscattered electron (BSE) detector in a scanning electron microscope (SEM). To quantitatively evaluate the diameter of the amorphous dendritic particles containing spherical and fragmented particles, the equivalent circle diameter (ECD), converted to the diameter of a circle with the same area as the actual area of the particles, was used for analysis. Figure 4 As shown, in Comparative Example 1 without added Si, columnar dendrites (CD) with an equivalent circle diameter greater than 10 μm were confirmed to precipitate as the main second precipitate phase. On the other hand, in Example 1, it was confirmed that spherical (S) dendrites with a diameter of 5 μm or less, or fragmented dendrites (FD) with an equivalent circle diameter of 5 μm or less, precipitated relatively uniformly as the second precipitate phase.
[0130] Figure 5SEM images of the morphology of the Fe-rich second precipitate formed in the Cu matrix in (a) Examples 4, (b) Examples 5, (c) Examples 6, (d) Examples 8, (e) Examples 11, and (f) Examples 14. More specifically, in Examples 4 and 14, fragmented dendritic (FD) precipitates with an equivalent circle diameter of less than 10 μm were mainly observed on the Cu matrix. Furthermore, in Examples 5 to 11, spherical precipitates (S) with an equivalent circle diameter of less than 5 μm were mainly precipitated on the Cu matrix. As described above, Examples 5 to 11 all contain compositions in which x values are 70% to 92% by weight and y values are 0.2% to 3.4% by weight in one embodiment of the present invention, which belongs to... Figure 1 The alloy in the area filled with black.
[0131] Figure 6 Cu 90 Fe 10-y Si y A pseudo-binary phase diagram of a ternary alloy system. The diagram shows... Figure 5 The illustrated embodiments provide temperature-dependent equilibrium phase information. More specifically, Embodiment 4 comprises a region in which a Fe-rich second precipitate first forms during solidification. Embodiments 5 to 14 comprise regions in which a Fe-rich second precipitate forms after first passing through a liquid-liquid phase separation region during solidification. Under the latter conditions, when the solidification interval after the liquid-liquid phase separation region is below 150 K, the spherical or fragmented dendritic second phase of the present invention can precipitate. Details will be described later.
[0132] Figure 7 SEM images showing the morphology of the second precipitate formed in the Cu matrix in experimental examples (Comparative Examples 5 to 8, Examples 19 to 21) containing complex concentrated alloys (CCA) with equal atomic ratios in a Cu matrix. Figure 7 The morphology of each of the second precipitates recorded in [Table 2] can be confirmed.
[0133] Figure 8 The XRD analysis results are for (a) Example 5, (b) Example 8, and (c) Comparative Example 2. In all three examples, a Cu peak in the FCC structure as the matrix phase and a Fe peak in the BCC structure as the precipitated phase were observed. In Comparative Example 2, the M(Cu-Fe)-Si intermetallic compound diffraction pattern was further confirmed.
[0134] Figure 9 Cu x Fe 99-x Si 1.0 With Cu x Fe98.6-x Si 1.4 The composition of the ternary alloy system on the pseudo-binary phase diagram, namely (a) Example 4 and (b) Example 5, is shown in the solidification behavior, microstructure differences, and final microstructure during cooling in the liquid phase. More specifically, the solidification behavior of Example 4 is as follows: during the solidification of the single mixed liquid phase of the Cu-Fe-Si ternary alloy, the Fe-rich precipitate first nucleates, and then, due to the diffusion behavior caused by the compositional difference between the precipitate and the liquid phase, it preferentially grows on a specific surface. Therefore, the Fe-rich precipitate in dendritic form preferentially grows and solidifies. Subsequently, the Cu-rich liquid phase region solidifies, and solidification is completed in a two-phase coexistence state. However, at this time, in Example 4 corresponding to the compositional region of the present invention, since the solidification interval for the formation of the second precipitate is short, it mainly precipitates in the form of fragmented dendritic (FD). The solidification behavior of Example 5 is as follows: during the solidification of the single mixed liquid phase of the Cu-Fe-Si ternary alloy, the liquid phase (Cu)-liquid phase (Fe) separation region is reached first, resulting in compositional separation, and then the liquid phase (Fe) preferentially solidifies. In the liquid phase (Cu)-liquid phase (Fe) separation region, the components have separated to near equilibrium. A stable interface with a large compositional deviation exists between the Cu and Fe liquid phases, thus inhibiting dendrite growth. The spherical, Fe-rich precipitates preferentially solidify. At this point, the growth of the spherical precipitates is suppressed when passing through the liquid phase separation region in a relatively short distance, resulting in an equivalent circle diameter of less than 10 μm. Subsequently, the Cu-rich liquid phase solidifies, completing the process in a two-phase coexistence state.
[0135] Figure 10 The following figures illustrate ΔT (liquid phase temperature) for Examples 4, 5, 6, 8, 11, 12, 14, and 15. L Fe precipitation phase formation temperature (T) Fe In these embodiments, the liquid phase temperature (T) L ) is the liquid phase separation temperature (T) LL ).based on Figure 6 SEM images of the embodiments and Figure 7 Cu 90 Fe 10-y Si yThe pseudo-binary phase diagram of the ternary alloy system confirmed the correlation between ΔT and microstructure based on y content. When solidification did not pass through the liquid-liquid phase separation region, Fe-rich second precipitates were mainly formed, resulting in FD-shaped second precipitates with an equivalent circular diameter of 10 μm or less (Examples 1 to 4). Furthermore, it was confirmed that spherical Fe-rich second precipitates could be mainly formed when passing through the liquid-liquid phase separation region and satisfying a composition range of ΔT below 150 K (Examples 5 to 14). In contrast, when passing through the liquid-liquid phase separation region and having ΔT in the range of greater than 150 K and less than 200 K, FD-shaped second precipitates were again formed (Example 15). When ΔT was greater than 200 K, it was confirmed that coarse Fe second precipitates mainly formed as columnar dendrites (CD) were formed (Comparative Examples 2 to 4).
[0136] If the above [Table 2] is a result of confirming the difference between Cu-CCA multi-component alloys with equiatomic ratios and Cu-(CCA+Si) multi-component alloys by comparing comparative examples and embodiments, then the following [Table 3] are embodiments of CCA composed in a non-equiatomic ratio, rather than an equiatomic ratio. The embodiments presented in [Table 3] also consist of 90% by weight of a Cu matrix and 10% by weight of the remaining elements.
[0137] The examples in [Table 3] are also not significantly different from the cases with equal atomic ratios proposed in [Table 2] above, and it can be confirmed that they show a fine structure of precipitated phases similar to the case where only Fe and Si are contained in the Cu matrix.
[0138] [Table 3] Figure 11 To illustrate the baseline for the further addition of a third element in Cu-Fe-Si or Cu-CCA-Si alloys to control the nucleation and growth rate of the second precipitate, i.e., added to the Cu matrix, the following is presented: (a) the effect of each element on the nucleation behavior influencing grain size, and (b) a graph representing the factors (relative to the columnar growth restriction factor (G)) indicating the ability of each element to inhibit the growth of columnar fine structures. Specifically, Figure 11 This is cited from the paper "Grain refinement of DHP copper by elemental additions" published by Balart, MJ et al. in the International Journal of Cast Metals Research, 28(4), pp. 248-256. Figure 11(a) analyzed the elements that promote the nucleation of precipitates in the Cu matrix. For example, elements such as Be, Mg, P, S, Ca, V, Mn, Zn, Sr, As, Se, Zr, Mo, In, Sn, Sb, Te, Ta, Tl, Pb, and Bi, which show grain sizes below the dashed (650 μm) region, can be expected to promote the nucleation of the second precipitate when further added to the Cu matrix. That is, adding such elements can be expected to reduce the Cu grain size and delay the growth of the second precipitate.
[0139] In addition, through Figure 11 In (b), based on the factor representing the ability of each element to inhibit the growth of columnar fine structures (relative columnar growth restriction factor (G)), elements that can relatively inhibit the growth of the second phase were analyzed. For example, elements below the region indicated by the dashed line (G value of 12), such as Li, Mg, Al, Fe, Mn, Cr, V, Zn, Ce, Ba, W, Ta, Au, and Bi, can be expected to inhibit the growth of columnar crystals in the Cu matrix and delay the growth of the second precipitated phase.
[0140] Figure 11 In both charts, the elements located below the dashed line indicate that they can simultaneously promote nucleation and inhibit growth; Mg, V, Mn, Zn, Ta, and Bi correspond to this. When Mg, Zn, Ta, and Bi, other than V and Mn (which act as FCC stabilizers), are added in amounts greater than 5% by weight, intermetallic compounds will form, which is therefore undesirable.
[0141] Based on this analysis, the inventors further added Mn, an element that can simultaneously promote nucleation and inhibit growth, to the Cu-TM-Si alloy, thus preparing the composition of Example 27. The second precipitated phase was observed by SEM in the same manner as in the examples described in Tables 1 and 2 above.
[0142] The composition of Example 27 is designed as follows: In a 90% by weight Cu matrix under the same conditions, in addition to Fe, Co, Ni, and Si, 10 atomic% Mn is added relative to elements other than Cu, i.e., Cu 90重量% (Fe 0.45 Co 0.2 Ni 0.2 Mn 0.1 Si 0.05 ) 10重量% .
[0143] Figure 12 Low-magnification SEM images for observing the morphology of the second precipitate phase in Example 27.
[0144] also, Figure 13The images shown are high-magnification SEM images of Example 27 and SEM-EDS elemental mapping images of the constituent elements of the precipitates formed on the Cu matrix of the fine structure.
[0145] pass Figure 12 and Figure 13 The images confirm that, as predicted during the design phase, the addition of trace amounts of Mn resulted in the precipitation of a second precipitate consisting of more uniform and finer spherical particles. Furthermore, it was confirmed that the precipitate in the Cu matrix consisted of Fe, Co, Ni, and Si, and the further added Mn element acted as an inoculant as expected.
[0146] Figure 14 SEM-EDS elemental line scan images were used to confirm the elemental distribution of the phases precipitated on the Cu matrix in Example 30. Figure 14 In the image, EDS elemental line scan analysis was performed along the direction indicated by the arrows within the SEM microstructure, such as... Figure 14 The line scan spectrum below confirms the concentrations of various metals in the precipitated phase opposite the Cu matrix. Specifically, it shows that the proportion of Cu decreases in the precipitated phase region, while the concentrations of Fe, Co, Ni, etc., relatively increase, thus forming a CCA solid solution.
[0147] The above description is merely an illustrative description of the technical concept of the present invention. Those skilled in the art can make various modifications and variations without departing from the essential characteristics of the present invention. Therefore, the disclosed embodiments are not intended to limit the technical concept of the present invention, but rather to illustrate it. The scope of the technical concept of the present invention is not limited by these embodiments. The scope of protection of the present invention should be interpreted through the following claims, and all technical concepts within the equivalent scope should be interpreted as being included within the scope of the claims of the present invention.
Claims
1. An alloy for electromagnetic wave shielding, comprising: The first phase is composed of a Cu matrix; as well as The second precipitate is rich in one or more ferromagnetic elements selected from Fe, Co, and Ni. The second precipitated phase comprises spherical or fragmented dendritic precipitates.
2. The electromagnetic wave shielding alloy according to claim 1, wherein, The second precipitated phase further comprises Si.
3. The electromagnetic wave shielding alloy according to claim 1, wherein, The alloy has a composition represented by Formula 1: [Formula 1] The x ™ 100-x-y Be y In Equation 1, TM must contain one or more selected from Fe, Co and Ni, and selectively contain one or more selected from Cr, Mn, V, Mg, Zn, Ta and Bi; x is 51-94% by weight, and y is 0.1-5% by weight.
4. The electromagnetic wave shielding alloy according to claim 3, wherein, The TM contains Fe, Ni, and Co with a total content of more than 50 atomic percent.
5. The electromagnetic wave shielding alloy according to claim 3, wherein, The TM is Fe.
6. The electromagnetic wave shielding alloy according to claim 5, wherein, The second precipitated phase comprises one or more of the following phases: Fe solid solution, FeSi, Fe2Si, Fe3Si, and Fe5Si3.
7. The electromagnetic wave shielding alloy according to claim 3, wherein, The x is 70-92% by weight and the y is 0.2-3.4% by weight.
8. The electromagnetic wave shielding alloy according to claim 3, wherein, The TM consists of three or more elements, and the three or more elements constitute a complex concentrated alloy (CCA).
9. The electromagnetic wave shielding alloy according to claim 8, wherein, The second precipitated phase includes one or more of the following: FCC CCA solid solution, (CCA)Si, (CCA)2Si, (CCA)3Si, and (CCA)5Si3.
10. The electromagnetic wave shielding alloy according to claim 3, wherein, When the TM contains one or more of Mg, Zn, Ta and Bi, the total content of Mg, Zn, Ta and Bi relative to the total weight of the TM is less than 5% by weight.
11. The electromagnetic wave shielding alloy according to claim 1, wherein, The alloy is obtained solely through a casting process.
12. The electromagnetic wave shielding alloy according to claim 1, wherein, The second precipitate does not contain columnar dendritic precipitates with an equivalent circular diameter greater than 10 μm.
13. The electromagnetic wave shielding alloy according to claim 1, wherein, The equivalent circular diameter of the precipitated particles of the second precipitate is less than 10 μm.
14. The electromagnetic wave shielding alloy according to claim 7, wherein, ΔT is below 150K, where ΔT = liquid-liquid phase separation temperature T L -Fe precipitation phase formation temperature T Fe .
15. A method for preparing an alloy for electromagnetic wave shielding, comprising the following steps: Molten Cu metal; Add a metallic element comprising one or more ferromagnetic elements selected from Fe, Co, and Ni and Si to the molten Cu metal; and The molten alloy is cast and then cooled.
16. The method for preparing the electromagnetic wave shielding alloy according to claim 15, wherein, The metallic element further includes one or more elements selected from Cr, Mn, V, Mg, Zn, Ta, and Bi.
17. The method for preparing the electromagnetic wave shielding alloy according to claim 15, wherein, The prepared alloys include: A first phase, the first phase being composed of a Cu matrix; and The second precipitate is rich in one or more ferromagnetic elements selected from Fe, Co, and Ni. The second precipitated phase comprises spherical or fragmented dendritic precipitates.
18. The method for preparing the electromagnetic wave shielding alloy according to claim 15, wherein, The step of cooling the molten alloy after casting is as follows: The alloy is cast in a single liquid phase region above the solubility gap and cooled through the solubility gap to ensure that ΔT is below 150K, where ΔT = liquid phase-liquid phase separation temperature T. L -Fe precipitation phase formation temperature T Fe .
19. The method for preparing the electromagnetic wave shielding alloy according to claim 15, wherein, Following the step of cooling the molten alloy after casting, a post-processing step of performing thermomechanical machining (TMT) is further included.
20. An electromagnetic wave shielding component, comprising: The alloy according to any one of claims 1 to 14; as well as Polymer resin.