Hot-rolled steel sheet and hot-dip galvanized steel sheet
Patent Information
- Application Number
- CN202580029968.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-30
- Filing Date
- 2025-04-30
- Publication Date
- 2026-11-20
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This disclosure relates to hot-rolled steel sheets and hot-dip galvanized steel sheets having a hot-dip galvanized coating formed on the surface of the hot-rolled steel sheet. Background Technology
[0002] Hot-rolled steel sheets are widely used in automobiles, motors, building materials, and construction machinery. To improve corrosion resistance, hot-rolled steel sheets used for these applications sometimes have a hot-dip galvanized coating applied to their surface. Hereinafter, hot-rolled steel sheets with a hot-dip galvanized coating will also be referred to as hot-dip galvanized steel sheets.
[0003] Sometimes hot-dip galvanized steel sheets are welded to other steel components. During welding, a portion of the hot-dip galvanizing coating melts. At this time, sometimes the molten metal (zinc) penetrates the grain boundaries of the hot-rolled steel sheet surface, causing cracks. Such cracks are called liquid metal embrittlement (LME).
[0004] For hot-rolled steel sheets, it is required that the hot-dip galvanized coating on the surface of the hot-rolled steel sheet can suppress the occurrence of LME (hereinafter, this characteristic is referred to as LME resistance).
[0005] Japanese Patent Application Publication No. 2018-145500 (Patent Document 1) discloses a molten Zn-Al-Mg coated steel sheet with excellent resistance to LME.
[0006] Patent Document 1 discloses a fused Zn-Al-Mg alloy coated steel sheet comprising a billet steel sheet and a fused Zn-Al-Mg alloy coating. The billet steel sheet has the following chemical composition: by mass %, it contains C: 0.01–0.08%, Si: less than 0.8%, Mn: 0.5–1.8%, P: less than 0.05%, S: less than 0.005%, N: 0.001–0.005%, Ti: 0.02–0.2%, B: 0.0005–0.010%, Al: 0.005–0.1%, with the balance being Fe and unavoidable impurities. In the above chemical composition, the Ti / C equivalent ratio (=(Ti / 48) / (C / 12)) is 0.4–1.5. Furthermore, the dislocation density in the billet steel sheet is 1.8 × 10⁻⁶. 14 / m 2 ~5.7×10 14 / m 2 In the billet steel plate, the main phase is either bainitic ferrite or any single phase of ferrite, or a phase containing both bainitic ferrite and ferrite, and the area fraction of hard second phase and cementite is less than 3%. Ti-containing carbides with an average particle size of less than 20 nm are also dispersed and precipitated in the billet steel plate.
[0007] Patent Document 1 describes that, in the molten Zn-Al-Mg coated steel sheet of Patent Document 1, excellent LME resistance can be obtained by having the above-mentioned chemical composition and microstructure.
[0008] Existing technical documents
[0009] Patent documents
[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-145500 Summary of the Invention
[0011] The problem the invention aims to solve
[0012] The hot-rolled steel sheet disclosed in Patent Document 1 has excellent LME resistance. However, excellent LME resistance can also be obtained by means different from those used for the hot-rolled steel sheet in Patent Document 1.
[0013] The purpose of this disclosure is to provide hot-rolled steel sheets and hot-dip galvanized steel sheets that can achieve excellent LME resistance.
[0014] Solution for solving the problem
[0015] The hot-rolled steel sheet disclosed herein contains, by mass percent, C: 0.030–0.110%, Si: 0.01–0.50%, Mn: 0.50–1.50%, P: less than 0.025%, S: less than 0.010%, Al: 0.010–0.070%, N: less than 0.0070%, Ti: 0.055–0.200%, Nb: 0.030–0.150%, B: 0.0010–0.0050%, V: 0–0.20%, and Cr: 0–1.00%, with the balance being Fe and impurities. In the microstructure, the area fraction of bainitic ferrite is 85% or more. BO2 was detected by time-of-flight secondary ion mass spectrometry in the surface region of the hot-rolled steel sheet extending from the surface along the thickness direction to a depth of 0.2 mm. - The total length of the original austenite grain boundary is 1.20 to 5.00 mm per 100 μm × 100 μm, and the boron segregation at the original austenite grain boundary is above 40.
[0016] The hot-dip galvanized steel sheet disclosed herein comprises: the aforementioned hot-rolled steel sheet; and a hot-dip galvanized coating formed on the surface of the aforementioned hot-rolled steel sheet, which contains 65.00% or more Zn by mass%.
[0017] The effects of the invention
[0018] The hot-rolled steel sheet and hot-dip galvanized steel sheet disclosed herein can achieve excellent resistance to LME. Attached Figure Description
[0019] Figure 1 This is a schematic diagram used to illustrate line analysis based on time-of-flight secondary ion mass spectrometry.
[0020] Figure 2 This is a schematic diagram of the B-detection intensity distribution obtained through line analysis.
[0021] Figure 3 This is a schematic diagram of the LME resistance evaluation test in the embodiment.
[0022] Figure 4 Viewed from the side Figure 3 A cross-sectional view of the LME resistance evaluation test. Detailed Implementation
[0023] Hot-rolled steel sheets suitable for applications such as automobiles, motors, building materials, and construction machinery require a certain level of strength. Therefore, the inventors conducted research on hot-rolled steel sheets suitable for these applications from the perspective of chemical composition. The results showed that a chemical composition containing, by mass percent, C: 0.030–0.110%, Si: 0.01–0.50%, Mn: 0.50–1.50%, P: 0.025% or less, S: 0.010% or less, Al: 0.010–0.070%, N: 0.0070% or less, Ti: 0.055–0.200%, V: 0–0.20%, and Cr: 0–1.00%, with the balance being Fe and impurities, and further having a bainitic ferrite area ratio of 85% or more, can potentially achieve sufficient strength.
[0024] Therefore, the inventors further investigated methods to improve the LME resistance of hot-rolled steel sheets having the above-described chemical composition and microstructure. As mentioned above, LME is caused by molten metal (zinc) intruding into the grain boundaries of the steel sheet surface. Therefore, the inventors considered including 0.0010 to 0.0050% B in the above-described chemical composition. B segregates at the grain boundaries and strengthens them. Therefore, it is possible to improve LME resistance.
[0025] However, simply including boron (B) in the above chemical composition is sometimes insufficient to achieve adequate resistance to ligand elongation (LME). Therefore, the inventors conducted further research. Here, the inventors focused on the length of the grain boundaries where boron segregates within the proto-austenite grain boundaries of the surface layer of hot-rolled steel sheets. LME tends to propagate along the proto-austenite grain boundaries. Therefore, the longer the length of the proto-austenite grain boundaries where boron segregates, the easier it is to suppress the propagation of LME along the grain boundaries.
[0026] Based on the above insights, the inventors further investigated methods to lengthen the original austenite grain boundaries that cause B segregation. As a result, the inventors discovered that by further containing 0.030 to 0.150% Nb in the above chemical composition, the total length of the original austenite grain boundaries with high B segregation can be increased.
[0027] Based on the above insights, the hot-rolled steel sheet of this embodiment and the hot-dip galvanized steel sheet using the hot-rolled steel sheet have the following configuration.
[0028] The hot-rolled steel sheet of this embodiment contains, by mass%, C: 0.030–0.110%, Si: 0.01–0.50%, Mn: 0.50–1.50%, P: less than 0.025%, S: less than 0.010%, Al: 0.010–0.070%, N: less than 0.0070%, Ti: 0.055–0.200%, Nb: 0.030–0.150%, B: 0.0010–0.0050%, V: 0–0.20%, and Cr: 0–1.00%, with the balance being Fe and impurities. In the microstructure, the area fraction of bainitic ferrite is 85% or more. BO2 was detected in the surface region of the hot-rolled steel sheet from the surface along the thickness direction to a depth of 0.2 mm by time-of-flight secondary ion mass spectrometry. - The total length of the original austenite grain boundary is 1.20 to 5.00 mm per 100 μm × 100 μm, and the boron segregation at the original austenite grain boundary is above 40.
[0029] The hot-rolled steel sheet of this embodiment may also contain one or more ingredients selected from the group consisting of V: 0.01 to 0.20% and Cr: 0.01 to 1.00% by mass%.
[0030] The hot-dip galvanized steel sheet of this embodiment comprises: the hot-rolled steel sheet of this embodiment; and a hot-dip galvanized coating formed on the surface of the hot-rolled steel sheet, which contains 65.00% or more Zn by mass%.
[0031] The hot-rolled steel sheet and hot-dip galvanized steel sheet of this embodiment will be described in detail below. Unless otherwise specified, "%" related to elements refers to mass%.
[0032] Hot-rolled steel plate
[0033] The hot-rolled steel sheet of this embodiment satisfies the following features 1 to 4.
[0034] (Feature 1)
[0035] The chemical composition, by mass%, contains C: 0.030–0.110%, Si: 0.01–0.50%, Mn: 0.50–1.50%, P: less than 0.025%, S: less than 0.010%, Al: 0.010–0.070%, N: less than 0.0070%, Ti: 0.055–0.200%, Nb: 0.030–0.150%, B: 0.0010–0.0050%, V: 0–0.20%, and Cr: 0–1.00%, with the balance being Fe and impurities.
[0036] (Feature 2)
[0037] In the microstructure, the area fraction of bainitic ferrite is over 85%.
[0038] (Feature 3)
[0039] BO2 was detected in the surface region of hot-rolled steel sheet from the surface along the thickness direction to a depth of 0.2 mm by time-of-flight secondary ion mass spectrometry. - The total length of the original austenite grain boundaries is 1.20 to 5.00 mm per 100 μm × 100 μm.
[0040] (Feature 4)
[0041] BO2 was detected by time-of-flight secondary ion mass spectrometry. - The boron segregation at the original austenite grain boundaries is above 40.
[0042] The following describes features 1 through 4.
[0043] [(Feature 1) Regarding chemical composition]
[0044] The hot-rolled steel sheet of this embodiment contains the following elements in its chemical composition.
[0045] C: 0.030~0.110%
[0046] Carbon (C) combines with Ti to form Ti carbides. These Ti carbides enhance the strength of hot-rolled steel sheets through precipitation strengthening. Furthermore, when the Ti content in the chemical composition is 0.055–0.200%, C readily forms bainitic ferrite. If the C content is less than 0.030%, even with the contents of other elements within the range of this embodiment, the aforementioned effects cannot be fully achieved.
[0047] On the other hand, if the carbon content exceeds 0.110%, even if the contents of other elements are within the range of this embodiment, excessive bainite will be generated in the microstructure, resulting in an excessively reduced area fraction of bainitic ferrite. Consequently, the workability of the hot-rolled steel sheet is reduced.
[0048] Therefore, the C content is 0.030–0.110%.
[0049] The preferred lower limit for C content is 0.032%, more preferably 0.034%, more preferably 0.036%, and more preferably 0.040%.
[0050] The preferred upper limit for C content is 0.105%, more preferably 0.100%, more preferably 0.095%, more preferably 0.090%, and more preferably 0.085%.
[0051] Si: 0.01~0.50%
[0052] Silicon (Si) deoxidizes the steel. Si further enhances the strength of the hot-rolled steel sheet through solid solution strengthening. If the Si content is less than 0.01%, the aforementioned effects cannot be fully achieved even if the contents of other elements are within the range specified in this embodiment.
[0053] On the other hand, if the Si content exceeds 0.50%, polygonal ferrite is easily formed in the hot-rolled steel sheet even if the contents of other elements are within the range of this embodiment. Therefore, the area fraction of bainitic ferrite in the hot-rolled steel sheet decreases. In this case, the strength of the hot-rolled steel sheet decreases.
[0054] Therefore, the Si content is 0.01–0.50%.
[0055] The preferred lower limit for Si content is 0.02%, more preferably 0.03%, and even more preferably 0.04%.
[0056] The preferred upper limit for Si content is 0.45%, more preferably 0.40%, and even more preferably 0.35%.
[0057] Mn: 0.50~1.50%
[0058] Manganese (Mn) enhances the strength of hot-rolled steel sheets through solid solution strengthening. If the Mn content is less than 0.50%, the aforementioned effects cannot be fully achieved even if the contents of other elements are within the range specified in this embodiment.
[0059] On the other hand, if the Mn content exceeds 1.50%, Mn segregation is easily generated in the hot-rolled steel sheet even if the contents of other elements are within the range of this embodiment. If the Mn content exceeds 1.50%, bainite is also easily formed in the hot-rolled steel sheet. As a result, the area ratio of bainitic ferrite in the hot-rolled steel sheet decreases. In this case, the cold workability of the hot-rolled steel sheet decreases.
[0060] Therefore, the Mn content is 0.50–1.50%.
[0061] The preferred lower limit for Mn content is 0.55%, more preferably 0.60%, more preferably 0.65%, and more preferably 0.70%.
[0062] The preferred upper limit for Mn content is 1.40%, more preferably 1.35%, more preferably 1.30%, more preferably 1.25%, and more preferably 1.20%.
[0063] P: below 0.025%
[0064] Phosphorus (P) segregates at grain boundaries, reducing the cold workability of hot-rolled steel sheets. P further reduces the weldability of hot-rolled steel sheets. If the P content exceeds 0.025%, the cold workability and weldability of hot-rolled steel sheets are significantly reduced even if the contents of other elements are within the range of this embodiment.
[0065] Therefore, the P content is below 0.025%.
[0066] The phosphorus (P) content is preferably as low as possible. However, excessive reduction in P content leads to decreased productivity and increased manufacturing costs. Therefore, considering industrial production, the preferred lower limit for P content is more than 0%, more preferably 0.001%, more preferably 0.002%, more preferably 0.003%, and more preferably 0.005%.
[0067] The preferred upper limit for the P content is 0.023%, more preferably 0.022%, and even more preferably 0.020%.
[0068] S: below 0.010%
[0069] Sulfur (S) segregates at grain boundaries, reducing the cold workability of hot-rolled steel sheets. If the S content exceeds 0.010%, the cold workability of hot-rolled steel sheets is significantly reduced even if the contents of other elements are within the range of this embodiment.
[0070] Therefore, the sulfur content is below 0.010%.
[0071] The sulfur (S) content is preferably as low as possible. However, excessive reduction in S content leads to decreased productivity and increased manufacturing costs. Therefore, considering industrial production, the preferred lower limit for S content is more than 0%, more preferably 0.001%, more preferably 0.002%, and more preferably 0.003%.
[0072] The preferred upper limit for the sulfur content is 0.009%, more preferably 0.008%, and even more preferably 0.007%.
[0073] Al: 0.010~0.070%
[0074] Aluminum (Al) deoxidizes steel. Al further combines with nitrogen to form Al nitrides. This inhibits the combination of boron (B) and nitrogen (N). If the Al content is less than 0.010%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the range of this embodiment.
[0075] On the other hand, if the Al content exceeds 0.070%, even if the contents of other elements are within the range of this embodiment, coarse Al nitrides will be generated excessively. As a result, the cold workability of the hot-rolled steel sheet is reduced.
[0076] Therefore, the Al content is 0.010–0.070%.
[0077] The preferred lower limit for Al content is 0.012%, more preferably 0.014%, more preferably 0.016%, more preferably 0.018%, and more preferably 0.020%.
[0078] The preferred upper limit for Al content is 0.065%, more preferably 0.060%, and even more preferably 0.055%.
[0079] N: below 0.0070%
[0080] Nitrogen (N) combines with boron (B) to form BN, reducing the amount of dissolved boron (B) in hot-rolled steel sheets. N further combines with titanium (Ti) to form TiN, hindering the formation of Ti carbides. If the N content exceeds 0.0070%, BN and TiN will be excessively generated even if the contents of other elements are within the range of this embodiment. As a result, the LME resistance of the hot-rolled steel sheet decreases. Consequently, the strength of the hot-rolled steel sheet also decreases.
[0081] Therefore, the nitrogen content is below 0.0070%.
[0082] The nitrogen (N) content is preferably as low as possible. However, excessive reduction in N content leads to decreased productivity and increased manufacturing costs. Therefore, considering industrial production, the preferred lower limit for N content is more than 0%, more preferably 0.0001%, more preferably 0.0005%, more preferably 0.0010%, more preferably 0.0015%, and more preferably 0.0020%.
[0083] The preferred upper limit for the nitrogen content is 0.0065%, more preferably 0.0060%, more preferably 0.0055%, more preferably 0.0050%, and more preferably 0.0040%.
[0084] Ti: 0.055~0.200%
[0085] Titanium (Ti) combines with carbon to form Ti carbides. These Ti carbides enhance the strength of hot-rolled steel sheets through precipitation strengthening. Furthermore, the amount of dissolved carbon in the steel sheet is adjusted through the formation of Ti carbides. Therefore, bainitic ferrite is readily formed in hot-rolled steel sheets. If the Ti content is less than 0.055%, polygonal ferrite is easily formed even if the contents of other elements are within the range of this embodiment, resulting in a lower area fraction of bainitic ferrite. In this case, the strength of the hot-rolled steel sheet decreases.
[0086] On the other hand, if the Ti content exceeds 0.200%, coarse TiC will be generated excessively, even if the contents of other elements are within the range of this embodiment. As a result, the cold workability of the hot-rolled steel sheet is reduced.
[0087] Therefore, the Ti content is 0.055–0.200%.
[0088] The preferred lower limit for Ti content is 0.060%, more preferably 0.065%, more preferably 0.070%, more preferably 0.075%, more preferably 0.080%, and more preferably 0.085%.
[0089] The preferred upper limit for Ti content is 0.190%, more preferably 0.180%, and even more preferably 0.170%.
[0090] Nb: 0.030~0.150%
[0091] Niobium (Nb) forms Nb precipitates (Nb carbides or Nb carbonitrides), causing the per 1 mm of hot-rolled steel sheet to... 2 The total length of the original austenite grain boundaries increases. Nb further promotes the segregation of boron to the original austenite grain boundaries. As a result, the degree of boron segregation at the original austenite grain boundaries increases. Consequently, the resistance of the hot-rolled steel sheet to LME is improved. Nb precipitates further improve the strength of the hot-rolled steel sheet through precipitation strengthening. If the Nb content is less than 0.030%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the range of this embodiment.
[0092] On the other hand, if the Nb content exceeds 0.150%, excessive Nb precipitates will be generated. In this case, even if the contents of other elements are within the range of this embodiment, the cold workability of the hot-rolled steel sheet will decrease.
[0093] Therefore, the Nb content is 0.030–0.150%.
[0094] The preferred lower limit for Nb content is 0.035%, more preferably 0.040%, and even more preferably 0.045%.
[0095] The preferred upper limit for Nb content is 0.145%, more preferably 0.140%, and even more preferably 0.135%.
[0096] B: 0.0010~0.0050%
[0097] Boron (B) is dissolved in hot-rolled steel sheet and segregates at the original austenite grain boundaries. The segregated B increases grain boundary strength. Therefore, B improves the LME resistance of the hot-rolled steel sheet. B further improves the hardenability of the steel. If the B content is less than 0.0010%, the above-mentioned effects cannot be fully obtained even if the contents of other elements are within the range of this embodiment. If the B content is less than 0.0010%, the phase transformation initiation temperature from austenite to ferrite further increases. In this case, the precipitation initiation temperature of Ti carbides also increases. Therefore, the Ti carbides become coarse. As a result, the strength of the hot-rolled steel sheet decreases.
[0098] On the other hand, if the boron content exceeds 0.0050%, the hardenability will become excessively high even if the contents of other elements are within the range of this embodiment. In this case, bainite is easily formed, and the area fraction of bainitic ferrite decreases. As a result, the machinability of the steel sheet decreases. If the boron content exceeds 0.0050%, Fe further precipitates at the original austenite grain boundaries. 23 CB6. In this case, the grain boundary strength of the original austenite grains decreases. Therefore, resistance to LME decreases.
[0099] Therefore, the B content is 0.0010 to 0.0050%.
[0100] The preferred lower limit for the content of B is 0.0012%, more preferably 0.0015%, more preferably 0.0020%, and more preferably 0.0025%.
[0101] The preferred upper limit for the B content is 0.0045%, more preferably 0.0043%, more preferably 0.0040%, and more preferably 0.0035%.
[0102] The hot-rolled steel sheet of this embodiment has a chemical composition balance of Fe and impurities. Here, impurities refer to substances that are permissible during the industrial manufacturing of hot-rolled steel sheets, introduced from raw materials such as ore, waste, or the manufacturing environment, and are within a range that does not adversely affect the hot-rolled steel sheet of this embodiment. Preferably, the hot-rolled steel sheet of this embodiment has a chemical composition balance of Fe and impurities. Here, the impurities are, for example, one or more selected from the group consisting of O: 0–0.01%, Mo: 0–0.10%, Cu: 0–0.50%, Ni: 0–0.30%, Co: 0–0.10%, Zr: 0–0.05%, Sn: 0–0.10%, Sb: 0–0.10%, Hf: 0–0.02%, Sc: 0–0.02%, Te: 0–0.01%, Sr: 0–0.02%, Bi: 0–0.10%, Ta: 0–0.02%, Zn: 0–0.02%, and rare earth elements (REM): 0–0.01%. The total content of these impurities is, for example, 0–1.00%.
[0103] [Optional elements]
[0104] The chemical composition of the hot-rolled steel sheet of this embodiment may further contain one or more elements selected from the group consisting of V: 0-0.20% and Cr: 0-1.00% to replace a portion of Fe. These elements are all arbitrary elements.
[0105] V: 0~0.20%
[0106] Vanadium (V) can be any element, or it can be absent. That is, the V content can be 0%.
[0107] In the presence of V, specifically when the V content exceeds 0%, V combines with C to form V carbides. V carbides enhance the strength of hot-rolled steel sheets through precipitation strengthening. Even a small amount of V is sufficient to achieve this effect to some extent.
[0108] However, if the V content exceeds 0.20%, V carbides will be generated excessively, even if the contents of other elements are within the range of this embodiment. In this case, the processability of the hot-rolled steel sheet decreases.
[0109] Therefore, the V content is 0-0.20%, and when it is present, the V content is below 0.20%.
[0110] The preferred lower limit for the V content is 0.01%, more preferably 0.05%, and even more preferably 0.08%.
[0111] The preferred upper limit for the V content is 0.18%, more preferably 0.16%, more preferably 0.14%, and more preferably 0.12%.
[0112] Cr: 0~1.00%
[0113] Chromium (Cr) can be any element, or it can be absent. That is, the Cr content can be 0%.
[0114] In the presence of Cr, i.e., when the Cr content exceeds 0%, Cr segregates at the original austenite grain boundaries, improving the LME resistance of hot-rolled steel sheets. Even a small amount of Cr can achieve this effect to some extent.
[0115] However, if the Cr content exceeds 1.00%, the cold workability of the hot-rolled steel sheet will decrease even if the contents of other elements are within the range of this embodiment.
[0116] Therefore, the Cr content is 0 to 1.00%, and when it is present, the Cr content is less than 1.00%.
[0117] The preferred lower limit for Cr content is 0.01%, more preferably 0.05%, more preferably 0.10%, more preferably 0.20%, and more preferably 0.30%.
[0118] The preferred upper limit for Cr content is 0.90%, more preferably 0.80%, more preferably 0.70%, more preferably 0.60%, and more preferably 0.55%.
[0119] Methods for determining the chemical composition of hot-rolled steel sheets
[0120] The chemical composition of the hot-rolled steel sheet in this embodiment can be determined using a known compositional analysis method according to JIS G0321:2017. Specifically, chips are collected from the hot-rolled steel sheet using a cutting tool such as a drill bit. The collected chips are dissolved in acid to obtain a solution. Elemental analysis of the chemical composition is performed on the solution using ICP-MAS (Inductively Coupled Plasma Mass Spectrometry). The C and S contents are determined using a known high-frequency combustion method (combustion-infrared absorption method). The N content is determined using a known inert gas melting-thermal conductivity method.
[0121] It should be noted that the content of each element is based on the significant figures specified in this embodiment, with the measured values rounded to the nearest decimal place. For example, the C content of the steel in this embodiment is specified to the third decimal place. Therefore, the C content is the value obtained by rounding the fourth decimal place of the measured value to the third decimal place.
[0122] In this embodiment, the content of other elements in the steel, except for C, is also the same. For the measured value, the value obtained by rounding the last digit of the value specified in this embodiment to the nearest whole number is taken as the content of that element.
[0123] It should be noted that rounding means that if the last digit is less than 5, it is discarded; if the last digit is 5 or more, it is rounded up.
[0124] [(Feature 2) Regarding the area ratio of bainitic ferrite]
[0125] In the microstructure of the hot-rolled steel sheet of this embodiment, the area fraction of bainitic ferrite is 85% or more. The microstructure of the hot-rolled steel sheet of this embodiment can be a single phase of bainitic ferrite. When the microstructure of the hot-rolled steel sheet of this embodiment is composed of bainitic ferrite and other structures, the other structures are, for example, one or more selected from the group consisting of polygonal ferrite, bainite, and cementite.
[0126] Bainitic ferrite can be distinguished from polygonal ferrite and bainite in the following ways.
[0127] [The difference between bainitic ferrite and polygonal ferrite]
[0128] Bainitic ferrite is an aggregate of grains with slightly different crystal orientations. Therefore, differences in contrast are observed within the grains. On the other hand, polygonal ferrite is a structure with almost no difference in crystal orientation within the grains. Therefore, it is observed with uniform contrast within the grains. Thus, bainitic ferrite can be distinguished from polygonal ferrite based on the contrast caused by differences in crystal orientation.
[0129] [The difference between bainitic ferrite and bainite]
[0130] The crystal structure of bainitic ferrite is the same as that of bainite, being a bcc structure. Therefore, it is difficult to distinguish bainitic ferrite from bainite based on crystal structure alone. Furthermore, it is difficult to distinguish bainitic ferrite from bainite based on differences in crystal orientation. However, the presence or absence of Fe carbides within the grains and at grain boundaries allows for the differentiation of bainitic ferrite from bainite. Here, Fe carbides refer to carbides containing Fe, such as cementite.
[0131] Specifically, in bainitic ferrite, Fe carbides are absent within the grains and at the grain boundaries. On the other hand, in bainite, Fe carbides are present within the laths and / or at the lath boundaries. Therefore, the presence or absence of Fe carbides within the grains and at the grain boundaries allows for the distinction between bainitic ferrite and bainite.
[0132] [Effect based on the area ratio of bainitic ferrite]
[0133] In the microstructure of hot-rolled steel sheets within the range of the chemical composition of each element in this embodiment, if the area ratio of bainitic ferrite is 85% or more, high strength can be obtained.
[0134] The preferred lower limit for the area fraction of bainitic ferrite is 88%, more preferably 90%, more preferably 92%, more preferably 94%, and more preferably 96%. The area fraction of bainitic ferrite can also be 100%.
[0135] [Method for determining the area ratio of bainitic ferrite]
[0136] The area ratio of bainitic ferrite can be determined by the following method.
[0137] Microstructure observation was performed using field emission scanning electron microscopy (FE-SEM). Microstructure observation was conducted using electron channeling contrast image (ECCI). The observation conditions were an accelerating voltage of 20 kV, a tilt angle (T) of 0°, and backscattered electron mode. Crystal orientation was determined using electron backscattered diffraction (EBSD).
[0138] The test specimen was collected from the center of the width of a hot-rolled steel sheet. The measurement location was set at a depth of 1 / 4 of the thickness of the hot-rolled steel sheet in the thickness direction from the surface of the test specimen, and the measurement range was set to 100μm × 100μm. The measurement range included a longitudinal section encompassing both the L direction (length direction) and the T direction (thickness direction) of the hot-rolled steel sheet. The measurement range was divided into regular hexagonal pixel units. The center-to-center distance between adjacent pixels (the measurement interval for EBSD) was set to 0.1μm. The center position of a pixel within the measurement range that encompasses the entire regular hexagonal pixel unit was designated as the measurement point. That is, pixels partially outside the field of view were excluded from the measurement. Furthermore, the reliability index (CI value) was 0.1 or higher.
[0139] Use EBSD analysis software to analyze the measurement data according to the following steps to identify and quantify polygonal ferrite and bainitic ferrite.
[0140] (Step 1)
[0141] A region surrounded by grain boundaries with an orientation difference of 15° or more is defined as a grain. It should be noted that if the equivalent circle diameter of a region surrounded by grain boundaries with an orientation difference of 15° or more is less than 1.0 μm, this region is considered measurement noise and is not considered a grain. That is, regions identified as measurement noise are not considered as objects.
[0142] (Step 2)
[0143] Calculate the average grain average misorientation (GAM value) within each grain. Grains with a GAM value below 0.5° are defined as polygonal ferrite. Grains with a GAM value above 0.5° are defined as bainitic ferrite.
[0144] It should be noted that in the above microstructure observations, structures different from bainitic ferrite and polygonal ferrite (bainite and cementite) can be easily distinguished by contrast.
[0145] The identified bainitic ferrite was quantified. Then, based on the area of the quantified bainitic ferrite and the total area of the measurement range (100 μm × 100 μm), the area fraction (%) of the bainitic ferrite was calculated. It should be noted that areas deemed as measurement noise were excluded from the total area of the measurement range.
[0146] It should be noted that any well-known program can be used for the EBSD analysis to calculate the GAM value. For example, TSL Solutions' OIM Data Acquisition / Analysis 6.2.0 can be used.
[0147] [(Feature 3) Grain boundary length GL of the original austenite grains on the surface]
[0148] Furthermore, in the hot-rolled steel sheet of this embodiment, BO2 was detected in the surface region by time-of-flight secondary ion mass spectrometry. - The total length of the original austenite grain boundaries ranges from 1.20 to 5.00 mm per 100 μm × 100 μm. Here, BO2 was detected per 100 μm × 100 μm using time-of-flight secondary ion mass spectrometry. - The total length of the original austenite grain boundaries is called the "grain boundary length GL" (mm).
[0149] If the grain boundary length GL is too short, there are few grain boundary regions with boron segregation. In this case, boron segregation cannot sufficiently contribute to the suppression of LME cracks. Therefore, the LME resistance of the hot-rolled steel sheet decreases. If the grain boundary length GL is 1.20 mm or longer, then the grain boundary length GL is sufficiently long. In this case, there are enough grain boundary regions in the surface region of the hot-rolled steel sheet to produce boron segregation. As a result, the LME resistance of the hot-rolled steel sheet improves.
[0150] The preferred lower limit for the grain boundary length GL is 1.25 mm, more preferably 1.40 mm, more preferably 1.60 mm, more preferably 1.80 mm, more preferably 1.90 mm, more preferably 2.00 mm, and more preferably 2.10 mm.
[0151] There is no particular upper limit to the grain boundary length GL. However, if an attempt is made to excessively extend the grain boundary length GL, the manufacturing cost increases significantly. Therefore, considering industrial production, the upper limit of the grain boundary length GL is 5.00 mm, more preferably 4.95 mm, more preferably 4.80 mm, more preferably 4.60 mm, and more preferably 4.40 mm.
[0152] [Method for determining grain boundary length GL]
[0153] The grain boundary length GL of the surface region is determined by the following method.
[0154] Collect a test piece with a cross-section parallel to both the rolling direction and the thickness direction of the hot-rolled steel sheet as the observation surface. The dimensions of the observation surface are, for example, 10 mm × sheet thickness in the rolling direction.
[0155] The observation surfaces of each test piece were mirror-polished using diamond polishing paste. The mirror-polished surfaces were then chemically polished using colloidal silica solution to remove the processing-induced alteration layer introduced during the mirror polishing process.
[0156] On the observation surface, in the surface region of the hot-rolled steel sheet extending from the surface along the thickness direction to a depth of 0.2 mm, a rectangular field of view of 100 μm × 100 μm is selected. Based on the method described in the above-mentioned [Method for Determining the Area Ratio of Bainitic Ferrite], the bainitic ferrite grain boundaries, polygonal ferrite grain boundaries, and bainitic grain boundaries in the field of view are determined.
[0157] In the same field of view, boron segregation at the proto-austenite grain boundaries was determined using time-of-flight secondary ion mass spectrometry (TOF-SIMS). First, as a pretreatment, the field of view was sputtered with a Cs (cesium) ion beam to remove contaminants and oxides. After pretreatment, the field of view was sputtered by primary ion irradiation from the primary ion source of the TOF-SIMS apparatus. Bi1 was used in the determination. + As primary ions, the beam diameter of the primary ions is 0.1 μm, the accelerating voltage is 30 keV, and the current is 2 pA.
[0158] BO2 was detected in secondary ions generated by sputtering primary ions. - (Mass-to-charge ratio m / z = 43) is a secondary ion containing B. This was determined by measuring BO2. - The flight time was used to create a B-distribution plot within the observed field of view. The B-distribution plot represents the detection of BO2. - A diagram showing the location of [the location].
[0159] Identify bainitic ferrite grain boundaries, polygonal ferrite grain boundaries, and bainite grain boundaries in the constructed B-distribution map. In the B-distribution map, grain boundaries other than bainitic ferrite, polygonal ferrite, and bainite grain boundaries are considered as proto-austenite grain boundaries. Within the proto-austenite grain boundaries, BO2 with an intensity count of 40 or higher is determined using known image processing techniques. - The total length of the grain boundary portion. The obtained total length of the grain boundary is taken as the grain boundary length GL (mm). The grain boundary length GL is the value obtained by rounding the third decimal place to the second decimal place.
[0160] It should be noted that the TOF-SIMS device, for example, uses the product name TOF-SIMS manufactured by IONTOF. 5.
[0161] [(Feature 4) Regarding the boron segregation at the original austenite grain boundaries]
[0162] In the hot-rolled steel sheet of this embodiment, BO2 was further detected in the surface region by time-of-flight secondary ion mass spectrometry. - The boron segregation at the original austenite grain boundaries is above 40. If the boron segregation at the original austenite grain boundaries is high, the original austenite grain boundaries are strengthened. Therefore, this can suppress the propagation of LME cracks along the grain boundaries.
[0163] If the boron segregation at the original austenite grain boundary is greater than 40, a high boron segregation grain boundary length GL is formed. Therefore, the propagation of LME cracks along the original austenite grain boundary can be significantly suppressed. As a result, the LME resistance of hot-rolled steel sheets is significantly improved.
[0164] The preferred lower limit for the degree of segregation B is 42, further preferably 44, further preferably 46, further preferably 50, further preferably 52, further preferably 55, further preferably 58, and further preferably 60.
[0165] There is no particular upper limit to the β segregation. However, for hot-rolled steel sheets that satisfy characteristics 1 to 3, the upper limit of the β segregation at the original austenite grain boundaries is, for example, 160, 150, 140, 130, and 120.
[0166] [Method for determining the boron segregation at the original austenite grain boundaries]
[0167] The boron segregation at the original austenite grain boundaries was determined by the following method.
[0168] Using the method described above [Method for determining grain boundary length GL], BO2 was detected in the field of view. -The original austenite grain boundaries. At any 5 points along the identified grain boundaries, line analysis is performed across the grain boundaries as follows.
[0169] Figure 1 This is a schematic diagram used to illustrate line analysis. (See reference...) Figure 1 BO2 was detected in the field of view - The original austenite grain boundaries AG were analyzed by scanning the ion beam once in a roughly perpendicular direction using TOF-SIMS to detect the B intensity. In the TOF-SIMS line analysis, Bi1 was used... + As a primary ion, the beam diameter of the primary ion is set to 0.1 μm. The length L1 of the line segment SE used for line analysis is set to 15 μm, and the measurement interval is set to 0.2 μm. It should be noted that the line segment SE intersects only one grain boundary AG, and not multiple grain boundary AGs. Furthermore, line analysis is performed by placing the grain boundary AG at approximately the center position of the length L1 of the line segment SE. Through line analysis, the B detection intensity distribution on the line segment SE can be obtained.
[0170] Figure 2 This is a schematic diagram of the B detection intensity distribution at line segment SE. Figure 2 The vertical axis represents the detection intensity B, and the horizontal axis represents the distance within line segment SE. (Refer to...) Figure 2 The maximum value of the detection intensity in the obtained B detection intensity distribution BC is set as the value of the detected BO2. - The intensity of B at the original austenite grain boundary AG was detected. p In the intensity distribution BC detected by B, the intensity distribution will be measured from endpoint E of line segment SE. L The total B detection intensity measured within a range L10 of 0.15 × L1 at intervals of 0.2 μm is compared with the intensity at the endpoint E of line segment SE. R The arithmetic mean of all B detection intensities measured within a range R10 of 0.15×L1 at 0.2μm intervals is taken as the value of the detected BO2. - The average B detection intensity within the original austenite grains surrounded by the original austenite grain boundaries AG. ave .
[0171] The intensity B at the original austenite grain boundary AG was measured using the obtained B. p The average B detection intensity within the original austenite grains. ave Based on equation (A), the segregation degree of B is calculated.
[0172] B segregation degree = B p / B ave × Bode content (ppm) in the chemical composition of hot-rolled steel sheet (A)
[0173] The arithmetic mean of the B segregation values obtained through line analysis at five locations is taken as the B segregation value at the original austenite grain boundaries in the surface region. The obtained B segregation value is an integer value obtained by rounding the first decimal place.
[0174] [Effects of the hot-rolled steel plate in this embodiment]
[0175] The hot-rolled steel sheet of this embodiment satisfies features 1 to 4. Therefore, excellent LME resistance can be obtained in the hot-rolled steel sheet of this embodiment.
[0176] [Regarding the strength of the hot-rolled steel sheet in this embodiment]
[0177] It should be noted that the hot-rolled steel sheet of this embodiment satisfies features 1 to 4. Therefore, the tensile strength of the hot-rolled steel sheet of this embodiment is 590 MPa or higher. Thus, the hot-rolled steel sheet of this embodiment can achieve both high strength and excellent LME resistance.
[0178] The preferred lower limit for the tensile strength of hot-rolled steel sheet is 600 MPa, more preferably 610 MPa, more preferably 620 MPa, more preferably 630 MPa, more preferably 640 MPa, and more preferably 650 MPa. The upper limit for the tensile strength of hot-rolled steel sheet is not particularly limited, for example, it is 930 MPa.
[0179] [Methods for determining tensile strength]
[0180] The tensile strength of hot-rolled steel sheet can be determined by tensile testing according to JIS Z2241:2022.
[0181] Specifically, a plate-shaped tensile test piece, equivalent to the JIS 5 test piece specified in JIS Z2241:2022, is collected from a hot-rolled steel plate. The longitudinal direction of the test piece is orthogonal to the rolling direction of the hot-rolled steel plate. Tensile tests are conducted at room temperature and in atmospheric conditions according to JIS Z2241:2022 to determine the tensile strength TS (MPa).
[0182] [On balancing strength and flanging]
[0183] In the hot-rolled steel sheet of this embodiment, it is preferable to also possess the aforementioned excellent strength and excellent flanging properties. When hot-rolled steel sheets are used in automobiles, motors, building materials, and construction machinery, various processing methods such as pressing and stretching flange processing are sometimes performed. In cases of such processing, high flanging properties of the hot-rolled steel sheet are preferable.
[0184] In this embodiment, the hot-rolled steel sheet exhibits an excellent strength / flanging balance. Specifically, it is preferable to use a strength / flanging balance SB defined by the following formula, where the tensile strength TS (MPa) and the expansion ratio λ (%) is 40000 (MPa·%) or higher. In this case, when the hot-rolled steel sheet is used for the aforementioned applications, lightweight components can be achieved.
[0185] SB=TS×λ
[0186] [Method for determining the strength / flanging balance (SB)]
[0187] The strength / flanging balance SB can be determined using the following method.
[0188] A 70mm × 70mm × plate thickness test piece was taken from a hot-rolled steel sheet. A punched hole was formed in the center of the test piece using a first punch and die. The diameter D0 of the first punch was 10.0mm. A die with a clearance of 12% of the test piece's plate thickness was used. The punched hole was circular, formed with its center aligning with the center of the 70mm × 70mm surface of the test piece.
[0189] For the freshly punched hole, a second punch with a 60° apex angle is pressed in from the opposite side of the burr formed on the edge of the hole to enlarge it. At this point, the moving speed of the second punch is set to 10 mm / min. The second punch is stopped when the hole has enlarged and the crack has penetrated along the thickness direction of the plate. After stopping the second punch, the inner diameter Db (mm) of the hole is measured.
[0190] Using the diameter D0 (mm) of the first punch and the inner diameter Db (mm) of the punching hole, the hole expansion rate λ (%) is calculated using the following formula.
[0191] λ=(Db-D0) / D0×100
[0192] Using the tensile strength TS (MPa) and expansion ratio λ (%) of the hot-rolled steel sheet obtained in the above [Method for Determining Tensile Strength], the strength / flanging balance SB (MPa·%) is calculated by the following formula.
[0193] SB=TS×λ
[0194] [Regarding the thickness of the hot-rolled steel plate in this embodiment]
[0195] The thickness of the hot-rolled steel sheet in this embodiment is not particularly limited. For example, the thickness of the hot-rolled steel sheet in this embodiment is 1.6 to 8.0 mm. The preferred lower limit of the thickness of the hot-rolled steel sheet in this embodiment is 1.8 mm, more preferably 2.0 mm. The preferred upper limit of the thickness of the hot-rolled steel sheet in this embodiment is 7.8 mm, more preferably 7.6 mm.
[0196] [Regarding hot-dip galvanized steel sheets using the hot-rolled steel sheet of this embodiment]
[0197] The hot-dip galvanized steel sheet of this embodiment includes the hot-rolled steel sheet of this embodiment described above and a hot-dip galvanized coating mainly containing Zn. The hot-dip galvanized coating is formed on the surface of the hot-rolled steel sheet. The hot-dip galvanized coating has a known structure. Hereinafter, the hot-dip galvanized coating will be described.
[0198] [About hot-dip galvanized coatings]
[0199] As described above, hot-dip galvanized coatings primarily contain Zn. Specifically, hot-dip galvanized coatings contain 65.00% or more Zn by mass. Hot-dip galvanized coatings can also be layers composed of so-called hot-dip galvanizing (GI). Hot-dip galvanizing contains less than 1.00% by mass of elements other than Zn, with the balance being Zn. Hot-dip galvanized coatings can also have chemical compositions other than hot-dip galvanizing (GI). Sufficient corrosion resistance can be obtained if the Zn content of the hot-dip galvanized coating is 65.00% or more by mass. The preferred lower limit for the Zn content of the hot-dip galvanized coating is 70.00%, more preferably 73.00%.
[0200] As mentioned above, hot-dip galvanized coatings can also have chemical compositions other than GI. The chemical composition of hot-dip galvanized coatings can be within a known range. For example, the chemical composition of hot-dip galvanized coatings can contain more than 65.00% Zn and 0.05% to 35.00% Al by mass%. Hot-dip galvanized coatings may contain impurities. Here, impurities refer to substances introduced from the raw materials during the hot-dip galvanizing process.
[0201] The preferred lower limit for Al content is 0.08%, more preferably 0.10%, and even more preferably 0.15%. The preferred upper limit for Al content is 33.00%, more preferably 30.00%, more preferably 28.00%, more preferably 25.00%, more preferably 23.00%, and even more preferably 21.00%.
[0202] The chemical composition of the hot-dip galvanized coating of this embodiment may further contain one or more elements selected from the first to seventh groups below. As is well known, these arbitrary elements are any elements that can be contained in the hot-dip galvanized coating. The percentages (%) for each arbitrary element below refer to mass%.
[0203] [Group 1]
[0204] Mg: 0–30.0%
[0205] [Group 2 (Sn Group)]
[0206] Select one or more from the group consisting of Sn: 0–2.00%, Bi: 0–2.00%, and In: 0–2.00%.
[0207] [Group 3 (Ca Group)]
[0208] Choose one or more from the group consisting of Ca: 0–3.00%, Y: 0–3.00%, La: 0–3.00%, and Ce: 0–3.00%.
[0209] [Group 4]
[0210] Si: 0~2.50%
[0211] [Group 5 (Cr group)]
[0212] Select one or more from the group consisting of Cr: 0–0.5%, Ti: 0–0.5%, Ni: 0–0.5%, Co: 0–0.5%, V: 0–0.5%, Nb: 0–0.5%, Cu: 0–0.5%, and Mn: 0–0.5%.
[0213] [Group 6]
[0214] Fe: 0~5.0%
[0215] [Group 7 (Sr Group)]
[0216] Select one or more from the group consisting of Sr: 0–0.5%, Sb: 0–0.5%, Pb: 0–0.5%, and B: 0–0.5%.
[0217] Mg is an easily oxidized element, and it improves the corrosion resistance of hot-dip galvanized coatings by sacrificing corrosion protection.
[0218] Tin (Sn), bismuth (Bi), and indium (In) form intermetallic compounds with Mg in hot-dip galvanized coatings. As a result, the corrosion resistance of hot-dip galvanized steel sheets is improved.
[0219] Calcium (Ca), yttrium (Y), lanthanum (La), and selenium (Ce) form intermetallic compounds with Al and Zn in hot-dip galvanized coatings. This results in improved corrosion resistance of hot-dip galvanized steel sheets.
[0220] Silicon (Si) improves the corrosion resistance of hot-dip galvanized steel sheets.
[0221] Chromium (Cr), titanium (Ti), nickel (Ni), cobalt (Co), vanadium (V), niobium (Nb), copper (Cu), and manganese (Mn) improve the appearance quality of hot-dip galvanized steel sheets.
[0222] Iron (Fe) increases the hardness of hot-dip galvanized coatings and improves the workability of hot-dip galvanized steel sheets.
[0223] Strontium (Sr), antimony (Sb), lead (Pb) and boron (B) enhance the metallic luster of hot-dip galvanized coatings and improve the appearance quality of hot-dip galvanized steel sheets.
[0224] [Methods for determining the chemical composition of hot-dip galvanized coatings]
[0225] The chemical composition of hot-dip galvanized coatings can be determined using the following method. The hot-dip galvanized coating is dissolved using hydrochloric acid with added inhibitors. For example, IBIT, manufactured by Asahi Chemical Industry Co., Ltd., can be used as an inhibitor. Elemental analysis is performed on the solution of the hot-dip galvanized coating, similar to the method described above in [Method for Determining the Chemical Composition of Hot-Rolled Steel Sheets]. The chemical composition of the hot-dip galvanized coating can be determined using this method.
[0226] Excellent resistance to LME can be obtained from the hot-dip galvanized steel sheets with hot-rolled steel sheet and hot-dip galvanized coating.
[0227] [Manufacturing method of hot-rolled steel sheet]
[0228] An example of a method for manufacturing a hot-rolled steel sheet according to this embodiment will be described. The method for manufacturing a hot-rolled steel sheet described below is an example used to manufacture the hot-rolled steel sheet of this embodiment.
[0229] An example of the method for manufacturing hot-rolled steel sheet according to this embodiment includes the following steps.
[0230] (Process 1) Blank preparation process
[0231] (Process 2) Rough rolling process
[0232] (Process 3) Finishing rolling process
[0233] (Process 4) Winding process
[0234] It should be noted that the above manufacturing method is implemented using manufacturing production line equipment. The manufacturing production line equipment, from upstream to downstream, includes a heating furnace, a roughing mill, a finishing mill, a water cooling unit, and a downcoiler. Multiple conveyor rollers are arranged between each piece of equipment.
[0235] The following is a description of each process.
[0236] [(Process 1) Blank Preparation Process]
[0237] In the billet preparation process, a billet with a chemical composition satisfying characteristic 1 is prepared. The slab is manufactured, for example, by the following method: Molten steel satisfying characteristic 1 is produced. Using the molten steel, a billet (slab or ingot) is manufactured by casting. For example, the slab is manufactured using the molten steel by a known continuous casting method. Alternatively, an ingot is manufactured using the molten steel by a known ingot casting method.
[0238] [(Process 2) Rough rolling process]
[0239] In the roughing process, a reversible roughing mill is used to hot-roll (rough rolling) the prepared billet (slab or ingot) to produce intermediate steel plates (bars). The heating temperature of the billet in the roughing process is, for example, 1250–1300°C. The time the billet spends in the furnace is 30 minutes or more, preferably 60 minutes or more. There is no particular upper limit to the furnace time, but it is, for example, 240 minutes.
[0240] [(Process 3) Finishing rolling process]
[0241] In the finishing rolling process, a finishing mill is used to further hot-roll (finish rolling) the intermediate steel plate to manufacture steel plates. The finishing mill is a tandem mill, consisting of multiple rolling stands ST1 to ST2 arranged in a row. K (K is a natural number). Each rolling mill stand ST has a pair of work rolls. The last rolling mill stand ST among the multiple rolling mill stands of the finishing mill is the one that presses down the intermediate steel plate. L The surface temperature of the steel plate at the exit side (where L is a natural number less than K) is defined as the finishing rolling temperature FT (°C). Rolling mill stand ST L It can be the rolling stand ST located at the very bottom of the finishing mill. K It can also be configured on a rolling mill stand ST K The rolling mill stand ST is located upstream.
[0242] In the finishing rolling process, the following conditions must be met.
[0243] (Condition 1)
[0244] Set the finishing rolling temperature FT (°C) to 850~950°C.
[0245] (Condition 2)
[0246] ST is the last rolling stand in the finishing mill that presses down the intermediate steel plate. L Upstream and adjacent to the rolling mill stand ST L ST configuration of rolling mill stand L-1 The reduction ratio R in L-1 Set it to 25% or higher.
[0247] (Condition 3)
[0248] ST rolling mill stand L The reduction ratio R in L For the reduction ratio R L-1 More than 0.90 times that of R. L / R L-1 Set it to 0.90 or higher.
[0249] (Condition 4)
[0250] By configuring it on the rolling mill stand ST L The water-cooling unit on the outlet side of the rolling mill stand ST L Cooling (water cooling) of the steel plate begins within 0.30 seconds after rolling is completed.
[0251] (Condition 5)
[0252] At the rolling mill stand ST L-1 The cooling of the steel plate in the water cooling device (water cooling) begins within 2.00 seconds after the rolling is completed.
[0253] (Condition 6)
[0254] The cooling rate CR1 between the finishing rolling temperature FT and the finishing rolling temperature FT-40℃ is set to be above 150℃ / second and below 250℃ / second.
[0255] (Condition 7)
[0256] The cooling rate CR2 from the finishing rolling temperature FT-40℃ to the coiling temperature CT is set to be above 25℃ / second and below 75℃ / second.
[0257] The following explains conditions 1 through 7.
[0258] [(Condition 1) Regarding the finishing temperature FT]
[0259] If the finishing rolling temperature FT exceeds 950°C, the grain boundary length GL becomes too short. Furthermore, the distance that boron (B) diffuses from the original austenite grains to the original austenite grain boundaries increases, reducing the boron segregation at the original austenite grain boundaries. On the other hand, if the finishing rolling temperature FT is below 850°C, it will place excessive load on the rolling mill stand ST. Therefore, the finishing rolling temperature FT is set at 850–950°C.
[0260] (Condition 2) Regarding the reduction ratio R L-1 ]
[0261] If the final rolling stand ST in the finishing mill is used to press down the intermediate steel plate... L Upstream and adjacent to the rolling mill stand ST L ST configuration of rolling mill stand L-1 The reduction ratio R in L-1If the reduction ratio is too low, the grain boundary length GL becomes too short. Furthermore, the distance that boron (B) diffuses from the original austenite grains to the original austenite grain boundaries increases, and the boron segregation at the original austenite grain boundaries decreases. Therefore, the reduction ratio R... L-1 Set it to 25% or higher.
[0262] (Condition 3) Regarding the reduction ratio R L ]
[0263] If the rolling mill stand ST L The reduction ratio R in L If it is too low, then at the ST of the rolling mill stand L-1 The strain imparted to the steel plate (coarse bar) in the rolling mill ST L During the reduction process, the strain accumulated in the steel plate immediately after finishing rolling becomes insufficient. In this case, the grain boundary length GL becomes too short. Furthermore, the diffusion distance of boron from the original austenite grains to the original austenite grain boundaries increases, and the boron segregation at the original austenite grain boundaries decreases. Therefore, the reduction rate R... L Let the reduction ratio be R. L-1 More than 0.90 times.
[0264] (Condition 4) Regarding the cooling start time t L ]
[0265] From the rolling mill stand ST L The rolling of the steel plate in the process is completed by the steel plate being mounted on the ST rolling mill stand. L The time from when the water-cooling device on the outlet side begins to cool the steel plate is defined as the cooling start time t. L If the cooling start time t L If the time is too long, the grain boundary length GL becomes too short. Furthermore, the distance that boron (B) diffuses from the original austenite grains to the original austenite grain boundaries increases, and the boron segregation at the original austenite grain boundaries decreases. Therefore, the cooling start time t... L Set it to less than 0.30 seconds.
[0266] Cooling start time t L The rolling mill stand ST can be determined using the following method. L The moving speed (m / s) of the steel plate at the exit side. Here, the rolling mill stand ST L The export side refers to the side connected to the rolling mill stand ST. L The point FP where the steel plate in contact with the pair of rollers just leaves the pair of work rollers. L Based on location FP L To be configured on the rolling mill stand ST L Calculate the cooling start time t by considering the distance from the starting position of the water-cooling device on the outlet side to the moving speed of the steel plate. L(seconds). The value obtained is rounded to the second decimal place after the third decimal place, and this value is taken as the cooling start time t. L (Second).
[0267] (Condition 5) Regarding the water cooling start time t L-1 ]
[0268] From the rolling mill stand ST L-1 The rolling of the steel plate in the process is completed by the steel plate being mounted on the ST rolling mill stand. L The time from when the water-cooling device on the outlet side begins to cool the steel plate is defined as the cooling start time t. L-1 If the cooling start time t L-1 If it is too long, then from the rolling mill stand ST L-1 The pressing is completed in the rolling mill stand ST. L The time from the start of the pressing process becomes too long. In this case, the rolling mill stand ST... L-1 The strain imparted to the steel plate by the compression during rolling mill stand ST L The pressure decreases during cooling. In this case, the grain boundary length GL becomes too short. Furthermore, the distance that boron diffuses from the original austenite grains to the original austenite grain boundaries increases, and the boron segregation at the original austenite grain boundaries decreases. Therefore, the cooling start time t... L-1 Set it to less than 2.00 seconds.
[0269] Cooling start time t L-1 The rolling mill stand ST can be determined using the following method. L-1 The moving speed (m / s) of the steel plate at the exit side. Here, the rolling mill stand ST L-1 The export side refers to the side connected to the rolling mill stand ST. L-1 The point FP where the steel plate in contact with the pair of rollers just leaves the pair of work rollers. L-1 Based on location FP L-1 to rolling mill stand ST L Location FP on the exit side L Given the distance and the moving speed of the steel plate, calculate the distance from point FP. L-1 to rolling mill stand ST L Location FP on the exit side L The conveying time of the steel plate (in seconds). The obtained value, rounded to the second decimal place, is taken as the cooling start time t. L-1 (seconds). The time obtained by adding the delivery time to the cooling start time tL is set as the cooling start time t. L-1 (Second).
[0270] [(Condition 6) Regarding the cooling rate CR1]
[0271] The average cooling rate in the temperature range from the finishing rolling temperature FT to FT-40℃ is defined as the cooling rate CR1 (℃ / second). If the cooling rate CR1 in this temperature range is too slow, the grain boundary length GL becomes too short. In addition, the distance that boron diffuses from the original austenite grains to the original austenite grain boundaries increases, and the boron segregation of the original austenite grain boundaries decreases.
[0272] On the other hand, if the cooling rate CR1 is too fast, the area ratio of bainitic ferrite in the manufactured hot-rolled steel sheet becomes too small.
[0273] Therefore, the cooling rate CR1 is set to be above 150°C / second and below 250°C / second.
[0274] The cooling rate CR1 can be calculated based on the time it takes for the surface temperature of the steel plate to rise from the finishing rolling temperature FT to the finishing rolling temperature FT-40℃. The cooling rate CR1 is the integer value obtained by rounding the first decimal place. It should be noted that within the temperature range from the finishing rolling temperature FT to FT-40℃, the steel plate is continuously cooled. That is, the temperature of the steel plate decreases continuously through cooling.
[0275] [(Condition 7) Regarding the cooling rate CR2]
[0276] The average cooling rate within the temperature range from the finishing rolling temperature FT-40℃ to the coiling temperature CT (℃) is defined as the cooling rate CR2.
[0277] If the cooling rate CR2 is too slow, the segregation of boron (B) towards the original austenite grain boundaries decreases. Consequently, excessive polygonal ferrite is formed, failing to achieve a sufficient area ratio of bainitic ferrite. Furthermore, the grain boundary length GL becomes too short, or the segregation degree of boron decreases.
[0278] On the other hand, if the cooling rate CR2 is too fast, the area ratio of bainitic ferrite in the manufactured hot-rolled steel sheet becomes too small.
[0279] Therefore, the cooling rate CR2 is above 25°C / second and below 75°C / second.
[0280] The cooling rate CR2 can be calculated based on the time it takes for the surface temperature of the steel sheet to rise from the finishing rolling temperature FT-40℃ to the coiling temperature CT (℃). The cooling rate CR2 is the integer value obtained by rounding the first decimal place. It should be noted that within the temperature range from the finishing rolling temperature FT-40℃ to the coiling temperature CT2, the steel sheet is continuously cooled. That is, the temperature of the steel sheet decreases continuously through cooling.
[0281] After cooling the steel plate from the finishing rolling temperature FT to FT-40℃ at a cooling rate CR1, without setting a residence time, the steel plate is rapidly cooled at a cooling rate CR2. That is, cooling at cooling rate CR1 and cooling at cooling rate CR2 are carried out continuously. Assuming that a residence time of more than 0.2 seconds is set after cooling at cooling rate CR1, the boron segregated at the original austenite grain boundaries will diffuse, and characteristic 3 or characteristic 4 will no longer be satisfied.
[0282] [(Process 4) Winding Process]
[0283] In the coiling process, a coiling device is used to coil the steel sheet that has passed through the cooling device into a coil shape. During the coiling process, Ti carbides are generated in the steel sheet. Here, the surface temperature of the steel sheet at the start of coiling is defined as the coiling temperature CT (°C). The coiling temperature CT also affects the microstructure of the hot-rolled steel sheet (the ratio of bainitic ferrite, polygonal ferrite, and bainite). Therefore, the coiling temperature CT is set to 500–630°C.
[0284] When the coiling temperature (CT) exceeds 630°C, coiling begins in the microstructure of the steel sheet before the phase transformation from austenite to bainitic ferrite is complete. Therefore, a portion of the austenite transforms into polygonal ferrite. As a result, the area fraction of bainitic ferrite in the hot-rolled steel sheet decreases.
[0285] On the other hand, if the coiling temperature CT is below 500°C, bainite is formed in the hot-rolled steel sheet. Therefore, the area ratio of bainitic ferrite in the hot-rolled steel sheet becomes lower.
[0286] The hot-rolled steel sheet of this embodiment is manufactured through the above manufacturing processes. As described above, the hot-rolled steel sheet of this embodiment can also be manufactured by other manufacturing methods besides the above-described manufacturing method.
[0287] Other processes in the manufacturing process of hot-rolled steel sheets
[0288] The method for manufacturing hot-rolled steel sheet according to this embodiment may include other processes besides those described above. For example, a surface finishing rolling process may be performed after the finishing rolling process and before the coiling process, or after the coiling process. In the surface finishing rolling process, the hot-rolled steel sheet is surface-finished. Through the surface finishing rolling process, the shape of the hot-rolled steel sheet is adjusted, or the surface roughness is adjusted, or the yield strength is adjusted. The thickness reduction rate in the surface finishing rolling process used to effectively obtain the above effects is, for example, 0.1% or more. The preferred upper limit of the thickness reduction rate in the surface finishing rolling process is 3.0%. In this case, it is possible to suppress the introduction of excessive strain into the hot-rolled steel sheet and maintain good ductility, bending, and flange properties.
[0289] [Method for manufacturing hot-dip galvanized steel sheet including the hot-rolled steel sheet of this embodiment]
[0290] The hot-dip galvanized steel sheet including the hot-rolled steel sheet of this embodiment can be manufactured by performing the following well-known hot-dip galvanizing process.
[0291] [Hot-dip galvanizing process]
[0292] In the hot-dip galvanizing process, a hot-dip galvanized coating having the aforementioned chemical composition is formed on the surface of a hot-rolled steel sheet. Specifically, a galvanizing bath is prepared. The composition of the galvanizing bath is adjusted according to the composition of the hot-dip galvanized coating to be formed. After immersing the hot-rolled steel sheet in the galvanizing bath for a certain period of time, the hot-rolled steel sheet is lifted out of the galvanizing bath using a known method. For example, a submersion roller is provided in the galvanizing bath. The hot-rolled steel sheet immersed in the galvanizing bath has its direction of travel changed to upward by the submersion roller.
[0293] A hot-dip galvanized coating is applied to the surface of a hot-rolled steel sheet removed from the galvanizing bath. The amount of hot-dip galvanized coating on the hot-rolled steel sheet is adjusted using a known gas wiping device. The hot-dip galvanized coating on the hot-rolled steel sheet removed from the galvanizing bath solidifies, forming a hot-dip galvanized coating layer. Through the above processes, a hot-dip galvanized steel sheet is manufactured.
[0294] Other processes in the manufacturing process of hot-dip galvanized steel sheets
[0295] The method for manufacturing hot-dip galvanized steel sheet according to this embodiment may also include manufacturing steps other than the hot-dip galvanizing process. For example, the method for manufacturing hot-dip galvanized steel sheet according to this embodiment may include a Ni pre-plating step before the hot-dip galvanizing process. In the Ni pre-plating step, the hot-rolled steel sheet is plated with Ni to form a Ni coating on the surface of the hot-rolled steel sheet. The hot-dip galvanizing process is then performed on the hot-rolled steel sheet with the Ni coating. In this case, the adhesion of the hot-dip galvanized coating to the hot-rolled steel sheet is improved.
[0296] The method for manufacturing hot-dip galvanized steel sheet according to this embodiment may further include a chemical conversion treatment step after the hot-dip galvanizing treatment step. In the chemical conversion treatment step, the manufactured hot-dip galvanized steel sheet is subjected to chemical conversion treatment to form a chemical conversion coating on the hot-dip galvanized coating. When performing the chemical conversion treatment step, the method of chemical conversion treatment is not particularly limited and can be a known method. For example, a known chromium chemical conversion coating can also be formed as the chemical conversion coating.
[0297] The method for manufacturing hot-dip galvanized steel sheet according to this embodiment can further include a surface rolling process after the hot-dip galvanizing process. In the surface rolling process, the manufactured hot-dip galvanized steel sheet is surface rolled. When performing the above-described chemical conversion treatment process, performing the surface rolling process before the chemical conversion treatment process can improve the adhesion of the chemical conversion coating. The thickness reduction rate in the surface rolling process is not particularly limited. A preferred thickness reduction rate in the surface rolling process is, for example, 0.1% to 3.0%.
[0298] The manufacturing method of hot-dip galvanized steel sheet may further include other manufacturing processes. The above-described manufacturing method is an example of a method for obtaining the hot-dip galvanized steel sheet of this embodiment. Therefore, the manufacturing method of hot-dip galvanized steel sheet of this embodiment is not limited to the above-described manufacturing method.
[0299] Example
[0300] The effects of one method of hot-rolled steel sheet and hot-dip galvanized steel sheet according to this embodiment will be explained in more detail through examples. The conditions in the following examples are examples of conditions adopted to confirm the feasibility and effects of hot-rolled steel sheet and hot-dip galvanized steel sheet according to this embodiment. Therefore, the hot-rolled steel sheet and hot-dip galvanized steel sheet according to this embodiment are not limited to this one example of conditions.
[0301] Hot-rolled steel sheets with the chemical composition shown in Table 1 were manufactured.
[0302] [Table 1]
[0303]
[0304] In Table 1, "-" indicates the absence of the corresponding element. It should be noted that the chemical composition of the steel plates for each test number was determined based on the method described in the above-mentioned [Determination Method of Chemical Composition of Hot-Rolled Steel Plates].
[0305] Slabs are manufactured by continuous casting of molten steel. The slabs are then subjected to roughing and finishing rolling processes. Specifically, the slabs are heated at 1250–1300°C for 60 minutes. The heated slabs are rolled using a roughing mill to produce intermediate steel plates. Furthermore, the intermediate steel plates are hot-rolled using a finishing mill to produce steel plates. The finishing rolling process involves (condition 1) the finishing temperature FT (°C) and (condition 2) the reduction rate R. L-1 (%), (Condition 3) Reduction rate R L / Reduction ratio R L-1 (Condition 4) Cooling start time t L (seconds), (Condition 5) Water cooling start time t L-1 The cooling rates CR1 (°C / sec) for (condition 6) and CR2 (°C / sec) for (condition 7) are shown in Table 2.
[0306] It should be noted that after cooling the steel plate from the finishing rolling temperature FT to the finishing rolling temperature FT-40°C at cooling rate CR1, no dwell time is set, and the steel plate is rapidly cooled at cooling rate CR2. That is, cooling at cooling rate CR1 and cooling at cooling rate CR2 are carried out continuously. In addition, within the temperature range from the finishing rolling temperature FT to FT-40°C, the temperature of the steel plate is continuously reduced by cooling. Similarly, within the temperature range from the finishing rolling temperature FT-40°C to the coiling temperature CT2, the temperature of the steel plate is continuously reduced by cooling.
[0307] [Table 2]
[0308]
[0309] The finished steel sheet was coiled into coils using a coiling device at a coiling temperature CT. The coiling temperature CT for each test number was 500–630℃. The coiled steel sheet was then allowed to cool naturally to room temperature, producing the hot-rolled steel sheets for each test number shown in Table 1. The thickness of the hot-rolled steel sheet was 2.3 mm.
[0310] [Evaluation Test]
[0311] The following evaluation tests were conducted on the hot-rolled steel plates for each test number.
[0312] (Experiment 1) Determination of the area ratio of bainitic ferrite
[0313] (Experiment 2) Determination of grain boundary length GL of the original austenite grains on the surface
[0314] (Experiment 3) Determination of Bo-segregation at the original austenite grain boundaries
[0315] (Test 4) Tensile Strength Test
[0316] (Experiment 5) Strength / Flange Balance Test
[0317] (Experiment 6) Evaluation Test of LME Resistance of Hot-Dip Galvanized Steel Sheet
[0318] The following describes Experiments 1 through 6.
[0319] [(Experiment 1) Determination of the area ratio of bainitic ferrite]
[0320] Based on the method described in the above-mentioned [Method for Determining the Area Ratio of Bainitic Ferrite], the area ratio (%) of bainitic ferrite in the hot-rolled steel sheet of each test number was calculated. The obtained area ratio of bainitic ferrite is shown in the "BF Area Ratio (%)" column of Table 3.
[0321] [Table 3]
[0322]
[0323] [(Experiment 2) Determination of grain boundary length GL of the original austenite grains on the surface]
[0324] Based on the method described in the above-mentioned [Method for Determining Grain Boundary Length GL], the grain boundary length GL (mm) of the surface region of the hot-rolled steel sheet for each test number was determined. The obtained grain boundary length GL is shown in the "Grain Boundary Length GL (mm)" column of Table 3.
[0325] [(Experiment 3) Determination of Bohr segregation at the original austenite grain boundaries]
[0326] Based on the method described above in "[Method for Determination of B Segregation at the Original Austenite Grain Boundaries]", the B segregation of the surface region of the hot-rolled steel sheet for each test number was determined. The obtained B segregation is shown in the "B Segregation" column of Table 3.
[0327] [(Test 4) Tensile Strength Test]
[0328] Based on the method described in the above-mentioned [Method for Determining Tensile Strength], the tensile strength TS (MPa) of the hot-rolled steel plate for each test number was determined. The obtained tensile strength TS is shown in the "TS (MPa)" column of Table 3.
[0329] [(Experiment 5) Strength / Flange Balance Test]
[0330] Based on the method described above in the [Method for Determining Strength / Flange Balance SB], the porosity λ (%) of the hot-rolled steel sheet for each test number was determined. Furthermore, using the tensile strength TS (MPa) and porosity (%) obtained in Test 4, the strength / flange balance SB was determined. The obtained porosity λ (%) is shown in the "λ (%)" column of Table 3. The obtained strength / flange balance SB is shown in the "SB (MPa·%)" column of Table 3.
[0331] [(Experiment 6) Evaluation Test of LME Resistance of Hot-Dip Galvanized Steel Sheet]
[0332] Manufacturing of hot-dip galvanized steel sheets
[0333] To evaluate the LME resistance of hot-dip galvanized steel sheets, hot-dip galvanized steel sheets were first manufactured using hot-rolled steel sheets of various test numbers. Specifically, the hot-dip galvanizing treatment of each test number was performed on the hot-rolled steel sheets, forming a hot-dip galvanized coating with the chemical composition shown in Table 4 on the surface of the hot-rolled steel sheets. The coating number of the hot-dip galvanized coating formed on the hot-rolled steel sheets of each test number is shown in the "Coating Number" column of "Coated Steel Sheets" in Table 3. The coating numbers shown in the "Coating Number" column of "Coated Steel Sheets" in Table 3 are equivalent to the coating numbers in Table 4. Through the above manufacturing process, hot-dip galvanized steel sheets were manufactured.
[0334] [Table 4]
[0335]
[0336] It should be noted that the element symbols listed to the left of the values in Table 4 refer to the elements contained therein. For example, in plating number P2, it refers to the element belonging to the Sn group, containing 0.11% Sn by mass. It should also be noted that the chemical composition of each plating number was determined using the method described in the above-mentioned [Determination Method of Chemical Composition of Hot-Dip Zinc-Conditioned Coatings].
[0337] The LME resistance of the manufactured hot-dip galvanized steel sheets for each test number was evaluated using the following method.
[0338] Sample steel sheets measuring 100mm × 75mm × thickness were collected from hot-dip galvanized steel sheets of each test number. The sample steel sheets were used to conduct [the following tests / procedures]. Figure 3 The arc welding is shown. Specifically, a cylindrical boss member 1 with a diameter of 20 mm and a length of 25 mm was prepared. The boss member 1 is made of steel equivalent to SS400 as specified in JIS G3101:2015.
[0339] like Figure 3 As shown, the boss member 1 is positioned at the center of the sample steel plate 2 with its axial direction aligned with the normal direction of the sample steel plate 2's surface. The boss member 1 is then welded to the sample steel plate 2 using arc welding. The welding wire used is YM-70CS as specified in JIS Z3312:2009 G69A2UCN1M2T. During arc welding, the weld bead 3, viewed from above, circles the boss member 1 clockwise. Arc welding continues beyond the weld start point until an overlapping area 4 is formed. The width of the overlapping area 4 is approximately 15 mm.
[0340] Set the current for arc welding to 190A and the voltage to 23V. Set the welding speed to 0.3m / min. Use a mixture of 20% CO2 and 80% argon as the shielding gas for arc welding. Set the shielding gas flow rate for arc welding to 20L / min.
[0341] In implementation Figure 3 Before the arc welding shown, as Figure 4 As shown, the sample steel plate 2 is pre-joined with the constraint plate 5. The constraint plate 5 is 120mm × 95mm × 4mm thick, and is made of steel plate equivalent to SS400 as specified in JIS G3101:2015. The sample steel plate 2 is placed on the surface of the constraint plate 5. The entire circumference of the placed sample steel plate 2 is welded to the constraint plate 5. The welding wire and welding conditions are set to be the same as those for welding the boss member 1 to the sample steel plate 2.
[0342] In implementation Figure 3 Before welding the boss component, such as Figure 4 As shown, the sample steel plate 2, circumferentially welded to the constraint plate 5, is placed on the stand 6. A clamp (not shown) is used to fix the sample steel plate 2 and the constraint plate 5 to the stand 6. After the sample steel plate 2 is fixed to the stand 6 by the clamp, as... Figure 3 As shown, the boss component 1 is welded to the sample steel plate 2 by arc welding.
[0343] After the boss component 1 is arc-welded to the sample steel plate 2, as follows: Figure 3 As shown, the boss member 1, sample steel plate 2, and constraint plate 5 were cut using a cutting surface 7 that passes through the central axis of the boss member 1 and through the overlapping area 4 of the weld bead 3. The cutting surface 7 was then observed at 100x magnification using an optical microscope. During the observation, the presence or absence of cracks (molten metal embrittlement cracks) in the sample steel plate 2 was visually confirmed. If cracks were observed, the crack length was measured. Specifically, the crack length (mm) in the depth direction (thickness direction) from the surface of the hot-rolled steel plate (the interface between the coating and the hot-rolled steel plate) was determined. The maximum crack length was determined from the measured crack lengths. If the maximum crack length is within 1.0 mm, it is judged as having excellent LME resistance (indicated by "E" (excellent) in the "LME resistance evaluation" column of Table 3). On the other hand, if the maximum crack length exceeds 1.0 mm, it is judged as having low LME resistance (indicated by "B" (poor) in the "LME resistance evaluation" column of Table 3).
[0344] [Evaluation Results]
[0345] Referring to Tables 1 to 4, the hot-rolled steel sheets tested from 1 to 18 meet characteristics 1 to 4. Therefore, excellent resistance to LME was obtained. It should be noted that in these hot-rolled steel sheets tested, the tensile strength TS is above 590 MPa, indicating high strength.
[0346] On the other hand, in test number 19, the Nb content was too low. Therefore, the grain boundary length GL was short, and the boron segregation was low. As a result, sufficient resistance to LME was not obtained.
[0347] In test number 20, the B content was too low. Therefore, the B segregation was low. As a result, adequate LME resistance was not achieved.
[0348] In tests 21 and 22, the finishing rolling temperature FT was too high. Consequently, the grain boundary length GL was short, and the boron segregation was low. As a result, sufficient resistance to LME was not achieved.
[0349] In tests 23 and 24, the reduction rate R... L-1 The value is too low. Therefore, the grain boundary length (GL) is short, and the boron segregation is low. As a result, sufficient resistance to LME is not achieved.
[0350] In tests 25 and 26, the reduction rate R... L relative to the reduction ratio R L-1 The ratio (=R) L / R L-1 The GL value is too low. Therefore, the grain boundary length (GL) is short, and the boron segregation is low. As a result, sufficient resistance to LME is not achieved.
[0351] In tests 27 and 28, the cooling start time t L The grain boundary length (GL) is too long. Therefore, the grain boundary length (GL) is short, and the boron segregation is low. As a result, sufficient resistance to LME is not achieved.
[0352] In experiments 29 and 30, the water cooling start time t L-1 The grain boundary length (GL) is too long. Therefore, the grain boundary length (GL) is short, and the boron segregation is low. As a result, sufficient resistance to LME is not achieved.
[0353] In tests 31 and 32, the cooling rate CR1 was too slow. Consequently, the grain boundary length GL was short, and the boron segregation was low. As a result, sufficient resistance to LME was not achieved.
[0354] In test number 33, the cooling rate CR1 was too fast. Therefore, the area ratio of bainitic ferrite was low. As a result, the strength / flanging balance SB was low.
[0355] In tests 34–36, the cooling rate CR2 was too slow. Therefore, in tests 34 and 35, the area fraction of bainitic ferrite was low, resulting in low boron segregation. Furthermore, in test 36, the boron segregation was also low. Consequently, in tests 34 and 35, sufficient LME resistance could not be obtained, and the tensile strength was less than 590 MPa. Furthermore, the strength / flanging balance SB was low. Additionally, in test 36, sufficient LME resistance was not obtained.
[0356] In test number 37, the cooling rate CR2 was too fast. Therefore, the area ratio of bainitic ferrite was low. As a result, the strength / flanging balance SB was low.
[0357] The embodiments of this disclosure have been described above. However, the above embodiments are merely illustrative examples for implementing this disclosure. Therefore, this disclosure is not limited to the above embodiments, and appropriate modifications can be made to the above embodiments without departing from its spirit.
Claims
1. A hot-rolled steel plate, which contains, by mass % C:0.030~0.110%、 Si: 0.01~0.50%, Mn: 0.50~1.50%, P: below 0.025% S: Below 0.010% Al:0.010~0.070%、 N: below 0.0070% Ti: 0.055~0.200%, Nb: 0.030~0.150%, B:0.0010~0.0050%、 V: 0~0.20%, and Cr:0~1.00%, The balance consists of Fe and impurities. In the microstructure, the area fraction of bainitic ferrite is over 85%. BO2 was detected by time-of-flight secondary ion mass spectrometry in the surface region of the hot-rolled steel sheet, extending from the surface along the thickness direction to a depth of 0.2 mm. - The total length of the original austenite grain boundaries is 1.20–5.00 mm per 100 μm × 100 μm. The boron segregation at the original austenite grain boundaries is above 40.
2. The hot-rolled steel plate according to claim 1, wherein it contains, by mass%, selected from... V: 0.01~0.20%, and Cr: 0.01% to 1.00% of one or more species in the group.
3. A hot-dip galvanized steel sheet, comprising: The hot-rolled steel sheet as described in claim 1 or claim 2; and Hot-dip galvanizing is a coating formed on the surface of the hot-rolled steel sheet, and contains more than 65.00% Zn by mass%.
Citation Information
Patent Citations
HIGH STRENGTH MOLTEN Zn-Al-Mg-BASED PLATED STEEL SHEET FOR AUTOMOBILE COMPONENT EXCELLENT IN FLEXURE PROCESSABILITY AND AUTOMOBILE COMPONENT USING THE SAME
JP2018145500A