Plated steel
By forming a coating with a specific composition and structure on the surface of coated steel, the problems of insufficient adhesion and corrosion resistance of coated steel in automotive parts are solved, and the coating achieves excellent performance and long-term corrosion resistance.
Patent Information
- Application Number
- CN202480091127.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2026-11-20
AI Technical Summary
When existing coated steel is used in automotive parts, the coating adhesion, post-coating corrosion resistance, substrate corrosion resistance, and sacrificial corrosion resistance are insufficient, making it difficult to meet the long-term durability requirements of corrosive environments.
By forming a coating with a specific composition and structure on the surface of the coated steel, including first, second and third regions with different Fe concentrations, the interface morphology between the coating and the base steel is controlled, and appropriate amounts of elements such as Al, Mg and Fe are added to the coating to optimize the chemical composition and microstructure of the coating, thereby improving the adhesion and corrosion resistance of the coating.
It achieves excellent coating adhesion, post-coating corrosion resistance, red rust resistance, and substrate corrosion resistance, thereby improving the service life and performance of coated steel in corrosive environments.
Smart Images

Figure CN123146708A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to coated steel. Background Technology
[0002] For example, steel structures are used in the civil engineering and infrastructure sector. These steel structures are exposed to harsh corrosive environments, such as coastal areas and areas where de-icing salt is applied. Therefore, stainless steel is used to inhibit corrosion and maintain the steel structure over the long term.
[0003] On the other hand, stainless steel uses high-cost alloying elements such as Cr and Ni. Therefore, the installation of steel structures using stainless steel is a costly undertaking. Consequently, pre-plated products (e.g., Zn-Al-Mg coated steel) are gradually being used as alternatives to stainless steel.
[0004] However, the coating can sometimes disappear due to welding in large steel structures and tubular steel structures. In addition, the coating can sometimes disappear partially due to corrosion from the cut ends. Moreover, steel components such as bolts and washers are inherently difficult to manufacture from sheet metal. In summary, generally speaking, large steel structures, tubular steel structures, bolts, washers and other steel components are manufactured by applying a plating treatment (so-called hot-dip galvanizing) to steel that has been processed into a specified shape.
[0005] As a post-plating treatment, molten Zn plating is widely used, but recently, Zn-Al-Mg plating has also been used to improve corrosion resistance.
[0006] Patent Document 1 describes a plated steel material comprising: a steel material; a surface coating disposed on the surface of the steel material and composed of a Zn-Al-Mg alloy layer with an Fe concentration of less than 3% by mass; an intermediate coating disposed between the steel material and the surface coating layer and comprising a Zn-Al-Mg alloy layer with a thickness of 3 μm or more and composed of an Fe concentration of 3% or more and less than 30% by mass; and an interface alloy layer disposed between the steel material and the intermediate coating layer, wherein the total thickness of the surface coating layer and the intermediate coating layer is 8 μm or more and less than 300 μm, the average chemical composition of the coating layer contains, by mass%, Zn: greater than 65.00%, Al: greater than 6.5% and less than 22.5%, Mg: greater than 3.0% and less than 12%, and impurities, and the Mg concentration of the intermediate coating layer is greater than 3.0% by mass. Existing technical documents Patent documents
[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-4403 Summary of the Invention The problem that the invention aims to solve
[0008] However, recent research has shown that hot-dip galvanized steel is used not only in the civil and infrastructure sectors but also as a raw material for automotive components. When using galvanized steel as a raw material for automotive components, there is a demand for improved coating adhesion, post-coating corrosion resistance, substrate corrosion protection, and sacrificial corrosion protection.
[0009] Patent document 1 describes the excellent resistance to red rust of the plated steel, but it makes no mention of the adhesion of the coating, the corrosion resistance after coating, the corrosion resistance of the substrate, and the sacrificial corrosion resistance.
[0010] Therefore, the objective of this invention is to provide coated steel with excellent coating adhesion, post-coating corrosion resistance, red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance. Methods for solving problems
[0011] To address the aforementioned issues, the present invention employs the following configuration. [1] A plated steel material comprising a base steel material and a coating disposed on the surface of the base steel material, wherein, The coating, as a chemical composition, contains, by mass%, Al: 5.0–40.0%, Mg: 0.5–15.0%, Fe: 5.0–40.0%, Si: 0–2.0%, Ca: 0–2.0%, and also contains one or two elements selected from groups A and B below, with the remainder being Zn and impurities. In a cross-section of the coated steel perpendicular to the surface, taking a cross-section of the coated steel of a predetermined length in a direction parallel to the surface as the observation area, the length L of the boundary line between the coating and the base steel satisfies the following equation (1). The coating comprises: a first region disposed on the surface side of the plated steel, having an Fe concentration of less than 5.0% by mass; a second region adjacent to the first region, having an Fe concentration of 5.0% by mass or more and less than 30.0% by mass; and a third region disposed between the second region and the parent steel, having an Fe concentration of 30.0% by mass or more and less than 80.0% by mass. The thickness of the first region is 5–100 μm, the thickness of the second region is 5–100 μm, and the thickness of the third region is 5–100 μm. The first region contains more than 0% and less than 5% Al-containing phase by area, wherein the Al-containing phase contains Zn and 20 to 99% by mass of Al. [Group A] Ni: 0 to 1.0%. [Group B] One or more of the following components, totaling 0-5%, are: Sb: 0-0.5%, Pb: 0-0.5%, Cu: 0-1.0%, Sn: 0-2.0%, Ti: 0-1.0%, Cr: 0-1.0%, Nb: 0-1.0%, Zr: 0-1.0%, Mn: 0-1.0%, Mo: 0-1.0%, Ag: 0-1.0%, Li: 0-1.0%, La: 0-0.5%, Ce: 0-0.5%, B: 0-0.5%, Y: 0-0.5%, P: 0-0.5%, Sr: 0-0.5%, Co: 0-0.5%, Bi: 0-0.5%, In: 0-0.5%, V: 0-0.5%, and W: 0-0.5%. (L-L0) / L0×100≥2.0(%) (1) In equation (1), L0 is the straight-line distance between one end and the other end of the boundary line in the observation area, and L is the length of the boundary line between the one end and the other end. [2] The plated steel according to [1] satisfies the following formula (2). (L-L0) / L0×100≥4.0(%) Equation (2) In equation (2), L0 is the straight-line distance between one end and the other end of the boundary line in the observation area, and L is the length of the boundary line between the one end and the other end. [3] The plated steel according to [1] satisfies the following formula (3). (L-L0) / L0×100≥6.0(%) Equation (3) In equation (3), L0 is the straight-line distance between one end and the other end of the boundary line in the observation area, and L is the length of the boundary line between the one end and the other end. [4] The plated steel according to any one of [1] to [3], wherein the thickness of the first region is 15 μm to 100 μm. [5] The plated steel according to any one of [1] to [3], wherein the area ratio of the Al-containing phase in the first region is less than 1%. [6] The coated steel according to any one of [1] to [3], wherein the first region contains a Mg-Zn phase comprising Zn and 20 to 60% by mass of Mg, and the area fraction of the Mg-Zn phase in the first region is 2% or more. [7] The coated steel according to any one of [1] to [3], wherein the first region contains a binary eutectic structure of Zn phase and Mg-Zn phase, and the area ratio of the binary eutectic structure in the first region is 1% or more. [8] The plated steel according to any one of [1] to [3], wherein the thickness of the second region is 15 μm to 100 μm. [9] The coated steel according to any one of [1] to [3], wherein the second region contains a Mg-Zn phase comprising Zn and 20 to 60% by mass of Mg, and the area fraction of the Mg-Zn phase in the second region is 5% or more.
[10] The plated steel according to any one of [1] to [3], wherein the second region contains an Fe-Al alloy phase with an equivalent circle diameter of 15 μm or less and an aspect ratio of 2 or more, and the area ratio of the Fe-Al alloy phase in the second region is 5% or more.
[11] The coated steel according to any one of [1] to [3], wherein the second region contains a binary eutectic structure of Zn phase and Mg-Zn phase, and the area ratio of the binary eutectic structure in the second region is 2% or more.
[12] The plated steel according to any one of [1] to [3], wherein the thickness of the third region is 15 μm to 100 μm.
[13] The coated steel according to any one of [1] to [3], wherein the third region contains a Mg-Zn phase comprising Zn and 20 to 60% by mass of Mg, and the area fraction of the Mg-Zn phase in the third region is 10% or more.
[14] The coated steel according to any one of [1] to [3], wherein the content of Mg in the chemical composition of the coating relative to the total amount of Zn and Mg (Mg / (Zn+Mg)(%)) is 5.0% or more.
[15] The coated steel according to any one of [1] to [3], wherein the content of Mg in the chemical composition of the coating relative to the total amount of Zn and Mg (Mg / (Zn+Mg)(%)) is 6.5% or more.
[16] The coated steel according to any one of [1] to [3], wherein the coating contains Sn at a concentration of 0.02 to 2.0% by mass, and the coating contains Mg2Sn phase. Invention Effects
[0012] According to the present invention, coated steel can be provided with excellent coating adhesion, post-coating corrosion resistance, red rust resistance, substrate corrosion resistance and sacrificial corrosion resistance. Attached Figure Description
[0013] Figure 1 This is a schematic cross-sectional view showing a plated steel material as an embodiment of the present invention. Figure 2This is a cross-sectional schematic diagram showing the plated steel as an embodiment of the present invention, and a diagram showing the observation area. Figure 3 This is a cross-sectional schematic diagram showing a plated steel material as an embodiment of the present invention, and a diagram illustrating the method for determining the extent of the first region and the second region. Figure 4 This is a cross-sectional schematic diagram showing a plated steel material as an embodiment of the present invention, and a diagram illustrating the method for determining the extent of the first region and the second region. Figure 5 This is a schematic cross-sectional view showing a plated steel material as an embodiment of the present invention. Figure 4 An enlarged view of region M1 in the image. Figure 6 This is a schematic cross-sectional view showing a plated steel material as an embodiment of the present invention. Figure 4 A magnified view of region M2 in the image. Detailed Implementation
[0014] The inventors conducted research to provide coated steel with excellent adhesion, corrosion resistance after coating, red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance.
[0015] Patent Document 1 describes a coated steel material that sometimes has an interface alloy layer with a thickness of 1 μm to 5 μm. Regarding the coated steel material described in Patent Document 1, if the interface alloy layer is formed too thickly, the adhesion and processability of the coating are drastically reduced; therefore, the thickness of the interface alloy layer is limited to 5 μm or less. However, the inventors have discovered that layers containing a large amount of Fe, such as the interface alloy layer, can sometimes improve the corrosion resistance of the substrate through a barrier effect. Therefore, the inventors have successfully formed a relatively thick layer containing a large amount of Fe between the Mg-Al-Zn alloy layer and the base steel, and controlled the morphology of the interface between the layer containing a large amount of Fe and the base steel. This improves the corrosion resistance of the substrate without reducing the adhesion of the coating, and further improves the corrosion resistance, red rust resistance, and sacrificial corrosion resistance after coating.
[0016] More specifically, it was found that by applying strain to the surface of the base steel before forming the coating using hot-dip galvanizing, and by controlling the cooling conditions after removal from the galvanizing bath to control the morphology of the interface between the base steel and the coating, it is possible to obtain coated steel with excellent corrosion resistance, coating adhesion, red rust resistance, substrate corrosion protection, and sacrificial corrosion protection. Furthermore, it was found that by suppressing the precipitation of Al-containing phases on the surface of the coating and keeping the Fe concentration low, the corrosion resistance and substrate corrosion protection after coating can be further improved.
[0017] The coated steel material according to embodiments of the present invention will be described below.
[0018] The plated steel of this embodiment is a plated steel having a base steel and a coating disposed on the surface of the base steel. The coating, as a chemical composition, contains, by mass%, Al: 5.0-40.0%, Mg: 0.5-15.0%, Fe: 5.0-40.0%, Si: 0-2.0%, Ca: 0-2.0%, and also contains one or two elements selected from groups A and B below, with the remainder being Zn and impurities. In a cross section perpendicular to the surface of the coated steel, when a cross section of the coated steel of a specified length in a direction parallel to the surface is taken as the observation area, the length L of the boundary line between the coating and the base steel satisfies the following formula (1), wherein the coating includes: a first region disposed on the surface side of the coated steel, having an Fe concentration of less than 5.0% by mass; a second region adjacent to the first region, having an Fe concentration of 5.0% by mass or more and less than 30.0% by mass; and a third region disposed between the second region and the base steel, having an Fe concentration of 30.0% by mass or more and less than 80.0% by mass, the thickness of the first region being 5 to 100 μm, the thickness of the second region being 5 to 100 μm, the thickness of the third region being 5 to 100 μm, and the first region containing 0% or more and less than 5% Al-containing phase in terms of area ratio, wherein the Al-containing phase contains Zn and 20 to 99% by mass of Al. [Group A] Ni: 0 to 1.0%. [Group B] One or more of the following components, totaling 0-5%, are: Sb: 0-0.5%, Pb: 0-0.5%, Cu: 0-1.0%, Sn: 0-2.0%, Ti: 0-1.0%, Cr: 0-1.0%, Nb: 0-1.0%, Zr: 0-1.0%, Mn: 0-1.0%, Mo: 0-1.0%, Ag: 0-1.0%, Li: 0-1.0%, La: 0-0.5%, Ce: 0-0.5%, B: 0-0.5%, Y: 0-0.5%, P: 0-0.5%, Sr: 0-0.5%, Co: 0-0.5%, Bi: 0-0.5%, In: 0-0.5%, V: 0-0.5%, and W: 0-0.5%. (L-L0) / L0×100≥2.0(%) (1) In equation (1), L0 is the straight-line distance between one end of the boundary line in the observation area and the other end, and L is the length of the boundary line between one end and the other end.
[0019] Furthermore, for the plated steel in this embodiment, it is preferable to satisfy the following formula (2). (L-L0) / L0×100≥4.0(%) Equation (2) Furthermore, for the plated steel in this embodiment, it is preferable to satisfy the following formula (3). (L-L0) / L0×100≥6.0(%) Equation (3) In equations (2) and (3), L0 is the straight-line distance between one end of the boundary line in the observation area and the other end, and L is the length of the boundary line between one end and the other end.
[0020] In addition, the thickness of the first region is preferably 15μm to 100μm. In addition, the area ratio of the Al-containing phase contained in the first region is preferably less than 1%. Furthermore, it is preferable that the first region contains a Mg-Zn phase comprising Zn and 20 to 60% by mass of Mg, and the area fraction of the Mg-Zn phase in the first region is 2% or more. Furthermore, it is preferable that the first region contains a binary eutectic structure of Zn phase and Mg-Zn phase, and the area ratio of the binary eutectic structure in the first region is more than 1%.
[0021] In addition, the thickness of the second region is preferably 15 μm to 100 μm. Furthermore, it is preferable that the second region contains a Mg-Zn phase comprising Zn and 20 to 60% by mass of Mg, and the area fraction of the Mg-Zn phase in the second region is 5% or more. Furthermore, it is preferable that the second region contains an Fe-Al alloy phase with an equivalent circle diameter of 15 μm or less and an aspect ratio of 2 or more, and the area fraction of the Fe-Al alloy phase in the second region is 5% or more. Furthermore, it is preferable that the second region contains a binary eutectic structure of Zn phase and Mg-Zn phase, and the area ratio of the binary eutectic structure in the second region is 2% or more.
[0022] In addition, the thickness of the third region is preferably 15μm to 100μm. Furthermore, it is preferable that the third region contains a Mg-Zn phase comprising Zn and 20 to 60% by mass of Mg, and the area fraction of the Mg-Zn phase in the third region is 10% or more.
[0023] In addition, the content of Mg in the chemical composition of the coating relative to the total amount of Zn and Mg (Mg / (Zn+Mg)(%)) is preferably 5.0% or more. In addition, the content of Mg in the chemical composition of the coating relative to the total amount of Zn and Mg (Mg / (Zn+Mg)(%)) is preferably 6.5% or more.
[0024] In addition, preferably, the coating contains Sn at a concentration of 0.02 to 2.0% by mass, and the coating contains the Mg2Sn phase.
[0025] In the following explanation, the "%" expression for the content of each element in the chemical composition refers to "mass %". The content of elements in the chemical composition is sometimes expressed as element concentration (e.g., Zn concentration, Mg concentration, etc.). "Coating adhesion" refers to the property of coatings being difficult to peel off. "Post-coating corrosion resistance" refers to the property of the coating itself to be difficult to corrode when a coating is applied to the surface of the coating. "Red rust resistance" refers to the property of inhibiting the formation of red rust in the coating during corrosion. "Substrate corrosion resistance" refers to the property of the coating itself being difficult to corrode. "Sacrificial corrosion resistance" refers to the property of inhibiting corrosion of the exposed parts of the base steel (such as the cut ends of the coated steel, the coating cracks during processing, and the parts of the base steel exposed by the peeling off of the coating).
[0026] like Figure 1 As shown, the plated steel 1 of this embodiment has a base steel 11. There are no particular limitations on the shape of the base steel 11; for example, examples of the shape of the base steel 11 include steel plates, angle bars with an L-shaped cross-section, and steel mesh. Furthermore, the base steel 11 can also be a formed base steel material such as steel pipes, civil engineering materials (fence ditches, corrugated pipes, drainage ditch covers, sand-proof boards, bolts, wire mesh, guardrails, waterproof walls, etc.), household appliance parts (air conditioner outdoor unit housings, etc.), and automotive parts (running parts, etc.). Additionally, the base steel 11 can also be composed of a formed product made by forming a steel plate into a predetermined shape. Furthermore, the base steel 11 can also be formed into the shape of, for example, an automotive part by welding two or more formed products made from steel plates into a predetermined shape together. Forming processes include various plastic forming methods such as stamping, roll forming, and bending.
[0027] There are no particular restrictions on the material of the master steel 11. The master steel 11 can be, for example, general steel, Al-killed steel, very low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steels containing strengthening elements such as Ni and Cr). The master steel 11 can also be hot-rolled steel plate, hot-rolled steel strip, cold-rolled steel plate, and cold-rolled steel strip as described in JIS G 3302:2010. There are also no particular restrictions on the manufacturing method of the steel plate (hot rolling method, pickling method, cold rolling method, etc.) or its specific manufacturing conditions.
[0028] Alternatively, the base steel 11 that becomes the base plate for plating can also be a pre-plated steel with a pre-plating layer formed on its surface. An example of a pre-plated steel is a Ni pre-plated steel with a Ni plating layer formed on the surface of the base steel 11. The pre-plated steel is obtained, for example, by electrolytic treatment or displacement plating. Electrolytic treatment is performed by immersing the base steel 11 in a sulfuric acid bath or chloride bath containing metal ions of various pre-plating components and then electrolytically treating it. Displacement plating is performed by immersing the base steel in an aqueous solution containing metal ions of various pre-plating components and pH adjusted with sulfuric acid, causing the metal to displace and precipitate.
[0029] The plated steel 1 of this embodiment has a plating layer 12 disposed on the surface of a base steel 11. As described later, the plating layer 12 includes a first region 12A with an Fe concentration of less than 5.0% by mass, a second region 12B with an Fe concentration of 5.0% by mass or more but less than 30.0% by mass, and a third region 12C with an Fe concentration of 30.0% by mass or more but less than 80.0% by mass. The plating layer 12, which includes the first region 12A, the second region 12B, and the third region 12C, contains Zn and other alloying elements in its chemical composition, and may also contain impurities. Alternatively, the plating layer 12 may also contain Zn and other alloying elements, with the remainder containing impurities.
[0030] The chemical composition of the coating will be described in detail below. It should be noted that, in order to solve the problem of the coated steel in this embodiment, elements with a lower limit of 0% concentration are not necessary, but are optional elements that are allowed to be included in the coating for the purpose of improving properties, etc.
[0031] <Al:5.0~40.0%> Al contributes to improved resistance to red rust, substrate corrosion protection, and sacrificial corrosion protection. Therefore, the Al concentration is set to 5.0% or higher. Alternatively, the Al concentration can be set to 10.0%, 15.0%, or 20.0% or higher. On the other hand, with excessive Al concentration, the Mg and Zn concentrations relatively decrease, and sacrificial corrosion protection may sometimes deteriorate. Furthermore, the appearance of the coating may sometimes be significantly reduced. Therefore, the Al concentration is set to 40.0% or lower. Alternatively, the Al concentration can be set to 35.0% or lower, or 30.0% or lower.
[0032] <Mg:0.5~15.0%> Mg is an essential element for ensuring post-coating corrosion resistance and sacrificial corrosion protection performance. It is also necessary for precipitating the MgZn₂ phase. Therefore, the Mg concentration is set to 0.5% or more. The Mg concentration may also be set to 2.0% or more, 3.0% or more, or 4.0% or more. On the other hand, if the Mg concentration is excessive, workability, particularly powdering resistance, may deteriorate, and further the base corrosion resistance may deteriorate. In addition, the appearance of the plating layer may be significantly degraded. Therefore, the Mg concentration is 15.0% or less. The Mg concentration may also be set to 10.0% or less, or 8.0% or less.
[0033] <Mg / (Zn+Mg): 5.0% or more, or 6.5% or more> The content ratio of Mg relative to the total amount of Zn and Mg in the chemical composition of the plating layer (Mg / (Zn+Mg) (%)) may be 5.0% or more, or 6.5% or more. Thereby, the sacrificial corrosion protection performance can be further improved. Mg and Zn in (Mg / (Zn+Mg)) are respectively the Mg concentration and Zn concentration in the plating layer.
[0034] <Fe: 5.0% to 40.0%> A certain amount of Fe is contained in the first region, the second region, and the third region of the plating layer according to the present embodiment. Most of the Fe is contained in the plating layer by diffusing from the base steel material serving as the plating original sheet into the plating layer. It has been confirmed that before the Fe concentration reaches 40.0% or less, even if Fe is contained in the plating layer, it does not adversely affect the performance. Most of Fe often exists as an Al-Fe alloy phase in the second region and the third region, so there is a tendency that the larger the thickness of the second region or the third region, the higher the Fe concentration. If the Fe concentration is less than 5.0%, the base corrosion resistance may deteriorate in the later stage of corrosion of the plating layer. Therefore, the Fe concentration is set to the range of 5.0 to 40.0%. The Fe concentration may be set to 10.0% or more, 15.0% or more, or 20.0% or more. In addition, the Fe concentration may be 30.0% or less, or 28.0% or less.
[0035] <Si: 0% to 2.0%> Si is an optionally added element, and may be 0%, but by containing Si, phases such as Mg₂Si phase, Al-Ca-Si-Zn phase, and Mg-Al-Si-Zn phase are formed in the plating layer, which can improve the corrosion resistance of the plating layer. Therefore, the Si concentration may also be set to more than 0%, 0.1% or more, or 0.2% or more. On the other hand, if the Si concentration is excessive, the base corrosion resistance and sacrificial corrosion protection performance may deteriorate. Therefore, the Si concentration is set to 2.0% or less. The Si concentration may also be set to 0.8% or less, or 0.6% or less.
[0036] <Ca: 0% to 2.0%> Ca is an optional additive element, and its content may be 0%. By containing Ca, phases such as Al-Ca-Zn phase, Al-Ca-Si-Zn phase, and Ca-Zn phase can be formed in the plating layer, which can improve the corrosion resistance of the plating layer. In addition, Ca is an element that can adjust the elution amount of Mg most suitable for imparting corrosion resistance to the substrate. Therefore, the Ca concentration may be 0.05% or more, or 0.1% or more. On the other hand, if the Ca concentration is excessive, the substrate corrosion resistance and workability may deteriorate. Therefore, the Ca concentration is set to 2.0% or less. The Ca concentration may also be set to 1.0% or less.
[0037] Further, the plating layer of the present embodiment may contain one or two elements selected from the group consisting of the following Group A and Group B.
[0038] [Group A] Ni: 0 to 1.0% [Group B] One or more of Sb: 0 to 0.5%, Pb: 0 to 0.5%, Cu: 0 to 1.0%, Sn: 0 to 2.0%, Ti: 0 to 1.0%, Cr: 0 to 1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mn: 0 to 1.0%, Mo: 0 to 1.0%, Ag: 0 to 1.0%, Li: 0 to 1.0%, La: 0 to 0.5%, Ce: 0 to 0.5%, B: 0 to 0.5%, Y: 0 to 0.5%, P: 0 to 0.5%, Sr: 0 to 0.5%, Co: 0 to 0.5%, Bi: 0 to 0.5%, In: 0 to 0.5%, V: 0 to 0.5%, W: 0 to 0.5%, with the total content being 0 to 5%.
[0039] <Ni: 0 to 1.0%> The concentration of Ni in Group A may be 0%. Ni contributes to the improvement of sacrificial corrosion resistance. Therefore, the Ni concentration may be set to 0.001% or more. On the other hand, if the Ni concentration is excessive, the substrate corrosion resistance may deteriorate. Therefore, the Ni concentration is set to 1.0% or less. The Ni concentration may be set to 0.8% or less, 0.6% or less, or 0.5% or less, 0.1% or less, 0.01% or less.
[0040] The plating layer of the present embodiment may contain a total of 0 to 5% of one or more of the above Group B elements. When the total content of Group B elements exceeds 5%, the substrate corrosion resistance or sacrificial corrosion resistance may decrease. Hereinafter, the elements of Group B will be described.
[0041] <Sb and Pb: 0 to 0.5% respectively> The concentrations of Sb and Pb may be 0%. Sb and Pb contribute to the improvement of sacrificial corrosion resistance. Therefore, the respective concentrations of Sb and Pb may be set to 0.001% or more, 0.005% or more, or 0.01% or more. On the other hand, if the concentrations of Sb and Pb are excessive, the base corrosion resistance may deteriorate in some cases. Therefore, the respective concentrations of Sb and Pb are set to 0.5% or less. The respective concentrations of Sb and Pb may be set to 0.3% or less, 0.1% or less, or 0.05% or less.
[0042] <Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li: 0 to 1.0% each> The concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li may each be 0%. These elements contribute to the improvement of sacrificial corrosion resistance. Therefore, the respective concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li may be set to 0.005% or more, or 0.01% or more. On the other hand, if the concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li are excessive, the base corrosion resistance may deteriorate in some cases. Therefore, the respective concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li are set to 1.0% or less. The respective concentrations of Cu, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li may be set to 0.5% or less, 0.1% or less, or 0.05% or less.
[0043] <Sn: 0 to 2.0%> The Sn concentration may also be 0%. Sn forms an intermetallic compound with Mg, and is an element that improves the sacrificial corrosion resistance of the coating. Therefore, the Sn concentration may be set to 0.01% or more, 0.02% or more, or 0.05% or more. However, if the Sn concentration is excessive, the base corrosion resistance may deteriorate in some cases. Therefore, the Sn concentration is set to 2.0% or less. The Sn concentration may be set to 1.5% or less, 1.0% or less, 0.5% or less, or 0.2% or less. To contain the Mg₂Sn phase, the Sn content is preferably 0.02 to 2.0%.
[0044] <La, Ce, B, Y, P and Sr: 0 to 0.5% each> The respective concentrations of La, Ce, B, Y, P and Sr may be 0%. La, Ce, B, Y, P and Sr contribute to the improvement of sacrificial corrosion resistance. Therefore, the concentrations of La, Ce, B, Y, P and Sr may each be set to 0.005% or more, or 0.01% or more. On the other hand, if the concentrations of La, Ce, B, Y, P and Sr are excessive, the substrate corrosion resistance may deteriorate in some cases. Therefore, the concentrations of La, Ce, B, Y, P and Sr are each set to 0.5% or less. The concentrations of La, Ce, B, Y, P and Sr may each be set to 0.2% or less, 0.1% or less, 0.05% or less, or 0.02% or less.
[0045] <Co, Bi, In, V, W: 0 to 0.5% each> The respective concentrations of Co, Bi, In, V and W may be 0%. Co, Bi, In, V and W contribute to the improvement of sacrificial corrosion resistance. Therefore, the concentrations of Co, Bi, In, V and W may each be set to 0.001% or more, 0.002% or more, or 0.004% or more. On the other hand, if the concentrations of Co, Bi, In, V and W are excessive, the substrate corrosion resistance may deteriorate in some cases. Therefore, the concentrations of Co, Bi, In, V and W are each set to 0.5% or less. The concentrations of Co, Bi, In, V and W may each be set to 0.1% or less, 0.05% or less, 0.02% or less, or 0.01% or less.
[0046] <Balance: Zn and impurities> The balance of the components of the plating layer according to the present embodiment is Zn and impurities. Zn is an element that imparts substrate corrosion resistance and sacrificial corrosion resistance to the plating layer. The Zn concentration is not particularly limited, and may be 15.0% or more, 30.0% or more, or 50.0% or more. Impurities refer to components contained in raw materials or components mixed in during the manufacturing process. For example, in the plating layer, components other than Fe may be slightly mixed as impurities in some cases due to mutual atomic diffusion between the base steel material and the plating bath.
[0047] The chemical composition of the plating layer is measured by the following method. First, an acid containing an inhibitor that suppresses corrosion of the base steel material is used for immersion at room temperature for 20 minutes, thereby obtaining an acid solution in which the plating layer is stripped and dissolved. Next, the obtained acid solution is subjected to quantitative analysis by ICP optical emission spectrometry. Thereby, the chemical composition of the plating layer can be obtained. As the acid containing the inhibitor, for example, a 10% hydrochloric acid solution added with 0.06 mass% of an inhibitor (IBIT 710K, manufactured by Asahi Chemical Industry Co., Ltd.) can be used. It should be noted that the chemical composition measured by the above method is the chemical composition of the entire plating layer.
[0048] Next, the plating layer of the present embodiment will be described in more detail. In the case of the coated steel in this embodiment, the interface between the coating and the base steel is an uneven surface. By making the interface between the coating and the base steel uneven, the adhesion of the coating is greatly improved.
[0049] Regarding the interface between the coating and the base steel, whether it represents an improvement in the adhesion of the coating depends on the surface texture. In a cross-section of the coated steel perpendicular to the surface, such as... Figure 2 As shown, when a cross-section of the coated steel, for example 100 μm long, parallel to the surface 1a of the coated steel, is used as the observation area, it can be confirmed by whether the length L of the boundary line 13 between the coating 12 and the base steel 11 satisfies the following formula (1). It should be noted that in Figure 2 In this study, a cross section of the coated steel with a length exceeding 100 μm in the direction parallel to surface 1a was observed. However, the length of this cross section is not limited to 100 μm and can be set to any length (specified length). Specifically, in the cross section of the coated steel perpendicular to surface 1a, a 100 μm long cross section of the coated steel in the direction parallel to surface 1a is taken as the observation area. Then, the straight-line distance L0 between one end 13a and the other end 13b of the boundary line 13 in the observation area, and the length L of the boundary line 13 between one end 13a and the other end 13b are calculated, and the value of (L-L0) / L0×100 is calculated. As shown in Equation (1), by making (L-L0) / L0×100 2.0% or more, the adhesion of the coating is improved. The coated steel of this embodiment can satisfy Equation (2) below, or it can satisfy Equation (3) below instead of Equation (1) below. There is no special requirement for the upper limit of (L-L0) / L0×100. If it is too large, the surface smoothness of the coating will be reduced. Therefore, it can be below 40.0%, below 10.0%, or below 9.0%.
[0050] (L-L0) / L0×100≥2.0(%) (1) (L-L0) / L0×100≥4.0(%) (2) (L-L0) / L0×100≥6.0(%) (3)
[0051] It should be noted that the observation area is defined as a cross-section of the coated steel, parallel to the surface 1a of the coated steel, observed using a SEM (JEOL JSM-7000F, accelerating voltage: 15kV) at a magnification of 1000x or higher. Regarding the resolution of the observation area, with a specified length of 100μm, it should be at least 2560 pixels horizontally and at least 1920 pixels vertically.
[0052] In addition, such as Figure 2As shown, when the surface 1a of the coated steel is not planar in the microscopic region (approximately 100 μm) of the observation area, it is possible to observe a larger area of the coated steel (e.g., several mm). 2 In the area described above, the direction parallel to the surface (e.g., the direction in which the plate extends when a plate is placed) is defined as the direction in which surface 1a extends. Based on this direction, the "section perpendicular to surface 1a" and the "direction parallel to surface 1a" are determined.
[0053] And, as Figure 2 As shown, one end 13a and the other end 13b of the boundary line 13 are the intersection points of the boundary line 13 and the straight line dividing the observation area. L0 is the length of the straight line connecting one end 13a and the other end 13b. L is the length of the boundary line 13 from one end 13a to the other end 13b. The length L of the boundary line 13 can be measured, for example, by using ImageJ, an image processing software that serves as the common domain. An image observed with SEM at a magnification of 1000x or higher is used as the image data at the resolution of 1000x or higher. For this image data, the length of the boundary line 13 is measured using the measurement function of ImageJ.
[0054] Next, the structure of the coating will be explained. The proportions of phases and microstructures contained in the coating of this embodiment affect the red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance of the coated steel. Even coatings with the same composition can have different phases or microstructures in their metallic microstructure due to different manufacturing methods, resulting in different properties. The metallic microstructure of the coating can be easily confirmed by mirror-finishing a cross-section of the coated steel perpendicular to the surface and analyzing this cross-section using an electron probe microanalyzer with a scanning electron microscope (SEM-EPMA, EPMA measuring device: JEOL JXA-8230, accelerating voltage: 15kV, current: 0.05μA, irradiation time: 50ms). The thickness of the coating in this embodiment is approximately 10–300 μm. For SEM, a magnification of 200–5000x was used to confirm a thickness of 36000 μm within this field of view. 2 The cross-section of the coating in the specified area. In this embodiment, the SEM field of view of the coating may become a localized observation field of view. Therefore, in order to obtain average information about the coating, 25 points of the field of view are selected from the aforementioned cross-section as the average information. That is, a total of 25 × 36000 μm is observed. 2 The metal structure within the field of view is used to determine the phase or area fraction of the metal structure constituting the coating. Multiple cross-sections can be measured as needed. It should be noted that the cross-section is preferably located near the center of the planar portion of the object being measured (sample).
[0055] Regarding the identification of each phase, in EPMA-based elemental analysis, the phase composition is confirmed through point analysis. Phases with similar compositions are read from the elemental mapping, thus identifying each phase. In point analysis, for 250 pixel × 250 pixel lattice points in the EPMA resolution results, the elements Al, Zn, Mg, Fe, and Si are analyzed. The electron beam diameter is set to less than 1 μm. Phases with similar compositions can be identified by elemental mapping, thus allowing for differentiation. That is, regarding the identification of each phase, for areas other than the layered structure [Al / MgZn2 binary eutectic structure], the phase composition is confirmed through point analysis in SEM-EPMA analysis. Phases with similar compositions are read from elemental mapping, etc., thus identifying the phase. The area of each phase is measured using the image analysis software "Image J (Ver. 1.54f)". The area ratio (%) of each phase is the proportion of the total area of each phase in the entire field of view.
[0056] It should be noted that the area ratio (area percentage) of each phase in the field of view is equivalent to the volume percentage in the first, second, or third region of that phase.
[0057] As described above, the coating of this embodiment includes a first region with an Fe concentration of less than 5.0% by mass, a second region with an Fe concentration of 5.0% by mass or more but less than 30.0% by mass, and a third region with an Fe concentration of 30.0% by mass or more but less than 80.0% by mass. Hereinafter, the phases and microstructures contained in any one or more of the first, second, and third regions will be described.
[0058] Al-containing phase The Al-containing phase in this embodiment is a phase containing Zn and 20–99% by mass of Al. The Zn content in the Al-containing phase can be 1–80% by mass. Additionally, the Al-containing phase may also contain other elements totaling less than 5% by mass. These other elements refer to Mg, Si, etc. The Al-containing phase can be a form in which Zn is dissolved in Al, or it can be an aggregate of fine Zn phase with a particle size less than 1 μm and fine Al phase with a particle size less than 1 μm. The Al-containing phase is determined by elemental mapping using EPMA, thereby enabling clear differentiation from other phases and structures.
[0059] Al-containing phases are sometimes present in the first region. However, since the corrosion resistance of coatings containing a large amount of Al-containing phases in the first region is reduced after application, it is preferable that the first region contains as little Al-containing phase as possible.
[0060] Mg-Zn phase The Mg-Zn phase is a phase containing Zn and 20–60% by mass of Mg. The Zn content in the Mg-Zn phase can be 40–80% by mass. Additionally, the Mg-Zn phase may also contain other elements totaling less than 5% by mass. These other elements refer to Mg, Si, etc. Specifically, examples of the Mg-Zn phase include MgZn2 and Mg2Zn. 11 Equal. The Mg-Zn phase is determined by using elemental mapping of EPMA to identify the phase containing Zn and 20–60% by mass of Mg, thus clearly distinguishing it from the Al-containing phase, [the binary eutectic structure of Zn / MgZn2], etc.
[0061] The Mg-Zn phase is contained in the first region. Additionally, the Mg-Zn phase is sometimes contained in the second and third regions. By including the Mg-Zn phase in the coating, resistance to red rust, substrate corrosion protection, and sacrificial corrosion protection are improved.
[0062] [Binary eutectic structure of Zn / MgZn2] The binary eutectic structure of Zn / MgZn2 is a eutectic structure composed of the η-Zn phase and the MgZn2 phase. The layered structure of the binary eutectic structure of Zn / MgZn2, represented by the η-Zn and MgZn2 phases, is clearly distinguishable from Al-, Mg-Zn, Zn, and Fe-Al phases in SEM backscattered electron images. It should be noted that for the identification of structures other than the aforementioned Al and Mg-Zn phases in the binary eutectic structure of Zn / MgZn2, it is sufficient to examine the remaining portions other than the layered structure of the binary eutectic structure of Zn / MgZn2.
[0063] The binary eutectic structure of Zn / MgZn2 is sometimes contained in the first or second region. By allowing the binary eutectic structure of Zn / MgZn2 to exist to some extent, the corrosion resistance after coating can be improved.
[0064] Fe-Al alloy phase The Fe-Al alloy phase is a phase containing Al and 20–60% by mass of Fe. The Al content in the Fe-Al alloy phase can also be 40–80% by mass. Additionally, the Fe-Al alloy phase may contain other elements totaling less than 5% by mass. These other elements refer to Si, etc. The Fe-Al alloy phase is primarily composed of Al₅Fe. Besides Al₅Fe, the Fe-Al alloy phase sometimes also contains AlFe, Al₃Fe, Al₅Fe₂, etc. Furthermore, when the coating contains Si, the Fe-Al alloy phase sometimes becomes a Fe-Al-Si compound phase. As identified Fe-Al-Si compound phases, there is the AlFeSi phase, and as isomers, there exist α, β, q₁, q₂-AlFeSi phases, etc.
[0065] The Fe-Al alloy phase is mainly contained in the second and third regions. Fe-Al alloys have certain corrosion resistance compared to Fe. In addition, the Fe-Al alloy phase is an intermetallic compound phase, thus possessing high insulation and resistance to corrosion.
[0066] Other intermetallic compounds may also be present in the coating as a remainder. Examples of other intermetallic compounds include Mg2Si phase, Mg2Sn phase, Zn phase, Al-Ca-Zn phase, Al-Ca-Si-Zn phase, Ca-Zn phase, and Mg-Al-Si-Zn phase.
[0067] Mg2Si phase In coatings containing Si, Si sometimes precipitates as the Mg2Si phase. The Mg2Si phase exhibits excellent corrosion resistance. The presence of Mg2Si can be determined using SEM / EPMA, as described later. A phase with Mg content of 50–70 atomic% and Si content of 30–50 atomic% can be identified as the Mg2Si phase.
[0068] Mg2Sn phase By including the Mg₂Sn phase in the coating, the corrosion resistance and substrate corrosion protection of the coated steel are further improved. The Mg₂Sn phase is present in small amounts, and its presence can be confirmed by X-ray diffraction. To ensure the presence of the Mg₂Sn phase, the preferred Sn content in the coating's chemical composition is 0.02–2.0%. The presence of the Mg₂Sn phase was determined by X-ray diffraction using Cu-Kα rays at an X-ray output of 50 kV and 300 mA, within a range of 2θ = 10–30°, with a scanning step of 0.02°. The presence of the Mg₂Sn phase was confirmed when a diffraction peak was detected at 23.4 ± 0.3°.
[0069] Zn phase The Zn phase can contain more than 80% by mass of Zn, less than 20% by mass of Al, and may also contain less than 5% by mass of other elements such as Si and Mg. The Zn phase is sometimes contained within the first or second region. The inclusion of the Zn phase further enhances corrosion resistance. The Zn phase appears white in backscattered electron microscopy (SEM) images, thus allowing for clear differentiation from other phases and structures.
[0070] Al-Ca-Zn phase, Al-Ca-Si-Zn phase, Ca-Zn phase, Mg-Al-Si-Zn phase If the plating bath contains Ca and Si, these intermetallic compound phases sometimes precipitate in the coating. These intermetallic compound phases exhibit superior corrosion resistance compared to the aforementioned Mg₂Si phase. Besides SEM and EPMA analysis, the presence of these intermetallic compound phases can also be confirmed by X-ray diffraction. The X-ray diffraction conditions can be the same as those for the Mg₂Sn phase.
[0071] As described above, the coating of this embodiment includes a first region with an Fe concentration of less than 5.0% by mass, a second region with an Fe concentration of 5.0% by mass or more but less than 30.0% by mass, and a third region with an Fe concentration of 30.0% by mass or more but less than 80.0% by mass. The boundaries of the first region, the second region, and the third region are defined as follows.
[0072] First, a section perpendicular to the surface of the coated steel is exposed. The exposed section is then mirror-finished. The Fe concentration is determined using point-based analysis with an electron probe microanalyzer (EPMA). It should be noted that the analytical results obtained from the EPMA can be used to identify the various phases of the coating.
[0073] First, as the first stage of measurement, such as Figure 3 As shown, multiple straight analytical lines are set in the cross-section of the coating 12, parallel to a direction orthogonal to the thickness direction of the coating 12. Ten analytical lines are evenly spaced along the thickness direction of the coating. Alternatively, when the coating thickness exceeds 100 μm, the spacing between the analytical lines is set to 10 μm. Ten measurement points are set at 10 μm intervals along each analytical line in a direction orthogonal to the thickness direction. If the length of the analytical line is less than 90 μm, making it impossible to set 10 measurement points at 10 μm intervals, the interval can be appropriately reduced or the number of measurement points reduced. Figure 3 In the diagram, the dashed lines are analytical lines, and the black dots on the analytical lines are measurement points. It should be noted that the analytical lines are set in a manner that maximizes the number of analytical lines in the cross-section of the coating 12. When the thickness of the coating 12 is less than 10 μm, the first stage of measurement is omitted, and the second stage of measurement is performed as described below.
[0074] At each measurement point, the Fe concentration (mass %) in the coating was determined by point analysis. The electron beam output for point analysis was set to 15 kV and 4 × 10⁻⁶. -7A. The spot diameter of the electron beam tip is set to 0.2 μm. For each analytical line, the average Fe concentration at 10 measurement points is calculated, and this average value is taken as the Fe concentration in each analytical line. Then, analytical line A, where the Fe concentration is less than 5.0% and the Fe concentration is closest to 5.0%, and analytical line B, where the Fe concentration exceeds 5.0% and the Fe concentration is closest to 5.0%, are determined. Furthermore, analytical line C, where the Fe concentration is less than 30.0% and the Fe concentration is closest to 30.0%, and analytical line D, where the Fe concentration exceeds 30.0% and the Fe concentration is closest to 30.0%, are determined.
[0075] Next, as the second stage of measurement, such as Figure 4 and Figure 5 As shown, Fe concentration was analyzed in the region between analytical lines A and B on the cross-section of coating 12. Additionally, as... Figure 4 and Figure 6 As shown, Fe concentration was also analyzed in the region between analytical lines C and D. Figure 4 This is a graph showing analysis lines A, B, C, and D among multiple analysis lines. Figure 5 yes Figure 4 An enlarged view of region M1 between analysis line A and analysis line B. Figure 6 yes Figure 4 An enlarged view of region M2 between analysis line C and analysis line D.
[0076] In the second phase of the determination, such as Figures 4-6 As shown, multiple analytical lines are set at 1 μm intervals along the thickness direction of the coating in the regions between analytical lines A and B, and between analytical lines C and D. Ten measurement points are set at 10 μm intervals along each analytical line. Figure 4 as well as Figure 5 As an example, an analysis line is shown positioned between analysis line A and analysis line B. Additionally, in... Figure 4 as well as Figure 6 The diagram shows a portion of the analytical line positioned between analytical line C and analytical line D. Then, at each measurement point, the Fe concentration (mass %) was determined by point analysis. The electron beam output and the spot diameter of the electron beam tip were set to be the same as in the first stage of the measurement.
[0077] For each analytical line, the average Fe concentration at 10 measurement points was calculated, and this average value was taken as the Fe concentration for each analytical line. Then, the analytical line with the Fe concentration closest to 5.0% was designated as the "Fe concentration 5.0% analytical line" (e.g., Figure 5 The analytical line F5). Additionally, the analytical line with the Fe concentration closest to 30.0% is designated as the "analytical line for Fe concentration of 30.0%" (e.g., Figure 6The analysis line F30 is used as the boundary line. Using the analysis line F5 with an Fe concentration of 5.0% by mass as the boundary line, the region closer to the surface 1a of the coated steel (the side of analysis line A) than analysis line F5 is designated as the first region 12A. Furthermore, using the analysis line F30 with an Fe concentration of 30.0% by mass as the boundary line, the region closer to the base steel than analysis line F30 is designated as the third region 12C. The region between analysis lines F5 and F30 is designated as the second region 12B.
[0078] That is, such as Figures 4-6 As shown, the first region 12A is defined as the region between the surface 1a of the coated steel and the analytical line F5 with an Fe concentration of 5.0% by mass. The second region 12B is defined as the region between the analytical line F5 with an Fe concentration of 5.0% by mass and the analytical line F30 with an Fe concentration of 30.0% by mass. The third region 12C is defined as the region between the analytical line F30 with an Fe concentration of 30.0% by mass and the interface 13 between the coating 12 and the base steel 11. The first region 12A, the second region 12B, and the third region 12C are layered throughout the entire topography of the coating 12. The first region 12A is located in the coating 12 closer to the surface 1a of the coated steel 1 than the second region 12B. The second region 12B is located in the coating 12 between the first region 12A and the third region 12C. The third region 12C is located in the coating 12 adjacent to the base steel 11, closer to the base steel 11 than the second region 12B.
[0079] <Region 1> The first region is a region disposed on the surface side of the coated steel with an Fe concentration of less than 5.0% by mass. The upper surface of the first region constitutes the surface of the coated steel. By having the first region, the red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance of the coated steel are improved. In addition, by having the first region with a low area ratio of Al phase, the corrosion resistance after coating is improved.
[0080] Sometimes, the first region contains an Al-containing phase at a proportion of less than 5% by area. The area proportion of the Al-containing phase is preferably less than 1%, and more preferably 0%. Since the higher the Al-containing phase content, the worse the corrosion resistance after coating, it is preferable that the first region does not contain an Al-containing phase, and even if it does, it is preferably less than 5% at most. If the area proportion of the Al-containing phase in the first region is more than 5%, the corrosion resistance after coating will decrease.
[0081] Furthermore, the first region may contain 2% or more of the Mg-Zn phase by area percentage. Compared with the Al-containing phase, the Mg-Zn phase exhibits superior corrosion resistance and sacrificial corrosion protection after coating. Therefore, to improve the corrosion resistance and sacrificial corrosion protection of the coated steel, it is preferable to include 2% or more of the Mg-Zn phase in the first region. The area percentage of the Mg-Zn phase in the first region is preferably 5% or more, 10% or more, 15% or more, 20% or more, 30% or more, or 40% or more. There is no particular upper limit to the Mg-Zn phase in the first region; for example, it is preferably 95% or less, but it can also be 90% or less.
[0082] Furthermore, the first region may contain 1% or more of the [Zn / MgZn2 binary eutectic structure] by area percentage. By including the [Zn / MgZn2 binary eutectic structure] in the first region, the corrosion resistance and sacrificial corrosion protection of the coated steel are further improved after coating. The area percentage of the [Zn / MgZn2 binary eutectic structure] in the first region is preferably 3% or more, 5% or more, or 10% or more. The upper limit of the [Zn / MgZn2 binary eutectic structure] in the first region is not particularly limited; for example, it is preferably 90% or less, but it may also be 80% or less, 60% or less, 50% or less, or 40% or less.
[0083] The first region may also contain Zn phase, Mg2Si phase, Mg2Sn phase, Al-Ca-Zn phase, Al-Ca-Si-Zn phase, Ca-Zn phase, Mg-Al-Si-Zn phase, etc. as the remainder. Furthermore, the first region may also contain Fe-Al alloy phase at an area fraction of less than 3%.
[0084] The thickness of the first region is 5–100 μm. By making the thickness of the first region 5 μm or more, the corrosion resistance, red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance after coating are improved. On the other hand, it is sometimes difficult to manufacture the first region to exceed 100 μm in thickness, so the upper limit is set to 100 μm or less. The thickness of the first region can be 70 μm or less, 50 μm or less, or 40 μm or less. In addition, the thickness of the first region can be 10 μm or more, or 15 μm or more. The thickness of the first region is defined as the average thickness. Regarding the average thickness, the distance in the thickness direction of the coating from the surface of the coating to the analytical line F5 of 5.0% Fe concentration is measured at 10 locations with intervals of 10 μm or more in the image obtained by observing the above-mentioned SEM, and the arithmetic mean of these measurements is taken as the average thickness.
[0085] <Second Region> The second region is located between the first and third regions and contains 5.0% by mass and less than 30.0% by mass of Fe. The second region contains Fe at a proportion of less than 30.0% by mass, and also contains Zn, Al, and Mg. Therefore, the second region sometimes contains Fe-Al alloy phase and Mg-Zn phase. Preferably, the second region contains more Mg-Zn phase than Fe-Al alloy phase. Furthermore, the second region may contain more Fe-Al alloy phase than Mg-Zn phase, and the difference in their contents, in terms of area ratio, may be less than 12%, preferably less than 10%, and more preferably less than 5%. The Mg-Zn phase improves resistance to red rust, substrate corrosion resistance, and sacrificial corrosion resistance, while the Fe-Al alloy phase improves substrate corrosion resistance.
[0086] By incorporating this second region into the coating, the substrate's corrosion resistance and resistance to red rust are improved, and the corrosion resistance after coating is further enhanced. The improved corrosion resistance and resistance to red rust resulting from the second region become apparent in the later stages of corrosion.
[0087] In addition, sometimes a binary eutectic structure of Zn / MgZn2 is contained in the second region. As a result, the corrosion resistance is improved after coating.
[0088] When observing the cross-section of the second region, the Fe-Al alloy phase contained in the second region is preferably needle-shaped with a circular equivalent diameter of 15 μm or less and an aspect ratio of 2 or more. The Fe-Al alloy phase contributes to improving the corrosion resistance of the substrate through its barrier effect. On the other hand, the Fe-Al alloy phase is prone to becoming the starting point for red rust formation during corrosion, but since the Fe-Al alloy phase contained in the second region is needle-shaped, it is more effective in suppressing the formation of red rust.
[0089] The morphology of the Fe-Al alloy phase that may be included in the second region can be determined by confirming the proportion of phases and structures contained in the coating of this embodiment using an electron probe microanalysis (SEM-EPMA) instrument. The morphology can be determined to be needle-shaped Fe-Al alloy phase with an equivalent circle diameter of 15 μm or less and an aspect ratio of 2 or more.
[0090] The area fraction of the Fe-Al alloy phase in the second region can be 5% or more. This further improves the corrosion resistance of the substrate. The area fraction of the Fe-Al alloy phase in the second region can be 10%, 20%, or 30% or more. There is no particular upper limit to the Fe-Al alloy phase content in the second region; for example, it is preferably 80% or less, 70% or less, or 60% or less.
[0091] The area fraction of the Mg-Zn phase in the second region can be 5% or more. This further improves sacrificial corrosion resistance, in addition to substrate corrosion resistance and resistance to red rust. Compared to the Fe-Al phase, the Mg-Zn phase offers higher sacrificial corrosion resistance. Therefore, from the viewpoint of sacrificial corrosion resistance, a higher concentration of Mg-Zn phase in the second region is preferred. The area fraction of the Mg-Zn phase in the second region can be 10% or more, 20% or more, 30% or more, or 40% or more. There is no particular upper limit for the Mg-Zn phase concentration in the second region; for example, it is preferably 70% or less, 60% or less, or 50% or less.
[0092] The area fraction of the [Zn / MgZn2 binary eutectic structure] in the second region can be 2% or more. This further improves the corrosion resistance and sacrificial corrosion protection of the coated steel. The area fraction of the [Zn / MgZn2 binary eutectic structure] in the second region can be 5% or more, 8% or more, or 10% or more. There is no particular upper limit to the [Zn / MgZn2 binary eutectic structure] in the second region; for example, it is preferably 90% or less, but it can also be 80% or less, 50% or less, 30% or less, or 20% or less.
[0093] The second region may also contain Al phase, Mg2Si phase, Mg2Sn phase, Zn phase, Al-Ca-Zn phase, Al-Ca-Si-Zn phase, Ca-Zn phase, Mg-Al-Si-Zn phase, etc., as a remainder. The area fraction of these remainder phases is preferably less than 10% in total.
[0094] The thickness of the second region is set to 5–100 μm. By making the thickness of the second region 5 μm or more, the substrate corrosion resistance, sacrificial corrosion resistance, and resistance to red rust are improved. Preferably, it is 15 μm or more. On the other hand, it is sometimes difficult to manufacture a second region thickness exceeding 100 μm, therefore the upper limit is set to 100 μm or less. The thickness of the second region can be 70 μm or less, 50 μm or less, 40 μm or less, or 30 μm or less. The thickness of the second region is set as the average thickness. Regarding the average thickness, the distance in the thickness direction of the coating between the analysis line of 5.0% Fe concentration and the analysis line of 30.0% Fe concentration was measured at 10 locations with intervals of more than 10 μm in the image obtained by the SEM observation described above, and the arithmetic mean of these measurements was taken as the average thickness.
[0095] <Third Region> The third region is located between the second region and the base steel and contains 30.0% to 80.0% Fe by mass. Within the third region, the presence of Fe in the range of 30.0% to 80.0% by mass results in a large amount of Fe-Al alloy phase. Of the phases or microstructure contained in the third region, the Fe-Al alloy phase accounts for the largest area fraction. Additionally, the third region sometimes contains approximately the same amount of Mg-Zn phase as the Fe-Al alloy layer. By including a third region with 30% or more Fe in the coating, the substrate corrosion resistance of the coating is improved. The reason for this improved substrate corrosion resistance is presumably because the third region contains 30.0% or more Fe, thus containing a large amount of Fe-Al alloy phase, which functions as a barrier layer for the base steel.
[0096] Furthermore, as mentioned above, the third region may contain not only the Fe-Al alloy phase but also the Mg-Zn phase. The area fraction of the Mg-Zn phase in the third region can be 10% or more, 15% or more, 20% or more, or 30% or more. This further improves sacrificial corrosion resistance. Compared to the Fe-Al phase, the Mg-Zn phase exhibits higher sacrificial corrosion resistance. Therefore, from the viewpoint of sacrificial corrosion resistance, a higher proportion of Mg-Zn phase in the third region is preferred. There is no particular upper limit to the amount of MgZn2 phase in the third region; for example, it is preferably 50% or less.
[0097] The third region may also contain Al phase, Mg2Si phase, Mg2Sn phase, Zn phase, Al-Ca-Zn phase, Al-Ca-Si-Zn phase, Ca-Zn phase, Mg-Al-Si-Zn phase, etc., as the remaining portion. The area fraction of these remaining phases is preferably less than 10% in total.
[0098] The thickness of the third region is set to 5–100 μm. By making the thickness of the third region 5 μm or more, the corrosion resistance of the substrate is improved. On the other hand, making the thickness of the third region exceed 100 μm is sometimes difficult in manufacturing, so the upper limit is set to 100 μm or less. The thickness of the third region can be 70 μm or less, 50 μm or less, 40 μm or less, or 30 μm or less. Furthermore, the thickness of the third region can exceed 5 μm or exceed 15 μm. The thickness of the third region is set as the average thickness. Regarding the average thickness, in the image obtained by the SEM observation described above, the distance in the thickness direction of the coating between the analytical line of 30.0% Fe concentration and the boundary line between the coating and the base steel is measured at 10 locations at intervals of 10 μm or more, and the arithmetic mean of these distances is taken as the average thickness.
[0099] The thickness of the coating is the combined thickness of the first region, the second region, and the third region. That is, the thickness of the coating is preferably 15 μm to 300 μm.
[0100] Furthermore, regarding the plated steel in this embodiment, it is preferable that the base steel and the third region are in direct contact. That is, it is preferable that there is no alloy layer different from the third region between the base steel and the third region.
[0101] Next, the manufacturing method of the plated steel according to this embodiment will be described. The method for manufacturing coated steel according to this embodiment includes: a shot peening process for shot peening the surface of a base steel; a flux coating process for coating the base steel after shot peening with flux; a first coating process for immersing the base steel after flux coating in a first coating bath and then lifting it out; a second coating process for immersing the base steel after the first coating process in a second coating bath and then lifting it out; and a cooling process for cooling the coating after the second coating process. Thus, the coated steel according to this embodiment is manufactured using a so-called two-stage coating method.
[0102] The first plating bath in the first plating process is a plating bath containing Zn, and the second plating bath in the second plating process is a plating bath containing Al, Mg, and Zn. The plating method in the first and second plating processes is the so-called immersion plating method.
[0103] In the shot peening process, the surface of the base steel is shot peened. This applies strain to the surface of the base steel. The conditions for shot peening are described below. Various shapes and materials of shot peening material can be considered, but steel shot peening material according to JIS Z0311:2004 is preferred, and spherical steel shot peening material is particularly preferred. The center particle size of the shot peening material can be in the range of 40 to 450 μm. The hardness can be Hv390 to 510. Specifically, for example, steel shot (TSH-30) manufactured by WINOA IKK JAPAN Co., Ltd. can be used.
[0104] In the shot peening process, following the general rules for shot peening treatment of billet adjustment (JIS Z 0310:2016), centrifugal force or air pressure is used to cause the shot to collide with the surface of the base steel. The amount of shot peening material projected can be 5–400 kg / m². 2 The range. The shot peening material can be projected at a rate of 10 kg / m. 2 The above can also be 15kg / m 2 That's all. Additionally, the shot peening material can be projected at a rate of 100 kg / m². 2 The following can also be 50kg / m 2 the following.
[0105] Strain is applied to the surface of the base steel through a shot peening process. If the strained base steel is subjected to a first plating process and a second plating process as an immersion plating method, when the base steel is immersed in the second plating bath, the reaction between Fe in the Fe-Zn layer formed by the base steel or the first plating process and Al in the plating bath becomes more active, resulting in the formation of a relatively large amount of Fe-Al alloy phase. In addition, by applying strain, the reaction rate between the base steel and Zn in the first plating process is distributed, thereby making the interface between the plating layer and the base steel more likely to become uneven, and a plating steel that satisfies the relationship of the above equation (1) can be obtained. As a result, the adhesion of the plating layer is improved.
[0106] Next, in the flux coating process, the base steel is immersed in a flux aqueous solution at 80°C for 30 seconds, then lifted out and dried in an atmospheric atmosphere at 150°C. As a flux, various salts such as NaCl, KCl, NaF, SnCl2, SnCl4, and BiCl3, as well as surfactants, are dissolved based on ZnCl2, and a solution acidic with hydrochloric acid is used as needed. By coating the base steel with flux before plating, the oxides on the surface of the base steel are removed, and the plating reaction is stabilized. Examples of fluxes include those prepared by dissolving NaCl in water at concentrations of 0–100 g / L, KCl at 0–100 g / L, SnCl2 at 0–20 g / L, and ZnCl2 at 100–300 g / L.
[0107] Next, in the first plating process, the flux-coated steel is immersed in the first plating bath and then lifted out. The first plating bath is composed mainly of Zn, and is known as a zinc plating bath.
[0108] A zinc plating layer is formed by immersing the base steel in a first plating bath. Furthermore, regarding the zinc plating layer, it is preferable to form an Fe-Zn alloy layer on the base steel side. That is, the zinc plating layer preferably consists of an Fe-Zn alloy layer and an n-Zn layer formed sequentially from the base steel side. The thickness of the Fe-Zn alloy layer in the zinc plating layer is not particularly limited. Alternatively, the Zn plating layer can also be an alloyed zinc plating layer where the alloying of Fe and Zn extends to the surface of the plating layer.
[0109] The thickness of the zinc plating layer or alloyed zinc plating layer is preferably 5 to 150 μm, more preferably 20 to 60 μm. When the thickness of these plating layers is less than 5 μm, the thickness of the third region is less than 5 μm, and the corrosion resistance of the substrate of the plating layer is reduced. In addition, it is difficult to manufacture these plating layers to a thickness of more than 150 μm.
[0110] The immersion time in the first plating bath can be, for example, in the range of 10 to 600 seconds. This forms an Fe-Zn alloy layer within the zinc plating layer. If the immersion time is less than 10 seconds, the Fe-Zn alloy layer cannot be sufficiently formed, and the interface between the final plating layer and the base steel is not easily formed, resulting in reduced adhesion of the plating layer. On the other hand, if the immersion time exceeds 600 seconds, the Fe-Zn alloy layer overgrows, which in turn reduces the adhesion of the plating layer.
[0111] The temperature of the first plating bath can be in the range of 420 to 480°C. When the bath temperature is high, the growth of the Fe-Zn alloy layer is faster, and the Fe-Zn alloy layer is excessively formed. However, when the bath temperature is low, the adhesion of the plating layer is sometimes reduced, and plating defects such as incomplete plating and foreign matter adhesion are more likely to occur.
[0112] After being lifted from the first plating bath, the amount of plating is adjusted as needed by methods such as purging and wiping with N2 gas and adjusting the speed at which the steel plate is extracted from the plating bath.
[0113] Next, in the second plating process, the base steel with a zinc plating layer or an alloyed zinc plating layer formed is immersed in the second plating bath and then lifted out. The composition of the second plating bath can be approximately the same as the chemical composition of the plating layer. Alternatively, the composition of the second plating bath can be appropriately adjusted to bring it into the range of the chemical composition of the plating layer of this embodiment. Specifically, it is preferable that the amount of Mg, Al, and other alloying elements other than Zn is about 1.01 to 1.20 times greater than the target value of the chemical composition of the plating layer, so as to bring it into the range of the chemical composition of the plating layer of this embodiment.
[0114] By immersing the parent steel with the zinc coating in a second plating bath, Zn is dissolved from the η-Zn layer contained in the zinc coating and Zn and Al are replaced in the Fe-Zn alloy layer, thereby forming a third region containing the Fe-Al alloy phase.
[0115] Furthermore, if the mother steel with the alloyed zinc coating is immersed in the second plating bath, Zn and Al are replaced in the Fe-Zn alloy layer of the alloyed zinc coating, thereby forming a third region containing the Fe-Al alloy phase.
[0116] The immersion time in the second plating bath can, for example, be in the range of 5 to 300 seconds. This promotes the growth of the third and second regions. When the immersion time is less than 5 seconds, the second and third regions cannot be fully formed. In addition, the interface between the coating and the base steel is not easily formed, resulting in reduced corrosion resistance of the substrate and decreased adhesion of the coating. On the other hand, if the immersion time exceeds 300 seconds, the second and third regions will overgrow, and the coating itself will be prone to cracking.
[0117] The temperature of the second plating bath can be in the range of 400℃ to 680℃, or 460℃ to 670℃. If the bath temperature is high, the growth of the Fe-Al alloy phase is faster, and excessive formation of the Fe-Al alloy phase may lead to the formation of other interfacial alloy layers between the third region and the base steel, resulting in a significant increase in the wear and tear on the plating equipment. At low bath temperatures, plating defects such as incomplete plating and foreign matter adhesion are more likely to occur.
[0118] After being lifted out of the second plating bath, the amount of plating is adjusted as needed by purging and wiping with N2 gas, and by adjusting the speed at which the mother steel is extracted from the plating bath.
[0119] Next, as a cooling process, the coating is cooled (controlled cooling). In this cooling process, cooling is performed at an average cooling rate of less than 5.0°C / second, more preferably less than 2.0°C / second, until the temperature of the coating drops from the bath temperature to 330°C, which is the controlled cooling stop temperature. The controlled cooling stop temperature is preferably 330°C or less. Cooling is performed, for example, by blowing cooling gas. When cooling is performed by blowing cooling gas, multiple blowing nozzles for cooling gas are arranged along the transport path of the base steel, and cooling gas is blown from these nozzles. The type of cooling gas can be air, nitrogen (N2), argon, etc., preferably nitrogen (N2).
[0120] By cooling at an average cooling rate of less than 5.0 °C / s, the alloying reaction of Fe and Al remaining in an unreacted state on the surface of the coating proceeds, consuming Al and Fe in the coating. As a result, a first region with an Fe concentration of less than 5.0% by mass is formed. Furthermore, the consumption of Al in the reaction with Fe results in less precipitation of the Al-containing phase, reducing the area fraction of the Al-containing phase in the first region. Additionally, by cooling from the bath temperature at an average cooling rate of less than 5.0 °C / s to a controlled cooling stop temperature, for example, 330 °C, Mg-Zn phase precipitation occurs. Subsequently, a eutectic reaction of the Zn and MgZn2 phases occurs, promoting the formation of a binary eutectic structure of the η-Zn and MgZn2 phases ([Zn / MgZn2 binary eutectic structure]).
[0121] On the other hand, on the base steel side of the coating, Fe diffusing from the base steel reacts with Al in the plating bath, thereby forming a second region with an Fe concentration of 5.0% or more. In this second region, in addition to containing a large amount of Fe-Al alloy phase, a Mg-Zn phase is sometimes also formed.
[0122] By operating as described above, the plated steel of this embodiment can be manufactured.
[0123] In addition, the coated steel of this embodiment can also be formed by methods such as vapor deposition, spraying, and cold spraying to achieve the same effect as when formed by hot-dip galvanizing. Example
[0124] The effects of the present invention will be specifically illustrated below through examples. As the master steel, master steel of the shapes described below A, B and C (SS400 as described in JIS G 3101) shall be used.
[0125] A: A steel plate with a length of 200mm, a width of 100mm, and a thickness of 3.2mm. B: The steel plate of A above was bent at the center of the plate width at a bending angle of 90°, and the cross-section is an L-shaped angle bar (length 200mm, short side length 50mm, plate thickness 3.2mm). C: Expanded metal mesh (XS-62 (plate thickness 3.2mm) as specified in JIS G 3351:1987). In the case of expanded metal mesh, "the surface of the coated steel" refers to the surface of the plate-shaped integral shape with multiple through holes, which is equivalent to a plane orthogonal to the plate thickness direction.
[0126] It should be noted that, in the case of materials B and C mentioned above, it is difficult to observe, measure, and evaluate the adhesion of the coating. Therefore, in the test cases where the parent steel is material B or material C, the parent steel was changed to material A to manufacture the coated steel. Observation, measurement, and evaluation were carried out on the coated steel with material A as the parent steel.
[0127] The aforementioned master steel was subjected to a shot peening process. In this process, steel shot (TSH-30) manufactured by WINOA IKK JAPAN Co., Ltd. was used as the shot material. Following the General Rules for Shot Peening Treatment of Billet Adjustment (JIS Z 0310:2016), the shot material was forced to collide with the surface of the master steel using air pressure. The amount of shot material projected was set as described in Tables 2A and 2B. The projection conditions were set as follows: blasting pressure: 0.5 MPa, distance from nozzle to sample (master steel): 800 mm, projection angle: 90°.
[0128] Next, the master steel after shot peening undergoes a flux coating process. In this process, the steel is immersed in a flux aqueous solution (ZnCl2 / NaCl / SnCl2=220g / 20g / 10g / L) at 80°C for 30 seconds, then lifted out and thoroughly dried in a drying oven at 150°C.
[0129] Next, the master steel after the flux coating process is immersed in the first plating bath and then lifted out, followed by immersion in the second plating bath and then lifted out. The temperature of the first plating bath is set to 460°C, and the temperature of the second plating bath is set as described in Tables 2A and 2B. The immersion time in the first plating bath is set to 180 seconds, and the immersion time in the second plating bath is set as described in Tables 2A and 2B. The first plating bath is a zinc plating bath containing more than 95% Zn. The thickness of the zinc plating layer formed by immersion in the first plating bath is in the range of 5 to 150 μm, and the zinc plating layer includes an Fe-Zn alloy layer and an n-zinc layer. The second plating bath is a Zn-Al-Mg plating bath containing Al, Mg, other alloying elements, and Zn. The composition of the second plating bath is appropriately adjusted so that the composition of the second plating bath is approximately the same as the chemical composition of the final coating, or is a target value for the chemical composition of the final coating. Specifically, the amounts of Mg, Al, and other alloying elements other than Zn are increased by 1.2 times compared to the target values for the chemical composition of the coating.
[0130] Next, as a cooling process, compressed air is blown onto the mother steel sample lifted from the second plating bath as a cooling gas, and cooling is performed while controlling the cooling rate from the plating bath temperature to the controlled cooling stop temperature of 330°C. The cooling rate is set as described in Tables 2A and 2B. The sample is then allowed to cool naturally within a temperature range below 330°C. This process is used to manufacture the plated steel.
[0131] Regarding the composition of the coating, for samples cut into 30mm×30mm pieces, the elements dissolved in the hydrochloric acid solution were quantitatively analyzed using ICP luminescence spectrophotometry, as described above, and the determination was carried out accordingly.
[0132] Whether the boundary between the coating and the base steel becomes a concave-convex surface that satisfies equation (1) is confirmed as follows.
[0133] First, a small sample measuring 20mm × 15mm × 3.2mm was collected from the coated steel. After resin embedding, it was ground to a mirror finish, exposing the cross-section of the coated steel perpendicular to the surface. The sample was observed using an electric field emission scanning electron microscope (SEM) (JEOL JSM-7000F, accelerating voltage: 15kV), and image data were obtained. A 100μm long cross-section of the coated steel, parallel to the surface of the coated steel, observed at a magnification of 1000x or higher, was used as the observation area. The image resolution was 2560 pixels or higher horizontally and 1920 pixels or higher vertically.
[0134] For the image data, L0 and L are calculated using the method described above. It should be noted that the coating and the base steel are distinguished based on an Fe concentration of 90% obtained from the EPMA analysis above; the portion with an Fe concentration above 90% is considered the base steel. Then, it is evaluated whether the relationship between L0 and L satisfies equation (1). The calculation results (values) on the left side of equation (1) are shown in Tables 3A and 3B.
[0135] In addition, the boundaries of the first, second, and third regions of the coating are defined as follows. Small samples measuring 20mm × 15mm × 3.2mm were collected from the coated steel. After resin embedding, the samples were ground to a mirror finish, exposing the cross-section perpendicular to the surface of the coated steel. The sample was observed using an electron probe microanalyzer with a scanning electron microscope (SEM-EPMA, EPMA measurement device: JEOL JXA-8230, accelerating voltage: 15kV, current: 0.05μA, irradiation time: 50ms), while the Fe concentration was determined based on point analysis.
[0136] First, as the first stage of measurement, such as Figure 3 As shown, in the exposed cross-section of the coating, straight analytical lines are set parallel to the direction orthogonal to the coating thickness direction. Ten analytical lines are set at equal intervals along the coating thickness direction. On each analytical line, ten measurement points are set at 10 μm intervals in a direction orthogonal to the coating thickness direction. Figure 3 In the diagram, the single-dot dashed line is the analysis line, and the black dots on the analysis line are the measurement points.
[0137] At each analytical line, the Fe concentration (mass %) in the coating was determined by point analysis. The point analysis conditions were set as described above. For each analytical line, the average Fe concentration at 10 measurement points was calculated, and this average value was taken as the Fe concentration for each analytical line. Then, analytical line A, where the Fe concentration is less than 5.0% and the Fe concentration is closest to 5.0%, and analytical line B, where the Fe concentration is greater than 5.0% and the Fe concentration is closest to 5.0%, were determined. Furthermore, analytical line C, where the Fe concentration is less than 30.0% and the Fe concentration is closest to 30.0%, and analytical line D, where the Fe concentration is greater than 30.0% and the Fe concentration is closest to 30.0%, were determined.
[0138] Next, as the second stage of measurement, analytical lines for 5.0% Fe concentration and 30.0% Fe concentration were determined using the above method. Using the 5.0% Fe concentration analytical line as the boundary, the region closer to the surface of the coated steel than this analytical line was designated as the first region. Similarly, using the 30.0% Fe concentration analytical line as the boundary, the region closer to the base steel than this analytical line was designated as the third region. Furthermore, the region between the 5.0% Fe concentration analytical line and the 30.0% Fe concentration analytical line was designated as the second region.
[0139] Next, the area fractions of the phases and microstructures in the first, second, and third regions were determined as follows: Using the samples used to determine the first, second, and third regions, cross-sections of the coating in the thickness direction perpendicular to the surface of the base steel were observed. The SEM magnification was set to 200–50,000x, confirming a thickness of 36,000 μm. 2 The cross-section of the coating in the specified area. Since the field of view of the coating observed by SEM may become a localized view, to obtain average information about the coating, 25 points are selected from any cross-section as the average information. That is, a total of 36000 × 25 μm is observed. 2 The metal structure in the field of view is used to determine the phase or area ratio of the metal structure that constitutes the coating.
[0140] First, the eutectic structure consisting of Zn and MgZn2 phases, exhibiting a layered structure, is defined as the [Zn / MgZn2 binary eutectic structure]. For regions other than the [Zn / MgZn2 binary eutectic structure], the phase containing Zn and 20–99% by mass of Al is defined as the Al-containing phase. Furthermore, the phase containing Zn and 20–60% by mass of Mg is defined as the Mg-Zn phase. Next, the phase containing Al and 20–60% by mass of Fe is defined as the Fe-Al alloy phase. Then, the area fraction of these phases and structures is determined.
[0141] Furthermore, the presence of the Mg2Sn phase was confirmed using the methods described above. The presence of the Mg2Sn phase was determined when a diffraction peak was detected at 23.4 ± 0.3°. The results are shown in Tables 3A and 3B.
[0142] The coating adhesion was evaluated as follows. The coated steel was subjected to a spalling test. Using a gravel impact tester, 400g of No. 6 gravel (JIS A500, particle size 5–13mm) was struck from a distance of 50cm at room temperature under an air pressure of 400kPa. The projection angle was set to 90° relative to the surface of the base steel. The test piece was then subjected to ultrasonic cleaning (room temperature, pure water, 10 minutes). The coating adhesion was evaluated based on the weight per unit area (g / m²) of the test piece before ultrasonic cleaning. 2The weight per unit area (g / m²) of the test piece after ultrasonic cleaning 2 The difference in weight reduction is used to evaluate the adhesion of the plating. The evaluation criteria are as follows, with AAA, AA, and A considered acceptable.
[0143] AAA: Weight reduction less than 10g / m 2 AA: Weight reduced to 10g / m 2 Above and below 60g / m 2 A: Weight reduced to 60g / m 2 Above and below 120g / m 2 B: Weight reduced to 120g / m 2 above
[0144] The corrosion resistance after coating was evaluated as follows. A primer, intermediate, and top coat were applied to the surface of the plating on the steel. The primer was formed by applying HI-PON 20 DECHLO epoxy resin coating (trade name: Nippon Paint Co., Ltd.), with a thickness of 50 μm. The intermediate coat was formed by applying HI-PON 30 MASTIC K (trade name: Nippon Paint Co., Ltd.), with a thickness of 30 μm. The top coat was formed by applying HI-PON 50 (trade name: Nippon Paint Co., Ltd.), with a thickness of 30 μm. The coated steel was then subjected to a corrosion acceleration test as specified in JASO-CCT-M609, with cuts made to the base steel using a cutting tool. After 360 cycles, the corrosion resistance after coating was determined by the maximum expansion width on one side of the cut. The evaluation criteria are as follows, with AAA, AA, and A considered as qualified.
[0145] AAA: Below 0.5mm AA: More than 0.5mm but less than 1mm A: More than 1mm but less than 2mm B: More than 2mm
[0146] Resistance to red rust was evaluated as follows: The coated steel was subjected to the corrosion-promoting test specified in JASO-CCT-M609. The number of cycles required to produce red rust was then determined. Based on the number of cycles required to produce red rust, the evaluation was performed according to the following criteria.
[0147] AAA: The red rust formation cycle is more than 1200 cycles. AA: The red rust formation cycle is more than 900 cycles but less than 1200 cycles. A: Red rust formation occurs within a cycle of 540 to 900 cycles. B: The red rust formation cycle is less than 540 cycles.
[0148] The corrosion resistance of the substrate was evaluated as follows. Coated steel was cut into samples 150 mm in length and 70 mm in width and subjected to a corrosion acceleration test as specified in JASO-CCT-M609. The corrosion depth (μm) in the samples after 1560 cycles was then measured for evaluation. During the test, a 30 mm section was observed at the midpoint of the sample's length (75 mm) and the center of its width. The section, embedded in resin and mirror-polished, was observed using an optical microscope at 40x magnification, and the resulting field of view was photographed. The maximum corrosion depth (μm) was measured at 30 mm in the width direction of the section. The evaluation criteria are as follows, with AAA, AA, and A considered acceptable.
[0149] AAA: Less than 50μm AA: 50μm or larger and less than 200μm A: Above 200μm and below 800μm B: Above 800μm
[0150] Sacrificial corrosion resistance is evaluated as follows: The coated steel is cut perpendicular to its surface using a fine cutter, exposing the cut end face. That is, the cross-section of the coating and the cross-section of the base steel are exposed at the cut end face. A neutral salt spray test as specified in JIS Z2371:2015 is then performed on the cut end face, and the time (in hours) until red rust appears is measured. The evaluation criteria are as follows, with AAA, AA, and A considered acceptable.
[0151] AAA: 2400h and above AA: 1500h or more but less than 2400h A: 720h or more but less than 1500h B: Less than 720h
[0152] As shown in Tables 1A to 4B, in Examples 1 to 35, the chemical composition of the coating, the thickness of the first region, the area ratio of the Al-containing phase in the first region, the thickness of the second region, and the thickness of the third region are all within the scope of this invention. Therefore, the coating exhibits excellent adhesion, post-coating corrosion resistance, red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance.
[0153] It should be noted that in the first region of Examples 1 to 35, one or more of the following phases are included as the remainder: Mg2Si phase, Mg2Sn phase, Zn phase, Al-Ca-Zn phase, Al-Ca-Si-Zn phase, Ca-Zn phase, and Mg-Al-Si-Zn phase. Furthermore, in some examples, the first region contains an Fe-Al alloy phase at an area ratio of 3% or less. Additionally, the third region of Examples 1 to 35 contains an Fe-Al alloy phase as the remainder. Furthermore, the remainders of the second and third regions sometimes include one or more of the following phases: Mg2Si phase, Mg2Sn phase, Zn phase, Al-Ca-Zn phase, Al-Ca-Si-Zn phase, Ca-Zn phase, and Mg-Al-Si-Zn phase.
[0154] On the other hand, as shown in Tables 1A to 4B, any one of the chemical composition of the coatings in Comparative Examples 36 to 46, the thickness of the first region, the area ratio of the Al-containing phase in the first region, the thickness of the second region, and the thickness of the third region is outside the scope of the present invention. As a result, at least one of the coating adhesion, post-coating corrosion resistance, red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance deteriorates.
[0155] The Al content of the coating in Comparative Example 36 was insufficient. As a result, the thickness of the second and third regions was insufficient, leading to poor resistance to red rust and poor substrate corrosion protection. The coating of Comparative Example 37 had an excess of Al. As a result, the flux reaction became abnormal, and the appearance of the coating deteriorated significantly.
[0156] The coating of Comparative Example 38 had insufficient Mg and excessive Fe. As a result, its corrosion resistance, red rust resistance, iron-based corrosion resistance, and sacrificial corrosion protection deteriorated after coating. The coating of Comparative Example 39 had an excess of Mg. As a result, the flux reaction became abnormal, and the appearance deteriorated significantly.
[0157] In Comparative Example 40, the coating has an excess of Si and an insufficient amount of Fe. As a result, the thickness of the second and third regions is insufficient, leading to poor resistance to red rust and reduced substrate corrosion protection. In Comparative Example 41, the coating had an excess of Ca. Furthermore, the Fe content was insufficient. Consequently, the flux reaction became abnormal, resulting in a significant deterioration in appearance.
[0158] In Comparative Example 42, the amount of shot peening applied in the shot peening process was insufficient. As a result, Equation (1) was not satisfied, and the adhesion of the coating deteriorated.
[0159] The cooling rate in the cooling process of Comparative Example 43 was too fast. As a result, the area ratio of the Al-containing phase in the first region deviated from the scope of the present invention, and the corrosion resistance deteriorated after coating.
[0160] In Comparative Example 44, the immersion time in the plating bath was insufficient. As a result, the thickness of the second region was insufficient, and the resistance to red rust deteriorated. In Comparative Example 45, the immersion time in the plating bath was insufficient. As a result, the thickness of the third region was insufficient, and the corrosion resistance of the substrate deteriorated.
[0161] Comparative Example 46 was not shot peened. As a result, sufficient strain could not be introduced into the base steel before plating, thus failing to satisfy Equation (1), and the adhesion of the plating layer deteriorated.
[0162] Table 1A
[0163] Table 1B The underlined part indicates that it is outside the scope of this invention.
[0164] Table 2A
[0165] Table 2B An underline indicates that the manufacturing conditions are outside the range of preferred manufacturing conditions.
[0166] Table 3A
[0167] Table 3B The underlined part indicates that it is outside the scope of this invention.
[0168] Table 4A
[0169] Table 4B Industrial availability
[0170] The coated steel of this invention exhibits excellent adhesion, post-coating corrosion resistance, red rust resistance, substrate corrosion resistance, and sacrificial corrosion resistance. Therefore, it has the potential for application in civil engineering and infrastructure fields, as well as in automotive components. Explanation of reference numerals in the attached figures
[0171] 1. Coated steel, 1a. Surface, 11. Base steel, 12. Coating, 12A. First area, 12B. Second area, 12C. Third area, 13. Boundary line (interface).
Claims
1. A plated steel material comprising a base steel material and a coating disposed on the surface of the base steel material, wherein, The coating, as a chemical composition, contains, by mass%, Al: 5.0–40.0%, Mg: 0.5–15.0%, Fe: 5.0–40.0%, Si: 0–2.0%, Ca: 0–2.0%, and also contains one or two elements selected from groups A and B below, with the remainder being Zn and impurities. In a cross-section of the coated steel perpendicular to the surface, taking a cross-section of the coated steel of a predetermined length in a direction parallel to the surface as the observation area, the length L of the boundary line between the coating and the base steel satisfies the following equation (1). The coating comprises: a first region disposed on the surface side of the plated steel, having an Fe concentration of less than 5.0% by mass; a second region adjacent to the first region, having an Fe concentration of 5.0% by mass or more and less than 30.0% by mass; and a third region disposed between the second region and the parent steel, having an Fe concentration of 30.0% by mass or more and less than 80.0% by mass. The thickness of the first region is 5–100 μm, the thickness of the second region is 5–100 μm, and the thickness of the third region is 5–100 μm. The first region contains 0% to less than 5% Al-containing phase by area, wherein the Al-containing phase contains Zn and 20-99% by mass of Al. [Group A]Ni: 0~1.0%; [Group B] One or more of the following: Sb: 0-0.5%, Pb: 0-0.5%, Cu: 0-1.0%, Sn: 0-2.0%, Ti: 0-1.0%, Cr: 0-1.0%, Nb: 0-1.0%, Zr: 0-1.0%, Mn: 0-1.0%, Mo: 0-1.0%, Ag: 0-1.0%, Li: 0-1.0%, La: 0-0.5%, Ce: 0-0.5%, B: 0-0.5%, Y: 0-0.5%, P: 0-0.5%, Sr: 0-0.5%, Co: 0-0.5%, Bi: 0-0.5%, In: 0-0.5%, V: 0-0.5%, W: 0-0.5%, totaling 0-5%; (L-L0) / L0×100≥2.0% (1) In equation (1), L0 is the straight-line distance between one end and the other end of the boundary line in the observation area, and L is the length of the boundary line between the one end and the other end.
2. The plated steel according to claim 1, which satisfies the following formula (2), (L-L0) / L0×100≥4.0% Equation (2) in, In equation (2), L0 is the straight-line distance between one end and the other end of the boundary line in the observation area, and L is the length of the boundary line between the one end and the other end.
3. The plated steel according to claim 1, which satisfies the following formula (3), (L-L0) / L0×100≥6.0% Equation (3) in, In equation (3), L0 is the straight-line distance between one end and the other end of the boundary line in the observation area, and L is the length of the boundary line between the one end and the other end.
4. The plated steel according to any one of claims 1 to 3, wherein, The thickness of the first region is 15μm to 100μm.
5. The plated steel according to any one of claims 1 to 3, wherein, The area fraction of the Al-containing phase in the first region is less than 1%.
6. The plated steel according to any one of claims 1 to 3, wherein, The first region contains a Mg-Zn phase comprising Zn and 20–60% by mass of Mg, wherein the area fraction of the Mg-Zn phase in the first region is 2% or more.
7. The plated steel according to any one of claims 1 to 3, wherein, The first region contains a binary eutectic structure of Zn phase and Mg-Zn phase, and the area fraction of the binary eutectic structure in the first region is more than 1%.
8. The plated steel according to any one of claims 1 to 3, wherein, The thickness of the second region is 15μm to 100μm.
9. The plated steel according to any one of claims 1 to 3, wherein, The second region contains a Mg-Zn phase comprising Zn and 20–60% by mass of Mg, wherein the area fraction of the Mg-Zn phase in the second region is 5% or more.
10. The plated steel according to any one of claims 1 to 3, wherein, The second region contains an Fe-Al alloy phase with an equivalent circle diameter of less than 15 μm and an aspect ratio of more than 2, and the area fraction of the Fe-Al alloy phase in the second region is more than 5%.
11. The plated steel according to any one of claims 1 to 3, wherein, The second region contains a binary eutectic structure of Zn phase and Mg-Zn phase, and the area fraction of the binary eutectic structure in the second region is more than 2%.
12. The plated steel according to any one of claims 1 to 3, wherein, The thickness of the third region is 15μm to 100μm.
13. The plated steel according to any one of claims 1 to 3, wherein, The third region contains a Mg-Zn phase comprising Zn and 20–60% by mass of Mg, wherein the area fraction of the Mg-Zn phase in the third region is 10% or more.
14. The plated steel according to any one of claims 1 to 3, wherein, The content of Mg in the chemical composition of the coating relative to the total amount of Zn and Mg, i.e., Mg / (Zn+Mg), is 5.0% or more.
15. The plated steel according to any one of claims 1 to 3, wherein, The content of Mg in the chemical composition of the coating relative to the total amount of Zn and Mg, i.e., Mg / (Zn+Mg), is 6.5% or more.
16. The plated steel according to any one of claims 1 to 3, wherein, The coating contains Sn at a concentration of 0.02 to 2.0% by mass, and the coating contains the Mg2Sn phase.
Citation Information