Method for producing a hardened steel component with a conditioned zinc anticorrosion layer

By treating the surface of zinc-based coated steel components with potassium hydroxide and lithium hydroxide solutions, the complexity of cleaning the zinc anti-corrosion layer of hardened steel components has been solved, enabling efficient production without mechanical cleaning and improving weldability and surface quality.

CN123146709APending Publication Date: 2026-11-20VOESTALPINE STAHL GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202580028431.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-19
Filing Date
2025-04-16
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies require complex cleaning processes in the treatment of zinc anti-corrosion coatings on hardened steel components, leading to increased labor costs and potential surface defects, especially limiting the dimensional accuracy of thin components.

Method used

The zinc-based coating is surface-treated with potassium hydroxide and lithium hydroxide solutions. By applying an alkaline aqueous solution before the forming and hardening process, a thin layer is formed to improve phosphating, paintability and weldability, avoiding subsequent mechanical cleaning steps.

Benefits of technology

This technology eliminates the need for mechanical cleaning during the hardening process, improving the weldability and surface gloss of components, reducing production costs, and enhancing dimensional accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to a method for producing a hardened steel component, wherein a blank is cut from a zinc-coated strip made of a hardenable steel alloy, which is subsequently cold formed to produce a component blank, and subsequently heated to a temperature at which the microstructure is transformed into austenite; the austenized component blank is subsequently introduced into a forming and hardening die, in which the component blank is held in a form-fitting manner by an upper die and a lower die, which have a shape corresponding substantially to the shape of the component blank; as a result of the material of the component blank lying against the die, in particular the cooled die, the heat is removed from the steel material so rapidly that martensitic hardening occurs; an aqueous potassium hydroxide solution and / or an aqueous lithium hydroxide solution is applied to the surface of the strip, the blank or the component blank after the zinc coating of the metal strip and before the temperature increase for the purpose of austenization.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention relates to a method for producing hardened steel components with a conditioned zinc alloy anti-corrosion coating.

[0002] It has long been known to apply protective coatings to metal sheets, especially metal strips, that may corrode under normal operating conditions.

[0003] Typically, the anti-corrosion layer on metal strips can be an organic coating, such as paint, which may also contain corrosion inhibitors.

[0004] Furthermore, it is known to protect metal strips using metallic coatings. These coatings can consist of electrochemically more expensive or electrochemically less expensive metals.

[0005] A coating composed of an electrochemically noble metal or a self-passivating metal such as aluminum is called a barrier protective layer. For example, when aluminum is applied to steel, the steel material will corrode if this barrier protective layer is no longer present in certain areas, for example, due to mechanical damage. The most commonly used barrier protective layer on steel is the aforementioned aluminum layer, which is typically applied by hot-dip galvanizing.

[0006] If an electrochemically base metal is applied as a protective layer, this is called a cathodic corrosion protection coating because, in the event of mechanical damage to the corrosion protection coating extending down to the steel material, the electrochemically base metal corrodes first, and then the steel material itself is exposed to corrosion.

[0007] The most commonly used cathodic protection coating on steel is zinc coating or zinc-based alloy.

[0008] Various galvanizing methods are known. One commonly used galvanizing method is so-called hot-dip galvanizing (also known as hot-dip zinc coating). In this method, steel is continuously (e.g., strip and wire) or batch-wise (e.g., components) immersed in a molten zinc bath (the melting point of zinc is 419.5°C) at a temperature of approximately 450°C to 600°C. The molten zinc bath, for example, has a zinc content of at least 98.0% by weight according to DIN EN ISO 1461. A ferro-zinc corrosion-resistant alloy layer is formed on the steel surface, upon which a firmly adhered pure zinc layer exists, the composition of which corresponds to the composition of the molten zinc bath. In the case of continuously galvanized strip, the zinc layer has a thickness of 5 µm to 40 µm. In the case of batch-galvanized components, the zinc layer can have a thickness of 50 µm to 150 µm.

[0009] In electrolytic zinc plating (electro-zinc plating), steel strips or sheets are not immersed in a molten zinc bath, but rather in a zinc electrolyte. In this method, the steel to be zinc-plated is introduced into the solution as the cathode, and an electrode made of zinc of the highest possible purity is used as the anode. An electric current is passed through the electrolyte solution. In this method, zinc, existing in ionic form (oxidized state +II), is reduced to metallic zinc and deposited on the steel surface. Compared to hot-dip galvanizing, electrolytic zinc plating allows for the application of a thinner zinc layer. The zinc layer thickness is proportional to the current intensity and duration, and, depending on the workpiece and anode geometry, produces a layer thickness distribution across the entire workpiece.

[0010] To ensure the adhesion and uniformity of the zinc coating, careful surface pretreatment is required. This may include, for example, degreasing, alkaline washing, pickling, rinsing, and / or deoxidation. After galvanizing, one or more post-treatments may be performed, such as phosphating, oiling, or application of an organic coating (e.g., cathodic dip coating, abbreviated as KTL).

[0011] In such cases, not only pure metal layers are typically deposited. Numerous known deposited alloys exist, and in addition to pure aluminum coatings, there are coatings containing both aluminum and zinc, as well as coatings containing a small amount of aluminum in addition to zinc in a predominantly high proportion. These may also contain other elements such as zinc, nickel, chromium, and magnesium, and mixtures thereof. References to zinc-based corrosion-resistant coatings or galvanized steel strips in this application also include zinc-based alloys.

[0012] Furthermore, it has long been known, particularly in order to reduce the weight of the vehicle body, to configure at least a portion of the vehicle body to have high strength to ensure sufficient strength in the event of a collision. Weight savings stem from the fact that high-strength steel grades with relatively thin walls can be used, resulting in lower weight.

[0013] When using high-strength steel, there are different approaches and a variety of steel grades that can be used.

[0014] High-strength steels are frequently used through quench hardening. Quenching hardening refers to selecting a cooling rate higher than the corresponding critical cooling rate to determine the microstructure. This critical cooling rate is approximately 15 to 20 Kelvin per second, but may be lower depending on the alloy composition. Common steels that can be hardened by quench hardening are so-called boron-manganese steels, such as the most commonly used 22MnB5, and its derivatives, such as 20MnB8 and 30MnB5. Non-hardenable steels, such as microalloyed steels, can also be hot-formed in direct or indirect processes.

[0015] This type of steel can be easily shaped and cut in its unhardened state.

[0016] There are essentially two different production routes for shaping and hardening this type of steel, especially in vehicle body construction.

[0017] The first and slightly older production route is called compression molding. In compression molding, a flat billet is cut from steel sheet or strip made of a hardenable steel alloy (such as 22MnB5 or similar manganese-boron steel). This flat billet is then heated to such a high temperature that the steel's microstructure exists in the form of γ-ferrite, or austenite. To obtain this microstructure, the so-called austenitizing temperature Ac3 must be exceeded, at least if complete austenitization is desired.

[0018] Depending on the steel, the temperature can be between 820°C and 900°C, in which such steel billets are heated, for example, to about 900°C to 930°C and held at that temperature until the microstructure transformation is complete.

[0019] These steel billets are then transferred, still hot, into a press, where they are shaped into the desired form in a single press stroke using correspondingly forming upper and lower dies. Due to the contact between the hot steel and the relatively cold, and particularly cooled, press dies (forming dies), energy is removed from the steel very rapidly. In particular, the heat must be removed rapidly enough to exceed the so-called critical hardening rate, which is typically between 15° and 25° Kelvin per second.

[0020] When cooling occurs so rapidly, the austenitic microstructure does not transform back to the initial ferrite microstructure, but instead acquires a martensitic microstructure. Because austenite can dissolve significantly more carbon in its lattice than martensite, carbon precipitation leads to lattice distortion, resulting in the high hardness of the final product. In essence, rapid cooling stabilizes the martensitic state. Therefore, hardness levels exceeding 1,500 MPa or tensile strength Rm can be achieved. The hardness distribution can also be shaped by appropriate measures, which will not be discussed in more detail here, such as complete or partial reheating.

[0021] Another, and slightly newer, method for producing hardened steel components, particularly those for vehicle body structures, is a form hardening method developed by the applicant. In form hardening, a flat steel billet is cut from steel strip, and the billet is subsequently formed in a cold state. Specifically, this forming does not occur in a single press stroke, but rather, as is common in conventional press production lines, for example, in a five-stage process. This process enables the production of considerably more complex shapes, ultimately allowing the production of complexly shaped components, such as B-pillars or longitudinal beams for motor vehicles.

[0022] To subsequently harden such fully formed components, the components are also austenitized in a furnace and transferred in an austenitized state into a forming die, which has the contour of the final component. Prior to heating, the pre-formed component is preferably shaped such that, after heating and thus thermal expansion, the component substantially corresponds to the final dimensions of the hardened component. The austenitized billet is placed in the forming die in its austenitized state, and the forming die is closed. Preferably, the component is contacted and held in a clamping manner by the forming die on all sides, and due to the contact with the forming die, heat is also removed in a manner capable of producing a martensitic microstructure.

[0023] No shrinkage can occur in the clamped state, allowing the hardened final component with the corresponding final size to be removed from the forming mold after hardening and cooling.

[0024] Since motor vehicle bodies typically have anti-corrosion coatings, the anti-corrosion layer closest to the metal material forming the body, especially steel, is a metal coating. In the past, anti-corrosion coatings for hardened components have also been sought and developed.

[0025] However, anti-corrosion coatings used on components undergoing hardening face different requirements than those used on unhardened components. The coating must withstand the high temperatures that occur during the hardening process. Since hot-dip aluminized coatings were long known to withstand high temperatures, mold-hardened steels with an aluminum protective layer were initially developed. Such coatings can withstand not only high temperatures but also hot-dip forming. However, a drawback is that the conventional steel grades used in motor vehicles are typically hot-dip galvanized rather than aluminized, and the use of different anti-corrosion systems is fundamentally problematic, especially in situations where there is a risk of contact corrosion.

[0026] The applicant has therefore developed a method to provide zinc coatings that can withstand the same high temperatures.

[0027] In principle, zinc coatings have far fewer problems than aluminum coatings in terms of forming, because aluminum coatings tend to peel or crack at normal forming temperatures. Zinc coatings do not exhibit this problem.

[0028] However, zinc coatings were initially expected to be unable to withstand high temperatures. However, special zinc coatings containing a certain proportion of oxyphilic elements can be processed at high temperatures because these elements rapidly diffuse to the air-facing surface and oxidize there, forming a glassy protective film on the zinc coating. Such zinc coatings have now been established, particularly for form hardening. These zinc coatings can also be used very successfully for compression molding.

[0029] To ensure optimal paint adhesion and weldability, it is known to clean fully formed and hardened components in a manner that allows the glass hard protective film layer to be smoothed or removed.

[0030] DE102010037077B4 discloses a method for conditioning the surface of a hardened, corrosion-resistant component made of steel plate, wherein the steel plate is coated with a metallic coating and is heated for hardening and quenching. After hardening, oxides present on the corrosion-resistant coating due to heating are removed. To condition the surface of the metallic coating, i.e., the corrosion-resistant layer, the component undergoes a mass finishing process. The corrosion-resistant coating is a zinc-based coating, and the surface conditioning is performed in such a manner that oxides located on or attached to the corrosion-resistant layer are abraded away, and in particular, micropores are exposed.

[0031] DE102007022174B3 discloses a method for preparing and removing a temporary protective layer of a cathode coating, wherein a steel sheet made of a hardenable steel alloy is coated with a zinc coating by a hot-dip galvanizing process, wherein the aluminum content in the zinc bath is adjusted such that an aluminum oxide surface scale is formed during melt hardening, and wherein the scale is removed or smoothed after hardening by sandblasting the metal sheet component with dry ice particles. Examples of this method are EP1630244B1 or EP2233508B1.

[0032] Such protective layers typically only appear on zinc coatings, while aluminum coatings often require no cleaning or only minimal cleaning.

[0033] WO2018 / 126471A1 discloses a sol-gel preconditioning process for layers to reduce oxide layer formation and improve weldability. The aim is to create an oxide protective coating for steel intended for compression curing. This coating is based on a binder containing silanes and titanium, along with oxide pigments, and is apparently applied using a sol-gel process. Solvents such as methanol are specifically used here, which are unsuitable for use on steel production lines. The coating is intended to self-detach after compression curing; although trials of titanium-based and silicon-based coatings were conducted in 2015 and 2016, neither thick nor thin wet films were successful. The coatings neither self-detach nor exhibit weldability suitable for industrial applications.

[0034] EP2536857B1 discloses a ceramic-based coating with a thickness ≤25 µm, intended to consist essentially of SiO2, Al2O3, and MgO2, optionally containing tin metal fibers. It has been found that such coatings render the substrate unsolderable and also cause film delamination.

[0035] EP4110972B1 discloses a coating for tin-coated zinc surfaces, which forms an oxide layer mixture of tin oxide and zinc oxide during the hardening process, eliminating the need to remove the mixture.

[0036] The object of this invention is to provide a method for producing hardened steel components, wherein an existing zinc anti-corrosion coating is treated in such a way that surface cleaning is unnecessary after hardening, particularly eliminating the need for cleaning by fluid jetting and / or particle jetting. Particularly preferably, the method is intended to eliminate the need for the use of tin or tin-containing solutions.

[0037] The objective is achieved by a method having the features of claim 1.

[0038] Advantageous further improvements are defined in the dependent claims.

[0039] Another objective is to provide a galvanized steel strip whose construction eliminates the need to remove oxide scale.

[0040] The objective is achieved by a galvanized metal strip having the features of claim 13.

[0041] Advantageous further improvements are defined in the dependent claims.

[0042] According to the present invention, it has been recognized that, in certain circumstances, cleaning of the surface of galvanized metal strips subjected to temperature increases for the purpose of microstructural transformation can be omitted. In particular, mechanical cleaning of galvanized steel sheets and hardened components made therefrom can be omitted.

[0043] Although post-cleaning is a controlled and mature process, it still results in greater workload. There is also a risk of additional surface defects, and overall, higher costs. For very thin components, it has been found that dimensional accuracy may be limited in some cases.

[0044] If there are interconnected process sequences that specify the online arrangement of these cleaning steps within the overall production process, it may be necessary to specify adjustments to the cycle time.

[0045] According to the present invention, steel sheet blanks or steel strips with zinc-based coatings are used.

[0046] Advantageously, the layer can have a thickness of 5 µm to 20 µm on each side. This ensures good corrosion protection. In particular, the coating can be Z40, Z60, Z80, Z120, Z140, or Z180 according to DIN EN 10346.

[0047] The zinc-based anti-corrosion coating may have a relatively high zinc content, ranging from 93 wt.% to 99.8 wt.%, particularly from 95 wt.% to 99.5 wt.%, preferably from 98 wt.% to 99.5 wt.%, and may also contain aluminum ranging from 0.2 wt.% to 2 wt.%, except for unavoidable impurities.

[0048] Particularly preferred is that the zinc-based metal anti-corrosion coating can be applied by a hot-dip process, i.e., hot-dip galvanizing. This provides a simple and robust application method.

[0049] According to the present invention, it has been found that surface treatment of the galvanized surface prior to the form hardening process successfully establishes phosphating, painting, and solderability. According to the present invention, oxide growth during the hardening process can be configured such that subsequent mechanical surface conditioning, such as centrifugal blasting, finishing, or dry ice blasting, is unnecessary. Similarly, treatment with tin or tin-containing solutions can be omitted.

[0050] According to the present invention, lithium and / or potassium have been found to unexpectedly appear to modify surfaces in a manner that requires no type of cleaning.

[0051] In particular and surprisingly, it has been found that when the concentration of the solution to be applied, expressed in g / L, satisfies the following relationship: [c] = [KOH] + 2 The [LiOH·H2O] solution, wherein the concentration of the lithium solution [LiOH·H2O] is between 0 and 100 g / L, and the potassium solution [KOH] is between 0 and 200 g / L, with a total concentration [c] between 30 and 200, produces particularly high effectiveness. Preferably, the total concentration [c] can be set between 30 and 120 to further improve effectiveness.

[0052] According to the invention, particularly after finishing rolling and before cold forming or annealing and hardening processes, an alkaline aqueous solution is applied to the galvanized surface, for example by means of a roll coater.

[0053] In this case, a very small layer thickness is used, which is 0.5 µm to 3 µm in the aqueous state, particularly 0.5 µm to 1.5 µm, and in the dry state, the thickness is 50 nm to 300 nm, particularly 75 nm to 125 nm, particularly 80 nm to 100 nm.

[0054] The solution can also be applied by dipping and squeezing, spraying, or other application methods.

[0055] Of course, all other methods capable of applying liquid ionic solutions to a surface are also suitable.

[0056] When the layer thickness is 1 µm in the aqueous state, the surface loading in mg / m² satisfies the following relationship: [c]=[K]+2 [Li] [Li] = 0 to 100 mg / m 2 [K] = 0 to 200 mg / m³ 2 [c] = 10 to 200, preferably 30 to 120 When using potassium hydroxide (KOH), the potassium surface loading is per m 2 1 mg to 140 mg potassium, especially per m 2 30 mg to 100 mg potassium. When using LiOH, the lithium surface loading is per m 2 1 mg to 40 mg lithium, especially per m 2 15 mg to 35 mg, and especially per m 2 20 mg to 30 mg lithium.

[0057] Surprisingly, the combination of potassium hydroxide and lithium hydroxide has been found to exhibit particularly advantageous properties regarding the weldability of treated steel sheets or components. According to the invention, it has been found that for the sheet to be hardened, the surface resistivity is very low at conventional annealing times, and only a very slight tendency for undercutting is detected in the paint film undercut test. Significantly less oxide is visually detected, manifested in the metallic luster of the annealed sheet. Such a silvery appearance is usually problematic as it indicates inadequate reaction. Studies have shown that the zinc-iron crystals in the zinc layer have reacted completely. Furthermore, good formation of phosphate crystals has been observed during phosphating.

[0058] Treatment with potassium hydroxide and / or lithium hydroxide resulted in an increase in emissivity from the initial 780°C until the γ-phase decomposition.

[0059] Overall, it is not yet possible to explain in detail how the K / Li solution works, but its effect is unexpected and absolutely clear.

[0060] The present invention therefore particularly relates to a method for producing hardened steel components, wherein a billet is cut from a strip made of a hardenable steel alloy and coated with a zinc-based coating, and the billet is subsequently cold-formed into a component blank and then heated to a temperature that causes the microstructure to transform into austenite, wherein the austenitized component blank is then fed into a forming hardening die, in which the component blank is held in a form-fitting manner by an upper die and a lower die having a shape substantially corresponding to the component blank, wherein, as the material of the component blank is in contact with the die, the die is particularly cooled, and heat is removed from the steel material sufficiently rapidly, such that martensitic hardening occurs due to cooling at a cooling rate higher than the critical cooling rate, wherein, after galvanizing the metal strip and before raising the temperature for the purpose of austenitization, an aqueous solution of potassium hydroxide and / or an aqueous solution of lithium hydroxide is applied to the surface of the strip or the billet or the component blank.

[0061] A further advantageous improvement is that the concentration of the solution to be applied, expressed in g / L, satisfies the following relationship: [c]=[KOH]+2 [LiOH·H2O] [LiOH·H2O] = 0 to 100 g / L, [KOH] = 0 to 200 g / L [c] = 10 to 200, preferably 30 to 120 A further advantageous improvement is that the surface loading of zinc is expressed in mg / m³. 2 The following relationship must be satisfied: [c]=[K]+2 [Li] [Li] = 0 to 100 mg / m 2 [K] = 0 to 200 mg / m³ 2 [c] = 10 to 200, preferably 30 to 120 A further advantageous improvement is that potassium and / or lithium are applied from an alkaline solution.

[0062] A further advantageous improvement is the application of an aqueous solution of potassium and / or lithium that has been adjusted to be alkaline.

[0063] An advantageous further improvement is that the aqueous solution is applied with a layer thickness of 0.5 µm to 3 µm, particularly 0.5 µm to 1.5 µm, wherein the layer thickness in the dry state is 50 nm to 300 nm, particularly 75 nm to 125 nm, particularly 80 nm to 100 nm.

[0064] A further advantageous improvement is that the potassium surface loading is per m 2 1 mg to 140 mg potassium, and especially per m 2 50 mg to 100 mg potassium.

[0065] A further advantageous improvement is that the surface loading of lithium is per m 2 1 mg to 40 mg lithium, especially per m 2 15 mg to 35 mg lithium, and especially per m 2 20 mg to 30 mg lithium.

[0066] A further advantageous improvement is the use of a solution with a concentration of 50 g / L to 200 g / L KOH.

[0067] A further advantageous improvement is the use of a solution with a concentration of 5 g / l to 100 g / l LiOH·H2O.

[0068] A further advantageous improvement lies in the combination of KOH with a solution concentration of 30 g / L to 200 g / L and LiOH·H₂O with a concentration of 4 g / L to 50 g / L. Advantageously, the combination of KOH and LiOH ensures that the component has particularly good weldability properties.

[0069] A further advantageous improvement is the use of a solution with a pH value of 10 to 14.

[0070] Another aspect of the invention relates to galvanized metal strip, particularly steel strip, coated with a coating per m 2 Potassium from 30 mg to 100 mg.

[0071] A further advantageous improvement is that the galvanized metal strip, particularly the steel strip, is coated with a coating per m 2 Lithium ranging from 5 mg to 30 mg.

[0072] The combination of potassium and lithium can be particularly advantageous as a coating on steel strip.

[0073] A further advantageous improvement is that the zinc-based coating comprises 95 wt.% to 99.8 wt.%, preferably 98 wt.% to 99.5 wt.%, of zinc, 0.2 wt.% to 2 wt.% of aluminum, and unavoidable impurities. The high zinc content ensures cathodic corrosion protection. Furthermore, good processability is ensured if the layer is primarily composed of zinc with the remainder comprising aluminum. Other elements, such as magnesium, may affect emissivity and thus the heating rate.

[0074] A further advantageous improvement is that the zinc-based coating has been applied by a hot-dip process, particularly by hot-dip galvanizing.

[0075] A further advantageous improvement is that the steel strip is formed from a hardenable steel alloy, particularly boron-manganese steel, and especially preferably 22MnB5, 20MnB8, or 34MnB5.

[0076] A further advantageous improvement is the use of strip with the following composition as the steel strip (all values ​​are in weight percent): Carbon content is at most 0.4%, preferably 0.10 to 0.30%, and Silicon content is at most 1.9, preferably 0.11 to 1.5, and Manganese up to 3.0, preferably 0.8 to 2.5, and Chromium up to 1.5, preferably 0.1 to 0.9, and The molybdenum content is at most 0.9, preferably 0.001 to 0.1, and Nickel up to 0.9, preferably up to 0.2, and Titanium content is at most 0.2, preferably 0.02 to 0.1, and Vanadium at most 0.2, and Tungsten at most 0.2, and Aluminum at most 0.2, preferably 0.02 to 0.07, and Boron at most 0.01, preferably 0.0005 to 0.005, and Sulfur content is at most 0.01, preferably at most 0.008, and... Phosphorus content is at most 0.025, preferably at most 0.01, and The balance consists of iron and smelting-related impurities.

[0077] Another aspect of the invention relates to the use of such steel strip produced by the aforementioned method in a process of forming a steel sheet, heating it for austenitizing purposes, and quenching and hardening it.

[0078] The present invention is illustrated by way of example with reference to the accompanying drawings. The drawings show: Figure 1 : Production routes based on existing form hardening processes or phs-ultraform processes; Figure 2 Production routes based on existing thermoforming processes, compression molding, or phs-directform processes; Figure 3 Production routes based on existing technologies such as multi-stage thermoforming processes, multi-stage compression hardening, or phs-multiform processes. Figure 4 : An apparatus diagram based on existing technology for hot-dip galvanizing equipment; Figure 5 : An apparatus diagram based on existing electroplating zinc equipment; Figure 6 A table of different exemplary embodiments with different potassium and / or lithium values; Figure 7 Taking 22MnB5 Z140 with a plate thickness of 1.5 mm as an example, a comparison is made between the heating curve conditioned according to the present invention and the heating curve according to the prior art. Figure 8 Taking 22MnB5 Z140 with a plate thickness of 1.5 mm as an example, the heating curves of the present invention and those according to the prior art are compared. Figure 7 The heating rate.

[0079] According to the present invention, the surface of a galvanized metal sheet, particularly a steel sheet, is conditioned with a lithium and / or potassium solution, wherein the galvanized metal sheet, particularly the steel sheet, is first cold-formed in multiple stages during a forming hardening process, and then heated as a component blank, fed into a forming hardening mold, and hardened therein, wherein the conditioning is discussed below.

[0080] Available potassium and lithium solutions have been described, with particularly suitable being conditioning solutions having a concentration conforming to the following formula: [c] = [KOH] + 2 [LiOH·H2O], where [c] is between 10 and 200 g / l.

[0081] The concentration of lithium solution [LiOH·H2O] is between 0 and 100 g / L, and the concentration of potassium solution [KOH] is between 0 and 200 g / L.

[0082] In this case, use an alkaline solution with a pH value of 10 to 14.

[0083] In this case, a very small layer thickness is used, which is 0.5 µm to 3 µm in the aqueous state, particularly 0.5 µm to 1.5 µm, and 50 nm to 300 nm in the dry state, particularly 75 nm to 125 nm, particularly 80 nm to 100 nm.

[0084] When using potassium hydroxide (KOH), the surface loading of potassium is per m 2 Potassium from 0 mg to 140 mg, especially per m 2 Potassium content of 50 mg to 100 mg. When used, the surface loading of lithium is per m³. 2 Lithium from 10 mg to 40 mg, especially per m 2 15 mg to 35 mg, and especially per m 2 20 mg to 30 mg of lithium.

[0085] Figures 1 to 3 This illustrates a conventional method in which galvanized steel sheet (with a zinc layer containing an oxygen-loving element, such as aluminum) is austenitized before or after forming, and in each case hardened by quenching in a press. This corresponds to the phs-ultraform process (…). Figure 1 In this process, after cold forming, the formed part is then austenitized above Ac3 and subsequently form hardened. Figure 2 The diagram illustrates the phs-directform process, in which the billet is first austenitized and formed in a hot state, and then trimmed. Figure 3 A variation thereof is shown, the so-called phs-multiform process, in which, after austenitization and optional pre-cooling to, in particular, 450°C to 650°C, a multi-stage process with multiple forming steps or cutting and punching operations is performed, these operations being categorized under the term "hot forming steps". After hardening, the sheet metal heat-treated in this manner has a layer on the surface, particularly a layer of alumina and zinc oxide, which is preferably removed.

[0086] According to the present invention, it can be determined that conditioning the surface with very small amounts of potassium hydroxide and / or lithium hydroxide obviously interferes with the formation of the oxide layer to such a large extent that the oxide layer does not form in that form or is conditioned to the point that it does not need to be removed.

[0087] Figure 4 and Figure 5 Hot-dip galvanizing apparatus and electrolytic galvanizing apparatus are shown respectively. In this case, potassium hydroxide solution and / or lithium hydroxide solution are preferably applied in the chemically passivated area (in... Figure 4 (in) or "passivation" section (in) Figure 5 Apply in (middle).

[0088] Figure 6 A table showing different exemplary embodiments with different values ​​of potassium hydroxide and / or lithium hydroxide is provided.

[0089] The effectiveness limits of KOH or LiOH can be seen from various embodiments. For this purpose, an aqueous solution having the corresponding KOH or LiOH value in g / l was applied to a 22MnB5 grade steel strip with a Z140 zinc coating on a 1.5 mm thick steel plate. This aqueous solution was applied using a roll coater, resulting in an aqueous layer of 1 µm thickness with the corresponding addition of KOH and / or LiOH.

[0090] Therefore, the table shows the values ​​in mg / m³ 2 The calculated potassium and / or lithium values ​​correspond to specific values ​​in g / L for an aqueous layer with a thickness of 1 µm, and for other layer thicknesses, the g / L of the solution needs to be recalculated accordingly. Additionally, the table includes a concentration factor [c], which is calculated according to the formula c = K + 2. Li is calculated. Depending on whether the factor [c] falls within the numerical range of 10 to 200, this embodiment may be an embodiment of the present invention or a non-inventive embodiment. Furthermore, the table also includes the average heating rate in K / s when steel plates, billets, or component blanks are heated from room temperature to the austenitizing temperature Ac3.

[0091] As can be seen, the embodiments of the present invention exhibit a significantly increased heating rate, which allows for faster heating, resulting in energy savings or CO2 savings.

[0092] Furthermore, the table also includes the performance of finished steel components in terms of phosphating (paintability), paint undercut, weldability, and contact resistance. In this case, compared to the prior art, specifically to 22MnB5 with a plate thickness of 1.5 mm, a Z140 coating, and without the conditioning of this invention, "--" indicates a significant negative effect, "-" indicates a slight negative effect, "~" indicates a comparable effect, "+" indicates a slight improvement, and "++" indicates a significant improvement.

[0093] Figure 7 Taking 22MnB5 Z140 with a plate thickness of 1.5 mm as an example, the heating curve conditioned according to the present invention is shown and compared with the heating curve of the prior art. In this case, a plate containing 70 mg K / m 2 and 4 mg Li / m 2 Aqueous solution.

[0094] Figure 8 Taking 22MnB5 Z140 with a plate thickness of 1.5 mm as an example, the heating curves of the conditioning process using the present invention are shown compared with those of the prior art. Figure 7 The heating rate.

[0095] Two pictures ( Figure 7 and Figure 8 It is clearly shown that the heating rate can be increased and the time required to reach the Ac3 temperature can be shortened by the conditioning of the present invention.

[0096] The coating can be applied online to the strip before it is cut into individual blanks. Alternatively, blanks cut from the strip can also be coated accordingly.

[0097] The blank is then formed into component blanks, particularly in a multi-stage process. It is also conceivable to coat the component blanks only with a solution containing potassium and / or lithium. However, it has been found that potassium and / or lithium coatings also tolerate the forming process well.

[0098] The component blank obtained in this manner is then heated to a temperature that transforms the microstructure into austenite. The austenitized component blank is then fed into a form-hardening die, in which the component blank is hardened in one stroke by contact with an upper and lower die, which are substantially the shape of or correspond to the blank. As the material of the component blank is in contact with the particularly cooled die, heat is removed from the steel material sufficiently quickly, resulting in martensitic hardening.

[0099] One advantage of the present invention is that the surface of steel sheets intended for form hardening or molding hardening can be prepared in such a way that the final mechanical cleaning for removing the oxide surface layer can be omitted, so that such sheets can be treated in the same way as, for example, hot-dip aluminized sheets, but with the advantage of achieving a higher cathodic corrosion protection effect compared to hot-dip aluminized sheets.

Claims

1. A method for producing hardened steel components, wherein a billet is cut from a strip made of a hardenable steel alloy and coated with a zinc-based coating, the billet is then cold-formed into a component billet and subsequently heated to a temperature that causes the microstructure to transform into austenite, wherein the austenitized component billet is then fed into a forming hardening die, in which the component billet is held in a form-fit manner by means of an upper die and a lower die having shapes substantially corresponding to the component billet, wherein... Since the material of the component blank is in contact with the mold, which is particularly cooled, and the heat is removed from the steel material at a sufficiently fast rate, martensitic hardening occurs due to cooling at a rate higher than the critical cooling rate. The method is characterized by applying an aqueous solution of potassium hydroxide and / or an aqueous solution of lithium hydroxide to the surface of the strip, the blank, or the component blank after galvanizing the metal strip and before raising the temperature for austenitizing purposes.

2. The method according to claim 1, characterized in that, The concentration of the solution to be applied, expressed in g / L, satisfies the following relationship: [c]=[COH]+2 [LiOH·H2O], [LiOH·H2O] = 0 to 100 g / L; [KOH] = 0 to 200 g / L [c] = 10 to 200, preferably 30 to 120.

3. The method according to claim 1 or 2, characterized in that, When the thickness of the layer to be applied is 1 μm, the surface loading is expressed in mg / m³. 2 The following relationship must be satisfied: [c]=[K]+2 [Li], [Li] = 0 to 100 mg / m 2 [K] = 0 to 200 mg / m³ 2 [c] = 10 to 200, preferably 30 to 120.

4. The method according to any one of the preceding claims, characterized in that, The potassium and / or lithium are applied from an alkaline solution.

5. The method according to any one of the preceding claims, characterized in that, Apply an aqueous solution of potassium and / or lithium that has been adjusted to be alkaline.

6. The method according to any one of the preceding claims, characterized in that, The aqueous solution is applied with a layer thickness of 0.5 μm to 3 μm, particularly 0.5 μm to 1.5 μm, wherein the layer thickness in the dry state is 50 nm to 300 nm, particularly 75 nm to 125 nm and more particularly 80 nm to 100 nm.

7. The method according to any one of the preceding claims, characterized in that, The surface loading of potassium is 1 mg / m 2 Up to 140 mg / m 2 Potassium, and specifically 50 mg / m³ 2 Up to 100 mg / m 2 Potassium.

8. The method according to any one of the preceding claims, characterized in that, The surface loading of lithium is 1 mg / m 2 Up to 40 mg / m 2 Lithium, especially at 15 mg / m³ 2 Up to 35 mg / m 2 Lithium, and more specifically 20 mg / m 2 Up to 30 mg / m 2 Lithium.

9. The method according to any one of the preceding claims, characterized in that, Use solutions with a concentration of 50 g / L to 200 g / L KOH.

10. The method according to any one of the preceding claims, characterized in that, Use a solution with a concentration of 5 g / L to 100 g / L LiOH·H2O.

11. The method according to any one of the preceding claims, characterized in that, The solution concentration is a combination of 30 g / l to 200 g / l KOH and 4 g / l to 50 g / l LiOH·H2O.

12. The method according to any one of the preceding claims, characterized in that, Use a solution with a pH of 10 to 14.

13. A galvanized metal strip, particularly a steel strip, coated with 30 mg / m 2 Up to 100 mg / m 2 Potassium.

14. A galvanized metal strip, particularly a steel strip, specifically according to claim 13, coated with a 5 mg / m² coating. 2 Up to 30 mg / m 2 Lithium.

15. Use of the steel strip according to claim 13 or 14, wherein the steel strip is produced by the method according to any one of claims 1 to 12, for use in a method in which a steel sheet is formed and subsequently heated to above the Ac3 temperature for austenitizing purposes, and cooled at a cooling rate higher than the critical cooling rate.

Citation Information

Patent Citations

  • Method of creating and removing a temporary protective layer for a cathodic coating

    DE102007022174B3

  • Method for conditioning the surface of hardened, corrosion-protected components made of sheet steel

    DE102010037077B4

  • Hot press formed product and method for production thereof

    EP1630244B1

  • Polymer compound and organic electroluminescent device using the same

    EP2233508A1

  • Method for producing hardened steel components with a conditioned zinc alloy corrosion protection layer

    EP4110972B1