Pattern forming method of colored resist and composition for the method
By setting a photoresist underlayer film between the substrate and the coloring photoresist film, and using a specific composition, the problems of residue and peeling in the formation of coloring photoresist patterns are solved, and good pattern formation effect is achieved.
Patent Information
- Application Number
- CN202580029687.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-23
- Filing Date
- 2025-04-21
- Publication Date
- 2026-11-20
AI Technical Summary
In the prior art, when using a colored resist material with dispersed pigments to form patterns, pigment residues that are insoluble in the developer are easily generated between adjacent resist patterns, and the adhesion between the colored resist film and the substrate is reduced, leading to pattern peeling problems.
A photoresist underlayer film is disposed between the substrate and the colored photoresist film. A photoresist underlayer film forming composition containing an alkali-soluble resin and a solvent is used. The photoresist underlayer film is formed by firing to ensure its solvent resistance to the colored photoresist film and its solubility in alkali developer, thereby preventing residue and peeling.
It effectively prevents the formation of residues between adjacent resist patterns and improves the adhesion between the colored resist film and the substrate, resulting in a good colored resist pattern.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a method for patterning a colored resist and a composition for the method. More specifically, this invention relates to a method for patterning a colored resist and a composition for forming a resist underlayer film, a resist underlayer film, a laminate, a self-emissive display element, and a liquid crystal display element. Background Technology
[0002] In self-emissive display elements such as organic light-emitting diodes (OLEDs) and micro-LEDs, anti-reflective circular polarizing plates have traditionally been used. However, when using polarizing plates, brightness is reduced due to light absorption by the polarizing plates. Therefore, in recent years, there has been a growing trend to abandon the use of anti-reflective circular polarizing plates.
[0003] A display device is proposed that does not use an anti-reflective circular polarizer. Instead, it suppresses the reflection of external light and improves brightness by setting a partition wall made of black material in the area surrounding the display area (see Patent Documents 1 and 2).
[0004] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2005-317271 Patent Document 2: Japanese Patent Publication No. 2023-518514 Summary of the Invention
[0005] The problem that the invention aims to solve In order to form black pixel spacers as shown in Patent Documents 1 and 2 above, the following method is used: a coloring resist material mixed with a coloring agent is applied to a substrate, and then the coloring resist is patterned through exposure and development processes.
[0006] Therefore, there is always a desire to provide a method that enables the patterning of color resists formed on a substrate.
[0007] The inventors have conducted repeated studies and found that when using a colored resist material with dispersed pigments to attempt to form a pattern of colored resist, residues of pigments, particles, and other colorants that are insoluble in the developer are generated on the substrate between adjacent resist patterns. Furthermore, it has been found that compared to a resist film without colorants, the adhesion between the colored resist film and the substrate is reduced, and the resist pattern is easily peeled off from the substrate.
[0008] To address the aforementioned issues of residue and pattern peeling, we also considered changing the composition of the resist material, but we did not expect that changing the composition would reduce the properties of the film itself as a colored resist film.
[0009] Therefore, it is desirable to provide a method for patterning a colored resist, in which the colored resist material is coated on a substrate and then exposed and developed to pattern the colored resist without changing the composition of the colored resist material so as not to sacrifice the properties of the film itself, and in a method for patterning the colored resist, no residue of the colorant that is insoluble in the developer is generated on the substrate between adjacent resist patterns, the resist pattern is not easily peeled off from the substrate, and a good colored resist pattern can be formed.
[0010] The present invention was made in view of the above circumstances, and its object is to provide a composition for forming a resist underlayer film for forming a resist underlayer film disposed between a substrate and a resist film, a resist underlayer film formed by the resist underlayer film forming composition, a laminate using the resist underlayer film, a method for forming a pattern of a resist, a self-emissive display element, and a liquid crystal element in order to form a good resist pattern.
[0011] Solution for solving the problem In order to solve the above-mentioned technical problems, the inventors conducted in-depth research and found that by setting a specific photoresist underlayer film between the substrate and the coloring photoresist film, the above-mentioned technical problems can be solved, thereby completing the present invention with the following main purpose.
[0012] That is, the present invention includes the following solutions.
[0013] [1] A composition for forming a photoresist underlayer film, used to form a photoresist underlayer film disposed between a substrate and a colored photoresist film, the composition for forming the photoresist underlayer film containing an alkali-soluble resin and a solvent, the photoresist underlayer film formed by firing the composition for forming the photoresist underlayer film exhibiting solvent resistance to the solvent contained in the photoresist material used to form the colored photoresist film, and exhibiting solubility in the alkali developer of the colored photoresist film.
[0014] [2] The composition for forming a resist underlayer film according to [1], wherein the alkali-soluble resin is polyamic acid.
[0015] [3] The composition for forming a photoresist underlayer according to [1] or [2], wherein the composition for forming a photoresist underlayer contains a crosslinking agent.
[0016] [4] The composition for forming a resist underlayer film according to [3], wherein the crosslinking agent is an epoxy compound.
[0017] [5] A composition for forming a resist underlayer film according to any one of [1] to [4], wherein the composition for forming a resist underlayer film contains a developing speed modifier.
[0018] [6] The composition for forming a resist underlayer film according to [5], wherein the developing speed modifier is a compound containing phenolic hydroxyl or carboxyl groups.
[0019] [7] A resist underlayer film, which is a cured film of the resist underlayer film forming composition as described in any one of [1] to [6].
[0020] [8] The photoresist underlayer film according to [7], wherein the photoresist underlayer film is non-photosensitive.
[0021] [9] A laminate comprising: a substrate, a resist underlayer as described in [7] or [8], and a colored resist film.
[0022]
[10] According to the laminate of [9], wherein the photoresist underlayer is configured such that the solvent resistance performance temperature of the photoresist underlayer relative to the solvent contained in the photoresist material used to form the colored photoresist film is lower than the developer insolubility temperature of the photoresist underlayer relative to the alkaline developer of the colored photoresist film.
[0023]
[11] A method for forming a pattern of a colored resist, comprising: a step of coating a resist underlayer film forming composition as described in any one of [1] to [6] onto a substrate and firing it to form a resist underlayer film; a step of forming a colored resist film on the resist underlayer film; and a step of exposing the colored resist film and developing a portion of the colored resist film and the resist underlayer film formed below the portion of the colored resist film to obtain a pattern of the colored resist.
[0024]
[12] According to the pattern forming method of the colored resist described in
[11] , the firing performed when forming the resist underlayer film is carried out at a temperature between the solvent resistance performance temperature of the resist underlayer film relative to the solvent contained in the resist material used to form the colored resist film and the developer insolubility temperature of the resist underlayer film relative to the alkaline developer of the colored resist film.
[0025]
[13] The pattern forming method of the colored resist according to
[11] or
[12] , wherein the colored resist film is formed using a pigment-dispersed resist material.
[0026]
[14] The patterning method of the colored resist according to
[11] or
[12] , wherein the colored resist film is formed by dispersing the resist material using metal oxide particles.
[0027]
[15] The laminate according to [9] or
[10] , wherein the resist underlayer and the colored resist film are patterned.
[0028]
[16] A self-emissive display element or liquid crystal display element having a laminate as described in
[15] .
[0029] Invention Effects According to the present invention, in order to form a good colored resist pattern, a resist underlayer film forming composition for forming a resist underlayer film disposed between a substrate and a colored resist film, a resist underlayer film formed by the resist underlayer film forming composition, a laminate using the resist underlayer film, a method for forming a colored resist pattern, a self-emissive display element, and a liquid crystal display element can be provided. Attached Figure Description
[0030] Figure 1 This is a graph showing the relationship between the firing temperature of the resist underlayer and the degree of solvent resistance exhibited by the resulting resist underlayer, as well as the relationship between the firing temperature of the resist underlayer and the degree of insolubility exhibited by the resulting resist underlayer.
[0031] Figure 2 This is a schematic diagram showing the relationship between firing temperature and the dissolution of the resist underlayer relative to the developer. Detailed Implementation
[0032] (Underlying film of the resist) The photoresist lower layer film of the present invention is disposed between the substrate and the colored photoresist film.
[0033] The resist underlayer film is formed by a resist underlayer film forming composition.
[0034] <Composition for forming a lower layer film of resist> The composition for forming the resist underlayer film of the present invention contains an alkali-soluble resin and a solvent.
[0035] The photoresist underlayer film formed by firing the composition for forming the photoresist underlayer film of the present invention exhibits solvent resistance to the solvent contained in the photoresist material used to form the colored photoresist film, and exhibits solubility in the alkaline developer of the colored photoresist film.
[0036] The composition for forming the resist underlayer film of the present invention may also include a crosslinking agent, a developing speed modifier, etc.
[0037] When a colored resist film formed on the resist underlayer film is exposed and developed using a specific resist underlayer film formed by the resist underlayer film of the present invention, and the colored resist is patterned, residues can be prevented from forming on the substrate between adjacent resist patterns, the resist patterns can be prevented from being easily peeled off from the substrate, and a good colored resist pattern can be formed.
[0038] <<Alkali-soluble resins>> The photoresist lower layer film formed by firing the photoresist lower layer film forming composition of the present invention containing an alkali-soluble resin is not particularly limited as long as it exhibits solvent resistance to the solvent contained in the photoresist material used to form the colored photoresist film and solubility in the alkaline developer of the colored photoresist film. It can be appropriately selected according to the purpose.
[0039] The alkali-soluble resin is more preferably polyamic acid.
[0040] <<<Polyamic Acid>>> Regarding the polyamic acid that is the alkali-soluble resin of the present invention, it is preferable to have a polyamic acid having repeating units as shown in the following formula (1). (R) 1 R is a tetravalent organic group that constitutes a tetracarboxylic acid or its derivative. 2 (k is a natural number; it represents the divalent organic group that constitutes the diamine.) There are no particular limitations on the method for obtaining this polyamic acid. Generally, it can be obtained by reacting and polymerizing a diamine with a tetracarboxylic acid dianhydride or a dicarboxylic acid dihalide, which are tetracarboxylic acids or their derivatives. Alternatively, a method can be used to react and polymerize a diamine with a tetracarboxylic acid dianhydride (hereinafter referred to as dianhydride) in a polar solvent such as N-methylpyrrolidone.
[0041] There are no particular limitations on the diamines that can be used to obtain polyamic acid; one or more of these can be used simultaneously.
[0042] Specific examples include: p-phenylenediamine, m-phenylenediamine, 4,4-methylene-bis(2,6-ethylaniline), 4,4'-methylene-bis(2-isopropyl-6-methylaniline), 4,4'-methylene-bis(2,6-diisopropylaniline), 2,4,6-trimethyl-1,3-phenylenediamine, 2,3,5,6-tetramethyl-1,4-phenylenediamine, o-toluidine, and meta-toluidine. 3,3',5,5'-Tetramethylbenzidine, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]hexafluoropropane, 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, 4,4'-diaminodiphenyl ether, 3,4-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 2,2 - bis(4-anilino)hexafluoropropane, 2,2-bis(3-anilino)hexafluoropropane, 2,2-bis(3-amino-4-tolyl)hexafluoropropane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,10-bis(4- Aminophenoxy)decane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 3,5-diaminobenzoic acid, 4-aminobenzoic acid-4-aminophenyl ester, 4,4'-diaminobenzoylaniline, etc.
[0043] In addition, diamines containing siloxanes are preferred to improve the adhesion to the substrate.
[0044] Examples of diamines containing siloxanes include the following diamines. (In the formula, p represents an integer from 1 to 10.) There are no particular limitations on the acid dianhydrides that can be used to obtain polyamic acid; one or more of these can be used simultaneously.
[0045] If we were to give specific examples of dianhydrides, we could list: pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 3,3',4,4'-benzophenone tetracarboxylic acid dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic acid dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic acid dianhydride, and other aromatic tetracarboxylic acid dianhydrides.
[0046] In addition, examples include: alicyclic tetracarboxylic anhydrides such as 1,2,3,4-cyclobutanetetracarboxylic anhydride, 1,2-dimethyl-1,2,3,4-cyclobutanetetracarboxylic anhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic anhydride, 1,2,3,4-cyclopentanetetracarboxylic anhydride, 1,2,4,5-cyclohexanetetracarboxylic anhydride, 3,4-dicarboxyl-1,2,3,4-tetrahydro-1-naphthous succinic anhydride, 2,3,5-tricarboxyl-2-cyclopentaneacetic anhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic anhydride, 2,3,4,5-tetrahydrofurantetracarboxylic anhydride, and 3,5,6-tricarboxyl-2-norborneneacetic anhydride, and aliphatic tetracarboxylic anhydrides such as 1,2,3,4-butanetetracarboxylic anhydride.
[0047] Considering the solubility of the polyamic acid resin coating film relative to the alkaline developing solution, the preferred formulations are 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, and 3,4-dicarboxylic acid-1,2,3... 4-Tetrahydro-1-naphthalenesuccinic dianhydride, 2,3,5-tricarboxy-2-cyclopentaneacetic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, 2,3,4,5-tetrahydrofurantetracarboxylic dianhydride, 3,5,6-tricarboxy-2-norborneneacetic dianhydride, etc., are acid dianhydrides composed of tetracarboxylic acids in which four carbonyl groups are not directly bonded to an aromatic ring, and more preferably 1,2,3,4-cyclobutanetetracarboxylic dianhydride.
[0048] During the polymerization of polyamic acid, the ideal ratio of the total moles of diamine to the total moles of dianhydride is 0.8 to 1.2.
[0049] Similar to conventional polycondensation reactions, the closer the molar ratio is to 1, the greater the degree of polymerization of the resulting polymer. When the polymerization is too low, the film strength becomes insufficient. Furthermore, when the polymerization is too high, the workability of the coating sometimes deteriorates. Therefore, the degree of polymerization of the product in this invention is preferably a reduced viscosity of 0.05 to 5.0 dl / g (0.5 g / dl in N-methylpyrrolidone at 30°C). The reduced viscosity is preferably 0.2 to 2.0 dl / g.
[0050] When reacting diamines with dianhydrides in polar solvents, the following polar solvents can be used: N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, N-vinylpyrrolidone, N-methylcaprolactam, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethyl sulfoxide, m-cresol, γ-butyrolactone, propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, etc. These can be used alone or in combination. Moreover, even solvents that do not dissolve polyamic acid can be mixed with the above solvents as long as the polyamic acid generated by the polymerization reaction will not precipitate.
[0051] Furthermore, the reaction temperature of diamine with acid dianhydride can be selected from any temperature between -20 and 150°C, preferably between -5 and 100°C.
[0052] The polyamic acid obtained in this way can be used directly, or it can be separated and recycled by precipitating it in undesirable solvents such as methanol, ethanol, and water.
[0053] The content of alkali-soluble resin in the composition for forming the lower layer of the resist film is not particularly limited, but is preferably 10% to 95% by mass, more preferably 20% to 90% by mass, relative to the film composition.
[0054] The film composition refers to the components in the composition used to form the lower layer of the resist film, excluding the solvent.
[0055] <<Solvent>> The resist underlayer film forming composition of the present invention can be easily prepared by uniformly mixing the constituent components and used in solution form by dissolving in a suitable solvent. Examples of solvents that can be used include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone. These solvents can be used alone or in combination of two or more. Furthermore, it can be used in combination with high-boiling-point solvents such as propylene glycol monobutyl ether and propylene glycol monobutyl ether acetate.
[0056] The composition for forming the lower layer film of the resist is preferably filtered using a filter with a pore size of about 0.2 μm before use.
[0057] The content of the solvent in the composition for forming the lower layer of the resist film is not particularly limited, but is preferably 50% to 99.99% by mass, more preferably 75% to 99.95% by mass, and particularly preferably 90% to 99.9% by mass.
[0058] <<Material Properties of Compositions for Forming Undercoat Films with Resist>> The composition for forming a photoresist underlayer film of the present invention can change the dissolution rate of the photoresist underlayer film relative to the alkaline developer of the colored photoresist film by means of the firing temperature conditions implemented during the formation of the photoresist underlayer film.
[0059] The composition for forming the lower layer of the resist film of the present invention is based on the firing temperature, for example... Figure 1 The substance exhibiting the properties shown.
[0060] Figure 1 It is the result of firing by changing the firing temperature of the resist underlayer film, and is a graph showing the degree of solvent resistance and the degree of insolubility of the resist underlayer film relative to the developer.
[0061] Figure 1 In the figure, reference numeral A indicates the degree of resistance of the resist underlayer film to the solvent contained in the resist material used to form the colored resist film.
[0062] also, Figure 1 In the figure, reference numeral B indicates the degree to which the resist underlayer is insoluble relative to the developer.
[0063] For example, when the composition for forming the resist lower layer film contains polyamic acid, as shown by line a1 in reference numeral A, the resist lower layer film obtained by firing the composition for forming the resist lower layer film of the present invention at a temperature of a1 or higher exhibits continuously increasing resistance to solvents contained in the resist material under the influence of the initial imidization reaction and crosslinking reaction. Up to a2, the higher the firing temperature, the higher the solvent resistance; when a2 or higher, the solvent resistance reaches a level where there are no problems.
[0064] Even when a colored resist material is coated onto a resist underlayer film obtained by firing at a firing temperature above a2, no mixing will occur.
[0065] Here, the firing temperature of a2 is also referred to as the "solvent resistance performance temperature" of the lower resist film relative to the solvent contained in the colored resist material.
[0066] On the other hand, as shown by line b1 in reference numeral B in the attached drawing, the resist lower layer film obtained by firing the composition for forming the resist lower layer film of the present invention at a temperature of b1 or higher will begin an imidization reaction and a crosslinking reaction. As this imidization and crosslinking proceed, the proportion of carboxylic acid in the composition decreases, thus increasing the degree of insolubility of the resist lower layer film relative to the alkaline developer. It should be noted that when the firing temperature is b2 or higher, the resist lower layer film becomes insoluble in the developer.
[0067] Here, the firing temperature of b2 is also referred to as the "developer insolubility temperature" of the lower resist film relative to the alkaline developer.
[0068] In this invention, it is preferable to use a resist underlayer film forming composition in which the "solvent resistance performance temperature" is set to be lower than the "developer insolubility temperature".
[0069] Furthermore, in this invention, the firing process performed when forming the resist underlayer film is between the aforementioned "solvent resistance performance temperature" and the aforementioned "developer insolubility temperature" (equivalent to...). Figure 1 It is best to perform the experiment under the temperature conditions indicated by the temperature range shown by the reference numeral T in the attached figure.
[0070] As a preferred firing temperature, for example, when the composition for forming the lower layer of the resist film contains polyamic acid, it is around 130°C to 220°C.
[0071] It should be noted that the firing process will also be explained in the section on the manufacturing method of the colored resist pattern below.
[0072] As described above, the resist underlayer film forming composition of the present invention may also contain crosslinking agents, developing speed modifiers, etc., in addition to alkali-soluble resins and solvents. The crosslinking agents and developing speed modifiers will be described in detail below.
[0073] For example, in the case of a composition for forming a resist underlayer film containing an alkali-soluble resin of polyamic acid and a crosslinking agent of an epoxy compound, when the composition for forming a resist underlayer film is fired, a portion of the polyamic acid may be imidized, or another portion may react with the epoxy compound.
[0074] The interval between the aforementioned "solvent resistance performance temperature" and the aforementioned "developer insolubility temperature" can be adjusted by adjusting the proportion of polyamic acid for imidization reaction, the proportion of epoxy compound, and the proportion of developing speed modifier in the composition for forming the lower layer of the resist film (equivalent to...). Figure 1 The temperature range indicated by the reference numeral T in the attached figure), and the slope of the developer dissolution rate of the resist underlayer film (equivalent to...). Figure 1(The slope of the broken line from b1 to b2 in the attached figure, labeled B).
[0075] The interval between the above-mentioned "solvent resistance performance temperature" and the above-mentioned "developer insolubility temperature" (equivalent to...) Figure 1 The wider the temperature range indicated by the numeral T in the attached diagram, the easier the operation is when fabricating the resist underlayer. Furthermore, the slope of the developer dissolution rate of the resist underlayer (equivalent to...) Figure 1 The smaller the slope of the broken line from b1 to b2 in the attached figure (label B), the wider the temperature margin.
[0076] Furthermore, in this invention, the slope of the developer dissolution rate of the resist underlayer film can be adjusted (equivalent to) by including a developer rate adjuster in the composition for forming the resist underlayer film. Figure 1 (The slope of the broken line from b1 to b2 in the attached figure, labeled B).
[0077] <<Cross-linking agent>> In addition to the above-mentioned alkali-soluble resin and solvent, the composition for forming the lower layer film of the resist of the present invention may also contain a crosslinking agent.
[0078] Examples of crosslinking agents include epoxy compounds.
[0079] There are no particular limitations on the type of compound as long as it has epoxy groups. Examples of compounds having at least two epoxy groups include: tris(2,3-epoxypropyl)isocyanurate, 1,4-butanediol diglycidyl ether, 1,2-epoxy-4-(epoxyethyl)cyclohexane, glycerol triglycidyl ether, diethylene glycol diglycidyl ether, 2,6-diglycidylphenyl glycidyl ether, 1,1,3-tris[p-(2,3-epoxypropoxy)phenyl]propane, 1,2-cyclohexane dicarboxylic acid diglycidyl ester, 4,4'-methylenebis(N,N-diglycidylaniline), 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylic acid ester, trimethylolethane triglycidyl ether, bisphenol A-diglycidyl ether, and pentaerythritol polyglycidyl ether, etc.
[0080] Furthermore, polymers having epoxy groups can be used as compounds having at least two epoxy groups. Such polymers can be used without particular restrictions, as long as they are polymers having epoxy groups.
[0081] Such polymers can be manufactured by addition polymerization using addition polymerizable monomers with epoxy groups. Alternatively, they can be manufactured by reacting hydroxyl-containing polymers with epoxy-containing compounds such as epichlorohydrin and glycidyl toluenesulfonate.
[0082] Examples include: polyglycidyl methacrylate, copolymers of glycidyl methacrylate and ethyl methacrylate, copolymers of glycidyl methacrylate, styrene, and 2-hydroxyethyl methacrylate, addition polymers of poly(3,4-epoxycyclohexyl methacrylate), and condensation polymers such as epoxy phenolic varnishes. The weight-average molecular weight of such polymers is, for example, 300 to 200,000.
[0083] Furthermore, examples of compounds having at least two epoxy groups include: SUMI-EPOXY ELM-434 and SUMI-EPOXY ELM-434L (manufactured by Sumitomo Chemical Co., Ltd.) as amino-containing epoxy resins; EPOLEAD GT-401, EPOLEAD GT-403, EPOLEAD GT-301, EPOLEAD GT-302, Celloxide 2021, and Celloxide 3000 (manufactured by Daicel Co., Ltd.) as epoxy resins having an oxycyclohexane structure; JER1001, JER1002, JER1003, JER1004, JER1007, JER1009, JER1010, and JER828 (manufactured by Mitsubishi Chemical Co., Ltd.) as bisphenol A type epoxy resins; and JER807 (manufactured by Mitsubishi Chemical Co., Ltd.) as a bisphenol F type epoxy resin. The following are examples of epoxy resins: JER152, JER154 (and above, manufactured by Mitsubishi Chemical Co., Ltd.), EPPN201, EPPN202 (and above, manufactured by Nippon Kayaku Co., Ltd.), etc., which are phenolic varnish-type epoxy resins; EOCN-102, EOCN-103S, EOCN-104S, EOCN-1020, EOCN-1025, EOCN-1027 (and above, manufactured by Nippon Kayaku Co., Ltd.), JER180S75 (manufactured by Mitsubishi Chemical Co., Ltd.), etc., which are cresol varnish-type epoxy resins; and Denacol EX-252 (manufactured by Nagase ChemteX Co., Ltd.), CY175, CY177, CY179 (and above, manufactured by CIBA-GEIGYA.G.), Araldite CY-182, Araldite, etc., which are alicyclic epoxy resins. CY-192, AralditeCY-184 (above, CIBA-GEIGYA.G-type), EPICLON 200, EPICLON 400 (and above, manufactured by DIC Co., Ltd.), JER871, JER872 (and above, manufactured by Mitsubishi Chemical Co., Ltd.), ED-5661, ED-5662 (and above, manufactured by Celanese Coating Co., Ltd.), etc.; as aliphatic polyglycidyl ethers, Denacol EX-611, Denacol EX-612, Denacol EX-614, Denacol EX-622, Denacol EX-411, Denacol EX-512, Denacol EX-522, Denacol EX-421, Denacol EX-313, Denacol EX-314, Denacol EX-321 (Nagase) ChemteX (manufactured by ChemteX Co., Ltd.), etc.; TEPIC-S, TEPIC-SS, TEPIC-HS, TEPIC-VL, TEPIC-FL (Nissan Chemical Co., Ltd.), etc., are triazine epoxides.
[0084] The content of the epoxy-containing compound is, for example, 70 parts by mass or less, preferably 50 parts by mass or less, and more preferably 45 parts by mass or less, relative to 100 parts by mass of the alkali-soluble resin. When the content of the epoxy-containing compound is greater than 70 parts by mass, sufficient solubility relative to the photoresist developer may not be obtained.
[0085] The content of the crosslinking agent in the composition for forming the lower layer of the resist film is not particularly limited, but is, for example, 70% by mass or less, preferably 50% by mass or less, relative to the alkali-soluble resin.
[0086] <<Developing Speed Adjuster>> In addition to the above-mentioned alkali-soluble resin and solvent, the composition for forming the resist lower film of the present invention may also contain a developing speed modifier.
[0087] To adjust the dissolution rate of the developer for photoresist, a developer speed adjuster can be used.
[0088] As a developing speed modifier, it is, for example, a compound containing phenolic hydroxyl or carboxyl groups.
[0089] For example, compounds having aromatic rings substituted with phenolic hydroxyl or carboxyl groups are preferred.
[0090] Examples include: 1-naphthoic acid, 2-naphthoic acid, 1-naphthol, 2-naphthol, 1-aminonaphthol, 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 3,7-dihydroxy-2-naphthoic acid, 6-bromo-2-hydroxynaphthoic acid, 1,2-naphthoic dicarboxylic acid, 1,3-naphthoic dicarboxylic acid, 1,4-naphthoic dicarboxylic acid, 1,5-naphthoic dicarboxylic acid, 1,6-naphthoic dicarboxylic acid, 1,7-naphthoic dicarboxylic acid, 1,8-naphthoic dicarboxylic acid, 2,3-naphthoic dicarboxylic acid, 2,6-naphthoic dicarboxylic acid, 1,2-dihydroxynaphthoic acid, 1,3-dihydroxynaphthoic acid, 1,4-dihydroxynaphthoic acid, 1,5-dihydroxynaphthoic acid, 1,6-dihydroxynaphthoic acid, 1,7-dihydroxynaphthoic acid, 1,8-dihydroxynaphthoic acid, 2,3-dihydroxynaphthoic acid, 2,6-dihydroxynaphthoic acid, 2,7-dihydroxynaphthoic ...3 Hydroxynaphthalene, 6-hydroxy-1-naphthoic acid, 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 6-hydroxy-2-naphthoic acid, 1-bromo-2-hydroxy-3-naphthoic acid, 1-bromo-4-hydroxy-3-naphthoic acid, 1,6-dibromo-2-hydroxy-3-naphthoic acid, 3-hydroxy-7-methoxy-2-naphthoic acid, 1-amino-2-naphthol, 1,5-dimercaptonaphthalene, 1,4,5,8-naphthalenetetracarboxylic acid, 3,5-dihydroxy-2-naphthoic acid, 1,4-dihydroxy-2-naphthoic acid, 2-ethoxy-1-naphthoic acid, 2,6-dichloro-1-naphthol, methyl 2-hydroxy-3-naphthoic acid, methyl 6-hydroxy-2-naphthoic acid, methyl 3-hydroxy-7-methoxy-2-naphthoic acid, 3,7-dihydroxy-3-naphthoic acid Methyl 2-naphthylcarboxylate, 2,4-dibromo-1-naphthol, 1-bromo-2-naphthol, 2-naphthylthiol, 4-methoxy-1-naphthol, 6-acetoxy-2-naphthoic acid, 1,6-dibromo-1-naphthol, 2,6-dibromo-1,5-dihydroxynaphthol, 1-acetyl-2-naphthol, 9-anthracarboxylic acid, 1,4,9,10-tetrahydroxyanthracene, and 1,8,9-trihydroxyanthracene, benzoic acid, 4-methylbenzoic acid, phthalic acid, isophthalic acid, terephthalic acid, 2-methoxybenzoic acid, isophthalic acid, p-phthalic acid, 2-hydroxybenzoic acid, 3-hydroxybenzoic acid, 4-hydroxybenzoic acid, 2-acetoxybenzoic acid, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, trimesic acid, 1, 4-Benzenedicarboxylic acid, 2,3-dimethoxybenzoic acid, 2,4-dimethoxybenzoic acid, 2,5-dimethoxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 4-acetylbenzoic acid, pyromellitic acid, pyromellitic tricarboxylic anhydride, 2-[bis-(4-hydroxyphenyl)-methyl]benzoic acid, 3,4,5-trihydroxybenzoic acid, 2-benzophenone carboxylic acid, m-phenylbenzoic acid, 3-(4'-hydroxyphenoxy)benzoic acid, 3-phenoxybenzoic acid, phenol, 1,4-dihydroxybenzene, 1,3-dihydroxybenzene, 1,2-dihydroxybenzene, 2-methylphenol, 3-methylphenol, 4-methylphenol, 1,3,5-trihydroxybenzene, 2...2-Bis-4-hydroxyphenylpropane, 2-hydroxybiphenyl, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2,4,6-tris(4-hydroxyphenylmethyl)-1,3-phenylene glycol, 4-benzyloxyphenol, polyhydroxystyrene, etc.
[0091] In addition, these compounds can be used by reacting with polymers or compounds having more than one reactive group.
[0092] For example, in the case of compounds having carboxyl groups or phenolic hydroxyl groups, compounds can be obtained by reacting them with epoxy compounds such as tris(2,3-epoxypropyl)isocyanurate, 1,4-butanediol diglycidyl ether, 1,2-epoxy-4-(epoxyethyl)cyclohexane, glycerol triglycidyl ether, diethylene glycol diglycidyl ether, 2,6-diglycidylphenyl glycidyl ether, 1,1,3-tris(p-(2,3-epoxypropoxy)phenyl)propane, 1,2-cyclohexane dicarboxylic acid diglycidyl ester, 4,4'-methylenebis(N,N-diglycidylaniline), 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylic acid ester, trimethylolethane triglycidyl ether, bisphenol-A-diglycidyl ether, and pentaerythritol polyglycidyl ether, as well as polymers with epoxy groups including glycidyl methacrylate.
[0093] Examples of such development speed modifiers include compounds such as those shown in (45) below. In formula (45), Ar is a benzene ring, naphthyl ring, or anthracene ring substituted with one or more hydroxyl and / or carboxyl groups, and may also be substituted with groups selected from the group consisting of alkyl groups having 1 to 5 carbon atoms, alkoxy groups having 1 to 5 carbon atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, nitro groups, cyano groups, thiol groups, thioalkyl groups having 1 to 5 carbon atoms, phenoxy groups, acetyl groups, alkoxycarbonyl groups having 1 to 5 carbon atoms, and vinyl groups. As a developing speed adjuster, it is preferable to use the epoxy compounds such as tris(2,3-epoxypropyl)isocyanurate and 1,4-butanediol diglycidyl ether in combination with 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 3,7-dihydroxy-2-naphthoic acid, 1,2-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,3-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 6-hydroxy-1-naphthoic acid, 3 Compounds obtained by reacting aromatic compounds having two or more carboxyl or phenolic hydroxyl groups, such as 1-hydroxy-2-naphthoic acid, 1-bromo-2-hydroxy-3-naphthoic acid, 1-bromo-4-hydroxy-3-naphthoic acid, 1,6-dibromo-2-hydroxy-3-naphthoic acid, 1,4,5,8-naphthotetracarboxylic acid, 3,5-dihydroxy-2-naphthoic acid, as well as 1,4-dihydroxy-2-naphthoic acid, p-phthalic acid, isophthalic acid, p-hydroxybenzoic acid, m-hydroxybenzoic acid, o-hydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,4-dihydroxybenzoic acid, 2,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, gallic acid, etc.
[0094] The content of the aforementioned developing speed adjuster is, for example, 50 parts by mass or less, or preferably 40 parts by mass or less, and more preferably 30 parts by mass or less, relative to 100 parts by mass of alkali-soluble resin.
[0095] It is preferable that the resist underlayer film formed by the resist underlayer film forming composition of the present invention is a non-photosensitive film.
[0096] For example, when using a photosensitive film as the underlying resist film, a specified amount of exposure is required in order to make the photosensitive film developable.
[0097] However, since the resist film of the present invention is a colored resist film, the resist material forming the colored resist film contains a colorant. When the colored resist film is to be exposed, it is hindered by the colorant, and the light transmittance decreases the further down the colored resist film layer goes. Therefore, when using a photosensitive material as the lower resist layer, the lower resist layer will be exposed to the weak light that has already passed through the colored resist film. In this case, insufficient exposure will occur, and the exposed photosensitive film will not be able to perform its intended function (e.g., developability).
[0098] Therefore, it is preferable to form a pattern of colored resist by controlling the solubility of the colored resist film relative to the developer by setting the firing temperature, regardless of whether the resist film is photosensitive or not.
[0099] Therefore, it is preferable to use a non-photosensitive film instead of a photosensitive film for the resist underlayer.
[0100] <Preparation of the Underlayer Resist> The resist underlayer film of the present invention is a cured film of the above-mentioned resist underlayer film forming composition.
[0101] The resist underlayer film can be manufactured, for example, by coating the above-mentioned resist underlayer film forming composition onto a substrate and then firing it.
[0102] (Layered structure) The laminate of the present invention comprises a substrate, a photoresist lower layer film of the present invention, and a colored photoresist film.
[0103] The substrate and the coloring resist film are described in detail below.
[0104] When fabricating laminates, it is best to set the solvent resistance performance temperature of the lower resist film to be lower than the insolubility temperature of the developer.
[0105] In other words, for example, such as Figure 1 As shown, the temperature at which the resist underlayer exhibits solvent resistance (refer to...) Figure 1 (See attached figure a2) below the developer insolubility temperature (refer to...) Figure 1 The temperature indicated by reference numeral b2 in the attached figure is ideal.
[0106] The firing conditions used to form the lower layer of the resist film are described in detail below.
[0107] It should be noted that the following method for forming a colored resist pattern can also be applied to the laminate of the present invention to create a laminate in which a resist lower layer film and a colored resist film are patterned.
[0108] Furthermore, the self-emissive display element or liquid crystal display element of the present invention can be provided by using a laminate having the pattern of the colored resist that has been patterned.
[0109] The self-emissive display element or liquid crystal display element of the present invention will be described in detail below.
[0110] (Method for forming patterns in colored resist) The method for forming the colored resist pattern of the present invention includes at least the following steps.
[0111] • A process of forming a photoresist underlayer film on a substrate using the photoresist underlayer film forming composition of the present invention; • The process of forming a colored resist film on the resist underlayer film; and • The process of exposing and developing a coloring resist.
[0112] The resist underlayer film forming composition of the present invention is coated onto a substrate using a suitable coating method such as a spin coater or a slot coater. Then, the resist underlayer film is formed by firing using a heating unit such as a heating plate.
[0113] <Substrate> Examples of substrates include: glass substrates, quartz substrates, glass substrates coated with metals such as aluminum, molybdenum, and chromium, glass substrates with inorganic films such as polycrystalline silicon, ITO, IZO, SiN, and SiO2, substrates with organic films, plastic films such as polyimide films, polyethylene terephthalate films, polycarbonate films, and cyclic olefin polymer films, as well as silicon wafers, gallium arsenide, gallium nitride, and other semiconductor substrates. Organic films include color filters, overcoats, planarization films, and other films obtained from UV-cured resins, but are not limited to these.
[0114] <Firing Process> The firing process performed during the formation of the resist underlayer film at the "solvent resistance performance temperature" of the resist underlayer film relative to the solvent contained in the resist material used to form the colored resist film (refer to...). Figure 1 (See attached figure a2) and the "developer insolubility temperature" of the alkaline developer relative to the tinted resist film (refer to the figure). Figure 1 It is best to carry out the experiment under the temperature conditions between (b2) in the attached figure.
[0115] In other words, Figure 1 It is preferable to form a resist underlayer film by firing a coating film composed of a resist underlayer film forming composition at a desired temperature within the temperature range indicated by reference numeral T in the attached figures.
[0116] For example, when the firing temperature is set above b2, a temperature below b2 is required because the lower resist film does not dissolve in the developer.
[0117] On the other hand, if the firing temperature is not set above a2, it will dissolve in the solvent of the coloring resist material, thus causing it to mix with the resist material.
[0118] Therefore, it is best to fire at a temperature that is above a2 and below b2, and at a temperature that will exhibit an ideal rate of development and dissolution.
[0119] Figure 2 This is a schematic diagram showing the relationship between firing temperature and the dissolution of the resist underlayer relative to the developer.
[0120] At once Figure 2Regarding (1), a photoresist underlayer film 2 is formed on the substrate 1. By firing the coating film of the photoresist underlayer film forming composition, a photoresist underlayer film resistant to the solvent contained in the colored photoresist material is formed.
[0121] At once Figure 2 Regarding (2), a colored resist film 3 is formed on the lower resist film 2. Figure 2 (2) shows the state in which the colored resist film 3 and the resist underlayer 2 formed below the colored resist film 3 are developed by irradiation from above the mask 4.
[0122] For example, when firing is carried out at an ideal firing temperature, the resist underlayer dissolves at a good developer dissolution rate, therefore, as Figure 2 As shown in (4), only the portion of the lower resist film 2 corresponding to the portion of the uncolored resist film 3 dissolves, forming a good resist pattern.
[0123] On the other hand, when firing is carried out at a temperature higher than the ideal firing temperature, the lower layer of the resist film is difficult to dissolve in the developer, therefore, as... Figure 2 As shown in (3), sometimes the lower resist film 2 formed under the colored resist film 3 is not fully dissolved in the portion corresponding to the portion of the uncolored resist film 3, leaving residues (residual film, residue, etc.). In this case, a resist pattern with a good shape cannot be obtained.
[0124] Furthermore, when firing is performed at a temperature lower than the ideal firing temperature, the lower resist film easily dissolves in the developer, therefore, as... Figure 2 As shown in (5), sometimes the lower resist film 2 formed under the colored resist film 3 may dissolve excessively in the portion corresponding to the portion of the uncolored resist film 3. In this case, a resist pattern with a good shape cannot be obtained.
[0125] Thus, by firing the coating formed by the resist underlayer film forming composition of the present invention at a suitable temperature condition that makes the dissolution rate of the resist underlayer film relative to the developer solution reach the desired rate, a resist pattern with a good shape can be formed.
[0126] The firing conditions can be appropriately selected from, for example, a firing temperature of 120°C to 250°C and a firing time of 0.5 minutes to 120 minutes. Preferably, the firing temperature is 130°C to 200°C and the firing time is 1 minute to 60 minutes.
[0127] The thickness of the underlying resist film is, for example, 0.001 μm (1 nm) to 10 μm, 0.002 μm (2 nm) to 1 μm, 0.005 μm (5 nm) to 0.5 μm (500 nm), 0.001 μm (1 nm) to 0.05 μm (50 nm), 0.002 μm (2 nm) to 0.05 μm (50 nm), 0.003 μm (3 nm) to 0.05 μm (50 nm), 0.004 μm (4 nm) to 0.05 μm (50 nm), and 0.005 μm (5 nm) to 0.05 μm (50 nm).
[0128] A colored resist film is formed on top of the resist underlayer film.
[0129] The thickness of the colored resist film is, for example, 50 μm or less, 30 μm or less, or 20 μm or less.
[0130] As a colored resist film formed on a resist underlayer by a known method (e.g., coating and firing of a colored resist material), there are no particular limitations as long as the colored resist film is responsive to the light or electron beam (EB) used in the irradiation. Either negative photoresist or positive photoresist can be used.
[0131] <Colored Resist Film> The colored resist film of the present invention is formed using a colored resist material.
[0132] Colored resist materials refer to materials that contain colorants among commonly known resist materials.
[0133] There are no particular restrictions on its use as a colorant; for example, organic or inorganic pigments can be used alone, or a mixture of two or more can be used. Furthermore, dyes can be included within a range that does not reduce heat resistance.
[0134] In addition, metal oxide particles can also be used as inorganic pigments, for example. In particular, white particles (titanium oxide, zirconium oxide, etc.) can also be included. Other examples of inorganic pigments include black inorganic pigments (carbon black, zirconium nitride, zirconium oxide, titanium black, etc.).
[0135] In addition, as organic pigments, black organic pigments (perylene black, lactam black, aniline black, anthraquinone black, azo black pigments, etc.) can also be used.
[0136] As a preferred embodiment of the colored resist film of the present invention, a colored resist film formed using a pigment-dispersed resist material can be cited.
[0137] Furthermore, as a preferred embodiment of the colored resist film of the present invention, a colored resist film formed by dispersing resist materials with metal oxide particles can be cited.
[0138] As long as it is a colorant that can be contained in a typical resist material, it can be used without any particular restrictions.
[0139] The preferred options for corrosion-resistant materials are described below.
[0140] It should be noted that in this specification, the resist that responds to the electron beam (EB) will also be referred to as a photoresist.
[0141] As photoresists, there are: positive photoresists composed of acrylic soluble resins such as phenolic varnish resin, cresol phenolic varnish resin, acrylic copolymer, methacrylic acid copolymer, hydroxystyrene copolymer, hydroxyphenyl acrylamide copolymer, hydroxyphenyl methacrylamide copolymer, and hydroxyphenyl maleimide copolymer, and 1,2-naphthoquinone diazidesulfonate; chemically amplified positive photoresists composed of binders with groups that increase the alkali dissolution rate due to acid decomposition and photoacid-generating agents; and low-molecular-weight compounds that increase the alkali dissolution rate of photoresists due to acid decomposition. Chemically amplified positive photoresist composed of alkali-soluble binders and photoacid generators; chemically amplified positive photoresist composed of binders having groups that increase the alkali dissolution rate due to acid decomposition, low molecular weight compounds that increase the alkali dissolution rate of photoresist due to acid decomposition, and photoacid generators; photoresist containing metal elements; negative photoresist composed of alkali-soluble resins, monomers containing polyvalent unsaturated groups, and photoradical initiators; negative photoresist composed of alkali-soluble resins, polyfunctional cationic polymerizable monomers, and photocationic initiators, etc.
[0142] For example, an alkaline developer is used in the development process.
[0143] Examples of developing temperatures include 5°C to 50°C.
[0144] For example, development time can range from 10 seconds to 300 seconds.
[0145] As an alkaline developer, for example, aqueous solutions of inorganic bases such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, and ammonia; primary amines such as ethylamine and n-propylamine; secondary amines such as diethylamine and di-n-butylamine; tertiary amines such as triethylamine and methyldiethylamine; alkanolamines such as dimethylethanolamine and triethanolamine; quaternary ammonium salts such as tetramethylammonium hydroxide and tetraethylammonium hydroxide; and cyclic amines such as pyrrole and piperidine can be used. Furthermore, an appropriate amount of alcohols such as isopropanol or nonionic surfactants can be added to the above-mentioned alkaline aqueous solutions. Among these, aqueous solutions of potassium hydroxide or quaternary ammonium salts are preferred, and aqueous solutions of tetramethylammonium hydroxide and choline are more preferred. Surfactants can also be added to these developers.
[0146] When the tinted resist film is, for example, a positive resist film, the tinted resist film in the exposed areas dissolves due to the developer during exposure, while the tinted resist film in the unexposed areas remains. In this case, during development, in addition to the tinted resist film in the exposed areas, the underlying resist film formed beneath the tinted resist film in the exposed areas also dissolves due to the developer. That is, the underlying resist film corresponding to the exposed areas where the tinted resist film disappears due to development is also removed during development. By removing the underlying resist film, the residue of the tinted resist film after development is also removed. Thus, the tinted resist film in the desired areas and the underlying resist film formed beneath the tinted resist film in the desired areas are removed by development, thereby preventing the formation of tinted resist film residue and the peeling off of the patterned tinted resist film, resulting in a good pattern of tinted resist.
[0147] Alternatively, if the resist film is, for example, a negative resist film, exposure will cause the resist film in the unexposed areas to dissolve due to the developer, leaving residue in the exposed areas. In this case, during development, in addition to the resist film in the unexposed areas, the underlying resist film formed beneath it will also be dissolved by the developer. That is, the underlying resist film corresponding to the unexposed areas where the resist film disappears during development will also be removed. By removing the underlying resist film, the residue from the resist film after development is also removed. Thus, the resist film in the desired area and the underlying resist film formed beneath it are removed by development, thereby preventing the formation of resist film residue and the peeling off of the patterned resist film, resulting in a well-formed resist pattern.
[0148] (Self-emissive display element) The self-emissive display element of the present invention has the above-described pattern formed by the patterning method of the color resist of the present invention.
[0149] In other words, the self-emissive display element of the present invention has a laminate, which is formed by applying the pattern of the above-described (laminate) to the laminate of the present invention described above, thereby forming a laminate of a resist lower layer film and a resist film through patterning.
[0150] Examples of self-emissive display elements include light-emitting diodes (OLEDs) and micro LEDs that utilize organic EL.
[0151] (Liquid crystal display element) The liquid crystal display element of the present invention has the color resist pattern formed by the pattern forming method of the color resist of the present invention as described above.
[0152] In other words, the liquid crystal display element of the present invention has a laminate, which is formed by applying the pattern of the above-described color resist to the laminate of the present invention described in the above (laminate) column, thereby forming a laminate of a resist underlayer film and a color resist film through patterning.
[0153] Here, examples of liquid crystal display elements include: TN (Twisted Nematic) mode, STN (Super Twisted Nematic) mode, IPS (In-Planes Switching) mode, VA (Vertical Alignment) mode, OCB (Optically Compensated Birefringence) mode, FFS (Fringe Field Switching) mode, or PSA (Polymer Sustained Alignment) mode.
[0154] Example Next, examples will be given to specifically illustrate the content of the present invention, but the present invention is not limited to these examples.
[0155] It should be noted that, in the embodiments, the apparatus and conditions used for sample preparation and property analysis are as follows.
[0156] (1) Ultraviolet irradiation device Device: Canon PLA-600FA (2) Developing apparatus Device: AD-1200 manufactured by Takizawa Sangyo Co., Ltd. (3) Gel permeation chromatography (GPC) Device: Manufactured by Shimadzu Corporation Column: Resonac Corporation's Shodex (registered trademark) GPC K-803L, GPC K-804L Column temperature: 40℃ Eluent: Tetrahydrofuran Number-average molecular weight (hereinafter referred to as Mn) and weight-average molecular weight (hereinafter referred to as Mw) are expressed in polystyrene conversion values.
[0157] (4) Residue evaluation Apparatus: MX61A optical microscope manufactured by Olympus Corporation Apparatus: Hitachi High-Technologies S-4800 scanning electron microscope The abbreviations have the following meanings.
[0158] PMDA: Pyromellitic dianhydride 6FDA: 4,4'-(hexafluoroisopropylidene)phthalic anhydride ODPA: 4,4'-O-diphthalic anhydride PA: Phthalic anhydride BAFP: 2,2-bis(3-amino-4-tolyl)hexafluoropropane DDS: 4,4'-Diaminodiphenyl sulfone TFMB: 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl DBA: 3,5-Diaminobenzoic acid PMA: Pyromellitic acid QD: A compound synthesized by the condensation reaction of 1 mol of α,α,α'-tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene with 2 mol of 1,2-naphthoquinone-2-diazido-5-sulfonyl chloride. GT-401: Butanetetracarboxylic acid tetra(3,4-epoxycyclohexylmethyl) modified ε-caprolactone [EPOLEAD GT-401 manufactured by Daicel Corporation] ELM-434: 4,4'-Methylenebis(N,N-diglycidylaniline) [Sumitomo Chemical Co., Ltd. manufactured SUMI-EPOXY ELM-434] PGME: Propylene Glycol Monomethyl Ether PGMEA: Propylene Glycol Monomethyl Ether Acetate TMAH: Tetramethylammonium hydroxide (Synthesis example 1) <Synthesis of polyamic acid> PMDA 4.36 g, DBA 1.19 g, and BAFP 4.26 g were reacted in PGME 55.6 g at 60 °C for 25 hours to obtain a solution containing polyamic acid [A]. GPC analysis of the obtained polyamic acid showed a weight-average molecular weight Mw = 7600 (converted to standard polystyrene) and a number-average molecular weight Mn = 4100.
[0159] (Synthesis example 2) <Synthesis of polyamic acid> 7.55 g of 6FDA, 2.48 g of DDS, and 1.52 g of DBA were reacted in 65.5 g of PGME at 40 °C for 24 hours. After cooling the resulting solution to room temperature, 0.89 g of PA and 5.0 g of PGME were added, and the mixture was reacted at room temperature for 12 hours to obtain a solution containing polyamic acid [B]. GPC analysis of the obtained polyamic acid showed a weight-average molecular weight Mw = 7040 (converted to standard polystyrene) and a number-average molecular weight Mn = 4570.
[0160] (Synthesis Examples 3 to 8) <Synthesis of polyamic acid> Using the compounds listed in Table 1, solutions containing polyamic acid [C] to [H] were obtained by the same method as in Synthesis Example 2. The compositions are listed in Table 1, and the molecular weights are listed in Table 2. (Synthesis Example 10) <Synthesis of Immunosorbent Modifying Compounds> 19.0 g of 3,7-dihydroxy-2-naphthoic acid, 10 g of tris(2,3-epoxypropyl)isocyanurate and 0.552 g of benzyltriethylammonium chloride were reacted in 118 g of cyclohexanone at 130 °C for 24 hours to obtain a solution containing a developer-adjusting compound (the compound of formula (t) below) as a developer speed adjuster [a]. (Example 1) <Preparation of Composition for Forming Undercoat Film with Resist> A composition for forming a photoresist underlayer was prepared by adding 4.38 g of a solution [a] containing a developer-adjusting compound, 0.630 g of 4,4'-methylenebis(N,N-diglycidylaniline), 52.3 g of PGME, and 67.5 g of PGMEA to a solution [A] containing polyamic acid [A] and stirring at room temperature for 30 minutes [1].
[0161] (Example 2) <Preparation of Composition for Forming Undercoat Film with Resist> A composition for forming a resist underlayer was prepared by adding 0.06 g of PMA, 0.03 g of 4,4'-methylenebis(N,N-diglycidylaniline), 11.98 g of PGME, and 5.88 g of PGMEA to 2.05 g of a solution [B] containing polyamic acid, and stirring at room temperature for 30 minutes.
[0162] (Examples 3-10) <Preparation of Composition for Forming Undercoat Film with Resist> The compositions for forming the resist underlayer film described in Table 3 [3] to
[10] were prepared by the same steps as in Example 2. (Refer to Example 1 for synthesis) <Synthesis of Acrylic Polymer A1> 8.20 g of N-(4-hydroxyphenyl)methacrylamide, 2.19 g of 2-hydroxyethyl methacrylate, 3.77 g of N-cyclohexylmaleimide, and 0.28 g of 2,2'-azobis(isobutyronitrile) were dissolved in 65.76 g of cyclopentanone and reacted at 90 °C for 20 hours to obtain an acrylic polymer solution (solid content concentration 18% by mass) (Al). The obtained acrylic polymer had a Mn of 5100 and a Mw of 7600.
[0163] (Refer to Example 2 for synthesis) <Synthesis of Acrylic Polymer A2> 6.20 g of N-(4-hydroxyphenyl)methacrylamide, 2.28 g of 2-hydroxyethyl methacrylate, 6.27 g of N-cyclohexylmaleimide, and 0.29 g of 2,2'-azobis(isobutyronitrile) were dissolved in 68.49 g of cyclopentanone and reacted at 90 °C for 20 hours to obtain an acrylic polymer solution (solid content concentration 18% by mass) (A2). The obtained acrylic polymer has a Mn of 5200 and a Mw of 10000.
[0164] (Refer to Example 3 for synthesis) <Preparation of Organic Black Pigment Resist> 5.82 g of acrylic polymer solution (A1), 7.18 g of acrylic polymer solution (A2), 0.73 g of QD, and 0.72 g of GT-401 were dissolved in 4.75 g of PGMEA and 1.39 g of cyclopentanone, and stirred at room temperature for 30 minutes. 3.15 g of a solution containing Irgaphor Black S0100CF (manufactured by BASF) dispersed in PGMEA (solid content concentration 21% by mass) was added to the resulting solution, and stirred at room temperature for 30 minutes, thereby preparing an organic black pigment resist [X] (solid content concentration 18% by mass).
[0165] (Evaluation 1) <Evaluation in the case of a resist underlayer film composed of a resist underlayer film forming composition> After applying a composition for forming a photoresist underlayer film [1] to a glass substrate with an ITO film using a spin coater, the substrate is dried at 100°C for 120 seconds on a hot plate, and then fired at 170°C, 175°C, and 180°C for 60 seconds on a hot plate to form a photoresist underlayer film with a thickness of 40 nm.
[0166] The resulting resist lower layer film is insoluble in PGME, PGMEA and cyclopentanone, respectively.
[0167] An organic black pigment resist film [X] with a thickness of 1 μm was formed on the obtained resist base film. The film was then irradiated with 250 mJ / cm² through a mask configured to form a linewidth / gap pattern of 1.0–50 μm. 2 The g, h, and i mixed ultraviolet rays.
[0168] Then, at 23°C, a 60-second immersion development was performed using a 2.38% TMAH aqueous solution, followed by a 30-second rinse with ultrapure water. The coating with the formed linewidth / gap pattern was observed using an optical microscope and a Hitachi High-Technologies S-4800 scanning electron microscope. Regardless of the temperature at which the photoresist underlayer was fired, the photoresist underlayer dissolved along with the photoresist in the exposed areas, exhibiting a close-fitting linewidth / gap pattern of 2.5 μm or more. No residue or residual film was found at the openings.
[0169] (Evaluation 2) <Evaluation under the condition of only having a colored photoresist film> An organic black pigment resist film [X] with a thickness of 1 μm was formed on a glass substrate with an ITO film. The film was then irradiated with 250 mJ / cm² using a mask configured to form a linewidth / gap pattern of 1.0–50 μm. 2 The g, h, and i mixed ultraviolet rays.
[0170] Then, after 60 seconds of immersion development using a 2.38% TMAH aqueous solution at 23°C, the film was rinsed with ultrapure water for 30 seconds. The coating with the formed linewidth / gap pattern was observed using an optical microscope and a Hitachi High-Technologies S-4800 scanning electron microscope. The exposed areas of the photoresist film dissolved, and a linewidth / gap pattern of 30 μm or more was tightly adhered, but the linewidth / gap pattern of less than 20 μm was completely peeled off. A large amount of granular residue was confirmed at the openings.
[0171] (Evaluation 3) <Evaluation of the case where a photoresist underlayer film composed of a photoresist underlayer film forming composition is provided at a low firing temperature> After applying a composition for forming a photoresist underlayer film [1] to a glass substrate with an ITO film using a spin coater, the substrate is dried at 100°C for 120 seconds on a hot plate, and then fired at 140°C and 150°C for 60 seconds on a hot plate to form a photoresist underlayer film with a thickness of 40 nm.
[0172] The resulting resist lower layer film was dissolved in PGME and cyclopentanone, respectively.
[0173] The obtained photoresist underlayer film was subjected to 60 seconds of spin-dip development with 2.38% TMAH aqueous solution at 23°C, followed by 30 seconds of running water rinsing with ultrapure water. However, the photoresist underlayer film had already dissolved.
[0174] Solvent resistance cannot be obtained regardless of the temperature at which the resist underlayer is fired.
[0175] (Rating 4) <Evaluation of the case where a photoresist underlayer film composed of a photoresist underlayer film forming composition is provided at a high firing temperature> After applying a composition for forming a photoresist underlayer film [1] to a glass substrate with an ITO film using a spin coater, the substrate is dried at 100°C for 120 seconds on a hot plate, and then fired at 230°C and 250°C for 60 seconds on a hot plate to form a photoresist underlayer film with a thickness of 40 nm.
[0176] The resulting resist lower layer film is insoluble in PGME, PGMEA and cyclopentanone, respectively.
[0177] The obtained photoresist underlayer film was subjected to 60 seconds of spin-dip development with 2.38% TMAH aqueous solution at 23°C, followed by 30 seconds of running water rinsing with ultrapure water, but the photoresist underlayer film did not dissolve.
[0178] Solvent resistance is obtained regardless of the temperature at which the resist underlayer is fired, but development is not possible.
[0179] (Evaluation 5-1) ~ (Evaluation 5-3) <Evaluation in the case of a resist underlayer film composed of a resist underlayer film forming composition> After applying the composition for forming a photoresist underlayer film [2] to an alkali-free glass substrate using a spin coater, the substrate is dried at 100°C for 120 seconds on a hot plate, and then fired at 165°C, 170°C, and 175°C for 60 seconds on a hot plate to form a photoresist underlayer film with a thickness of 50 nm.
[0180] The resulting resist lower layer film is insoluble in PGMEA.
[0181] A conventional negative black pigment resist [Y] film, comprising a composition containing PGMEA and black pigment, was formed with a thickness of 1 μm on the obtained resist lower layer film. The film was then irradiated with 600 mJ / cm² through a mask configured to form a linewidth / gap pattern of 5.0–75 μm. 2 The g, h, and i mixed ultraviolet rays.
[0182] Then, after immersion development at 23°C for 60 seconds using a 0.04% KOH aqueous solution, the film was rinsed with ultrapure water for 30 seconds. The coating with linewidth / gap pattern was observed using an optical microscope and a Hitachi High-Technologies S-4800 scanning electron microscope. Regardless of the temperature at which the photoresist underlayer was fired, the photoresist underlayer dissolved along with the photoresist in the unexposed areas, and formed a linewidth / gap pattern of more than 15 μm. No residue or residual film was found at the openings. The results of Evaluations 5-1 to 5-3 (collectively referred to as Evaluation 5) are recorded in Table 4.
[0183] (Rating 6-1) ~ (Rating 11-1) <Evaluation in the case of a resist underlayer film composed of a resist underlayer film forming composition> The compositions [3] to [8] for forming the resist underlayer film described in Table 3 were evaluated using the same procedure as in Evaluation 5. The results of Evaluation 6-1 to Evaluation 11-1 are recorded in Table 4.
[0184] (Evaluation 12-1) <Evaluation in the case of only having a colored photoresist film> A common negative black pigment resist [Y] film with a thickness of 1 μm was formed on an alkali-free glass substrate using a composition comprising PGMEA and black pigment. The film was then irradiated with 600 mJ / cm² using a mask configured to form a linewidth / gap pattern of 5.0–75 μm. 2 The g, h, and i mixed ultraviolet rays.
[0185] Then, after immersion development at 23°C for 60 seconds using a 0.04% KOH aqueous solution, the film was rinsed with ultrapure water for 30 seconds. The coating with the linewidth / gap pattern was observed using an optical microscope and a Hitachi High-Technologies S-4800 scanning electron microscope. For samples with any development time, the unexposed areas of the photoresist film dissolved, forming a dense linewidth / gap pattern of more than 15 μm, but a large amount of granular residue was confirmed at the openings. The results of Evaluation 12-1 are recorded in Table 4. The evaluation criteria in Table 4 are as follows.
[0186] [Pattern Evaluation Criteria] ○: Patterns with linewidth / gap greater than 15μm ×: More than half of the material was peeled off. [Residue Evaluation Criteria] 〇: No residue ×: There are residues. [Solvent Resistance Evaluation Criteria] ○: Reduced membrane size ×: Membrane dissolution (Rating 13) <Evaluation of the case where a resist underfilm is provided, which is composed of a resist underfilm forming composition> After applying the composition for forming a photoresist underlayer film [2] to an alkali-free glass substrate using a spin coater, the substrate is dried at 100°C for 120 seconds on a hot plate and then fired at 175°C for 60 seconds on a hot plate to form a photoresist underlayer film with a thickness of 50 nm.
[0187] The resulting resist lower layer film is insoluble in PGMEA.
[0188] A conventional negative black pigment resist [Z] film, comprising a composition containing PGMEA and black pigment, was formed on the obtained resist base layer with a thickness of 1.6 μm. The film was then irradiated with 20 mJ / cm² through a mask configured to form a linewidth / gap pattern of 5.0–20 μm. 2The ultraviolet rays of g, h, i mixture or i line.
[0189] Then, after immersion development at 23°C for 30 seconds using a 0.04% KOH aqueous solution, the film was rinsed with ultrapure water for 30 seconds. The coating with linewidth / gap patterns was observed using an optical microscope and a Hitachi High-Technologies S-4800 scanning electron microscope. Regardless of the temperature at which the photoresist underlayer was fired, the photoresist underlayer dissolved along with the photoresist in the unexposed areas, exhibiting a close-fitting linewidth / gap pattern of 15 μm or more. No residue or residual film was found at the openings.
[0190] (Rating 14) ~ (Rating 15) <Evaluation of the case where a resist underfilm is provided, which is composed of a resist underfilm forming composition> The compositions [9] to
[10] for forming the resist underlayer film described in Table 3 were evaluated using the same steps as in Evaluation 13.
[0191] The results of evaluations 13–15 are shown in Table 5 below. It should be noted that the evaluation criteria for pattern, residue, and solvent resistance in Table 5 are the same as those in Table 4.
[0192] As shown in the above embodiments, by using a resist underlayer film forming composition that can change the dissolution rate of the resist underlayer film relative to the developer, and by firing the resist underlayer film forming composition at a suitable temperature that achieves the desired dissolution rate in the developer, the resulting resist underlayer film exhibits solvent resistance to the solvent contained in the resist material used to form the colored resist film, and exhibits solubility in the alkaline developer of the colored resist film. Furthermore, when patterning the colored resist by disposing such a resist underlayer film between the substrate and the colored resist film, no residue of the colorant insoluble in the developer is generated on the substrate between adjacent resist patterns, and the resist pattern is not easily peeled off from the substrate, thereby forming a good colored resist pattern.
[0193] Explanation of reference numerals in the attached figures 1: Substrate; 2: Underlying film of the resist; 3: Colored resist film; 4: Mask.
Claims
1. A composition for forming a photoresist underlayer film, used to form a photoresist underlayer film disposed between a substrate and a colored photoresist film. The composition for forming the lower layer film of the resist contains an alkali-soluble resin and a solvent. The photoresist underlayer film formed by firing the composition for forming the photoresist underlayer film exhibits solvent resistance to the solvent contained in the photoresist material used to form the colored photoresist film, and exhibits solubility in the alkaline developer of the colored photoresist film.
2. The composition for forming a resist underlayer film according to claim 1, wherein, The alkali-soluble resin is polyamic acid.
3. The composition for forming a resist underlayer film according to claim 1, wherein, The composition for forming the lower layer film of the resist contains a crosslinking agent.
4. The composition for forming a resist underlayer film according to claim 3, wherein, The crosslinking agent is an epoxy compound.
5. The composition for forming a resist underlayer film according to claim 1, wherein, The composition for forming the resist underlayer film contains a developing speed modifier.
6. The composition for forming a resist underlayer film according to claim 5, wherein, The developing speed modifier is a compound containing phenolic hydroxyl or carboxyl groups.
7. A photoresist underlayer film, which is a cured film of the photoresist underlayer film forming composition as described in any one of claims 1 to 6.
8. The resist underlayer film according to claim 7, wherein, The underlying layer of the resist is non-photosensitive.
9. A laminate comprising: a substrate, a photoresist underlayer as described in claim 7, and a colored photoresist film.
10. The laminate according to claim 9, wherein, The photoresist underlayer is configured such that the solvent resistance temperature of the photoresist underlayer relative to the solvent contained in the photoresist material used to form the colored photoresist film is lower than the solvent insolubility temperature of the photoresist underlayer relative to the alkaline developer of the colored photoresist film.
11. A method for forming a pattern of a colored resist, comprising: The process of coating a substrate with the composition for forming a photoresist underlayer as described in any one of claims 1 to 6 and firing it to form a photoresist underlayer; The process of forming a colored resist film on the resist underlayer film; as well as The process of exposing the colored resist film, developing the colored resist film of the desired portion and the underlying resist film formed beneath the colored resist film of the desired portion, thereby obtaining a pattern of colored resist.
12. The method for forming a pattern of a colored resist according to claim 11, wherein, The firing process performed during the formation of the resist underlayer film is carried out at a temperature between the solvent resistance temperature of the resist underlayer film relative to the solvent contained in the resist material used to form the colored resist film and the developer insolubility temperature of the resist underlayer film relative to the alkaline developer of the colored resist film.
13. The method for forming a pattern of a colored resist according to claim 11, wherein, The colored resist film is formed using pigment-dispersed resist materials.
14. The method for forming a pattern of a colored resist according to claim 11, wherein, The colored resist film is formed using metal oxide particles to disperse the resist material.
15. The laminate according to claim 9, wherein, The resist underlayer film and the colored resist film are patterned.
16. A self-emissive display element or liquid crystal display element having a laminate as described in claim 15.
Citation Information
Patent Citations
Organic el display device
JP2005317271A
Display element and display device
JP2023518514A