Method for preparing a battery assembly and battery assembly prepared thereby
By using isostatic pressing, pre-pressed units with different structures are stacked and mechanically pressed, which solves the problem of low yield in the assembly of all-solid-state battery cells, achieves efficient and tight contact between electrodes and solid electrolyte, and improves the preparation yield and performance of battery modules.
Patent Information
- Application Number
- CN202580030183.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-03
- Filing Date
- 2025-06-27
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies suffer from low yields due to mechanical pressing during the fabrication of all-solid-state battery cells, especially large cells, making it difficult to achieve close contact and efficient assembly of electrodes and solid electrolytes.
The isostatic pressing method is used to stack pre-pressed units with different structures and then mechanically press them to form a battery assembly. This ensures close contact between the electrodes and the solid electrolyte, and the pressure and temperature are controlled during the isostatic pressing process to avoid damaging the battery cell assembly.
High-yield (at least 80%, 85%, 90% or 95%) battery module fabrication was achieved, ensuring close contact between electrodes and solid electrolytes, and improving the overall performance and reliability of battery modules.
Smart Images

Figure CN123147033A_ABST
Abstract
Description
[0001] Cross-referencing
[0002] This application claims the benefit of U.S. Serial No. 63 / 667,391, filed July 3, 2024, the entire contents of which are incorporated herein by reference. Technical Field
[0003] This disclosure generally relates to methods for preparing battery modules and battery modules prepared therefrom. Background Technology
[0004] Compared to conventional batteries with liquid electrolytes, all-solid-state batteries (ASSBs) utilize solid electrolytes that exhibit better safety characteristics because they do not leak liquid electrolytes. Assembling the solid electrolyte (SE) with the electrodes is challenging due to the solid-solid interface. To reduce the SE / electrode interface resistance, compression is typically applied to the stack of cell components to maintain tight contact between the solid electrolyte and electrodes. Mechanical pressing or isostatic pressing is commonly used to bring the cell components together. Isostatic pressing utilizes a fluid medium such as oil, water, or gas to compress the cell sealed in a pouch. However, this isostatic pressing is only suitable for small cells or assemblies. Once the cell size becomes relatively large, it becomes too large to fit into the cavity used for isostatic pressing. For large cells, mechanical pressing must be used, which results in low yield due to damage during compression. Therefore, a new design and methodology is still needed to fabricate cell assemblies with high yield. Summary of the Invention
[0005] A method for fabricating battery components with high yield is disclosed. The method includes stacking a first-type pre-compression unit on top of one or more second-type pre-compression units, wherein the first and second types have different constructions, the bottom of the first-type pre-compression unit is functionally complementary to the top of the second-type pre-compression unit, and there is no structural redundancy at the interface between adjacent units. In some embodiments, when multiple second-type pre-compression units are present, the bottom of the first pre-compression unit of the second type is functionally complementary to the top of the second pre-compression unit, and there is no structural redundancy at the interface between them.
[0006] In some embodiments, this disclosure provides a method for fabricating a battery assembly including a plurality of first electrodes, a plurality of second electrodes, and a plurality of solid electrolyte (SE) layers, each SE layer being disposed between the first and second electrodes. The method includes:
[0007] a) A type A pre-compression unit is provided, which is compressed by isostatic compression. The type A unit sequentially includes a top first electrode current collector, a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector.
[0008] b) Provide one or more pre-compression units of type B, each type B unit being compressed onto each of the one or more type B units by isostatic compression, wherein each type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector.
[0009] c) A type A pre-compression unit is stacked on top of one or more type B pre-compression units to form a pre-assembly, wherein the bottom first electrode current collector in the type A pre-compression unit is adjacent to the top first electroactive material layer in one of the one or more type B pre-compression units, and
[0010] d) Pressurize the pre-component to obtain the component.
[0011] In some implementations, the method includes stacking a top first electrode current collector on one or more Type B pre-pressing units to form a pre-assembly and pressurizing the pre-assembly to obtain an assembly.
[0012] In some implementations, the methods disclosed herein can achieve yields of at least 80%, at least 85%, at least 90%, or at least 95%. Attached Figure Description
[0013] Non-limiting embodiments of the present disclosure will be described by way of example with reference to the accompanying drawings, which are schematic and not intended to be drawn to scale. In the drawings, each identical or substantially identical component is generally denoted by the same reference numeral. For clarity, not every component is labeled in every drawing, nor is every component of every embodiment of the present disclosure shown, unless illustrations are required to allow those skilled in the art to understand the disclosure.
[0014] Figure 1 This is a schematic diagram illustrating a typical structure of a battery cell assembly according to one embodiment of the present disclosure.
[0015] Figure 2 This is a schematic diagram illustrating a typical structure of a battery cell assembly according to one embodiment of the present disclosure.
[0016] Figure 3 This is a schematic diagram illustrating a typical construction of a pre-compression unit of type A according to one embodiment of the present disclosure.
[0017] Figure 4 This is a schematic diagram illustrating a typical construction of a pre-compression unit of type A according to another embodiment of this disclosure.
[0018] Figure 5 This is a schematic diagram illustrating a typical construction of a pre-compression unit of type B according to one embodiment of the present disclosure.
[0019] Figure 6 This is a schematic diagram illustrating a typical construction of a pre-compression unit of type B according to another embodiment of this disclosure.
[0020] Figure 7 This is a schematic diagram illustrating a typical structure of a battery cell assembly according to one embodiment of the present disclosure. Detailed Implementation
[0021] This document discloses a method for fabricating battery modules. The method includes stacking a first-type preloaded unit on top of one or more second-type preloaded units, wherein the first and second types have different constructions, and the bottom of the first-type preloaded unit is functionally complementary to the top of the second-type preloaded unit without structural redundancy. In some embodiments, when multiple second-type preloaded units are present, the bottom of the first preloaded unit of the second type is functionally complementary to the top of the second preloaded unit of the second type, without structural redundancy at the interface between them.
[0022] In one implementation, such as Figure 1As shown, a cell assembly (100) is prepared by stacking a type A pre-compression unit (10A) on top of one or more type B pre-compression units (10B) to form a pre-assembly and exposing the pre-assembly to external compression via mechanical pressing to obtain an assembly. In some embodiments, the type A unit sequentially includes a top first electrode current collector (11-1), a top first electroactive material layer (11-2), a top solid electrolyte layer (31), an optional top second electroactive material layer (not shown), a second electrode current collector (2-1), an optional bottom second electroactive material layer (not shown), a bottom solid electrolyte layer (32), a bottom first electroactive material layer (12-2), and a bottom first electrode current collector (12-1). In some embodiments, the type B cell sequentially comprises a top first electroactive material layer (11-2), a top solid electrolyte layer (31), an optional top second electroactive material layer (not shown), a second electrode current collector (2-1), an optional bottom second electroactive material layer (not shown), a bottom SE layer (32), a bottom first electroactive material layer (12-2), and a bottom first electrode current collector (12-1). In some embodiments, the type A or type B cell is compressed by isostatic pressing to independently obtain each pre-compressed cell of type A and type B.
[0023] like Figure 2 As shown, a cell assembly (100) is prepared by stacking a top first electrode current collector (11-1) on one or more type B pre-pressing units (10B) to form a pre-assembly and pressurizing the pre-assembly to obtain an assembly.
[0024] Using this method, components of the battery cell assembly (such as tabs) are protected and will not be damaged or broken due to compression.
[0025] In some embodiments, isostatic pressing for preparing type A and type B units is performed independently within a certain temperature range. In some embodiments, isostatic pressing is cold isostatic pressing (CIP) or warm isostatic pressing (WIP). In some embodiments, isostatic pressing is performed at temperatures ranging from 0°C to 150°C, 0°C to 140°C, 0°C to 130°C, 0°C to 120°C, 0°C to 110°C, 0°C to 100°C, 0°C to 80°C, 0°C to 60°C, 0°C to 40°C, 10°C to 150°C, 10°C to 140°C, 10°C to 130°C, 10°C to 120°C, 10°C to 110°C, 10°C to 100°C, 10°C to 80°C, 10°C to 60°C, 10°C to 40°C, and 20°C to 1... The temperature shall be within any and all ranges and subranges of 50°C, 20°C to 140°C, 20°C to 130°C, 20°C to 120°C, 20°C to 110°C, 20°C to 100°C, 20°C to 80°C, 20°C to 60°C, 20°C to 40°C, 30°C to 150°C, 30°C to 140°C, 30°C to 130°C, 30°C to 120°C, 30°C to 110°C, 30°C to 100°C, 30°C to 80°C, 30°C to 60°C, or between.
[0026] In some embodiments, the isostatic pressing of each unit has a range of 10 MPa to 1000 MPa, 10 MPa to 800 MPa, 10 MPa to 600 MPa, 10 MPa to 400 MPa, 10 MPa to 200 MPa, 10 MPa to 150 MPa, 10 MPa to 125 MPa, 10 MPa to 100 MPa, 10 MPa to 75 MPa, 10 MPa to 50 MPa, 20 MPa to 1000 MPa, 20 MPa to 800 MPa, 20 MPa to 600 MPa, 20 MPa to 400 MPa, 20 MPa to 200 MPa, 20 MPa to 150 MPa, 20 MPa to 125 MPa, 20 MPa to 100 MPa, 20 MPa to 75 MPa, 20 MPa to 5... Operating pressure within any and all ranges and subranges of 0 MPa, 30 MPa to 1000 MPa, 30 MPa to 800 MPa, 30 MPa to 600 MPa, 30 MPa to 400 MPa, 30 MPa to 200 MPa, 30 MPa to 150 MPa, 30 MPa to 125 MPa, 30 MPa to 100 MPa, 30 MPa to 75 MPa, 30 MPa to 50 MPa, 50 MPa to 1000 MPa, 50 MPa to 800 MPa, 50 MPa to 600 MPa, 50 MPa to 400 MPa, 50 MPa to 200 MPa, 50 MPa to 150 MPa, 50 MPa to 125 MPa, 50 MPa to 100 MPa, 50 MPa to 75 MPa, or between.
[0027] In some embodiments, the operating pressure is applied at a controlled rate to allow the cell bag and the cell stack therein to deform slowly, which is crucial for avoiding stress concentration and thus achieving the desired consistency and uniformity. In some embodiments, the operating pressure of the working fluid is specified as 0.1 MPa / min to 20 MPa / min, 0.1 MPa / min to 15 MPa / min, 0.1 MPa / min to 10 MPa / min, 0.1 MPa / min to 7.5 MPa / min, 0.1 MPa / min to 5 MPa / min, 0.1 MPa / min to 2.5 MPa / min, 0.1 MPa / min to 1 MPa / min, 0.1 MPa / min to 0.75 MPa / min, 0.1... MPa / min to 0.5 MPa / min, 0.25 MPa / min to 20 MPa / min, 0.25 MPa / min to 15 MPa / min, 0.25 MPa / min to 10 MPa / min, 0.25 MPa / min to 7.5 MPa / min, 0.25 MPa / min to 5 MPa / min, 0.25 MPa / min to 2.5 MPa / min, 0.25 MPa / min to 1 MPa / min, 0.25 MPa / min to 0.75 MPa / min min, 0.5MPa / min to 20MPa / min, 0.5MPa / min to 15MPa / min, 0.5MPa / min to 10MPa / min, 0.5MPa / min to 7.5MPa / min, 0.5MPa / min to 5MPa / min, 0.5MPa / min to 2.5MPa / min, 0.5MPa / min to 1MPa / min, 1MPa / min to 20MPa / min, 1MPa / min to 15MPa / min, 1MP Rate increases within any and all ranges and subranges of 1 MPa / min to 10 MPa / min, 1 MPa / min to 7.5 MPa / min, 1 MPa / min to 5 MPa / min, 1 MPa / min to 2.5 MPa / min, 2 MPa / min to 20 MPa / min, 2 MPa / min to 15 MPa / min, 2 MPa / min to 10 MPa / min, 2 MPa / min to 7.5 MPa / min, 2 MPa / min to 5 MPa / min, or between.
[0028] In some implementations, the operating pressure of each unit is independently maintained within any and all ranges and subranges of 1 to 60 minutes, 2 to 60 minutes, 3 to 60 minutes, 5 to 60 minutes, 10 to 60 minutes, 1 to 50 minutes, 2 to 50 minutes, 3 to 50 minutes, 5 to 50 minutes, 10 to 50 minutes, 1 to 40 minutes, 2 to 40 minutes, 3 to 40 minutes, 5 to 40 minutes, 10 to 40 minutes, 1 to 30 minutes, 2 to 30 minutes, 3 to 30 minutes, 5 to 30 minutes, 10 to 30 minutes, 1 to 20 minutes, 2 to 20 minutes, 3 to 20 minutes, 5 to 20 minutes, 10 to 20 minutes, or between.
[0029] In some embodiments, isostatic compression for each cell of type A and type B is performed independently before, simultaneously with, or after heating to elevated temperatures within any and all ranges and subranges of 20°C to 150°C, 30°C to 150°C, 40°C to 150°C, 50°C to 150°C, 60°C to 150°C, 70°C to 150°C, 20°C to 120°C, 30°C to 120°C, 40°C to 120°C, 50°C to 120°C, 60°C to 120°C, 70°C to 120°C, 20°C to 100°C, 30°C to 100°C, 40°C to 100°C, 50°C to 100°C, 60°C to 100°C, 70°C to 120°C or between.
[0030] In some implementations, the first electrode is substantially parallel to the second electrode.
[0031] In some implementations, the pre-component is pressurized by placing it in a vacuum bag and then evacuating the bag to a preset vacuum percentage. The vacuum percentage is atmospheric pressure (P0). atm ) and the pressure (P) in the vacuum system v The relative value obtained by dividing the pressure difference between the two points by the atmospheric pressure used as a reference value and multiplying by 100% is (P) atm -P v ) / P atm x100%.
[0032] In some implementations, the preset vacuum percentage is at least 99.0%, at least 99.5%, at least 99.6%, at least 99.7%, at least 99.8%, or at least 99.9%.
[0033] In some embodiments, the vacuum bag is made of a flexible material. In some embodiments, the vacuum bag includes at least one selected from the group consisting of polyethylene (PE), polyvinylidene chloride (PVDC), polypropylene (PP), polyvinyl chloride (PVC), polyester (such as polyethylene terephthalate (PET)), and polyamide (PA). In some embodiments, the vacuum bag includes a film made of biaxially oriented PET (BoPET) (also known as Mylar).
[0034] In some embodiments, the cell assembly may include multiple layers. In some embodiments, the cell assembly, including a cell bag and a cell stack, has a thickness within any and all ranges and sub-ranges of 1 mm to 20 mm, 1 mm to 15 mm, 1 mm to 10 mm, 1 mm to 7.5 mm, 1 mm to 5 mm, 1 mm to 4 mm, 1 mm to 3 mm, 1 mm to 2.5 mm, 1.0 mm to 2.0 mm, 2 mm to 20 mm, 2 mm to 15 mm, 2 mm to 10 mm, 2 mm to 7.5 mm, 2 mm to 5 mm, 2 mm to 4 mm, 2 mm to 3 mm, 2 mm to 2.5 mm, 3 mm to 20 mm, 3 mm to 15 mm, 3 mm to 10 mm, 3 mm to 7.5 mm, 3 mm to 5 mm, 3 mm to 4 mm, or between. In some embodiments, the cell assembly has a smaller thickness than the original cell assembly. In some implementations, the cell assembly has a thickness that is approximately 5%, 10%, 15%, or 20% lower than that of the original cell assembly before isostatic compression.
[0035] In some embodiments, the tabs are made of metal or alloy and are used to electrically connect the battery cell assembly to an external circuit. In some embodiments, non-limiting specific metals include aluminum and copper.
[0036] In some embodiments, the battery cell bag is airtight. In some embodiments, the battery cell bag is made of a material selected from the group consisting of: aluminum foil, aluminum foil with one surface coated with at least one polymer layer, aluminum foil with two surfaces each coated with at least one polymer layer, and combinations thereof.
[0037] In some embodiments, the working fluid in the cavity does not permeate into the cell bag. In some embodiments, under isostatic pressing, the working fluid in the cavity does not permeate into the pressing bag.
[0038] In some embodiments, the compressed bag is made of a material that can seal and isolate the bag from the working fluid. In some embodiments, the bag is made of a membrane. In some embodiments, the membrane is made of polyethylene terephthalate (PET), polyethylene (PE), PU, latex, or mixtures thereof. In some embodiments, the membrane is made of biaxially oriented PET (BoPET) (also known as Mylar). In some embodiments, the film of the compressed bag has a thickness of 0.01 mm to 0.5 mm, 0.01 mm to 0.4 mm, 0.01 mm to 0.3 mm, 0.01 mm to 0.2 mm, 0.01 mm to 0.15 mm, 0.01 mm to 0.10 mm, 0.01 mm to 0.08 mm, 0.01 mm to 0.06 mm, 0.01 mm to 0.04 mm, 0.02 mm to 0.5 mm, 0.02 mm to 0.4 mm, 0.02 mm to 0.3 mm, 0.02 mm to 0.2 mm, 0.02 mm to 0.15 mm, 0.02 mm to 0.10 mm, 0.02 mm to 0.08 mm, or 0.02 mm to 0. Thicknesses ranging from 0.06mm, 0.02mm to 0.04mm, 0.04mm to 0.5mm, 0.04mm to 0.4mm, 0.04mm to 0.3mm, 0.04mm to 0.2mm, 0.04mm to 0.15mm, 0.04mm to 0.10mm, 0.04mm to 0.08mm, 0.04mm to 0.06mm, 0.05mm to 0.5mm, 0.05mm to 0.4mm, 0.05mm to 0.3mm, 0.05mm to 0.2mm, 0.05mm to 0.15mm, 0.05mm to 0.10mm, 0.05mm to 0.08mm, or any and all ranges and subranges thereof.
[0039] In some embodiments, the membrane comprises PE reinforced with polymer fibers (such as nylon) having diameters ranging from 5 μm to 1000 μm, 5 μm to 750 μm, 5 μm to 500 μm, 5 μm to 250 μm, 5 μm to 100 μm, 5 μm to 75 μm, 5 μm to 50 μm, 5 μm to 25 μm, 10 μm to 1000 μm, 10 μm to 750 μm, 10 μm to 500 μm. Within any and all ranges and subranges of μm, 10μm to 250μm, 10μm to 100μm, 10μm to 75μm, 10μm to 50μm, 10μm to 25μm, 25μm to 1000μm, 25μm to 750μm, 25μm to 500μm, 25μm to 250μm, 25μm to 100μm, 25μm to 75μm, 25μm to 50μm or between.
[0040] In some embodiments, the working fluid is a liquid or a gas. Non-limiting specific fluids include water, oil, argon, air, nitrogen, carbon dioxide, and mixtures thereof.
[0041] In some embodiments, the cell assembly is a cell assembly of an all-solid-state battery (ASSB). In some embodiments, the methods described herein are used to prepare an ASSB cell assembly.
[0042] In some embodiments, the ASSB includes a cell stack in which at least one of one or more electrolyte layers contains a solid electrolyte.
[0043] In some embodiments, the solid electrolyte includes polymer solid electrolytes, oxide-based solid electrolytes, sulfide-based solid electrolytes, and any combination thereof.
[0044] In some embodiments, the solid electrolyte is an oxide-based solid electrolyte or a sulfide-based electrolyte. In one embodiment, the solid electrolyte has the formula Li x M1 y M2 z P 1-p M3 p S 6-a-b-q O q Cl a Br b (Formula I), where 4≤x≤8, 0≤y<1, 0≤z<1, 0≤p<1, 0≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6, 0<1-p≤1, where M1 is at least one element other than H or Li in Group 1 or Group 11 of the periodic table, M2 is at least one element in Group 2 of the periodic table, and M3 is at least one element in Group 14 of the periodic table.
[0045] In some embodiments, the solid electrolyte has the formula Li x M1 y M2 z P 1-p M3 p S 6-a-b-q O q Cl a Br b (Equation I), where 4≤x≤8, 0≤y<1, 0≤z<1, 0≤p<1, 0≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6, 0<1-p≤1, and where M1 is at least one element other than H or Li in Group 1 or Group 11 of the periodic table, M2 is at least one element in Group 2 of the periodic table, and M3 is at least one element in Group 14 of the periodic table.
[0046] In some embodiments, M1 is at least one selected from the group consisting of: Na, K, Rb, Cs, Cu, Ag, and Au. In some embodiments, M2 is at least one selected from the group consisting of: Be, Mg, Ca, Sr, and Ba. In some embodiments, M3 is at least one selected from the group consisting of: Si, Ge, Sn, and Pb.
[0047] In some implementations, b / a has a value in the range of 0 to 20, i.e., 0 ≤ b / a ≤ 20.
[0048] In some embodiments, the sulfide solid electrolyte in the electrolyte layer has the formula (i.e., Li x M1 y M2 z P 1- p M3 p S 6-a-b-q O q Cl a Br b It does not include any one of M1, M2, M3, or O, that is, y=z=p=q=0, corresponding to equation Li x PS 6-a- b Cl a Br b .
[0049] In some embodiments, the sulfide electrolyte comprises at least one element selected from the group consisting of: M1, M2, M3, and O. In some embodiments, formula (I) comprises one element selected from the group consisting of: M1, M2, M3, and O. In some embodiments, formula I is selected from the group consisting of:
[0050] 1) Li x M1 y PS 6-a-b Cl a Br b , where 4≤x≤8, 0<y<1, 0≤a≤2, 0≤b<2, 0<6-ab<6;
[0051] 2) Li x M2 z PS 6-a-b Cl a Br b , where 4≤x≤8, 0<z≤1, 0≤a≤2, 0≤b<2, 0<6-ab<6;
[0052] 3) Li x P 1-p M3 p S6-a-b Cl a Br b Where 4≤x≤8, 0<p≤1, 0≤a≤2, 0≤b<2, 0<6-ab<6, 0<1-p<1; and
[0053] 4) Li x PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0<q≤1, 0≤a≤2, 0≤b<2, 0<6-abq<6.
[0054] In some embodiments, formula (I) contains O and an element selected from the group consisting of: M1, M2, and M3. In some embodiments, the sulfide solid electrolyte has a formula selected from the group consisting of: Li x M1 y PS 6-a-b- q O q Cl a Br b (4≤x≤8, 0<y<10≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6), Li x M2 z P1S 6-a-b- q O q Cl a Br b (4≤x≤8, 0<z<1, 0≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6) and Li x P 1- p M3 p S 6-a-b-q O q Cl a Br b (4≤x≤8, 0<p<1, 0≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6, 0<1-p<1). In one embodiment, formula (I) contains O but not M1, M2, or M3. In one embodiment, the sulfide electrolyte has the formula Li. x PS 6-a-b-q O q Cl a Br b(4≤x≤8, 0<q<1, 0≤a≤2, 0≤b<2, 0<6-a-b-q<6). In some embodiments, M1 is at least one element other than H or Li from Group 1 or Group 11 of the Periodic Table of Elements. In some embodiments, M1 is at least one selected from the group consisting of: Na, K, Rb, Cs, Cu, Ag and Au. In some embodiments, M2 is at least one element from Group 2 of the Periodic Table of Elements. In some embodiments, M2 is at least one selected from the group consisting of: Be, Mg, Ca, Sr and Ba. In some embodiments, M3 is at least one element from Group 14 of the Periodic Table of Elements. In some embodiments, M3 is at least one selected from the group consisting of: Si, Ge, Sn and Pb.
[0055] In one embodiment, the sulfide solid electrolyte has the formula Li x PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0<q≤1, 0≤a≤2, 0≤b<2, 0<6-a-b-q<6. Introducing oxygen into the formula makes this material more stable. In some embodiments, the molar amount of O represented by q has a value in the range of 0 to 0.1, 0 to 0.2, 0 to 0.3, 0 to 0.4, 0 to 0.5, 0 to 0.6, 0.001 to 0.1, 0.001 to 0.2, 0.001 to 0.3, 0.001 to 0.4, 0.001 to 0.5, 0.001 to 0.6, 0.002 to 0.1, 0.002 to 0.2, 0.002 to 0.3, 0.002 to 0.4, 0.002 to 0.5, 0.002 to 0.6, 0.005 to 0.1, 0.005 to 0.2, 0.005 to 0.3, 0.005 to 0.4, 0.005 to 0.5, 0.005 to 0.6, or any and all ranges and subranges therebetween. In one embodiment, the formula is Li 5.8 PS 4.7 O 0.1 Cl 1.2 .
[0056] In some embodiments, the formula is Li x PS 6-a-b-q O q Cl a Br b, where 4≤x≤8, 0<q≤1, 0≤a≤2, 0<b<2, 0<6-a-b-q<6. In some embodiments, b / a has a value greater than zero. In some embodiments, b / a has a value in the range of 0 to 3.5. In some embodiments, b / a has a value in the range of 0 to 7. In some embodiments, b / a has a value in the range of 0 to 10, 0 to 15, or 0 to 20.
[0057] In some embodiments, when the formula is Li x M1 y PS 6-a-b-q Cl a Br b , 4≤x≤8, 0<y<1, 0≤a≤2, 0≤b<2, 0<6-a-b<6, and b / a has a value in the range of 0 to 3.5. In some embodiments, b / a has a value in the range of 0 to 7. In some embodiments, b / a has a value in the range of 0 to 10, 0 to 15, or 0 to 20. In some embodiments, b / a has a value greater than zero.
[0058] In some embodiments, when the formula is Li x M2 z PS 6-a-b Cl a Br b , where 4≤x≤8, 0<z≤1, 0≤a≤2, 0≤b<2, 0<6-a-b<6, and b / a has a value in the range of 0 to 3.5. In some embodiments, b / a has a value in the range of 0 to 7. In some embodiments, b / a has a value in the range of 0 to 10, 0 to 15, or 0 to 20. In some embodiments, b / a has a value greater than zero.
[0059] In one embodiment, when the formula is Li x P 1-p M3 p S 6-a-b Cl a Br b , 4≤x≤8, 0<p≤1, 0≤a≤2, 0≤b<2, 0<6-a-b<6, 0<1-p<1, and b / a has a value in the range of 0 to 3.5. In some embodiments, b / a has a value in the range of 0 to 7. In some embodiments, b / a has a value in the range of 0 to 10, 0 to 15, or 0 to 20. In some embodiments, b / a has a value greater than zero.
[0060] In some embodiments, formula (I) contains O and an element selected from the group consisting of: M1, M2, and M3. In some embodiments, the sulfide solid electrolyte has a formula selected from the group consisting of: Li x M1 y PS 6-a-b- q O q Cl a Br b (4≤x≤8, 0<y<1, 0<q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6), Li x M2 z PS 6-a-b- q O q Cl a Br b (4≤x≤8, 0<z<1, 0≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6) and Li x P 1- p M3 p S 6-a-b-q O q Cl a Br b (4≤x≤8, 0<p<1, 0<q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6, 0<1-p<1). In one embodiment, formula (I) contains O but not M1, M2 or M3. In one embodiment, the sulfide electrolyte has the formula Li. x PS 6-a-b-q O q Cl a Br b (4≤x≤8, 0<q<1, 0≤≤2, 0≤b<2, 0<6-abq<6). In some embodiments, the molar amount of Br in the formula has a value greater than zero, i.e., b>0.
[0061] In some embodiments, the total molar amount of halogens in the sulfide electrolyte is not greater than 2, i.e., a + b ≤ 2. In one embodiment, the total molar amount of halogens is not less than 2 and not greater than 3, i.e., 2 ≤ a + b ≤ 3. In one embodiment, the total molar amount of halogens is not less than 2 and less than 4, i.e., 2 ≤ a + b < 4. In one embodiment, the total molar amount of Br and Cl is not greater than 2 (i.e., a + b ≤ 2), not less than 2 and not greater than 3 (i.e., 2 ≤ a + b ≤ 3), or not less than 2 and less than 4 (i.e., 2 ≤ a + b < 4).
[0062] In some embodiments, the sulfide solid electrolyte has a formula selected from the group consisting of:
[0063] 1) Li x PS 6-a-b Cl a Br b , where 4≤x≤8, 0≤a≤2, 0≤b<2, 0<6-ab<6;
[0064] 2) Li x M1 y PS 6-a-b Cl a Br b , where 4≤x≤8, 0<y<1, 0≤a≤2, 0≤b<2, 0<6-ab<6;
[0065] 3) Li x M2 z PS 6-a-b Cl a Br b , where 4≤x≤8, 0<z<1, 0≤a≤2, 0≤b<2, 0<6-ab<6;
[0066] 4) Li x P 1-p M3 p S 6-a-b Cl a Br b , where 4≤x≤8, 0<p<1, 0≤a≤2, 0≤b<2, 0<6-ab<6, 0<1-p<1;
[0067] 5) Li x PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0<q≤1, 0≤a≤2, 0≤b<2, 0<6-abq<6;
[0068] 6) Li x M1 y PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0<y<1, 0<q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6;
[0069] 7) Li x M2 z PS 6-a-b-q O q Cl a Br b, where 4≤x≤8, 0<z<1, 0≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6;
[0070] 8) Li x P 1-p M3 p S 6-a-b-q O q Cl a Br b Where 4≤x≤8, 0<p<1, 0<q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6, 0<1-p<1; and
[0071] 9) Its mixture.
[0072] In some implementations, the first electrode is a cathode or an anode.
[0073] In some implementations, the anode comprises lithium metal or a lithium alloy.
[0074] In some implementations, the first electrode is a cathode.
[0075] In some implementations, the method achieves a yield of at least 80%, at least 85%, at least 90%, at least 91%, at least 92%, at least 93%, at least 94%, or at least 95%. Yield is calculated by dividing the number of cell assemblies tested for short circuits by the total number of cell assemblies and multiplying by 100%.
[0076] In some embodiments, this disclosure provides batteries prepared according to any of the methods disclosed herein.
[0077] In some embodiments, each type A preloaded unit may comprise 2n layers of first electroactive material, where n is an integer equal to or greater than 0. In some embodiments, n may be 0, 2, 4, 6, 8, or 10. When n is 0, it refers to the case where the type A preloaded unit is a top first electrode current collector, such as... Figure 2 As shown.
[0078] like Figure 1 and Figure 3 As representatively shown, type A pre-compression units consist of two layers. For example... Figure 4 As shown, a type A pre-compression unit comprises four layers. In some embodiments, a type A pre-compression unit includes:
[0079] • Four first electroactive material layers, namely 11-2, 12-2, 13-2, and 14-2.
[0080] • Three first electrode current collectors, namely 11-1, 12-1, and 14-1,
[0081] • Four SE layers, namely 31, 32, 33, and 34, and
[0082] • Two second electrodes, namely 21 and 22, wherein the first second electrode 21 includes 21-1 as a current collector, and the second second electrode includes a current collector, namely 22-1.
[0083] In some embodiments, the type B pre-compression unit may comprise 2m layers of first electroactive material, where m is an integer equal to or greater than 1. In some embodiments, m may be 2, 4, 6, 8, or 10. Figure 5 As representatively shown, the type B preloading unit comprises two layers, with... Figure 1 Same as shown in B. Figure 6 As shown, the type B preloading unit comprises four layers. In some embodiments, a type B preloading unit includes:
[0084] • Four first electroactive material layers, namely 11-2, 12-2, 13-2, and 14-2.
[0085] • Two first electrode current collectors, namely 12-1 and 14-1,
[0086] • Four SE layers, namely 31, 32, 33, and 34, and
[0087] • Two second electrodes, namely 21 and 22, wherein the first second electrode 21 includes 21-1 as a current collector, and the second second electrode includes a current collector, namely 22-1.
[0088] In some implementations, a cell assembly can be fabricated by stacking a type A preload cell with 2n layers on top of one or more type B preload cells with 2m layers, where n is an integer equal to or greater than 0, and m is an integer equal to or greater than 1. In some implementations, n and m may be the same or different.
[0089] In some embodiments, the method includes stacking a first-type preloading unit on top of one or more second-type preloading units, wherein the first and second types have different constructions, the bottom of the first-type preloading unit is functionally complementary to the top of the second-type preloading unit, and there is no structural redundancy at the interface between adjacent units. In some embodiments, when multiple second-type preloading units are present, the bottom of the first preloading unit of the second type is also functionally complementary to the top of the second preloading unit of the second type, and there is no structural redundancy at the interface between them. In some embodiments, such as Figure 1As shown, the bottom of the type A pre-loaded unit (10A) is or is configured as the first electrode current collector (12-1). The bottom of the type A pre-loaded unit (10A) is functionally complementary to the top of the type B pre-loaded unit (10B), which is configured as the first electroactive material layer (11-2). Furthermore, the bottom of the type B pre-loaded unit (also configured as the first electrode current collector (12-1)) is functionally complementary to the top of another type B pre-loaded unit. When a type A pre-loaded unit and one or more type B pre-loaded units are stacked along the stacking direction, they form a complete battery assembly.
[0090] The construction and combination of different types of units (or models) are not limited to those illustrated in the figures. In some embodiments, the bottom of the first and second type preloaded units is a first electrode current collector, while the top of the second type preloaded unit is a first electroactive material layer.
[0091] In some embodiments, the bottom of the first and second type pre-loading units is a first electroactive material layer, while the top of the second type pre-loading unit is a first electrode current collector. In some cases, the pre-assembly also includes one or two current collectors, such that the terminating layer of the final assembly is the first or second electrode current collector instead of the electroactive material layer or the SE layer. In some cases, a first type pre-loading unit may have p layers of the first electroactive material layer, where p is an integer equal to or greater than 0. In some cases, a second type pre-loading unit may have q layers of the first electroactive material layer, where q is an integer equal to or greater than 0.
[0092] In some implementations, the first electrode is a cathode or an anode.
[0093] In some embodiments, the battery is an anode-less or anode-free battery, wherein an anode active material layer is formed after the first charge. In some embodiments, the bottom of the first and second type pre-loaded units is an anode current collector, while the top of the second type pre-loaded unit is an SE layer. In some embodiments, the bottom of the first and second type pre-loaded units is an SE layer, while the top of the second type pre-loaded unit is an anode current collector.
[0094] In some embodiments, a first-type preloading unit sits atop one or more second-type preloading units, wherein the first and second types have different constructions. On one hand, the bottom of the first-type preloading unit is functionally complementary to the top of the second-type preloading unit, with no structural redundancy between adjacent units. On the other hand, the bottom of the second-type first preloading unit is functionally complementary to the top of the second-type second preloading unit, with no structural redundancy between adjacent units, wherein the second preloading unit is below the first preloading unit.
[0095] In some implementations, the preload unit of type A, which is typically of the first type, can be further divided into two or more components. For example, the type A preload unit can be divided into a top first electrode current collector (11-1) and a type B preload unit (as of the second type). Figure 2 As shown, a cell assembly can be fabricated by stacking a top first electrode current collector (11-1) on top of one or more type B pre-loaded cells, which are typical of the second type. The bottom of the type A pre-loaded cell is functionally complementary to the top of the type B pre-loaded cell, without structural redundancy. Structural redundancy refers to two components in two sub-cells that, after stacking, do not introduce new functionality beyond that of the individual sub-cells (i.e., before the sub-cells are stacked or combined into a larger assembly). Structural redundancy can lead to lower energy density if the redundant components contribute little or nothing to the energy density.
[0096] In some embodiments, the type A preload unit can be further divided into two or more components. For example, the type A preload unit can be divided into a top first electrode current collector (11-1) and a type B preload unit. In some embodiments, the cell assembly (100) is fabricated by stacking multiple first electrode current collectors with one or more type C preload units, such as... Figure 7 As exemplarily shown in the example.
[0097] In some embodiments, the type B preload unit is further divided into a bottom first electrode current collector (12-1) and a type C preload unit. For example, the assembly (100) can be fabricated by stacking a top first electrode current collector (11-1), one or more type C preload units, and one or more bottom first electrode current collectors (12-1), as shown below. Figure 7 As shown.
[0098] In some implementations, the assembly can be fabricated by stacking a type A preload unit, one or more type C preload units, and one or more bottom electrode current collectors.
[0099] In some implementations, the assembly can be fabricated by stacking a type A preload unit, one or more type B preload units, one or more type C preload units, and one or more bottom electrode current collectors.
[0100] Although the disclosed teachings have been described with reference to various applications, methods, compounds, compositions, and materials, it should be understood that various changes and modifications may be made to them without departing from the teachings herein. The following examples are provided to better illustrate the disclosed teachings and are not intended to limit the scope of the teachings presented herein. As described herein, when a component such as a layer, unit, part, etc., is described as “on another component,” “above another component,” or “on top of another component,” this includes scenarios where the component is directly on top of another component and scenarios where a third component is located between the two components. Terms such as “first” and “second” can be used to describe a variety of components, but components should not be limited by the terms. Terms such as “top” and “bottom” are used to distinguish one component from another based on their relative positions and are not limited to a fixed configuration where the top component is on top of the bottom component. For example, a top first electrode current collector should be interpreted as a first electrode current collector placed above or below another component to the left or right of the other component.
[0101] Although this teaching has been described with reference to these exemplary embodiments, those skilled in the art will readily understand that many variations and modifications of these exemplary embodiments are possible without excessive experimentation. All such variations and modifications are within the scope of the teachings of this disclosure.
[0102] Example
[0103] Preparation of battery cell components
[0104] Type A pre-pressed units are prepared by sequentially stacking the top first electrode current collector, the top first electroactive material layer, the top solid electrolyte layer, the second electrode current collector, the bottom solid electrolyte layer, the bottom first electroactive material layer, and the bottom first electrode current collector into a bag, performing isostatic pressing, and then removing the stacked units from the bag. Type B pre-pressed units are prepared in a similar manner, except that they do not include the top first electrode current collector.
[0105] Cell assemblies are fabricated by stacking one Type A pre-loaded cell on top of one or more Type B pre-loaded cells, followed by pressurization in a vacuum chamber to achieve a vacuum percentage of at least 99.8%. A 4Ah capacity cell assembly is assembled using one Type A pre-loaded cell and one Type B pre-loaded cell, where each cell has a capacity of 2Ah. An 8Ah capacity cell assembly is assembled using one Type A pre-loaded cell and three Type B pre-loaded cells. For comparative examples, cell assemblies are fabricated using a one-step WIP process, where all components are stacked without forming cells. Yields are summarized in Table 1. Yield is determined by dividing the number of cell assemblies that pass the short-circuit test by 100% of all cell assemblies.
[0106] The results show that the comparative method achieves yields of approximately 77% and 66% for modules with capacities of 4Ah and 8Ah, respectively. As module capacity increases, more layers are required for stacking, potentially leading to lower yields. In contrast, this method achieves a constant yield of approximately 95% for both cell modules.
[0107] Table 1. Yield of all-solid-state battery (ASSB) modules
[0108]
[0109] All aspects
[0110] In a first aspect of this disclosure, a method for fabricating a battery assembly is disclosed, wherein the battery assembly includes a plurality of first electrodes, a plurality of second electrodes, and a plurality of solid electrolyte (SE) layers, each SE layer being disposed between the first electrodes and the second electrodes. The method includes:
[0111] A preloading unit of type I is stacked on top of one or more preloading units of type II to form a pre-assembly, wherein the type I and type II have different constructions, and the bottom of the preloading unit of type I is functionally complementary to the top of the preloading unit of type II without structural redundancy; and
[0112] Pressure is applied to the pre-component to obtain the component.
[0113] In the second aspect of the first aspect, the pre-component includes a first pre-compression unit and a second pre-compression unit of the second type, and the bottom of the first pre-compression unit of the second type is functionally complementary to the top of the second pre-compression unit of the second type without structural redundancy.
[0114] According to the third aspect of the first aspect, the first type of pre-compression unit is a type A pre-compression unit prepared by compressing a type A unit by isostatic compression. The type A unit sequentially includes a top first electrode current collector, a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector. Each second type of pre-compression unit is a type B pre-compression unit prepared by compressing a type B unit by isostatic compression. Each type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector. The bottom first electrode current collector in the type A pre-compression unit is adjacent to the top first electroactive material layer in one or more type B pre-compression units.
[0115] In the fourth aspect of the first aspect, the first type of pre-compression unit is a first electrode current collector, and each second type of pre-compression unit is a type B pre-compression unit prepared by compressing a type B unit by isostatic compression, wherein each type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector, and the top first electrode current collector of the first type is adjacent to the top first electroactive material layer in one of the one or more type B pre-compression units.
[0116] In the fifth aspect of the first aspect, the first electrode is a cathode and the second electrode is an anode.
[0117] In the sixth aspect according to the fifth aspect, the anode contains lithium metal or a lithium alloy.
[0118] According to the seventh aspect of the first aspect, the battery is an all-solid-state battery (ASSB) comprising a polymer electrolyte, an inorganic oxide electrolyte, or an inorganic sulfide electrolyte. In some embodiments, the inorganic sulfide electrolyte has the formula (I): Li x M1 y M2 z P 1-p M3 p S 6-a-b-q O q Cl a Br b(Formula I), where 4≤x≤8, 0≤y<1, 0≤z<1, 0≤p<1, 0≤q<1, 0≤a≤2, 0≤b<2, 0<6-abq<6, 0<1-p≤1, where M1 is at least one element other than H or Li in Group 1 or Group 11 of the periodic table, M2 is at least one element in Group 2 of the periodic table, and M3 is at least one element in Group 14 of the periodic table.
[0119] According to the eighth aspect of the first aspect, isostatic compression for each unit of the first and second types is performed independently at a temperature ranging from 0°C to 150°C and at a pressure ranging from 10 MPa to 1000 MPa perpendicular to the surface of the first electroactive material layer. In some embodiments, isostatic compression for each unit of the first and second types is performed independently before, simultaneously with, or after heating to an elevated temperature ranging from 20°C to 150°C.
[0120] In the ninth aspect according to the first aspect, the first electrode is substantially parallel to the second electrode.
[0121] In the tenth aspect of the first aspect, the pre-component is pressurized by placing the pre-component in a vacuum bag and then evacuating the vacuum bag to a preset vacuum percentage.
[0122] In the eleventh aspect of the tenth aspect, the preset vacuum percentage is at least 99.0%.
[0123] In the twelfth aspect according to any of the foregoing aspects, the method achieves a yield of at least 80%, wherein the yield is obtained by dividing the number of cell assemblies tested by short circuit by the total number of cell assemblies multiplied by 100%.
[0124] In the thirteenth aspect of this disclosure, the method includes:
[0125] a) A type A pre-compression unit is provided, which is compressed by isostatic compression. The type A unit sequentially includes a top first electrode current collector, a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector.
[0126] b) Provide one or more pre-compression units of type B, each type B unit being compressed onto each of the one or more type B units by isostatic compression, wherein each type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector.
[0127] c) A type A pre-compression unit is stacked on top of one or more type B pre-compression units to form a pre-assembly, wherein the bottom first electrode current collector in the type A pre-compression unit is adjacent to the top first electroactive material layer in one of the one or more type B pre-compression units, and
[0128] d) Pressurize the pre-component to obtain the component.
[0129] In the fourteenth aspect according to the thirteenth aspect, the first electrode is a cathode and the second electrode is an anode. In some embodiments, the first electrode is substantially parallel to the second electrode. In some embodiments, the pre-assembly is pressurized by placing the pre-assembly in a vacuum bag and then evacuating the vacuum bag to a preset vacuum percentage. In some embodiments, the preset vacuum percentage is at least 99.0%.
[0130] In the fifteenth aspect of this disclosure, the method includes:
[0131] Set the top first electrode collector.
[0132] One or more Type B pre-compression units are provided, each Type B unit being compressed onto each of the one or more Type B units by isostatic compression, wherein each Type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector.
[0133] A top first electrode current collector is stacked on one or more type B pre-pressed units to form a pre-assembly, wherein the top first electrode current collector is adjacent to a top first electroactive material layer in the type B pre-pressed unit, and
[0134] Pressure is applied to the pre-component to obtain the component.
[0135] In some embodiments, the first electrode is a cathode, and the second electrode is an anode. In some embodiments, the anode comprises lithium metal or a lithium alloy. In some embodiments, isostatic compression for each cell of type A and type B is performed independently at a temperature ranging from 0°C to 150°C and at a pressure ranging from 10 MPa to 1000 MPa perpendicular to the surface of the first electroactive material layer. In some embodiments, isostatic compression for each cell of type B is performed before, simultaneously with, or after heating to an elevated temperature ranging from 20°C to 150°C.
[0136] In some embodiments, this disclosure provides batteries prepared according to any of the foregoing aspects.
[0137] While this specification contains details of numerous specific embodiments, these should not be construed as limiting the scope of any invention or the scope that may be claimed, but rather as descriptions of features specific to particular embodiments of a particular invention. Certain features described in the specification within the context of separate embodiments may also be implemented in combination in a single embodiment. Conversely, various features described in the context of a single embodiment may also be implemented separately or in any suitable sub-combination in multiple embodiments. Furthermore, although features may be described above as functioning in certain combinations and even initially claimed in this way, in some cases, one or more features from the claimed combination may be removed from the combination, and the claimed combination may involve sub-combinations or variations of sub-combinations.
[0138] All transitional phrases (such as “including,” “contains,” “carries,” “has,” “includes,” “involves,” “holds,” “constituts,” etc.) should be understood as open-ended, meaning including but not limited to. Only the transitional phrases “constituts of” and “substantially constitutes of” should be closed or semi-closed transitional phrases, respectively.
[0139] This document describes various embodiments of the features of this disclosure. However, it should be understood that such embodiments are provided merely as examples, and many variations, modifications, and substitutions will occur to those skilled in the art without departing from the scope of this disclosure. It should also be understood that various alternatives to the specific embodiments described herein are also within the scope of this disclosure.
Claims
1. A method for fabricating a battery assembly, the battery assembly comprising a plurality of first electrodes, a plurality of second electrodes, and a plurality of solid electrolyte layers, i.e., a plurality of SE layers, each SE layer being disposed between the first electrodes and the second electrodes, the method comprising: • A pre-compression unit of type 1 is stacked on top of one or more pre-compression units of type 2 to form a pre-assembly, wherein the type 1 and type 2 have different constructions, and the bottom of the pre-compression unit of type 1 is functionally complementary to the top of the pre-compression unit of type 2 without structural redundancy. as well as • Pressurize the pre-component to obtain the component.
2. The method of claim 1, wherein the pre-component comprises a first pre-compression unit and a second pre-compression unit of the second type, and the bottom of the first pre-compression unit of the second type is functionally complementary to the top of the second pre-compression unit of the second type without structural redundancy.
3. The method according to claim 1, wherein the first type of pre-compression unit is a type A pre-compression unit prepared by compressing a type A unit through isostatic compression. The type A unit sequentially includes a top first electrode current collector, a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector. Each pre-compressed unit of the second type is a type B pre-compressed unit prepared by compressing a type B unit through isostatic compression. Each type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector. The bottom first electrode current collector in the type A pre-pressing unit is adjacent to the top first electroactive material layer in one or more type B pre-pressing units.
4. The method of claim 1, wherein the first type of pre-compression unit is a first electrode current collector, each of the second type of pre-compression units is a type B pre-compression unit prepared by compressing a type B unit by isostatic compression, wherein each type B unit sequentially comprises a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector, and the first type of top first electrode current collector is adjacent to the top first electroactive material layer in one or more type B pre-compression units.
5. The method of claim 1, wherein the first electrode is a cathode and the second electrode is an anode.
6. The method of claim 5, wherein the anode comprises lithium metal or a lithium alloy.
7. The method according to claim 1, wherein the battery is an all-solid-state battery comprising a polymer electrolyte, an inorganic oxide electrolyte, or an inorganic sulfide electrolyte, i.e., an ASSB comprising a polymer electrolyte, an inorganic oxide electrolyte, or an inorganic sulfide electrolyte.
8. The method of claim 1, wherein the isostatic compression for each unit of the first type and the second type is performed independently at a temperature in the range of 0°C to 150°C and at a pressure in the range of 10 MPa to 1000 MPa perpendicular to the surface of the first electroactive material layer, and the isostatic compression for each unit of the first type and the second type is performed independently before, simultaneously with or after heating to an elevated temperature in the range of 20°C to 150°C.
9. The method of claim 1, wherein the first electrode is substantially parallel to the second electrode.
10. The method of claim 1, wherein the pre-component is pressurized by placing the pre-component in a vacuum bag and then evacuating the vacuum bag to a preset vacuum percentage.
11. The method of claim 10, wherein the preset vacuum percentage is at least 99.0%.
12. The method according to any one of the preceding claims, wherein the method achieves a yield of at least 80%, wherein the yield is achieved by dividing the number of cell assemblies tested by short circuit by the total number of cell assemblies multiplied by 100%.
13. A method for fabricating a battery assembly, the battery assembly comprising a plurality of first electrodes, a plurality of second electrodes, and a plurality of solid electrolyte layers, i.e., a plurality of SE layers, each SE layer disposed between the first electrodes and the second electrodes, the method comprising: a) A type A pre-compression unit is provided, which is compressed by isostatic compression. The type A unit sequentially includes a top first electrode current collector, a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector. b) Provide one or more pre-compression units of type B, each type B unit being compressed onto each of the one or more type B units by isostatic compression, wherein each type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector. c) A type A pre-compression unit is stacked on top of one or more type B pre-compression units to form a pre-assembly, wherein the bottom first electrode current collector in the type A pre-compression unit is adjacent to the top first electroactive material layer in one of the one or more type B pre-compression units, and d) Pressurize the pre-component to obtain the component.
14. The method of claim 13, wherein the first electrode is a cathode and the second electrode is an anode.
15. A method for preparing a battery assembly, the battery assembly comprising a plurality of first electrodes, a plurality of second electrodes, and a plurality of solid electrolytes, each solid electrolyte disposed between the first electrodes and the second electrodes, the method comprising: a) Set the top first electrode collector. b) Provide one or more pre-compression units of type B, each type B unit being compressed onto each of the one or more type B units by isostatic compression, wherein each type B unit sequentially includes a top first electroactive material layer, a top solid electrolyte layer, an optional top second electroactive material layer, a second electrode current collector, an optional bottom second electroactive material layer, a bottom solid electrolyte layer, a bottom first electroactive material layer, and a bottom first electrode current collector. c) The top first electrode current collector is stacked on one of the one or more Type B pre-pressing units to form a pre-assembly, wherein the top first electrode current collector is adjacent to the top first electroactive material layer in the Type B pre-pressing unit, and d) Pressurize the pre-component to obtain the component.