Printed wiring board

By forming a stacked portion with excellent organizational integrity on the printed wiring board, the problem of uniform etching of the substrate layer and electroplated coating layer is solved, and the miniaturization and rectangularity of the circuit are improved.

CN123147242APending Publication Date: 2026-11-20SUMITOMO ELECTRIC INDUSTRIES LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580027088.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-12
Filing Date
2025-03-13
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In the process of miniaturizing printed wiring boards, existing technologies make it difficult to uniformly etch the substrate layer and electroplating layer, resulting in damage to the rectangularity of the circuit.

Method used

By forming a laminate with excellent microstructure on the base film, uniform etching of the base layer and the electroplated coating is ensured. The grain distribution is determined by electron backscatter diffraction, and the grain area ratio is controlled to improve the microstructure of the laminate.

Benefits of technology

It achieves excellent rectangularity of printed wiring board circuits, improves etching uniformity and circuit miniaturization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123147242A_ABST
    Figure CN123147242A_ABST
Patent Text Reader

Abstract

A printed wiring board has a base film and a laminated portion. The base film has a main surface. The laminated portion is disposed on the main surface. When a cross section of the laminated portion is measured by electron backscatter diffraction method under conditions in which a grain boundary threshold value is 10° or less, in a first region from the main surface to 4 μm, a proportion of an area occupied by a crystal grain having an equivalent circle diameter of 3 μm or more is set as a first area ratio. The first area ratio is 0.8 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a printed wiring board. This application claims priority to international application PCT / JP2024 / 014864, filed April 12, 2024. The entire contents of that application are incorporated herein by reference. Background Technology

[0002] International Publication No. 2019 / 208077 (Patent Document 1) discloses a substrate for a printed wiring board having a base film and an electroless plating layer.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: International Publication No. 2019 / 208077 Summary of the Invention

[0006] The printed wiring board disclosed herein includes a base film and a laminate. The base film has a main surface. The laminate is disposed on the main surface. When measuring the cross-section of the laminate using electron backscatter diffraction under conditions where the grain boundary threshold is 10° or less, in a first region from the main surface to 4 μm, the proportion of the area occupied by grains with an equivalent circle diameter of 3 μm or more is set as a first area ratio. The first area ratio is 0.8 or more. Attached Figure Description

[0007] Figure 1 This is a cross-sectional view showing the structure of the printed wiring board substrate according to Embodiment 1.

[0008] Figure 2 This is a flowchart illustrating a method for manufacturing a printed wiring board substrate according to Embodiment 1.

[0009] Figure 3 This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board substrate according to Embodiment 1.

[0010] Figure 4 This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board substrate according to Embodiment 1.

[0011] Figure 5 This is a cross-sectional view showing a modified example of the structure of the printed wiring board substrate according to Embodiment 1.

[0012] Figure 6 This is a flowchart illustrating a modified example of the manufacturing method of the printed wiring board substrate according to Embodiment 1.

[0013] Figure 7This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board substrate according to Embodiment 1.

[0014] Figure 8 This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board substrate according to Embodiment 1.

[0015] Figure 9 This is a schematic diagram of the plating apparatus.

[0016] Figure 10 This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board substrate according to Embodiment 1.

[0017] Figure 11 This is a cross-sectional view showing the structure of the printed wiring board according to Embodiment 2.

[0018] Figure 12 This is a flowchart illustrating the manufacturing method of the printed wiring board according to Embodiment 2.

[0019] Figure 13 This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board according to Embodiment 2.

[0020] Figure 14 This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board according to Embodiment 2.

[0021] Figure 15 This is a cross-sectional view showing one step of the manufacturing method of the printed wiring board according to Embodiment 2.

[0022] Figure 16 It is a printed wiring board that shows the orientation distribution of crystals.

[0023] Figure 17 yes Figure 11 A schematic cross-sectional view of the stacked portion shown in region XVII.

[0024] Figure 18 This is a cross-sectional view of a printed wiring board substrate, which is the object of measurement for the orientation distribution of crystals.

[0025] Figure 19 This refers to the grain distribution in the stacked portion of sample 1.

[0026] Figure 20 This refers to the grain distribution in the stacked portion of sample 7.

[0027] Figure 21 This refers to the grain distribution in the stacked portion of sample 1.

[0028] Figure 22This refers to the grain distribution in the stacked portion of sample 7.

[0029] Figure 23 This is a top view of the TEG (Test Element Group) used for evaluation. Detailed Implementation

[0030] [The technical problem this disclosure aims to solve]

[0031] The miniaturization of printed circuit boards is required. In the semi-additive process, suitable for forming miniaturized circuits, a circuit is formed by a series of steps including resist patterning, electroplating, resist removal, and substrate etching on the surface of a base film with a substrate layer. This process creates a circuit consisting of a stack of layers containing a substrate layer and an electroplated layer. However, in the etching process of the substrate layer, it is difficult to uniformly etch both the substrate layer and the electroplated layer, potentially compromising the rectangularity of the circuit.

[0032] The purpose of this disclosure is to provide a printed wiring board with circuitry exhibiting excellent rectangularity.

[0033] [The Effects of This Disclosure]

[0034] According to this disclosure, a printed wiring board with circuitry exhibiting excellent rectangularity can be provided.

[0035] [Summary of Implementation Methods]

[0036] First, embodiments of this disclosure will be described.

[0037] (1) The printed wiring board of this disclosure includes a base film and a laminate. The base film has a main surface. The laminate is disposed on the main surface. When measuring the cross-section of the laminate by electron backscatter diffraction under conditions where the grain boundary threshold is 10° or less, in a first region from the main surface to 4 μm, the proportion of the area occupied by grains with an equivalent circle diameter of 3 μm or more is set as a first area ratio. The first area ratio is 0.8 or more.

[0038] (2) In the printed wiring board of (1) above, the proportion of the area occupied by grains with an equivalent circle diameter of 3 μm or more in the second region other than the first region in the cross section of the laminate can also be set as the second area ratio. The first area ratio can also be 0.8 times or more of the second area ratio.

[0039] (3) In the printed wiring board of (1) and (2) above, the direction perpendicular to the main surface may be designated as the first direction. The direction perpendicular to the first direction may be designated as the second direction. The direction perpendicular to both the first and second directions may be designated as the third direction. The laminate may also be formed in a linear manner extending along the second direction. The laminate may also include adjacent first and second laminates. The width of each of the first and second laminates may be 15 μm or less. The shortest distance in the third direction from the first laminate to the second laminate may also be 15 μm or less.

[0040] (4) In the printed wiring board of (3) above, the width of the first layer stack and the width of the second layer stack can also be 10 μm or less. The shortest distance in the third direction from the first layer stack to the second layer stack can also be 10 μm or less.

[0041] (5) In the printed wiring board of (3) or (4) above, the width of the first layer stack and the width of the second layer stack can also be 2 μm or more. The shortest distance in the third direction from the first layer stack to the second layer stack can also be 2 μm or more.

[0042] (6) In any of the printed wiring boards described in (1) to (5) above, the laminate may also include a substrate layer and an electroplated coating layer. The substrate layer may also be in contact with the main surface. The electroplated coating layer may also be in contact with the substrate layer.

[0043] [Details of the implementation method]

[0044] The embodiments of this disclosure will be described in detail with reference to the accompanying drawings. In the following drawings, the same or equivalent parts will be labeled with the same reference numerals and will not be described repeatedly. The printed wiring board substrate and the printed wiring board involved in the embodiments will be referred to as the printed wiring board substrate 100 (100a, 100b) and the printed wiring board 200, respectively.

[0045] (Structure of substrate for printed wiring board)

[0046] The structure of the printed wiring board substrate 100a will be described below.

[0047] Figure 1 This is a cross-sectional view of the printed wiring board substrate 100a. (Example) Figure 1 As shown, the substrate 100a for printed wiring boards includes a base film 1 and a base layer 2.

[0048] The base film 1 has a main surface 1s. The base film 1 is formed of a flexible insulating material. For example, the base film 1 is formed of polyimide.

[0049] The substrate layer 2 is in contact with the main surface 1s. The substrate layer 2 is composed of either a sputtered copper layer or a nano-copper sintered body layer. In the case of a nano-copper sintered body layer, this nano-copper sintered body layer is formed from a plurality of sintered copper particles. Therefore, the nano-copper sintered body layer is porous. The average particle size of the copper particles contained in the nano-copper sintered body layer can also be 1 nm or more or 30 nm or more. The average particle size of the copper particles contained in the nano-copper sintered body layer can also be 100 nm or less or 500 nm or less. That is, the copper particles contained in the nano-copper sintered body layer can also be nano-copper particles. In addition, the average particle size of the copper particles contained in the paste used to form the nano-copper sintered body layer is measured by a particle size distribution measuring device (e.g., a Microtrac particle size analyzer UPA-150EX manufactured by Nikkiso Corporation). As described later, an electroless copper plating layer (not shown) can also be formed on the main surface 1s.

[0050] like Figure 1 As shown, the direction perpendicular to the main surface 1s is defined as the first direction X. The substrate layer 2 has a substrate surface 2s. The substrate surface 2s is the surface opposite to the surface of the substrate layer 2 that contacts the main surface 1s. The distance H (thickness H of the substrate layer 2) from the main surface 1s to the substrate surface 2s in the first direction can also be less than 1 μm or less than 0.5 μm. As will be described later, when the thickness H of the substrate layer 2 is less than 1 μm, the fine line formation property of the laminate 20 is improved. As a result, the circuit of the printed wiring board 200 can be miniaturized.

[0051] (Manufacturing method of substrate for printed wiring board)

[0052] The manufacturing method of the printed wiring board substrate 100a will be described below. Figure 2 This is a flowchart illustrating the manufacturing method of the printed wiring board substrate 100a. For example... Figure 2 As shown, the manufacturing method of the printed wiring board substrate 100a includes a step S1a of preparing the base film 1 and a step S2a of forming the base layer 2.

[0053] The process of forming the substrate layer S2a is performed after the process of preparing the base film 1 S1a.

[0054] Figure 3 This is a cross-sectional view illustrating step S1a of preparing the base film 1. In step S1a of preparing the base film 1, as follows... Figure 3 As shown, a base film 1 is prepared. In step S1a of preparing the base film 1, a substrate layer 2 is not disposed on the main surface 1s of the prepared base film 1.

[0055] Before the substrate layer 2 is disposed on the main surface 1s, the main surface 1s is subjected to, for example, alkali treatment and excimer treatment. In the case where the substrate film 1 is, for example, polyimide, the polyimide is hydrolyzed by alkali treatment of the main surface 1s. Specifically, alkali treatment is performed on the main surface 1s of the substrate film 1 by spraying an alkaline solution onto it. Alkali treatment can also be performed by immersing the substrate film 1 in an alkaline solution. The alkaline solution can be, for example, an aqueous solution containing potassium hydroxide or sodium hydroxide. The amount (by weight) of potassium hydroxide or sodium hydroxide added to the alkaline solution is 200g or more and 300g or less per liter of alkaline solution. Next, the main surface 1s of the substrate film 1 is dried for dehydration. The drying temperature during the drying process is, for example, 30°C or more and 60°C or less. For example, if the drying temperature is 40°C, the drying time during the drying process can be, for example, 30 minutes or more and 5 hours or less. As a result, carboxyl groups are formed on the main surface 1s, and the base film 1 becomes hydrophilic. When the main surface 1s is metallized with copper by coating with a paste or by electroless plating, crystal growth becomes uniform. Specifically, by stacking copper with uniformly sized grains on the main surface 1s, the microstructure of the electroplated layer 3 grows continuously relative to the microstructure of the base layer 2. As a result, the microstructure of the electroplated layer 3 becomes integrated with the microstructure of the base layer 2, and the integrity of the microstructure in the stacked portion 20 is improved.

[0056] To further enhance the hydrophilicity of the master surface 1s, it can be subjected to excimer laser treatment after alkali treatment. Specifically, the master surface 1s is irradiated with excimer light. The wavelength of the excimer light is, for example, 172 nm. This allows for controllable crystal growth to achieve uniformity.

[0057] Figure 4 This is a cross-sectional view illustrating process S2a in forming the substrate layer 2. In process S2a in forming the substrate layer 2, as... Figure 4 As shown, the substrate layer 2 is formed on the main surface 1s. In this process S2a, firstly, a paste containing copper particles is applied to the main surface 1s. Secondly, the solvent contained in the applied paste is dried. Thirdly, the dried paste is sintered. Thus, the copper particles contained in the dried paste sinter together to form the substrate layer 2. The substrate layer 2 can also be formed by sputtering. The substrate layer 2 can also be formed using the plating apparatus 300 described later. After forming the substrate layer 2 using the plating apparatus 300, the base film 1 is annealed at an annealing temperature of 300°C for 1 hour.

[0058] Manufacturing through the above methods Figure 1 The printed wiring board substrate 100a shown is an example of such a manufactured substrate 100a. Figure 18As shown, when the electroplated coating 3 is formed on the substrate layer 2s, the structure of the electroplated coating 3 and the structure of the substrate layer 2 grow together as an integral unit. That is, with the improved integrity of the structure in the stacked portion 20, the etching rate of the stacked portion 20 in the first direction X becomes uniform. The stacked portion 20 is composed of the electroplated coating 3 and the substrate layer 2. As will be described later, the etchant used in the semi-additive method is generally a sulfuric acid-hydrogen peroxide etchant. As a result, a stacked portion 20 with excellent rectangularity is formed. Thus, the printed wiring board 200 according to Embodiment 2 described later is obtained.

[0059] The integrity of the structure in the laminate 20, which consists of the substrate layer 2 and the electroplated coating layer 3, is evaluated by the proportion of the area occupied by the grains in the laminate 20. As described later, the area occupied by the grains in the printed wiring board substrate 100 is measured by electron backscattering diffraction pattern (EBSD). Specifically, for example, as... Figure 18 As shown, when the stacked portion 20 is formed including an electroplated layer 3 and a substrate layer 2, the electroplated layer 3 is in contact with the substrate layer 2. The stacked portion 20 has a first surface 21s. The first surface 21s is arranged such that the height Ht of the stacked portion from the main surface 1s to the first surface 21s is 1 μm or more. Before measuring the area occupied by the die on the printed wiring board substrate 500 with the stacked portion 20 formed thereon by EBSD, the printed wiring board substrate 500 is cross-sectionally processed by argon ion polishing. The accelerating voltage of the ion beam is set to, for example, 6 kV. Next, the area occupied by the die in the stacked portion 20 is measured by EBSD. The area occupied by the die is measured using a Germini450 manufactured by ZEISS and a Symmetry manufactured by Oxford. The EBSD measurement conditions are as follows: The accelerating voltage is 15 kV. The electron beam irradiation current is 20 nA. The electron beam accumulation time is 0.8 ms. The SEM worktable has a tilt angle of 70°. The working distance (WD) of the SEM is 15mm.

[0060] When evaluating the integrity of the microstructure in the laminate 20, the grains of the evaluation target are measured by EBSD under conditions where the grain boundary threshold is 10° or less. Furthermore, the equivalent circle diameter of the grains of the evaluation target is set to 3.0 μm or more to ensure that the grains of the evaluation target do not include minute grains. Additionally, grains containing twin boundaries are excluded from the evaluation target. The "equivalent circle diameter" is the diameter of a circle having an area equal to the projected area of ​​the grain.

[0061] The integrity of the structure in the laminate 20 is evaluated based on the area occupied by the grains included in the laminate 20 in the first region V1. Specifically, the first region V1 is the region from the main surface 1s to 4μm. The proportion of the area occupied by grains with an equivalent circle diameter of 3.0μm or more in the first region V1 is defined as the first area ratio r1. That is, the first area ratio r1 is the proportion of the area occupied by grains with an equivalent circle diameter of 3.0μm or more relative to the area occupied by the first region V1. The first area ratio r1 in the printed wiring board substrate 100 according to Embodiment 1 is 0.8 or more. In this way, a printed wiring board substrate 100a with improved integrity of the structure in the laminate 20 is obtained.

[0062] Comparison is also possible Figure 18 The first region V1 and the second region V2 are shown as the proportion of the area occupied by the grains in their respective stacked portions 20. The second region V2 is the region outside the first region V1 in the cross-section of the stacked portion 20. That is, the second region V2 is the region from the first surface 21s to the first region V1. The proportion of the area occupied by grains with an equivalent circle diameter of 3.0 μm or more contained in the second region V2 is defined as the second area ratio r2. That is, the second area ratio r2 is the proportion of the area occupied by grains with an equivalent circle diameter of 3.0 μm or more relative to the area occupied by the second region V2.

[0063] The first area ratio r1 can be more than 0.8 times or more than 1.0 times the second area ratio r2.

[0064] (Structure of a modified example of a substrate for printed wiring boards)

[0065] Figure 5 This is a cross-sectional view of a modified example of the printed wiring board substrate 100a according to Embodiment 1. Figure 5 Corresponding to Figure 1 . Figure 5 The printed wiring board substrate 100b shown basically has the same characteristics as... Figure 1 The printed wiring board substrate 100a shown has the same structure, but differs in that the base layer 2 includes an electroless copper plating layer. Specifically, the base layer 2 includes a first base layer 2a and a second base layer 2b. Specifically, the first base layer 2a is composed of either a sputtered copper layer or a nano-copper sintered body layer. The first base layer 2a has an intermediate base layer surface s. In the first base layer 2a, the intermediate base layer surface s is the side opposite to the main surface 1s. The second base layer 2b is in contact with the first base layer 2a at the intermediate base layer surface s. The second base layer 2b is, for example, a copper plating formed by electroless plating. Thus, the base layer 2 is formed.

[0066] The distance Ha (thickness Ha of the first basal layer 2a) from the main surface 1s to the intermediate basal layer s in the first direction can also be less than 0.5 μm or less than 0.1 μm.

[0067] The substrate 2 may also exclude the first substrate 2a. Specifically, the substrate 2 may consist only of a second substrate 2b, which is composed of an electroless copper plating layer.

[0068] (Manufacturing method of substrate for printed wiring board)

[0069] The manufacturing method of the printed wiring board substrate 100b is described below.

[0070] Figure 6 This is a flowchart illustrating the manufacturing method of the substrate 100b for printed wiring boards. Figure 6 Corresponding to Figure 2 .like Figure 6 As shown, the manufacturing method of the printed wiring board substrate 100b includes: a step S1b of preparing a base film 1, a step S2b of forming a first base layer 2a, a step S3b of forming a second base layer 2b, and a step S4b of annealing the printed wiring board substrate 100b.

[0071] The process S2b of forming the first substrate layer 2a is performed after the process S1b of preparing the base film 1. The process S3b of forming the second substrate layer 2b is performed after the process S2b of forming the first substrate layer 2a. The process S4b of annealing the printed wiring board substrate 100b is performed after the process S3b of forming the second substrate layer 2b.

[0072] Figure 7 This is a cross-sectional view illustrating step S1b of preparing the base film 1. In step S1b of preparing the base film 1, as follows... Figure 7 As shown, a base film 1 is prepared. In the base film 1 prepared in step S1b, the substrate layer 2 is not disposed on the main surface 1s. Before the substrate layer 2 is disposed, the main surface 1s is subjected to alkali treatment and excimer treatment.

[0073] Figure 8 This is a cross-sectional view illustrating process S2b in forming the first substrate layer 2a. In process S2b in forming the first substrate layer 2a, as... Figure 8As shown, a first substrate layer 2a is formed on the main surface 1s. In this step S2b, firstly, a paste containing copper particles is applied to the main surface 1s. Secondly, the solvent contained in the applied paste is dried. Thirdly, the dried paste is fired. Thus, the copper particles contained in the dried paste sinter together to form the first substrate layer 2a. The paste containing copper particles can also be heat-treated using an intermittent hot blast furnace to form the first substrate layer 2a. When heat-treating the paste containing copper particles using an intermittent hot blast furnace, the paste is heat-treated at a firing temperature of 250°C or higher for 30 minutes or more. This promotes the sintering between the copper particles. As a result, when the electrolytic plating layer 3 is formed on the substrate layer 2, the growth rate of the copper plating is made uniform. When heat-treating the paste containing copper particles using an intermittent hot blast furnace, the paste is heat-treated at a firing temperature of 300°C or higher for 30 minutes or more. The first substrate layer 2a can also be formed by photo-firing a paste containing copper particles using a flash lamp. In the case of photo-firing a paste containing copper particles using a flash lamp, for example, the paste containing copper particles is irradiated with light for 500 μs using a flash lamp supplied with a voltage of 2.5 kV. As a result, the copper particles are instantaneously sintered. This suppresses the heat load on the main surface 1s compared to heat treatment using an intermittent hot blast furnace, and allows the copper particles to be sintered without reducing the effects obtained by alkaline treatment and excimer laser treatment performed on the main surface 1s. As a result, the growth rate of the copper plating can be made uniform when the electrolytic plating layer 3 is formed on the substrate layer 2. The first substrate layer 2a can also be formed by sputtering. Alternatively, the step S2b of forming the first substrate layer 2a can be omitted.

[0074] The process S3b of forming the second substrate layer 2b is performed using a plating apparatus 300. Figure 9 This is a schematic structural diagram of the plating apparatus 300 used in process S3b, which forms the second substrate layer 2b. Figure 9 As shown, the plating apparatus 300 includes a plating treatment tank 310, multiple rollers 320, electrode rollers 331 and 332, and a power supply 340.

[0075] A plating solution is stored in the plating treatment tank 310. The plating solution contains copper. Additionally, nickel may also be included in the plating solution. An electrode 311 is disposed inside the plating treatment tank 310. The electrode 311 is formed of a conductive material. For example, the electrode 311 is formed of titanium. The electrode 311 is immersed in the plating solution.

[0076] Multiple rollers 320 are positioned along the conveying direction of the base film 1 (see reference). Figure 9(Arrows in the diagram) are arranged. The base film 1 is conveyed along the conveying direction by rotating multiple rollers 320. During the conveying process, the base film 1 passes through the plating solution stored in the plating treatment tank 310.

[0077] Electrode rollers 331 and 332 are positioned to contact the base film 1 before it passes through the plating solution. At least one of electrode rollers 331 and 332 is in contact with the first substrate layer 2a. Electrode rollers 331 and 332 are, for example, made of stainless steel.

[0078] Power supply 340 is electrically connected to electrode 311, electrode roller 331, and electrode roller 332. More specifically, the positive terminal of power supply 340 is electrically connected to electrode 311, and the negative terminal of power supply 340 is electrically connected to electrode roller 331 and electrode roller 332.

[0079] Figure 10 This is a cross-sectional view illustrating process S3b in forming the second substrate layer 2b. In process S3b, energization is achieved between electrode 311 and electrode rollers 331 and 332 via power supply 340. Figure 10 As shown, driven by the electrical energy accompanying the energization, the second substrate layer 2b is rapidly formed on the surface of the first substrate layer 2a (intermediate substrate layer s). Thereafter, the energization between the electrode 311 and the electrode rollers 331 and 332 is stopped.

[0080] Next, a process S4b is performed to anneal the printed wiring board substrate 100b. Specifically, for example, the printed wiring board substrate 100b is annealed for 1 hour at an annealing temperature of 300°C in an inert gas atmosphere such as nitrogen. As a result, the substrate layer 2 is fixed to the base film 1. The oxygen concentration contained in the inert gas can be, for example, 50 ppm or less, or 10 ppm or less. This allows for a uniform crystalline state of the copper contained in the substrate layer 2.

[0081] Manufacturing through the above methods Figure 5 The printed wiring board substrate 100b with the structure shown is formed in the same way as the printed wiring board substrate 100a, with a base layer 2 that can improve the integrity of the structure in the laminate 20.

[0082] (Structure of printed wiring board)

[0083] The structure of the printed wiring board 200 will be described below. Figure 11 This is a cross-sectional view of the printed wiring board 200. (Example) Figure 11 As shown, the printed wiring board 200 includes a base film 1 and multiple laminated portions 20.

[0084] Let the direction perpendicular to the principal plane 1s be defined as the first direction X. Let the direction orthogonal to the first direction X be defined as the second direction Y. Let the direction orthogonal to both the first direction X and the second direction Y be defined as the third direction Z.

[0085] Multiple stacked portions 20 are disposed on the main surface 1s. The multiple stacked portions 20 are formed in a linear manner extending along the second direction Y. The multiple stacked portions 20 are disposed at equal intervals in the third direction Z. If the shortest distance S in the third direction Z between two adjacent stacked portions 20 and the width L of each of the multiple stacked portions 20 are less than 2 μm, then forming the resist pattern 4 in the step S5 of forming the resist pattern 4 described later will require a longer time. Therefore, as... Figure 11 As shown, the shortest distance S in the third direction Z between two adjacent stacked portions 20 can also be 2 μm or more. The width L of each of the multiple stacked portions 20 can also be 2 μm or more.

[0086] Specifically, the plurality of stacked portions 20 include adjacent first stacked portions 20a and second stacked portions 20b. The shortest distance S in the third direction Z from the first stacked portion 20a to the second stacked portion 20b can also be 2 μm or more. The shortest distance S in the third direction Z from the first stacked portion 20a to the second stacked portion 20b can be 15 μm or less, or 10 μm or less.

[0087] The width L of each of the multiple stacked portions 20 can be less than 15 μm or less than 10 μm. Specifically, the width L of each of the first stacked portion 20a and the second stacked portion 20b can be less than 15 μm or less than 10 μm.

[0088] The laminate 20 includes a substrate layer 2 and an electroplated coating layer 3. The substrate layer 2 is in contact with the main surface 1s. The electroplated coating layer 3 is in contact with the substrate layer 2. The electroplated coating layer 3 is a copper layer formed by electroplating.

[0089] (Manufacturing method of printed wiring board 200)

[0090] The manufacturing method of the printed wiring board 200 will be described below.

[0091] Figure 12 This is a flowchart illustrating the manufacturing method of the printed wiring board 200. The printed wiring board 200 is basically manufactured using a semi-additive method. Specifically, as... Figure 12 As shown, the manufacturing method of the printed wiring board 200 includes: step S5 of forming a resist pattern 4, step S6 of forming an electroplated coating 3, step S7 of removing the resist pattern 4, and step S8 of removing the substrate layer 2.

[0092] First, step S5, which forms the resist pattern 4, is performed. In step S5, the resist pattern 4 is formed on the substrate layer 2. Any method, such as photolithography, can be used to form the resist pattern 4. Step S6, which forms the electroplated coating layer 3, is performed after step S5, which forms the resist pattern 4. Step S7, which removes the resist pattern 4, is performed after step S6, which forms the electroplated coating layer 3. Step S8, which removes the substrate layer 2, is performed after step S7, which removes the resist pattern 4. The printed wiring board 200 is manufactured using the printed wiring board substrate 100a or the printed wiring board substrate 100b according to Embodiment 1.

[0093] Figure 13 This is a cross-sectional view illustrating step S5, which involves forming the resist pattern 4. In step S5, as... Figure 13 As shown, the resist pattern 4 is formed on the substrate layer 2.

[0094] The resist pattern 4 has an opening 4a. The opening 4a is the area where the resist pattern 4 is not formed. The substrate layer 2 is exposed from the opening 4a.

[0095] In step S5, which forms the resist pattern 4, firstly, a film-like resist is adhered to the substrate layer 2. Secondly, the resist disposed on the substrate layer 2 is exposed and developed. As a result, the remaining portion of the resist that was not removed becomes the resist pattern 4, and the portion of the resist that was removed becomes the opening 4a.

[0096] Figure 14 This is a cross-sectional view illustrating step S6 of forming the electroplated coating 3. In step S6 of forming the electroplated coating 3, as... Figure 14 As shown, an electroplated layer 3 is formed on the substrate layer 2 exposed from the opening 4a. The electroplated layer 3 is formed by passing an electric current through the substrate layer 2 in a plating solution containing copper.

[0097] Figure 15 This is a cross-sectional view illustrating step S7, which removes the resist pattern 4. In step S7, the process is as follows: Figure 15 As shown, the resist pattern 4 is removed from the substrate 2. As a result, the substrate 2 is exposed between two adjacent electroplated layers 3.

[0098] In step S8, which removes the substrate layer 2, the portion of the substrate layer 2 exposed between two adjacent electroplated layers 3 is removed by etching. Specifically, the substrate layer 2 is removed using a sulfuric acid-hydrogen peroxide etching solution. Since the structure of the substrate layer 2 and the structure of the electroplated layer 3 are not integrated, the etching rates in the stacked portion 20 are different. Even when the structure of the substrate layer 2 and the structure of the electroplated layer 3 are not integrated, etching is also performed on the side surface of the stacked portion 20 for 20 seconds until the substrate layer 2 is etched down to the main surface for 1 second. As a result, a stacked portion 20 with deteriorated rectangularity is formed. If the printed wiring board substrate 100 according to Embodiment 1 is used, the integrity of the structure in the stacked portion 20 is improved. Therefore, the etching rate of the stacked portion 20 in the first direction X becomes uniform, resulting in a stacked portion 20 with excellent rectangularity.

[0099] Through the above methods, Figure 11 The printed wiring board 200 with the structure shown is shown.

[0100] Figure 16 This is a cross-sectional view of the printed wiring board 200 showing the measurement area of ​​the crystal orientation distribution. The integrity of the structure in the stack 20, which consists of the substrate layer 2 and the electroplated coating layer 3, is evaluated by the proportion of the area occupied by the grains in the stack 20. As described later, the area occupied by the grains in the printed wiring board substrate 100 is measured by EBSD. Specifically, the stack 20 includes the substrate layer 2 and the electroplated coating layer 3. The substrate layer 2 is in contact with the main surface 1s. The electroplated coating layer 3 is in contact with the substrate layer 2. Figure 16 As shown, in the cross-section of the laminate 20, the first region V1 is the region from the main surface 1s to 4μm. The proportion of the area occupied by grains with an equivalent circle diameter of 3.0μm or more contained in the first region V1 is defined as the first area ratio r1. That is, the first area ratio r1 is the proportion of the area occupied by grains with an equivalent circle diameter of 3.0μm or more relative to the first region V1. In the printed wiring board 200 according to Embodiment 1, the first area ratio r1 is 0.8 or more. Thus, a printed wiring board 200 with improved integrity of the structure in the laminate 20 is obtained.

[0101] Comparison is also possible Figure 16 The first region V1 and the second region V2 are shown as the proportion of the area occupied by the grains in their respective stacked portions 20. The second region V2 is the region outside the first region V1 in the cross-section of the stacked portion 20. That is, the second region V2 is the region from the first surface 21s to the first region V1. The proportion of the area occupied by grains with an equivalent circle diameter of 3.0 μm or more contained in the second region V2 is defined as the second area ratio r2. That is, the second area ratio r2 is the proportion of the area occupied by grains with an equivalent circle diameter of 3.0 μm or more relative to the area occupied by the second region V2.

[0102] The first area ratio r1 can be more than 0.8 times or more than 1.0 times the second area ratio r2.

[0103] Figure 17 yes Figure 11 The diagram shows a schematic cross-sectional view of the laminate 20 in region XVII. Depending on the integrity of the organization within the laminate 20, the width of the laminate 20 may vary in the first direction X. The rectangularity of the laminate 20 is evaluated using a rectangularity evaluation index Et. Specifically, in a cross-section of the laminate 20 perpendicular to the second direction Y, the laminate 20 has a first surface 21s, a second surface 22s, a minimum surface 23s, a maximum surface 24s, and two side surfaces 20s. The first surface 21s is the surface of the laminate 20 furthest from the main surface 1s in the first direction X. The second surface 22s is the surface of the laminate 20 that contacts the main surface 1s. The two side surfaces 20s connect the first surface 21s and the second surface 22s. The minimum surface 23s and the maximum surface 24s may also be surfaces disposed between the first surface 21s and the second surface 22s. The minimum surface 23s and the maximum surface 24s may also be surfaces along the main surface 1s. The minimum surface 23s has a minimum width W3. The minimum width W3 is the smallest third-direction width in the Z-direction among the widths in the third direction of the stacked portion 20. Depending on the etching conditions, the first face 21s may become the minimum face 23s. The maximum face 24s has the maximum width W4. The maximum width W4 is the largest third-direction width in the Z-direction among the widths in the third direction of the stacked portion 20. Depending on the etching conditions, the second face 22s may become the maximum face 24s. In this case, if the rectangularity evaluation index is set to Et, then Et = W3 / W4.

[0104] The rectangularity evaluation index Et (the value obtained by dividing the minimum width W3 by the maximum width W4) needs to be 0.8 or higher. Specifically, the rectangularity evaluation index Et should be 0.8 or higher. The rectangularity evaluation index Et can also be 0.9 or higher. In this way, the rectangularity of the stacked portion 20 can be evaluated.

[0105] The rectangularity of the laminate 20 can also be evaluated from another perspective. Specifically, the rectangularity of the laminate 20 can be evaluated by either the amount of recess L1 or the amount of protrusion L2. When the structure of the base layer 2 and the electroplated coating layer 3 are not integrated, the shape of the side surface 20s of the laminate 20 can be an inwardly protruding V-shape. Specifically, at least one of the two side surfaces 20s can also include a first point p1 and a first recess p3a. The first point p1 is the point where the side surface 20s intersects with the first surface 21s. On the side surface 20s, viewed from the first point p1, the first recess p3a is located on the side where the first surface 21s is located in the third direction Z. The first recess p3a is located at the position with the longest distance from the first point p1 in the third direction Z. From a different viewpoint, the first recess p3a is located at the position where it overlaps with the first surface 21s when viewed from the first direction X in a top view. In this case, the amount of recess L1 is L1 = l1 / Ht. Distance l1 is the distance on the third direction Z from the first point p1 to the first concave point p3a.

[0106] The distance l1 along the third direction Z from the first point p1 to the first concave point p3a can be less than 0.15 times, less than 0.10 times, or less than 0.05 times the height Ht of the stacked portion 20 from the main surface 1s to the first surface 21s. Specifically, the concavity amount L1 is less than 0.15. The concavity amount L1 can be less than 0.10 or less than 0.05.

[0107] At least one of the two side surfaces 20s may also include a second point p2 and a second concave point p3b. The second point p2 is the point where side surface 20s intersects with the second surface 22s. On side surface 20s, viewed from the second point p2, the second concave point p3b is located on the side where the second surface 22s is located in the third direction Z. The second concave point p3b is located at the position with the longest distance from the second point p2 in the third direction Z. At this time, the protrusion amount L2 is L2 = l2 / Ht. The distance l2 is the distance from the second point p2 to the second concave point p3b in the third direction Z. In addition, the first concave point p3a is the point used to evaluate the concavity amount L1, and the second concave point p3b is the point used to evaluate the protrusion amount L2. Furthermore, when the shape of the laminate 20 is symmetrical, the first concave point p3a and the second concave point p3b in the two side surfaces 20s are arranged in a position that is linearly symmetrical about the central axis (axis of symmetry) of the laminate 20.

[0108] The distance l2 along the third direction Z from the second point p2 to the second concave point p3b can be less than 0.15 times, less than 0.10 times, or less than 0.05 times the height Ht of the stacked portion 20 from the main surface 1s to the first surface 21s. Specifically, the protrusion L2 is less than 0.15. The protrusion L2 can be less than 0.10 or less than 0.05.

[0109] (Effects)

[0110] The printed wiring board 200 according to this disclosure includes a base film 1 and a laminate 20. The base film 1 has a main surface 1s. The laminate 20 is disposed on the main surface 1s. When measuring the cross-section of the laminate 20 by electron backscatter diffraction under conditions where the grain boundary threshold is 10° or less, in a first region V1 from the main surface 1s to 4 μm, the proportion of the area occupied by grains with an equivalent circle diameter of 3 μm or more is set as a first area ratio r1. The first area ratio r1 is 0.8 or more.

[0111] In this way, a printed wiring board 200 with improved integrity of the organization in the stacked portion 20 and excellent rectangularity of the circuit can be obtained.

[0112] In the printed wiring board 200 described above, in the second region V2 other than the first region V1 in the cross-section of the laminate 20, the proportion of the area occupied by grains with an equivalent circular diameter of 3 μm or more is set as a second area ratio r2. The first area ratio r1 is 0.8 times or more of the second area ratio r2.

[0113] In this way, a printed wiring board 200 with improved integrity of the organization in the stacked portion 20 and excellent rectangularity of the circuit can be obtained.

[0114] In the printed wiring board 200 described above, the direction perpendicular to the main surface 1s is designated as the first direction X. The direction perpendicular to the first direction X is designated as the second direction Y. The direction perpendicular to both the first direction X and the second direction Y is designated as the third direction Z. The stacked portion 20 is formed in a linear manner extending along the second direction Y. The stacked portion 20 includes adjacent first stacked portions 20a and second stacked portions 20b. The width of each of the first stacked portion 20a and the second stacked portion 20b is 15 μm or less. The shortest distance S in the third direction Z from the first stacked portion 20a to the second stacked portion 20b is 15 μm or less.

[0115] Thus, a printed wiring board 200 with fine circuitry can be obtained.

[0116] In the printed wiring board 200 described above, the width of each of the first laminate 20a and the second laminate 20b is 10 μm or less. The shortest distance S in the third direction Z from the first laminate 20a to the second laminate 20b is 10 μm or less. The width of each of the first laminate 20a and the second laminate 20b may also be 6 μm or less. The shortest distance S in the third direction Z from the first laminate 20a to the second laminate 20b may also be 6 μm or less.

[0117] Thus, a printed wiring board 200 with fine circuitry can be obtained.

[0118] In the printed wiring board 200 described above, the width of both the first layer stack 20a and the second layer stack 20b is 2 μm or more. The shortest distance S in the third direction Z from the first layer stack 20a to the second layer stack 20b is 2 μm or more.

[0119] Thus, a printed wiring board 200 with fine circuitry can be obtained.

[0120] In the printed wiring board 200 described above, the laminate 20 includes a substrate layer 2 and an electroplated coating layer 3. The substrate layer 2 is in contact with the main surface 1s. The electroplated coating layer 3 is in contact with the substrate layer 2.

[0121] Thus, a printed wiring board 200 with fine circuitry can be obtained.

[0122] To verify the effectiveness of the printed wiring board substrate 100 as described above and the printed wiring board 200 manufactured from the printed wiring board substrate 100, the following measurements were performed.

[0123] (Sample preparation)

[0124] First, a printed wiring board substrate 500, whose base film 1 is made of polyimide, is prepared. The printed wiring board substrates 500 of samples 1 to 6 are comparative examples. The printed wiring board substrates 500 of samples 7 to 11 are exemplary examples. The manufacturing conditions and evaluation results of the printed wiring board substrates 500 shown in samples 1 to 11 are shown in Tables 1 to 4.

[0125]

[0126] In the printed wiring board substrate 500 of Sample 1, no alkaline treatment or excimer treatment is performed as a pretreatment. The base layer 2 of this printed wiring board substrate 500 is composed of a Ni-Cr seed layer and a sputtered copper layer as a first base layer 2a, and an electroless copper plating layer as a second base layer 2b. The thickness Ha of the first base layer 2a is 0.006 μm. The electroless copper plating layer as the second base layer 2b is formed with a thickness of 0.355 μm. The thickness H of the base layer 2 is 0.361 μm. Furthermore, the thickness of the second base layer 2b is obtained by subtracting the thickness Ha of the first base layer 2a from the thickness H of the base layer 2. After forming the electroless copper plating layer, no annealing is performed.

[0127] In the printed wiring board substrate 500 of sample 2, alkaline treatment and excimer laser treatment were performed as pretreatments. The base layer 2 of this printed wiring board substrate 500 is composed of a nano-copper sintered body layer as a first base layer 2a and an electroless copper plating layer as a second base layer 2b. The thickness Ha of the first base layer 2a is 0.034 μm. The electroless copper plating layer as the second base layer 2b is formed with a thickness of 0.225 μm. The thickness H of the base layer 2 is 0.259 μm. After the electroless copper plating layer is formed, annealing is not performed.

[0128] In the printed wiring board substrate 500 of sample 3, excimer laser treatment was performed as a pretreatment. The substrate 2 of this printed wiring board substrate 500 is composed of a nano-copper sintered body layer as a first substrate layer 2a and an electroless copper plating layer as a second substrate layer 2b. The thickness Ha of the first substrate layer 2a is 0.041 μm. The electroless copper plating layer as the second substrate layer 2b is formed with a thickness of 0.223 μm. The thickness H of the substrate layer 2 is 0.264 μm. After the electroless copper plating layer is formed, annealing is performed. Specifically, annealing is performed at a temperature of 300°C for 1 hour in an atmosphere of inert gas such as nitrogen.

[0129] In the printed wiring board substrate 500 of sample 4, only alkaline treatment was performed as a pretreatment. The base layer 2 of this printed wiring board substrate 500 is composed of a nano-copper sintered body layer as a first base layer 2a and an electroless copper plating layer as a second base layer 2b. The thickness Ha of the first base layer 2a is 0.026 μm. The electroless copper plating layer as the second base layer 2b is formed with a thickness of 0.185 μm. The thickness H of the base layer 2 is 0.211 μm. After the electroless copper plating layer is formed, annealing is performed. Specifically, annealing is performed at a temperature of 300°C for 1 hour in an atmosphere of inert gas such as nitrogen.

[0130] In the printed wiring board substrate 500 of sample 5, only excimer laser treatment was performed as a pretreatment. The base layer 2 of this printed wiring board substrate 500 is composed of an electroless copper plating layer. The thickness H of the base layer 2 is 1.150 μm. After the electroless copper plating layer is formed, annealing is performed. Specifically, annealing is carried out at a temperature of 300°C for 1 hour in an atmosphere of inert gas such as nitrogen.

[0131] In the printed wiring board substrate 500 of sample 6, alkaline treatment and excimer laser treatment were performed as pretreatments. The base layer 2 of this printed wiring board substrate 500 is composed of a nano-copper sintered body layer as a first base layer 2a and an electroless copper plating layer as a second base layer 2b. The thickness Ha of the first base layer 2a is 0.400 μm. The electroless copper plating layer as the second base layer 2b is formed with a thickness of 2.180 μm. The thickness H of the base layer 2 is 2.580 μm. After the electroless copper plating layer is formed, annealing is performed. Specifically, annealing is performed at a temperature of 300°C for 1 hour in an atmosphere of inert gas such as nitrogen.

[0132] In the printed wiring board substrate 500 of sample 7, alkaline treatment and excimer laser treatment were performed as pretreatments. The base layer 2 of the printed wiring board substrate 500 is composed of an electroless copper plating layer. The thickness H of the base layer 2 is 0.452 μm. After the electroless copper plating layer is formed, annealing is performed. Specifically, annealing is carried out at a temperature of 300°C for 1 hour in an atmosphere of inert gas such as nitrogen.

[0133] In the printed wiring board substrate 500 of sample 8, alkaline treatment and excimer laser treatment were performed as pretreatments. The base layer 2 of the printed wiring board substrate 500 is composed of a sputtered copper layer. The thickness H of the base layer 2 is 0.070 μm. After the base layer 2 is formed, no annealing is performed.

[0134] In the printed wiring board substrate 500 of sample 9, alkaline treatment and excimer treatment were performed as pretreatments. The base layer 2 of this printed wiring board substrate 500 is composed of a nano-copper sintered body layer. The thickness H of the base layer 2 is 0.155 μm. Since an electroless copper plating layer was not formed, annealing was not performed after the base layer 2 was formed.

[0135] In the printed wiring board substrate 500 of sample 10, alkaline treatment and excimer laser treatment were performed as pretreatments. The base layer 2 of this printed wiring board substrate 500 is composed of a nano-copper sintered body layer as a first base layer 2a and an electroless copper plating layer as a second base layer 2b. The thickness Ha of the first base layer 2a is 0.156 μm. The electroless copper plating layer as the second base layer 2b is formed with a thickness of 0.130 μm. The thickness H of the base layer 2 is 0.286 μm. After the electroless copper plating layer is formed, annealing is performed. Specifically, annealing is performed at a temperature of 300°C for 1 hour in an atmosphere of inert gas such as nitrogen.

[0136] In the printed wiring board substrate 500 of sample 11, alkaline treatment and excimer laser treatment were performed as pretreatments. The base layer 2 of this printed wiring board substrate 500 is composed of a nano-copper sintered body layer as a first base layer 2a and an electroless copper plating layer as a second base layer 2b. The thickness Ha of the first base layer 2a is 0.195 μm. The electroless copper plating layer as the second base layer 2b is formed with a thickness of 0.672 μm. The thickness H of the base layer 2 is 0.867 μm. After the electroless copper plating layer is formed, annealing is performed. Specifically, annealing is performed at a temperature of 300°C for 1 hour in an atmosphere of inert gas such as nitrogen.

[0137] By forming an electrolytic plating layer 3 on each of the samples 1 to 11 prepared in the manner described above, a sample with an electrolytic plating layer 3 is prepared. Figure 18 The printed wiring board substrate 500 of the stacked portion 20 shown.

[0138] <Evaluation of organizational integrity in layered sections>

[0139] The integrity of the structure in the laminate 20 was evaluated using printed wiring board substrate 500 of samples 1 to 11. Figure 18 This is a cross-sectional view of a printed wiring board substrate 500 with an electroplated coating layer 3, showing the measurement area of ​​the crystal orientation distribution. The integrity of the structure in the laminate 20 composed of the substrate layer 2 and the electroplated coating layer 3 is evaluated by the proportion of the area occupied by the grains in the laminate 20. The area occupied by the grains in the printed wiring board 200 is measured by EBSD.

[0140] Before measuring the area occupied by the die using EBSD, the printed wiring board substrate 500 with the electrolytically plated coating 3 is cross-sectionally processed by argon ion polishing. The accelerating voltage of the ion beam is set to, for example, 6 kV.

[0141] Next, the area occupied by the grains in the stack 20 was measured using EBSD. The area occupied by the grains was measured using a Germini 450 from ZEISS and a Symmetry from Oxford. The EBSD measurement conditions are as follows: accelerating voltage: 15 kV; electron beam irradiation current: 20 nA; electron beam accumulation time: 0.8 ms; SEM stage tilt angle: 70°; SEM working distance (WD): 15 mm.

[0142] When evaluating the integrity of the microstructure in the laminate 20, the grains of the evaluation target are measured by EBSD under conditions where the grain boundary threshold is 10° or less. Furthermore, the equivalent circle diameter of the grains of the evaluation target is set to 3.0 μm or more to ensure that no tiny grains are included in the evaluation target. Additionally, grains containing twin boundaries are excluded from the evaluation target.

[0143] The integrity of the structure within the laminate 20 is evaluated based on the area occupied by the grains contained in the laminate 20 within the first region V1. Specifically, the first region V1 is the region from the principal plane 1s to 4 μm. The proportion of the area occupied by grains with an equivalent circle diameter of 3.0 μm or more contained within the first region V1 is defined as a first area ratio r1. That is, the first area ratio r1 is the proportion of the area occupied by grains with an equivalent circle diameter of 3.0 μm or more relative to the area occupied by the first region V1.

[0144] When the first area ratio r1 is 0.95 or higher, the evaluation of the integrity of the tissue in the laminated portion 20 is recorded as A in Tables 1 to 4. When the first area ratio r1 is 0.80 or higher and less than 0.95, the evaluation of the integrity of the tissue in the laminated portion 20 is recorded as B in Tables 1 to 4. When the first area ratio r1 is 0.70 or higher and less than 0.80, the evaluation of the integrity of the tissue in the laminated portion 20 is recorded as C in Tables 1 to 4. When the first area ratio r1 is less than 0.70, the evaluation of the integrity of the tissue in the laminated portion 20 is recorded as D in Tables 1 to 4.

[0145] In sample 1, the first area ratio r1 is 0.650. In sample 2, the first area ratio r1 is 0.744. In sample 3, the first area ratio r1 is 0.795. In sample 4, the first area ratio r1 is 0.782. In sample 5, the first area ratio r1 is 0.759. In sample 6, the first area ratio r1 is 0.686.

[0146] In sample 7, the first area ratio r1 is 0.933. In sample 8, the first area ratio r1 is 0.836. In sample 9, the first area ratio r1 is 0.993. In sample 10, the first area ratio r1 is 0.981. In sample 11, the first area ratio r1 is 0.936.

[0147] Based on the first area ratio r1 of samples 1 to 11, as shown in Tables 1 to 4, the integrity of the tissue in the laminated portion 20 in samples 1 to 6 is evaluated as C or D. On the other hand, the integrity of the tissue in the laminated portion 20 in samples 7 to 11 is evaluated as A or B. In particular, the integrity of the tissue in the laminated portion 20 in samples 9 and 10 is evaluated as A.

[0148] That is, when no electroless copper plating layer is formed in the substrate layer 2, and alkaline treatment and excimer treatment are performed in the pretreatment, and the thickness H of the substrate layer 2 is within 1 μm, the integrity of the structure in the laminate 20 is improved. Alternatively, when the substrate layer 2 includes an electroless copper plating layer, and alkaline treatment and excimer treatment are performed in the pretreatment, and annealing is carried out under certain conditions after the formation of the electroless copper plating layer, and the thickness H of the substrate layer 2 is within 1 μm, the integrity of the structure in the laminate 20 is improved. In other words, the larger the first area ratio r1, the better the integrity of the structure in the laminate 20 is. As a result, the rectangularity of the laminate 20 in samples 7 to 11 is improved.

[0149] When no alkali treatment or excimer laser treatment is performed in the pretreatment, as in Sample 1, the integrity of the structure in the laminate 20 is evaluated as D. When only either alkali treatment or excimer laser treatment is performed in the pretreatment, as in Samples 3 and 4, the integrity of the structure in the laminate 20 is evaluated as C. When the substrate layer 2 includes an electroless copper plating layer, and the printed wiring board substrate 500 is not annealed after the electroless copper plating layer is formed, as in Sample 2, the integrity of the structure in the laminate 20 is evaluated as C. When the thickness H of the substrate layer 2 exceeds 1 μm, as in Samples 5 and 6, the integrity of the structure in the laminate 20 is evaluated as C or D.

[0150] Furthermore, when evaluating the integrity of the organization in the laminate 20 of the printed wiring board 200 with wiring formed as described later, the object area for performing the above-described measurements is... Figure 16 The first region V1 is shown.

[0151] The integrity of the structure in the laminate 20 can also be evaluated based on the ratio of the first area ratio r1 to the second area ratio r2. In the value obtained by dividing the first area ratio r1 by the second area ratio r2 (=r1 / r2), the first area ratio r1 can be more than 0.8 times or more than 1.0 times the second area ratio r2.

[0152] Figure 19 This refers to the grain distribution in the stacked portion 20 of sample 1. Figure 20 This refers to the grain distribution in the stacked portion 20 of sample 7. Figure 19 as well as Figure 20 The grain distribution shown represents the grain boundaries as measured by EBSD. For example... Figure 19 As shown, in sample 1, grain boundaries are concentrated near the substrate layer 2. On the other hand, as... Figure 20 As shown, in sample 7, the grain boundaries are not concentrated near the substrate layer 2.

[0153] <Evaluation of the Rectangularity of the Stacked Parts>

[0154] The rectangularity of the stacked portion 20 of the printed wiring board 200 manufactured using the printed wiring board substrate 500 of samples 1 to 11 was evaluated.

[0155] The rectangularity of the laminate 20 is evaluated using the rectangularity evaluation index Et. For example... Figure 17 As shown, the minimum face 23s and the maximum face 24s can also be faces disposed between the first face 21s and the second face 22s. The minimum face 23s has a minimum width W3. The minimum width W3 is the smallest width among the widths in the third direction Z of the stacked portion 20. The maximum face 24s has a maximum width W4. The maximum width W4 is the largest width among the widths in the third direction Z of the stacked portion 20. Depending on the etching conditions, the first face 21s becomes the minimum face 23s. Depending on the etching conditions, the second face 22s may become the maximum face 24s. In this case, if the rectangularity evaluation index is set to Et, then Et = W3 / W4.

[0156] When the rectangularity evaluation index Et is 0.9 or higher, the rectangularity evaluation of the laminate is A. When the rectangularity evaluation index Et is 0.8 or higher but less than 0.9, the rectangularity evaluation of the laminate is B. When the rectangularity evaluation index Et is 0.7 or higher but less than 0.8, the rectangularity evaluation of the laminate is C. When the rectangularity evaluation index Et is less than 0.7, the rectangularity evaluation of the laminate is D.

[0157] As shown in Tables 1 to 4, the rectangularity of the laminate 20 in samples 1 to 6 is rated as C or D. On the other hand, the rectangularity of the laminate 20 in samples 7 to 11 is rated as A or B. In particular, the rectangularity of the laminate 20 in samples 9 and 10 is rated as A. As will be described later, this has a significant impact on the integrity of the tissue within the laminate 20.

[0158] Figure 21 This refers to the grain distribution in the stacked portion 20 of sample 1. Figure 22 This refers to the grain distribution in the stacked portion 20 of sample 7. Figure 19 as well as Figure 20 The grain distribution shown represents the grain boundaries as measured by EBSD. For example... Figure 21 As shown, in sample 1, the width of the stacked portion 20 in the third direction Z is inconsistent in the first direction X. This is because the microstructure of the substrate layer 2 and the microstructure of the electroplated layer 3 are not integrated, resulting in different etching rates in the stacked portion 20. On the other hand, in sample 7, the microstructure of the substrate layer 2 and the microstructure of the electroplated layer 3 are integrated, thus the substrate layer 2 and the electroplated layer 3 are etched uniformly, improving the rectangularity of the stacked portion 20. Therefore, as... Figure 22As shown, the width of the stacked portion 20 is substantially uniform in the first direction X.

[0159] <Evaluation of the fine line formation properties of the layered portion>

[0160] The fine line formation properties of the laminate 20 of the printed wiring board 200 manufactured using the printed wiring board substrate 500 of samples 1 to 11 were evaluated.

[0161] Evaluation TEG was used in the evaluation of the fine line formation of the laminate 20. Figure 23 This is a top-down view of the TEG (Transformer for Geometry and Geometry) used for evaluation. For example... Figure 23 As shown, the evaluation TEG has a base film 1 and multiple laminated portions 20. In the evaluation TEG, the main surface 1s has 20 wiring forming regions R1, 20 wiring forming regions R2, and 20 wiring forming regions R3. The 20 wiring forming regions R1, R2, and R3 are arranged in a row along the left-right direction.

[0162] Multiple stacked portions 20 are formed in wiring forming regions R1, R2, and R3. The stacked portion 20 formed in wiring forming region R1 extends along the vertical direction (…). Figure 23 The second direction (Y) extends. The laminate 20 formed on the wiring forming region R2 and the laminate 20 formed on the wiring forming region R3 extend in directions inclined at 45° and -45° respectively relative to the vertical direction.

[0163] The L / S ratio of the stacked portion 20 formed on the nth wiring forming region R1 from the right (n is a natural number less than 20) is nμm / 100μm. L is the width of each of the stacked portions 20. S is the shortest distance between two adjacent stacked portions 20. The L / S ratio of the stacked portions 20 formed on the wiring forming region R2 and the stacked portions 20 formed on the wiring forming region R3 is also nμm / 100μm, just like the L / S ratio of the stacked portion 20 formed on the wiring forming region R1. In addition, the aspect ratio of the stacked portion 20 (the value obtained by dividing the height Ht of the stacked portion 20 by the width L of the stacked portion 20) is 1 or more and 2 or less.

[0164] For each of the 20 wiring formation regions R1, each of the 20 wiring formation regions R2, and each of the 20 wiring formation regions R3, the stack 20 was observed using SEM (Scanning Electron Microscope) to determine whether fine wire formation had been performed appropriately.

[0165] In Tables 1 to 4, if the minimum width L of the stackable portion 20 that can be appropriately formed is 6 μm or less, the evaluation is A. If the minimum width L of the stackable portion 20 that can be appropriately formed is more than 6 μm but less than 10 μm, the evaluation is B. If the minimum width L of the stackable portion 20 that can be appropriately formed is more than 10 μm but less than 15 μm, the evaluation is C. If the minimum width L of the stackable portion 20 that can be appropriately formed is more than 15 μm, the evaluation is D.

[0166] As shown in Tables 1 to 4, the fine line formation performance of the laminate 20 in samples 5 and 6 is rated as C or D. On the other hand, the fine line formation performance of the laminate 20 in samples 1 to 4 and samples 7 to 11 is rated as A or B. Based on these results, it can be concluded that the thickness H of the substrate layer 2 has a significant impact on the fine line formation performance of the laminate 20. In samples 5 and 6, the thickness H of the substrate layer 2 exceeds 1 μm. On the other hand, in samples 1 to 4 and samples 7 to 11, the thickness H of the substrate layer 2 is less than 1 μm, therefore the fine line formation performance of the laminate 20 is good.

[0167] <Overall Evaluation>

[0168] As can be seen from the above, by improving the integrity of the structure in the stacked portion 20 of the printed wiring board, the rectangularity of the stacked portion 20 is improved. Furthermore, by improving the fine line formation properties of the stacked portion 20, a printed wiring board 200 with fine circuitry is obtained. In particular, the printed wiring board 200 manufactured using the printed wiring board substrates of samples 9 and 10 exhibits good rectangularity and fine line formation properties in the stacked portion 20.

[0169] The embodiments disclosed herein are illustrative in all respects and should not be considered restrictive. The essential scope of this disclosure is not defined by the above embodiments but by the claims, and is intended to include all modifications equivalent to and within the scope of the claims.

[0170] Explanation of reference numerals in the attached figures

[0171] 1: Base film, 1s: Main surface, 2: Base layer, 2a: First base layer, 2b: Second base layer, 2s: Base layer, 3: Electrolytic plating layer, 4: Resist pattern, 4a: Opening, 20: Stacked portion, 20a: First stacked portion, 20b: Second stacked portion, 20s: Side surface, 21s: First surface, 22s: Second surface, 23s: Minimum surface, 24s: Maximum surface, 100, 100a, 100b, 500: Substrate for printed wiring board, 200: Printed wiring board, 300: Plating apparatus, 310: Plating treatment tank, 311: Electrode, 320: Roller, 331, 3 32: Electrode roller, 340: Power supply, r1: First area ratio, r2: Second area ratio, Et: Rectangularity evaluation index, H, Ha, l1, l2: Distance, H, Ha: Thickness, Ht: Height, L: Width, L1: Depression amount, L2: Protrusion amount, R1, R2, R3: Wiring formation area, S: Shortest distance, V1: First region, V2: Second region, W3: Minimum width, W4: Maximum width, X: First direction, Y: Second direction, Z: Third direction, p1: First point, p2: Second point, p3a: First depression, p3b: Second depression, s: Intermediate base layer.

Claims

1. A printed wiring board, comprising: Base film, having a main surface; and The laminated portion is disposed on the main surface. When the cross-section of the laminated portion is determined by electron backscatter diffraction under conditions where the grain boundary threshold is below 10°, In the first region extending from the main surface to 4 μm, if the proportion of the area occupied by grains with an equivalent circle diameter of 3 μm or more is defined as the first area ratio, Then the first area ratio is 0.8 or higher.

2. The printed wiring board according to claim 1, wherein, In the second region outside the first region of the cross-section of the laminated portion, if the proportion of the area occupied by grains with an equivalent circular diameter of 3 μm or more is set as the second area ratio, Then the first area ratio is more than 0.8 times the second area ratio.

3. The printed wiring board according to claim 1 or 2, wherein, The direction perpendicular to the main surface is defined as the first direction. Define the direction perpendicular to the first direction as the second direction. When the direction perpendicular to the first direction and the second direction is set as the third direction... The stacked portion is formed in a linear manner extending along the second direction, and thus... The stacked portion includes adjacent first stacked portions and second stacked portions. The width of both the first and second stacked portions is less than 15 μm. The shortest distance in the third direction from the first stack to the second stack is less than 15 μm.

4. The printed wiring board according to claim 3, wherein, The width of both the first and second stacked portions is less than 10 μm. The shortest distance in the third direction from the first stack to the second stack is less than 10 μm.

5. The printed wiring board according to claim 3 or 4, wherein, The width of both the first and second stacked portions is 2 μm or more. The shortest distance in the third direction from the first stack to the second stack is 2 μm or more.

6. The printed wiring board according to any one of claims 1 to 5, wherein, The laminated portion includes a base layer in contact with the main surface and an electroplated coating layer in contact with the base layer.

Citation Information

Patent Citations

  • Printed-wiring board base material and method of manufacturing printed-wiring board base material

    WO2019208077A1