Sealing material for photoelectric conversion element, dam material, filling material, method for manufacturing device using dam material, and method for manufacturing device using filling material

By controlling the contact angle and viscosity of the sealing material, and combining cationic polymeric compounds and inorganic fillers, the adhesion and wetting spread problems of the sealing material for photoelectric conversion elements in the dam filling method were solved, thereby improving the reliability and shape accuracy of the device.

CN123147277APending Publication Date: 2026-11-20DENKA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202580028668.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-19
Filing Date
2025-04-09
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing sealing materials for photoelectric conversion elements suffer from problems such as insufficient adhesion between the dam material and the substrate, unstable discharge volume, and insufficient wetting and spreading of the filling material in the dam filling method, which affect the reliability of the device.

Method used

By controlling the contact angle and viscosity of the sealing material over time, a sealing material containing cationic polymerizable compounds, photocationic polymerization initiators, and sensitizers is designed to ensure stable shape and adhesion under specific conditions. Inorganic fillers are used to improve the strength of the dam material.

Benefits of technology

It improves the reliability and sealing of the photoelectric conversion element device, reduces uneven dispensing and bubble generation, and ensures shape and position accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123147277A_ABST
    Figure CN123147277A_ABST
Patent Text Reader

Abstract

The sealing material for a photoelectric conversion element for a dam-filling method of the present invention contains (A) a cationically polymerizable compound, (B) a photocationic polymerization initiator, and (C) a sensitizer, and the contact angle θa after 15 seconds of liquid application is 35° or more and 90° or less in the contact angle over time measured by a prescribed step i.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a sealing material, a dam material, a filler material, a method for manufacturing a device using a dam material, and a method for manufacturing a device using a filler material for a photoelectric conversion element. More specifically, it relates to a sealing material, a dam material, a filler material, a device comprising a photoelectric conversion element, a method for manufacturing a device using a dam material, and a method for manufacturing a device using a filler material. Background Technology

[0002] In the past, photoelectric conversion elements used in displays such as liquid crystal displays, organic electroluminescent displays, and electronic paper, or in silicon solar cells, dye-sensitized solar cells, and organic thin-film solar cells, were sealed with sealing materials that have water vapor barrier properties.

[0003] Organic light-emitting diodes (OLEDs) have attracted attention as devices capable of emitting high-brightness light. However, OLEDs are known to be susceptible to moisture, and their light-emitting properties can be reduced by moisture or impurities penetrating into the OLED.

[0004] On the other hand, as one sealing method, the dam and fill method is known. In the dam and fill method, firstly, a first curing adhesive is applied to the substrate using a dispenser to form a ring-shaped dam (dam) to surround the photoelectric conversion element, and then a second curing adhesive is filled inside the dam. Next, the photoelectric conversion element is embedded in the second curing adhesive inside the dam, and a transparent panel is placed on the dam to cover it, allowing the second curing adhesive to cure, thereby bonding the transparent panel to the substrate.

[0005] As a sealing material used in this type of dam filling method, for example, a thermosetting liquid composition for sealing organic light-emitting elements is disclosed in Patent Document 1 (Japanese Patent Application Publication No. 2023-024361), which includes: an adhesive substance comprising an aliphatic tetrafunctional epoxy compound; and a cationic initiator.

[0006] Furthermore, for example, in Patent Document 2 (International Publication No. 2017 / 099055), from the perspective of sealing without directly exposing the organic EL element to UV, a sealing composition comprising at least one compound selected from N-glycidyl compounds, N-vinyl compounds and N-allyl compounds (excluding N-glycidyl isocyanurate) is disclosed as a dam material.

[0007] Furthermore, for example, in Patent Document 3 (International Publication No. 2017 / 094809), from the viewpoint of sealing without directly exposing the organic EL element to UV, a sealing composition comprising a glycol urea compound that is weakly basic to the cation generated by the photocationic polymerization initiator is disclosed as a filler material.

[0008] Existing technical documents

[0009] Patent documents

[0010] Patent Document 1: Japanese Patent Application Publication No. 2023-024361

[0011] Patent Document 2: International Publication No. 2017 / 099055

[0012] Patent Document 3: International Publication No. 2017 / 094809 Summary of the Invention

[0013] However, when using conventional sealing materials and sealing photoelectric conversion elements by damming, there is room for improvement in the reliability of the sealing materials in order to maintain the function of the photoelectric conversion elements.

[0014] More specifically, there are sometimes cases where the adhesion between the dam material and the substrate is insufficient, or when the dam material is applied using a dispenser, the amount dispensed is unstable, making it difficult to form the dam of the desired shape.

[0015] Furthermore, more specifically, due to insufficient wetting and spreading properties of the filler material, the adhesion between the filler material and the substrate or the filling properties of the filler material into the dam frame are sometimes insufficient.

[0016] The inventors, through in-depth research aimed at improving the reliability of sealing materials, discovered that a seal with a desired shape can be obtained by controlling the contact angle of the sealing material over time. Furthermore, further research led to the design of a new index related to the contact angle, and it was found that sealing materials meeting this index can improve reliability, thus completing this invention.

[0017] According to the present invention, the following sealing materials and related technologies are provided.

[0018] 1. A sealing material for a photoelectric conversion element, used in a dam filling method, wherein the sealing material for the photoelectric conversion element comprises:

[0019] (A) cationic polymerizable compounds, (B) photocationic polymerization initiators, and (C) sensitizers.

[0020] In the contact angle measured over time by the following step i, the contact angle θa after 15 seconds of contact with the liquid is greater than 35° and less than 90°.

[0021] (Step i) Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the sealing material for the photoelectric conversion element into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass.

[0022] (Condition ii)

[0023] • Measurement method: Changes over time

[0024] • Control method: Standard

[0025] • Analytical methods and techniques: droplet method, θ / 2 method

[0026] • Field of view: Wide angle 2

[0027] • Droplet volume: 5 μl

[0028] 2. The sealing material for the photoelectric conversion element according to 1, wherein,

[0029] In the contact angle measured through step i, the contact angle θb after 120 seconds of contact with the liquid is greater than 12° and less than 32°.

[0030] 3. The sealing material for the photoelectric conversion element according to 2, wherein,

[0031] The contact angle θa is greater than 1.5 and less than 5.0 relative to the contact angle θb (θa / θb).

[0032] 4. The sealing material for the photoelectric conversion element according to any one of 1 to 3, wherein,

[0033] The photoelectric conversion element was sealed with 0.5 ml of material and a CPA-52Z conical plate was used. The viscosity measured at 25°C and 25 rpm was above 2000 mPa·s and below 50000 mPa·s.

[0034] 5. The sealing material for the photoelectric conversion element according to any one of 1 to 4, further comprising (D) a phosphoric acid compound.

[0035] 6. The sealing material for the photoelectric conversion element according to any one of 1 to 5, wherein,

[0036] (A) The cationic polymerizable compound contains one or more of the following: (A-1) alicyclic compounds having an epoxy group, (A-2) aromatic compounds having an epoxy group, and (A-3) glycidyl ether compounds and their derivatives.

[0037] 7. The sealing material for the photoelectric conversion element according to any one of 1 to 6, further comprising a stabilizer.

[0038] 8. A dam material comprising a sealing material for a photoelectric conversion element as described in any one of 1 to 7, and (E) an inorganic filler.

[0039] 9. According to the dam material described in 8, wherein,

[0040] (E) The content of inorganic filler is 20 to 300 parts by mass relative to 100 parts by mass of (A) cationic polymeric compound.

[0041] 10. The dam material according to 8 or 9, wherein,

[0042] The dam material was set to 0.5 ml, and the viscosity measured using a CPA-52Z conical plate at 25°C and 0.7 rpm was above 100,000 mPa·s and below 1,200,000 mPa·s.

[0043] 11. A solidified body, which is a solidified form of the dam material described in any one of 8 to 10.

[0044] 12. An apparatus comprising a photoelectric conversion element sealed with the dam material described in any one of 8 to 10.

[0045] 13. The apparatus according to 12, wherein,

[0046] The photoelectric conversion element is an organic electroluminescent element.

[0047] 14. A method for manufacturing an apparatus, comprising:

[0048] The process of attaching the filling material and the dam material surrounding the filling material to the first component;

[0049] The process of embedding the photoelectric conversion element into the filler material;

[0050] The process of configuring the second component in a manner that covers the filling material and the dam material; and

[0051] The process of curing the filler material by bonding the first component and the second component together.

[0052] The dam material is any one of the dam materials described in 8 to 10.

[0053] 15. A sealing material for a photoelectric conversion element, used in a dam filling method, the sealing material for the photoelectric conversion element comprising:

[0054] (A) cationic polymerizable compounds and (B) photocationic polymerization initiators,

[0055] In the contact angle measured over time by the following step i, the contact angle θc after 5 seconds of contact with the liquid is less than 30°.

[0056] (Step i) Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the sealing material for the photoelectric conversion element into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass.

[0057] (Condition ii)

[0058] • Measurement method: Changes over time

[0059] • Control method: Standard

[0060] • Analytical methods and techniques: droplet method, θ / 2 method

[0061] • Field of view: Wide angle 2

[0062] • Droplet volume: 5 μl

[0063] 16. The sealing material for the photoelectric conversion element according to 15, wherein,

[0064] In the contact angle measured through step i, the contact angle θd after 30 seconds of contact with the liquid is less than 20°.

[0065] 17. The sealing material for the photoelectric conversion element according to 15, wherein,

[0066] The contact angle θc is greater than or equal to 1.0 and less than or equal to 2.3 relative to the contact angle θd (θc / θd).

[0067] 18. The sealing material for the photoelectric conversion element according to any one of 15 to 17, wherein,

[0068] The photoelectric conversion element was sealed with 0.5 ml of material and a CPA-40Z conical plate was used. The viscosity measured at 25°C and 50 rpm was above 50 mPa·s and below 1000 mPa·s.

[0069] 19. The sealing material for a photoelectric conversion element according to any one of 15 to 18, further comprising at least one of (C2) a reactive diluent, (D) a phosphoric acid compound and (F) a stabilizer.

[0070] 20. The sealing material for the photoelectric conversion element according to any one of 15 to 19, wherein,

[0071] (A) The cationic polymerizable compound contains one or more of the following: (A-1) alicyclic compounds having an epoxy group, (A-2) aromatic compounds having an epoxy group, and (A-3) glycidyl ether compounds and their derivatives.

[0072] 21. The sealing material for the photoelectric conversion element according to any one of 15 to 20, wherein it is used as a filler material.

[0073] 22. A cured body, which is a cured body of the sealing material for the photoelectric conversion element according to any one of 15 to 21.

[0074] 23. An apparatus comprising a photoelectric conversion element sealed with a sealing material according to any one of 15 to 20.

[0075] 24. The apparatus according to 23, wherein,

[0076] The photoelectric conversion element is an organic electroluminescent element.

[0077] 25. A method for manufacturing an apparatus, comprising:

[0078] The process of attaching the filling material and the dam material surrounding the filling material to the first component;

[0079] The process of embedding the photoelectric conversion element into the filler material;

[0080] The process of configuring the second component in a manner that covers the filling material and the dam material; and

[0081] The process of curing the filler material by bonding the first component and the second component together.

[0082] The filling material is any one of the sealing materials for photoelectric conversion elements described in 15 to 20.

[0083] 26. A polymerizable composition, wherein,

[0084] In the contact angle measured over time by following step i, the contact angle θa after 15 seconds of contact with the liquid is greater than 35° and less than 90°.

[0085] (Step i) Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the polymeric composition into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet onto the prepared alkali-free glass.

[0086] (Condition ii)

[0087] • Measurement method: Changes over time

[0088] • Control method: Standard

[0089] • Analytical methods and techniques: droplet method, θ / 2 method

[0090] • Field of view: Wide angle 2

[0091] • Droplet volume: 5 μl

[0092] 27. A polymerizable composition, wherein,

[0093] In the contact angle measured by following step i, the contact angle θc after 5 seconds of contact with the liquid is less than 30°.

[0094] (Step i) Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the polymeric composition into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet onto the prepared alkali-free glass.

[0095] (Condition ii)

[0096] • Measurement method: Changes over time

[0097] • Control method: Standard

[0098] • Analytical methods and techniques: droplet method, θ / 2 method

[0099] • Field of view: Wide angle 2

[0100] • Droplet volume: 5 μl

[0101] According to the present invention, a technique is provided that can improve the reliability of devices using sealing materials. Attached Figure Description

[0102] Figure 1 This is a schematic cross-sectional view showing an example of the apparatus of this embodiment.

[0103] Figure 2 This is a diagram showing the positional relationship between the filling material and the dam material in a top view of the device of this embodiment.

[0104] Figure 3 This is a schematic diagram illustrating an example of a method for manufacturing the apparatus according to this embodiment. Detailed Implementation

[0105] In this specification, unless otherwise specified, the designation "a~b" in the description of numerical ranges indicates a or more and b or less. For example, "1~5 mass%" means "more than 1 mass% and less than 5 mass%". Furthermore, the lower and upper limits of the numerical ranges can be arbitrarily combined with the lower and upper limits of other numerical ranges.

[0106] Unless otherwise specified, each ingredient and material listed in this instruction manual may be used individually or in combination with two or more.

[0107] The embodiments of the present invention will now be described using the accompanying drawings. When multiple identical constituent elements exist on the same drawing, sometimes only one label is used instead of all labels. All drawings are for illustrative purposes only. The shapes or dimensions of the components in the drawings may not necessarily correspond to actual objects.

[0108] The damming method is a sealing technology used in electronic components, etc., and involves the combined use of dam materials and filler materials. The dam material is a material with higher viscosity and shape retention than the filler material, used to form the wall (dam). The filler material is a material with higher flowability than the dam material, used to fill the area surrounded by the dam material. By partially or completely curing the dam material and filler material, a sealing structure can be achieved.

[0109] <Sealing materials for photoelectric conversion elements>

[0110] The following describes examples of preferred methods for sealing materials used in photoelectric conversion elements.

[0111] This embodiment is a composition. The composition is preferably a polymerizable composition. The polymerizable composition preferably contains a polymerizable compound and a polymerization initiator. The polymerizable compound is preferably (A) a cationic polymerizable compound. The polymerization initiator is preferably a photopolymerization initiator or a cationic polymerization initiator, more preferably (B) a photocationic polymerization initiator. The composition is preferably a sealing material for photoelectric conversion elements.

[0112] 1. First Implementation Method

[0113] The sealing material for the photoelectric conversion element in this embodiment is used in the dam filling method and includes (A) a cationic polymerizable compound, (B) a photocationic polymerization initiator and (C) a sensitizer. In the contact angle measured over time by step i, the contact angle θa after 15 seconds of liquid contact is 35° or more and 90° or less.

[0114] (Step i) Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the sealing material for the photoelectric conversion element into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass.

[0115] (Condition ii)

[0116] • Measurement method: Changes over time

[0117] • Control method: Standard

[0118] • Analytical methods and techniques: droplet method, θ / 2 method

[0119] • Field of view: Wide angle 2

[0120] • Droplet volume: 5 μl

[0121] By setting the contact angle θa after 15 seconds of contact with the liquid within the aforementioned range, the shape and positional accuracy of the sealing material for the photoelectric conversion element can be improved, and a seal with the desired shape can be obtained. As a result, the reliability of the device using the sealing material for the photoelectric conversion element of this embodiment can be improved.

[0122] Although the details of the reason are not yet clear, it is speculated to be as follows.

[0123] First, when the sealing material for the photoelectric conversion element is applied using a dispenser, it is sprayed from the tip of the nozzle, adheres to the substrate (first component), and is configured into the desired shape. At this time, the sealing material for the photoelectric conversion element in contact with the substrate does not completely wet but gradually stabilizes its shape and adheres. Therefore, it is believed that by controlling the contact angle when the sealing material for the photoelectric conversion element contacts the substrate and stabilizes its shape, the configuration or shape of the sealing material for the photoelectric conversion element can be controlled with higher precision. Furthermore, it is speculated that when a dam is formed using the sealing material for the photoelectric conversion element, the dam can be manufactured according to the design, and as the dam material, it can block the outflow of the internal filling material, thereby achieving uniformity and improving the reliability of the device using the photoelectric conversion element.

[0124] [Contact Angle]

[0125] The contact angle θa after 15 seconds of contact with the liquid is 35° or more, preferably 38° or more, and more preferably 40° or more. This reduces uneven dispensing during dispensing, suppresses the generation of ripples and bubbles, and also improves reliability.

[0126] On the other hand, the contact angle θa after 15 seconds of contact with the liquid is 90° or less, preferably 85° or less, and more preferably 70° or less. This reduces uneven dispensing during ejection, suppresses the generation of ripples and bubbles, and also improves reliability. Furthermore, from the viewpoint of achieving even higher reliability, θa is further preferably 55° or less.

[0127] Furthermore, in the contact angle measured in step i, the contact angle θb after 120 seconds of liquid contact is preferably 12° or more and 32° or less. It is believed that after 120 seconds of liquid contact, the sprayed photoelectric conversion element is wetted and diffused to a certain extent by the sealing material, and its shape is roughly stable. Therefore, by controlling the contact angle θb after 120 seconds of liquid contact, a more stable dam width can be obtained.

[0128] Furthermore, the contact angle θa (°) relative to the contact angle θb (°) (θa / θb) is preferably 1.3 or more, and more preferably 1.4 or more.

[0129] On the other hand, the contact angle θa (°) relative to the contact angle θb (°) (θa / θb) is preferably 3.0 or less, more preferably 2.6 or less, and even more preferably 2.2 or less.

[0130] The sealing material for photoelectric conversion elements that meets the above-mentioned contact angle can be achieved by selecting the types of components constituting the sealing material and adjusting the dosage. Specifically, from the viewpoint of obtaining wettability, for example, an alicyclic compound having an epoxy group (A-1) or a phosphoric acid compound and a stabilizer (D) can be used. Furthermore, from the viewpoint of ensuring the desired physical properties of the sealing material for photoelectric conversion elements, a method of combining an aromatic compound having an epoxy group (A-2) and a glycidyl ether compound (A-3) with an alicyclic compound having an epoxy group (A-1) can also be cited.

[0131] [Viscosity]

[0132] Furthermore, the viscosity of the photoelectric conversion element is preferably 2000 mPa·s or more, more preferably 3000 mPa·s or more, and even more preferably 3500 mPa·s or more, when the sealing material for the photoelectric conversion element is set to 0.5 ml and a conical plate CPA-52Z is ​​used, and measured at 25°C and 25 rpm.

[0133] On the other hand, the viscosity of the sealing material for the photoelectric conversion element is preferably 50,000 mPa·s or less, more preferably 40,000 mPa·s or less, and even more preferably 30,000 mPa·s or less.

[0134] By setting the viscosity of the sealing material for the photoelectric conversion element within the aforementioned range, uneven dispensing during dispensing can be reduced, and the generation of ripples and bubbles can be suppressed.

[0135] Furthermore, ripples refer to phenomena caused by the inability to uniformly coat the sealing material for photoelectric conversion elements into a linear pattern, the inability of the sealing material to diffuse evenly resulting in decreased fluidity, or the excessive viscosity of the sealing material preventing uniform expulsion. Additionally, bubbles refer to air bubbles contained in the sealing material that do not detach after coating, or air bubbles that arise due to poor wetting of the substrate surface after coating.

[0136] The following describes the composition of the sealing material used in photoelectric conversion elements.

[0137] (A) Cationic polymeric compounds

[0138] The sealing material for the photoelectric conversion element in this embodiment requires (A) a cationic polymeric compound as an essential component. (A) The cationic polymeric compound is preferably photopolymeric.

[0139] (A) The cationic polymerizable compound contains one or more of the following: (A-1) alicyclic compounds with epoxy groups, (A-2) aromatic compounds with epoxy groups, and (A-3) glycidyl ether compounds and their derivatives. This results in good coatability, adhesion, and low moisture permeability.

[0140] Furthermore, (A) the cationic polymerizable compound may have one or more halogen elements, for example, it may have one or more elements selected from the group consisting of fluorine and bromine.

[0141] (A-1) Alicyclic compounds with epoxy groups

[0142] Examples of alicyclic compounds having an epoxy group (hereinafter also referred to as alicyclic epoxy compounds) include compounds or their derivatives obtained by epoxidation of compounds having at least one cycloalkane ring (e.g., cyclohexene ring, cyclopentene ring, pinene ring, etc.) with a suitable oxidizing agent such as hydrogen peroxide or peroxide, and hydrogenated epoxy compounds obtained by hydrogenating aromatic epoxy compounds (e.g., bisphenol A type epoxy resin, bisphenol F type epoxy resin, etc.). One or more of these compounds may be used.

[0143] Examples of alicyclic epoxy compounds include 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate, 3,4-epoxycyclohexylalkyl (meth)acrylates (e.g., 3,4-epoxycyclohexylmethyl (meth)acrylate), (3,3',4,4'-diepoxy)biscyclohexyl, hydrogenated bisphenol A type epoxy resin, and hydrogenated bisphenol F type epoxy resin.

[0144] Among alicyclic epoxides, alicyclic epoxides having a 1,2-epoxycyclohexane structure are preferred. Among alicyclic epoxides having a 1,2-epoxycyclohexane structure, compounds represented by the following formula (A1-1) are preferred.

[0145] [Chemical Formula 1]

[0146]

[0147] In formula (A1-1), X represents a single bond or a linking group (a divalent group with more than one atom), and the linking group is a divalent hydrocarbon group, carbonyl group, ether bond, ester bond, carbonate group, amide bond, or a group in which multiple of them are linked.

[0148] Preferably, X is a linking group. Among the linking groups, functional groups having ester bonds are preferred. Among these, 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate is preferred.

[0149] From the viewpoint of moisture permeability or storage stability, the molecular weight of the alicyclic epoxy compound is preferably 450 or less, more preferably 400 or less, further preferably less than 300, and even more preferably 100 to 280.

[0150] When alicyclic epoxide has a molecular weight distribution, it is preferable that the number average molecular weight of the alicyclic epoxide is within the above-mentioned range. Furthermore, in this specification, the number average molecular weight represents the value converted from polystyrene as measured by gel permeation chromatography (GPC).

[0151] (A-2) Aromatic compounds with epoxide groups

[0152] As an aromatic compound having an epoxy group (hereinafter also referred to as an aromatic epoxy compound), any of monomers, oligomers or polymers can be used, and examples include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, fluorene type epoxy resin, phenolic varnish type epoxy resin, cresol phenolic varnish type epoxy resin, and their modified forms.

[0153] Furthermore, it can be a multifunctional epoxy resin having two or more epoxy groups. Examples of epoxy resins having two or more (especially two) epoxy groups include bisphenol A type multifunctional epoxy resin, bisphenol F type multifunctional epoxy resin, bisphenol AF type multifunctional epoxy resin, hydrogenated bisphenol A type multifunctional epoxy resin, and biphenyl type multifunctional epoxy resin.

[0154] Furthermore, examples of epoxy resins having three or more epoxy groups include naphthalene-type multifunctional epoxy resins, phenolic varnish-type multifunctional epoxy resins, cresolic varnish-type multifunctional epoxy resins, dicyclopentadiene-type multifunctional epoxy resins, epoxypropylamine-type multifunctional epoxy resins, epoxypropyl ester-type multifunctional epoxy resins, rubber-modified multifunctional epoxy resins, chelated modified multifunctional epoxy resins, multifunctional alicyclic epoxy resins, and multifunctional epoxidized polybutadiene.

[0155] These epoxy resins can be selected from one or more types.

[0156] Among these, aromatic epoxy compounds having a bisphenol structure are preferred. Of these aromatic epoxy compounds having a bisphenol structure, compounds represented by the following formula (A2-1) are preferred.

[0157] [Chemical Formula 2]

[0158]

[0159] In equation (A2-1), n ​​represents a real number from 0 to 30, and R... 21 R 22 R 23 and R 24 Each alkyl group, consisting of 1 to 5 carbon atoms and either a hydrogen atom or substituted or unsubstituted alkyl groups, can be used independently.

[0160] R 21 R 22 R 23 and R 24 Preferably, it contains hydrogen atoms or methyl groups. R 21 R 22 R 23 and R 24 The same is preferred. n is preferably a real number between 0.1 and 30.

[0161] Among aromatic epoxy compounds having a bisphenol structure, one or more are preferably selected from the group consisting of bisphenol A type epoxy resin and bisphenol F type epoxy resin.

[0162] (A-2-1) Bisphenol A type epoxy resin

[0163] Bisphenol A type epoxy resin can be, for example, R in formula (A2-1). 21 R22 R 23 and R 24 The epoxy resin is methyl. Bisphenol A type epoxy resin refers to, for example, a resin obtained by condensing bisphenol A with epichlorohydrin in the presence of a base catalyst. Furthermore, modified epoxy resins, such as those obtained by reacting fatty acids from vegetable oils or modifiers with the epoxy groups or hydroxyl groups of the aforementioned bisphenol A type epoxy resin, can be used. In addition, hydrogenated epoxy compounds (e.g., hydrogenated bisphenol A type epoxy resins equivalent to the aforementioned alicyclic epoxy compounds) are not included in bisphenol A type epoxy resins.

[0164] (A-2-2) Bisphenol F type epoxy resin

[0165] Bisphenol F type epoxy resin can be, for example, R in formula (A2-1). 21 R 22 R 23 and R 24 Epoxy resins containing hydrogen atoms. Bisphenol F type epoxy resins refer to, for example, resins obtained by condensing bisphenol F with epichlorohydrin in the presence of a base catalyst. Furthermore, modified epoxy resins, such as those obtained by reacting fatty acids from vegetable oils or modifiers with the epoxy groups or hydroxyl groups of the aforementioned bisphenol F type epoxy resin, can be used. In addition, hydrogenated epoxy compounds (e.g., hydrogenated bisphenol F type epoxy resins equivalent to the aforementioned alicyclic epoxy compounds) are not included in bisphenol F type epoxy resins.

[0166] From the viewpoint of moisture permeability, the molecular weight of the aromatic epoxy compound, especially the molecular weight of (A-2-1) bisphenol A type epoxy resin or (A-2-2) bisphenol F type epoxy resin, is preferably 100 to 5000, more preferably 150 to 1000, and most preferably 200 to 450.

[0167] When aromatic epoxy compounds have a molecular weight distribution, it is preferable that the number average molecular weight of the aromatic epoxy compounds is within the above-mentioned range. Furthermore, in this specification, the number average molecular weight represents the converted value of polystyrene obtained by gel permeation chromatography (GPC) under the above-mentioned measurement conditions.

[0168] (A-3) Glycidyl ether compounds

[0169] Examples of glycidyl ether compounds include monoglycidyl ether compounds and polyglycidyl ether compounds.

[0170] As a monoglycidyl ether compound, there are no particular limitations; examples include methyl glycidyl ether, 2-ethylhexyl glycidyl ether, butyl glycidyl ether, decyl glycidyl ether, mixed alkyl glycidyl ethers with 12 to 13 carbon atoms, phenyl-2-methyl glycidyl ether, cetyl glycidyl ether, stearyl glycidyl ether, p-sec-butylphenyl glycidyl ether, p-tert-butylphenyl glycidyl ether, glycidyl methacrylate, isopropyl glycidyl ether, and alkenes. Propyl glycidyl ether, ethyl glycidyl ether, 2-methyl octyl glycidyl ether, phenyl glycidyl ether, 4-n-butylphenyl glycidyl ether, 4-phenylphenol glycidyl ether, toluyl glycidyl ether, dibromotolyl glycidyl ether, decyl glycidyl ether, methoxy polyethylene glycol monoglycidyl ether, ethoxy polyethylene glycol monoglycidyl ether, butoxy polyethylene glycol monoglycidyl ether, phenoxy polyethylene glycol monoglycidyl ether, dibromophenyl glycidyl ether, etc.

[0171] There are no particular limitations on the polyglycidyl ether compounds, and examples include diglycidyl ethers of alkylene glycols (e.g., diglycidyl ethers of ethylene glycol, propylene glycol, and 1,6-hexanediol), polyglycidyl ethers of polyols (e.g., di or triglycidyl ethers of glycerol or its alkylene oxide adducts), and diglycidyl ethers of polyalkylene glycols (e.g., diglycidyl ethers of polyethylene glycol or its alkylene oxide adducts, and diglycidyl ethers of polypropylene glycol or its alkylene oxide adducts). Here, aliphatic compounds such as ethylene oxide and propylene oxide can be cited as alkylene oxides.

[0172] The glycidyl ether compound preferably contains one or more halogen elements, and more preferably contains bromine.

[0173] Specifically, examples include halogenated phenyl glycidyl ethers such as bromophenyl glycidyl ether and dibromophenyl glycidyl ether, brominated tolyl glycidyl ether, and brominated bisphenol A type epoxy resins (e.g., diglycidyl ether of tetrabromobisphenol A).

[0174] The cationic polymerizable compound in embodiment (A) may include other cationic polymerizable compounds besides those described in (A-1), (A-2) and (A-3) above, such as one or more compounds composed of cyclobutane compounds and vinyl ether compounds.

[0175] As for oxetane compounds, there are no particular limitations. Examples include 3-ethyl-3-hydroxymethyloxetane (manufactured by TOAGOSEI CO.,LTD., trade name ARON OXETANE OXT-101, etc.), 1,4-bis[(3-ethyl-3-oxetane-butyl)methoxymethyl]benzene (same as OXT-121, etc.), 3-ethyl-3-(phenoxymethyl)oxetane (same as OXT-211, etc.), di(1-ethyl-(3-oxetane-butyl))methyl ether (same as OXT-221, etc.), and 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane (same as OXT-212, etc.). Oxetane compounds refer to compounds that have one or more oxetane rings within their molecules.

[0176] As a vinyl ether compound, there is no particular limitation, and examples include diethylene glycol diethylene ether, diethylene glycol diethylene ether, triethylene glycol monoethylene ether, triethylene glycol diethylene ether, propylene glycol diethylene ether, dipropylene glycol diethylene ether, butanediethylene glycol diethylene ether, hexanediethylene glycol diethylene ether, cyclohexanediethanol diethylene ether, trimethylolpropane triethylene ether, etc. (diethylene or triethylene ether compounds), ethylene glycol monoethylene ether, hydroxyethyl monoethylene ether, hydroxynonyl monoethylene ether, ethyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, octadecyl vinyl ether, cyclohexyl vinyl ether, hydroxybutyl vinyl ether, 2-ethylhexyl vinyl ether, cyclohexanediethanol monoethylene ether, n-propyl vinyl ether, isopropyl vinyl ether, isopropylene ether, o-propylene carbonate, dodecyl vinyl ether, diethylene glycol monoethylene ether, octadecyl vinyl ether, etc. (monoethylene ether compounds).

[0177] The content of the alicyclic compound having an epoxy group in (A-1) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, out of 100 parts by mass of the cationic polymerizable compound in (A). This tends to further improve the durability of the cured body.

[0178] On the other hand, the content of the alicyclic compound having an epoxy group in (A-1) is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less in 100 parts by mass of the cationic polymerizable compound (A).

[0179] When the aromatic compound having an epoxy group (A-2) is included, the content of the aromatic compound having an epoxy group (A-2) in 100 parts by mass of the cationic polymerizable compound (A) is preferably 40 parts by mass or more, more preferably 45 parts by mass or more, and even more preferably 50 parts by mass or more. This tends to further improve the durability of the cured body.

[0180] On the other hand, there is no particular limit to the content of aromatic compounds with epoxy groups in (A-2). For example, in 100 parts by mass of cationic polymeric compound (A), it can be less than 70 parts by mass, or it may not contain aromatic compounds with epoxy groups in (A-2).

[0181] When the compound (A-3) is included, the content of the glycidyl ether compound (A-3) is preferably 60 parts by mass or more, more preferably 65 parts by mass or more, and even more preferably 70 parts by mass or more, out of 100 parts by mass of the cationic polymerizable compound (A). This tends to further improve the durability of the cured body.

[0182] On the other hand, there is no particular limit to the content of (A-3) glycidyl ether compound. For example, in 100 parts by mass of (A) cationic polymeric compound, it can be less than 85 parts by mass, or it can be without (A-3) glycidyl ether compound.

[0183] In 100 parts by mass of the cationic polymeric compound (A), the total content of the alicyclic compound having an epoxy group (A-1), the aromatic compound having an epoxy group (A-2), and the glycidyl ether compound (A-3) is preferably 60 parts by mass or more, more preferably 80 parts by mass or more, most preferably 90 parts by mass or more, and even more preferably 100 parts by mass.

[0184] (B) Photocationic polymerization initiator

[0185] The sealing material for the photoelectric conversion element in this embodiment requires (B) a photocationic polymerization initiator as an essential component. When using a photocationic polymerization initiator, the sealing material for the photoelectric conversion element in this embodiment can be cured by irradiation with energy rays such as ultraviolet light.

[0186] As a photocationic polymerization initiator (B), there are no particular limitations, but examples include aryl sulfonate derivatives (e.g., Cyracure UVI-6990 and Cyracure UVI-6974 manufactured by Dow Chemical Company, ADEKA Optomer SP-150, ADEKA Optomer SP-152, ADEKA Optomer SP-170 and ADEKA Optomer SP-172 manufactured by Asahi Denka Kogyo K.K., CPI-100P, CPI-101A, CPI-200K, CPI-210S, CPI-310FG and LW-S1 manufactured by San-Apro Ltd., and Chivacure 1190 manufactured by Double Bond Chemical Ind. Co., Ltd.), aryl iodine, etc. Salt derivatives (e.g., Irgacure 250 from Ciba Specialty Chemicals, RP-2074 from Rhodia Japan Ltd.), alkyne-ion complex derivatives, diazonium salt derivatives, triazine initiators, and other acid-generating agents such as halides. The cationic species preferred as photocationic polymerization initiators are those represented by formula (B-1). Salt.

[0187] (B) As a photocationic polymerization initiator, there are no particular limitations; examples represented by formula (B-1) can be cited. Salt.

[0188] [Chemical Formula 3]

[0189]

[0190] (A represents an element of group VIA to VIIA with valence m. m represents 1 to 2. p represents 0 to 3. m and p are preferably integers. R represents an organic group bonded to A. D is a group formed by the following formula (B-1-1):)

[0191] [Chemical Formula 4]

[0192]

[0193] The divalent group represented. In formula (B-1-1), E represents a divalent group, and G represents -O-, -S-, -SO-, -SO2-, -NH-, -NR'-, -CO-, -COO-, -CONH-, or an alkylene or phenylene group with 1 to 3 carbon atoms (R' is an alkyl group with 1 to 5 carbon atoms or an aryl group with 6 to 10 carbon atoms). a represents 0 to 5. a+1 E's and a's G's can be the same or different. a is preferably an integer. X - for The counter ions number p+1 per molecule.

[0194] Equation (B-1) The ion is not particularly limited, but examples include 4-(phenylthio)phenyl diphenylsulfonium, bis[4-(diphenylsulfonium)phenyl]sulfide, bis[4-{bis[4-(2-hydroxyethoxy)phenyl]sulfonium}phenyl]sulfide, bis{4-[bis(4-fluorophenyl)sulfonium]phenyl}sulfide, 4-(4-benzoyl-2-chlorophenylthio)phenyl bis(4-fluorophenyl)sulfonium, 4-(4-benzoylphenylthio)phenyl diphenylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracene-2-yl di-p-tolylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracene-2-yl di-p-tolylsulfonium, and 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracene-2-yl di-p-tolylsulfonium. -10-Thia-9,10-dihydroanthracene-2-yldiphenylsulfonium, 2-[(di-p-tolyl)sulfonyl]thioxanthone, 2-[(diphenyl)sulfonyl]thioxanthone, 4-[4-(4-tert-butylbenzoyl)phenylthio]phenyldi-p-tolylsulfonium, 4-(4-benzoylphenylthio)phenyldiphenylsulfonium, 5-(4-methoxyphenyl)thiaxanthene, 5-phenylthiaxanthene, diphenylbenzylsulfonium, 4-hydroxyphenylmethylbenzylsulfonium, 2-naphthylmethyl(1-ethoxycarbonyl)ethylsulfonium, 4-hydroxyphenylmethylbenzylsulfonium, octadecylmethylbenzylsulfonium, etc.

[0195] R is an organic group bonded to A. R can represent, for example, an aryl group with 6 to 30 carbon atoms, a heterocyclic group with 4 to 30 carbon atoms, an alkyl group with 1 to 30 carbon atoms, an alkenyl group with 2 to 30 carbon atoms, or an alkynyl group with 2 to 30 carbon atoms. These can be substituted with at least one of the following groups: alkyl, hydroxyl, alkoxy, alkyl carbonyl, arylcarbonyl, alkoxycarbonyl, aryloxycarbonyl, arylthiocarbonyl, acyloxy, arylthio, alkylthio, aryl, heterocyclic, aryloxy, alkylsulfinyl, arylsulfinyl, alkylsulfonyl, arylsulfonyl, alkoxy, amino, cyano, nitro, and halogens. The number of Rs is m + p(m-1) + 1, and they can be the same or different. Furthermore, two or more Rs can be bonded directly to each other or via -O-, -S-, -SO-, -SO2-, -NH-, -NR'-, -CO-, -COO-, -CONH-, alkylene or phenylene with 1 to 3 carbon atoms to form a ring structure containing element A. Here, R' is an alkyl with 1 to 5 carbon atoms or an aryl with 6 to 10 carbon atoms.

[0196] Among the above, aryl groups with 6 to 30 carbon atoms can be listed as monocyclic aryl groups such as phenyl, and fused polycyclic aryl groups such as naphthyl, anthraquinone, phenanthrene, pyrene, thiol, naphthenyl, benzoanthrene, anthraquinone, fluorenyl, naphthoquinone, and anthraquinone.

[0197] The aforementioned aryl groups with 6 to 30 carbon atoms, heterocyclic groups with 4 to 30 carbon atoms, alkyl groups with 1 to 30 carbon atoms, alkenyl groups with 2 to 30 carbon atoms, or alkynyl groups with 2 to 30 carbon atoms may have at least one substituent. Examples of substituents include straight-chain alkyl groups with 1 to 18 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl; and isopropyl, isobutyl, sec-butyl, and tert-butyl. Branched alkyl groups with 1-18 carbon atoms, such as isopentyl, neopentyl, tert-pentyl, and isohexyl; cycloalkyl groups with 3-18 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl; hydroxyl groups; straight-chain or branched alkoxy groups with 1-18 carbon atoms, such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, sec-butoxy, tert-butoxy, hexoxy, decoxy, and dodecoxy; acetyl, propionyl, butyryl, 2-methylpropionyl, heptanoyl, and 2- Alkyl carbonyl groups with 2 to 18 carbon atoms, such as methylbutyryl, 3-methylbutyryl, octanoyl, decanoyl, dodecanoyl, and octadecanoyl; aryl carbonyl groups with 7 to 11 carbon atoms, such as benzoyl and naphthyl; and methoxycarbonyl, ethoxycarbonyl, propoxycarbonyl, isopropoxycarbonyl, butoxycarbonyl, isobutoxycarbonyl, sec-butoxycarbonyl, tert-butoxycarbonyl, octoxycarbonyl, tetradecoxycarbonyl, and octadecoxycarbonyl, with 2 to 19 carbon atoms. Straight-chain or branched alkoxy carbonyl groups; aryloxy carbonyl groups with 7 to 11 carbon atoms, such as phenoxy carbonyl and naphthoxy carbonyl; arylthio carbonyl groups with 7 to 11 carbon atoms, such as phenylthiocarbonyl and naphthiocarbonyl; and acyloxy groups with 2 to 19 carbon atoms, such as acetoxy, ethyl carbonyloxy, propyl carbonyloxy, isopropyl carbonyloxy, butyl carbonyloxy, isobutyl carbonyloxy, sec-butyl carbonyloxy, tert-butyl carbonyloxy, octyl carbonyloxy, tetradecyl carbonyloxy, and octadecyl carbonyloxy.Benzylthio, 2-methylbenzenethio, 3-methylbenzenethio, 4-methylbenzenethio, 2-chlorobenzenethio, 3-chlorobenzenethio, 4-chlorobenzenethio, 2-bromobenzenethio, 3-bromobenzenethio, 4-bromobenzenethio, 2-fluorobenzenethio, 3-fluorobenzenethio, 4-fluorobenzenethio, 2-hydroxybenzenethio, 4-hydroxybenzenethio, 2-methoxybenzenethio, 4-methoxybenzenethio, 1-naphthalene Thioyl, 2-naphthioyl, 4-[4-(phenylthio)benzoyl]phenylthio, 4-[4-(phenylthio)phenoxy]phenylthio, 4-[4-(phenylthio)phenyl]phenylthio, 4-(phenylthio)phenylthio, 4-benzoylphenylthio, 4-benzoyl-2-chlorophenylthio, 4-benzoyl-3-chlorophenylthio, 4-benzoyl-3-methylthiophenylthio 4-benzoyl-2-methylthiophenylthio, 4-(4-methylthiobenzoyl)phenylthio, 4-(2-methylthiobenzoyl)phenylthio, 4-(p-methylbenzoyl)phenylthio, 4-(p-ethylbenzoyl)phenylthio, 4-(p-isopropylbenzoyl)phenylthio, 4-(p-tert-butylbenzoyl)phenylthio, and other arylthio groups with 6 to 20 carbon atoms; methylthio Alkylthio groups with 1 to 18 carbon atoms, including ethylthio, propylthio, isopropylthio, butylthio, isobutylthio, sec-butylthio, tert-butylthio, pentylthio, isopentylthio, neopentylthio, tert-pentylthio, octylthio, decylthio, dodecylthio, etc.; aryl groups with 6 to 10 carbon atoms, including phenyl, tolyl, dimethylphenyl, naphthyl, etc.; thiophene, furanyl, pyranyl, pyrroleyl, etc. Azolyl, thiazolyl, pyridyl, pyrimidinyl, pyrazinyl, indoleyl, benzofuranyl, benzothiophenyl, quinolinyl, isoquinolinyl, quin Heterocyclic groups with 4 to 20 carbon atoms, such as linyl, quinazolinyl, carbazole, acridine, benzothiaphenyl, phenazinyl, flavonyl, thienoflavonyl, and benzofuranyl; aryloxy groups with 6 to 10 carbon atoms, such as phenoxy and naphthoxy; and straight-chain or branched alkyl sulfinyl groups with 1 to 18 carbon atoms, such as methyl sulfinyl, ethyl sulfinyl, propyl sulfinyl, isopropyl sulfinyl, butyl sulfinyl, isobutyl sulfinyl, sec-butyl sulfinyl, tert-butyl sulfinyl, pentyl sulfinyl, isopentyl sulfinyl, neopentyl sulfinyl, tert-pentyl sulfinyl, and octyl sulfinyl. Alkyl sulfonyl groups with 6 to 10 carbon atoms, such as phenylsulfinyl, tolylsulfinyl, and naphthylsulfinyl; alkyl sulfonyl groups with 1 to 18 carbon atoms, such as methylsulfonyl, ethylsulfonyl, propylsulfonyl, isopropylsulfonyl, butylsulfonyl, isobutylsulfonyl, sec-butylsulfonyl, tert-butylsulfonyl, pentylsulfonyl, isopentylsulfonyl, neopentylsulfonyl, tert-pentylsulfonyl, and octylsulfonyl; aryl sulfonyl groups with 6 to 10 carbon atoms, such as phenylsulfonyl, tolylsulfonyl (tolylsulfonyl), and naphthylsulfonyl; and those derived from formula (B-1-2).

[0198] [Chemical Formula 5]

[0199]

[0200] The following are listed: alkeneoxy groups (Q represents hydrogen or methyl, k represents an integer from 1 to 5); unsubstituted amino groups; amino groups monosubstituted or disubstituted with alkyl groups having 1 to 5 carbon atoms and / or aryl groups having 6 to 10 carbon atoms; cyano groups; nitro groups; halogens such as fluorine, chlorine, bromine, and iodine.

[0201] In equation (B-1), p represents [DA] + R m-1 The number of repeating units of the [] key, preferably an integer from 0 to 3.

[0202] As in equation (B-1) Ions [A] + The preferred ions are sulfonium and iodine. Ions, selenium Ions, as representative examples, can be listed below.

[0203] Examples of sulfonium ions include triphenylsulfonium, tri-p-tolylsulfonium, tri-o-tolylsulfonium, tris(4-methoxyphenyl)sulfonium, 1-naphthyldiphenylsulfonium, 2-naphthyldiphenylsulfonium, tris(4-fluorophenyl)sulfonium, tri-1-naphthylsulfonium, tri-2-naphthylsulfonium, tris(4-hydroxyphenyl)sulfonium, 4-(phenylthio)phenyldiphenylsulfonium, and 4-(p-tolylthio)phenyl 4-(4-methoxyphenylthio)phenylbis(4-methoxyphenyl)sulfonium, 4-(phenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(phenylthio)phenylbis(4-methoxyphenyl)sulfonium, 4-(phenylthio)phenylbis-p-tolylsulfonium, bis[4-(diphenylsulfonyl)phenyl]sulfide, bis[4-{bis[4-(2- [Hydroxyethoxy]phenyl]sulfonyl]phenyl]sulfide, bis{4-[bis(4-fluorophenyl)sulfonyl]phenyl]sulfide, bis{4-[bis(4-methylphenyl)sulfonyl]phenyl]sulfide, bis{4-[bis(4-methoxyphenyl)sulfonyl]phenyl]sulfide, 4-(4-benzoyl-2-chlorophenylthio)phenylbis(4-fluorophenyl)sulfonium, 4 -(4-benzoyl-2-chlorophenylthio)phenyl diphenylsulfonium, 4-(4-benzoylphenylthio)phenyl bis(4-fluorophenyl)sulfonium, 4-(4-benzoylphenylthio)phenyl diphenylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracene-2-yldi-p-tolylsulfonium, 7-isopropyl-9-oxo-10-thia- 9,10-Dihydroanthracene-2-yldiphenylsulfonium, 2-[(di-p-tolyl)sulfonyl]thioxanthone, 2-[(diphenyl)sulfonyl]thioxanthone, 4-[4-(4-tert-butylbenzoyl)phenylthio]phenyldi-p-tolylsulfonium, 4-[4-(4-tert-butylbenzoyl)phenylthio]phenyldiphenylsulfonium, 4-[4-(benzoylphenylthio)]phenyldi-p-tolylsulfonium, 4-[4-(benzoylphenylthio)]phenyldiphenylsulfonium, 5-(4-methoxyphenyl)thoxanthene, 5-phenylthoxanthene, 5-tolylthoxanthene, 5-(4-ethoxyphenyl)thoxanthene, 5-(2,4,6-trimethylphenyl)thoxanthene, and other triarylsulfoniums; diphenylbenzylsulfonium, diphenyl4- Nitrophenylmethyl sulfonium, diphenylbenzyl sulfonium, diphenylmethyl sulfonium, and other diaryl sulfoniums; phenylmethylbenzyl sulfonium, 4-hydroxyphenylmethylbenzyl sulfonium, 4-methoxyphenylmethylbenzyl sulfonium, 4-acetyloxyphenylmethylbenzyl sulfonium, 2-naphthylmethylbenzyl sulfonium, 2-naphthylmethyl(1-ethoxycarbonyl)ethyl sulfonium, phenylmethylbenzyl sulfonium, 4-hydroxyphenylmethylbenzyl sulfonium Monoaryl sulfoniums such as methylsulfonium, 4-methoxyphenylmethylbenzylsulfonium, 4-acetyloxyphenylmethylbenzylsulfonium, 2-naphthylmethylbenzylsulfonium, 2-naphthyloctadecylbenzylsulfonium, and 9-anthraylmethylbenzylsulfonium; trialkylsulfoniums such as dimethylbenzylsulfonium, benzyltetrahydrothione, dimethylbenzylsulfonium, benzyltetrahydrothione, and octadecylmethylbenzylsulfonium.

[0204] These Among the ions, sulfonium ions and iodine ions are preferred. The ion may consist of one or more types, with sulfonium ions being more preferred. Preferred sulfonium ions include triphenylsulfonium, tri-p-tolylsulfonium, 4-(phenylthio)phenyldiphenylsulfonium, bis[4-(diphenylsulfonium)phenyl]sulfide, bis[4-{bis[4-(2-hydroxyethoxy)phenyl]sulfonium}phenyl]sulfide, bis{4-[bis(4-fluorophenyl)sulfonium]phenyl}sulfide, 4-(4-benzoyl-2-chlorophenylthio)phenylbis(4-fluorophenyl)sulfonium, 4-(4-benzoylphenylthio)phenyldiphenylsulfonium, and 7-isopropyl-9 -Oxo-10-thia-9,10-dihydroanthracene-2-yldi-p-tolylsulfonium, 7-isopropyl-9-oxo-10-thia-9,10-dihydroanthracene-2-yldiphenylsulfonium, 2-[(di-p-tolyl)sulfonyl]thioxanthone, 2-[(diphenyl)sulfonyl]thioxanthone, 4-[4-(4-tert-butylbenzoyl)phenylthio]phenyldi-p-tolylsulfonium, 4-[4-(benzoylphenylthio)]phenyldiphenylsulfonium, 5-(4-methoxyphenyl)thiazanthracene 5-Phenylenthione One or more of the following: diphenylbenzylsulfonium, 4-hydroxyphenylmethylbenzylsulfonium, 2-naphthylmethyl(1-ethoxycarbonyl)ethylsulfonium, 4-hydroxyphenylmethylbenzylsulfonium, and octadecylmethylbenzylsulfonium.

[0205] In equation (B-1), X - These are counter ions. Their number is p+1 per molecule. There are no particular limitations on counter ions; examples include halides such as boron compounds, phosphorus compounds, antimony compounds, arsenic compounds, alkyl sulfonic acid compounds, and methyl compounds. As X - For example, F can be listed. - Cl - ,Br - I - Halogen ions; OH - ClO4 - FSO3 - ClSO3 - CH3SO3 - C6H5SO3 - CF3SO3 - Sulfonate ions; HSO4 - SO4 2- Sulfate ions; HCO3 - CO3 2- Carbonate ions; H2PO4 - HPO4 2- PO4 3- Phosphate ions; PF6 - PF5OH- Fluorophosphate ions such as fluorinated alkyl fluorophosphate ions; BF4 - B(C6F5)4 - B(C6H4CF3)4 - Boronate ions; AlCl4 - BiF6 - Etc. In addition, SbF6 can be listed. - SbF5OH - Isofluronic acid ions or AsF6 - AsF5OH - Such as fluorinated arsenate ions, etc.

[0206] Examples of fluorinated alkyl fluorophosphate ions include those represented by formula (B-1-3).

[0207] (Rf) b PF 6-b ]- (B-1-3)

[0208] In formula (B-1-3), Rf represents an alkyl group substituted with a fluorine atom. The number b of Rf is 1 to 5, preferably an integer. The b Rf can be the same or different. The number b of Rf is more preferably 2 to 4, and most preferably 2 to 3.

[0209] In the fluorinated alkyl fluorophosphate ion represented by formula (B-1-3), Rf represents an alkyl group substituted with a fluorine atom, preferably having 1 to 8 carbon atoms, and more preferably 1 to 4 carbon atoms. Examples of alkyl groups include straight-chain alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, and octyl; branched-chain alkyl groups such as isopropyl, isobutyl, sec-butyl, and tert-butyl; and cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl. Specific examples include CF3, CF3CF2, (CF3)2CF, CF3CF2CF2, CF3CF2CF2CF2, (CF3)2CFCF2, CF3CF2(CF3)CF, and (CF3)3C.

[0210] As a specific example of a preferred fluorinated alkyl fluorophosphate anion, [(CF3CF2)2PF4] can be cited. - [(CF3CF2)3PF3] - [(CF3)2CF)2PF4] - [(CF3)2CF)3PF3] - [(CF3CF2CF2)2PF4] - [(CF3CF2CF2)3PF3] - , [((CF3)2CFCF2)2PF4] -, [((CF3)2CFCF2)3PF3] - [(CF3CF2CF2CF2)2PF4] - and [(CF3CF2CF2CF2)3PF3] - wait.

[0211] To facilitate dissolution in epoxy compounds and epoxy resins, photocationic polymerization initiators can be pre-dissolved in solvents. Examples of solvents include propylene carbonate, ethylene carbonate, 1,2-butene carbonate, dimethyl carbonate, diethyl carbonate, and other carbonates.

[0212] These photocationic polymerization initiators can be selected from one or more.

[0213] Examples of anionic initiators for (B) photocationic polymerization include halides such as boron compounds, phosphorus compounds, antimony compounds, arsenic compounds, and alkyl sulfonic acid compounds. One or more of these anionic initiators may be used. Among these, fluorides are preferred from the viewpoint of excellent photocurability and improved adhesion and adhesion durability. Among fluorides, hexafluoroantimonates are preferred.

[0214] In the photocationic polymerization initiator (B), one or more of the following are preferred: triarylsulfonium hexafluoroantimonate represented by formula (B-2) and diphenyl 4-phenoxyphenylsulfonium tri(pentafluoroethyl) trifluorophosphate represented by formula (B-3), with triarylsulfonium hexafluoroantimonate being more preferred.

[0215] [Chemical Formula 6]

[0216]

[0217] [Chemical Formula 7]

[0218]

[0219] (B) The content of the photocationic polymerization initiator relative to 100 parts by mass of the cationic polymerizable compound (A) is preferably 0.05 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, and even more preferably 0.5 to 2 parts by mass. It tends that if the content of the photocationic polymerization initiator is 0.05 parts by mass or more, the photocurability is further improved; if it is 5 parts by mass or less, the adhesion durability is further improved.

[0220] (C1) Photosensitizer

[0221] The sealing material for the photoelectric conversion element in this embodiment contains a (C) sensitizer. Preferably, a (C1) photosensitizer is used as the (C) sensitizer. A (C1) photosensitizer is a compound that absorbs energy rays and effectively generates cations from a photocationic polymerization initiator.

[0222] As (C1) photosensitizers, there are no particular limitations, and examples include benzophenone derivatives, phenanthrene-thiazine derivatives, phenyl ketone derivatives, naphthalene derivatives, anthracene derivatives, phenanthrene derivatives, naphthone derivatives, benzo[a]benzene derivatives, perylene derivatives, pentane derivatives, acridine derivatives, benzo[a]thiazole derivatives, benzoin derivatives, fluorene derivatives, naphthoquinone derivatives, anthraquinone derivatives, thioxanol derivatives, thioxanone derivatives, coumarin derivatives, ketocumarin derivatives, anthocyanin derivatives, acridine derivatives, and thiazine derivatives. Azine derivatives, dihydroindole derivatives, Derivatives, triallylmethane derivatives, phthalocyanine derivatives, spiropyran derivatives, spiropyran Azide derivatives, thiospiropyran derivatives, and organorruthenium complexes, etc.

[0223] Among these, phenyl ketone derivatives such as 2-hydroxy-2-methyl-1-phenyl-propane-1-one and anthracene derivatives are preferred, and anthracene derivatives are even more preferred.

[0224] Examples of anthracene derivatives include anthracene, 1,2-benzanthracene, 9-cyanoanthracene, 9,10-dicyanoanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, 9,10-diepoxypropyloxyanthracene, and 9,10-bis(phenylethyl)anthracene. Among these, 9,10-diethoxyanthracene is preferred.

[0225] From the viewpoint that the photocurability does not deteriorate and the storage stability does not decrease, the content of the photosensitizer (C1) is preferably 0.01 to 10 parts by mass relative to 100 parts by mass of the cationic polymeric compound (A), more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass.

[0226] (D) Phosphoric acid compounds

[0227] The sealing material for the photoelectric conversion element in this embodiment may contain a (D) phosphate compound. This results in a tendency to reduce viscosity and good storage stability. Consequently, reliability is also easily improved.

[0228] (D) The phosphoric acid compound is selected from one or more of the group consisting of (D1) phosphate esters and (D2) phosphites. As a phosphoric acid compound, an organophosphate compound is preferred, and (D1) phosphate ester is more preferred.

[0229] Examples of (D1) phosphate esters include diethylbenzyl phosphate, trimethyl phosphate, triethyl phosphate, tri-n-butyl phosphate, tri(butoxyethyl) phosphate, tri(2-ethylhexyl) phosphate (trioctyl phosphate), (RO)3P=O [R = lauryl, cetyl, stearyl or oleyl], tri(2-chloroethyl) phosphate, tri(2-dichloropropyl) phosphate, triphenyl phosphate, butylpyrrole phosphate, trimethylmethyl phosphate, tridimethylmethyl phosphate, trioctyl phosphate, octyl diphenyl phosphate, tolyl diphenyl phosphate, diphenyl diphosphate, monobutyl phosphate, dibutyl phosphate, di-2-ethylhexyl phosphate, monoisodecyl phosphate, ammonium ethyl acid phosphate, and 2-ethylhexyl acid phosphate salts.

[0230] (D1) Phosphate preferably contains at least one of the group consisting of a compound represented by formula (D1-1), a compound represented by formula (D1-2), and a compound represented by formula (D1-3), and more preferably contains a compound represented by formula (D1-2).

[0231] [Chemical Formula 8]

[0232]

[0233] [Chemical Formula 9]

[0234]

[0235] [Chemical Formula 10]

[0236]

[0237] In equations (D1-1), (D1-2), and (D1-3), R 1 R 2 R 3 R 4 R 5 and R 6 Each can be represented independently as a hydrocarbon group that may have substituents.

[0238] R in equation (D1-2) 2 R 3 and R 4 and R in equation (D1-3) 5 and R 6 Preferably, the same functional groups are used in each formula.

[0239] As R 1 R 2 R 3 R 4 R 5 and R 6The hydrocarbon group in R can have substituents, such as oxoalkyl groups, etc. 1 R 2 R 3 R 4 R 5 and R 6 The hydrocarbon group in the sample is preferably an unsubstituted hydrocarbon group.

[0240] R 1 R 2 R 3 R 4 R 5 and R 6 The hydrocarbon group is preferably alkyl or aryl, more preferably alkyl or phenyl, and even more preferably alkyl. The alkyl group may have, for example, 1 to 18 carbon atoms, preferably 4 to 13.

[0241] As a compound represented by formula (D1-1), it can be, for example, a monoalkyl phosphate ester (i.e., R 1 Compounds that are alkyl groups, etc., as specific examples, include monoethyl phosphate, mono-n-butyl phosphate, mono(butoxyethyl) phosphate, mono(2-ethylhexyl) phosphate, etc.

[0242] As the compound represented by formula (D1-2), a trialkyl phosphate ester (i.e., R) is preferred. 2 R 3 and R 4 (For compounds that are alkyl groups). In this case, R... 2 R 3 and R 4 The alkyl group preferably has 1 to 18 carbon atoms, more preferably 4 to 12, and even more preferably 8.

[0243] Specific examples of trialkyl phosphates include triethyl phosphate, tri-n-butyl phosphate, tri(butoxyethyl) phosphate, tri(2-ethylhexyl) phosphate (trioctyl phosphate), and (RO)3P=O (where R is lauryl, cetyl, stearyl, or oleyl).

[0244] Examples of compounds represented by formulas (D1-3) include, for example, dialkyl phosphates (i.e., R...). 5 and R 6 Compounds that are alkyl groups, etc. Specific examples of dialkyl phosphates include dibutyl phosphate, bis(2-ethylhexyl) phosphate, etc.

[0245] In equations (D1-1), (D1-2), and (D1-3), R 1 R 2 R 3 R 4 R 5 and R6 It can be independently one or more of the following: a hydrocarbon group containing an alkyl group, a hydrocarbon group containing an aromatic ring, or a hydrocarbon group containing an aliphatic ring. The hydrocarbon group can have some unsaturated groups, and can also have any atoms or substituents. In this case, R 1 R 2 R 3 R 4 R 5 and R 6 Preferably, it contains an alkyl group. Furthermore, the alkyl group is preferably an unsubstituted saturated group. R 1 R 2 R 3 R 4 R 5 and R 6 The same is preferred.

[0246] Examples of (D2) phosphites include trimethyl phosphite, triethyl phosphite, tri-n-butyl phosphite, tri(2-ethylhexyl) phosphite, triisooctyl phosphite, tridecyl phosphite, triisodecyl phosphite, tri(tridecyl) phosphite, trioleyl phosphite, tristearyl phosphite, triphenyl phosphite, tri(nonylphenyl) phosphite, tri(2,4-di-tert-butylphenyl) phosphite, phenyl diisooctyl phosphite, phenyl diisodecyl phosphite, diphenyl mono(2-ethylhexyl) phosphite, diphenyl isooctyl phosphite, diphenyl monodecyl phosphite, diphenyl monoisodecyl phosphite, diphenyl mono(tridecyl) phosphite, and bis(nonylphenyl)dinonylphenyl. Phosphites, tetraphenyl dipropylene glycol diphosphate, poly(dipropylene glycol) phenyl phosphite, diisodecyl neopentyltetraphosphate, bis(tridecyl) neopentyltetraphosphate, distearate neopentyltetraphosphate, bis(nonylphenyl) neopentyltetraphosphate, tetraphenyltetra(tridecyl) neopentyltetraphosphate, tetra(tridecyl)-4,4'-isopropylidene diphenyl phosphite, trilauryl trithiophosphite, dimethyl hydrogen phosphite, dibutyl hydrogen phosphite, di(2-ethylhexyl) hydrogen phosphite, dilauryl hydrogen phosphite, dioleyl hydrogen phosphite, diphenyl hydrogen phosphite, diphenyl mono(2-ethylhexyl) phosphite, diphenyl monodecyl phosphite, and diphenyl mono(tridecyl) phosphite, etc.

[0247] (D) The content of the phosphoric acid compound relative to 100 parts by mass of the cationic polymeric compound (A) is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass.

[0248] If the content of (D) phosphoric acid compound is 0.01 parts by mass or more, it can suppress the increase in viscosity after light irradiation and improve reliability; if it is 5 parts by mass or less, it can maintain good photocurability.

[0249] [other]

[0250] In addition to the components (A) to (D) mentioned above, the sealing material for photoelectric conversion elements may also contain known additives such as silane coupling agents, initiators, crown ethers, and other stabilizers.

[0251] (F1) stabilizer

[0252] Storage stability can be improved by including (F1) stabilizer.

[0253] As a (F1) stabilizer, there are no particular limitations, and examples include amino acid derivative compounds such as carbonyl diimidazole, antioxidants, ether compounds, or mixtures thereof.

[0254] Among these, ether compounds are preferred, such as polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and other polyepoxides or cyclic crown ethers. Carbonyl diimidazole and crown ethers are particularly preferred.

[0255] As a crown ether, there are no particular limitations; examples include 12-crown-4 ether, 15-crown-5 ether, 18-crown-6 ether, and dicyclohexane-18-crown-6 ether.

[0256] When (F1) contains a stabilizer, the content of the stabilizer (F1) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, out of 100 parts by mass of the cationic polymeric compound (A). This improves storage stability.

[0257] On the other hand, there is no particular limit to the content of (F1) stabilizer. For example, in 100 parts by mass of (A) cationic polymeric compound, it can be less than 5 parts by mass.

[0258] (Silane coupling agent)

[0259] There are no particular limitations on silane coupling agents, and examples include γ-chloropropyltrimethoxysilane, vinyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyl-tris(β-methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-epoxypropoxypropyltrimethoxysilane, γ-epoxypropoxypropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-ureapropyltriethoxysilane, etc. One or more of these silane coupling agents can be used. Among these, one or more are preferably selected from the group consisting of β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-epoxypropoxypropyltrimethoxysilane, γ-epoxypropoxypropyltriethoxysilane, and γ-(meth)acryloyloxypropyltrimethoxysilane, and more preferably γ-epoxypropoxypropyltrimethoxysilane.

[0260] When a silane coupling agent is included, the content of the silane coupling agent is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, out of 100 parts by mass of the cationic polymerizable compound (A). This provides good adhesion and adhesive durability.

[0261] On the other hand, there is no particular limit to the content of silane coupling agent. For example, in 100 parts by mass of (A) cationic polymeric compound, it can be less than 5 parts by mass, or it can be free of silane coupling agent.

[0262] <Dam Materials>

[0263] The dam material of this embodiment includes the aforementioned sealing material for photoelectric conversion elements and (E) inorganic filler. In the dam material, the sealing material for photoelectric conversion elements and (E) inorganic filler can be mixed or separated. The mixing method is not particularly limited, and the same method used for the sealing material for photoelectric conversion elements can be used.

[0264] The dam material of this embodiment can preferably be used as a dam material in the cofferdam filling method. That is, by including (E) inorganic filler, the viscosity and mechanical strength can be improved.

[0265] A dam is obtained by solidifying the dam material of this embodiment using the method described later.

[0266] (E) Inorganic packing

[0267] The dam material in this embodiment requires (E) inorganic filler as an essential component. (E) Inorganic filler is a solid component composed of inorganic substances.

[0268] As (E) inorganic fillers, one or more of the following may be listed: crystalline silica such as quartz, amorphous silica such as fused silica and colloidal silica, zircon, zirconium oxide, magnesium oxide, olivine, spinel, clay, mullite, corundum, silica, cordierite, talc, kaolin, mica, chromite, biotite, ceramic stone, obsidian, perlite, glass, glaze, diatomite, paraffin stone, vermiculite, bentonite, aluminosilicate, graphite, carbon, sodium silicate, zinc oxide, calcium oxide, titanium oxide, zinc carbonate, magnesium carbonate, calcium carbonate, silicon carbide, silicon nitride, and boron nitride.

[0269] Inorganic fillers can be used to hydrophobically treat surfaces. For example, epoxy silanes, amino silanes, (meth)acrylate silanes, vinyl silanes, methylchlorosilanes, dimethylpolysiloxanes, etc., can be used, and surface treatment can be performed by known methods.

[0270] (E) The content of inorganic filler relative to 100 parts by mass of (A) cationic polymeric compound is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and from the viewpoint of further improving durability and reliability, it is even more preferably 80 parts by mass or more, and more preferably 100 parts by mass or more.

[0271] On the other hand, the content of (E) inorganic filler is preferably 300 parts by mass or less, more preferably 200 parts by mass or more, relative to 100 parts by mass of (A) cationic polymeric compound. This results in good extrusion properties.

[0272] [Viscosity]

[0273] The dam material in this embodiment is set to 0.5 ml. Using a conical plate CPA-52Z, the viscosity measured at 25°C and 0.7 rpm is preferably 100,000 mPa·s or more, more preferably 200,000 mPa·s or more, and even more preferably 250,000 mPa·s or more.

[0274] On the other hand, the viscosity of the dam material is preferably below 1,200,000 mPa·s, more preferably below 800,000 mPa·s, and even more preferably below 500,000 mPa·s.

[0275] By setting the viscosity of the dam material within the aforementioned range, uneven discharge during ejection can be reduced, and the generation of ripples and bubbles can be suppressed.

[0276] 2. Second Implementation Method

[0277] The sealing material for the photoelectric conversion element in this embodiment is used in the dam filling method and includes (A) a cationic polymerizable compound and (B) a photocationic polymerization initiator. In the contact angle measured over time by the following step i, the contact angle θc after 5 seconds of liquid contact is 30° or less.

[0278] (Step i) Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the sealing material for the photoelectric conversion element into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass.

[0279] (Condition ii)

[0280] • Measurement method: Changes over time

[0281] • Control method: Standard

[0282] • Analytical methods and techniques: droplet method, θ / 2 method

[0283] • Field of view: Wide angle 2

[0284] • Droplet volume: 5 μl

[0285] By setting the contact angle θc after 5 seconds of contact with the liquid to below the aforementioned upper limit, the wettability of the sealing material for the photoelectric conversion element can be improved. As a result, the adhesion between the sealing material for the photoelectric conversion element and the substrate can be improved, and the filling capacity of the sealing material for the photoelectric conversion element within the dam frame can be improved, thus enhancing the reliability of the device using the sealing material for the photoelectric conversion element of this embodiment.

[0286] Although the details of the reason are not yet clear, it is speculated to be as follows.

[0287] First, the low contact angle θc after 5 seconds of contact with the liquid indicates that the sealing material for the photoelectric conversion element is rapidly wetted and adheres to the substrate immediately after coating. Therefore, it is speculated that air bubbles are less likely to enter, which improves the reliability of devices using sealing materials for photoelectric conversion elements.

[0288] [Contact Angle]

[0289] The contact angle θc after 5 seconds of contact with the liquid is 30° or less, preferably 25° or less, and more preferably 22° or less. This improves the wettability of the sealing material used in photoelectric conversion elements.

[0290] On the other hand, from the point of view of obtaining wettability, there is no particular limitation on the lower limit of the contact angle θc after 5 seconds of contact with the liquid. From the point of view of good operability, it can be set to 1° or more, or it can be set to 5° or more.

[0291] Furthermore, in the contact angle measured in step i, the contact angle θd after 30 seconds of contact with the liquid is preferably 20° or less, more preferably 18° or less, and even more preferably 17° or less. This improves the wettability of the sealing material for the photoelectric conversion element.

[0292] On the other hand, from the viewpoint of obtaining wettability, there is no particular limitation on the lower limit of the contact angle θd after 30 seconds of contact with the liquid. From the viewpoint of good operability, it can be set to 1° or more, or 3° or more.

[0293] Furthermore, the contact angle θc (°) is preferably 1.0 or more relative to the contact angle θd (°) (θc / θd).

[0294] On the other hand, the contact angle θb (°) is preferably 2.3 or less relative to the contact angle θa (°) (θc / θd), more preferably 2.0 or less, and even more preferably 1.7 or less.

[0295] The sealing material for photoelectric conversion elements that meets the aforementioned contact angle can be achieved by selecting the types of components constituting the sealing material and adjusting the dosage. Specifically, from the viewpoint of obtaining wettability, examples include using (A-1) an alicyclic compound having an epoxy group, or using (C2) a reactive diluent, (D) a phosphoric acid compound, and (F2) a stabilizer, as described later. Furthermore, from the viewpoint of ensuring the desired physical properties of the sealing material for photoelectric conversion elements, methods such as combining (A-2) an aromatic compound having an epoxy group and (A-3) a glycidyl ether compound with (A-1) an alicyclic compound having an epoxy group can also be cited.

[0296] [Viscosity]

[0297] Furthermore, the viscosity of the photoelectric conversion element is preferably 50 mPa·s or more, more preferably 80 mPa·s or more, and even more preferably 100 mPa·s or more, when the sealing material for the photoelectric conversion element is set to 0.5 ml and a conical plate CPA-40Z is used, measured at 25°C and 50 rpm.

[0298] On the other hand, the viscosity of the sealing material for the photoelectric conversion element is preferably 1000 mPa·s or less, more preferably 800 mPa·s or less, and even more preferably 700 mPa·s or less.

[0299] The following describes the composition of the sealing material used in photoelectric conversion elements.

[0300] (A) Cationic polymeric compounds

[0301] The sealing material for the photoelectric conversion element in this embodiment requires (A) a cationic polymeric compound as an essential component. (A) The cationic polymeric compound is preferably photopolymeric.

[0302] As (A) a cationic polymerizable compound, the same cationic polymerizable compound as described in the first embodiment can be used.

[0303] In this embodiment, the content of the alicyclic compound having an epoxy group (A-1) in 100 parts by mass of the cationic polymerizable compound (A) is preferably 20 parts by mass or more, more preferably 30 parts by mass or more, and even more preferably 40 parts by mass or more. This tends to further improve the durability of the cured body.

[0304] On the other hand, the content of the alicyclic compound having an epoxy group in (A-1) is preferably 85 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 75 parts by mass or less in 100 parts by mass of the cationic polymerizable compound (A).

[0305] In this embodiment, when the aromatic compound having an epoxy group (A-2) is included, the content of the aromatic compound having an epoxy group (A-2) in 100 parts by mass of the cationic polymerizable compound (A) is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more. This tends to further improve the durability of the cured body.

[0306] On the other hand, there is no particular limit to the upper limit of the content of aromatic compounds with epoxy groups in (A-2). For example, in 100 parts by mass of cationic polymeric compound (A), it can be less than 50 parts by mass, or it can not contain aromatic compounds with epoxy groups in (A-2).

[0307] In this embodiment, when the (A-3) glycidyl ether compound is included, the content of the (A-3) glycidyl ether compound is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, out of 100 parts by mass of the (A) cationic polymerizable compound. This tends to further improve the durability of the cured body.

[0308] On the other hand, there is no particular limit to the content of (A-3) glycidyl ether compound. For example, in 100 parts by mass of (A) cationic polymeric compound, it can be less than 65 parts by mass, or it can be without (A-3) glycidyl ether compound.

[0309] In this embodiment, in 100 parts by mass of the cationic polymeric compound (A), the total content of the alicyclic compound having an epoxy group (A-1), the aromatic compound having an epoxy group (A-2), and the glycidyl ether compound (A-3) is preferably 60 parts by mass or more, more preferably 80 parts by mass or more, most preferably 90 parts by mass or more, and even more preferably 100 parts by mass.

[0310] (B) Photocationic polymerization initiator

[0311] The sealing material for the photoelectric conversion element in this embodiment requires (B) a photocationic polymerization initiator as an essential component. When using a photocationic polymerization initiator, the sealing material for the photoelectric conversion element in this embodiment can be cured by irradiation with energy rays such as ultraviolet light.

[0312] As (B) photocationic polymerization initiator, the same photocationic polymerization initiator described in the first embodiment can be used.

[0313] In this embodiment, the content of (B) photocationic polymerization initiator relative to 100 parts by mass of (A) cationic polymerizable compound is preferably 0.05 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, and even more preferably 0.2 to 2 parts by mass. There is a tendency that if the content of the photocationic polymerization initiator is 0.05 parts by mass or more, the photocurability is further improved; if it is 5 parts by mass or less, the adhesion durability is further improved.

[0314] [(C2) Reactive diluent]

[0315] The sealing material for the photoelectric conversion element in this embodiment can contain a reactive diluent (C2). This results in a tendency to reduce viscosity. Consequently, reliability is also easily improved.

[0316] (C2) Reactive diluents can be listed as compounds having two or more glycidyl ether functional groups on an aliphatic hydrocarbon chain and a molecular weight of 150 to 600. Furthermore, they can further have other polymerizable functional groups, such as unsaturated groups such as vinyl, allyl, alkenyl, acryloyl, methacryloyl, etc.

[0317] By setting the molecular weight above the aforementioned lower limit, the volatilization of the reactive diluent can be suppressed, thereby achieving good adhesion. Conversely, by setting the molecular weight below the aforementioned lower limit, good reactivity can be obtained.

[0318] Examples of (C2) reactive diluents include diepoxides of ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, butylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, and cyclohexanediethanol diglycidyl ether; monoepoxides of phenyl glycidyl ether and butylphenyl glycidyl ether; and triepoxides of trimethylolpropane triglycidyl ether and glycerol triglycidyl ether.

[0319] (C2) The total amount of reactive diluent relative to the sealing material for photoelectric conversion element is preferably 0.1 to 10% by mass, more preferably 0.5 to 8% by mass.

[0320] By setting the content of the (C2) reactive diluent to the lower limit or above mentioned above, wettability can be improved and good adhesion can be obtained. On the other hand, by setting the content of the (C2) reactive diluent to the upper limit or below mentioned above, good strength after curing can be obtained and reliability can be improved.

[0321] [(D) Phosphoric acid compounds]

[0322] The sealing material for the photoelectric conversion element in this embodiment may contain a (D) phosphate compound. This results in a tendency to reduce viscosity and good storage stability. Consequently, reliability is also easily improved.

[0323] As (D) phosphoric acid compound, the same phosphoric acid compound as described in the first embodiment can be used.

[0324] In this embodiment, the content of (D) phosphoric acid compound relative to 100 parts by mass of (A) cationic polymeric compound is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass.

[0325] If the content of (D) phosphoric acid compound is 0.01 parts by mass or more, it can suppress the increase in viscosity after light irradiation and improve reliability; if it is 5 parts by mass or less, it can maintain good photocurability.

[0326] [other]

[0327] In this embodiment, the sealing material for the photoelectric conversion element may contain known additives such as (F2) stabilizer, silane coupling agent, initiator, and sensitizer, in addition to the above-mentioned components (A) to (D).

[0328] Furthermore, the sealing material for the photoelectric conversion element in this embodiment preferably does not contain (E) inorganic filler.

[0329] [(F2) stabilizer]

[0330] Storage stability can be improved by including (F2) stabilizer.

[0331] As a (F2) stabilizer, there are no particular limitations, and examples include carboxylic amide compounds, antioxidants, ether compounds, amino acid derivative compounds, or mixtures thereof.

[0332] For example, phosphorus antioxidants such as tris(2,4-di-tert-butylphenyl) phosphite, diphenyl mono(2-ethylhexyl) phosphite, diphenyl monodecyl phosphite, neopentyltetrol bis(2,6-di-tert-butyl-4-phenyl) phosphite, and 2,2'-methylene bis(4,6-di-tert-butylphenyl)-2-ethylhexyl phosphite can be used as (F2) stabilizers.

[0333] Examples of ether compounds include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and other polyepoxides or cyclic crown ethers. Carbonyl diimidazoles and crown ethers are preferred. There are no particular limitations on the crown ether used; examples include 12-crown-4 ether, 15-crown-5 ether, 18-crown-6 ether, and dicyclohexane-18-crown-6 ether.

[0334] When (F2) contains a stabilizer, the content of the stabilizer in (F2) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, out of 100 parts by mass of the cationic polymeric compound (A). This improves storage stability.

[0335] On the other hand, there is no particular limit to the content of the (F2) stabilizer, for example, it can be less than 5 parts by mass in 100 parts by mass of the (A) cationic polymeric compound.

[0336] (Silane coupling agent)

[0337] As a silane coupling agent, the same silane coupling agent as described in the first embodiment can be used.

[0338] The common structure, characteristics, and uses of the sealing materials for photoelectric conversion elements described in the first and second embodiments will be further explained below.

[0339] <Uses>

[0340] The sealing material for photoelectric conversion elements in this embodiment is preferably used for applications such as liquid crystal displays, organic EL displays, and electronic paper displays, or for sealing applications of photoelectric conversion elements such as silicon solar cells, dye-sensitized solar cells, and organic thin-film solar cells.

[0341] <Manufacturing Method>

[0342] Regarding the manufacturing method of the sealing material for the photoelectric conversion element in this embodiment, there are no particular limitations as long as the above-mentioned components can be thoroughly mixed. There are no particular limitations on the mixing method for each component; examples include stirring methods utilizing the stirring force accompanying the rotation of a propeller, and methods using conventional dispersers such as planetary mixers based on rotation and revolution. From the viewpoint of achieving stable mixing at low cost, these mixing methods are preferred.

[0343] <Device>

[0344] The apparatus of this embodiment includes a photoelectric conversion element sealed with a sealing material by the aforementioned photoelectric conversion element.

[0345] Hereinafter, an example of the apparatus of this embodiment will be described using the accompanying drawings.

[0346] like Figure 1 As shown, the device 100 of this embodiment includes a photoelectric conversion element 31, a filling material 21 covering the photoelectric conversion element 31, a dam material 22 arranged to surround the filling material 21, and a pair of members (member 11 and member 12) clamping them. Furthermore, the photoelectric conversion element 31 is disposed on the member 12.

[0347] In this embodiment, the dam material 22 is formed using the aforementioned sealing material for photoelectric conversion elements and (E) inorganic filler.

[0348] The photoelectric conversion element 31 is sealed by the filling material 21 and the dam material 22.

[0349] Figure 2 This is a diagram showing the positional relationship between the filling material 21 and the dam material 22 from a top view of the device 100. (See diagram below.) Figure 2 As shown, the filling material 21 is surrounded by the dam material 22. In other words, the sidewalls of the filling material 21 are in contact with the dam material 22.

[0350] Specifically, the device 100 may include displays such as liquid crystal displays, organic EL displays, and electronic paper displays, as well as silicon solar cells, dye-sensitized solar cells, and organic thin-film solar cells.

[0351] Next, an example of a method for manufacturing the apparatus 100 of this embodiment will be described.

[0352] like Figure 3 As shown, the manufacturing method of the device 100 in this embodiment includes:

[0353] The process of attaching filling material 21 and dam material 22 surrounding filling material 21 to component 11 (first component);

[0354] The process of embedding the photoelectric conversion element 31 into the filling material 21;

[0355] The process of arranging component 12 (the second component) by covering the filling material 21 and the dam material 22; and

[0356] The process of curing the filling material 21 by bonding the components 11 and 12, and the dam material 22 includes the aforementioned sealing material for the photoelectric conversion element and (E) inorganic filler.

[0357] The following is a detailed explanation.

[0358] (Attachment process)

[0359] First, such as Figure 3 As shown in (a), a filler material 21 and a dam material 22 surrounding the filler material 21 are attached to the component 11. The order in which the filler material 21 is attached and the dam material 22 surrounding the filler material 21 is not particularly limited. Furthermore, it is preferable to apply the dam material 22 to the desired position while dispensing it using a dispenser. This facilitates the formation of a dam of the desired shape. Regarding the application of the filler material 21, there are no particular limitations; for example, inkjet printing can be used to apply it in a planar manner within the frame of the dam material 22 (see reference). Figure 2 ).

[0360] Furthermore, the thickness of the dam material 22 and the filling material 21 is not particularly limited as long as it can fully seal the photoelectric conversion element 31 and achieve flatness and thin film properties; for example, it can be set to 5 to 10 μm.

[0361] Component 11 can be configured as a transparent panel that serves as the display surface of a monitor. Examples of transparent panels include glass and transparent resin.

[0362] The filler material 21 applied to component 11 can be further photocured (see reference). Figure 3 (b) That is, after the filler material 21 is activated by irradiation light, the photoelectric conversion element 31 is embedded in the filler material 21 and attached to the member 11 and the member 12, so that the photoelectric conversion element 31 does not need to be irradiated by light for the activation of the filler material 21.

[0363] Ultraviolet light is preferred as the light source. For example, a high-pressure mercury lamp at 100 mW / cm² is preferred. 2 After 30 seconds of exposure to ultraviolet (UV) light, the viscosity 10 minutes later was less than 5 times that before UV irradiation.

[0364] (Embedding process)

[0365] Next, the photoelectric conversion element 31 is embedded in the filling material 21. The embedding method is not particularly limited; for example, ... Figure 3As shown in (c), a photoelectric conversion element 31 can be pre-installed on the component 12, and the surface of the component 12 with the photoelectric conversion element 31 is arranged facing the filling material 21 and the dam material 22, thereby embedding the photoelectric conversion element 31 into the filling material 21. Furthermore, it is preferable to embed the photoelectric conversion element 31 during the period until the filling material 21 irradiated by light is completely cured.

[0366] Furthermore, if the filler material 21 and the dam material 22 are thermosetting, they can also be thermosetting by heating rather than by light irradiation.

[0367] (The process of configuring component 12 (the second component))

[0368] like Figure 3 As shown in (d), component 12 is arranged to cover the filling material 21 and the dam material 22. Thus, component 11 and component 12 are stacked via the photoelectric conversion element 31 embedded in the filling material 21, the filling material 21 and the dam material 22.

[0369] Component 12 may include the same components as component 11. Furthermore, the materials constituting component 12 and component 11 may be the same or different materials.

[0370] As described above, component 12 can be installed simultaneously with the embedding process.

[0371] (The process of curing the filler material)

[0372] Next, the components 11 and 12 are bonded together, and the filler material 21 is cured. For example, the filler material 21 can be cured by heating to 60–200°C. This accelerates the curing speed after light irradiation. From the viewpoint of not damaging the organic electroluminescent element when used for sealing, the heating temperature is preferably 150°C or lower, more preferably 80°C or lower. Furthermore, the post-heating temperature is preferably 60°C or higher.

[0373] The device 100 can be obtained through the steps described above.

[0374] Furthermore, the light source used in the manufacturing method of device 100 is not particularly limited, and examples include halogen lamps, metal halide lamps, high-power metal halide lamps (containing indium, etc.), low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, xenon excimer lamps, xenon flash lamps, and light-emitting diodes (hereinafter referred to as LEDs). From the viewpoint of being able to effectively irradiate the energy line corresponding to the reaction wavelength of each (B) photocationic polymerization initiator, these light sources are preferred.

[0375] The aforementioned light sources each have different radiation wavelengths or energy distributions. Therefore, these light sources can be appropriately selected based on factors such as the reaction wavelength of the photocationic polymerization initiator. Furthermore, natural light (sunlight) can also serve as a reaction initiation light source.

[0376] Irradiation from the aforementioned light source can be achieved through direct illumination, focused illumination based on mirrors or optical fibers, etc. Low-wavelength cutoff filters, hot-wire cutoff filters, cold-light mirrors, etc., can also be used.

[0377] The preferred embodiments of the present invention have been described above, but the present invention is not limited to the above embodiments.

[0378] In the above embodiments, a sealing material for a photoelectric conversion element used in the dam filling method was described, but it can also be configured as follows: comprising (A) a cationic polymerizable compound, (B) a photocationic polymerization initiator and (C) a sensitizer, and in the contact angle measured by the specified step i, the contact angle θa after 15 seconds of liquid contact is 35° or more and 90° or less.

[0379] Furthermore, in the above embodiment, a sealing material for a photoelectric conversion element used in the dam filling method was described, but it can also be configured as follows: comprising (A) a cationic polymerizable compound and (B) a photocationic polymerization initiator, and in the contact angle measured by the specified step i, the contact angle θc after 5 seconds of liquid contact is 30° or less.

[0380] In all cases, the composition exhibits good wettability, thus enabling its application as dam and filler materials in display devices, as sealing materials for light-emitting diode elements (including organic electroluminescent display elements or microLEDs) or solar cells (including perovskite solar cells).

[0381] The embodiments of the present invention have been described above with reference to the accompanying drawings, but these are merely examples of the present invention, and various configurations other than those described above are also possible.

[0382] Example

[0383] Next, the present invention will be described in detail through embodiments, but the content of the present invention is not limited to the embodiments.

[0384] <Invention of the First Embodiment>

[0385] 1. Raw materials for sealing and dam materials used in photoelectric conversion elements

[0386] (A-1) Alicyclic compounds with epoxy groups

[0387] • Alicyclic compound with epoxy group 1: (3,3',4,4'-diepoxy)bicyclohexyl, “CELOXIDE8010”, manufactured by Daicel Corporation

[0388] • Alicyclic compound with epoxy group 2: 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate, "Celloxide 2021P", manufactured by Daicel Chemical Industries, Ltd.

[0389] (A-2) Aromatic compounds with epoxide groups

[0390] • Aromatic compounds with epoxy groups 1: Bisphenol A type epoxy resin, epoxy equivalent 160-170 g / eq, "JER-806", manufactured by Mitsubishi Chemical Corporation

[0391] • Aromatic compounds with epoxy groups 2: Bisphenol A type epoxy resin, epoxy equivalent 184-194 g / eq, "JER-828", manufactured by Mitsubishi Chemical Corporation

[0392] • Aromatic compounds with epoxy groups 3: Phenolic varnish-type multifunctional epoxy resin, epoxy equivalent 184-194 g / eq, “N-775”, manufactured by DIC Corporation

[0393] (A-3) Glycidyl ether compounds

[0394] • Glycidyl ether compound 1: dibromophenyl glycidyl ether, “BR-250H”, manufactured by Nippon Kayaku Co., Ltd.

[0395] • Glycidyl ether compound 2: Tetrabromobisphenol A glycidyl ether, “EPICLON 153”, manufactured by DIC CORPORATION

[0396] • Glycidyl ether compound 3: Phenyl glycidyl ether, "PEG", manufactured by Sakamoto Yakuhin Kogyo Co., Ltd.

[0397] "JP-200"

[0398] • Glycidyl ether compound 4: Epoxidized polybutadiene, “JP-200”, manufactured by Nippon Soda Co., Ltd.

[0399] (B) Photocationic polymerization initiator

[0400] • Photocationic polymerization initiator 1: Triarylsulfonium tetra(pentafluorophenyl)carbamate, “CPI-310FG”, manufactured by San-Apro Ltd.

[0401] • Photocationic polymerization initiator 2: Triarylsulfonium hexafluoroantimonate, “SP-170”, manufactured by ADEKA Corporation

[0402] (C1) sensitizer

[0403] Sensitizer 1: 9,10-Diethoxyanthracene, “DEA”, manufactured by Kawasaki Kasei Kogyo Co., Ltd.

[0404] Sensitizer 2: 2-Hydroxy-2-methylphenylacetone, “DAROCUR1173”, manufactured by BASF Japan Ltd. (formerly Ciba).

[0405] (D) Phosphoric acid compounds

[0406] • Phosphoric acid compound 1: Trioctyl phosphate, “TOP”, manufactured by Daihachi Chemical Industry Co., Ltd.

[0407] (other)

[0408] • Stabilizer: Crown ether (18-crown-6 ether), "O-18", manufactured by Nippon Kayaku Co., Ltd.

[0409] • Silane coupling agents: Epoxy-containing silane coupling agents, γ-epoxypropoxypropyltrimethoxysilane, “KBM-403”, manufactured by Shin-Etsu Chemical Co., Ltd.

[0410] (E) Inorganic packing

[0411] Inorganic filler 1: Molten spherical silica, commercially available.

[0412] • Inorganic filler 2: Flake talc 1, "#5000PA", manufactured by Matsumura Sangyo Co., Ltd.

[0413] Inorganic filler 3: Flake talc 2, "#5000PJ", manufactured by Matsumura Sangyo Co., Ltd.

[0414] 2. Sealing material for photoelectric conversion elements

[0415] The sealing materials for photoelectric conversion elements of the Examples and Comparative Examples were prepared by mixing (A-1) to (A-3), (B), (C1), (D) and other components in the proportions (parts by mass) shown in Table 1 using metal blades (Teflon-processed) as stirring blades in a glass container. The following measurements were performed using the sealing materials for photoelectric conversion elements.

[0416] [Contact Angle]

[0417] Using a sealing material for photoelectric conversion elements, the contact angles over time were measured through step i, and the contact angles θa after 15 seconds of contact and θb after 120 seconds of contact were calculated. Furthermore, a controller was used when creating droplets or removing foam. The results are shown in Table 1.

[0418] (Step i) Alkali-free glass, degreased with acetone and then ozone-cleaned for 15 minutes, was prepared. A syringe containing the sealing material for the photoelectric conversion element was placed in a contact angle meter, and a droplet was prepared under the following condition ii. The contact angle over time was measured by applying the droplet to the prepared alkali-free glass.

[0419] (Condition ii)

[0420] • Measurement method: Changes over time

[0421] • Control method: Standard

[0422] • Analytical methods and techniques: droplet method, θ / 2 method

[0423] • Field of view: Wide angle 2

[0424] Droplet volume: 5 μl

[0425] Furthermore, the following instruments and devices were used in the measurement of the contact angle.

[0426] Alkali-free glass: Lightly beveled Corning Eagle XG (made by Testpiece) 0.7×100×100mm

[0427] • Ozone cleaning device: ASM2001N, manufactured by Asumi Giken, Limited

[0428] • Contact angle measuring device: Dynamic contact angle meter DMo-602, controller DMC-3 (manufactured by Kyowa InterfaceScience Co., Ltd.)

[0429] [Viscosity - 1]

[0430] The viscosity of the photoelectric conversion element was measured using a 0.5 ml sealing material and a CPA-52Z conical plate at 25 °C and 25 rpm. The measurements were performed in air. The results are shown in Table 1.

[0431] 3. Dam materials

[0432] Dam materials were prepared by mixing (A-1) to (A-3), (B), (C1), (D), (E), and other components in the proportions (parts by mass) shown in Table 1 using metal blades (Teflon-processed) as stirring blades in a glass container. The obtained dam materials were then subjected to the following measurements / evaluations.

[0433] [Viscosity - 2]

[0434] The viscosity of the dam material was measured using a 0.5 ml sample and a CPA-52Z conical plate at 25°C and 0.7 rpm. The measurements were conducted in air. The results are shown in Table 1.

[0435] Furthermore, the following apparatus was used in the viscosity measurement.

[0436] • Measuring apparatus: manufactured by BROOKFIELD Corporation

[0437] [evaluate]

[0438] On one side of a 25mm square alkali-free glass substrate, a dam material is applied using a dispenser along a 5mm line from the outer edge to the inner edge of the substrate, and the dam material is arranged in a rectangular frame shape. Next, another 25mm square alkali-free glass substrate is prepared and bonded to the dam material under 0.9MPa air pressure, and then subjected to a high-pressure mercury lamp at 6000mJ / cm². 2 Curing was performed under light curing conditions such as light irradiation. Next, a 1 kg weight was placed in the center of the outermost layer of the substrate, and the dam material was heated and cured at 85°C for 60 minutes to form a dam. The substrates were then fixed together to obtain a substrate with a dam.

[0439] (1) Deviation in dam width

[0440] The width of the dam material was measured when the dam material was arranged in a rectangular frame. Based on the maximum and minimum dam width (mm), the deviation U was calculated using the following formula.

[0441] Deviation U = (maximum value - minimum value) / (maximum value + minimum value)

[0442] (2) The appearance of the dam width

[0443] Furthermore, the appearance of the dam material when it is configured in a rectangular frame shape was evaluated according to the following criteria.

[0444] (Benchmark)

[0445] OK: No ripples or bubbles can be observed at all.

[0446] NG: Ripples and bubbles were observed.

[0447] (3) Preservation of dam width: reliability

[0448] The obtained substrate with the dam was stored at 85°C and 85%RH, and the dam was observed before and after storage. It was evaluated according to the following criteria.

[0449] (Benchmark)

[0450] A: Even after 6 weeks of storage, no delamination was observed at the interface between the dam and the substrate, indicating high reliability.

[0451] B: Even after a week of storage, no delamination was observed at the interface between the dam and the substrate, indicating high reliability.

[0452] C: Delamination was observed at the interface between the dam and the substrate after one week of storage, indicating low reliability.

[0453]

[0454] In Table 1, "*1" indicates that the liquid cannot form droplets properly due to excessively high viscosity.

[0455] <Invention of the Second Embodiment>

[0456] 1. Raw materials for sealing and dam materials used in photoelectric conversion elements

[0457] (A-1) Alicyclic compounds with epoxy groups

[0458] • Alicyclic compound with epoxy group 1: (3,3',4,4'-diepoxy)bicyclohexyl, “CELOXIDE8010”, manufactured by Daicel Corporation

[0459] • Alicyclic compound with epoxy group 2: 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexane carboxylate, "Celloxide 2021P", manufactured by Daicel Chemical Industries, Ltd.

[0460] (A-2) Aromatic compounds with epoxide groups

[0461] • Aromatic compounds with epoxy groups 1: Bisphenol A type epoxy resin, epoxy equivalent 160-170 g / eq, "JER-806", manufactured by Mitsubishi Chemical Corporation

[0462] • Aromatic compounds with epoxy groups 2: Bisphenol A type epoxy resin, epoxy equivalent 184-194 g / eq, "JER-828", manufactured by Mitsubishi Chemical Corporation

[0463] (A-3) Glycidyl ether compounds

[0464] • Glycidyl ether compound 1: dibromophenyl glycidyl ether, “BR-250H”, manufactured by Nippon Kayaku Co., Ltd.

[0465] • Glycidyl ether compound 2: Tetrabromobisphenol A glycidyl ether, “EPICLON 153”, manufactured by DIC Corporation

[0466] (B) Photocationic polymerization initiator

[0467] • Photocationic polymerization initiator 1: Triarylsulfonium tetra(pentafluorophenyl)carbamate, “CPI-310FG”, manufactured by San-Apro Ltd.

[0468] • Photocationic polymerization initiator 2: Triarylsulfonium hexafluoroantimonate, “SP-170”, manufactured by ADEKA Corporation

[0469] • Photocationic polymerization initiator 3: Benzyl (4-hydroxyphenyl)methylsulfonium hexafluoroantimonate, “SI-100”, manufactured by SANSHIN CHEMICAL INDUSTRY CO.,LTD.

[0470] (C2) Reactive diluent

[0471] • Reactive diluent 1:1,6-hexanediol diglycidyl ether, “ED-503G”, manufactured by ADEKA Corporation

[0472] (D) Phosphoric acid compounds

[0473] • Phosphoric acid compound 1: Trioctyl phosphate, “TOP”, manufactured by Daihachi Chemical Industry Co., Ltd.

[0474] (F2) stabilizer

[0475] • Stabilizer 1: Crown ether (18-crown-6 ether), "O-18", manufactured by Nippon Kayaku Co., Ltd.

[0476] • Stabilizer 2: Carboxylic amide, “CDI-4309”, manufactured by King Industries, Inc.

[0477] Stabilizer 3: Diphenyl monodecyl phosphite, “JPM-331”, manufactured by Johoku Chemical Co., Ltd.

[0478] (other)

[0479] • Silane coupling agents: Epoxy-containing silane coupling agents, γ-epoxypropoxypropyltrimethoxysilane, “KBM-403”, manufactured by Shin-Etsu Chemical Co., Ltd.

[0480] 2. Sealing material for photoelectric conversion elements

[0481] The sealing materials for photoelectric conversion elements of the Examples and Comparative Examples were prepared by mixing (A) to (E) and other components in the proportions (parts by mass) shown in Table 2 using metal blades (Teflon-finished) as stirring blades in a glass container. The following measurements were performed using the sealing materials for photoelectric conversion elements.

[0482] [Contact Angle]

[0483] Using a sealing material for photoelectric conversion elements, the contact angles over time were measured through step i, and the contact angles θc after 5 seconds of contact and θd after 30 seconds of contact were calculated. Furthermore, a controller was used when creating droplets or removing foam. The results are shown in Table 1.

[0484] (Step i) Alkali-free glass, degreased with acetone and then ozone-cleaned for 15 minutes, was prepared. A syringe containing the sealing material for the photoelectric conversion element was placed in a contact angle meter, and a droplet was prepared under the following condition ii. The contact angle over time was measured by applying the droplet to the prepared alkali-free glass.

[0485] (Condition ii)

[0486] • Measurement method: Changes over time

[0487] • Control method: Standard

[0488] • Analytical methods and techniques: droplet method, θ / 2 method

[0489] • Field of view: Wide angle 2

[0490] • Droplet volume: 5 μl

[0491] Furthermore, the following instruments and devices were used in the measurement of the contact angle.

[0492] • Alkali-free glass: Lightly beveled Corning Eagle XG (made by Testpiece) 0.7×100×100mm

[0493] • Ozone cleaning device: ASM2001N, manufactured by Asumi Giken, Limited

[0494] • Contact angle measuring device: Dynamic contact angle meter DMo-602, controller DMC-3 (manufactured by Kyowa InterfaceScience Co., Ltd.)

[0495] [Viscosity]

[0496] The viscosity of the photoelectric conversion element was measured using a 0.5 ml sealing material and a CPA-40Z conical plate at 25°C and 50 rpm. The measurements were performed in air. The results are shown in Table 2.

[0497] Furthermore, the following apparatus was used in the viscosity measurement.

[0498] • Measuring apparatus: manufactured by BROOKFIELD

[0499] 3. Evaluation

[0500] [Wetting properties]

[0501] First, a sample was made following these steps.

[0502] (1) Cut the glass plate (alkali-free glass; lightly beveled Corning Eagle XG, Testpiece) into 5cm squares and remove dust and other substances from the surface by degreasing with acetone and blowing with air.

[0503] (2) A dam material is applied to the surface of the glass plate to make it into a 4cm square frame, and a sealing material (filling material) for each photoelectric conversion element, which is made into 16 dots, is applied inside the frame.

[0504] (3) The inorganic glass was configured by covering the dam material and filling material on the glass plate, with the dam material and filling material in between, and the glass plate and the inorganic glass were bonded together in the glove box (dew point -20℃ DP).

[0505] (4) The sample was taken out of the glove box and further pressed with a press (-0.02MPa, 0.1kN, 30s) to obtain the sample.

[0506] Next, the state of the filling material in the obtained samples was observed through inorganic glass and evaluated according to the following evaluation criteria.

[0507] (Evaluation Criteria)

[0508] A: The filler material wets and diffuses evenly (the entire surface of the glass is wetted).

[0509] B: Although the filler material slightly wets and spreads, there is unevenness (a portion of the glass surface has unwetted areas, and multiple unwetted areas were observed).

[0510] C: The filler material was not wetted and diffused (the glass surface was not wetted).

[0511] [reliability]

[0512] First, the organic EL element was fabricated following these steps.

[0513] Each photoelectric conversion element was coated onto glass using a sealing material (filler) under nitrogen atmosphere via a coating device, and then bonded to the organic EL element substrate with a bonding thickness of 10 μm. This process was carried out under a high-pressure mercury lamp at 6000 mJ / cm². 2 Organic EL devices are fabricated by curing them under photocuring conditions such as light irradiation. The cathode side of the organic EL device substrate is then bonded to the glass using a sealing material (filler) via a photoelectric conversion element.

[0514] Next, the freshly fabricated organic EL element was exposed to 85°C and 85% relative humidity for 1000 hours. Then, a 6V voltage was applied for 10 seconds, and the luminescence state of the organic EL element was observed visually and under a microscope. The average diameter (μm) of the dark spot was measured, and the evaluation was carried out according to the following criteria.

[0515] (Benchmark)

[0516] OK: The average diameter (μm) of the dark spot is below 300μm.

[0517] NG: The average diameter (μm) of dark spots exceeds 300 μm.

[0518]

[0519] This application claims priority based on Japanese Patent Application No. 2024-068213, filed on April 19, 2024, and Japanese Patent Application No. 2024-068237, filed on April 19, 2024, the entire contents of which are incorporated herein by reference.

[0520] Symbol Explanation

[0521] 11 components

[0522] 12 components

[0523] 21. Filling material

[0524] 22 Dam Materials

[0525] 31 Photoelectric conversion element

[0526] 100 devices

Claims

1. A sealing material for a photoelectric conversion element, used in a dam filling method, wherein the sealing material for the photoelectric conversion element comprises: (A) cationic polymerizable compounds, (B) photocationic polymerization initiators, and (C) sensitizers. In the contact angles measured through step i below, the contact angle θa after 15 seconds of contact with the liquid is greater than 35° and less than 90°. Step i: Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the sealing material for the photoelectric conversion element into a contact angle meter. Prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass. Condition ii: • Measurement method: Changes over time • Control methods: Standard • Analytical methods and techniques: droplet method, θ / 2 method • Field of view: Wide angle 2 • Droplet volume: 5 μl.

2. The sealing material for photoelectric conversion elements according to claim 1, wherein, In the contact angle measured through step i, the contact angle θb after 120 seconds of contact with the liquid is greater than 12° and less than 32°.

3. The sealing material for photoelectric conversion elements according to claim 2, wherein, The contact angle θa is greater than 1.5 and less than 5.0 relative to the contact angle θb, i.e., θa / θb.

4. The sealing material for a photoelectric conversion element according to any one of claims 1 to 3, wherein, The photoelectric conversion element was sealed with 0.5 ml of material and a CPA-52Z conical plate was used. The viscosity measured at 25°C and 25 rpm was above 2000 mPa·s and below 50000 mPa·s.

5. The sealing material for a photoelectric conversion element according to any one of claims 1 to 4, further comprising (D) a phosphoric acid compound.

6. The sealing material for a photoelectric conversion element according to any one of claims 1 to 5, wherein, (A) The cationic polymerizable compound contains one or more of the following: (A-1) alicyclic compounds having an epoxy group, (A-2) aromatic compounds having an epoxy group, and (A-3) glycidyl ether compounds and their derivatives.

7. The sealing material for a photoelectric conversion element according to any one of claims 1 to 6, further comprising a stabilizer.

8. A dam material comprising a sealing material for a photoelectric conversion element according to any one of claims 1 to 7 and (E) an inorganic filler.

9. The dam material according to claim 8, wherein, (E) The content of inorganic filler is 20 to 300 parts by mass relative to 100 parts by mass of (A) cationic polymeric compound.

10. The dam material according to claim 8 or 9, wherein, The dam material was set to 0.5 ml, and the viscosity measured using a CPA-52Z conical plate at 25°C and 0.7 rpm was above 100,000 mPa·s and below 1,200,000 mPa·s.

11. A solidified body, which is a solidified form of the dam material according to any one of claims 8 to 10.

12. An apparatus comprising a photoelectric conversion element sealed with the dam material as described in any one of claims 8 to 10.

13. The apparatus according to claim 12, wherein, The photoelectric conversion element is an organic electroluminescent element.

14. A method for manufacturing an apparatus, comprising: The process of attaching the filling material and the dam material surrounding the filling material to the first component; The process of embedding the photoelectric conversion element into the filler material; The process of configuring the second component in a manner that covers the filling material and the dam material; and The process of curing the filler material by bonding the first component and the second component together. The dam material is the dam material according to any one of claims 8 to 10.

15. A sealing material for a photoelectric conversion element, used in a dam filling method, the sealing material for the photoelectric conversion element comprising: (A) cationic polymerizable compounds and (B) photocationic polymerization initiators, In the contact angles measured through step i below, the contact angle θc after 5 seconds of contact with the liquid is less than 30°. Step i: Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the sealing material for the photoelectric conversion element into a contact angle meter. Prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass. Condition ii: • Measurement method: Changes over time • Control methods: Standard • Analytical methods and techniques: droplet method, θ / 2 method • Field of view: Wide angle 2 • Droplet volume: 5 μl.

16. The sealing material for a photoelectric conversion element according to claim 15, wherein, In the contact angle measured through step i, the contact angle θd after 30 seconds of contact with the liquid is less than 20°.

17. The sealing material for a photoelectric conversion element according to claim 16, wherein, The contact angle θc is greater than or equal to the contact angle θd, i.e., θc / θd, which is between 1.0 and 2.

3.

18. The sealing material for a photoelectric conversion element according to any one of claims 15 to 17, wherein, The photoelectric conversion element was sealed with 0.5 ml of material and a CPA-40Z conical plate was used. The viscosity measured at 25°C and 50 rpm was above 50 mPa·s and below 1000 mPa·s.

19. The sealing material for a photoelectric conversion element according to any one of claims 15 to 18, further comprising at least one of (C2) a reactive diluent, (D) a phosphoric acid compound, and (F) a stabilizer.

20. The sealing material for a photoelectric conversion element according to any one of claims 15 to 19, wherein, (A) The cationic polymerizable compound contains one or more of the following: (A-1) alicyclic compounds having an epoxy group, (A-2) aromatic compounds having an epoxy group, and (A-3) glycidyl ether compounds and their derivatives.

21. The sealing material for a photoelectric conversion element according to any one of claims 15 to 20, wherein it is used as a filler material.

22. A cured body, which is a cured body of the sealing material for a photoelectric conversion element according to any one of claims 15 to 21.

23. An apparatus comprising a photoelectric conversion element sealed with a sealing material for a photoelectric conversion element according to any one of claims 15 to 21.

24. The apparatus according to claim 23, wherein, The photoelectric conversion element is an organic electroluminescent element.

25. A method for manufacturing an apparatus, comprising: The process of attaching the filling material and the dam material surrounding the filling material to the first component; The process of embedding the photoelectric conversion element into the filler material; The process of configuring the second component in a manner that covers the filling material and the dam material; and The process of curing the filler material by bonding the first component and the second component together. The filling material is the sealing material for the photoelectric conversion element according to any one of claims 15 to 21.

26. A polymerizable composition, wherein, In the contact angles measured over time through the following steps i, the contact angle θa after 15 seconds of contact with the liquid is greater than 35° and less than 90°. Step i: Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the polymeric composition into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass. Condition ii: • Measurement method: Changes over time • Control methods: Standard • Analytical methods and techniques: droplet method, θ / 2 method • Field of view: Wide angle 2 • Droplet volume: 5 μl.

27. A polymerizable composition, wherein, In the contact angles measured over time using the following steps (i), the contact angle θc after 5 seconds of contact with the liquid is less than 30°. Step i: Prepare alkali-free glass that has been degreased with acetone and then ozone-cleaned for 15 minutes. Place a syringe containing the polymeric composition into a contact angle meter, prepare a droplet under the following condition ii, and measure the contact angle over time by applying the droplet to the prepared alkali-free glass. Condition ii: • Measurement method: Changes over time • Control methods: Standard • Analytical methods and techniques: droplet method, θ / 2 method • Field of view: Wide angle 2 • Droplet volume: 5 μl.

Citation Information

Patent Citations

  • Thermosetting liquid composition for sealing material of organic light emitting element

    JP2023024361A

  • Gift box event for live streamers and viewers

    JP2024068213A

  • Chemical pre-stressed concrete and production method of chemical pre-stressed concrete

    JP2024068237A

  • Sealing composition

    WO2017094809A1

  • Sealing composition

    WO2017099055A1