A grain-boundary junction film, a method for manufacturing the same, a cut grain-boundary junction integrated film, a method for manufacturing the same, and a semiconductor device and a method for manufacturing the same

By introducing surface-treated silver-containing particles and specific compounds into the grain bonding film, combined with materials such as thermosetting resins, the problem of insufficient heat dissipation in semiconductor devices is solved, realizing a grain bonding film with high thermal conductivity and good adhesion, as well as an integrated film for cutting and bonding grains, suitable for power semiconductor devices.

CN123147290APending Publication Date: 2026-11-20RESONAC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202580029748.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-21
Filing Date
2025-06-18
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Semiconductor devices manufactured using existing die bonding films and die-cutting and die bonding integrated films do not have sufficient heat dissipation.

Method used

By introducing silver-containing particles treated with a surface treatment agent and a specific compound into a grain bonding film, combined with a thermosetting resin, a curing agent and an elastomer, a grain bonding film with high thermal conductivity is prepared, and then combined with a cutting tape to form a cutting grain bonding integrated film.

Benefits of technology

It significantly improves the heat dissipation of semiconductor devices, ensuring better thermal conductivity and adhesion, and is suitable for the heat dissipation requirements of power semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123147290A_ABST
    Figure CN123147290A_ABST
Patent Text Reader

Abstract

A crystal grain bonding film is disclosed. The crystal grain bonding film contains silver-containing particles produced by a reduction method and a compound represented by formula (1). The content of the silver-containing particles is 70% by mass or more based on the total amount of the crystal grain bonding film. In formula (1), R 1 , R 2 , R 3 , and R 4 independently represent a hydrogen atom, a halogen atom, a methyl group which can be substituted with a halogen atom, or an ethyl group which can be substituted with a halogen atom, wherein at least one of R 1 , R 2 , R 3 , and R 4 is a halogen atom, a methyl group which can be substituted with a halogen atom, or an ethyl group which can be substituted with a halogen atom.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a grain bonding film and its manufacturing method, a grain-cutting and bonding integrated film and its manufacturing method, and a semiconductor device and its manufacturing method. Background Technology

[0002] Conventionally, semiconductor devices are manufactured through the following processes. First, a semiconductor wafer is attached to a pressure-sensitive adhesive sheet for dicing, and in this state, the semiconductor wafer is monolithically formed into a semiconductor chip (dicing process). Afterwards, ultraviolet irradiation, pick-up, pressing, and die bonding processes are performed. Patent Document 1 discloses an adhesive pressure-sensitive adhesive sheet (dicing and die bonding integrated film) that combines the functions of fixing the semiconductor wafer in the dicing process and bonding the semiconductor chip to the substrate in the die bonding process. In the dicing process, by monolithically forming the semiconductor wafer and the adhesive layer, a chip with an adhesive layer can be obtained.

[0003] In recent years, devices called power semiconductor devices, which are used for power control and other applications, have become widespread. Power semiconductor devices are prone to generating heat due to the current they receive, thus requiring excellent heat dissipation. Patent Document 2 discloses a conductive grain bonding film with higher heat dissipation after curing than before curing, and a cutting tape with the grain bonding film (cutting grain bonding integrated film).

[0004] Previous technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2008-218571 Patent Document 2: Japanese Patent No. 6396189 Summary of the Invention

[0005] The technical problem to be solved by the invention However, the heat dissipation of semiconductor devices manufactured using conventional die bonding films and die-cutting and bonding integrated films is insufficient and there is still room for improvement.

[0006] Therefore, the object of the present invention is to provide a die bonding film and a die-cutting and bonding integrated film capable of manufacturing semiconductor devices with excellent heat dissipation.

[0007] means for solving technical problems In order to solve the above-mentioned problems, the inventors conducted in-depth research and found that by including silver-containing particles that have been surface-treated with a surface treatment agent and a specified compound in the grain bonding film, the thermal conductivity of the grain bonding film is improved, thereby completing the present invention.

[0008] The present invention provides a method for manufacturing the grain bonding film described in [1] to [7], a method for manufacturing the integrated grain-cutting bonding film described in [8], a method for manufacturing the semiconductor device described in [9], the grain bonding film described in

[10] to

[12] , the integrated grain-cutting bonding film described in

[13] , and the semiconductor device described in

[14] .

[0009] [1] A method for manufacturing a grain bonding film, comprising: The first step involves preparing a raw material varnish containing silver particles manufactured by reduction, a compound represented by formula (1), and an organic solvent; In the second step, the raw material varnish is mixed to obtain an adhesive varnish; and In the third step, the adhesive varnish is applied to the support film, and the organic solvent is removed, thereby obtaining a grain-bonded film. The content of the silver particles is 70% by mass or more, based on the total solid content of the adhesive varnish.

[0010] In equation (1), R 1 R 2 R 3 and R 4 Each can be independently represented by a hydrogen atom, a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom. Among them, R 1 R 2 R 3 and R 4 At least one of them is a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom.

[0011] [2] A method for manufacturing a grain bonding film, comprising: The first step involves preparing a raw material varnish containing silver particles that have been surface-treated with a surface treatment agent, a compound represented by formula (1), and an organic solvent; In the second step, the raw material varnish is mixed to obtain an adhesive varnish; and In the third step, the adhesive varnish is applied to the support film, and the organic solvent is removed, thereby obtaining a grain-bonded film. The content of the silver particles is 70% by mass or more, based on the total solid content of the adhesive varnish.

[0012] In equation (1), R 1 R 2 R 3 and R 4Each can be independently represented by a hydrogen atom, a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom. Among them, R 1 R 2 R 3 and R 4 At least one of them is a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom.

[0013] [3] The method for manufacturing a grain bonding film according to [1] or [2], wherein, The second step is to mix the raw material varnish at a temperature of 50°C or higher.

[0014] [4] The method for manufacturing a grain bonding film according to any one of [1] to [3], wherein, The raw material varnish further contains thermosetting resin, curing agent and elastomer.

[0015] [5] According to the method for manufacturing the grain bonding film described in [4], wherein, The thermosetting resin includes epoxy resin, which is liquid at 25°C.

[0016] [6] A method for manufacturing a grain bonding film according to any one of [1] to [3], wherein, The second step is to add thermosetting resin, curing agent and elastomer to the mixed raw material varnish to obtain a binder varnish containing them.

[0017] [7] According to the method for manufacturing the grain bonding film described in [6], wherein, The thermosetting resin includes epoxy resin, which is liquid at 25°C.

[0018] [8] A method for manufacturing a grain-cutting and bonding integral film, comprising the following steps: Prepare a cutting tape having a substrate layer and a pressure-sensitive adhesive layer disposed on the substrate layer; and A grain bonding film manufactured by any one of the manufacturing methods of [1] to [7] is bonded to the pressure-sensitive adhesive layer of the cut tape to form an adhesive layer formed by the grain bonding film on the pressure-sensitive adhesive layer.

[0019] [9] A method for manufacturing a semiconductor device, comprising the following steps: The adhesive layer of the die-cutting bonded integral film manufactured by the manufacturing method of the die-cutting bonded integral film described in [8] is attached to the semiconductor wafer; Monolithize the semiconductor wafer and the adhesive layer; Pick up the semiconductor chip with adhesive layer from the cutting tape; and The semiconductor chip with the adhesive layer is bonded to the support component by means of the adhesive layer.

[0020]

[10] A grain bonding film containing silver-containing particles manufactured by a reduction method and a compound represented by formula (1), The content of silver particles is 70% by mass or more, based on the total amount of the grain bonding film.

[0021] In equation (1), R 1 R 2 R 3 and R 4 Each can be independently represented by a hydrogen atom, a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom. Among them, R 1 R 2 R 3 and R 4 At least one of them is a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom.

[0022]

[11] The grain bonding film according to

[10] further contains a thermosetting resin, a curing agent and an elastomer.

[0023] As described in

[11] , a grain bonding film, wherein, The thermosetting resin includes epoxy resin, which is liquid at 25°C.

[0024]

[13] A grain-cutting and bonding integrated film, comprising: A cutting tape having a substrate layer and a pressure-sensitive adhesive layer disposed on the substrate layer; and An adhesive layer disposed on the pressure-sensitive adhesive layer of the cut tape and formed of any one of

[10] to

[12] .

[0025]

[14] A semiconductor device comprising: Semiconductor chips; Support component, housing the semiconductor chip; and An adhesive component is disposed between the semiconductor chip and the support component to bond the semiconductor chip and the support component. The adhesive component comprises a cured grain bonding film as described in any one of

[10] to

[12] .

[0026] Invention Effects According to the present invention, a die bonding film and a die-cutting and die-bonding integral film capable of manufacturing semiconductor devices with excellent heat dissipation are provided. Furthermore, according to the present invention, a method for manufacturing the latter is provided. Moreover, according to the present invention, a semiconductor device using such a die bonding film and a method for manufacturing a semiconductor device using a die-cutting and die-bonding integral film are provided. Attached Figure Description

[0027] Figure 1 This is a schematic cross-sectional view showing one embodiment of the grain bonding film.

[0028] Figure 2 This is a schematic cross-sectional view illustrating one embodiment of a grain-jointed integral film.

[0029] Figure 3 This is a schematic cross-sectional view illustrating one embodiment of a method for manufacturing a semiconductor device. Figure 3 (a), (b), (c), (d), (e), and (f) are schematic cross-sectional views representing each process.

[0030] Figure 4 This is a schematic cross-sectional view illustrating one embodiment of a semiconductor device. Detailed Implementation

[0031] Hereinafter, embodiments of the present invention will be described with appropriate reference to the accompanying drawings. However, the present invention is not limited to the following embodiments. In the following embodiments, except as specifically stated, the constituent elements (including steps, etc.) are not essential. The sizes of the constituent elements in each figure are conceptual sizes, and the relative sizes between the constituent elements are not limited to the relationships shown in the figures.

[0032] The numerical values ​​and their ranges used in this specification are the same and do not limit the invention. In this specification, the numerical range indicated by "~" represents the range encompassed by the values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper or lower limit value described in one numerical range can be replaced by the upper or lower limit value of other numerical ranges described in stages. Furthermore, the upper or lower limit value of the numerical ranges described in this specification can also be replaced by the values ​​shown in the embodiments.

[0033] In this specification, "(meth)acrylate" refers to at least one of acrylate and its corresponding methacrylate. The same applies to other similar expressions such as "(meth)acryloyl". Furthermore, "(poly)" refers to both the case with and without the prefix "poly". "A or B" may include either A or B, or both. Moreover, unless otherwise specified, the materials exemplified below may be used individually or in combination of two or more. Regarding the content of each component in the composition, in the case where multiple substances corresponding to each component are present in the composition, unless otherwise specified, the total amount of the multiple substances present in the composition is indicated.

[0034] [Grain bonding film] Figure 1 This is a schematic cross-sectional view illustrating one embodiment of the grain-bonding film. (e.g.) Figure 1 As shown, Figure 1 The grain bonding film 10A shown can be disposed on the support film 20. The grain bonding film 10A is thermosetting, and after a semi-cured (B-stage) state, it can become a cured (C-stage) state.

[0035] The grain bonding film 10A contains silver-containing particles manufactured by reduction or coated silver-containing particles that have been surface-treated with a surface treatment agent (component (a)) and a compound represented by formula (1) (component (b)). The grain bonding film 10A may further contain a thermosetting resin (component (c)), a curing agent (component (d)) and an elastomer (component (e)) as needed.

[0036] (a) Composition: Silver-containing particles manufactured by reduction method or (coated) silver-containing particles that have undergone surface treatment with a surface treatment agent. (a) The component is used to improve the thermal conductivity of the grain bonding film and to improve the heat dissipation of the semiconductor device. The silver particles can be, for example, particles composed of silver (particles composed solely of silver, silver particles) or silver-coated metal particles obtained by coating the surface of metal particles (copper particles, etc.) with silver. Examples of silver-coated metal particles include, for example, silver-coated copper particles. (a) The component can also be particles composed of silver (silver particles).

[0037] (a) The composition may be silver particles manufactured by reduction (silver particles manufactured by liquid-phase (wet) reduction using a reducing agent). In liquid-phase (wet) reduction using a reducing agent, a surface treatment agent (lubricant) is usually added from the viewpoint of controlling particle size and preventing agglomeration-welding, so that the silver particles manufactured by liquid-phase (wet) reduction using a reducing agent are surface-treated (coated) by the surface treatment agent (lubricant). That is, silver particles (containing silver particles) manufactured by reduction are usually surface-treated by a surface treatment agent (lubricant). Surface treatment agents may include fatty acid compounds such as oleic acid (melting point: 13.4℃), myristic acid (melting point: 54.4℃), palmitic acid (melting point: 62.9℃), and stearic acid (melting point: 69.9℃); fatty acid amide compounds such as oleamide (melting point: 76℃) and stearamide (melting point: 100℃); aliphatic alcohol compounds such as pentanol (melting point: -78℃), hexanol (melting point: -51.6℃), oleyl alcohol (melting point: 16℃), and stearyl alcohol (melting point: 59.4℃); and aliphatic nitrile compounds such as oleoyl nitrile (melting point: -1℃). Surface treatment agents may be those with low melting points (e.g., below 100℃) and high solubility in organic solvents, such as fatty acid compounds. That is, component (a) may be (coated) silver particles (containing silver particles) that have been surface-treated using a fatty acid compound.

[0038] (a) The shape of the component is not particularly limited; for example, it can be in the form of flakes, plates, needles, spheres, etc. When the shape of (a) component is spherical, it tends to easily obtain a grain-bonded film with improved surface roughness (Ra).

[0039] The average particle size of component (a) can be 0.01 to 10 μm. When the average particle size of component (a) is 0.01 μm or more, it tends to: prevent viscosity increase during the preparation of adhesive varnish, enable the die bonding film to contain the desired amount of component (a), and ensure the wettability of the die bonding film to the adherend, resulting in better adhesion. When the average particle size of component (a) is 10 μm or less, it tends to have better film formability and improve thermal conductivity by adding component (a), thereby improving the heat dissipation of the semiconductor device. Furthermore, by setting it to this range, it tends to: further reduce the thickness of the die bonding film, thereby enabling high-layer semiconductor chip stacking, and prevent the generation of chip cracks caused by conductive particles protruding from the die bonding film. (a) The average particle size of the component may be greater than 0.1 μm, greater than 0.5 μm or greater than 1.0 μm, and may be less than 8.0 μm, less than 5.0 μm or less than 3.0 μm.

[0040] In this specification, the average particle size of component (a) refers to the particle size at which the ratio (volume fraction) of component (a) to the total volume of component (a) is 50% (laser 50% particle size (D) 50 Average particle size (D) 50 The particle size distribution can be determined by using a laser scattering particle size analyzer (e.g., Microtrac) and by using laser scattering to measure the suspension obtained by suspending component (a) in water.

[0041] The content of component (a) is 70% by mass or more based on the total amount of the grain bonding film (or the total amount of solid components of the adhesive varnish described later). When the content of component (a) is 70% by mass or more based on the total amount of the grain bonding film, the thermal conductivity of the grain bonding film can be improved, resulting in improved heat dissipation. The content of component (a) can be 72% by mass or more, 74% by mass or more, or 75% by mass or more based on the total amount of the grain bonding film. There is no particular upper limit to the content of component (a), which can be 90% by mass or less, 85% by mass or less, or 80% by mass or less based on the total amount of the grain bonding film. When the content of component (a) is 90% by mass or less based on the total amount of the grain bonding film, the grain bonding film can contain more of the other components. This ensures the wettability of the grain bonding film to the adhered object, resulting in better adhesion.

[0042] The content of component (a) can be 24.0% by volume or more, 24.5% by volume or more, or 25.0% by volume or more, based on the total amount (total volume) of the grain bonding film. When the content of component (a) is 24.0% by volume or more, based on the total amount (total volume) of the grain bonding film, the thermal conductivity of the grain bonding film can be improved, resulting in improved heat dissipation of the semiconductor device. The content of component (a) can be 33.0% by volume or less, 30.0% by volume or less, or 28.0% by volume or less, based on the total amount (total volume) of the grain bonding film. When the content of component (a) is 33.0% by volume or less, based on the total amount (total volume) of the grain bonding film, the grain bonding film can contain other components more fully. This ensures the wettability of the grain bonding film to the adherend, resulting in better adhesion.

[0043] For example, let the density of the grain-bonded film be x (g / cm³). 3 Let the density of component (a) be y (g / cm³). 3When the mass proportion of component (a) in the grain bonding film is set as z (mass%), the content (volume%) of component (a) can be calculated using the following formula (I). Furthermore, the mass proportion of component (a) in the grain bonding film can be determined, for example, by performing thermogravimetric analysis using a differential thermogravimetric analysis (TG-DTA) apparatus. Moreover, the densities of the grain bonding film and component (a) can be determined by measuring their mass and specific gravity using a hydrometer.

[0044] (a) Content of component (volume %) = (x / y) × z (I) Measurement conditions for TG-DTA: temperature range 30–600℃ (heating rate 30℃ / min), maintained at 600℃ for 20 minutes. Air flow rate: 300 mL / min Thermogravimetric Differential Thermal Analysis Apparatus: Manufactured by Seiko Instruments Inc., TG / DTA220 Hydrometer: Manufactured by ALFA MIRAGE CO.,LTD., EW-300SG (b) Components: Compounds represented by formula (1) The grain bonding film 10A contains component (b). By containing components (a) and (b) in the grain bonding film, the thermal conductivity of the grain bonding film can be improved, thereby improving the heat dissipation of the semiconductor device.

[0045] In equation (1), R 1 R 2 R 3 and R 4 Each can be independently represented by a hydrogen atom, a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom.

[0046] Examples of halogen atoms include, for example, fluorine, chlorine, bromine, and iodine atoms.

[0047] A methyl group that can be substituted by a halogen atom refers to an unsubstituted methyl group or a methyl group in which at least one of the hydrogen atoms of a methyl group is substituted by a halogen atom. Examples of methyl groups substituted by halogen atoms include fluoromethyl, chloromethyl, bromomethyl, iodomethyl, difluoromethyl, trifluoromethyl, etc.

[0048] An ethyl that can be substituted by a halogen atom refers to an unsubstituted ethyl or an ethyl in which at least one hydrogen atom of the ethyl is substituted by a halogen atom. Examples of ethyls substituted by halogen atoms include fluoroethyl, chloroethyl, bromoethyl, iodoethyl, 1,1-difluoroethyl, 2,2-difluoroethyl, 2,2,2-trifluoroethyl, perfluoroethyl, etc.

[0049] R1 R 2 R 3 and R 4 At least one of them is a halogen atom, a methyl group that can be substituted with a halogen atom, or an ethyl group that can be substituted with a halogen atom. Among these, R 1 R 2 R 3 and R 4 At least one of them can be methyl. 1 R 2 R 3 and R 4 In this context, the number of halogen atoms, methyl groups that can be substituted by halogen atoms, and ethyl groups that can be substituted by halogen atoms can be one. That is, R 1 R 2 R 3 and R 4 One of them can be a halogen atom, a methyl group that can be substituted with a halogen atom, or an ethyl group that can be substituted with a halogen atom, R 1 R 2 R 3 and R 4 The other three can be hydrogen atoms.

[0050] Examples of compounds represented by formula (1) that satisfy this condition include 2-methylglutaric acid, 2-ethylglutaric acid, 2-fluoroglutaric acid, 2-chloroglutaric acid, 2-bromoglutaric acid, 2-iodoglutaric acid, 2-(trifluoromethyl)glutaric acid, 2-(difluoromethyl)glutaric acid, 2-(chloromethyl)glutaric acid, 2-(fluoromethyl)glutaric acid, 2-(dichloromethyl)glutaric acid, 2-(trichloromethyl)glutaric acid, 2-(2-fluoroethyl)glutaric acid, 2-(2,2,2-trifluoroethyl)glutaric acid, 2-(2-chloroethyl)glutaric acid, and 2-(2,2-difluoroethyl)glutaric acid. Among these, the compounds represented by formula (1) may include 2-methylglutaric acid.

[0051] When the total amount of component (a) is set to 100 parts by mass, the content of component (b) can be 0.1 to 5 parts by mass. When the total amount of component (a) is set to 100 parts by mass, if the content of component (b) is 0.1 parts by mass or more, there is a tendency to further improve the thermal conductivity of the grain-bonded film. When the total amount of component (a) is set to 100 parts by mass, if the content of component (b) is 5 parts by mass or less, there is a tendency to ensure sufficient amounts of other components (especially components (c), (d), and (e)) while achieving excellent film formation properties.

[0052] (b) The content of the component is based on the total amount of the grain bonding film (or the total amount of solid components of the adhesive varnish described below), and may be more than 0.2% by mass or more than 0.3% by mass, and may be less than 3% by mass or less than 2% by mass.

[0053] (c) Composition: Thermosetting resin (c) The component is one that has the property of forming three-dimensional bonds between molecules and curing by heating or the like, and exhibits adhesive properties after curing. (c) The component may be an epoxy resin. (c) The component may contain epoxy resin that is liquid at 25°C. Epoxy resins can be used without particular restrictions as long as they have epoxy groups within their molecules. Epoxy resins may have two or more epoxy groups within their molecules.

[0054] Examples of epoxy resins include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenolic varnish type epoxy resin, cresol varnish type epoxy resin, bisphenol A varnish type epoxy resin, bisphenol F varnish type epoxy resin, stilbene type epoxy resin, triazine-containing skeleton epoxy resin, benzoylene-containing skeleton epoxy resin, triphenol-methane type epoxy resin, biphenyl type epoxy resin, xylylene type epoxy resin, biphenyl aralkyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, polyfunctional phenols, anthracene, and other polycyclic aromatic diglycidyl ether compounds. Among these, from the viewpoint of the heat resistance of the cured product, the epoxy resin can be either a bisphenol type epoxy resin or a cresol varnish type epoxy resin.

[0055] Epoxy resins can include epoxy resins that are liquid at 25°C (hereinafter, sometimes simply referred to as "liquid epoxy resins"). By including such liquid epoxy resins, there is a tendency to easily obtain grain-bonded films with improved surface roughness (Ra). Commercially available examples of liquid epoxy resins include, for example, EXA-830CRP (product name, manufactured by DIC Corporation) and YDF-8170C (product name, manufactured by NIPPON STEEL Chemical & Material Co., Ltd.).

[0056] There is no particular limitation on the epoxy equivalent of the epoxy resin, which can be 90–300 g / eq or 110–290 g / eq. When the epoxy equivalent of the epoxy resin is within this range, it tends to maintain the bulk strength of the grain-bonded film while easily ensuring the flowability of the adhesive composition when forming the grain-bonded film.

[0057] (c) The content of the component is based on the total amount of the grain bonding film (or the total amount of solid components of the adhesive varnish described below), and may be more than 1% by mass, more than 3% by mass, or more than 5% by mass, and may be less than 15% by mass, less than 12% by mass, or less than 10% by mass.

[0058] When component (c) contains liquid epoxy resin, the mass ratio of the amount of liquid epoxy resin to the total amount of component (c) (amount of liquid epoxy resin (mass) / total amount of component (c) (total mass)) can be more than 20%, more than 30%, more than 40% or more than 50%, and can be less than 100%, less than 90%, less than 80% or less than 70%.

[0059] (d) Ingredients: Curing agent (d) The component can be a phenolic resin that can serve as a curing agent for epoxy resins. Phenolic resins can be used without particular restriction as long as they possess phenolic hydroxyl groups within their molecules. Examples of phenolic resins include phenolic varnish-type phenolic resins obtained by condensing or co-condensing phenolic compounds such as phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthol with aldehyde-containing compounds such as formaldehyde under an acidic catalyst; phenolic aralkyl resins synthesized from allylated bisphenol A, allylated bisphenol F, allylated naphthalene glycol, phenolic varnish, phenol, and / or naphthols with dimethoxy-p-xylene or bis(methoxymethyl)biphenyl; naphthol aralkyl resins; biphenyl aralkyl-type phenolic resins; and phenyl aralkyl-type phenolic resins.

[0060] The hydroxyl equivalent of phenolic resin can be 40–300 g / eq, 70–290 g / eq, or 100–280 g / eq. When the hydroxyl equivalent of phenolic resin is above 40 g / eq, it tends to further increase the storage modulus of the membrane; when it is below 300 g / eq, it can prevent defects caused by foaming, degassing, etc.

[0061] From the viewpoint of curability, the ratio of the epoxy equivalent of the epoxy resin as component (c) to the hydroxyl equivalent of the phenolic resin as component (d) (epoxy equivalent of epoxy resin as component (c) / hydroxyl equivalent of phenolic resin as component (d)) can be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40, or 0.45 / 0.55 to 0.55 / 0.45. When this equivalent ratio is 0.30 / 0.70 or higher, there is a tendency to obtain more sufficient curability. When this equivalent ratio is 0.70 / 0.30 or lower, it is possible to prevent the viscosity from becoming too high and to obtain more sufficient flowability.

[0062] (d) The content of the component is based on the total amount of the grain bonding film (or the total amount of solid components of the adhesive varnish described later), and can be more than 1% by mass, more than 3% by mass, or more than 5% by mass, and can be less than 15% by mass, less than 12% by mass, or less than 10% by mass.

[0063] (e) Component: Elastomer As component (e), examples include acrylic resins (including acrylate rubbers), urethane resins (including urethane rubbers), silicone resins (including silicone rubbers), and styrene-based elastomers. Component (e) can be one of these resins, which can be either a resin having crosslinking functional groups or an acrylic resin having crosslinking functional groups. Here, acrylic resin refers to a polymer containing constituent units derived from (meth)acrylates. Acrylic resin can be a polymer whose constituent units include (meth)acrylates having crosslinking functional groups such as epoxy groups, alcoholic hydroxyl groups, phenolic hydroxyl groups, or carboxyl groups. Furthermore, acrylic resin can also be an acrylate rubber, such as a copolymer of (meth)acrylate and acrylonitrile.

[0064] Commercially available acrylic resins include, for example, SG-P3, SG-70L, SG-708-6, WS-023 EK30, and SG-280 EK23 (all manufactured by Nagase ChemteX Corporation).

[0065] (e) The glass transition temperature (Tg) of component (e) can be -50 to 50°C or -30 to 20°C. When the Tg of the acrylic resin is above -50°C, the viscosity of the grain-bonded film decreases, thus tending to further improve workability. When the Tg of the acrylic resin is below 50°C, there is a tendency to more adequately ensure the flowability of the adhesive composition when forming the grain-bonded film. Here, the (Tg) of component (e) refers to the value measured using a DSC (Differential Scanning Calorimeter) (e.g., manufactured by Rigaku Corporation, product name: Thermo Plus 2).

[0066] (e) The weight-average molecular weight (Mw) of component (e) can be 50,000 to 1.6 million, 100,000 to 1.4 million, or 300,000 to 1.2 million. When the Mw of component (e) is above 50,000, it tends to have better film-forming properties. When the Mw of component (e) is below 1.6 million, it tends to have better flowability of the adhesive composition when forming a grain-bonded film. In addition, Mw is a value determined by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene.

[0067] (e) The apparatus and conditions for measuring the Mw of the component are as follows.

[0068] Pump: L-6000 (manufactured by Hitachi, Ltd.) Tube Column: A tube column consisting of Gelpack GL-R440 (manufactured by Resonac Holdings Corporation), Gelpack GL-R450 (manufactured by Resonac Holdings Corporation), and Gelpack GL-R400M (manufactured by Resonac Holdings Corporation) (each 10.7mm (diameter) × 300mm) connected in sequence. Eluent: Tetrahydrofuran (hereinafter referred to as "THF"). Sample: The solution obtained by dissolving 120 mg of the sample in 5 mL of THF. Flow rate: 1.75 mL / min (e) The content of the component is based on the total amount of the grain bonding film (or the total amount of solid components of the adhesive varnish described later), and may be more than 1% by mass, more than 3% by mass, or more than 5% by mass, and may be less than 15% by mass, less than 12% by mass, or less than 10% by mass.

[0069] (f) Ingredients: Curing accelerator The grain bonding film 10A may further contain a curing accelerator (component (f)). By containing component (f) in the grain bonding film, there is a tendency to balance adhesion and bonding reliability. Examples of component (f) include, for example, imidazoles and their derivatives, organophosphorus compounds, secondary amines, tertiary amines, quaternary ammonium salts, etc. Among these, from a reactivity point of view, component (f) can be imidazoles and their derivatives.

[0070] Examples of imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole.

[0071] The content of component (f) is based on the total amount of the grain bonding film (or the total amount of solid components of the adhesive varnish described later), and can be 0.001 to 1% by mass. When the content of component (f) is within this range, it tends to balance adhesion and connection reliability.

[0072] The grain-bonding film 10A may further contain coupling agents, antioxidants, rheology control agents, leveling agents, etc., in addition to components (a) to (f). Examples of coupling agents include 3-ureopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane. The content of other components, based on the total amount of the grain-bonding film, may be 0.01 to 3% by mass.

[0073] [Method for manufacturing grain bonding film] Figure 1 The grain bonding film 10A shown can be obtained by a method comprising the following steps: a first step, preparing a raw material varnish containing (a) component (silver-containing particles manufactured by reduction method or silver-containing particles surface-treated with a surface treatment agent), (b) component and organic solvent; a second step, mixing the raw material varnish to obtain an adhesive varnish; and a third step, applying the adhesive varnish to a support film and removing the organic solvent, thereby obtaining the grain bonding film.

[0074] The first step is to prepare a raw material varnish containing (a) component (silver particles manufactured by reduction or silver particles that have been surface-treated using a surface treatment agent), (b) component, and an organic solvent.

[0075] There are no particular limitations on the organic solvent as long as it can dissolve the components other than (a). Examples of organic solvents include aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-isopropyltoluene; aliphatic hydrocarbons such as hexane and heptane; cyclic alkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; and amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. Among these, from the viewpoint of solubility and boiling point, the organic solvent can be toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, or cyclohexanone. The concentration of solid components in the raw material varnish is based on the total amount of the raw material varnish and can be 10 to 80% by mass.

[0076] Raw material varnishes can be obtained, for example, by adding the various components to a container used in a mixer. In this case, there are no particular restrictions on the order of addition of the components, and it can be appropriately set according to the properties of each component.

[0077] The second step is to mix the raw material varnish to obtain the adhesive varnish.

[0078] Regarding mixing, common mixers such as homogenizers, three-in-one motors, agitators, planetary mixers, and pounders can be appropriately combined. The mixers can be equipped with heating devices such as heater units capable of managing the temperature of the raw material varnish (or adhesive varnish). When using a homogenizer for mixing, the homogenizer's rotational speed can be 4000 rpm or higher.

[0079] The second step can be a process of mixing the raw material varnish at a temperature above 50°C. The mixing temperature can be adjusted as needed using heating equipment, heat preservation equipment, etc. When the mixing temperature is above 50°C, for example, the resulting grain-bonded film easily forms a sintered body of component (a) in the cured product (C-stage) state after curing treatment, which can further improve the thermal conductivity of the grain-bonded film. The mixing temperature can be above 55°C, above 60°C, above 65°C, or above 70°C. The upper limit of the mixing temperature can be, for example, below 120°C, below 110°C, below 100°C, below 90°C, or below 80°C. The mixing time can be, for example, more than 1 minute, more than 5 minutes, more than 10 minutes, or more than 20 minutes, and can be less than 80 minutes, less than 60 minutes, or less than 40 minutes.

[0080] Regarding components (c), (d), (e), (f), and others, these components can be independently included in the raw material varnish or adhesive varnish at any stage, depending on their properties. For example, it can be done as follows: in step 1, a raw material varnish further containing these components is prepared; in step 2, the raw material varnish is mixed to obtain an adhesive varnish containing components (a), (b), (c), (d), (e), (f), and others. Furthermore, it can be done as follows: in step 1, a raw material varnish is prepared; in step 2, the raw material varnish is mixed and these components are added to the mixed raw material varnish, thereby obtaining an adhesive varnish containing components (a), (b), (c), (d), (e), (f), and others. Furthermore, for example, it can be done as follows: In the first step, a raw material varnish further containing components (c) and (d) is prepared; in the second step, the raw material varnish is mixed and components (e), (f), and other components are added to the mixed raw material varnish, thereby obtaining an adhesive varnish containing components (a), (b), (c), (d), (e), (f), and other components. When at least one component selected from the group consisting of components (c), (d), (e), (f), and other components is added to the mixed raw material varnish in the second step, mixing can be carried out after the addition of the component, for example, at a temperature condition below 50°C (e.g., room temperature (25°C)). Regarding the mixing conditions in this case, mixing can be carried out at room temperature (25°C) for 0.1 to 48 hours.

[0081] In this way, an adhesive varnish containing the specified components can be obtained. The resulting adhesive varnish can be degassed using methods such as vacuum degassing to remove air bubbles.

[0082] (a) The content of the component is 70% by mass or more, based on the total solid content of the adhesive varnish. In this specification, the solid content of the adhesive varnish refers to the total amount of components other than organic solvents. (a) The content of the component, based on the total solid content of the adhesive varnish, can be 72% by mass or more, 74% by mass or more, or 75% by mass or more, and can be 90% by mass or less, 85% by mass or less, or 80% by mass or less.

[0083] The third step is to obtain the grain bonding film 10A by applying an adhesive varnish to the support film 20 and removing the organic solvent.

[0084] There are no particular limitations on the support film 20; for example, films made of polytetrafluoroethylene, polyethylene, polypropylene, polymethylpentene, polyethylene terephthalate, and polyimide can be used. The support film can be demolded. The thickness of the support film 20 can be, for example, 10–200 μm or 20–170 μm.

[0085] As a method for applying adhesive varnish to the support film 20, known methods can be used, such as blade coating, roller coating, spraying, gravure coating, bar coating and curtain coating.

[0086] Organic solvents remaining after the adhesive varnish is applied to the support film can be removed by heat drying. There are no particular limitations regarding heat drying, as long as the organic solvents used are sufficiently evaporated; for example, the heat drying temperature can be 50–200°C, and the heat drying time can be 0.1–30 minutes. Heat drying can also be carried out in stages at different heat drying temperatures or for different heat drying times.

[0087] The thickness of the die bonding film 10A can be appropriately adjusted according to the application, for example, it can be 3 to 200 μm. When the thickness of the die bonding film 10A is 3 μm or more, it tends to have sufficient adhesion strength to the semiconductor wafer, and when it is 200 μm or less, it tends to have sufficient thermal conductivity. From the viewpoint of adhesion strength and the thinning of semiconductor devices, the thickness of the die bonding film 10A can be 5 to 100 μm or 10 to 50 μm.

[0088] The thermal conductivity (25℃±1℃) of the grain-bonded film 10A after thermosetting at 170℃ for 3 hours (C-order state) can be 4.0 W / (m·K) or higher. When the thermal conductivity is 4.0 W / (m·K) or higher, it tends to have better heat dissipation performance for semiconductor devices. The thermal conductivity can be 4.5 W / (m·K) or higher, 5.0 W / (m·K) or higher, 5.5 W / (m·K) or higher, or 6.0 W / (m·K) or higher. There is no particular upper limit to the thermal conductivity (25℃±1℃) of the grain-bonded film 10A in the C-order state, and it can be 30 W / (m·K) or lower.

[0089] The thermal conductivity (25℃±1℃) of a grain-bonded film 10A after heat curing at 170℃ for 3 hours (C-order state) can be determined, for example, by the following method. First, the grain-bonded film is cut to a specified size, and a specified number of film sheets are prepared so that the thickness is 200μm when laminated. For example, if a grain-bonded film with a thickness of 25μm is used, 8 film sheets are prepared. If a grain-bonded film with a thickness of 10μm is used, 20 film sheets are prepared. These film sheets are laminated on a hot plate at 70℃ using rubber rollers to prepare a laminate with a thickness of 200μm. Next, each laminate is heat-cured in a clean oven (manufactured by ESPEC Corp.) at 170℃ for 3 hours to obtain a sample in the C-order state. The obtained sample is cut into 1cm×1cm pieces and used as a film for thermal conductivity measurement. The thermal conductivity is measured under the following measurement items / conditions.

[0090] (Calculation of thermal conductivity) The thermal conductivity λ of the film used for thermal conductivity measurement is calculated using the following formula in the thickness direction.

[0091] Thermal conductivity λ (W / (m·K)) = thermal diffusivity α (m 2 / s) × Specific heat Cp (J / (kg·K)) × Density ρ (g / cm³) 3 ) In addition, thermal diffusivity α, specific heat Cp, and density ρ are determined by the following methods. A high thermal conductivity λ indicates better heat dissipation in semiconductor devices.

[0092] (Determination of thermal diffusivity α) The test sample is prepared by blackening both sides of the membrane used for measuring thermal conductivity using graphite spraying. For the test sample, the thermal diffusivity α of the membrane used for measuring thermal conductivity is determined by laser flash method (xenon flash method) under the following conditions, for example, using the following measuring apparatus.

[0093] • Measuring apparatus: Thermal diffusivity measuring apparatus (manufactured by NETZSCH Japan KK Corporation, product name: LFA447nanoflash) • Pulse width of pulsed light irradiation: 0.1ms • Applied voltage for pulsed light irradiation: 236V • Sample preparation: Both sides of the membrane used for thermal conductivity measurement were blackened using graphite spraying. • Measured ambient temperature: 25℃±1℃ (Determination of specific heat Cp (25℃)) The specific heat Cp (25°C) of the membrane used for thermal conductivity measurement is determined, for example, by differential scanning calorimetry (DSC) under the following conditions using the measuring apparatus described below.

[0094] • Measuring apparatus: Differential scanning calorimetry apparatus (manufactured by PerkinElmer Japan Co., Ltd., product name: Pyris1) • Reference material: Sapphire • Heating rate: 10℃ / minute • Heating temperature range: room temperature (25℃) ~ 60℃ (Determination of density ρ) The density ρ of a membrane used for measuring thermal conductivity is determined, for example, by the Archimedes method using the following measuring apparatus under the following conditions.

[0095] • Measuring device: Electronic hydrometer (manufactured by ALFA MIRAGE CO.,LTD., trade name: SD200L) Water temperature: 25℃ By including components (a) and (b) in the grain bonding film, thermal conductivity can be improved, thereby enhancing the heat dissipation of semiconductor devices. Therefore, the grain bonding film can be combined with a cutting tape (cutting film) having a pressure-sensitive adhesive layer and is preferably used as an integral grain bonding film.

[0096] [Integrated membrane with grain cutting and bonding] Figure 2 This is a schematic cross-sectional view illustrating one embodiment of a grain-jointed integral film. Figure 2 The integrated grain bonding membrane 100 shown includes: a cutting tape 50 (cutting film) having a substrate layer 40 and a pressure-sensitive adhesive layer 30 disposed on the substrate layer 40; and an adhesive layer 10 disposed on the pressure-sensitive adhesive layer 30 of the cutting tape 50 and formed from the grain bonding membrane 10A. The integrated grain bonding membrane 100 can be in the form of a film, sheet, or strip. The integrated grain bonding membrane 100 may have a support film 20 on the surface of the adhesive layer 10 opposite to the pressure-sensitive adhesive layer 30.

[0097] As the substrate layer 40 in the cutting tape 50, examples include plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, and polyimide film. Furthermore, the substrate layer 40 can be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, and etching treatment as needed.

[0098] The pressure-sensitive adhesive layer 30 on the cutting tape 50 is not particularly limited in that it has sufficient pressure-sensitive adhesive force to prevent the semiconductor chip from scattering during cutting, and low pressure-sensitive adhesive force to prevent damage to the semiconductor chip during subsequent semiconductor chip pick-up processes. Any pressure-sensitive adhesive layer conventionally known in the field of cutting tapes can be used. The pressure-sensitive adhesive layer 30 can be a pressure-sensitive adhesive layer formed from a non-UV-curable pressure-sensitive adhesive or a pressure-sensitive adhesive layer formed from a UV-curable pressure-sensitive adhesive. When the pressure-sensitive adhesive layer is formed from a UV-curable pressure-sensitive adhesive, the adhesiveness of the pressure-sensitive adhesive layer can be reduced by irradiating it with UV light.

[0099] From the perspective of economy and membrane operability, the thickness of the cutting tape 50 (substrate layer 40 and pressure-sensitive adhesive layer 30) can be 60-150 μm or 70-130 μm.

[0100] Figure 2 The die bonding integrated film 100 shown can be obtained by a manufacturing method comprising the following steps: preparing a die bonding film 10A and a cutting tape 50 having a substrate layer 40 and a pressure-sensitive adhesive layer 30 disposed on the substrate layer 40; and bonding the die bonding film 10A to the pressure-sensitive adhesive layer 30 of the cutting tape 50. As a method for bonding the die bonding film 10A to the pressure-sensitive adhesive layer 30 of the cutting tape 50, a known method can be used.

[0101] Semiconductor devices and manufacturing methods thereof Figure 3 This is a schematic cross-sectional view illustrating one embodiment of a method for manufacturing a semiconductor device. Figure 3 (a), (b), (c), (d), (e), and (f) are schematic cross-sectional views illustrating each process. The method for manufacturing a semiconductor device includes the process of attaching a semiconductor wafer W to the adhesive layer 10 of the aforementioned die-bonding integral film 100 (wafer lamination process, see reference). Figure 3 (a) and (b)); the process of monolithizing the semiconductor wafer W and the adhesive layer 10 (dicing process, see reference) Figure 3 (c) ; as needed, a process of irradiating the pressure-sensitive adhesive layer 30 (through the substrate layer 40) with ultraviolet light (ultraviolet irradiation process, see reference) Figure 3 (d)); the process of picking up the semiconductor chip 60 with the adhesive layer from the cutting tape 50 (pressure-sensitive adhesive layer 30) (picking process, see reference). Figure 3 (e)); the process of bonding the semiconductor chip 60 with the adhesive layer to the support member 80 by means of the adhesive layer 10a (semiconductor chip bonding process, see reference). Figure 3(f)); and, as needed, the process of thermally curing the adhesive layer 10a bonded to the semiconductor chip 60 with the adhesive layer on the support member 80 (thermal curing process).

[0102] <Wafer Lamination Process> In this process, firstly, the die-cutting and bonding integrated film 100 is placed in a prescribed apparatus. Next, the surface Ws of the semiconductor wafer W (see reference) is attached to the adhesive layer 10 of the die-cutting and bonding integrated film 100. Figure 3 (a) and (b)). The circuit surface of the semiconductor wafer W can be located on the side opposite to the surface Ws.

[0103] As semiconductor wafers W, examples include monocrystalline silicon, polycrystalline silicon, various ceramics, gallium arsenide and other compound semiconductors.

[0104] <Cutting Process> In this process, the semiconductor wafer W and the adhesive layer 10 are cut into single-piece wafers (see reference). Figure 3 (c) At this time, a portion of the pressure-sensitive adhesive layer 30 or all of the pressure-sensitive adhesive layer 30 and a portion of the substrate layer 40 can also be cut and monolithized. In this way, the cut grain bonding integral film 100 also functions as a cutting disc.

[0105] <Ultraviolet Irradiation Process> When the pressure-sensitive adhesive layer 30 is a pressure-sensitive adhesive layer formed of a UV-curable pressure-sensitive adhesive, the semiconductor device manufacturing method may include a UV irradiation step. In this step, the pressure-sensitive adhesive layer 30 (within the substrate layer 40) is irradiated with UV light (see reference). Figure 3 (d) In ultraviolet irradiation, the wavelength of ultraviolet light can be 200–400 nm. Regarding ultraviolet irradiation conditions, the illuminance and irradiation dose can be 30–240 mW / cm², respectively. 2 The range is 50–500 mJ / cm 2 The range.

[0106] <Pickup Process> In this process, the monolithically formed semiconductor chips 60 with adhesive layers are separated from each other by expanding the substrate layer 40, and the semiconductor chips 60 with adhesive layers that are ejected from the substrate layer 40 side by the ejector pin 72 are picked up using a pick-up chuck 74 and removed from the pressure-sensitive adhesive layer 30a (see reference). Figure 3(e) Additionally, the semiconductor chip 60 with adhesive layer has a semiconductor chip Wa and an adhesive layer 10a. The semiconductor chip Wa is obtained by monolithizing the semiconductor wafer W, and the adhesive layer 10a is obtained by monolithizing the adhesive layer 10. Furthermore, the pressure-sensitive adhesive layer 30a is obtained by monolithizing the pressure-sensitive adhesive layer 30. After picking up the semiconductor chip 60 with adhesive layer, the pressure-sensitive adhesive layer 30a may remain on the substrate layer 40. In this process, it is not necessarily necessary to extend the substrate layer 40, but extending the substrate layer 40 can further improve pickability.

[0107] The push-up amount of the ejector pin 72 can be appropriately set. Furthermore, from the viewpoint of ensuring sufficient pick-up even for extremely thin wafers, for example, two or three stages of push-up can be performed. Also, semiconductor chips 60 with adhesive layers can be picked up using methods other than using the pick-up chuck 74.

[0108] <Semiconductor chip bonding process> In this process, the picked-up semiconductor chip 60 with adhesive layer is bonded to the support member 80 (reference) via adhesive layer 10a through thermoforming. Figure 3 (f)). Multiple semiconductor chips 60 with adhesive layers can be bonded to the support component 80.

[0109] The heating temperature during hot pressing can be, for example, 80–160°C. The load during hot pressing can be, for example, 5–15 N. The heating time during hot pressing can be, for example, 0.5–20 seconds.

[0110] <Thermosetting Process> In this process, the adhesive layer 10a bonded to the semiconductor chip 60 with the adhesive layer attached to the support member 80 is thermally cured. By thermally curing the adhesive layer 10a or the cured adhesive layer 10ac (further) that bonds the semiconductor chip Wa to the support member 80, a more secure bond can be achieved. Furthermore, by thermally curing the adhesive layer 10a or the cured adhesive layer 10ac (further), it is easier to obtain a sintered body of component (a). During thermal curing, pressure can also be applied simultaneously to cure it. The heating temperature in this process can be appropriately varied depending on the composition of the adhesive layer 10a. The heating temperature can be, for example, 60–200°C, 90–190°C, or 120–180°C. The heating time can be 30 minutes to 5 hours, 1–3 hours, or 2–3 hours. Alternatively, the temperature or pressure can be varied in stages.

[0111] The adhesive layer 10a can be cured into a cured adhesive layer 10ac via a semiconductor chip bonding process or a thermal curing process. The cured adhesive layer 10ac may contain a sintered body of component (a). Therefore, the resulting semiconductor device can be a semiconductor device with excellent heat dissipation.

[0112] The manufacturing method of a semiconductor device may include, as needed, a step (wire bonding step) of electrically connecting the ends of the terminals (inner leads) of a support component to the electrode pads on a semiconductor chip using bonding leads. Examples of bonding leads used are gold wire, aluminum wire, and copper wire. The temperature for wire bonding can be in the range of 80–250°C or 80–220°C. The heating time can be from several seconds to several minutes. Wire bonding can also be performed while heated within the above temperature range using ultrasonic vibration energy and pressure-based crimping energy.

[0113] The manufacturing method of a semiconductor device may also include, as needed, a process of sealing the semiconductor chip with a sealing material (sealing process). This process is performed to protect the semiconductor chip or bonding leads mounted on a support component. This process can be performed by molding a sealing resin (sealing resin) using a mold. For example, an epoxy resin can be used as the sealing resin. By embedding the support component and residues through heat and pressure during sealing, delamination caused by air bubbles at the bonding interface can be prevented.

[0114] The manufacturing method of a semiconductor device may also include, as needed, a step (post-curing step) to fully cure the sealing resin that was not adequately cured in the sealing process. If the adhesive layer was not thermally cured in the sealing process, it can be thermally cured simultaneously with the sealing resin in this step to achieve bonding and fixation. The heating temperature in this step can be appropriately set depending on the type of sealing resin, for example, in the range of 165–185°C, and the heating time can be approximately 0.5–8 hours.

[0115] The manufacturing method of a semiconductor device may also include, as needed, a step (heating and melting step) in which a semiconductor chip with an adhesive layer bonded to a support component is heated in a reflow oven. In this step, the resin-sealed semiconductor device can be surface-mounted onto the support component. Examples of surface-mount methods include reflow soldering, where solder is pre-supplied onto a printed circuit board and then melted using hot air or similar methods. Examples of heating methods include hot air reflow soldering and infrared reflow soldering. Furthermore, the heating method can be applied to the entire device or to a specific area. The heating temperature can be, for example, in the range of 240–280°C.

[0116] Figure 4This is a schematic cross-sectional view illustrating one embodiment of a semiconductor device. Figure 4 The semiconductor device 200 shown includes a semiconductor chip Wa, a support member 80 mounting the semiconductor chip Wa, and an adhesive member 12. The adhesive member 12 is disposed between the semiconductor chip Wa and the support member 80, bonding the semiconductor chip Wa to the support member 80. The adhesive member 12 is a cured die bonding film (cured adhesive layer 10ac). The connection terminals (not shown) of the semiconductor chip Wa can be electrically connected to external connection terminals (not shown) via leads 70. The semiconductor chip Wa can also be sealed by a sealing material layer 92 formed of sealing material. Solder balls 94 can be formed on the side of the support member 80 opposite to surface 80A for electrical connection to an external substrate (motherboard) (not shown).

[0117] Semiconductor chip Wa can be, for example, an IC (integrated circuit). Supporting components 80 can include, for example, alloy lead frames, copper lead frames, etc.; plastic films such as polyimide resin and epoxy resin; modified plastic films obtained by impregnating polyimide resin, epoxy resin, etc., in glass nonwoven fabric and then curing them; ceramics such as alumina, etc.

[0118] The semiconductor device 200 has a cured product of the aforementioned grain bonding film as an adhesive component, thus exhibiting excellent heat dissipation.

[0119] Example The present invention will now be described in detail based on embodiments, but the present invention is not limited thereto.

[0120] (Example 1 and Comparative Examples 1 and 2) [Fabrication of Grain Bonding Film] <Preparation of Adhesive Varnish> Using the symbols and composition ratios (unit: parts by mass) shown in Table 1, cyclohexanone as an organic solvent was added to components (a), (b) or (b'), (c), (d), and (e) to prepare a raw material varnish. This raw material varnish was stirred for 20 minutes at a mixing temperature of 70°C using a homogenizer (manufactured by Tajima Chemical Machinery Co., Ltd., TKHOMO MIXER MARKII). Then, the raw material varnish was allowed to stand until it reached 20–30°C, at which point components (f) and (g) were added, and the mixture was stirred overnight using a three-in-one motor at 250 rpm. Thus, adhesive varnishes of Examples 1 and Comparative Examples 1 and 2 were prepared with a total content of 61–62% by mass for components (a), (b) or (b'), (c), (d), (e), (f), and (g), respectively.

[0121] The symbols for each component in Table 1 refer to the following components.

[0122] (a) Composition: Silver-containing particles manufactured by reduction method (coated silver-containing particles that have undergone surface treatment using a surface treatment agent) (a-1) Silver particles AG-3-1F (product name, manufactured by DOWA Electronics Materials Co., Ltd., shape: spherical, average particle size (laser 50% particle size (D)) 50 ): 1.4μm) (b) Components: Compounds represented by formula (1) (b-1)2-Methylglutaric acid (b') Components: Compounds other than those represented by formula (1) (b'-1)3-methylglutaric acid (b'-2)3,3-Tetramethyleneglutaric acid (c) Composition: Thermosetting resin (c-1) N-500P-10 (Product name, manufactured by DIC Corporation, cresol phenolic resin clear varnish type epoxy resin, epoxy equivalent: 204g / eq, softening point: 84℃) (c-2) EXA-830CRP (Product name, manufactured by DIC Corporation, bisphenol F type epoxy resin, epoxy equivalent: 159g / eq, liquid at 25℃) (d) Ingredients: Curing agent (d-1) MEH-7800M (Product name, manufactured by MEIWA PLASTICS INDUSTRIES, LTD. (now UBE Corporation), phenyl aralkyl phenolic resin, hydroxyl equivalent: 174 g / eq, softening point: 80℃) (e) Component: Elastomer (e-1) SG-P3 Solvent Change Product (Product name, manufactured by Nagase ChemteX Corporation, acrylate rubber, weight average molecular weight: 800,000, Tg: 12℃) (f) Ingredients: Curing accelerator (f-1) 1B2MZ (Product name, manufactured by SHIKOKU CHEMICALS CORPORATION, 1-benzyl-2-methylimidazolium) (g) Component: Coupling agent (g-1) Z-6119 (Product name, manufactured by Dow Toray Co., Ltd., 3-ureidopropyltriethoxysilane) <Fabrication of Grain Bonding Film> Grain bonding films were prepared using the aforementioned adhesive varnishes. Each adhesive varnish was vacuum degassed, and the resulting varnish was applied to a polyethylene terephthalate (PET) film (thickness: 38 μm) that had undergone a demolding treatment, serving as a support film. The applied adhesive varnish was then heated and dried in two stages at different temperatures: 90°C for 5 minutes followed by 130°C for 5 minutes, thereby obtaining grain bonding films of Example 1 and Comparative Examples 1 and 2 with a thickness of 25 μm in the B-stage state on the support film.

[0123] <Calculation of volume %> Regarding the content (volume %) of component (a), the density of the grain-bonded film is set as x (g / cm³). 3 Let the density of component (a) be y (g / cm³). 3 The mass percentage of component (a) in the grain bonding film was set as z (mass%) and calculated using the following formula (I). Furthermore, the mass percentage of component (a) in the grain bonding film was determined by thermogravimetric analysis using a differential thermogravimetric analysis (TG-DTA) apparatus. The densities of the grain bonding film and component (a) were determined by measuring their mass and specific gravity using a hydrometer.

[0124] (a) Content of component (volume %) = (x / y) × z (I) Measurement conditions for TG-DTA: temperature range 30–600℃ (heating rate 30℃ / min), maintained at 600℃ for 20 minutes. Air flow rate: 300 mL / min Thermogravimetric Differential Thermal Analysis Apparatus: Manufactured by Seiko Instruments Inc., TG / DTA220 Hydrometer: Manufactured by ALFA MIRAGE CO.,LTD., EW-300SG [Evaluation of Grain-Bound Films (Determination of Thermal Conductivity)] (Preparation of a membrane for measuring thermal conductivity) The grain bonding films were cut to specified dimensions, and eight films (thickness: 25 μm) of the grain bonding films of Examples 1 and Comparative Examples 1 and 2 were prepared. These films were then laminated on a hot plate at 70°C using a rubber roller to prepare a laminate with a thickness of 200 μm. Each laminate was then thermocured in a clean oven (manufactured by ESPEC Corp.) at 170°C for 3 hours, thereby obtaining samples in the C-order state. The prepared samples were punched into 1 cm × 1 cm pieces and used as films for thermal conductivity measurement. The thermal conductivity was measured under the following measurement items / conditions. The results are shown in Table 1. Note that the values ​​shown in Table 1 are relative values ​​when the thermal conductivity value of Comparative Example 1 is set to 100.

[0125] (Calculation of thermal conductivity) The thermal conductivity λ in the thickness direction of the film used for thermal conductivity measurement was calculated using the following formula.

[0126] Thermal conductivity λ (W / (m·K)) = thermal diffusivity α (m 2 / s) × Specific heat Cp (J / (kg·K)) × Density ρ (g / cm³) 3 ) In addition, the thermal diffusivity α, specific heat Cp, and density ρ were determined using the following methods. A high thermal conductivity λ indicates superior heat dissipation in semiconductor devices.

[0127] (Determination of thermal diffusivity α) The test sample was prepared by blackening both sides of the membrane used for measuring thermal conductivity using graphite spraying. The thermal diffusivity α of the membrane was determined using the following measuring apparatus under the following conditions via laser flash method (xenon flash method) for the test sample.

[0128] • Measuring apparatus: Thermal diffusivity measuring apparatus (manufactured by NETZSCH Japan KK Corporation, product name: LFA447nanoflash) • Pulse width of pulsed light irradiation: 0.1ms • Applied voltage for pulsed light irradiation: 236V • Sample preparation: Both sides of the membrane used for thermal conductivity measurement were blackened using graphite spraying. • Measured ambient temperature: 25℃±1℃ (Determination of specific heat Cp (25℃)) The specific heat Cp (25°C) of the membrane used for thermal conductivity measurement is determined by differential scanning calorimetry (DSC) under the following conditions using the following measuring apparatus.

[0129] • Measuring apparatus: Differential scanning calorimetry apparatus (manufactured by PerkinElmer Japan Co., Ltd., product name: Pyris1) • Reference material: Sapphire • Heating rate: 10℃ / minute • Heating temperature range: room temperature (25℃) ~ 60℃ (Determination of density ρ) The density ρ of the membrane used for measuring thermal conductivity was determined by the Archimedes method using the following measuring apparatus under the following conditions.

[0130] • Measuring device: Electronic hydrometer (manufactured by ALFA MIRAGE CO.,LTD., trade name: SD200L) Water temperature: 25℃ [Table 1]

[0131] As shown in Table 1, the grain bonding film of Example 1 containing the compound represented by Formula (1) exhibits superior thermal conductivity compared to the grain bonding films of Comparative Examples 1 and 2, which do not contain the compound represented by Formula (1). These results confirm that the integrated grain bonding film of the present invention can be used to manufacture semiconductor devices with excellent heat dissipation.

[0132] Symbol Explanation 10-Adhesive layer, 10A-Die bonding film, 10a-Adhesive sheet, 10ac-Cure of adhesive sheet, 12-Adhesive component, 20-Support film, 30, 30a-Pressure-sensitive adhesive layer, 40-Substrate layer, 50-Cut tape, 60-Semiconductor chip with adhesive sheet, 70-Lead wire, 72-Ejector pin, 74-Suction chuck, 80-Support component, 92-Sealing material layer, 94-Solder ball, 100-Cut die bonding integrated film, 200-Semiconductor device, W-Semiconductor wafer, Wa-Semiconductor chip.

Claims

1. A method for manufacturing a grain bonding film, comprising: The first step involves preparing a raw material varnish containing silver particles manufactured by reduction, a compound represented by formula (1), and an organic solvent; In the second step, the raw material varnish is mixed to obtain an adhesive varnish; and In the third step, the adhesive varnish is applied to the support film, and the organic solvent is removed, thereby obtaining a grain-bonded film. The content of silver particles is 70% by mass or more, based on the total solid content of the adhesive varnish. In equation (1), R 1 R 2 R 3 and R 4 Each can be independently represented by a hydrogen atom, a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom. Among them, R 1 R 2 R 3 and R 4 At least one of them is a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom.

2. A method for manufacturing a grain bonding film, comprising: The first step involves preparing a raw material varnish containing silver particles that have been surface-treated with a surface treatment agent, a compound represented by formula (1), and an organic solvent; In the second step, the raw material varnish is mixed to obtain an adhesive varnish; and In the third step, the adhesive varnish is applied to the support film, and the organic solvent is removed, thereby obtaining a grain-bonded film. The content of silver particles is 70% by mass or more, based on the total solid content of the adhesive varnish. In equation (1), R 1 R 2 R 3 and R 4 Each can be independently represented by a hydrogen atom, a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom. Among them, R 1 R 2 R 3 and R 4 At least one of them is a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom.

3. The method for manufacturing a grain bonding film according to claim 1 or 2, wherein, The second step is to mix the raw material varnish at a temperature of 50°C or higher.

4. The method for manufacturing a grain bonding film according to claim 1 or 2, wherein, The raw material varnish further contains thermosetting resin, curing agent and elastomer.

5. The method for manufacturing a grain bonding film according to claim 4, wherein, The thermosetting resin includes epoxy resin, which is liquid at 25°C.

6. The method for manufacturing a grain bonding film according to claim 1 or 2, wherein, The second step is to add thermosetting resin, curing agent and elastomer to the mixed raw material varnish to obtain a binder varnish containing them.

7. The method for manufacturing a grain bonding film according to claim 6, wherein, The thermosetting resin includes epoxy resin, which is liquid at 25°C.

8. A method for manufacturing a grain-cutting and bonding integral film, comprising the following steps: Prepare a cutting tape having a substrate layer and a pressure-sensitive adhesive layer disposed on the substrate layer; and The grain bonding film manufactured by the manufacturing method of the grain bonding film according to claim 1 or 2 is bonded to the pressure-sensitive adhesive layer of the cut tape to form an adhesive layer formed by the grain bonding film on the pressure-sensitive adhesive layer.

9. A method for manufacturing a semiconductor device, comprising the following steps: The adhesive layer of the die-cutting bonded integral film manufactured by the manufacturing method of the die-cutting bonded integral film according to claim 8 is attached to a semiconductor wafer. Monolithize the semiconductor wafer and the adhesive layer; Pick up the semiconductor chip with adhesive layer from the cutting tape; and The semiconductor chip with the adhesive layer is bonded to the support component by means of the adhesive layer.

10. A grain-bonded film comprising silver-containing particles manufactured by a reduction method and a compound represented by formula (1), The content of silver particles is 70% by mass or more, based on the total amount of the grain-bonding film. In equation (1), R 1 R 2 R 3 and R 4 Each can be independently represented by a hydrogen atom, a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom. in, R 1 R 2 R 3 and R 4 At least one of them is a halogen atom, a methyl group that can be substituted by a halogen atom, or an ethyl group that can be substituted by a halogen atom.

11. The grain bonding film according to claim 10, further comprising a thermosetting resin, a curing agent, and an elastomer.

12. The grain bonding film according to claim 11, wherein, The thermosetting resin includes epoxy resin, which is liquid at 25°C.

13. A single-layer film for grain cutting and bonding, comprising: A cutting tape having a substrate layer and a pressure-sensitive adhesive layer disposed on the substrate layer; and An adhesive layer disposed on the pressure-sensitive adhesive layer of the cut tape and formed of a grain bonding film according to any one of claims 10 to 12.

14. A semiconductor device comprising: Semiconductor chips; Support component, housing the semiconductor chip; and An adhesive component is disposed between the semiconductor chip and the support component to bond the semiconductor chip and the support component. The adhesive component comprises a cured product of the grain bonding film according to any one of claims 10 to 12.

Citation Information

Patent Citations

  • Novel cyclic amide compound

    JP1988096189A

  • Dicing die bond film

    JP2008218571A